Method for removing impurities from crude metal hydroxide leaching slurry, method for removing impurities from crude metal hydroxide, and method for preparing sulfate

Through the removal method of crude metal hydroxide leaching slurry and the collaborative leaching technology of nickel sulfonium raw materials, the problems of high electrolytic nickel price, large MHP leaching process and high requirements of high ice nickel equipment are solved, and the cost reduction and efficiency improvement are achieved effect.

WO2024235328A1PCT designated stage expired Publication Date: 2024-11-21CNGR ADVANCED MATERIAL CO LTD +2

Patent Information

Application Number
PCT/CN2024/094049
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-07-31
Filing Date
2024-05-17
Publication Date
2024-11-21

AI Technical Summary

Technical Problem

In the existing process of preparing battery-grade nickel sulfate, electrolytic nickel has high price, high cost of reducing agent during MHP leaching process, and the introduction of sodium leads to an increase in crystallization cost. High ice nickel equipment has high requirements and large initial capital investment, and there are many calcium impurities introduced, which has economic benefits. Poor problem.

Method used

Using the impurity removal method of crude metal hydroxide leaching slurry, through acid leaching and synergistic leaching technology, nickel-containing raw materials and oxidizing agents are used to remove impurities, reduce the introduction of calcium impurities, reduce the cost of auxiliary materials, and use nickel sulfonium raw materials under acidic conditions. As a reducing agent and oxidant, synergistic leaching of nickel elements is achieved to avoid additional reducing agent and oxidant.

Benefits of technology

It reduces production costs, improves economic benefits, reduces the introduction of impurities and ions in the system, reduces the evaporation cost, increases the production capacity of the nickel sulfonium raw material leaching system, has a gentler and safer reaction, and simplifies the process flow.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN2024094049_21112024_PF_FP_ABST
    Figure CN2024094049_21112024_PF_FP_ABST
Patent Text Reader

Abstract

The present disclosure provides a method for removing impurities from a crude metal hydroxide leaching slurry and a method for preparing a sulfate, and relates to the technical field of hydrometallurgy. A crude metal hydroxide is subjected to acid leaching. Method I involves: converting ferrous iron in the leaching slurry into ferric iron by adding an oxidizing agent, and reacting a nickel-containing raw material with an acid in the slurry to consume the acid in the slurry and adjust the pH value of the slurry, such that at least one of impurities including manganese, iron, aluminum, calcium, magnesium, copper, chromium and zinc is precipitated, and an impurity-removed liquid containing at least one of nickel and cobalt is obtained, thereby reducing the introduction of calcium impurities, lowering the production cost, and improving the economic benefits. Method II involves: adding a nickel-containing raw material during acid leaching without the need to additionally add a reducing agent or an oxidizing agent, thereby significantly lowering the auxiliary material cost during the MHP leaching process, reducing the introduction of impurity ions in the system, and decreasing the evaporation cost.
Need to check novelty before this filing date? Find Prior Art

Description

Method for removing impurities from crude metal hydroxide leaching slurry, method for removing impurities from crude metal hydroxide, and method for preparing sulfate

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] The present disclosure claims priority to Chinese patent application No. 202310560609.3 filed on May 18, 2023, entitled “A method for leaching nickel elements and a method for preparing nickel sulfate” and Chinese patent application No. 202310952540.9 filed on July 31, 2023, entitled “A method for removing impurities from crude metal hydroxide leaching slurry and a method for preparing sulfate”, and the entire contents of the above two applications are incorporated into the text by reference. Technical Field

[0003] The present disclosure relates to the technical field of hydrometallurgy, and in particular to a method for removing impurities from a crude metal hydroxide leaching slurry, a method for removing impurities from a crude metal hydroxide, and a method for preparing sulfate. Background Art

[0004] At present, the mainstream raw materials for preparing battery-grade nickel sulfate are electrolytic nickel, nickel cobalt hydroxide raw materials (abbreviated as: MHP) and high-grade nickel matte. Among them, the mainstream process for preparing battery-grade nickel sulfate from electrolytic nickel is the leaching-deironing process. This method has a short process flow and low equipment investment. It has been the main method for preparing battery-grade nickel sulfate in the past. However, with the rapid development of new energy, the price of electrolytic nickel has risen sharply, resulting in the problem of high cost of this process. The mainstream process for preparing battery-grade nickel sulfate from MHP is the leaching-deironing-extraction and impurity removal process. This method has stable raw materials and short reaction time. It is currently an important method for preparing battery-grade nickel sulfate. However, this method consumes a large amount of reducing agent during the leaching process, and there is a risk of introducing sodium into the system, resulting in increased crystallization costs. The mainstream process for preparing battery-grade nickel sulfate from high-grade nickel matte is the atmospheric pressure oxygen leaching-pressure leaching-extraction and impurity removal process. This method has a high nickel content in the raw materials, low transportation cost per ton of nickel and low slag volume. It is also an important method for preparing battery-grade nickel sulfate. However, this method has high equipment requirements and large initial capital investment.

[0005] Benefiting from the rapid development of the new energy vehicle sector, the consumption of nickel cobalt manganese sulfate, an important battery raw material, continues to grow every year. In the existing process for preparing nickel cobalt manganese sulfate, crude metal hydroxide is often used as a starting material. Among them, crude metal hydroxides can be selected from MHP (short for nickel cobalt hydroxide), cobalt intermediates, nickel cobalt manganese waste slag produced by battery recycling smelting, etc. MHP can be derived from laterite nickel ore as raw material, and then a low-concentration nickel cobalt solution is obtained through high-pressure acid leaching technology, and then crude nickel cobalt hydroxide is obtained by precipitation with hydroxide.

[0006] In the prior art, calcium carbonate is added after MHP acid leaching to consume residual acid and to aid filtration of the subsequent leaching slurry. Hydrogen peroxide is added to oxidize ferrous ions to generate Fe(OH)3 precipitates for joint iron removal. However, this method has the disadvantages of introducing a large amount of calcium impurities, poor economic benefits, and a relatively complex process.

[0007] Summary of the Invention

[0008] The purpose of the present disclosure is to provide a method for removing impurities from a crude metal hydroxide leaching slurry, a method for removing impurities from a crude metal hydroxide, and a method for preparing sulfate, so as to solve at least one of the above problems.

[0009] To achieve the above objectives, the present disclosure adopts the following technical solution: a method for removing impurities from a crude metal hydroxide leaching slurry, comprising:

[0010] Leaching process: A crude metal hydroxide is used as a starting material for acid leaching to obtain a leaching slurry. The crude metal hydroxide includes at least one of crude nickel hydroxide and crude cobalt hydroxide. The slurry also includes impurities, and the impurities include at least one of manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc.

[0011] The impurity removal method can be specifically divided into method one and method two:

[0012] Method 1: A method for removing impurities from a crude metal hydroxide leaching slurry, comprising:

[0013] Leaching step: using crude metal hydroxide as a starting material to acid-leach to obtain a leaching slurry, wherein the crude metal hydroxide includes at least one of crude nickel hydroxide and crude cobalt hydroxide, and the slurry also includes impurities, and the impurities include at least one of manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc;

[0014] Impurity removal process: nickel-containing raw materials and oxidants are added to the leaching slurry to remove impurities. The nickel-containing raw materials can be used as a neutralizer in the leaching process to obtain impurity-removed liquid and impurity-removed slag.

[0015] The divalent iron in the leaching slurry can be converted into trivalent iron by adding an oxidizing agent, and the nickel-containing raw material is used to react with the acid in the slurry to consume the acid in the slurry, adjust the slurry pH, and precipitate at least one of the impurities including manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc, and obtain a de-impurity liquid containing at least one of nickel and cobalt, thereby reducing the introduction of calcium impurities, reducing production costs, and improving economic benefits.

[0016] Method 2: A method for leaching nickel elements, comprising: primary leaching: co-leaching a nickel cobalt hydroxide raw material and a nickel matte raw material under acidic conditions to obtain a leached solution; the nickel cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; the nickel matte raw material contains nickel element.

[0017] That is to say, the nickel-containing raw material (such as nickel matte raw material) can be added during acid leaching, or introduced in a separate impurity removal process after acid leaching.

[0018] The method for leaching nickel provided herein uses nickel cobalt hydroxide and nickel matte as leaching raw materials. When leaching the nickel cobalt hydroxide raw material, the elemental nickel in the nickel matte raw material serves as a reducing agent, while when leaching the nickel cobalt hydroxide raw material, the manganese in the nickel cobalt hydroxide raw material serves as an oxidizing agent. This eliminates the need for additional reducing or oxidizing agents, significantly reducing the cost of auxiliary materials in the MHP leaching process. Compared with other processes, this method reduces the introduction of impurity ions (such as sodium ions) into the system, lowering evaporation costs. Furthermore, it reduces oxygen consumption and equipment investment costs during the nickel matte leaching process, shortens the leaching process, and significantly increases the production capacity of the nickel matte leaching system. The reaction process does not require the introduction of oxygen, nor does it produce hydrogen, making the reaction milder and safer.

[0019] About Method 1:

[0020] In an optional embodiment, the crude metal hydroxide comprises at least one of Co2O3, Co(OH)3, and MnO2;

[0021] Optionally, the crude metal hydroxide is selected from one of nickel cobalt hydroxide and crude cobalt hydroxide;

[0022] Optionally, the crude metal hydroxide is selected from nickel cobalt hydroxide;

[0023] Optionally, the crude metal hydroxide has a dry basis content of Ni element of 35-60%, a dry basis content of Co element of less than 5%, and a dry basis content of Mn element of less than 10%.

[0024] In an optional embodiment, the temperature of the acid leaching is 40-100°C;

[0025] Optionally, the stirring speed of the acid leaching is 200-800 rpm;

[0026] Optionally, the reaction time of acid leaching is 1-4 hours.

[0027] In an optional embodiment, the method further includes a step of removing impurities: adding a nickel-containing raw material and an oxidant to the leaching slurry to remove impurities, thereby obtaining a liquid after impurities removal and a residue after impurities removal;

[0028] During the impurity removal process, the pH of the leaching slurry is adjusted to 3.5 or above.

[0029] In an optional embodiment, the nickel-containing raw material includes at least one of Ni element, Ni3S2, Ni2O3, and Ni(OH)3;

[0030] Optionally, the nickel-containing raw material includes nickel matte;

[0031] Optionally, the nickel-containing raw material is selected from high-matte nickel;

[0032] Optionally, when the nickel-containing raw material is selected from high-matte nickel, the nickel content of the high-matte nickel on a dry basis is greater than or equal to 50%;

[0033] Optionally, the nickel-containing raw material has a dry basis content of Ni element of 65-75%, a dry basis content of Co element of less than 2%, and a dry basis content of Mn element of less than 1%.

[0034] In an optional embodiment, the nickel-containing raw material and the oxidant are added to the leaching slurry to remove impurities, such that: the amount of the nickel-containing raw material added is 1 / 100-1 / 10 of the natural basis weight of the crude metal hydroxide;

[0035] Optionally, the amount of nickel-containing raw material added is 1 / 70-1 / 50 of the natural basis weight of the crude metal hydroxide;

[0036] Optionally, the reaction temperature is 40-100°C; Optionally, the reaction temperature is 60-70°C;

[0037] Optionally, the oxidant is selected from any one of oxygen, hydrogen peroxide, and ozone;

[0038] Optionally, when the oxidant is oxygen, the oxygen introduction rate is 2-3 L / min;

[0039] Optionally, the impurity removal time is 1-10 hours.

[0040] About Method 2:

[0041] In an optional embodiment, the crude metal hydroxide is a nickel-cobalt hydroxide raw material, and the nickel-cobalt hydroxide raw material and the nickel matte raw material are co-leached under acidic conditions; the nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; and the nickel matte raw material contains elemental nickel.

[0042] In an optional embodiment, the dry basis content of manganese dioxide in the nickel cobalt hydroxide raw material is 1% to 10%; and / or the dry basis content of elemental nickel in the nickel matte raw material is 5% to 25%;

[0043] Optionally, the nickel matte raw material is high-grade nickel matte.

[0044] In an optional embodiment, the mass ratio of the nickel cobalt hydroxide raw material to the nickel matte raw material is 1:(0.01-0.09);

[0045] Optionally, water is added during the co-leaching, and the solid-liquid ratio of the nickel cobalt hydroxide raw material to water is 1 g: (1.5-3) mL;

[0046] Optionally, the acidic conditions for the coordinated leaching are: pH controlled at 1.0 to 2.0;

[0047] Optionally, the co-leaching temperature is 85-100° C. and the time is 2-6 hours.

[0048] In an optional embodiment, solid-liquid separation is performed after the co-leaching to obtain a post-leaching liquid and a leaching residue;

[0049] Method 2 also includes:

[0050] Pressure leaching: The leaching residue is adjusted to pH with acid solution and then leached under pressure to obtain a pressure leachate.

[0051] In an optional embodiment, the pH of the leached residue is adjusted to 1.5-2.0 with an acid solution and then pressure leached.

[0052] In an optional embodiment, the pressure leaching temperature is 160-180° C., the oxygen partial pressure is 0.6-1.0 MPa, and the time is 4-7 hours.

[0053] The present disclosure also provides a method for preparing sulfate, comprising the above-mentioned impurity removal method; extracting and separating the liquid after impurity removal to obtain a sulfate solution; and pressurizing oxygen leaching the slag after impurity removal to obtain a sulfate solution and hematite slag.

[0054] In an optional embodiment, the initial acidity pH of the pressurized oxygen immersion is 1.0-1.2, the temperature of the pressurized oxygen immersion is 160-200° C., the oxygen partial pressure is 0.3-0.8 MPa, and the reaction time is 2-10 h.

[0055] The present disclosure also provides a method for preparing nickel sulfate, comprising the above-mentioned impurity removal method.

[0056] In an optional embodiment, the method further comprises: performing solid-liquid separation after the co-leaching to obtain a post-leaching liquid and a leaching residue;

[0057] Iron removal: Add hydrogen peroxide to the leached liquid and stir to remove iron. The solid-liquid separation will obtain the iron-removed liquid and iron-removed slag.

[0058] In an optional embodiment, the molar ratio of the ferrous iron content in the leached solution to the hydrogen peroxide content in the added hydrogen peroxide is controlled to be 1:(1.5-3.0);

[0059] Optionally, after the stirring is completed, the pH is adjusted to 3.5-4.5, and then the solid-liquid separation is performed to obtain the iron-removed liquid and the iron-removed slag. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] To more clearly illustrate the technical solutions of the embodiments of the present disclosure, the following briefly introduces the drawings required for use in the embodiments of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and those skilled in the art can derive other drawings based on the drawings without inventive effort.

[0061] FIG1 is a schematic process flow diagram of a method for removing impurities from a crude metal hydroxide leaching slurry according to some embodiments of the present disclosure;

[0062] FIG2 is a scanning electron microscope morphology result of the slag after impurity removal in Example 7;

[0063] FIG3 is a scanning electron microscope morphology result diagram of the slag after impurity removal in Comparative Example 9. DETAILED DESCRIPTION

[0064] As used in this disclosure, the terms "comprising," "including," "having," "containing," or any other variations thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises a listed element is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.

[0065] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values ​​and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed alone. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including the range of "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in the present disclosure, unless otherwise stated, the range is intended to include its endpoints and all integers and fractions within the range.

[0066] In the present disclosure, “and / or” is used to indicate that one or both of the described situations may occur, for example, A and / or B includes (A and B) and (A or B).

[0067] In this disclosure, "nickel cobalt hydroxide" is sometimes referred to as nickel cobalt hydroxide or MHP, which have the same meaning. In this disclosure, unless otherwise specified, the percentages are by mass.

[0068] Throughout this disclosure, "natural basis" refers to the material in its natural state (containing water), and "dry basis" refers to the material after water has been removed. For example, if the water content of the MHP raw material is 50.09%, this refers to the water content on a natural basis. After drying the MHP raw material, the Ni content on a dry basis is 54.67%. Unless otherwise specified, all element or component contents in this disclosure refer to the dry basis, i.e., the content of the element or component after water has been removed.

[0069] In some embodiments of the present disclosure, referring to FIG1 , a method for removing impurities from a crude metal hydroxide leaching slurry, also referred to as a crude metal hydroxide impurity removal method, i.e., method 1, specifically comprises the following steps:

[0070] Leaching process: using crude metal hydroxide as a starting material to acid-leach to obtain a leaching slurry, wherein the crude metal hydroxide includes at least one of crude nickel hydroxide and crude cobalt hydroxide, and the slurry further includes impurities, wherein the impurities include at least one of manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc;

[0071] Impurity removal process: adding nickel-containing raw materials and oxidants to the leaching slurry to remove impurities. The nickel-containing raw materials can be used as a neutralizer in the leaching process to obtain impurity-removed liquid and impurity-removed slag.

[0072] In this embodiment, an oxidant is added to convert the divalent iron in the leaching slurry into trivalent iron, and a nickel-containing raw material is used to react with the acid in the slurry, thereby consuming the acid in the slurry and adjusting the pH of the slurry to precipitate at least one of the impurities including manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc, and obtain a decontaminated liquid containing at least one of nickel and cobalt, thereby reducing the introduction of calcium impurities, reducing production costs, and improving economic benefits.

[0073] In some optional embodiments, the crude metal hydroxide includes at least one of Co2O3, Co(OH)3, and MnO2.

[0074] Furthermore, the crude metal hydroxide is selected from one of nickel cobalt hydroxide and crude cobalt hydroxide;

[0075] Among them, nickel cobalt hydroxide, abbreviated as MHP in English, is a nickel smelting intermediate and belongs to the nickel hydrometallurgy intermediate. Its source can be the pressure leaching of laterite nickel ore and the nickel precipitation process of magnesium oxide. The main elements of the prepared nickel cobalt hydroxide include nickel, cobalt, manganese and magnesium. Among them, nickel, cobalt and manganese mainly exist in the form of hydroxides and oxides. Some laterite nickel ores may contain copper.

[0076] Among them, crude cobalt hydroxide is a cobalt smelting intermediate that can be produced through a wet process. Its production process can be direct leaching of copper-cobalt oxide ore, extraction to remove copper, and precipitation of cobalt with magnesium oxide. The main elements include cobalt, manganese, copper, magnesium, etc. Among them, cobalt mainly exists in the form of cobalt hydroxide, cobalt oxyhydroxide and cobalt trioxide, and manganese mainly exists in the form of manganese hydroxide and manganese dioxide.

[0077] In particular, nickel cobalt hydroxide and crude cobalt hydroxide can also come from the wet treatment process of battery recycle, for example, they can come from the slag obtained by leaching and adding alkali to the battery recycle.

[0078] Furthermore, the crude metal hydroxide is selected from nickel cobalt hydroxide.

[0079] In some optional embodiments, the crude metal hydroxide has a dry basis content of Ni element of 35-60%, a dry basis content of Co element of less than 5%, and a dry basis content of Mn element of less than 10%.

[0080] In some optional embodiments, the acid leaching satisfies at least one of the following conditions E to G:

[0081] E. The temperature of the pickling is 40-100°C, for example, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C or 100°C;

[0082] F. The stirring speed of the acid leaching is 200-800 rpm, for example, 200 rpm, 250 rpm, 300 rpm, 350 rpm, 400 rpm, 450 rpm, 500 rpm, 550 rpm, 600 rpm, 650 rpm, 700 rpm, 750 rpm or 800 rpm;

[0083] G. The reaction time of acid leaching is 1-4 hours, for example, it can be 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours.

[0084] It is understood that, before acid leaching the crude metal hydroxide, the process may further include: adding the crude metal hydroxide to water to form a slurry, and then adding an acid solution to the prepared slurry for acid leaching. The acid solution may be sulfuric acid, and the slurry concentration may be 10%-80%, for example, 10%, 20%, 30%, 40%, 50%, 60%, 70%, or 80%. The slurry concentration is the ratio of the solid mass to the total mass of the slurry.

[0085] In some optional embodiments, the nickel-containing raw material includes at least one of elemental Ni, Ni3S2, Ni2O3, and Ni(OH)3, thereby reacting with the acid and / or oxygen in the solution to adjust the pH of the solution;

[0086] In some optional embodiments, the pH of the leaching slurry is adjusted to 3.5 or above during the impurity removal process, so as to completely precipitate the iron.

[0087] In some optional embodiments, the oxidant is selected from any one of oxygen, hydrogen peroxide, and ozone, and other oxidants are prone to introduce impurities.

[0088] In some optional embodiments, the oxidant is oxygen, and the oxygen introduction rate is 2-3 L / min;

[0089] In this embodiment, the reaction in which Fe participates includes: FeSO4+O2+H2O→FeOOH↓+H2SO4. By controlling the oxygen introduction rate, the iron can be precipitated and removed in the form of crystalline goethite, which is loosely arranged, facilitating faster filtration.

[0090] In some optional embodiments, the nickel-containing raw material includes nickel matte, which is also called nickel matte. It is a mixture of metals such as nickel, cobalt, iron, and their sulfides, and is an intermediate product of nickel pyrometallurgy. More specifically, the nickel matte includes at least one of elemental nickel and Ni3S2, and also includes iron as an impurity.

[0091] In this embodiment, the reactions in which nickel matte participates may include: Ni+H2SO4+O2→NiSO4+H2O; Ni3S2+H2SO4+O2→NiS+NiSO4+H2O; MnO2+Ni3S2+H2SO4+O2→MnSO4+NiSO4+NiS+H2O;

[0092] The Ni and Ni3S2 in the nickel matte can consume the acid in the slurry, thereby adjusting the pH and precipitating impurity metal elements. In addition, Ni3S2 can be converted into NiSO4 and NiS by utilizing the disproportionation reaction of Ni3S2 in the presence of oxygen and acid and the reaction of Ni3S2 with high-valent manganese in crude metal hydroxide.

[0093] In some optional embodiments, the nickel-containing raw material is selected from high-grade nickel matte, which is nickel matte with a high nickel content and a low impurity content. The components in the high-grade nickel matte and their reaction products in the impurity removal process are separate fine particles, which are conducive to rapid filtration.

[0094] In this embodiment, the general processing flow for high-grade nickel matte is atmospheric pressure acid leaching to dissolve elemental nickel → atmospheric pressure acid leaching with oxygen to convert nickel disulfide into nickel sulfide → oxygen pressure acid leaching of nickel sulfide → nickel sulfate. In this embodiment, Ni3S2 is converted into NiSO4 and NiS during the impurity removal process, completing the pretreatment for high-grade nickel matte oxygen pressure leaching. This achieves the coordinated treatment of MHP and high-grade nickel matte, reduces acid consumption, lowers auxiliary material costs, and improves production efficiency.

[0095] Furthermore, the nickel content in the dry basis of high nickel matte is greater than or equal to 50%, for example 50%-80%, preferably 55%-80%, more preferably 60%-80%, more preferably 65-75%, and can also be 65%-70%, 70%-75%, etc.

[0096] Furthermore, the nickel-containing raw material has a dry basis content of Ni element of 65-75%, a dry basis content of Co element of less than 2%, and a dry basis content of Mn element of less than 1%.

[0097] In some optional embodiments, the amount of nickel-containing raw material added is 1 / 100-1 / 10 of the natural basis weight of the crude metal hydroxide, for example, it can be 1 / 100, 1 / 90, 1 / 80, 1 / 70, 1 / 60, 1 / 50, 1 / 40, 1 / 30, 1 / 20 or 1 / 10.

[0098] In some optional embodiments, the amount of nickel-containing raw material added is 1 / 70-1 / 50 of the natural basis weight of the crude metal hydroxide.

[0099] In some optional embodiments, the reaction temperature of the impurity removal process is 40-100°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C or 100°C; preferably, the reaction temperature is 60-70°C.

[0100] In some optional embodiments, the impurity removal time is 1-10 hours, for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.

[0101] In other embodiments of the present disclosure, a method for preparing sulfate is also provided, comprising the above-mentioned method for removing impurities from the crude metal hydroxide leaching slurry; extracting and separating the liquid after impurities removal to obtain a sulfate solution; and subjecting the slag after impurities removal to pressurized oxygen leaching to obtain a sulfate solution and hematite slag.

[0102] In some embodiments of the present disclosure, the initial acidity pH of the pressurized oxygen immersion is 1.0-1.2, the temperature of the pressurized oxygen immersion is 160-200°C, for example, it can be 160°C, 170°C, 180°C, 190°C or 200°C, the oxygen partial pressure is 0.3-0.8 MPa, for example, it can be 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa or 0.8 MPa, and the reaction time is 2-10 h, for example, it can be 2 h, 3 h, 4 h, 5 h, 6 h, 7 h, 8 h, 9 h or 10 h.

[0103] The small amount of high-valent cobalt and manganese (such as MnO2 and Co(OH)3) remaining in the slag after impurity removal reacts with NiS in the slag under pressure, eliminating the intermediate reduction leaching process required in the general process. The reactions that occur in this step may include:

[0104]

[0105]

[0106] The high-valent cobalt and manganese (such as MnO2 and Co(OH)3) remaining in the slag after impurity removal usually requires the addition of reducing agents such as sodium metabisulfite, sodium sulfite, and hydrogen peroxide for reduction leaching. The disclosed solution directly subjects the slag after impurity removal to oxygen pressure acid leaching to complete the recovery of high-valent cobalt and manganese, and can recover most of the high-valent metals in the metal powder.

[0107] Nickel cobalt hydroxide (MHP) is a nickel smelting intermediate, often referred to by those skilled in the art as nickel cobalt hydroxide. It is produced through a hydrometallurgical nickel smelting process using pressure leaching of laterite nickel ore followed by nickel precipitation with magnesium oxide. The resulting nickel intermediate primarily contains nickel, cobalt, manganese, and magnesium, with nickel, cobalt, and manganese primarily existing as hydroxides and oxides. Some laterite nickel ores may contain copper.

[0108] Nickel matte, also known as nickel matte, is a mixture of nickel, cobalt, iron and other metals and their sulfides. It is an intermediate product of nickel pyrometallurgy. Nickel matte with a higher nickel content is usually called high nickel matte. The nickel content (dry basis) of high nickel matte is usually above 50%, such as 50%-80%, preferably 55%-80%, more preferably 60%-80%, and can also be 65%-70%, 70%-75%, 65%-75%, etc.

[0109] In certain embodiments, the high nickel matte production process is to obtain low nickel matte with high iron and sulfur content by pyrometallurgical smelting of laterite nickel ore raw materials, and the low nickel matte is blown in a converter to obtain high nickel matte with high nickel content and low iron and sulfur content.

[0110] In existing nickel leaching systems using nickel cobalt hydroxide as raw material, the addition of a reducing agent is required, increasing the cost of auxiliary materials and introducing other impurity ions, increasing the cost of subsequent impurity removal. Existing high-grade nickel matte leaching systems typically use an oxygen pressure leaching process, which requires the introduction of large amounts of oxygen as an oxidant and produces hydrogen during the leaching process.

[0111] In this disclosure, "nickel cobalt hydroxide raw material" is sometimes referred to as nickel cobalt hydroxide or MHP, which have the same meaning. In the present invention, unless otherwise specified, the percentage content is by mass percentage.

[0112] Throughout this disclosure, "natural basis" refers to the natural state of a material (containing water), while "dry basis" refers to the state of the material after water has been removed. For example, in Material A in Table 1, the water content is 46.51%, which refers to the water content on a natural basis. After drying Material A, the dry basis yields a Ni content of 38.57%. Unless otherwise specified, the content of an element or component herein refers to the dry basis, i.e., the content of the element or component after water has been removed.

[0113] The present disclosure also provides a method for leaching nickel, also known as a method for removing impurities from crude metal hydroxides, namely, Method 2, which comprises: a primary leaching process: co-leaching a nickel-cobalt hydroxide raw material and a nickel matte raw material under acidic conditions to obtain a leached solution; the nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide, and manganese dioxide; and the nickel matte raw material contains elemental nickel. Co-leaching of the crude metal hydroxide and the nickel-containing raw material can also be achieved by adding a nickel-containing raw material during the acid leaching process.

[0114] Certain embodiments of the present disclosure use nickel cobalt hydroxide raw materials and nickel matte raw materials as leaching raw materials, so that when the nickel cobalt hydroxide raw material is leached, the elemental nickel in the nickel matte raw material can be used as a reducing agent, and when the nickel matte raw material is leached, the tetravalent manganese in the nickel cobalt hydroxide raw material can be used as an oxidant, thereby eliminating the need to add additional reducing agents or oxidizing agents as auxiliary materials, and directly co-leaching nickel.

[0115] It should be noted that in some embodiments of the present disclosure, the "leaching process" can be understood as a "primary leaching process," i.e., a single leaching process comprising co-leaching a nickel-cobalt hydroxide raw material and a nickel matte raw material under acidic conditions to obtain a leached solution; the nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide, and manganese dioxide; and the nickel matte raw material contains elemental nickel. In certain embodiments of the present disclosure, the description of "primary leaching" can be understood as a description of the "leaching process."

[0116] Preferably, the dry basis content of Mn in the nickel cobalt hydroxide raw material is 1% to 10%, preferably 1.5% to 8%; for example, it can be 1.5% to 4%, or 4% to 6%, or 5% to 10%. Preferably, the dry basis content of Mn in the nickel cobalt hydroxide is 5% to 10%. The dry basis content of elemental nickel in the nickel matte raw material is 5% to 25%, for example, it can be 5% to 10%, or 10% to 15%, or 15% to 20%, or 20% to 25%, or 15% to 25%. Preferably, the dry basis content of elemental nickel in the nickel matte raw material is 15% to 25%. Preferably, the nickel matte raw material is high-grade nickel matte.

[0117] In certain embodiments, the dry basis content of Co in nickel cobalt hydroxide is 2% to 3%, for example, 2% to 2.4%, or 2.4% to 2.6%, or 2.6% to 3%; the dry basis content of Ni in nickel cobalt oxyhydroxide is 30% to 40%, for example, 30% to 35%, or 35% to 37%, or 37% to 40%.

[0118] In some embodiments, the dry basis content of iron in the nickel matte raw material is 2% to 5%, for example, 2% to 3%, or 3% to 4%, or 4% to 5%; the dry basis content of Co in the nickel matte raw material is 0.5% to 2%, for example, 0.5% to 0.7%, or 0.7% to 0.8%, or 0.8% to 1%, or 1% to 1.5%, or 1.5% to 2%.

[0119] Preferably, the mass ratio of the nickel cobalt hydroxide raw material to the nickel matte raw material is 1:(0.01-0.09); for example, it can be 1:(0.015, 0.02, 0.025, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08 or 0.09), preferably 1:0.015-0.05, and more preferably 1:0.015-0.03.

[0120] Preferably, a certain amount of water needs to be added during the primary leaching. The amount of water added during the primary leaching is appropriate to ensure that the leached nickel element (such as nickel sulfate) is not precipitated. The solid-liquid ratio of the nickel cobalt hydroxide and water is 1g: (1.5-3)mL, for example, 1g: 1.5mL, or 1g: 2mL, or 1g: 3mL.

[0121] Those skilled in the art may conceive of first diluting a mixture of water and sulfuric acid before leaching, or directly using the diluted acid solution.

[0122] The disclosed solution only requires mixing and leaching MHP and nickel matte raw materials, without other complicated operations, and is highly feasible.

[0123] Preferably, the temperature of the primary leaching is 85-100°C, for example, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, 95°C, 96°C, 97°C, 98°C, 99°C or 100°C.

[0124] Preferably, the pH of the primary leaching is 1.0 to 2.0, for example, 1.0, 1.5 or 2.0, and the leaching time is 2 to 6 hours, for example, 2 hours, 3 hours, 4 hours, 5 hours or 6 hours.

[0125] Preferably, before obtaining the post-leaching liquid, the process further includes: solid-liquid separation to obtain the post-leaching liquid and leaching residue; the method further includes adjusting the pH of the leaching residue with acid solution and then pouring it into a pressure autoclave for pressure leaching to obtain a pressurized leachate, which is then returned to the primary leaching process. Further pressure leaching of the leaching residue after the stirred leaching can increase the nickel leaching rate. The leaching residue is used as raw material for the pressure leaching process of the nickel matte raw material system. The leaching residue has a lower nickel content, which can significantly reduce the pressure leaching reaction time and increase the production capacity of the nickel matte raw material system.

[0126] Preferably, the leached residue is adjusted to a pH of 1.5 to 2.0 with acid solution and then poured into a pressure autoclave for pressure leaching.

[0127] Usually, pressure leaching is performed after the pH is stabilized in the above range for 0.5 to 1.5 hours.

[0128] Preferably, the pressure leaching temperature is 160-180°C, for example, 160°C, 165°C, 170°C, 175°C or 180°C, the oxygen partial pressure is 0.6-1.0 MPa, for example, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa or 1.0 MPa, and the time is 4-7 h, for example, 4 h, 5 h, 6 h or 7 h.

[0129] Generally, the oxygen partial pressure during oxygen pressure leaching is high, reaching above 1.0 MPa. The leached residue obtained through one leaching process in the present invention can be leached at a lower oxygen partial pressure, which is preferably 0.6 to 0.9 MPa, and more preferably 0.6 to 0.8 MPa.

[0130] Compared with the leaching and iron removal process of the nickel matte raw material system, the single leaching process disclosed in the present invention has a shorter reaction time and an efficiency improvement of 100-200%. In addition, the reaction process of this solution is milder, does not require the introduction of oxygen, does not produce hydrogen, and is safer.

[0131] The present disclosure also provides a method for preparing nickel sulfate, including the above-mentioned method for leaching nickel elements.

[0132] Preferably, the method further comprises:

[0133] Iron removal: Hydrogen peroxide is added to the leached liquid and stirred to remove iron. The solid-liquid separation produces iron-removed liquid and iron-removed slag. The iron-removed liquid can also be fed into a subsequent extraction system for further impurity removal.

[0134] Preferably, the molar ratio of the ferrous iron content in the leached liquid to the hydrogen peroxide content in the added hydrogen peroxide is controlled to be 1:(1.5-3.0), for example, 1:1.5, or 1:2.0, or 1:2.5, or 1:3.0.

[0135] Preferably, after stirring, the pH is adjusted to 3.5 to 4.5, for example, 3.5, 4.0 or 4.5, and then solid-liquid separation is performed to obtain the deironing liquid and deironing slag. Preferably, the pH is stabilized at 3.5 to 4.5 for 1 to 2 hours, and then solid-liquid separation is performed.

[0136] Compared with the prior art, the advantages of the present invention include:

[0137] The method for leaching nickel provided herein uses nickel cobalt hydroxide and nickel matte as leaching raw materials. When leaching the nickel cobalt hydroxide raw material, the elemental nickel in the nickel matte raw material serves as a reducing agent, while when leaching the nickel cobalt hydroxide raw material, the manganese in the nickel cobalt hydroxide raw material serves as an oxidizing agent. This eliminates the need for additional reducing or oxidizing agents, significantly reducing the cost of auxiliary materials in the MHP leaching process. Compared with other processes, this method reduces the introduction of impurity ions (such as sodium ions) into the system, lowering evaporation costs. Furthermore, it reduces oxygen consumption and equipment investment costs during the nickel matte leaching process, shortens the leaching process, and significantly increases the production capacity of the nickel matte leaching system. The reaction process does not require the introduction of oxygen, nor does it produce hydrogen, making the reaction milder and safer.

[0138] This method not only solves the existing problems of high reducing agent consumption and high sodium introduction in the MHP leaching process, but also addresses the long leaching time and low leaching efficiency in the atmospheric pressure leaching of high-grade nickel matte, reducing oxygen consumption. This method requires no reducing agent or oxidizing agent auxiliary materials, resulting in extremely low auxiliary material costs. It also offers simple operation, a mild reaction process, and enhanced safety and feasibility. Compared to the leaching and iron removal processes in high-grade nickel matte systems, this solution achieves a shorter single-stage leaching reaction time and a 100% to 200% increase in efficiency, resulting in excellent overall results.

[0139] The examples described below are illustrative and are intended only to explain the present disclosure and are not to be construed as limiting the present disclosure. Where specific techniques or conditions are not specified in the examples, the methods were performed according to those described in the literature in the art or according to the product specifications. Reagents or instruments used, for which the manufacturer is not specified, are commercially available conventional products.

[0140] The elemental composition of the MHP raw materials used in Examples 1-6 and Comparative Examples 1-7 of the present disclosure is shown in Table 1, and further analysis of the chemical composition of the MHP raw materials is shown in Table 2. The elemental composition of the high-matte nickel raw materials used is shown in Table 3, and further analysis of the chemical composition of the high-matte nickel raw materials is shown in Table 4.

[0141] Table 1 Elemental composition of MHP

[0142] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0143] Table 2 Chemical composition of MHP

[0144] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0145] Table 3 Element composition of nickel matte

[0146] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0147] Table 4 Chemical composition of high nickel matte

[0148] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0149] Example 1

[0150] (1) First, take 600g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0151] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 65%, the slag rate is 4.51%, and the Ni, Co, and Mn contents in the leached liquid are 125.45 g / L, 4.89 g / L, and 5.743 g / L, respectively. The Fe, Al, and Si contents are 245 mg / L, 125 mg / L, and 114 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 37.74%, 0.15%, 0.04%, 2.41%, and 20.82%, respectively.

[0152] (3) Take 1L of the leached liquid obtained in step (2) and place it in a 2L beaker. Set the temperature to room temperature. Add 0.36mL of hydrogen peroxide (the molar coefficient ratio of divalent iron to hydrogen peroxide in the leached liquid is 1:2.0) and mix and stir for 10 minutes. After stirring, add a certain amount of calcium powder to adjust the pH to 4.5. After the pH stabilizes for 1 to 2 hours, separate the solid and liquid to obtain the iron-removing liquid and iron-removing slag. The iron-removing liquid enters the subsequent extraction system. The iron-removing slag is washed and discarded. The Fe and Al in the iron-removing liquid are reduced to below 1mg / L.

[0153] (4) Take 24g of the leaching residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 160℃ and the oxygen partial pressure is set to 0.8Mpa. After reacting for 6h, solid-liquid separation is performed to obtain a pressurized leachate and a pressurized leachate residue. The pressurized leachate enters the previous process step (2) as a solution, and the pressurized leachate residue is treated according to the hematite leaching treatment method. The Ni and Fe in the pressurized leachate are 117g / L and 0.12g / L, respectively, and the dry basis contents of nickel and iron in the pressurized leachate residue are 4.32% and 49.44%, respectively.

[0154] Example 2

[0155] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0156] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 68%, the slag rate is 3.15%, and the Ni, Co, and Mn contents in the leached liquid are 131.24 g / L, 3.94 g / L, and 9.147 g / L, respectively. The Fe, Al, and Si contents are 382 mg / L, 119 mg / L, and 130 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 35.45%, 0.24%, 0.08%, 2.05%, and 21.42%, respectively.

[0157] (3) 1 L of the leached liquid obtained in step (2) was placed in a 2 L beaker and the temperature was set to room temperature; 0.36 mL of hydrogen peroxide (the molar coefficient ratio of the divalent iron in the leached liquid to hydrogen peroxide was 1:1.5) was added and the mixture was stirred for 10 min. After the stirring was completed, a certain amount of calcium powder was added to adjust the pH to 4.5. After the pH was stable for 1 to 2 hours, the solid-liquid separation was performed to obtain the iron-removing liquid and the iron-removing slag. The iron-removing liquid was fed into the subsequent extraction system, and the iron-removing slag was washed and discarded. The Fe and Al in the iron-removing liquid were reduced to below 1 mg / L.

[0158] (4) Take 24g of the leaching residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 160℃ and the oxygen partial pressure is set to 0.8Mpa. After reacting for 6h, solid-liquid separation is performed to obtain a pressurized leachate and a pressurized leachate residue. The pressurized leachate enters the previous process step (2) as a solution, and the pressurized leachate residue is treated according to the hematite leaching treatment method. The Ni and Fe in the pressurized leachate are 117g / L and 0.12g / L, respectively, and the dry basis contents of nickel and Fe in the pressurized leachate are 4.32% and 49.44%, respectively.

[0159] Example 3

[0160] (1) First, take 600 g of MHP powder of material C and put it into a crusher. Turn on the stirring and crushing for 10 minutes to obtain MHP powder.

[0161] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 10g of sample 3 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 70%, the slag rate is 2.94%, and the Ni, Co, and Mn contents in the leached liquid are 134.11 g / L, 4.86 g / L, and 11.52 g / L, respectively. The Fe, Al, and Si contents are 308.86 mg / L, 162.24 mg / L, and 237.35 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 41.33%, 0.03%, 0.04%, 2.68%, and 15.54%, respectively.

[0162] (3) 1 L of the leached liquid obtained in step (2) was placed in a 2 L beaker and the temperature was set to room temperature; 0.48 mL of hydrogen peroxide (the molar coefficient ratio of divalent iron to hydrogen peroxide in the leached liquid was 1:2.6) was added and the mixture was stirred for 10 min. After the stirring was completed, a certain amount of calcium powder was added to adjust the pH to 4.5. After the pH was stable for 1 to 2 h, solid-liquid separation was performed to obtain the iron-removing liquid and iron-removing slag. The iron-removing liquid was fed into the subsequent extraction system, and the iron-removing slag was washed and discarded. The Fe and Al in the iron-removing liquid were reduced to below 1 mg / L.

[0163] (4) Take 20g of the leaching residue obtained in step (2) in a 1L beaker, add a certain amount of sulfuric acid to adjust the pH to 2.0, and pour it into a pressure autoclave after stabilization for 1h. The temperature is set to 180℃ and the oxygen partial pressure is set to 0.7Mpa. After reacting for 6h, solid-liquid separation is performed to obtain a pressurized leachate and a pressurized leachate residue. The pressurized leachate enters the previous process step (2) as a solution, and the pressurized leachate residue is treated according to the hematite leaching treatment method. The Ni and Fe in the pressurized leachate are 123.06g / L and 0.26g / L, respectively, and the dry basis contents of nickel and iron in the leachate residue are 3.38% and 58.87%, respectively.

[0164] Example 4

[0165] (1) First, take 600g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0166] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 32g of sample 1 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4h. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 55%, the slag rate is 10.17%, and the Ni, Co, and Mn contents in the leached liquid are 101.09 g / L, 3.57 g / L, and 8.693 g / L, respectively. The Fe, Al, and Si contents are 396.7 mg / L, 250.66 mg / L, and 270.7 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 48.33%, 0.07%, 0.05%, 3.68%, and 20.54%, respectively.

[0167] Example 5

[0168] (1) First, take 600g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0169] (2) Take 400g of the MHP powder obtained in step (1) and put it in a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 15.2g of sample 2 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4h. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 60%, the slag rate is 8.71%, the Ni, Co and Mn contents in the leachate are 112.79 g / L, 1.77 g / L and 8.347 g / L respectively, and the Fe, Al and Si contents are 276.7 mg / L, 140.6 mg / L and 230.9 mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leaching slag are 42.73%, 0.07%, 0.05%, 2.96% and 18.54% respectively.

[0170] Example 6

[0171] (1) First, take 600g of MHP powder of material A into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0172] (2) Take 400g of the MHP powder obtained in step (1) and put it into a 1L beaker. Add 800mL of pure water at a liquid-solid ratio of 2:1 and start stirring. Set the temperature to 95°C and add 7.75g of sample 4 high-grade nickel matte powder. After reaching the reaction temperature, add a certain amount of sulfuric acid to maintain the pH at 1.5 for a total of 4 hours. After the reaction time is reached, perform solid-liquid separation to obtain the leached liquid and leached residue. The MHP nickel leaching rate is greater than 99%, the high matte nickel leaching rate is greater than 70%, the slag rate is 3.47%, the Ni, Co and Mn contents in the leachate are 128.47 g / L, 2.44 g / L and 8.783 g / L respectively, and the Fe, Al and Si contents are 206.7 mg / L, 140.6 mg / L and 360.7 mg / L respectively; the dry basis contents of Ni, Co, Mn, Fe and S in the leaching slag are 25.77%, 0.07%, 0.04%, 2.08% and 18.94% respectively.

[0173] Comparative Example 1

[0174] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0175] (2) Take 400 g of the MHP powder obtained in step (1) and put it into a 1 L beaker. Add 1000 mL of pure water at a liquid-to-solid ratio of 2.5:1 and start stirring. Set the temperature to 95 ° C. After reaching the reaction temperature, slowly add 317 mL of hydrogen peroxide and a certain amount of sulfuric acid to maintain the pH at 1.5. The addition time is 3 hours and the pH stabilization time is 2 hours. After the time is reached, solid-liquid separation is performed to obtain the leached liquid and leached residue. The MHP nickel leaching rate is 99%, the slag rate is 1.04%, the Ni, Co, and Mn contents in the leachate are 102 g / L, 1.02 g / L, and 5.52 g / L, respectively, and the Fe, Al, and Si contents are 115.3 mg / L, 104.6 mg / L, and 65.12 mg / L, respectively; the dry basis contents of Ni, Co, Mn, and Fe in the leached slag are 2.65%, 0.04%, 0.025%, and 0.59%, respectively. The hydrogen peroxide consumption is approximately 7.21 times the theoretical amount, and the cost of auxiliary materials is high.

[0176] Comparative Example 2

[0177] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0178] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1, and stirring was started. The temperature was set at 95°C. After reaching the reaction temperature, 31.86 g of sodium metabisulfite and a certain amount of sulfuric acid were slowly added to maintain the pH at 1.5. The addition time was 3 hours, and the pH was stabilized for 2 hours. After the time was reached, solid-liquid separation was performed to obtain a leached liquid and a leached residue. The MHP nickel leaching rate was 99%, the residue rate was 1.14%, and the Ni, Co, and Mn contents in the leachate were 104 g / L, 1.12 g / L, and 4.89 g / L, respectively. The Fe, Al, Si, and Na contents were 125.2 mg / L, 126.6 mg / L, 61.12 mg / L, and 7712 mg / L, respectively. The dry basis contents of Ni, Co, Mn, and Fe in the leached residue were 2.65%, 0.04%, 0.025%, and 0.59%, respectively. The sodium content in the leachate is high, and the subsequent evaporation and crystallization pressure is high.

[0179] Comparative Example 3

[0180] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0181] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1, and stirring was started. The temperature was set at 95°C. After reaching the reaction temperature, 22 g of nickel sulfide powder and a certain amount of sulfuric acid were added to maintain the pH at 1.5. The reaction time was 4 h. After the reaction time was reached, solid-liquid separation was performed to obtain a leachate and a leach residue. The MHP nickel leaching rate was only 92%, and the slag rate was 22.45%. The Ni, Co, and Mn contents in the leachate were 98.21 g / L, 0.82 g / L, and 1.19 g / L, respectively, and the Fe, Al, and Si contents were 109.2 mg / L, 229.6 mg / L, and 54.12 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leach residue were 11.54%, 0.18%, 6.5%, 1.59%, and 34.47%, respectively. Nickel sulfide powder is not effective as a reducing agent and has a low leaching rate.

[0182] Comparative Example 4

[0183] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0184] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1, and stirring was started. The temperature was set at 95 ° C. After reaching the reaction temperature, 23 g of nickel cobalt sulfide powder and a certain amount of sulfuric acid were added to maintain the pH at 1.5. The reaction time was 4 h. After the time was reached, solid-liquid separation was performed to obtain a leached liquid and a leached residue. The MHP nickel leaching rate was only 92%, and the residue rate was 22.85%. The Ni, Co, and Mn contents in the leachate were 99.21 g / L, 0.92 g / L, and 1.39 g / L, respectively, and the Fe, Al, and Si contents were 165.2 mg / L, 119.6 mg / L, and 65.12 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached residue were 7.47%, 4.81%, 6.25%, 1.78%, and 36.47%, respectively. The effect of nickel cobalt sulfide powder as a reducing agent is not obvious and the leaching rate is low.

[0185] Comparative Example 5

[0186] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0187] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1, and stirring was started. The temperature was set to 95 ° C., and 8 g of metallic nickel powder was added. After reaching the reaction temperature, a certain amount of sulfuric acid was added to maintain the pH at 1.5. The reaction time was 4 h. After the reaction time was reached, solid-liquid separation was performed to obtain the leached liquid and leached residue. MHP nickel leaching rates exceed 99%, metallic nickel leaching rates exceed 98%, and the slag rate is only 0.85%. The Ni, Co, and Mn contents in the leachate are 128g / L, 3.58g / L, and 4.35g / L, respectively; the Fe, Al, and Si contents are 109.8mg / L, 124.87mg / L, and 48.16mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 31.42%, 0.034%, 0.0422%, 0.54%, and 0.004%, respectively. Using metallic nickel as a reducing agent yields excellent leaching results and high efficiency, but the cost of metallic nickel powder is extremely high.

[0188] Comparative Example 6

[0189] (1) First, take 600g of MHP powder of material B into a crusher, start stirring and crushing for 10 minutes to obtain MHP powder.

[0190] (2) 400 g of the MHP powder obtained in step (1) was placed in a 1 L beaker, 1000 mL of pure water was added at a liquid-to-solid ratio of 2.5:1, and stirring was started. The temperature was set to 95 ° C., and 12 g of nickel-iron alloy powder was added. After reaching the reaction temperature, a certain amount of sulfuric acid was added to maintain the pH at 1.5. The reaction time was 4 h. After the reaction time was reached, solid-liquid separation was performed to obtain the leached liquid and the leached residue. The nickel leaching rate of MHP is greater than 99%, and the nickel leaching rate of ferronickel is greater than 75%. The slag fraction is 2.85%. The Ni, Co, and Mn contents in the leachate are 123 g / L, 3.23 g / L, and 4.62 g / L, respectively. The Fe, Al, and Si contents are 4587 mg / L, 104.78 mg / L, and 55.34 mg / L, respectively. The dry basis contents of Ni, Co, Mn, Fe, and S in the leached slag are 35.32%, 0.004%, 0.02%, 45.45%, and 0.004%, respectively. Using ferronickel as a reducing agent has a certain leaching effect, but it increases the iron content in the leachate.

[0191] Comparative Example 7

[0192] (1) First, take 1000g of sample 3 high-grade nickel matte in a 10L beaker, add 5L of water at a liquid-solid mass ratio of 5:1, set the temperature to 65°C, and after reaching the reaction temperature, add 333mL of sulfuric acid and continuously introduce oxygen. After the reaction reaches a pH value of 5.0, solid-liquid separation is started and atmospheric pressure leaching residue and atmospheric pressure leaching liquid are obtained. The reaction time is 10h, the high-grade nickel matte leaching rate is 45%, and the Ni content in the atmospheric pressure leaching liquid is 90.58g / L.

[0193] (2) The atmospheric leaching residue was placed in a 3L pressure autoclave, and 2L of water and 50mL of sulfuric acid were added and stirred. After stirring for 1 hour, the autoclave was sealed and the temperature in the autoclave was set to 200°C. After reaching the set temperature, oxygen was introduced into the autoclave until the oxygen partial pressure reached 1.0 MPa and the reaction was carried out for 6 hours. After the reaction, pressure leaching residue and pressure leaching liquid were obtained. The residue rate was about 3.5%. The main components of the residue were iron and nickel, with dry basis contents of 52.1% and 3.2%, respectively. The content of various impurities was less than 0.01%. In the conventional leaching process of high-grade nickel matte, the reaction time of the atmospheric oxygen leaching section was long, the oxygen consumption was large, and the leaching conditions of the pressure leaching section were demanding.

[0194] The schemes and leaching results of the various embodiments and comparative examples are shown in Table 5. According to Table 5, it can be seen that Examples 1 to 6 of the disclosed scheme simultaneously use nickel cobalt hydroxide and high nickel matte as leaching raw materials, which can improve the nickel leaching rate of nickel cobalt hydroxide and the nickel leaching rate of high nickel matte, and the method is low in cost and does not introduce other impurities. It not only solves the problems of large reducing agent consumption and high sodium introduction in the MHP leaching process in the prior art, but also solves the problems of long leaching time and low leaching efficiency in the atmospheric pressure leaching process of high nickel matte, and reduces oxygen consumption. In addition, according to Example 2 and Examples 4-6, the higher the elemental nickel content of the high nickel matte, the higher the nickel leaching rate of the high nickel matte, and the higher the liquid nickel content after leaching.

[0195] Table 5 Schemes and leaching results of various embodiments and comparative examples

[0196] Note: In Table 5, when both the oxidant and the reductant contain nickel, the nickel leaching rates of MHP and high-grade nickel matte are estimated values, because there are great differences in the morphology of the leaching residues of MHP and high-grade nickel matte. The MHP leaching rate greater than 99% means that the MHP has been completely dissolved and there is no leaching residue.

[0197] The crude metal hydroxide used in Examples 7-9 and Comparative Examples 8-14 of the present disclosure was nickel cobalt hydroxide (MHP), and the chemical composition of the MHP raw material is shown in Table 6. The nickel-containing raw material used in the present disclosure was high-matte nickel, and the chemical composition of the high-matte nickel raw material is shown in Table 7. The process flow chart of the method for removing impurities from the crude metal hydroxide leaching slurry in the present disclosure is shown in Figure 1.

[0198] Table 6 Chemical composition of MHP raw materials

[0199] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0200] Table 7 Chemical composition of nickel matte

[0201] Note: Water content is the natural basis content, and other ingredients in the table are the dry basis content.

[0202] Example 7

[0203] (1) 2000 g of MHP natural-based raw material was added to pure water to prepare a slurry with a slurry concentration of 25 wt%.

[0204] (2) Add 98% sulfuric acid to the prepared slurry for acid leaching, control the temperature to 80° C., the stirring speed to 300 rpm, the pH to 1.0-1.5, and the reaction time to 1.5 h to obtain a leached slurry.

[0205] (3) Add 40g of high-grade nickel matte to the leaching slurry (the weight ratio of high-grade nickel matte to MHP natural base is 1:50), and introduce oxygen, control the oxygen flow rate to 2-3L / min, and the temperature to 65°C until the pH is 3.5, and perform impurity removal (impurity removal time is 2h). After the impurity removal reaction is completed, solid-liquid separation is performed, and the filtration rate is 26.40L / h to obtain a nickel concentration of 105.23g / L, a calcium concentration of 0.33g / L, and 188.60g of impurity-removed slag. The concentrations of each element in the impurity-removed liquid obtained in Example 7 are shown in Table 8. It can be seen from Table 8 that the impurity-removed liquid in Example 7 meets the relevant standards for iron concentration and aluminum concentration in "T / ATCRR12-2020 Battery Grade Nickel Sulfate".

[0206] Table 8 Concentration of each element in the impurity-removed liquid of Example 7

[0207] The scanning electron microscope morphology of the impurity-removed slag obtained in Example 7 is shown in FIG2 . The particles of the impurity-removed slag are uniform, fine, and loosely arranged, thereby enabling rapid filtration, reducing filtration time, and improving production efficiency.

[0208] (4) The impurity-removed slag obtained in step (3) is controlled to have a liquid-to-solid ratio of 3:1, the liquid is a liquid containing sulfuric acid, the initial acidity pH is 1.0, the temperature is 180° C., the oxygen partial pressure is 0.5 MPa, and the reaction is performed for 4 hours to perform pressurized oxygen leaching to obtain an oxygen pressure leaching liquid nickel-cobalt-manganese sulfate solution and an oxygen pressure leaching slag hematite slag.

[0209] The content and concentration of each element in the impurity-removed slag, the oxygen pressure leaching solution, and the oxygen pressure leaching slag of Example 7 are shown in Table 9. As shown in Table 9, the cobalt and manganese in the impurity-removed slag exist in the form of high-valent compounds. The phase analysis of Example 7 combined with Table 9 shows that the high-valent cobalt and manganese compounds present in the impurity-removed slag are converted into low-valent cobalt sulfate and manganese sulfate after oxygen pressure leaching and enter the oxygen pressure leaching solution, thereby eliminating the need for a separate reduction leaching step for the high-valent cobalt and manganese, shortening the process flow, and improving production efficiency.

[0210] Table 9 Content and concentration of each element in the slag after impurity removal, oxygen pressure leaching solution and oxygen pressure leaching slag

[0211] (5) The pH of the impurity-removed liquid obtained in step (3) is adjusted to 4.0, and calcium impurities are removed by extraction with P204, manganese impurities are extracted with P507, and magnesium and cobalt impurities are extracted with C272. The raffinate is a nickel sulfate solution, which is deoiled to obtain a finished nickel sulfate solution.

[0212] Example 8

[0213] The difference from Example 7 is that

[0214] The mass of high-grade nickel matte added in step (3) is 28.57g (the weight ratio of high-grade nickel matte to MHP natural base is 1:70), and oxygen is introduced, and the oxygen flow rate is controlled at 2-3L / min and the temperature is 65°C until the pH = 3.5, and impurities are removed (the impurity removal time is 4.5h). After the impurity removal reaction is completed, solid-liquid separation is carried out, and the filtration rate is 20.21L / h to obtain a nickel concentration of 103.67g / L, an iron concentration of 0.0010g / L, an aluminum concentration of 0.0001g / L, and a calcium concentration of 0.30g / L. The impurity-removed liquid and 176.10g of impurity-removed slag are obtained. The impurity-removed liquid meets the relevant standards for iron concentration and aluminum concentration in "T / ATCRR12-2020 Battery Grade Nickel Sulfate".

[0215] (4) The impurity-removed slag obtained in step (3) is controlled to have a liquid-to-solid ratio of 3:1, the liquid is a liquid containing sulfuric acid, the initial acidity pH is 1.0, the temperature is 180° C., the oxygen partial pressure is 0.5 MPa, and the reaction is performed for 4 hours to perform pressurized oxygen leaching to obtain an oxygen pressure leaching liquid nickel-cobalt-manganese sulfate solution and an oxygen pressure leaching slag hematite slag.

[0216] The components of the impurity-removed slag, oxygen pressure leaching slag, and oxygen pressure leaching liquid obtained in this example are shown in Table 10.

[0217] Table 10 Content and concentration of elements in the slag after impurity removal, oxygen pressure leaching solution and oxygen pressure leaching slag

[0218] Example 9

[0219] The difference from Example 7 is that

[0220] The mass of high-grade nickel matte added in step (3) is 100g (the weight ratio of high-grade nickel matte to MHP natural base is 1:20), and oxygen is introduced, and the oxygen flow rate is controlled at 2-3L / min and the temperature is 65°C until the pH = 3.5, and impurities are removed (the impurity removal time is 1h). After the impurity removal reaction is completed, solid-liquid separation is carried out, and the filtration rate is 31.66L / h to obtain a nickel concentration of 107.11g / L, an iron concentration of 0.0008g / L, an aluminum concentration of 0.0001g / L, and a calcium concentration of 0.29g / L. The impurity-removed liquid and 252.43g of impurity-removed slag are obtained. The impurity-removed liquid meets the relevant standards for iron concentration and aluminum concentration in "T / ATCRR12-2020 Battery Grade Nickel Sulfate".

[0221] The impurity-removed slag obtained in step (3) was controlled to have a liquid-to-solid ratio of 3:1, a temperature of 180° C., an oxygen partial pressure of 0.5 MPa, and reacted for 4 hours for pressurized oxygen leaching to obtain an oxygen pressure leaching solution, a nickel-cobalt-manganese sulfate solution, and an oxygen pressure leaching slag (hematite slag). The element contents of the oxygen pressure leaching solution and the oxygen pressure leaching slag are shown in Table 11.

[0222] Table 11 Content and concentration of each element in the slag after impurity removal, oxygen pressure leaching solution and oxygen pressure leaching slag of Example 9

[0223] Comparative Example 8

[0224] (1) 2000 g of MHP natural-based raw material was added to pure water to prepare a slurry with a slurry concentration of 25 wt%.

[0225] (2) Add 98% sulfuric acid to the prepared slurry for acid leaching, control the temperature to 80° C., the stirring speed to 300 rpm, the pH to 1.0-1.5, and the reaction time to 1.5 h to obtain a leached slurry.

[0226] (3) 62.18 g of calcium carbonate was added to the leached slurry, the pH was adjusted to 5.0, and 57.48 mL of hydrogen peroxide was added. The reaction time was 3 h for impurity removal. After impurity removal, the slurry was subjected to solid-liquid separation at a filtration rate of 18.82 L / h to obtain a decontaminated liquid with a nickel concentration of 102.73 g / L and a calcium concentration of 0.79 g / L, as well as 233.16 g of decontaminated residue. The element concentrations of the decontaminated liquid of Comparative Example 8 are shown in Table 12.

[0227] Table 12 Concentration of each element in the impurity-removed liquid of Comparative Example 8

[0228] (4) Take 200 g of the impurity-removed residue of step (3), control the dry basis liquid-solid ratio to 2.5:1, add pure water to make a slurry, add sulfuric acid and sodium metabisulfite to the slurry for reduction leaching, control the reduction leaching temperature to 80° C., control the pH to 1.5, and react for 1 h to obtain a reduction leaching solution with a nickel concentration of 105.58 g / L and 74.56 g of reduction leaching residue.

[0229] (4) Take 200 g of the impurity-removed residue of step (3), control the dry basis liquid-solid ratio to 2.5:1, add pure water to make a slurry, add sulfuric acid and sodium metabisulfite to the slurry for reduction leaching, control the reduction leaching temperature to 80° C., control the pH to 1.5, and react for 1 h to obtain a reduction leaching solution with a nickel concentration of 105.58 g / L and 74.56 g of reduction leaching residue.

[0230] (5) Adding a solidifying agent, sodium fumarate, to the reduced leaching liquid to remove iron, separate the solid and liquid, and return the filtrate to the liquid after impurity removal for extraction separation, and the slag forms scrap iron slag.

[0231] (6) The reduced leaching residue is washed, and the washing liquid is returned to the slurry after acid leaching, and the washing residue forms waste calcium residue.

[0232] Comparative Example 8 uses calcium carbonate as a neutralizing agent, which has the problems of long reaction time, introduction of calcium impurities, poor economic benefits, and relatively complex process.

[0233] Comparative Example 9

[0234] (1) 2000 g of MHP natural-based raw material was added to pure water to prepare a slurry with a slurry concentration of 25 wt%.

[0235] (2) Add 98% sulfuric acid to the prepared slurry for acid leaching, control the temperature to 80° C., the stirring speed to 300 rpm, the pH to 1.0-1.5, and the reaction time to 1.5 h to obtain a leached slurry.

[0236] (3) 176.84 g of natural MHP was added to the leached slurry, the pH was adjusted to 5.0, 60.10 mL of hydrogen peroxide was added, and the reaction time was 3 h for impurity removal. After impurity removal, the slurry was subjected to solid-liquid separation at a filtration rate of 6.21 L / h to obtain a nickel concentration of 125.41 g / L, a calcium concentration of 0.37 g / L, and 210.06 g of impurity-removed slag. The scanning electron microscopy morphology of the impurity-removed slag of Comparative Example 9 is shown in FIG3 . The constituent particles of the impurity-removed slag are amorphous and clustered. The particles are tightly packed. During the filtration process, the filter cake solution has a low pass rate, poor water permeability, and difficulty in filtration, resulting in a slow filtration rate.

[0237] (4) Take 200 g of the impurity-removed residue of step (3), control the dry basis liquid-solid ratio to 2.5:1, add pure water to make a slurry, add sulfuric acid and sodium metabisulfite to the slurry for reduction leaching, control the reduction leaching temperature to 80° C., control the pH to 1.5, and react for 1 h to obtain a reduction leaching solution with a nickel concentration of 100.26 g / L and 2.44 g of reduction leaching residue.

[0238] (5) Adding a solidifying agent, sodium fumarate, to the reduced leaching liquid to remove iron, separate the solid and liquid, and return the filtrate to the liquid after impurity removal for extraction separation, and the slag forms scrap iron slag.

[0239] (6) The reduced leaching residue is washed, and the washing liquid is returned to the slurry after acid leaching, and the washing residue forms waste calcium residue.

[0240] Comparative Example 10

[0241] The difference from Example 7 is that the neutralizer used in step (3) is nickel carbonate, the pH is adjusted to 5.0, hydrogen peroxide is added for impurity removal, and the slurry is subjected to solid-liquid separation after impurity removal. The filtration rate is 7.04 L / h to obtain a de-impurity liquid with a nickel concentration of 123.87 g / L and a calcium concentration of 0.40 g / L and 176.22 g of de-impurity residue.

[0242] Comparative Example 11

[0243] The difference from Example 7 is that the neutralizer used in step (3) is nickel hydroxide, the pH is adjusted to 5.0, hydrogen peroxide is added for impurity removal, and the slurry is subjected to solid-liquid separation after impurity removal. The filtration rate is 6.33 L / h, and a de-impurified liquid with a nickel concentration of 127.21 g / L and a calcium concentration of 0.38 g / L and 201.63 g of de-impurified residue are obtained.

[0244] Comparative Example 12

[0245] Steps (1) to (3) are the same as those in Example 7. The difference from Example 7 is that the impurity-removed slag is subjected to reduction leaching before oxygen pressure leaching:

[0246] (4) Take 200 g of the impurity-removed residue of step (3), control the dry basis liquid-solid ratio to 3:1, add pure water to make a slurry, add sulfuric acid and sodium metabisulfite to the slurry for reduction leaching, control the reduction leaching temperature to 80° C., control the pH to 1.5, and react for 1 h to obtain a reduction leaching slurry.

[0247] (5) The reduction leaching slurry of step (4) is subjected to oxygen pressure leaching, the temperature is controlled to 180°C, the oxygen partial pressure is 0.5 MPa, and the reaction time is 4 h, to obtain oxygen pressure leaching solution nickel cobalt manganese sulfate solution and oxygen pressure leaching slag hematite slag. The composition of the oxygen pressure leaching solution and the oxygen pressure leaching slag are shown in Table 13. The content of each element is basically the same as that in Example 7. Comparative Example 12 and Example 7 can achieve the same effect, indicating that pre-leaching is achieved while using high-matte nickel as a neutralizer, and the filter residue is subsequently subjected to oxygen pressure leaching to obtain a sulfate solution, thereby reducing the reduction leaching process.

[0248] Table 13 Content and concentration of each element in the oxygen pressure leaching solution and oxygen pressure leaching residue of Comparative Example 12

[0249] Comparative Example 13

[0250] Steps (1) to (2) are the same as in Example 7. The difference from Example 7 is that in the impurity removal process in step (3), the pH is controlled to 2.5 for impurity removal, and solid-liquid separation is performed after the impurity removal reaction is completed to obtain a de-impurified liquid with a nickel concentration of 121.04 g / L, an Fe concentration of 0.842 g / L, and an Al concentration of 0.212 g / L. As shown in Table 14, the de-impurified liquid of Comparative Example 13 does not meet the relevant standards for iron concentration and aluminum concentration in "T / ATCRR12-2020 Battery Grade Nickel Sulfate".

[0251] Table 14 Concentration of each element in the impurity-removed liquid of Comparative Example 13

[0252] Comparative Example 14

[0253] Steps (1) to (2) are the same as those in Example 7. The difference from Example 7 is that in step (3), oxygen is not introduced for impurity removal until the pH reaches 3.5. The impurity removal time is 4 hours. After the impurity removal reaction is completed, solid-liquid separation is performed to obtain a de-impurified liquid with a nickel concentration of 124.28 g / L, an Fe concentration of 0.995 g / L, and an Al concentration of 0.0010 g / L.

[0254] Without oxygen, the addition of high-grade nickel matte significantly slows down the rate of consumption of residual acid in the iron-aluminum process, and the ferrous ions are not oxidized, and goethite precipitation cannot be formed, resulting in the liquid iron concentration after impurities removal not meeting the relevant standards for iron concentration in "T / ATCRR12-2020 Battery-Grade Nickel Sulfate".

[0255] The methods for removing impurities from the MHP leaching slurry of the various embodiments and comparative examples of the present disclosure are shown in Table 15. By comparison, it can be seen that the use of high-grade nickel matte as a neutralizer in Examples 7 to 3 not only effectively improves the filtration efficiency but also introduces fewer impurities.

[0256] Table 15 Methods for removing impurities from MHP leaching slurry in various embodiments and comparative examples

[0257] It should be noted that the present disclosure is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and within the scope of the technical solution of the present disclosure, embodiments having substantially the same structure as the technical concept and exerting the same effects are all included in the technical scope of the present disclosure. In addition, within the scope of the present disclosure, various modifications that can be conceived by those skilled in the art to the embodiments, and other methods constructed by combining some of the constituent elements of the embodiments are also included in the scope of the present disclosure. Industrial Applicability

[0258] This disclosure involves acid leaching crude metal hydroxides, providing two acid leaching methods. Method 1 precipitates at least one of the impurities, including manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc, and produces a decontaminated solution containing at least one of nickel and cobalt. This reduces the introduction of calcium impurities, lowers production costs, and improves economic benefits. Method 2 does not require the addition of additional reducing agents or oxidizing agents, significantly reducing auxiliary material costs in the MHP leaching process, minimizing the introduction of impurity ions into the system, and lowering evaporation costs. Both methods have excellent industrial application value.

Claims

1. A method for removing impurities from a crude metal hydroxide leaching slurry, characterized in that: include: Leaching process: using crude metal hydroxide as a starting material for acid leaching to obtain a leaching slurry, wherein the crude metal hydroxide includes at least one of crude nickel hydroxide and crude cobalt hydroxide, and the slurry also includes impurities, and the impurities include at least one of manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc; Impurity removal process: adding nickel-containing raw materials and oxidants to the leaching slurry to remove impurities, wherein the nickel-containing raw materials can be used as a neutralizing agent in the leaching process to obtain impurity-removed liquid and impurity-removed slag.

2. A method for removing impurities from a crude metal hydroxide, characterized in that: include: Leaching process: using crude metal hydroxide as a starting material for acid leaching to obtain a leaching slurry, wherein the crude metal hydroxide includes at least one of crude nickel hydroxide and crude cobalt hydroxide, and the slurry also includes impurities, and the impurities include at least one of manganese, iron, aluminum, calcium, magnesium, copper, chromium, and zinc.

3. The impurity removal method according to claim 1 or 2, characterized in that: The crude metal hydroxide comprises at least one of Co2O3, Co(OH)3, and MnO2; Optionally, the crude metal hydroxide is selected from one of nickel cobalt hydroxide and crude cobalt hydroxide; Optionally, the crude metal hydroxide is selected from nickel cobalt hydroxide; Optionally, the crude metal hydroxide has a dry basis content of Ni element of 35-60%, a dry basis content of Co element of less than 5%, and a dry basis content of Mn element of less than 10%.

4. The impurity removal method according to claim 1 or 2, characterized in that: The acid leaching temperature is 40-100°C; Optionally, the stirring speed of the acid leaching is 200-800 rpm; Optionally, the reaction time of the acid leaching is 1-4h.

5. The impurity removal method according to claim 1 or 2, characterized in that: The process also includes a removal step: adding a nickel-containing raw material and an oxidant to the leaching slurry to remove impurities, thereby obtaining a liquid after impurities removal and a residue after impurities removal; In the impurity removal process, the pH of the leaching slurry is adjusted to 3.5 or above.

6. The impurity removal method according to claim 1 or 5, characterized in that: The nickel-containing raw material includes at least one of Ni element, Ni3S2, Ni2O3, and Ni(OH)3; Optionally, the nickel-containing raw material includes nickel matte; Optionally, the nickel-containing raw material is selected from high-matte nickel; Optionally, when the nickel-containing raw material is selected from high-matte nickel, the nickel content of the high-matte nickel on a dry basis is greater than or equal to 50%; Optionally, the nickel-containing raw material has a dry basis content of Ni element of 65-75%, a dry basis content of Co element of less than 2%, and a dry basis content of Mn element of less than 1%.

7. The impurity removal method according to any one of claims 1, 5-6, characterized in that: Adding a nickel-containing raw material and an oxidant to the leaching slurry for impurity removal satisfies: the amount of the nickel-containing raw material added is 1 / 100-1 / 10 of the natural basis weight of the crude metal hydroxide; Optionally, the amount of the nickel-containing raw material added is 1 / 70-1 / 50 of the natural basis weight of the crude metal hydroxide; Optionally, the reaction temperature is 40-100°C; Optionally, the reaction temperature is 60-70°C; Optionally, the oxidant is selected from any one of oxygen, hydrogen peroxide and ozone; Optionally, when the oxidant is oxygen, the oxygen introduction rate is 2-3 L / min; Optionally, the impurity removal time is 1-10h.

8. The impurity removal method according to any one of claims 2 to 4, characterized in that: The crude metal hydroxide is a nickel-cobalt hydroxide raw material, and the nickel-cobalt hydroxide raw material and the nickel matte raw material are co-leached under acidic conditions; the nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; the nickel matte raw material contains nickel element.

9. The impurity removal method according to claim 8, characterized in that: The dry content of manganese dioxide in the nickel-cobalt hydroxide raw material is 1% to 10%; and / or the dry content of elemental nickel in the nickel matte raw material is 5% to 25%; Optionally, the nickel matte raw material is high-grade nickel matte.

10. The impurity removal method according to claim 8 or 9, characterized in that: The mass ratio of the nickel cobalt hydroxide raw material to the nickel matte raw material is 1:(0.01-0.09); Optionally, water is added during the coordinated leaching, and the solid-liquid ratio of the nickel cobalt hydroxide raw material to water is 1g: (1.5-3)mL; Optionally, the acidic conditions of the collaborative leaching are: pH is controlled at 1.0 to 2.0; Optionally, the temperature of the collaborative leaching is 85-100° C., and the time is 2-6 hours.

11. The impurity removal method according to any one of claims 8 to 10, characterized in that: After the coordinated leaching, solid-liquid separation is performed to obtain leached liquid and leached residue; The method further comprises: Pressure leaching: The leaching residue is adjusted to pH with acid solution and then subjected to pressure leaching to obtain a pressure leaching solution.

12. The impurity removal method according to claim 11, characterized in that: The leached residue is adjusted to pH 1.5-2.0 with acid solution and then leached under pressure.

13. The impurity removal method according to claim 11 or 12, characterized in that: The pressure leaching temperature is 160-180° C., the oxygen partial pressure is 0.6-1.0 MPa, and the time is 4-7 hours.

14. A method for preparing sulfate, characterized in that: The impurity removal method according to any one of claims 1 and 5 to 7; the impurity-removed liquid is subjected to extraction and separation to obtain a sulfate solution; the impurity-removed slag is subjected to pressurized oxygen leaching to obtain a sulfate solution and hematite slag; Optionally, the initial acidity pH of the pressurized oxygen immersion is 1.0-1.2, the temperature of the pressurized oxygen immersion is 160-200° C., the oxygen partial pressure is 0.3-0.8 MPa, and the reaction time is 2-10 h.

15. A method for preparing nickel sulfate, characterized in that: The impurity removal method comprising any one of claims 8 to 13; Optionally, the method further comprises: performing solid-liquid separation after the coordinated leaching to obtain a post-leaching liquid and a leaching residue; Iron removal: adding hydrogen peroxide to the leached liquid to remove iron, and separating the solid and liquid to obtain iron-removed liquid and iron-removed slag; Optionally, the molar ratio of the ferrous iron content in the leached solution to the hydrogen peroxide content in the added hydrogen peroxide is controlled to be 1:(1.5-3.0); Optionally, after the stirring is completed, the pH is adjusted to 3.5-4.5, and then the solid-liquid separation is performed to obtain the iron-removed liquid and the iron-removed slag.

16. A method for leaching nickel, characterized in that: include: Primary leaching: co-leaching of nickel cobalt hydroxide raw material and nickel matte raw material under acidic conditions to obtain leached liquid; The nickel-cobalt hydroxide raw material contains nickel hydroxide, cobalt hydroxide and manganese dioxide; the nickel matte raw material contains nickel element.

Citation Information

Patent Citations

  • Combined leaching process of cobalt nickel hydroxide and cobalt nickel sulfide

    CN106834675A

  • Nickel-cobalt hydroxide residue low-cost treatment device and method

    CN110699557A

  • Method for preparing battery-grade nickel sulfate and cobalt sulfate from mixed nickel cobalt hydroxide

    CN111455174A

  • Method for continuously preparing large-particle-size beta-type cobalt sulfide crystals

    CN111533179A

  • Impurity removal method of crude metal hydroxide leaching slurry and sulfate preparation method

    CN116970807A

Cited By

  • Pretreatment method, impurity removal method and application of nickel-containing sludge

    CN119661039A

  • A pretreatment method, impurity removal method and application of nickel-containing sludge

    CN119661039B

  • Wet treatment process for laterite-nickel ore

    CN119685622A

  • Normal-pressure acid leaching and iron-silicon combined impurity removal method for high nickel matte

    CN121087297A