Lithium iron phosphate positive electrode material, preparation method therefor, and use thereof
By introducing aluminum and titanium elements into the lithium iron phosphate positive electrode material, combined with carbon coating technology, the compaction density and conductivity of the material are improved, and the problem of poor conductivity of lithium iron phosphate positive electrode material is solved, achieving efficient battery performance improvement .
Patent Information
- Application Number
- PCT/CN2023/096303
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-28
AI Technical Summary
The lithium ion diffusion coefficient and electronic conductivity of lithium iron phosphate positive electrode material have low lithium ion diffusion coefficient and electronic conductivity, resulting in poor conductivity and low energy density of terminal batteries, which cannot meet the needs of improving the range of new energy vehicles.
By mixing iron, phosphorus, lithium, carbon, aluminum and titanium sources, grinding and calcining, using carbon thermal reduction method and nano-normal effect of titanium elements, combined with amorphous carbon coating, lithium iron phosphate is improved by improving the carbon phosphate by using carbon thermal reduction method and nano-normal carbon coating. Compacting density and conductivity of particles.
The high compaction density and low resistivity of lithium iron phosphate positive electrode material are achieved, the process is simplified, the production cost is reduced, and it is suitable for lithium-ion battery applications.
Smart Images

Figure PCTCN2023096303-FTAPPB-I100001 
Figure 00000010_0000 
Figure 00000010_0001
Abstract
Description
A lithium iron phosphate positive electrode material and its preparation method and application Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a lithium iron phosphate positive electrode material and a preparation method and application thereof. Background Art
[0002] As a lithium-ion battery cathode material, lithium iron phosphate (LiFePO4) boasts abundant raw material reserves, high safety, environmental friendliness, and a long service life, making it widely used in power batteries and energy storage. However, due to its structural characteristics, it suffers from disadvantages such as low lithium ion diffusion coefficient, low electronic conductivity, and low compaction density. The resulting end-use battery products exhibit poor conductivity and low energy density. In recent years, the installed capacity of LiFePO4 power batteries has increased year by year, and market demands for longer driving range in new energy vehicles have necessitated the development of a LiFePO4 material with high compaction density and low resistivity.
[0003] Related technologies for increasing the compaction density of lithium iron phosphate (LFP) include reducing the carbon coating on the LFP particle surface; using different primary particle size grading methods; and increasing the sintering temperature. These methods all increase the compaction density by increasing the size of the LFP primary particles. This, however, reduces electronic conductivity, leading to poor capacity utilization and reduced rate performance. Reducing the carbon coating can also affect the material's processing properties.
[0004] The related patent, "A Method for Preparing High-Density, High-Capacity Lithium Iron Phosphate Cathode Material" (CN114524424A), sinters a lithium iron phosphate precursor in a sagger protected by an inert atmosphere and containing a thermally conductive material, producing the lithium iron phosphate cathode material after sufficient reaction. The patent also describes "A Method for Preparing High-Density Lithium Iron Phosphate" (CN114538401A), which uses a sol-gel method to prepare bulk-doped and carbon-coated lithium iron phosphate particles. These patents have complex production processes and high production costs.
[0005] Summary of the Invention
[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a method for preparing a lithium iron phosphate positive electrode material. The process is simple, and the prepared lithium iron phosphate positive electrode material has a high compaction density and low resistivity.
[0007] The present invention also provides a lithium iron phosphate positive electrode material.
[0008] The present invention also provides the use of the lithium iron phosphate positive electrode material in the preparation of lithium ion batteries.
[0009] The present invention also provides a battery comprising the lithium iron phosphate positive electrode material.
[0010] A method for preparing a lithium iron phosphate positive electrode material according to an embodiment of the first aspect of the present invention comprises the following steps:
[0011] S1. Mixing an iron source, a phosphorus source, a lithium source, a carbon source, an aluminum source, a titanium source, and a solvent to obtain a mixed slurry;
[0012] The titanium source is titanium dioxide;
[0013] S2, grinding the mixed slurry to obtain a first slurry and a second slurry of different finenesses;
[0014] S3. After mixing the first slurry and the second slurry, drying, and calcining under the protection of an inert gas, to obtain the lithium iron phosphate positive electrode material.
[0015] The preparation method according to the embodiment of the present invention has at least the following beneficial effects:
[0016] The preparation method of the embodiment is simple. Through carbothermal reduction, the synergistic effect of carbon, aluminum, and titanium is exploited to rapidly grow some lithium iron phosphate particles during the sintering process, achieving an appropriate particle size distribution. This increases the compacted density of the lithium iron phosphate powder while also reducing its powder resistivity. This preparation method is not only applicable to current iron phosphate systems but also has practical significance for other iron salt systems.
[0017] Aluminum is easily doped into lithium ion sites, resulting in lattice defects and Li vacancies, which can improve the electronic conductivity of the material to a certain extent; the introduction of titanium is conducive to the nano-sizing of primary particles, which can effectively shorten the migration distance of lithium ions and enhance their conductivity; the carbon source forms amorphous carbon under high-temperature inert gas conditions, which is coated on the outer layer of lithium iron phosphate particles, effectively dispersing the lithium iron phosphate particles and preventing the growth of lithium iron phosphate particles, increasing the contact between particles, improving the conductive properties, and increasing the compaction density.
[0018] According to some embodiments of the present invention, the molar ratio of iron to phosphorus in the iron source and the phosphorus source is 1:0.8-1.2.
[0019] According to some embodiments of the present invention, a molar ratio of the iron source to the lithium source is 1:1 to 1.05.
[0020] According to some embodiments of the present invention, the phosphorus source includes at least one of ferric phosphate, ammonium dihydrogen phosphate, ammonium phosphate, lithium dihydrogen phosphate, diammonium hydrogen phosphate, and phosphoric acid, preferably ferric phosphate.
[0021] According to some embodiments of the present invention, the iron source includes at least one of ferric phosphate, ferrous oxalate, iron powder, ferric oxide, and ferric nitrate, preferably ferric phosphate.
[0022] According to some embodiments of the present invention, the lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium dihydrogen phosphate, lithium acetate, and lithium citrate.
[0023] According to some embodiments of the present invention, the aluminum source includes at least one of nano-scale aluminum phosphate and nano-scale aluminum oxide. Specifically, the aluminum source is a nano-scale aluminum source.
[0024] According to some embodiments of the present invention, the amount of the aluminum source added is 0.1% to 1.0% by mass of the iron source, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9% or 1.0%.
[0025] According to some embodiments of the present invention, the titanium source is a nanoscale titanium source.
[0026] According to some embodiments of the present invention, the amount of the titanium source added is 0.1% to 0.7% of the mass of the iron source, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6% or 0.7%.
[0027] According to some embodiments of the present invention, the solid content of the mixed slurry is 25% to 45%, for example, 25%, 30%, 35%, 40% or 45%.
[0028] According to some embodiments of the present invention, the D 50 ≥1μm. Preferably, the D 50 The thickness is 1 μm to 1.4 μm. For example, it can be 1 μm, 1.05 μm, 1.10 μm, 1.15 μm, 1.20 μm, 1.25 μm, 1.30 μm, 1.35 μm or 1.4 μm.
[0029] According to some embodiments of the present invention, the second slurry D 50 ≤0.5μm. Preferably, the D 50 The thickness is 0.3 μm to 0.45 μm. For example, it can be 0.3 μm, 0.33 μm, 0.36 μm, 0.39 μm, 0.42 μm or 0.45 μm.
[0030] According to some embodiments of the present invention, the average particle size of the first slurry is greater than the average particle size of the second slurry, and the mass ratio of the first slurry to the second slurry is 1:1.3 to 2. For example, it can be 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9, or 1:2.
[0031] According to some embodiments of the present invention, the carbon source includes one or more of glucose, polyethylene glycol, sucrose, polyvinyl alcohol, carbon nanotubes, starch, dextrin, and polyvinyl pyrrolidone. Preferably, the carbon source includes glucose and polyethylene glycol; the glucose is added in an amount of 5% to 10% by weight of the iron source; and the polyethylene glycol is added in an amount of 5% to 10% by weight of the iron source. Specifically, the polyethylene glycol includes but is not limited to polyethylene glycol 1000, polyethylene glycol 1500, polyethylene glycol 4000, polyethylene glycol 6000, or polyethylene glycol 10000.
[0032] According to some embodiments of the present invention, the amount of the carbon source added is 10% to 20% of the mass of the iron source, for example, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, or 20%.
[0033] According to some embodiments of the present invention, the solvent is water.
[0034] According to some embodiments of the present invention, the calcination temperature in step S3 is 700° C. to 850° C. For example, it can be 710, 720, 730, 740, 750, 760, 770, 780, 790, 800, 810, 820, 830, 840 or 850° C.
[0035] According to some embodiments of the present invention, the calcination time in step S3 is 6 hours to 25 hours, for example, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24 or 25 hours.
[0036] According to some embodiments of the present invention, the inert gas is at least one of nitrogen and argon.
[0037] According to some embodiments of the invention, the drying comprises spray drying.
[0038] According to some embodiments of the present invention, the inlet air temperature of the spray drying is 180°C to 240°C. For example, it can be 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C or 240°C.
[0039] According to some embodiments of the present invention, the outlet air temperature of the spray drying is 70°C to 120°C, for example, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C.
[0040] A lithium iron phosphate positive electrode material according to an embodiment of the second aspect of the present invention is prepared by the preparation method described in the embodiment of the first aspect.
[0041] The lithium iron phosphate positive electrode material according to the embodiment of the present invention has at least the following beneficial effects:
[0042] The lithium iron phosphate positive electrode material of the embodiment has the advantages of high compaction density and low resistivity.
[0043] According to the third aspect of the present invention, the lithium iron phosphate positive electrode material described in the second aspect of the embodiment is used in the preparation of lithium-ion batteries.
[0044] A battery according to a fourth embodiment of the present invention includes the lithium iron phosphate cathode material as described in the second embodiment. Since the battery adopts all the technical solutions of the lithium iron phosphate cathode material of the above embodiment, it has at least all the beneficial effects brought about by the technical solutions of the above embodiment.
[0045] According to some embodiments of the present invention, the battery further comprises a negative electrode material and an electrolyte.
[0046] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] FIG1 is a SEM image of a lithium iron phosphate cathode material according to Example 2 of the present invention;
[0048] FIG2 is a SEM image of the lithium iron phosphate cathode material of Comparative Example 1 of the present invention;
[0049] FIG3 is a SEM image of the lithium iron phosphate cathode material of Comparative Example 2 of the present invention;
[0050] FIG4 is a SEM image of the lithium iron phosphate positive electrode material of Comparative Example 3 of the present invention. DETAILED DESCRIPTION
[0051] The following will clearly and completely describe the concept and technical effects of the present invention in conjunction with the embodiments to fully understand the purpose, features and effects of the present invention. Obviously, the embodiments described are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0052] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or those recommended by the manufacturer. All reagents or instruments used, if the manufacturer is not specified, are commercially available conventional products.
[0053] In the description of the present invention, if there is a description of first, second, etc., it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the order of the indicated technical features.
[0054] In the description of the present invention, the terms "comprises" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus that includes a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to the process, method, product or apparatus.
[0055] In the following examples, aluminum phosphate dihydrate and titanium dioxide are both nanometer-sized.
[0056] Example 1
[0057] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, the steps of which are as follows:
[0058] S1. Mix iron phosphate and lithium carbonate in a molar ratio of iron phosphate to lithium carbonate of 1:1, add polyethylene glycol 1500 in an amount of 7% by mass of the iron phosphate, add glucose in an amount of 7% by mass of the iron phosphate, add aluminum phosphate dihydrate in an amount of 0.2% by mass of the iron phosphate, add titanium dioxide in an amount of 0.5% by mass of the iron phosphate, and then add an appropriate amount of deionized water to obtain a mixed slurry with a solid content of 30%.
[0059] S2, ball milling the mixed slurry obtained in step S1 to obtain a particle size distribution D 50 =1.3μm first-stage slurry; take 60% of the first-stage slurry mass and continue ball milling to form a particle size distribution D 50 =0.35μm secondary slurry; the primary slurry and the secondary slurry are mixed evenly to obtain a mixture.
[0060] S3. The mixed material obtained in step S2 is spray-dried at an inlet air temperature of 220° C. and an outlet air temperature of 105° C. to obtain a dried material.
[0061] S4. The dried material is first calcined at 800° C. for 6 hours under a nitrogen protective atmosphere, and then naturally cooled and crushed using a jet mill to obtain a lithium iron phosphate positive electrode material.
[0062] Example 2
[0063] This embodiment provides a method for preparing a lithium iron phosphate positive electrode material, the steps of which are as follows:
[0064] S1. Mix iron phosphate and lithium carbonate at a molar ratio of iron phosphate to lithium carbonate of 1:1.05, add polyethylene glycol 1500 in an amount of 7% by mass of the iron phosphate, add glucose in an amount of 7% by mass of the iron phosphate, add aluminum phosphate dihydrate in an amount of 0.8% by mass of the iron phosphate, add titanium dioxide in an amount of 0.208% by mass of the iron phosphate, and then add an appropriate amount of deionized water to obtain a mixed slurry with a solid content of 40%.
[0065] S2, ball milling the mixed slurry obtained in step S1 to obtain a particle size distribution D 50 =1.05μm first-stage slurry; take 65% of the first-stage slurry mass and continue ball milling to form a particle size distribution D 50 =0.42 μm secondary slurry; the primary slurry and the secondary slurry are mixed evenly to obtain a mixture.
[0066] S3. The mixed material obtained in step S2 is spray-dried at an inlet air temperature of 220° C. and an outlet air temperature of 105° C. to obtain a dried material.
[0067] S4. The dried material was first calcined at 750° C. for 10 hours under a nitrogen protective atmosphere, and then naturally cooled and crushed using a jet mill to obtain a lithium iron phosphate positive electrode material.
[0068] Comparative Example 1
[0069] This comparative example provides a preparation method of a lithium iron phosphate positive electrode material, which is basically the same as Example 2, except that aluminum phosphate dihydrate and titanium dioxide are not added.
[0070] Comparative Example 2
[0071] This comparative example provides a preparation method of a lithium iron phosphate positive electrode material, which is basically the same as Example 2, except that aluminum phosphate dihydrate is not added.
[0072] Comparative Example 3
[0073] This comparative example provides a preparation method of a lithium iron phosphate positive electrode material, which is basically the same as Example 2, with the main difference being that titanium dioxide is not added.
[0074] Test example
[0075] 1. The morphology of the lithium iron phosphate positive electrode materials prepared in Example 2 and Comparative Examples 1 to 3 was analyzed using a scanning electron microscope.
[0076] The analysis results are shown in Figures 1 to 4.
[0077] Figure 1 shows lithium iron phosphate prepared by adding aluminum phosphate dihydrate at a rate of 0.8% of the mass of iron phosphate and titanium dioxide at a rate of 0.208% of the mass of iron phosphate; the electron microscope image shows that the particle size matching effect is obvious.
[0078] Figure 2 shows lithium iron phosphate prepared without adding aluminum phosphate dihydrate and titanium dioxide, and its particles exhibit uniform size and morphology;
[0079] FIG3 shows lithium iron phosphate prepared without adding aluminum phosphate dihydrate, and its particles are smaller than those in FIG2 ;
[0080] FIG4 shows lithium iron phosphate prepared without adding titanium dioxide, in which some particles have abnormally grown;
[0081] By comparison, it can be seen that the lithium iron phosphate particles prepared without adding aluminum phosphate dihydrate and titanium dioxide are of uniform size.
[0082] 2. The powder compaction density and powder resistivity of the lithium iron phosphate positive electrode materials prepared in Examples 1 and 2 and Comparative Examples 1 to 3 were tested using a powder compaction device and a powder resistivity tester.
[0083] The test results are shown in Table 1.
[0084] Table 1
[0085] By incorporating aluminum phosphate dihydrate and titanium dioxide, the powder compaction density of the lithium iron phosphate positive electrode material can be significantly increased and its powder resistivity can be reduced. Titanium dioxide has the effect of refining the grains. The raw materials for preparing the lithium iron phosphate in Comparative Example 3 do not contain titanium dioxide, resulting in abnormally large particles and a lack of small particles to fill the gaps, resulting in a lower compaction density than that of Example 2. The raw materials for preparing the lithium iron phosphate in Comparative Example 2 contain titanium dioxide, which leads to particle refinement, resulting in a lower compaction density than that of Comparative Example 1.
[0086] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the scope of knowledge possessed by ordinary technicians in the relevant technical field without departing from the scope of the present invention.
Claims
1. A method for preparing a lithium iron phosphate positive electrode material, characterized in that: The following steps are involved: S1, mixing an iron source, a phosphorus source, a lithium source, a carbon source, an aluminum source, a titanium source and a solvent to obtain a mixed slurry; The titanium source is titanium dioxide; S2, grinding the mixed slurry to obtain a first slurry and a second slurry of different finenesses; S3. After mixing the first slurry and the second slurry, drying, and calcining under the protection of an inert gas, the lithium iron phosphate positive electrode material is obtained.
2. The preparation method according to claim 1, characterized in that: The molar ratio of iron and phosphorus in the iron source and the phosphorus source is 1:0.8-1.2; Preferably, the phosphorus source includes at least one of iron phosphate, ammonium dihydrogen phosphate, ammonium phosphate, lithium dihydrogen phosphate, diammonium hydrogen phosphate and phosphoric acid; Preferably, the iron source includes at least one of ferric phosphate, ferrous oxalate, iron powder, ferric oxide, and ferric nitrate; Preferably, the lithium source includes at least one of lithium hydroxide, lithium carbonate, lithium nitrate, lithium oxalate, lithium dihydrogen phosphate, lithium acetate, and lithium citrate.
3. The preparation method according to claim 1, characterized in that: The aluminum source includes at least one of nano-scale aluminum phosphate and nano-scale aluminum oxide; Preferably, the added amount of the aluminum source is 0.1% to 1.0% of the mass of the iron source.
4. The preparation method according to claim 1, characterized in that: The added amount of the titanium source is 0.1% to 0.7% of the mass of the iron source.
5. The preparation method according to claim 1, characterized in that: The solid content of the mixed slurry is 25% to 45%; Preferably, the D of the first slurry is 50 ≥1μm; Preferably, the second slurry D 50 ≤0.5μm; Preferably, the mass ratio of the first slurry to the second slurry is 1:1.3-2.
6. The preparation method according to claim 1, characterized in that: The carbon source includes one or more of glucose, sucrose, polyvinyl alcohol, carbon nanotubes, starch, dextrin, and polyvinyl pyrrolidone; Preferably, the added amount of the carbon source is 10% to 20% of the mass of the iron source; Preferably, the solvent is water.
7. The preparation method according to claim 1, characterized in that: The calcination temperature in step S3 is 700°C to 850°C; Preferably, the calcination time is 6h to 25h; Preferably, the inert gas is at least one of nitrogen and argon.
8. A lithium iron phosphate positive electrode material, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 7.
9. Use of the lithium iron phosphate positive electrode material described in claim 8 in the preparation of lithium ion batteries.
10. A battery, characterized in that: Including the lithium iron phosphate positive electrode material described in claim 8.
Citation Information
Patent Citations
Phosphate-coated nano-grade lithium iron phosphate cathode material and preparation method thereof
CN102842713A
Low-cost lithium iron phosphate material, and preparation method and application thereof
CN106602060A
Preparation method and application of lithium iron phosphate positive electrode material
CN107814372A
High-compaction lithium iron phosphate material and preparation method thereof
CN111217347A
Preparation method of high-compaction lithium iron phosphate material and lithium iron phosphate material prepared by same
CN112875671A
Cited By
Lithium iron phosphate material as well as preparation method and application thereof
CN119735187A
Lithium iron phosphate positive electrode material, preparation method thereof, positive electrode plate and lithium ion battery
CN119976780A
Preparation method of lithium iron phosphate material with high compaction density
CN120039851A
Uniform carbon-coated lithium iron phosphate positive electrode material and preparation method thereof
CN120149384A
High-compaction and high-capacity lithium iron phosphate material as well as preparation method and application thereof
CN120208182A