Magnetic body, magnet, and method for manufacturing magnetic body

The synthesis and processing of FeNiN particles to form flat-shaped magnetic particles with enhanced coercive force address the limitations of existing FeNi ordered alloys, resulting in improved magnetic properties and performance for applications like motors.

WO2024219436A1PCT designated stage expired Publication Date: 2024-10-24DENSO CORP +1

Patent Information

Application Number
PCT/JP2024/015324
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-04-21
Filing Date
2024-04-17
Publication Date
2024-10-24

AI Technical Summary

Technical Problem

Magnetic materials with FeNi ordered alloys have limited coercive force, which is essential for high-performance applications such as motors, where higher coercivity is required for improved magnetic properties.

Method used

A method involving the synthesis of FeNiN particles, followed by flattening, coating with a non-magnetic material, heat treatment, and denitrification to enhance the regularity and coercive force of the FeNi ordered alloy, resulting in magnetic particles with a flat shape and aligned easy magnetization axis, thereby increasing coercive force.

Benefits of technology

The method achieves a higher coercive force and regularity in magnetic particles, enhancing their magnetic properties and suitability for applications like motors, with improved resistance to demagnetizing fields and higher magnetic flux density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024015324_24102024_PF_FP_ABST
    Figure JP2024015324_24102024_PF_FP_ABST
Patent Text Reader

Abstract

In a magnetic body (2) comprising magnetic particles (3) containing an FeNi ordered alloy of an L10 type ordered structure, the magnetic particles each have a flat shape in which a long axis (31) and a short axis (32) shorter than the long axis intersect each other, and in which a flat surface (33) along the long axis is wider than an end surface (34) along the short axis. The axis (35) of easy magnetization of the L10 type ordered structure is along the flat surface.
Need to check novelty before this filing date? Find Prior Art

Description

Magnetic body, magnet, and method for manufacturing magnetic body CROSS-REFERENCE TO RELATED APPLICATIONS

[0001] This application is based on Japanese Patent Application No. 2023-69919, filed on April 21, 2023, the contents of which are incorporated herein by reference.

[0002] The present disclosure relates to L1 0 The present invention relates to a magnetic material containing an FeNi ordered alloy with a type ordered structure, a magnet, and a method for producing the magnetic material.

[0003] L1 superlattice structure 0 Magnetic materials with an ordered structure have high magnetic anisotropy and are therefore expected to be used as magnet materials and magnetic recording materials. 0 The ordered structure is found in alloys such as FePt, FePd, AuCu, etc. Here, the FeNi superlattice, i.e., L1, is mainly composed of iron and nickel, which are abundant and inexpensive raw materials. 0 FeNi ordered alloys with a type-ordered structure have been attracting attention. Magnetic materials containing such FeNi ordered alloys have higher heat resistance than conventional rare earth magnetic materials, and therefore can be suitably applied to electric appliances such as motors. For example, the magnetic material described in Patent Document 1 is known as such a magnetic material. The magnetic material described in Patent Document 1 has an L1 order of 0.5 or more as determined by measurement with an X-ray diffraction device. 0 The present invention includes an FeNi ordered alloy powder of the type.

[0004] Patent No. 6528865

[0005] It is desirable to obtain a higher coercive force in a magnetic material or magnetic body containing such an FeNi ordered alloy. The present disclosure has been made in consideration of the circumstances exemplified above. The purpose of the present disclosure is to provide a magnetic material or magnetic body containing an FeNi ordered alloy having a high coercive force and an L1 0 The present invention provides a magnetic body containing an FeNi ordered alloy with a type ordered structure, a magnet, and a method for producing the magnetic body.

[0006] The magnetic body according to the first aspect of the present disclosure has an L1 0The magnetic particles each have a flat shape in which a major axis intersects with a minor axis that is shorter than the major axis, and the flat surface along the major axis is wider than the side surface along the minor axis, and L1 0 The magnetization easy axis of the ordered structure is along the flat plane. The magnet according to the second aspect of the present disclosure includes such a magnetic material. 0 A method for producing a magnetic body having magnetic particles containing an FeNi ordered alloy with a regular structure includes flattening FeNiN particles and subjecting the flattened FeNiN particles to a denitrification treatment.

[0007] In addition, in each section of the application documents, each element may be assigned a reference symbol in parentheses. In this case, the reference symbol merely indicates an example of the correspondence between the element and the specific configuration described in the embodiment described below. Therefore, the present disclosure is not limited in any way by the description of the reference symbol.

[0008] 1 is a schematic diagram of a magnet; 2 is a schematic diagram of a magnetic substance contained in a magnet; 3 is a schematic diagram of a magnetic particle; 4 is a schematic diagram showing the cross-sectional structure of a magnetic particle; and 5 is a schematic diagram of an L1 contained in a magnetic particle. 0 1 is a schematic diagram showing the lattice structure of an FeNi ordered alloy of type L1. 013 is a schematic diagram showing the lattice structure of FeNiN, which is a precursor of an FeNi ordered alloy of the type. FIG. 14 is a flowchart showing an outline of one embodiment of a method for manufacturing a magnetic body. FIG. 15 is a flowchart showing an outline of a method for manufacturing a magnetic body according to Comparative Example 1. FIG. 16 is a table comparing evaluation results of Comparative Example 1 and Examples 1 to 3. FIG. 17 is an SEM photograph showing a precursor. FIG. 18 is an SEM photograph enlarging region A in FIG. 10. FIG. 19 is an SEM photograph enlarging region B in FIG. 10. FIG. 19 is a graph showing XRD patterns of an example and a comparative example. FIG. 20 is an enlarged graph of region C in FIG. 21. FIG. 22 is a graph showing hysteresis curves of an example and a comparative example. FIG. 23 is an SEM photograph of FeNiN particles in Comparative Example 1. FIG. 24 is an SEM photograph of FeNiN particles in Example 1. FIG. 25 is an SEM photograph of FeNiN particles in Example 2. FIG. 26 is an SEM photograph of FeNiN particles in Example 3. FIG. 27 is a graph showing the relationship between minor axis length and degree of order in the examples and comparative examples. FIG. 28 is a graph showing the relationship between major axis length and coercivity in the examples. FIG. 29 is a TEM photograph of FeNiN particles in Example 2. 23. is a photograph showing an electron beam diffraction image of the FeNiN particles of FIG. 22. is a photograph showing a dark-field image corresponding to the diffraction spot shown in region F of FIG. 23. is a photograph showing a dark-field image corresponding to the diffraction spot shown in region G of FIG. 23. is a TEM photograph of the FeNiN particles in Example 3. is a photograph showing an electron beam diffraction image of the FeNiN particles of FIG. 26. is a flowchart showing an outline of a manufacturing method for a magnetic body according to Comparative Example 2. is an SEM photograph of the FeNi particles in Comparative Example 2. is a table showing evaluation results of Comparative Example 2 and Example 2. is a flowchart showing an outline of a manufacturing method for a magnetic body according to Example 4. is a table showing evaluation results of Examples 3 and 4. is a flowchart showing an outline of a manufacturing method for a magnetic body according to Example 5. is a table showing evaluation results of Examples 3 and 5. is a TEM photograph showing the cross-sectional shape of the magnetic particles in Example 3. is a TEM photograph showing the cross-sectional shape of the magnetic particles in Example 5.

[0009] (Embodiments) Hereinafter, embodiments of the present disclosure will be described with reference to the drawings. However, the embodiments described below are examples for embodying the technical ideas of the present disclosure, and the present disclosure is not limited to the following. In this specification, the term "process" includes not only an independent process, but also a process that cannot be clearly distinguished from other processes, as long as the intended purpose of the process is achieved. The same applies to the terms "processing" and "procedure."

[0010] 1 to 4 show a magnet 1, a magnetic body 2, and magnetic particles 3. The magnet 1 contains a magnetic body 2. The magnet 1 is formed by molding the magnetic body 2 into a shape appropriate for the intended use.

[0011] The magnetic body 2 contains magnetic particles 3. The magnetic body 2 contains individual magnetic particles 3. "Individual" refers to a state in which the particles are in the form of primary particles that are not aggregated or adhered to each other, and exist independently without being supported by a support such as a substrate. In other words, the magnetic body 2 is the individual magnetic particles 3 themselves, a powder as an aggregate of individual magnetic particles 3, granules of such powder, or a lump-shaped compact of such powder.

[0012] As shown in FIG. 3 , each magnetic particle 3 has two flat surfaces 33 spaced apart from each other and a ring-shaped side surface 34 located between and connecting the two flat surfaces 33. The side surface 34 has a smaller area than the flat surfaces 33. A major axis 31 runs along the flat surfaces 33, and a minor axis 32 runs along the side surface 34. The major axis 31 and the minor axis 32 intersect. The minor axis 32 runs in the direction in which the two flat surfaces 33 are aligned. The length of the major axis 31 of the magnetic particle 3 is longer than the length of the minor axis 32. Thus, each magnetic particle 3 has a flat shape. In the magnetic particle 3, the easy axis of magnetization 35 runs along the flat surfaces 33. The major axis length refers to the longest length in the direction along the flat surfaces 33. The minor axis length refers to the longest length in the direction along the side surface 34 and intersecting the major axis 31.

[0013] As shown in FIG. 4, the magnetic particle 3 of this embodiment includes an alloy particle 36 and a coating layer 37 .

[0014] The alloy particles 36 are L1 0 The alloy particles 36 contain an FeNi ordered alloy with a regular structure. In addition to Fe and Ni, the alloy particles 36 may contain additives such as sulfur and unavoidable impurities. The alloy particles 36 form the shape of the magnetic particles 3 and have the magnetic properties of the magnetic particles 3.

[0015] The coating layer 37 covers the surface of the alloy particle 36. For example, as shown in Figures 35 and 36, the thickness of the coating layer 37 is expected to be uniform across the entire surface of the alloy particle 36. The coating layer 37 forms the flat surfaces 33 and side surfaces 34 of the magnetic particle 3 of this embodiment, but their shapes are determined by the alloy particle 36. The shape of the flat surfaces 33 is determined by the main surfaces of the alloy particle 36, and the shape of the side surfaces 34 is determined by the annular surfaces of the alloy particle 36. Therefore, the above-mentioned major axis 31 is along the main surfaces, and the minor axis 32 intersects the major axis 31 and is along the annular surfaces. The easy axis of magnetization 35 is along the main surfaces. Note that the magnetic particle 3 does not need to have the coating layer 37. If the magnetic particle 3 does not have the coating layer 37, the main surfaces of the alloy particle 36 correspond to the flat surfaces 33, and the annular surfaces correspond to the side surfaces 34.

[0016] The coating layer 37 functions to separate the magnetic coupling, in other words, the exchange interaction, between, for example, multiple adjacent magnetic grains 3, in this case, between alloy grains 36, within the magnetic body 2. For this reason, the coating layer 37 can also be called a "magnetic separation layer" or a "magnetic separation coating layer."

[0017] As described above, the alloy particles 36 are L1 0 It contains an FeNi ordered alloy with a type ordered structure. 0 The unit cell of the FeNi ordered alloy of the type ordered structure is shown in FIG. 5 as an FeNi superlattice 40. As shown in FIG. 0An FeNi ordered alloy with a type ordered structure has a face-centered cubic lattice as its base, with Fe and Ni arranged in layers in the (001) direction. Specifically, an FeNi superlattice 40 has an I site 41, which is the uppermost layer in the layered structure of the (001) plane of the face-centered cubic lattice, and an II site 42, which is an intermediate layer located between the uppermost layer and the lowermost layer. In FIG. 5 , the locations of atoms in the I site 41 are indicated by white circles, and the locations of atoms in the II site 42 are indicated by black circles. In this crystal structure, the a-axis 43 is the (010) direction, and the c-axis 44 is the (001) direction. The c-axis 44 is the easy axis of magnetization 35. In an FeNi superlattice 40 with a degree of order of 1 (described below), only Ni atoms are present in the I site 41, and only Fe atoms are present in the II site 42, among the Fe and Ni atoms.

[0018] The magnetic particles 3 are nanoparticles. That is, the major axis length and minor axis length are at the submicron level. The major axis length is 1000 nm or less, or several hundred nm or less. The minor axis length is 100 nm or less, or several tens of nm or less. "nm" indicates "nanometer."

[0019] When the magnetic body 2 contains a plurality of magnetic particles 3, it is assumed that not all of these magnetic particles 3 are necessarily present as individual particles, but that at least some of them are connected to each other. However, even in such a connected state, the flat shape and L1 of each of the magnetic particles 3 are 0 It is presumed that if there is no fundamental change in the ordered structure, the properties of the magnetic particles 3 will not be different from each other.

[0020] In this embodiment, the magnetic body 2 is formed so that the degree of ordering measured by powder X-ray diffraction is greater than 0.7, preferably 0.76 or more, and more preferably 0.8 or more. As described in Patent Document 1, Japanese Patent No. 6528865, the "degree of ordering" is an index showing the degree of ordering in the FeNi superlattice 40. When the ratio of metal A present in the I site 41 shown in FIG. 5 is x and the ratio of metal B present is 1-x, the ratio of metal A and metal B present in the I site 41 is A. x B1-x Similarly, when the ratio of metal B present at the II site 42 is x and the ratio of metal A present at the II site 42 is 1-x, the ratio of metal A and metal B present at the II site 42 is A 1-x B x where x satisfies 0.5≦x≦1. In this case, if the degree of order is expressed as OP, the degree of order is defined as OP=2x−1. The degree of order in the actually manufactured magnetic substance 2 is measured by powder X-ray diffraction. A method for measuring the degree of order by powder X-ray diffraction will be described later.

[0021] (Manufacturing Method) A manufacturing method for the magnetic body 2 according to this embodiment will be outlined below. In the manufacturing method according to this embodiment, FeNiN, which is a precursor material for the FeNi ordered alloy, is synthesized, and then the FeNiN is subjected to a denitrification treatment, thereby obtaining the magnetic body 2 containing the FeNi ordered alloy. FeNiN has the crystal structure shown in FIG. 6, which can be identified from the XRD diffraction pattern. XRD stands for X-ray diffraction. The FeNiN lattice 50 has an I site 51, a II site 52, and a III site 53. The I site 51 is located at the L1 0 The I site 41 corresponds to the I site in the ordered structure. The II site 52 corresponds to the L1 0 The III site 53 corresponds to the II site 42 in the ordered structure. The III site 53 is located at the middle position between the adjacent I sites 51 in the stacking direction. In FeNiN 50, it is expected that a Ni atom exists at the I site 51, an Fe atom exists at the II site 52, and an N atom exists at the III site 53.

[0022] As shown in FIG. 7 , the manufacturing method for the magnetic body 2 or magnetic particles 3 according to this embodiment involves executing the following procedures, processes, or steps 11 to 17 in this order. In the flowchart of FIG. 7 , "S" is an abbreviation for "step." This also applies to the other flowcharts described below. Step 11: FeNiN synthesis...FeNiN, which serves as a precursor material for the FeNi ordered alloy, is synthesized. Step 12: Coarse pulverization...The synthesized FeNiN is pulverized to produce FeNiN particles. Step 13: Flattening...The coarsely pulverized FeNiN particles are flattened by applying a mechanical force, such as mechanical shear force. Step 14: Classification...The flattened FeNiN particles have a particle size distribution. Therefore, flattened FeNiN particles of the desired particle size or particle size range are selected. Hereinafter, to avoid cumbersome notation, the flattened FeNiN particles will be designated by a symbol and referred to as flattened FeNiN particles 61. The flattened surface of the flattened FeNiN particle 61, corresponding to the flattened surface 33 of the magnetic particle 3, is referred to as the flattened surface 611. The long and short axes of the flattened FeNiN particle 61, corresponding to the long and short axes 31 and 32 of the magnetic particle 3, are referred to as the long axis 612 and the short axis 613. The c-axis of the flattened FeNiN particle 61, corresponding to the c-axis 44 of the magnetic particle 3, is referred to as the c-axis 614. The direction and orientation of the c-axis 44 or the c-axis 614 are simply referred to as the "c-axis direction" or "c-axis orientation." Meanwhile, FeNiN particles according to Comparative Example 1, which have not undergone at least a flattening treatment, are referred to as first comparative example particles 62. Furthermore, an aggregate of the flattened FeNiN particles 61 or the first comparative example particles 62 is referred to as the magnetic precursor 60. Step 15: Coating...The surfaces of the selected flattened FeNiN particles 61 are coated with a constituent material of the coating layer 37, such as silica. Step 16: Heat treatment...The flattened FeNiN particles 61 that have been subjected to coarse grinding and flattening may have defects due to deformation. In order to repair these defects, heat treatment (annealing) is performed. Step 17: Denitrification...The flattened FeNiN particles 61 that have undergone the above steps are subjected to a denitrification treatment. In this way, flattened magnetic particles 3 and the magnetic body 2 containing these are manufactured. Details and examples of each of the above steps are explained below.

[0023] (1) Synthesis of FeNiN The precursor material, FeNiN, can be synthesized using techniques already known or well-known at the time of filing of this application. For example, techniques described in Patent Document 1 and Japanese Patent No. 6627818 can be used. Specifically, FeNiN can be synthesized by nitriding powder of an FeNi disordered alloy produced by, for example, a thermal plasma method, a flame spray method, or a coprecipitation method. Alternatively, FeNiN can be obtained by reducing and nitriding FeNi oxide. The FeNi oxide used in the reduction step may contain Fe oxide or Ni oxide, or may contain an oxide containing Fe and Ni.

[0024] The Fe oxide is not particularly limited, but examples thereof include FeO, Fe 2 O 3 , Fe 3 O 4 Examples of the oxide include oxides obtained by oxidizing raw materials such as metallic iron, iron hydroxide, iron carbonate, iron chloride, iron iodide, iron bromide, iron sulfate, iron nitrate, iron phosphate, and iron oxalate. Examples of Ni oxide include, but are not limited to, NiO. Examples of the oxide include oxides obtained by oxidizing raw materials such as metallic nickel, nickel hydroxide, nickel carbonate, nickel chloride, nickel iodide, nickel bromide, nickel sulfate, nickel nitrate, nickel phosphate, and nickel oxalate. An oxide containing Fe and Ni can be produced by mixing a solution containing Fe and Ni with a precipitant to obtain a precipitate containing Fe and Ni (precipitation step), and then heat-treating the precipitate to obtain an oxide containing Fe and Ni (oxidation step). This method makes it easy to control the average particle size and particle size distribution of the resulting Fe and Ni oxide, and tends to produce a uniform distribution of Fe and Ni in the Fe and Ni oxide.

[0025] The Fe raw material and the Ni raw material are not limited as long as they can be dissolved in an acidic solution. Examples of Fe raw materials include metallic iron, iron oxide, iron hydroxide, iron carbonate, iron chloride, iron iodide, iron sulfate, iron nitrate, iron phosphate, and iron oxalate. Examples of Ni raw materials include metallic nickel, nickel oxide, nickel hydroxide, nickel carbonate, nickel chloride, nickel iodide, nickel sulfate, nickel nitrate, nickel phosphate, and nickel oxalate. Examples of acidic solutions include sulfuric acid, nitric acid, hydrochloric acid, and phosphoric acid. The concentration of the solution containing Fe and Ni can be appropriately adjusted within a range in which the Fe raw material and the Ni raw material are substantially soluble in the acidic solution. The reaction between the solution containing Fe and Ni and a precipitant may be carried out by adding the precipitant to the solution containing Fe and Ni, or by adding the solution containing Fe and Ni to the precipitant. Furthermore, the solution containing Fe and Ni referred to here may be any solution containing Fe and Ni upon reaction with the precipitant. Alternatively, raw materials containing Fe and Ni may be prepared as separate solutions, and each solution may be added to react with the precipitant. Even when prepared as separate solutions, the contents of each raw material are appropriately adjusted so that they substantially dissolve in the acidic solution. The precipitant is not limited as long as it reacts with the solution containing Fe and Ni to produce a precipitate, and examples thereof include oxalic acid and alkaline solutions such as aqueous sodium hydroxide, aqueous sodium bicarbonate, aqueous potassium hydroxide, and aqueous lithium hydroxide. Furthermore, a precipitate can be obtained by blowing carbon dioxide gas into the solution containing Fe and Ni. Examples of precipitates that can be produced include oxalates, carbonates, and hydroxides. Specifically, FeNiN can be obtained by air-sintering, hydrogen-reducing, and nitriding iron-nickel oxalate powder.

[0026] (2) Coarse Pulverization As a method for coarsely pulverizing FeNiN, a general pulverization method such as a ball mill can be used.

[0027] (3) Flattening Flattening can be easily performed using, but is not limited to, mechanical shearing force. For example, it can be performed by subjecting a slurry containing FeNiN particles to a wet bead mill. Specifically, a slurry is prepared by dispersing coarsely pulverized FeNiN particles in a solvent containing a surfactant. Surfactants that have good coating properties on the FeNiN particles can be used. Examples of surfactants include nitrogen-containing surfactants such as oleylamine and trioctylamine, sulfur-containing surfactants such as octanethiol and triazinedithiol, and polymer surfactants such as polyvinyl alcohol, polyacrylic acid, polyethyleneimine, and polyvinylpyrrolidone. A liquid that can stably disperse FeNiN particles coated with a surfactant can be used as the solvent. Examples include pure water, alcohols such as ethanol and isopropyl alcohol, and nonpolar solvents such as toluene and cyclohexane. In the example, a slurry containing 5% by weight of FeNiN particles in ethanol was placed in a bead mill (Fritsch Planetary Ball Mill PL-7) together with zirconia media having a diameter of 0.1 mm, and processed at 600 rpm for 30 minutes.

[0028] (4) Classification: To obtain a high coercive force, small flattened FeNiN particles 61 are extracted. Particle size classification can be performed by centrifuging the slurry. By centrifuging at 500 G for 10 minutes, at 4000 G for 10 minutes, and at 4000 G for 120 minutes in this order, the flattened FeNiN particles 61 with larger particle size were precipitated in order and collected.

[0029] (5) Coating As described above, the coating layer 37 serves to decouple the magnetic coupling between multiple magnetic particles 3 located nearby within the magnetic body 2. To this end, the coating layer 37 is formed of a non-magnetic material. Furthermore, the coating layer 37 must be made of a material that can be subjected to subsequent heat treatment and denitrification treatment and that does not react with the alloy particles 36. Materials that satisfy these requirements for the coating layer 37 include, for example, oxides of Group III-VII and Group XIII-XVI elements, such as silica, titania, zirconia, yttria, and alumina. Alternatively, films made of insulating materials, such as nitride films, may also be used. The thickness of the insulating film that constitutes the coating layer 37 is optional, but is preferably 1 nm or greater.

[0030] In this example, the classified flattened FeNiN particles 61 were coated with silica (silica coated). Coating at this stage suppresses particle sintering due to subsequent heat treatment or denitrification. It also suppresses contact between the alloy particles 36 contained in the magnetic body 2 during molding of the magnet 1. As a result, deterioration of the magnetic properties is suppressed.

[0031] When silica is used for the coating layer 37, a powder of the flattened FeNiN particles 61 is mixed into a solvent such as water or ethanol to which tetraethoxysilane has been added, and then an aqueous ammonia solution is poured in. As a result, the tetraethoxysilane is hydrolyzed and condensed to produce silica, and the flattened FeNiN particles 61 are coated with silica. The flattened FeNiN particles 61 are coated with the coating layer 37.

[0032] (6) Heat Treatment The flattened FeNiN particles 61 are heat-treated (annealed). This annealing aligns the atoms of the flattened FeNiN particles 61. The flattened FeNiN particles 61, whose atomic arrangement has been aligned by this annealing, are then denitrified. This increases the degree of ordering and coercivity of the denitrified FeNi ordered alloy (alloy particles 36). The annealing can be performed, for example, in ammonia gas. Specifically, in this embodiment, the flattened FeNiN particles 61 are placed in an electric furnace into which ammonia gas can be introduced, and the heat treatment is performed in ammonia gas. The ambient temperature can be set to 300 to 450°C, and the treatment time can be set to 4 to 48 hours. Since the flattened FeNiN particles 61 may contain sulfur as an impurity or additive, optimal treatment conditions vary depending on the particle size and the amount of sulfur present in the raw materials, but it is preferable to perform the annealing at a temperature lower than the nitriding temperature. This is because the stabilizing effect of sulfur on FeNiN weakens after pulverization, making it more susceptible to decomposition at high temperatures.

[0033] (7) Denitrification The denitrification treatment can be performed using the apparatus and method described in Patent Document 1 and Japanese Patent No. 6627818. Specifically, the denitrification treatment can be performed, for example, by heat treatment in a hydrogen atmosphere. The flow rate of hydrogen in the denitrification treatment can be set to 0.01 to 10 liters / min, and preferably 0.1 to 5 liters / min, per gram of flattened FeNiN particles 61. The heat treatment temperature can be set to, for example, 100 to 400°C, and preferably 200 to 350°C. The heat treatment time can be set to, for example, 1 to 24 hours, and preferably 2 to 10 hours.

[0034] (Effects) The effects achieved by the configuration and manufacturing method according to this embodiment will be described below using examples and comparative examples.

[0035] As Comparative Example 1, magnetic particles 3 were prepared using the manufacturing method shown in FIG. 8. In the manufacturing method shown in FIG. 8, the following steps 21 to 24 are performed. Step 21: FeNiN synthesis...FeNiN, which serves as a precursor material for an FeNi ordered alloy, is synthesized. Step 22: Pulverization...The synthesized FeNiN is pulverized to obtain first comparative example particles 62. The processing conditions are the same as those in Step 12. Step 23: Heat treatment...Defects may have occurred in the first comparative example particles 62 that have been subjected to the pulverization process. Therefore, heat treatment (annealing) is performed to repair these defects. Step 24: Denitrification...The first comparative example particles 62 obtained as described above are subjected to a denitrification process. In this way, magnetic bodies 2 and magnetic particles 3 are obtained as comparative examples.

[0036] As is clear from the above description, step 21 is the same as step 11, step 22 is the same as step 12, step 23 is the same as step 16, and step 24 is the same as step 17. The manufacturing method of Comparative Example 1 omits steps 13 to 15 in the manufacturing method of the Example.

[0037] FIG. 9 is a table showing the evaluation results of Comparative Example 1 and Examples 1 to 3. In the table, "CE" indicates "Comparative Example" and "PE" indicates Example. That is, "CE1" indicates "Comparative Example 1" and "PE1" indicates "Example 1". "CC" indicates classification conditions and "SHP" indicates particle shape. With regard to particle shape, "IS" indicates an irregular shape, i.e., a non-flat shape, and "FL" indicates a flat shape. "MA" indicates the major axis length, "SA" indicates the minor axis length, "CF" indicates coercive force, and "CFr" indicates relative coercive force. These are the same in the other drawings.

[0038] The method for measuring the major axis length and minor axis length will be described below with reference to Figures 10 to 12. Figure 10 is an SEM photograph of the magnetic precursor 60. SEM stands for scanning electron microscope. Figure 11 is an enlarged view of region A in Figure 10, with the arrow indicating the major axis length, which is the length of the major axis 612. Figure 12 is an enlarged view of region B in Figure 10, with the space between a pair of opposing arrows indicating the minor axis length, which is the length of the minor axis 613. The major axis length was calculated using image analysis software as follows.

[0039] An SEM photograph of an example or comparative example to be measured is selected and displayed. As shown in FIGS. 11 and 12 , the shapes of the flat surfaces 611 of the multiple flattened FeNiN particles 61 vary. Therefore, there are flattened FeNiN particles 61 for which it is easy to determine the longest length of the flat surfaces 611, and flattened FeNiN particles 61 for which it is difficult to do so. In other words, there are flattened FeNiN particles 61 for which it is easy to determine the longest length of the major axis 612, and flattened FeNiN particles 61 for which it is difficult to do so. The inventor selected, from the flattened FeNiN particles 61 shown in the photograph, particles for which it is easy to determine the longest axis length, such as those with an elliptical flat surface 611, and did not select particles for which it is difficult to determine the longest axis length, such as those with a U-shaped or J-shaped flat surface 611. The inventor measured the longest axis length of the selected flattened FeNiN particles 61.

[0040] Specifically, the length of a line segment corresponding to the major axis length can be determined by drawing the line segment on the screen using a straight line drawing tool in image analysis software. The length of the line segment can be converted into the actual measured size of the flattened FeNiN particle 61 by calibration using the scale bar shown in the photograph. Note that the image analysis software can be commercially available or free software available in the public domain at no charge.

[0041] In this embodiment, the major axis length is the average value measured for 100 flattened FeNiN particles 61. Therefore, the major axis length shown in FIG. 9 can also be referred to as the "average major axis length." For Comparative Example 1, since the particle shape is substantially spherical, the major axis length and minor axis length are not distinguished, and the average particle diameter for 100 first comparative particle 62 is used. Furthermore, the standard deviation of the measured values ​​for 100 flattened FeNiN particles 61 can be evaluated as the measurement error of the major axis length, and such measurement error is shown in FIG. 9 . The same applies to the first comparative particle 62. Because the measurement error of the major axis length is defined as a multiplicative error, there is variation in the measurement error between Comparative Example 1 and each example. Specifically, the measured major axis length of Example 1 was 640 nm, with a measurement error (standard deviation) of 205 nm. In contrast, the measured major axis length of Example 2 was 221 nm, with a measurement error of 82 nm.

[0042] The minor axis length is also measured in the same manner as the major axis length. That is, as shown in FIG. 12 , flattened FeNiN particles 61 in which a minor axis 613 is observed in the photograph are selected, and the thickest part of each particle is measured. The average value measured for 100 flattened FeNiN particles 61 is then taken as the minor axis length, and the standard deviation is taken as the measurement error. Since the measurement error of the minor axis length is multiplied, there is variation in the measurement error between Comparative Example 1 and each Example. Specifically, the minor axis length of Example 1 was measured at 49 nm, with a measurement error (standard deviation) of 15 nm. In contrast, the minor axis length of Example 2 was measured at 33 nm, with a measurement error of 8 nm.

[0043] As shown in Figure 11, in the flattened FeNiN particles 61 in which the major axis 612 can be observed, the minor axis 613 is difficult to observe. Conversely, as shown in Figure 12, in the flattened FeNiN particles 61 in which the minor axis 613 can be observed, the major axis 612 is difficult to observe. Therefore, the flattened FeNiN particles 61 in which the major axis 612 is measured are different from the flattened FeNiN particles 61 in which the minor axis 613 is measured. The objects to be measured for the major axis 612 and the minor axis 613 are different. However, as described above, 100 flattened FeNiN particles 61 were selected for each of the major axis 612 and the minor axis 613. The average values ​​of the major axis length and the minor axis length were calculated. Therefore, although the measurement objects of the major axis 612 and the minor axis 613 are different as described above, it is expected that the influence of the difference in the measurement objects on the calculated major axis length and minor axis length will be small.

[0044] As described above, the major axis length and minor axis length of the flattened FeNiN particles 61 before denitrification are measured, rather than the major axis length and minor axis length of the magnetic particles 3 after denitrification. The reason for this is as follows. As is clear from the flowchart of FIG. 7 , which shows the flow of a series of steps in the manufacturing method, in this example, the coating process of step 15 to form the coating layer 37 is performed before the denitrification process of step 17. Therefore, in the magnetic particles 3 obtained by denitrification, the outer surfaces of the alloy particles 36 are covered with the coating layer 37. Because the coating layer 37 is electrically insulating, charge-up makes it difficult to take SEM photographs. This makes it difficult to measure the major axis length and minor axis length of the magnetic particles 3. For this reason, the major axis length and minor axis length of the flattened FeNiN particles 61 are measured, rather than the major axis length and minor axis length of the magnetic particles 3.

[0045] It is estimated that the denitrification process reduces the size of the magnetic particles 3, in other words, the alloy particles 36, to a certain extent compared to the flattened FeNiN particles 61. It is estimated that the change from the FeNiN lattice 50 to the FeNi superlattice 40 reduces the lattice constant by approximately 10%. However, this change in size is within the range of the measurement error (standard deviation) mentioned above. It is also estimated that the particle shape and size distribution do not change significantly before and after denitrification. As mentioned above, the film thickness of the coating layer 37 is approximately 1 nm, which is also within the range of measurement error. For these reasons, the major axis length and minor axis length based on the measurement results from the SEM photograph of the flattened FeNiN particles 61 are considered to be the major axis length and minor axis length of the magnetic particles 3.

[0046] Additionally, the alloy particles 36 covered with the coating layer 37 can be observed using an SEM if gold or other metal is sputtered onto them. However, the additional thickness of the sputtered layer makes it difficult to accurately estimate the size. For this reason, we have decided not to adopt this method.

[0047] The method for evaluating the degree of order will be described below with reference to Figures 13 and 14. Figures 13 and 14 show XRD patterns of Comparative Example 1 and Example 3. In the figures, the lower pattern designated by symbol CE1 is Comparative Example 1, and the upper pattern designated by symbol PE3 is Example 3. Figure 14 is an enlarged view of region C surrounded by a dashed line in Figure 13. The degree of order is calculated by the following formula.

[0048] "(I sup / I fund ) obs "In "I fund As shown in FIG. 13, in the XRD pattern, the FeNi alloy and L1 0 The integral intensity of the fundamental diffraction peak, which is a diffraction peak that appears in both the FeNi ordered alloy and the I type ordered alloy. sup " is the L1 observed in the XRD pattern as shown in FIG. 0 This is the integrated intensity of the superlattice diffraction peak, which is a diffraction peak specific to an ordered alloy of this type. sup / I fund ) obs" is the ratio of the integrated intensity of the superlattice diffraction peak to the integrated intensity of the fundamental diffraction peak in the measured X-ray diffraction pattern. sup / I fund ) cal " is the ratio of the integrated intensity of the superlattice diffraction peak to the integrated intensity of the fundamental diffraction peak in an FeNi ordered alloy with an order degree of "1" estimated from Rietveld simulation. As for the powder X-ray diffractometer, a general one such as "SmartLab" manufactured by Rigaku Corporation can be used, but the order degree can be determined with high accuracy by using Fe-kβ rays as the X-rays.

[0049] In Figure 9, the measurement error is also shown for the measured value of the degree of order. The measurement error is estimated as follows. The measurement value may fluctuate slightly due to slight differences in the sample setting in the device and the analytical conditions. Specifically, for example, in the case of an FeNi alloy and an L1 0 The intensity of the ordered diffraction line of the FeNi ordered alloy is extremely small, and therefore it is easily affected by noise and background removal. sup This corresponds to a waveform obtained by smoothing the jagged XRD waveform in the region excluding the peak waveform region corresponding to I. By subtracting waveform BG from waveform FF obtained by smoothing the entire XRD waveform, I sup The waveform BG changes depending on the presence of components other than Fe and Ni, for example. That is, in addition to the pattern of the target sample, the components of the substrate, such as non-reflective silicon or silica coating, appear as a halo in the XRD pattern. This halo is removed as background by fitting using a polynomial in the analysis software attached to the instrument, but I can be estimated depending on the slight difference in the fitting parameters. sup changes. Therefore, even if the same sample is measured using Fe-kβ radiation, which allows easy observation of ordered diffraction lines, an intensity error of about 10% occurs. In this embodiment, the value of the degree of order corresponding to an intensity ratio of about 10% is taken as the measurement error. Since the measurement error of the degree of order is defined as multiplying the error, there is variation in the measurement error between the comparative example and each example.

[0050] The coercive force is determined by applying a magnetic field to a sample of the obtained magnetic material 2, and measuring the magnetic field strength at which the magnetization direction of the FeNi ordered alloy changes under the influence of the magnetic field. In Figure 15, the dashed hysteresis curve represents Comparative Example 1, and the solid hysteresis curve represents Example 3. A sample was prepared by molding it into a pellet of a predetermined cylindrical shape, and a sufficiently large magnetic field was applied to this sample to bring it to a saturated state where the magnetization of the sample no longer increases. A magnetic field in the opposite direction was then applied, and the timing at which the magnetization of the sample becomes zero was detected. The magnetic field strength at this time was taken as the coercive force. In Figure 15, the point corresponding to the measured coercive force in Example 3 is indicated by the symbol X. The coercive force was measured using a compact, cryogen-free physical property measurement system, PPMS VersaLab (PPMS is a registered trademark, VersaLab is a trademark) manufactured by Quantum Design, with a magnetic field sweep rate of 8 kA / m·sec, a measurement temperature of 300 K, and a magnetic field sweep range of -2.4 to 2.4 MA / m. The measurement error of the coercive force is at most ±4 kA / m. Therefore, the last digit of the measured coercive force value can be evaluated as being within the error range. For this reason, the coercive force values ​​shown in FIG. 9 are shown with the last digit set to 0, taking into account such error range. The relative coercive force values ​​shown in FIG. 9 indicate the relative values ​​of the coercive force, with the coercive force of Comparative Example 1 being set to a reference value of 1.

[0051] Comparative Example 1 corresponds to an example in which the flattening step 13, the classification step 14, and the coating step 15 in the Examples were omitted. Examples 1 to 3 were obtained by changing the processing conditions (classification conditions) for the classification step 14. FIG. 16 shows an SEM image of a magnetic precursor 60, which is an aggregate of first comparative example particles 62. FIGS. 17 to 19 show SEM images of magnetic precursor 60, which is an aggregate of flattened FeNiN particles 61 in Examples 1 to 3, respectively. As shown in FIG. 16, the particle shape in Comparative Example 1 was not flattened, whereas as shown in FIGS. 17 to 19, the particle shape in the Examples was flattened. Furthermore, these figures confirmed that particle size could be controlled depending on the classification conditions. That is, it was confirmed that smaller diameter particles could be obtained by increasing the rotation speed of the centrifuge and extending the processing time.

[0052] 9, it was confirmed that Examples 1 to 3, in which the particle shape was flattened, had a higher degree of ordering and a larger coercive force than Comparative Example 1, in which the particle shape was not flattened. Specifically, in Comparative Example 1, the degree of ordering did not exceed 0.7. In contrast, in each Example, the degree of ordering exceeded 0.7.

[0053] Among the examples, Example 1 has the lowest degree of order, and Example 3 has the highest degree of order. Specifically, in Example 1, the degree of order is 0.80, and the measurement error is 0.04. In Example 3, the degree of order is 0.89, and the measurement error is 0.05. Therefore, in this example, the range of possible values ​​for the degree of order that can be expected is 0.76 or more and 0.94 or less.

[0054] 20 is a graph showing the relationship between the degree of order and the minor axis length in Comparative Example 1 and Examples 1 to 3. Comparative Example 1 is shown by a triangular plot, and Examples 1 to 3 are shown by a square plot. The error range is also shown by an error bar.

[0055] As shown in FIG. 20 , the degree of order tends to increase as the minor axis length decreases. Specifically, in a graph of FIG. 20 using a logarithmic scale of the minor axis length on the horizontal axis and an equally spaced linear scale of the degree of order on the vertical axis, a negative linear relationship is observed between the minor axis length and the degree of order, as one decreases, the other increases, as indicated by the dashed line L1 in the figure. In particular, it is expected that a degree of order of 0.7 or more can be achieved by setting the minor axis length to 100 nm or less, or several tens of nm or less. Specifically, for example, the minor axis length is preferably on the order of several tens of nm, 50 nm or less, preferably 30 nm or less, and more preferably 20 nm or less. A possible lower limit of the minor axis length is several nm. A range of the minor axis length for a degree of order of 0.76 or more is considered to be several nm or more to 50 nm or less.

[0056] 21 is a graph showing the relationship between coercive force and major axis length in Examples 1 to 3. Examples are shown as circular plots, and error ranges are shown as error bars.

[0057] As shown in FIG. 21 , the shorter the major axis length, the higher the coercivity tends to be. Specifically, in a graph in FIG. 21 using a logarithmic scale of major axis length on the horizontal axis and an equally spaced linear scale of coercivity on the vertical axis, a linear relationship is observed between the major axis length and coercivity, with a negative slope indicated by the dashed line L2 in the figure, in which a decrease in one corresponds to an increase in the other. In particular, good coercivity can be obtained by setting the major axis length to 1,000 nm or less, or several hundred nm or less. Specifically, for example, the major axis length is preferably on the order of several hundred nm, 350 nm or less, and preferably 300 nm or less. This results in a coercivity of 200 kA / m or more. The lower limit of the major axis length is considered to be several tens of nm or approximately 10 nm. The range of the major axis length in which good coercivity can be obtained is considered to be several tens of nm or more and 350 nm or less.

[0058] FIG. 22 is a TEM bright-field image of a flattened FeNiN particle 61 in Example 2 having a major axis length of 300 nm or more, measured at 346 nm. TEM stands for Transmission Electron Microscope. The solid arrow in FIG. 22 indicates the major axis 612. FIG. 23 shows an electron beam diffraction image of the flattened FeNiN particle 61. FIG. 24 is a dark-field image corresponding to the spot surrounded by region F in the diffraction image of FIG. 23. FIG. 25 is a dark-field image corresponding to the spot surrounded by region G in the same diffraction image. The dark-field image in FIG. 24 corresponds to region D surrounded by a dashed line at the top of the flattened FeNiN particle 61 shown in FIG. 22. The dark-field image in FIG. 25 corresponds to region E surrounded by a dashed line at the bottom of the flattened FeNiN particle 61.

[0059] Thus, when the diffraction spots of the flattened FeNiN particles 61 of Example 2 were observed by electron beam diffraction, diffraction spots indicating that the c-axis 614 was located within the flat surface 611 were observed. Furthermore, it was confirmed that the spread of such spots, i.e., the angle θ1 between the two white lines in FIG. 23, was approximately 20°. Therefore, as shown by the dashed arrow in FIG. 22, it was confirmed that the c-axis direction was located within the flat surface 611 in the flattened FeNiN particles 61 of Example 2. Furthermore, it was also confirmed that the flattened FeNiN particles 61 of Example 2, which have a long major axis length, have a structure in which multiple regions with different c-axis directions are arranged along the major axis. The orientation of the c-axis 614 is equivalent in the FeNi ordered alloy after denitrification.

[0060] Figure 26 is a TEM image of a flattened FeNiN particle 61 having a major axis length of about 150 nm and an actual measured value of 137 nm in Example 3. As in Figure 22, the solid arrow indicates the major axis 612, and the dashed arrow indicates the direction of the c-axis 614. As shown in Figure 26, it can be confirmed that the c-axis direction is within the flat surface 611 in the flattened FeNiN particle 61 in Example 3 as well.

[0061] Fig. 27 shows an electron beam diffraction image of the flattened FeNiN particle 61. From Fig. 27, it was confirmed that the spread θ2 of the diffraction spot was about 5°. Thus, the spread of the diffraction spot was smaller in Example 3, which had a shorter major axis length, than in Example 2, which had a longer major axis length.

[0062] These results suggest a correlation between the shorter the major axis length and the smaller the orientation distribution. It is believed that the shorter the major axis length, the narrower the distribution in the c-axis direction, which increases the degree of order and the coercive force.

[0063] 28 shows a manufacturing method of Comparative Example 2. In Comparative Example 2, the processes were performed in the following order: FeNiN synthesis process was performed in step 31, coarse grinding process was performed in step 32, and coating process was performed in step 33. Then, heat treatment was performed in step 34, denitrification process was performed in step 35, and flattening process was performed in step 36. Finally, classification process was performed in step 37. Comparative Example 2 is an example in which the flattening process in step 13 and the subsequent classification in step 14 in the example were performed after denitrification in step 17.

[0064] Figure 29 shows an SEM image of second comparative particle 70, which is an FeNi particle in Comparative Example 2. Figure 30 shows the evaluation results of Comparative Example 2 and Example 2, which were obtained using the same classification conditions. Note that a flattening treatment was performed after the coating treatment. For this reason, it is presumed that part of the coating on second comparative particle 70 has peeled off. For this reason, it is presumed that the image of second comparative particle 70 shown in Figure 29 is less blurred than the image of an FeNi particle that was flattened before the coating treatment.

[0065] As shown in FIG. 29 , the particle shape is also flattened in Comparative Example 2. However, as shown in FIG. 30 , although the particle size and shape are almost similar between Comparative Example 2 and Example 2, differences in the degree of order and coercive force occurred. That is, in Comparative Example 2, in which flattening was performed after denitrification, although the particle shape was flattened, the degree of order and coercive force were lower, and were actually lower than those of Comparative Example 1. Furthermore, analysis of the electron beam diffraction image of the second comparative example particle 70 revealed that, although a diffraction pattern typical of polycrystalline particles was observed, no spots corresponding to {001} or {002}, which would appear if the c-axis 44 were present within the flat surface 33, were observed. Therefore, it was confirmed that the second comparative example particle 70 is polycrystalline and does not have a specific crystal orientation direction (i.e., is non-oriented).

[0066] 31 shows a manufacturing method of Example 4. Example 4 is a process carried out in the following order: FeNiN synthesis is carried out in step 41, coarse pulverization is carried out in step 42, flattening is carried out in step 43, classification is carried out in step 44, and coating is carried out in step 45. Finally, denitrification is carried out in step 46. Example 4 is an example in which the heat treatment in step 16 in Examples 1 to 3 is omitted.

[0067] Figure 32 shows the evaluation results for Example 3 and Example 4, which were classified under the same conditions. As shown in Figure 32, Example 4 also achieved better order and coercive force than the comparative example. However, Example 3, which underwent annealing, showed improved order and coercive force. Thus, it can be confirmed that annealing improves order, which in turn improves coercive force.

[0068] Furthermore, the following can be inferred from a comparison between Comparative Example 2 and Examples 3 and 4. In Comparative Example 2, after an FeNi superlattice is formed by denitrification, the particles are subjected to mechanical force in the flattening treatment. This is presumed to have disrupted the crystal orientation or introduced defects. In contrast, in Examples 3 and 4, denitrification was performed on flattened FeNiN particles 61 whose crystal orientation had been improved by mechanical force in the flattening treatment. This is presumed to have promoted denitrification due to the reduction in grain boundaries accompanying the improved crystal orientation, improving the degree of ordering, and obtaining good c-axis orientation in the axial direction. Furthermore, while flattening improves the crystal orientation in FeNiN, it is presumed that flattening has no effect on the FeNi superlattice. Furthermore, in Example 3, it is presumed that annealing further improved the c-axis orientation and successfully repaired defects.

[0069] Fig. 33 shows a manufacturing method of Example 5. Example 5 was performed in the following order: FeNiN synthesis in step 51, coarse pulverization in step 52, flattening in step 53, classification in step 54, and heat treatment in step 55. Finally, denitrification was performed in step 46. Example 5 is an example in which the coating in step 15 in Examples 1 to 3 was omitted.

[0070] Fig. 34 shows the evaluation results of Example 3 and Example 5, which were classified under the same conditions. Fig. 35 is a TEM image of the magnetic particle 3 according to Example 3. Fig. 36 is a TEM image of the magnetic particle 3 according to Example 5.

[0071] As shown in FIG. 35, in the magnetic body 2 of Example 3 that was coated, SiO 2 constituting the coating layer 37 is present between the adjacent alloy particles 36. 2 On the other hand, as shown in Figure 36, in the magnetic body 2 of Example 5 in which no coating was performed, it was confirmed that contact occurred between adjacent alloy particles 36.

[0072] As shown in Figure 34, Example 5 also achieved a better coercive force than the comparative example. Furthermore, Example 3 also showed improved coercive force. The improvement in coercive force in Example 3 is presumed to be due to the fact that coating the particles before annealing or denitrification suppressed contact and sintering between particles during annealing or denitrification, thereby maintaining particle isolation. Furthermore, the coating layer 37 is presumed to have a magnetic isolation effect between adjacent particles, thereby achieving high coercive force.

[0073] As described above, according to this embodiment or example, the magnetic particle 3 alone has a flat shape having a major axis 31 and a minor axis 32, and the axis of easy magnetization 35 is aligned with the flat surface 33 along which the major axis 31 is aligned. Such a structure in which the axis of easy magnetization 35 faces the inside of the flat surface 33 makes it less susceptible to the influence of demagnetizing fields, and it becomes possible to increase the coercive force.

[0074] The direction of the magnetocrystalline anisotropy and the direction of the shape magnetic anisotropy can be made parallel, resulting in a high squareness ratio, and therefore superior magnetic properties to those of spherical particles.

[0075] By providing a structure in which the magnetic particles 3 are coated with the coating layer 37, the magnetic coupling between the particles can be broken, thereby making it possible to increase the coercive force.

[0076] Flat particles have a smaller surface area per unit volume than acicular particles, which means that the amount of coating required is also smaller. For this reason, flat particles are more advantageous than acicular particles for achieving a higher space factor of the magnetic material during filling, making it possible to achieve a higher density during molding. This results in a higher magnetic flux density and coercive force for magnet 1.

[0077] The magnetic particles 3 have the above-described properties when they are free-standing and not supported by a support such as a substrate, which makes it easy to mold the magnet 1 using these magnetic particles 3.

[0078] According to this embodiment or example, the coercive force is higher than that of the conventional L1 0 It is possible to provide magnetic particles 3 having a regular structure, magnetic substance 2, magnet 1, and a method for manufacturing magnetic substance 2.

[0079] (Modifications) The present disclosure is not limited to the above-described embodiment. Therefore, the above-described embodiment can be modified as appropriate. Representative modifications will be described below. In the following description of the modifications, differences from the above-described embodiment will be mainly described. Furthermore, the same reference numerals are used for parts that are identical or equivalent to each other in the above-described embodiment and the modifications. Therefore, in the following description of the modifications, the description of the above-described embodiment can be used as appropriate for components that have the same reference numerals as the above-described embodiment, unless there is a technical contradiction or special additional explanation.

[0080] The use and shape of the magnet 1 are not particularly limited. Furthermore, the use of the magnetic substance 2 is not limited to the manufacture of the magnet 1, but can also be applied to magnetic recording media, etc. Furthermore, as described above, the claims of rights based on this disclosure can be made to individual magnetic substance particles 3, powders that are aggregates of such particles, and bulk compacts of such powders. Furthermore, the alloy particles 36 that constitute the magnetic substance particles 3 may contain components other than Fe and Ni. Furthermore, the flattening method is not limited to the ball mill or bead mill used in the examples, as long as the particles can be flattened satisfactorily. Furthermore, the expression "degree of order measured by powder X-ray diffraction" does not necessarily mean that the degree of order is measured directly by powder X-ray diffraction, but includes degrees of order calculated using various patterns, waveforms, values, etc. measured by powder X-ray diffraction. Therefore, "degree of order measured by powder X-ray diffraction" can also be rephrased as "degree of order determined by measurement by powder X-ray diffraction."

[0081] It goes without saying that the elements constituting the above-described embodiments are not necessarily essential unless expressly stated as essential or clearly considered essential in principle. Furthermore, when numerical values ​​such as the number, amount, range, etc. of components are mentioned, the present disclosure is not limited to those specific numerical values ​​unless expressly stated as essential or clearly limited to specific numerical values ​​in principle. Similarly, when the shape, direction, positional relationship, etc. of components are mentioned, the present disclosure is not limited to those shapes, directions, positional relationships, etc. unless expressly stated as essential or clearly limited to specific shapes, directions, positional relationships, etc. in principle.

[0082] (Aspects) As is clear from the above-described description of the embodiments and modifications, the disclosure of this specification includes at least the following aspects. [Aspect 1] A magnetic body (2) having magnetic particles (3) containing an FeNi ordered alloy with an L10-type ordered structure, wherein the magnetic particles each have a flat shape in which a major axis (31) intersects with a minor axis (32) shorter than the major axis, and a flat surface (33) along the major axis is wider than a side surface (34) along the minor axis, and the magnetic easy axis (35) of the L10-type ordered structure is aligned with the flat surface. [Aspect 2] The magnetic body according to Aspect 1, wherein the length of the major axis is 1,000 nanometers or less. [Aspect 3] The magnetic body according to Aspect 1 or 2, wherein the length of the minor axis is 100 nanometers or less. [Aspect 4] The magnetic body according to any one of Aspects 1 to 3, wherein the degree of order measured by powder X-ray diffraction is 0.76 or more. [Aspect 5] The magnetic body according to any one of Aspects 1 to 4, wherein the magnetic particles comprise alloy particles (36) containing the FeNi ordered alloy having an L10-type ordered structure, and a coating layer (37) covering the surfaces of the alloy particles. [Aspect 6] A magnet (1) comprising the magnetic body according to any one of Aspects 1 to 5. [Aspect 7] A method for producing a magnetic body (2) having magnetic particles (3) containing an FeNi ordered alloy having an L10-type ordered structure, the method comprising: flattening FeNiN particles; and subjecting the flattened FeNiN particles to a denitrification treatment. [Aspect 8] The method for producing a magnetic body according to Aspect 7, the method comprising annealing the flattened FeNiN particles and then subjecting them to the denitrification treatment.

Claims

1. L1 0 A magnetic material (2) having magnetic particles (3) containing an FeNi ordered alloy of a type ordered structure, wherein the magnetic particles each have a flat shape in which a major axis (31) intersects with a minor axis (32) that is shorter than the major axis, and a flat surface (33) along the major axis is wider than a side surface (34) along the minor axis, and the L1 0 A magnetic body in which the axis of easy magnetization (35) of the ordered structure is aligned along the flat plane.

2. The magnetic body according to claim 1, wherein the length of said major axis is 1000 nanometers or less.

3. The magnetic body according to claim 2, wherein the length of the minor axis is 100 nanometers or less.

4. The magnetic material according to claim 1, which has a degree of order of 0.76 or more as measured by powder X-ray diffraction method.

5. The magnetic particles are 0 2. The magnetic body according to claim 1, comprising alloy particles (36) containing an FeNi ordered alloy having a type ordered structure, and a coating layer (37) covering the surfaces of the alloy particles.

6. A magnet (1) comprising the magnetic body according to any one of claims 1 to 5.

7. L1 0 A method for producing a magnetic material (2) having magnetic particles (3) containing an FeNi ordered alloy having a type ordered structure, the method comprising: flattening FeNiN particles; and performing a denitrification treatment on the flattened FeNiN particles.

8. The method for producing a magnetic material according to claim 7, wherein the denitrification treatment is carried out after the flattened FeNiN particles are annealed.

Citation Information

Patent Citations

  • Iron nitride magnetic powder and bond magnet including same

    JP2016146388A

  • FeNi REGULAR ALLOY, MANUFACTURING METHOD OF FeNi REGULAR ALLOY AND MAGNETIC MATERIAL CONTAINING FeNi REGULAR ALLOY

    JP2017075388A

  • Rare earth-free permanent magnetic materials based on fe-ni

    JP2017535062A

  • Method for manufacturing rare earth iron-based permanent magnet

    JP2018056525A

  • MAGNETIC MATERIAL CONTAINING A FeNi REGULAR ALLOY AND METHOD FOR PRODUCING SAME

    JP2018193571A

Cited By

  • Magnetic body and magnet

    WO2026088551A1

  • Method for producing granulated substance, method for producing magnetic body, granulated substance, and magnetic body

    WO2026088552A1