Inorganic-coated sand, production method therefor, inorganic-coated sand composition, and casting mold

The use of metasilicate hydrate and amorphous SiO2 in the inorganic binder layer addresses the stability and strength issues of conventional inorganic coated sands, enhancing storage stability and mechanical strength for improved mold performance.

WO2024253166A1PCT designated stage expired Publication Date: 2024-12-12KAO CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/020736
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-06-06
Filing Date
2024-06-06
Publication Date
2024-12-12

AI Technical Summary

Technical Problem

Conventional inorganic coated sands suffer from poor storage stability and insufficient mechanical strength, leading to issues in mold manufacturing and performance.

Method used

A dry inorganic coated sand with a refractory aggregate and an inorganic binder layer made of metasilicate hydrate and amorphous SiO2, having a melt viscosity between 32 mPa·s and 150 mPa·s at 80°C, a hydration amount of metasilicate hydrate between 6 and 8, and a melting point of 40°C to 60°C, which improves both storage stability and mechanical strength.

Benefits of technology

The solution provides a balance between storage stability and mechanical strength, ensuring the inorganic coated sand remains dry and maintains mold integrity during storage and use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure 00000035_0000
    Figure 00000035_0000
Patent Text Reader

Abstract

This inorganic-coated sand is dry inorganic-coated sand comprising a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate. The inorganic binder layer comprises a metasilicate hydrate and fine particles including amorphous SiO2, and an inorganic binder forming the inorganic binder layer has a melt viscosity at 80°C of 32-150 mPa·s.
Need to check novelty before this filing date? Find Prior Art

Description

Inorganic coated sand and its manufacturing method, inorganic coated sand composition, and casting mold

[0001] The present invention relates to an inorganic coated sand and a method for producing the same, an inorganic coated sand composition, and a casting mold.

[0002] Known molds used in casting include those obtained by molding a desired shape using inorganic coated sand having a refractory aggregate and an inorganic binder layer formed on the surface of the refractory aggregate. Technologies related to such inorganic coated sand include those described in Patent Document 1 (WO 2018 / 097180), Patent Document 2 (JP 53-025803 B), and Patent Document 3 (JP 2020-11296 A).

[0003] Patent Document 1 discloses coated sand in a dry state having fluidity at room temperature, in which the surface of a refractory aggregate is covered with a coating layer containing water glass, and the coating layer contains spherical particles.

[0004] In Patent Document 2, an alkali metasilicate solution prepared by adding a caustic alkali to water glass is added to refractory particles such as silica sand and kneaded together, or an alcohol is further added during kneading, so that crystalline alkali silicate is deposited and adhered to the surface of the refractory particles such as silica sand, and then SiO generated during Fe-Si refining is added to the surface of the refractory particles. 2 The document describes a method for producing a mold, which comprises heating a powder-mixed sand prepared by adding and mixing fine dust mainly composed of the above-mentioned crystalline alkali silicate to a temperature at least equal to or higher than the melting point of the above-mentioned crystalline alkali silicate, and hardening the sand.

[0005] Patent Document 3 discloses dry inorganic coated sand having a refractory aggregate and an inorganic binder layer formed on the surface of the refractory aggregate, wherein the inorganic binder layer contains at least one metasilicate hydrate selected from sodium metasilicate pentahydrate and sodium metasilicate nonahydrate.

[0006] International Publication No. 2018 / 097180 Japanese Patent Publication No. 53-025803 Japanese Patent Application Laid-Open No. 2020-11296

[0007] According to the inventors' investigations, the conventional inorganic-coated sands disclosed in Patent Documents 1 to 3 tend to become wet during storage, which can make it impossible to manufacture molds thereafter. On the other hand, it has been found that even if the storage stability of the inorganic-coated sand is good, the mechanical strength of molds made using the inorganic-coated sand may not be sufficient. In other words, the present invention relates to achieving both higher storage stability for dry inorganic-coated sand and improved mechanical strength of molds made from the coated sand after storage.

[0008] The present inventors have conducted research into achieving both storage stability in inorganic coated sand and the mechanical strength of molds made from the coated sand after storage. As a result, they have found that it is effective to set the melt viscosity of the inorganic binder in the inorganic binder layer within a specific range, to set the amount of water of hydration of the metasilicate hydrate in the inorganic binder layer within a specific range, and to ensure that the fusion point of the inorganic coated sand, as measured in accordance with JACT Test Method C-1 Fusion Point Test Method, is 40°C or higher and 60°C or lower, and have completed the present invention.

[0009] According to the present invention, there is provided a dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 The inorganic coated sand contains fine particles, and the inorganic binder constituting the inorganic binder layer has a melt viscosity at 80°C of 32 mPa·s or more and 150 mPa·s or less.

[0010] According to the present invention, there is also provided a dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is composed of metasilicate hydrate and amorphous SiO 2 There is provided inorganic coated sand containing fine particles, in which the amount of water of hydration of the metasilicate hydrate is 6 or more and 8 or less.

[0011] According to the present invention, there is also provided a dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is composed of metasilicate hydrate and amorphous SiO 2 There is provided inorganic coated sand which contains fine particles and has a fusion point of 40°C or higher and 60°C or lower according to JACT Test Method C-1 Fusion Point Test Method.

[0012] The present invention also provides an inorganic coated sand composition containing the above inorganic coated sand.

[0013] The present invention also provides a casting mold using the above inorganic coated sand.

[0014] The present invention also provides a casting mold using the above inorganic coated sand composition.

[0015] Furthermore, according to the present invention, there is provided a method for producing dry inorganic-coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, the method comprising: a step (1) of mixing the refractory aggregate, metasilicate nonahydrate, and metasilicate pentahydrate to obtain a mixture; and a step (2) of cooling the mixture, wherein the step (1) comprises mixing at a temperature equal to or higher than the melting point of a mixture consisting of the metasilicate nonahydrate and the metasilicate pentahydrate, and the step (2) comprises cooling to a temperature below the melting point of the mixture consisting of the metasilicate nonahydrate and the metasilicate pentahydrate.

[0016] The present invention also provides a method for producing the above-mentioned inorganic coated sand, comprising the step (3) of mixing the refractory aggregate with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate.

[0017] According to the present invention, it is possible to provide inorganic coated sand that can improve the mechanical strength of a mold using the inorganic coated sand while maintaining good storage stability of the inorganic coated sand.

[0018] Hereinafter, embodiments of the present invention will be described. Furthermore, in this specification, unless otherwise specified, "A to B" indicating a numerical range represents a range from A to B, and includes both end values. Furthermore, the components and elements described in each embodiment can be combined as appropriate as long as the effects of the invention are not impaired.

[0019] <Inorganic Coated Sand> The inorganic coated sand of this embodiment is a dry inorganic coated sand containing a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, and the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 The inorganic binder layer contains fine particles and satisfies at least one of the following conditions (i) to (iii): (i) the inorganic binder constituting the inorganic binder layer has a melt viscosity at 80°C of 32 mPa·s or more and 150 mPa·s or less, (ii) the amount of water of hydration of the metasilicate hydrate is 6 to 8, and (iii) the inorganic coated sand has a fusion point of 40°C or more and 60°C or less, as measured in accordance with the JACT Test Method C-1 Fusion Point Test. This allows for both good storage stability of the dry inorganic coated sand containing a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, and good mechanical strength of the molds using the same.

[0020] First, in the inorganic coated sand of this embodiment, the metasilicate constituting the inorganic binder layer is hydrated. This improves the crystallinity of the inorganic binder layer, and the inorganic coated sand is in a dry state, which makes it excellent in fluidity at room temperature and improves the strength of the mold using this. Furthermore, when the inorganic binder layer is amorphous SiO 2 By further including the contained fine particles, the particles of the inorganic coated sand are bonded to each other by amorphous SiO 2 Since the particles contained can be more firmly bound, the strength of the mold can be easily improved.

[0021] In addition, the inorganic coated sand of this embodiment has the following advantages: (i) the inorganic binder constituting the inorganic binder layer has a melt viscosity at 80°C of 32 mPa·s or more and 150 mPa·s or less, so that when the inorganic binder layer melts to form an adhesive layer, the inorganic binder aggregates at the adhesive points between the inorganic coated sand particles, thereby contributing to an improvement in the mechanical strength of the mold using the inorganic coated sand, and also contributing to an improvement in the mechanical strength of the mold using the inorganic coated sand, since the inorganic binder aggregates at the adhesive points between the inorganic coated sand particles when the inorganic binder layer melts to form an adhesive layer. 2 It is believed that this can prevent the reactivity with other components, such as the contained fine particles, from becoming too high and becoming easily wet.

[0022] On the other hand, the inorganic coated sand of this embodiment can have (ii) the amount of water of hydration of the metasilicate hydrate be 6 or more and 8 or less.

[0023] Here, the present inventors have found that the amount of hydration water of metasilicate hydrate affects the mechanical strength of the mold and the storage stability of the inorganic-coated sand. Specifically, it has been found that the greater the amount of hydration water of metasilicate hydrate, the more likely the inorganic-coated sand becomes wet during storage, while the mold strength immediately after the inorganic-coated sand is produced tends to be higher. Although the details of the mechanism are not clear, it is believed that the greater the amount of hydration water of metasilicate hydrate, the more likely the inorganic-coated sand is to become wet during storage, while the mold strength immediately after the inorganic-coated sand is produced tends to be higher. 2 It was speculated that the reactivity with other components, such as the contained fine particles, would increase, resulting in a tendency for the material to become wet, but that the mechanical strength would be improved. Therefore, in the inorganic-coated sand of this embodiment, the amount of water of hydration of the metasilicate hydrate is preferably 6 or more, thereby improving the mechanical strength of the mold, while the amount of water of hydration of the metasilicate hydrate is preferably 8 or less, thereby improving the storage stability of the inorganic-coated sand while maintaining good mechanical strength of the mold. More specifically, even when compared with inorganic-coated sand using the same refractory aggregate, the inorganic-coated sand of this embodiment, when the amount of water of hydration of the metasilicate hydrate is 6 or more and 8 or less, can achieve a higher level of balance between the mechanical strength and storage stability of the mold than inorganic-coated sand using a metasilicate hydrate with a water of hydration of more than 6 or more and 8 or less.

[0024] The amount of water of hydration of the metasilicate hydrate can be adjusted by the method described below.

[0025] The amount of water of hydration of metasilicate hydrate in inorganic-coated sand can be confirmed by the following method. [1] Measurement of the amount of water (%) (A) in inorganic-coated sand The amount of water (%) A in inorganic-coated sand can be measured by either method 1 or 2 below. (Method 1) A crucible that has been preheated and weighed is filled with amorphous SiO 2 10 g of inorganic coated sand before adding additives such as fine particles is weighed and placed in a container, and the amount of mass loss (%) after heating at 900°C for 1 hour is used to calculate the moisture content (%) (A) in the inorganic coated sand. A = [(M1 - M2) / M3] x 100 (M1: total mass (g) of the crucible and inorganic coated sand before firing, M2: total mass (g) of the crucible and inorganic coated sand after firing, M3: mass (g) of the inorganic coated sand before firing) (Method 2) Amount of amorphous SiO2 is measured using a differential thermal-thermogravimetric simultaneous analyzer (e.g., Thermo plus EVO2 TG-DTA8122 (manufactured by Rigaku Corporation)). 2 The inorganic coated sand before adding additives such as fine particles is measured under the following conditions, and the weight loss (%) (A) at 200°C is calculated. <Measurement conditions> Measurement atmosphere: Air Sample amount: Approximately 8 mg Heating rate: 10.0°C / min

[0026] [2] Measurement of solid content (%) of metasilicate hydrate (B) The solid content (%) of metasilicate hydrate (B) in inorganic coated sand can be measured by either method 1 or 2 below. (Method 1) Amorphous SiO 2100 g of inorganic coated sand before adding additives such as fine particles is weighed, immersed in 200 mL or more of water or hot water, and stirred for at least 1 hour to extract metasilicate hydrate. The refractory aggregate is removed from the resulting extract by filtration, and the water is removed by vacuum distillation using a rotary evaporator at 40°C and an internal pressure of 15 mmHg or less. The resulting mixture is then dried by heating at a temperature of 120°C to 180°C for 1 to 3 hours, and the weight of the dried product is weighed. The dry solid content (%) (B) of metasilicate hydrate in the inorganic coated sand is calculated. B = (M12 / M11) x 100 (M11: mass (g) of inorganic coated sand, M12: weight (g) of the dried product) (Method 2) Measurement is performed according to the following procedure. <Preparation of Extract> Amorphous SiO 2 30 g of inorganic-coated sand before adding additives such as fine particles was placed in a 200 ml tall beaker, 100 ml of pure water was added, and the mixture was stirred for 25 minutes using a magnetic stirrer to prepare an extract. The supernatant of the extract was then filtered through a membrane filter (pore size: 0.45 μm), and 10 ml of the filtrate was placed in a 100 ml beaker. <Titration> 20 ml of 0.1 mol / L HCl aqueous solution was added to the 100 ml beaker containing the 10 ml of filtrate. Then, while stirring with a magnetic stirrer, 0.1 mol / L NaOH aqueous solution was titrated using an automatic titrator (e.g., Eco Titrator (Metrohm)). The titration amount X (ml) at which the pH reached 7 was measured using a pH meter. <Calculation of metasilicate solid content> Acid consumption Y (mol) = ([Amount of HCl aqueous solution (ml)] - [Titer amount X (ml)]) / 1000 x [Concentration of HCl aqueous solution (mol / l)] = (20 - X) / 1000 x 0.1 B = ([Amount of acid consumption Y (mol)] x 10 x [Molecular weight of metasilicate anhydride] / [Na valence]) / (Amount of inorganic coated sand (g)) x 100 = (Y x 10 x Molecular weight of metasilicate anhydride / 2) / 30 x 100

[0027] [3] Calculation of the amount of water of hydration of metasilicate hydrate The amount of water of hydration of metasilicate hydrate is calculated by applying the amount of water (%) (A) in the obtained inorganic coated sand and the solid content (%) (B) of metasilicate hydrate to the following formula: Amount of water of hydration of metasilicate hydrate = [(A) / molecular weight of water] / [(B) / molecular weight of metasilicate anhydride]

[0028] The inorganic coated sand is in a dry state. Dry coated sand means coated sand for which a measurement value can be obtained when measuring the dynamic angle of repose regardless of the moisture content. The dynamic angle of repose is preferably 80° or less, more preferably 45° or less, and even more preferably 30° or less.

[0029] The dynamic angle of repose can be measured by the following method. (Method for measuring the dynamic angle of repose) Coated sand is placed in a cylindrical transparent plastic bottle to half its volume, and the bottle is held with its axis horizontal and rotated around the horizontal axis at a constant speed. The inclined surface of the coated sand layer flowing inside the cylinder becomes flat. The angle formed between this inclined surface and the horizontal plane is measured. Note that if the coated sand does not flow inside the cylinder, or if it flows but the inclined surface of the coated sand layer does not form a flat surface, and as a result the dynamic angle of repose cannot be measured, the coated sand is in a wet state.

[0030] The inorganic coated sand is specifically composed of inorganic coated sand particles, and the refractory aggregate is specifically composed of refractory aggregate particles. From the viewpoint of improving fluidity and further improving the fillability into a molding die, the inorganic coated sand is preferably spherical. Here, "spherical" inorganic coated sand refers to sand having a round, ball-like shape. More specifically, from the viewpoints of improving fluidity, mold quality, and mold strength, and of ease of mold formation, the sphericity of the inorganic coated sand is preferably 0.75 or more, more preferably 0.80 or more, and even more preferably 0.82 or more. Furthermore, the upper limit of the sphericity is specifically 1 or less. In this embodiment, the sphericity of the inorganic coated sand specifically matches the sphericity of the refractory aggregate.

[0031] Here, the sphericity of the inorganic coated sand is determined by analyzing an image (photograph) of the particle obtained by an optical microscope or a digital scope (for example, VH-8000 model, manufactured by Keyence Corporation) to determine the area of ​​the projected cross section of the particle and the perimeter of the cross section, and then calculating the sphericity = [area of ​​the projected cross section of the particle (mm 2 The particle diameter can be determined by calculating the perimeter (mm) of a circle having the same area as the particle diameter (mm) / the perimeter (mm) of the projected cross section of the particle, and averaging the values ​​obtained for any 50 particles.

[0032] The average particle size of the inorganic-coated sand is preferably 0.05 mm or more, more preferably 0.1 mm or more, from the viewpoints of improving mold quality and mold strength, and ease of mold production. Furthermore, when the average particle size of the inorganic-coated sand is equal to or greater than the above-mentioned lower limit, the amount of coating layer used during mold production can be reduced, making it easier to regenerate the inorganic-coated sand. From the viewpoints of improving mold quality and mold strength, and ease of mold production, the average particle size of the inorganic-coated sand is preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. Furthermore, when the average particle size of the inorganic-coated sand is equal to or less than the above-mentioned upper limit, the porosity is reduced during mold production, making it easier to increase mold strength.

[0033] In this embodiment, the average particle size of the inorganic coated sand and the refractory aggregate described later can be specifically measured by the following method.

[0034] (Method for Measuring Average Particle Diameter) When the sphericity of a particle from a projected cross section is 1, the diameter (mm) is measured. On the other hand, when the sphericity is <1, the major axis diameter (mm) and minor axis diameter (mm) of randomly oriented particles are measured to calculate (major axis diameter + minor axis diameter) / 2, and the average of the values ​​obtained for 100 randomly selected particles is used as the average particle diameter (mm). The major axis diameter and minor axis diameter are defined as follows: When a particle is stabilized on a flat surface and its projected image on the flat surface is sandwiched between two parallel lines, the width of the particle at the smallest distance between the parallel lines is called the minor axis diameter, and the distance when the particle is sandwiched between two parallel lines perpendicular to the parallel lines is called the major axis diameter. The major axis diameter and minor axis diameter of a particle can be determined by taking an image (photograph) of the particle using an optical microscope or a digital scope (e.g., Keyence Corporation, VH-8000 model) and analyzing the obtained image.

[0035] Furthermore, the inorganic coated sand (iii) may have a fusion point of 40°C or higher and 60°C or lower, as determined in accordance with JACT Test Method C-1 Fusion Point Test for Inorganic Coated Sand. The fusion point of the inorganic coated sand may be 40°C or higher, preferably 42°C or higher, from the viewpoint of facilitating the molding of molds with complex shapes. Furthermore, from the viewpoint of improving mold strength, the fusion point may be 60°C or lower, more preferably 58°C or lower, even more preferably 55°C or lower, and particularly preferably 50°C or lower. The fusion point (°C) of the inorganic coated sand can be measured in accordance with JACT Test Method C-1 Fusion Point Test ("Test Methods for Molds and Mold Materials," published in May 1999 by the Japan Small and Medium Enterprise Agency, Information and Technology Department, Technical Support Division).

[0036] Each component of the inorganic coated sand will be described below.

[0037] [Refractory Aggregate] The refractory aggregate according to this embodiment may be natural sand or artificial sand. Examples of natural sand include silica sand, chromite sand, zircon sand, olivine sand, and alumina sand, which are mainly composed of quartz. Examples of artificial sand include synthetic mullite sand and SiO 2 SiO 2 Al-based foundry sand 2 O 3Al, the main component of which is 2 O 3 Foundry sand of the SiO 2 / Al 2 O 3 Foundry sand of the SiO 2 / MgO-based foundry sand, SiO 2 / Al 2 O 3 / ZrO 2 Foundry sand of the SiO 2 / Al 2 O 3 / Fe 2 O 3 Examples of suitable foundry sand include foundry sand derived from refractory aggregates and slag. Here, the term "main component" refers to the component that is most abundant among the components contained in the sand. Artificial sand refers to foundry sand that is not naturally occurring, but is made by artificially preparing metal oxide components and melting or sintering them. Also usable are recycled sand made from recovered used refractory aggregates and recycled sand that has been subjected to a recycling process. These may be used alone or in combination of two or more types.

[0038] The refractory aggregate according to this embodiment is made of SiO from the viewpoint of improving mold strength. 2 and Al 2 O 3 The refractory aggregate according to the present embodiment is preferably artificial sand from the viewpoint of improving mold strength, and among the artificial sands, synthetic mullite sand, SiO 2 Al-based foundry sand 2 O 3 Foundry sand of the SiO 2 / Al 2 O 3 Foundry sand of the SiO 2 / Al 2 O 3 / ZrO 2 System foundry sand and SiO 2 / Al 2 O 3 / Fe 2 O 3 It is preferable to use at least one type selected from the group consisting of foundry sands of the same type.

[0039] SiO in refractory aggregate 2 , Al 2 O 3, Fe 2 O 3 The content of each component can be measured using known analytical methods, such as X-ray fluorescence. X-ray fluorescence can be analyzed by the following method. Refractory aggregate is adjusted to 0.1 μm or less using a vibration mill and heated at 1050°C for 1 hour. 5 g of lithium tetraborate and 0.5 g of refractory aggregate are then mixed and heated at 1200°C for 10 minutes to melt the mixture, and then cooled to prepare a glassy sample (glass bead method). The sample is subjected to X-ray fluorescence analysis using a ZSX Primus II X-ray fluorescence analyzer (manufactured by Rigaku Corporation) using the fundamental parameter (FP) method.

[0040] The amorphization degree of the refractory aggregate is preferably 30% or more, more preferably 50% or more, even more preferably 65% ​​or more, and even more preferably 80% or more, from the viewpoint of making the surface of the aggregate smoother and further improving mold strength, and from the viewpoint of obtaining low thermal expansion. The upper limit of the amorphization degree of the refractory aggregate is not limited, but may be, for example, 100% or less, or 99% or less.

[0041] There are various methods for controlling the degree of amorphization of refractory aggregate, but it is generally preferable to use a manufacturing method that rapidly cools the molten material. For example, there is a method in which the raw material is melted and rapidly cooled by air crushing, or a method in which it is treated in a flame and rapidly cooled. In either case, the cooling method may be selected appropriately at various speeds depending on the material and particle size. Another possible method is to amorphize a material that has been crystallized by heat treatment and cooling treatment.

[0042] The degree of amorphization of a refractory aggregate can be determined by the X-ray diffraction method shown below. (X-ray Diffraction Method) The refractory aggregate is pulverized in a mortar and then compressed onto an X-ray glass holder of a powder X-ray diffractometer for measurement. The powder X-ray diffractometer is a MultiFlex (CuKα radiation source, 40 kV tube voltage, 40 mA tube current) manufactured by Rigaku Denki Co., Ltd., and is measured at a scanning interval of 0.01°, a scanning speed of 2° / min, and slits DS1, SS1, and RS0.3 mm in the range of 2θ = 5° to 90°. A straight line is drawn between the X-ray intensities on the low-angle and high-angle sides in the range of 2θ = 10° to 50°, and the area under the line is used as the background. The degree of crystallinity is calculated using the software provided with the instrument and subtracted from 100 to obtain the degree of amorphization. Specifically, for the area above the background, the amorphous peak (halo) and each crystalline component are separated by curve fitting, and the area of ​​each is determined, and the degree of amorphousness (%) is calculated using the following formula: degree of amorphousness (%) = (area of ​​halo) / (area of ​​crystalline component + area of ​​halo) × 100

[0043] The refractory aggregate is preferably spherical from the viewpoint of improving the fluidity of the inorganic coated sand and further improving the fillability into a mold. The preferred range of sphericity of the refractory aggregate is the same as that of the inorganic coated sand. The sphericity of the refractory aggregate can be measured in the same manner as that of the inorganic coated sand.

[0044] The preferred range of the average particle size of the refractory aggregate is the same as that of the inorganic coated sand. The average particle size of the refractory aggregate can be measured in the same manner as that of the inorganic coated sand.

[0045] [Inorganic Binder Layer] The inorganic binder layer is formed on the surface of the refractory aggregate and serves as a coating layer that covers the surface of the refractory aggregate. However, "covering the surface" does not necessarily mean that the layer is continuous, and may include discontinuous regions.

[0046] The inorganic binder layer contains an inorganic binder, and is composed of metasilicate hydrate and amorphous SiO 2 The inorganic binder layer is composed of fine particles as an essential component. Specifically, for example, the inorganic binder layer may contain metasilicate hydrate, amorphous SiO 2A layer coated with the mixed fine particles; a layer coated with the metasilicate hydrate and amorphous SiO 2 A layer further coated with fine particles containing the compound; or a layer coated with a mixture of metasilicate hydrate and amorphous silica and then coated with amorphous SiO 2 The fine particles contained therein may be further coated as a layer.

[0047] The amount of the inorganic binder layer contained in the inorganic-coated sand is, for example, 0.1 parts by mass or more, preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and still more preferably 2 parts by mass or more, relative to 100 parts by mass of the refractory aggregate, from the viewpoint of obtaining a high-strength casting mold. The amount of the inorganic binder layer contained in the inorganic-coated sand is, for example, 15 parts by mass or less, preferably 10 parts by mass or less, and more preferably 8 parts by mass or less, relative to 100 parts by mass of the refractory aggregate, from the viewpoint of obtaining a high-strength casting mold.

[0048] The water content (including water of crystallization) in the inorganic binder layer contained in the inorganic-coated sand is preferably 75 parts by mass or more, more preferably 80 parts by mass or more, and even more preferably 85 parts by mass or more, per 100 parts by mass of metasilicate (anhydrous equivalent), from the viewpoints of obtaining a high-strength casting mold and easily manufacturing the mold; and from the viewpoints of improving fluidity and further improving mold fillability, is preferably 130 parts by mass or less, more preferably 125 parts by mass or less, and even more preferably 120 parts by mass or less.

[0049] Hereinafter, the components constituting the inorganic binder layer of this embodiment will be described.

[0050] (Inorganic Binder) The inorganic binder functions to firmly bind the foundry sand particles together to obtain the desired mold when the inorganic-coated sand is used to form the mold. The inorganic binder is also one of the components constituting the inorganic binder layer. The inorganic binder includes, for example, a water-soluble silicate compound, preferably at least one selected from sodium silicate and sodium metasilicate. The inorganic binder may further include one containing a water-soluble silicate compound other than those mentioned above as the main component. Specific examples of silicate compounds other than sodium silicate and sodium metasilicate include potassium silicate, potassium metasilicate, lithium silicate, and ammonium silicate.

[0051] The melt viscosity of the inorganic binder at 80°C is 32 mPa·s or more, preferably 35 mPa·s or more, from the viewpoint of improving the mechanical strength of the mold, while the melt viscosity of the inorganic binder at 80°C is 150 mPa·s or less, preferably 120 mPa·s or less, from the viewpoint of improving the storage stability of the inorganic-coated sand while maintaining good mechanical strength of the mold.

[0052] The melt viscosity of the inorganic binder at 80°C was measured using a rheometer, a parallel plate (PP60) was used as a jig, and the temperature was set at 80°C and the shear rate was 100 s ―1 This can be done under the following conditions.

[0053] (Metasilicate hydrate) Metasilicate hydrate is one of the components constituting the inorganic binder layer and also one of the components constituting the inorganic binder. The use of metasilicate hydrate is preferable because it can improve the crystallinity of the inorganic binder layer and furthermore, the inorganic coated sand becomes a dry state, resulting in excellent room temperature fluidity. Furthermore, the use of metasilicate hydrate allows the inorganic binder layer to be formed on the surface of the refractory aggregate without being dissolved in water. That is, in the process of producing the inorganic coated sand, more specifically, in the process of mixing the refractory aggregate and the inorganic binder, there is no need to use an aqueous solution of metasilicate hydrate, so the water removal step can be omitted, thereby simplifying the production method. Furthermore, because the metasilicate in the inorganic binder layer is a hydrate, there is no need to ventilate the mold with water vapor to harden it, thereby simplifying the equipment. The metasilicate hydrate can also be produced by using a mixture of metasilicate hydrate crystals, water glass, caustic alkali, and water in a specific ratio, a mixture of metasilicate anhydride and water in a specific ratio, a mixture of metasilicate pentahydrate and water in a specific ratio, or a metasilicate melt obtained by volatilizing a specific amount of water from a melt of metasilicate nonahydrate. These raw materials can also be added separately to a refractory aggregate to form a metasilicate hydrate composition on the surface of the refractory aggregate. Note that the metasilicate in this embodiment refers to a silicate containing SiO 2 / Na 2 It refers to a compound having a mol ratio of 0.9 to 1.1.

[0054] Specific examples of water glass include one or more types selected from the group consisting of sodium silicates No. 1 to No. 5. Here, sodium silicate is SiO 2 / Na 2 Sodium silicate Nos. 1 to 3 are also specified in the group standard (implementation date: March 1, 2022) created by the Sodium Silicate Committee of the Japan Inorganic Chemicals Association. 2 / Na 2 The molar ratio of sodium silicate No. 1 to SiO is specifically as follows: 2 / Na 2Molar ratio of Sodium silicate No. 2:SiO 2 / Na 2 Molar ratio of sodium silicate No. 3 to SiO 2 / Na 2 Molar ratio of Sodium silicate No. 4:SiO 2 / Na 2 Molar ratio of Sodium silicate No. 5:SiO 2 / Na 2 Molar ratio of SiO = 3.6 to 3.8. Also, by mixing two or more types of sodium silicate, 2 / Na 2 The molar ratio of O may be adjusted to a desired level. The water glass is preferably at least one selected from sodium silicate No. 1 and sodium silicate No. 2.

[0055] In this embodiment, the amount of water of hydration of the metasilicate hydrate is 6 or more and 8 or less. By setting the amount within this range, it is possible to obtain good storage stability of the inorganic coated sand while improving the mechanical strength of the mold using the same. Furthermore, by setting the amount of water of hydration of the metasilicate hydrate to be equal to or more than the above-mentioned lower limit, it is possible to improve the mechanical strength of the mold while maintaining good storage stability. On the other hand, by setting the amount of water of hydration of the metasilicate hydrate to be equal to or less than the above-mentioned upper limit, it is possible to improve the storage stability while maintaining good mechanical strength of the mold.

[0056] The salt of metasilicate hydrate is preferably an alkali metal, and more preferably one or more selected from lithium, sodium, and potassium, more preferably at least one of sodium and potassium, and even more preferably sodium.

[0057] From the viewpoints of improving the mold strength and improving the surface shape of the mold, the content of metasilicate hydrate in the inorganic binder layer is preferably 25% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, and particularly preferably 40% by mass or more, based on the total mass of the inorganic binder layer. Also, from the viewpoint of improving the surface shape of the mold, the content of metasilicate hydrate in the inorganic binder layer is preferably 95% by mass or less, more preferably 90% by mass or less, based on the total mass of the inorganic binder layer.

[0058] The content of metasilicate (anhydride equivalent) in the inorganic binder is preferably 11% by mass or more, more preferably 45% by mass or more, from the viewpoint of improving the storage stability of the inorganic coated sand, while it is preferably 56% by mass or less, more preferably 48% by mass or less, from the viewpoint of improving the mold strength.

[0059] From the viewpoints of improving mold strength and improving the surface shape of the mold, the content of metasilicate hydrate in the inorganic-coated sand is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.5 parts by mass or more, still more preferably 0.8 parts by mass or more, and especially preferably 1 part by mass or more, per 100 parts by mass of the refractory aggregate. From the viewpoint of improving the fillability into the molding die, the content of metasilicate hydrate in the inorganic-coated sand is preferably 9 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, and even more preferably 4 parts by mass or less, per 100 parts by mass of the refractory aggregate.

[0060] (amorphous SiO 2 Containing fine particles) Amorphous SiO 2 The contained fine particles are used because of their high reactivity with metasilicate hydrate, which makes it easier to improve the mechanical strength. 2 The particulates contained include precipitated silica, pyrogenic silica produced in an electric arc or by flame hydrolysis, ZrSiO 4Examples of silica include silica produced by thermal decomposition of silica, silica produced during the production of Fe—Si, silica produced by oxidation of metallic silicon with an oxygen-containing gas, and spherical particles of quartz glass powder produced from crystalline quartz by melting and subsequent rapid cooling. These can naturally be used alone, or two or more types can be used in combination.

[0061] Amorphous SiO 2 The degree of amorphousness of the contained fine particles is determined by the degree of amorphous SiO 2 From the viewpoint of more firmly binding via the contained fine particles, the content is preferably 80% or more, more preferably 90% or more, even more preferably 93% or more, still more preferably 95% or more, and particularly preferably 98% or more. 2 There is no upper limit to the degree of amorphization of the contained fine particles, but it is, for example, 100% or less, and may be 99.8% or less, or may be 99% or less.

[0062] Amorphous SiO 2 The degree of amorphousness of the contained fine particles can be determined by the same X-ray diffraction method as that for the refractory aggregate.

[0063] Amorphous SiO 2 The contained fine particles are preferably in the form of particles. 2 The average particle size of the contained fine particles is preferably 0.1 μm or more, more preferably 0.3 μm or more, from the viewpoint of improving mold strength per unit mass and improving handleability. 2 The average particle size of the contained fine particles is preferably 2.0 μm or less, more preferably 1.0 μm or less, even more preferably 0.8 μm or less, and even more preferably 0.6 μm or less. 2 The average particle size of the contained fine particles can be determined from images observed with a scanning electron microscope, and various image analysis methods can be used for this purpose. Irregular particle selection can also be performed as a pretreatment. For example, amorphous SiO 2 After determining the contained fine particles, any amorphous SiO 2100 particles were selected from the contained particles, and their particle diameters were measured. A total of 20 amorphous SiO particles were selected, consisting of 10 particles counted from the largest particle diameter and 10 particles counted from the smallest particle diameter. 2 80 amorphous SiO particles excluding contained fine particles 2 The average particle size of the contained fine particles is determined by the amorphous SiO 2 It can be the average particle size of the contained fine particles.

[0064] Amorphous SiO 2 SiO in the contained fine particles 2 From the viewpoint of improving mold strength, the mass % is preferably 50 mass % or more, more preferably 70 mass % or more, even more preferably 80 mass % or more, particularly preferably 85 mass % or more, and even more particularly preferably 90 mass % or more. 2 SiO in the contained fine particles 2 The mass % can be measured by the X-ray fluorescence method in the same manner as for the refractory aggregate.

[0065] Amorphous SiO 2 The content of the contained fine particles is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 3 parts by mass or less, relative to 100 parts by mass of the refractory aggregate, from the viewpoints of improving the mold strength and improving the mold surface shape while obtaining storage stability, and suppressing dust scattering. 2 The content of the contained fine particles is preferably 25 parts by mass or more, more preferably 30 parts by mass or more, and preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 145 parts by mass or less, per 100 parts by mass of metasilicate (anhydrous equivalent).

[0066] (Other) The inorganic binder layer is made of metasilicate hydrate and amorphous SiO 2 As a component other than the contained fine particles, the above-mentioned amorphous SiO 2 The toner may contain other additives such as inorganic particles other than the fine particles, coupling agents, lubricants, and mold release agents.

[0067] Amorphous SiO 2The inorganic particles other than the contained fine particles are not particularly limited, but examples thereof include carbonates such as crystalline silica, silicon, zinc carbonate, basic zinc carbonate, iron carbonate, manganese carbonate, copper carbonate, aluminum carbonate, barium carbonate, magnesium carbonate, calcium carbonate, lithium carbonate, potassium carbonate, and sodium carbonate; borates such as sodium tetraborate, potassium tetraborate, lithium tetraborate, ammonium tetraborate, calcium tetraborate, strontium tetraborate, silver tetraborate, sodium metaborate, potassium metaborate, lithium metaborate, ammonium metaborate, calcium metaborate, silver metaborate, copper metaborate, lead metaborate, and magnesium metaborate; sodium sulfate, potassium sulfate, Examples of suitable inorganic salts include sulfates such as lithium sulfate, magnesium sulfate, calcium sulfate, strontium sulfate, barium sulfate, titanium sulfate, aluminum sulfate, zinc sulfate, and copper sulfate; phosphates such as sodium phosphate, sodium hydrogen phosphate, potassium phosphate, potassium hydrogen phosphate, lithium phosphate, lithium hydrogen phosphate, magnesium phosphate, calcium phosphate, titanium phosphate, aluminum phosphate, and zinc phosphate; hydroxides such as lithium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, barium hydroxide, aluminum hydroxide, and zinc hydroxide; and oxides of silicon, zinc, magnesium, aluminum, calcium, lithium, copper, iron, boron, and zirconium.

[0068] Coupling agents include, but are not limited to, silane coupling agents, zirconium coupling agents, titanium coupling agents, etc. Lubricants include, but are not limited to, waxes such as paraffin wax, synthetic polyethylene wax, and montanic acid wax; fatty acid amides such as stearic acid amide, oleic acid amide, and erucic acid amide; alkylene fatty acid amides such as methylene bis-stearic acid amide and ethylene bis-stearic acid amide; stearic acid; stearyl alcohol; metal stearates such as lead stearate, zinc stearate, calcium stearate, and magnesium stearate; stearic acid monoglyceride; stearyl stearate; and hydrogenated oils. Mold release agents include, but are not limited to, paraffin, wax, light oil, machine oil, spindle oil, insulating oil, waste oil, vegetable oil, fatty acid esters, organic acids, graphite particles, mica, vermiculite, fluorine-based mold release agents, and silicone-based mold release agents.

[0069] <Method for manufacturing inorganic coated sand> Next, a method for manufacturing inorganic coated sand will be described. The method for manufacturing inorganic coated sand of this embodiment is to produce dry inorganic coated sand having refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 This is a manufacturing method for producing inorganic-coated sand containing fine particles and satisfying at least one of the following (i) to (iii): (i) the inorganic binder constituting the inorganic binder layer has a melt viscosity at 80°C of 32 mPa·s or more and 150 mPa·s or less, (ii) the amount of water of hydration of the metasilicate hydrate is 6 or more and 8 or less, and (iii) the fusion point of the inorganic-coated sand is 40°C or more and 60°C or less, as measured in accordance with JACT Test Method C-1 Fusion Point Test Method.

[0070] First, an example of a method for producing the inorganic coated sand of this embodiment includes the following steps (1) and (2): Step (1): Mixing a refractory aggregate, metasilicate nonahydrate, and metasilicate pentahydrate to obtain a mixture; and Step (2): Cooling the mixture.

[0071] Step (1) is carried out at a temperature equal to or higher than the melting point of the mixture of metasilicate nonahydrate and metasilicate pentahydrate used. The mixture can be obtained by mixing metasilicate nonahydrate and metasilicate pentahydrate in any desired ratio. By mixing a refractory aggregate, metasilicate nonahydrate, and metasilicate pentahydrate at a temperature equal to or higher than the melting point of the mixture, an inorganic binder having a melt viscosity of 32 to 150 mPa·s at 80°C is obtained, and inorganic coated sand having a metasilicate hydrate water content of 6 to 8 can be obtained. Furthermore, for example, by mixing metasilicate nonahydrate and metasilicate pentahydrate in a molar ratio of 75:25 and appropriately adjusting the mixing procedure and conditions, the metasilicate hydrate water content can be controlled to 8.

[0072] Examples of a method for mixing refractory aggregate with metasilicate nonahydrate and metasilicate pentahydrate at a temperature equal to or higher than the melting point of a mixture of metasilicate nonahydrate and metasilicate pentahydrate include a method in which metasilicate nonahydrate and metasilicate pentahydrate are added to refractory aggregate heated to a temperature equal to or higher than the melting point of the mixture, and the refractory aggregate and metasilicate hydrate are mixed while melting the metasilicate hydrate (step (1A)), or a method in which a mixture of metasilicate nonahydrate and metasilicate pentahydrate that has been heated and melted is added to refractory aggregate and mixed (step (1B)). Further examples include a method of adding refractory aggregate heated to a temperature equal to or higher than the melting point of a mixture of metasilicate nonahydrate and metasilicate pentahydrate to the mixture, and mixing the refractory aggregate and metasilicate hydrate while melting the metasilicate hydrate (step (1C)), or a method of adding refractory aggregate to a mixture of metasilicate nonahydrate and metasilicate pentahydrate that has been heated and melted to a temperature equal to or higher than the melting point of the mixture, and mixing the mixture (step (1D)). Among these, step (1B) is preferred from the viewpoint of shortening the time required for covering the surface of the refractory aggregate with fluidized metasilicate hydrate.

[0073] From the same viewpoint, it is preferable that in step (1), metasilicate nonahydrate and metasilicate pentahydrate are mixed without being previously prepared into an aqueous solution. It is also preferable that step (1) does not include a step of intentionally adding water. The mixing conditions, such as the stirring speed and treatment time, when mixing the refractory aggregate with the metasilicate nonahydrate and metasilicate pentahydrate can be appropriately determined depending on the amount of the mixture to be treated.

[0074] In step (2), the mixture obtained in step (1) is cooled to a temperature below the melting point of the mixture to reduce the fluidity of the metasilicate hydrate and fix the metasilicate hydrate to the surface of the refractory aggregate, thereby forming a metasilicate hydrate layer, i.e., an inorganic binder layer, thereby obtaining the inorganic-coated sand according to this embodiment.

[0075] Next, another example of the method for producing the inorganic coated sand of this embodiment includes a production method including the following step (3): Step (3): Mixing a refractory aggregate with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate.

[0076] In step (3), SiO in a mixture of water glass, caustic alkali, and water 2 : M 2 O (M is an alkali metal): H 2 The metasilicate hydrate melt of this embodiment can be prepared by adjusting the molar ratio of O molecules to 1:1:6-8. This results in an inorganic binder having a melt viscosity at 80°C of 32 mPa·s or more and 150 mPa·s or less, and an inorganic-coated sand having a metasilicate hydrate with a hydration water content of 6 to 8. Water glass serves as the inorganic binder constituting the inorganic binder layer. Examples of caustic alkali include caustic soda (sodium hydroxide; NaOH) and caustic potash (potassium hydroxide; KOH). The mixing conditions for the water glass, caustic alkali, and water are not particularly limited, and known methods can be used. For example, mixing may be performed at ambient temperature. Alternatively, if the melt generates heat, mixing may be continued and then allowed to cool to ambient temperature.

[0077] In addition, examples of the method for mixing the refractory aggregate with the solution containing water glass, caustic alkali, and water include a method in which the solution is poured into the refractory aggregate and mixed (step (3A)), and a method in which the refractory aggregate is poured into the solution and mixed (step (3B)).

[0078] In this way, the inorganic coated sand according to this embodiment can be obtained.

[0079] [Casting Mold] Next, the casting mold according to this embodiment will be described. The casting mold according to this embodiment is formed from inorganic-coated sand. The method for manufacturing the casting mold includes the following steps (4) and (5). Step (4): Filling the inorganic-coated sand into a mold that will provide the desired mold. Step (5): Heating the mold filled with the inorganic-coated sand to harden the inorganic-coated sand.

[0080] In step (4), the mold is preferably preheated to maintain its temperature, from the viewpoint of improving mold productivity and mold strength. The heating temperature is preferably 100°C or higher, more preferably 150°C or higher, and is preferably 300°C or lower, more preferably 250°C or lower, from the viewpoint of improving mold productivity and mold strength.

[0081] In step (5), the mold filled with the inorganic coated sand is heated without passing water vapor through it. By using the inorganic coated sand of this embodiment, the inorganic coated sand can be hardened without passing water vapor through it, and equipment for passing water vapor through it is not required. The heating temperature is preferably 100°C or higher, more preferably 150°C or higher, and preferably 300°C or lower, more preferably 250°C or lower, from the viewpoint of improving mold productivity and mold strength. The heating time is preferably 30 seconds or higher, more preferably 60 seconds or higher, and preferably 600 seconds or lower, from the viewpoint of obtaining stable mold strength.

[0082] The inorganic coated sand according to this embodiment can be used alone or in combination with other known refractory aggregates and other additives to form a desired casting mold.

[0083] <Inorganic Coated Sand Composition> The inorganic coated sand composition of this embodiment is a mixture of the above-mentioned inorganic coated sand with refractory aggregate, inorganic particles, coupling agents, lubricants, and mold release agents. It is also possible to manufacture a casting mold using the inorganic coated sand composition in the same manner as the above-mentioned inorganic coated sand. The content of the inorganic coated sand relative to the total amount of the inorganic coated sand composition is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, in order to obtain good strength and other properties due to the inorganic coated sand. The refractory aggregate, inorganic particles, coupling agents, lubricants, and mold release agents used in the inorganic coated sand composition may be the same as those used in the above-mentioned inorganic coated sand.

[0084] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various other configurations may be adopted. Furthermore, modifications and improvements within the scope of the present invention are included in the present invention.

[0085] In relation to the above-described embodiments, the present invention further discloses the following inorganic-coated sand, a method for manufacturing the inorganic-coated sand, and a method for manufacturing a casting mold.

[0086] <1> Dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is composed of metasilicate hydrate and amorphous SiO 2 <2> Inorganic coated sand in a dry state, comprising a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is composed of metasilicate hydrate and amorphous SiO 2The inorganic binder layer contains metasilicate hydrate and amorphous SiO 2 <3> Dry inorganic coated sand containing refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 <4> Inorganic-coated sand according to any one of <1> to <3>, wherein the amount of water of hydration of the metasilicate hydrate is 6 to 8. <5> Inorganic-coated sand according to any one of <1> to <4>, wherein the inorganic binder layer contained in the inorganic-coated sand is 0.1 parts by mass or more, preferably 0.2 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, still more preferably 2 parts by mass or more, and 15 parts by mass or less, preferably 10 parts by mass or less, more preferably 8 parts by mass or less, relative to 100 parts by mass of the refractory aggregate. <6> Inorganic-coated sand according to any one of <1> to <5>, wherein the amount of amorphous SiO 2<7> The inorganic coated sand according to any one of <1> to <6>, wherein the content of the fine particles contained is 0.1 parts by mass or more, preferably 0.2 parts by mass or more and 10 parts by mass or less, preferably 5 parts by mass or less, and more preferably 3 parts by mass or less, relative to 100 parts by mass of the refractory aggregate. <7> The inorganic coated sand according to any one of <1> to <6>, wherein the dynamic angle of repose of the inorganic coated sand is preferably 80° or less, more preferably 45° or less, and even more preferably 30° or less. <8> The inorganic coated sand according to any one of <1> to <7>, wherein the degree of amorphization of the refractory aggregate is preferably 30% or more, more preferably 50% or more, even more preferably 65% ​​or more, and even more preferably 80% or more, and is preferably 100% or less, more preferably 99% or less. <9> The inorganic coated sand according to any one of <1> to <8>, wherein the sphericity of the refractory aggregate is preferably 0.80 or more, more preferably 0.85 or more, even more preferably 0.90 or more, still more preferably 0.95 or more, and still more preferably 0.97 or more. <10> The inorganic coated sand according to any one of <1> to <9>, wherein the average particle size of the refractory aggregate is preferably 0.05 mm or more, more preferably 0.1 mm or more, and preferably 2 mm or less, more preferably 1 mm or less, and even more preferably 0.5 mm or less. <11> The inorganic-coated sand according to any one of <1> to <10>, wherein the water content (including water of crystallization) in the inorganic binder layer contained in the inorganic-coated sand is preferably 75 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 85 parts by mass or more, relative to 100 parts by mass of metasilicate (anhydrous equivalent), and is preferably 130 parts by mass or less, more preferably 125 parts by mass or less, even more preferably 120 parts by mass or less.<12> The inorganic coated sand according to any one of <1> to <11>, wherein the content of metasilicate hydrate in the inorganic binder layer is preferably 25% by mass or more, more preferably 30% by mass or more, even more preferably 35% by mass or more, particularly preferably 40% by mass or more, and preferably 95% by mass or less, more preferably 90% by mass or less, based on the entire inorganic binder layer. <13> The inorganic coated sand according to any one of <1> to <12>, wherein the content of metasilicate (anhydride equivalent) in the inorganic binder is preferably 11% by mass or more, more preferably 45% by mass or more, and preferably 56% by mass or less, more preferably 48% by mass or less. <14> The inorganic coated sand according to any one of <1> to <13>, wherein the content of metasilicate hydrate in the inorganic coated sand is preferably 0.1 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.5 parts by mass or more, still more preferably 0.8 parts by mass or more, particularly preferably 1 part by mass or more, and preferably 9 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, and still more preferably 4 parts by mass or less, relative to 100 parts by mass of the refractory aggregate. <15> The inorganic coated sand according to any one of <1> to <14>, wherein the content of amorphous SiO. 2 <16> The inorganic-coated sand according to any one of <1> to <15>, wherein the amorphous degree of the contained fine particles is preferably 80% or more, more preferably 90% or more, even more preferably 93% or more, still more preferably 95% or more, and particularly preferably 98% or more, and is 100% or less. 2The inorganic-coated sand, in which the average particle size of the contained fine particles is preferably 0.1 μm or more, more preferably 0.3 μm or more, and preferably 2.0 μm or less, more preferably 1.0 μm or less, even more preferably 0.8 μm or less, and even more preferably 0.6 μm or less. <17> A casting mold using the inorganic-coated sand according to any one of <1> to <16>. <18> An inorganic-coated sand composition containing the inorganic-coated sand according to any one of <1> to <16>. <19> The inorganic-coated sand composition according to <18>, in which the content of the inorganic-coated sand relative to the total amount of the inorganic-coated sand composition is preferably 70 mass% or more, more preferably 80 mass% or more, and even more preferably 90 mass% or more. <20> A casting mold using the inorganic-coated sand composition according to <18> or <19>. <21> A method for producing inorganic coated sand according to any one of <1> to <16>, comprising: step (1) of mixing the refractory aggregate, metasilicate nonahydrate, and metasilicate pentahydrate to obtain a mixture; and step (2) of cooling the mixture, wherein step (1) comprises mixing at a temperature equal to or higher than the melting point of a mixture of the metasilicate nonahydrate and the metasilicate pentahydrate, and step (2) comprises cooling to a temperature below the melting point of the mixture of the metasilicate nonahydrate and the metasilicate pentahydrate. <22> A method for producing inorganic coated sand according to any one of <1> to <16>, comprising step (3) of mixing the refractory aggregate with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate.

[0087] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0088] (1) Materials Materials used in the following examples and comparative examples will be described.

[0089] [Refractory aggregates] Refractory aggregate 1: Mikawa silica sand R6 (manufactured by Mikawa Silica Co., Ltd., average particle size: 200 μm, amorphousness: 0.2%, sphericity: 0.85) Refractory aggregate 2: Espearl #60L (manufactured by Yamakawa Sangyo Co., Ltd., average particle size: 241 μm, amorphousness: 45%, sphericity: 0.97)

[0090] [Metasilicate hydrate (inorganic binder)] Metasilicate 1: Sodium metasilicate nonahydrate (Na 2 SiO 3 ・9H 2 O), melting point 47°C. Metasilicate 2: Sodium metasilicate pentahydrate (Na 2 SiO 3 ・5H 2 0), melting point 72°C. Metasilicate 3: Sodium metasilicate anhydrous manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. Metasilicates 4 to 6: Aqueous solutions containing each water glass prepared by the following procedure.

[0091] (Procedure) Water glass, caustic soda (NaOH), and water were mixed in a mixer for 10 minutes in the ratios (parts by mass) shown in Table 1 below to obtain metasilicates 4 to 6 having the amounts of water of hydration shown in Table 1, respectively.

[0092]

[0093] No. 1 50 water glass: manufactured by Fuji Chemical Co., Ltd., SiO 2 (%)=30.0, Na 2 O (%) = 14.7, solid content 44.7 mass% No. 1 59 water glass: manufactured by Fuji Chemical Co., Ltd., SiO 2 (%)=36.2, Na 2 O (%) = 18.2, solid content 54.4 mass% NaOH: caustic soda, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., NaOH, granular

[0094] [Amorphous SiO 2 Containing fine particles] Amorphous SiO 2 Containing fine particles 1: Denka fused silica SFP-20M (average particle size: 0.4 μm, amorphousness: 99.5% or more, SiO 2 Mass %: 99 mass % or more) Amorphous SiO 2 Containing fine particles 2: Silica fume EFACO manufactured by Tomoe Engineering (average particle size: 0.3 μm, amorphous degree 95% or more, SiO2 Mass%: 92.4% by mass)

[0095] (2) Preparation of Inorganic Coated Sand <Examples 1, 3-4, 6-8, Comparative Examples 1-6> Refractory aggregate 1 (100 parts by mass) was charged into a mixer. Next, a mixture of metasilicate 1 and metasilicate 2 in the amounts (parts by mass) shown in Table 2 was heated to 80°C to melt and obtain a molten liquid. Next, the molten liquid was charged into the mixer, and kneading was started uniformly with refractory aggregate 1. While continuing to stir, the mixture was allowed to cool naturally to below the melting point of the mixture of metasilicate 1 and metasilicate 2, and the stirring was stopped 7 minutes after the start of kneading, obtaining dry sand with room temperature fluidity. Using this dry sand, the amount of hydrate shown in Table 2 was measured using the hydrate amount measurement method described below. Thereafter, amorphous SiO in the amount (parts by mass) shown in Table 2 was further added. 2 The fine particles were added and kneaded for 2 minutes. The composition of the resulting inorganic-coated sand is shown in Table 2. The melting points of the mixtures of metasilicate 1 and metasilicate 2 were both lower than 80°C, and in the range of 48 to 63°C when the amount of water of hydration was 8 to 6.

[0096] Example 2: A mixture of metasilicate 3 and water and amorphous SiO in the amounts (parts by mass) shown in Table 2 was added to refractory aggregate 1 (100 parts by mass). 2 The inorganic coated sand shown in Table 2 was obtained in the same manner as in Example 1, except that the fine particles were added.

[0097] Example 5: A mixture of metasilicate 2 and water and amorphous SiO in the amounts (parts by mass) shown in Table 2 was added to refractory aggregate 1 (100 parts by mass). 2 The inorganic coated sand shown in Table 2 was obtained in the same manner as in Example 1, except that the fine particles were added.

[0098] Examples 9 to 11: Refractory aggregate 1 (100 parts by mass) was mixed with any one of metasilicates 4 to 6 and amorphous SiO 2 The inorganic coated sand shown in Table 2 was obtained in the same manner as in Example 1, except that the contained fine particles were added in the amounts (parts by mass) shown in Table 2.

[0099] Examples 12 to 15, Comparative Examples 7 and 8: Refractory aggregate 2 (100 parts by mass) was mixed with metasilicate 1, metasilicate 2, and amorphous SiO 2 The inorganic coated sand shown in Table 2 was obtained in the same manner as in Example 1, except that the contained fine particles were added in the amounts (parts by mass) shown in Table 2.

[0100] Examples 16 to 18: Refractory aggregate 2 (100 parts by mass) with any one of metasilicates 4 to 6 and amorphous SiO 2 The inorganic coated sand shown in Table 2 was obtained in the same manner as in Example 1, except that the contained fine particles were added in the amounts (parts by mass) shown in Table 2.

[0101] (3) Evaluation and Measurement The following evaluation and measurement were carried out for each metasilicate hydrate (inorganic binder) or each inorganic coated sand.

[0102] <Measurement of the amount of water of hydration> (1) Amount of amorphous SiO 2 10 g of inorganic coated sand before adding additives such as fine particles was weighed and placed in a container, and the amount of mass loss (%) after heating at 900°C for 1 hour was used to calculate the moisture content (%) (A) in the inorganic coated sand. A = [(M1 - M2) / M3] x 100 (M1: total mass (g) of the crucible and inorganic coated sand before firing, M2: total mass (g) of the crucible and inorganic coated sand after firing, M3: mass (g) of the inorganic coated sand before firing) (2) Amorphous SiO 2100 g of inorganic-coated sand before the addition of additives such as fine particles was weighed, immersed in 200 mL or more of hot water, and stirred for at least 1 hour to extract metasilicate hydrate. The refractory aggregate was filtered from the resulting extract, and the extract was then subjected to vacuum distillation at 40°C and an internal pressure of 15 mmHg or less using a rotary evaporator to remove water. The extract was then dried at 180°C for 3 hours, and the dried product was weighed. The dry solids content (%) (B) of metasilicate hydrate in the inorganic-coated sand was calculated. B = (M12 / M11) x 100 (M11: mass (g) of inorganic-coated sand, M12: dry product weight (g)). (3) The water content (%) (A) in the resulting inorganic-coated sand and the dry solids content (%) (B) of metasilicate hydrate were applied to the following formula to calculate the amount of water of hydration of metasilicate hydrate. Amount of water of hydration of metasilicate hydrate = [(A) / molecular weight of water] / [(B) / molecular weight of metasilicate anhydride]

[0103] <Melt viscosity measurement of inorganic binder> Each metasilicate hydrate heated to 80°C was measured at a shear rate of 100 s using a parallel plate (PP60) in a rheometer MARS40 manufactured by Thermo Scientific Corporation at 80°C. ―1 The viscosity of each of the samples was measured. The evaluation results are shown in Table 2.

[0104] <Fusion Point Measurement> The fusion point (°C) of the inorganic coated sand was measured in accordance with JACT Test Method C-1 Fusion Point Test Method ("Test Methods for Molds and Mold Materials," published in May 1999 by the Japan Small and Medium Enterprise Agency, Information and Technology Department, Technical Support Division). However, taking into consideration the characteristics of the inorganic coated sand, the measurement method was as follows: Two hot plates (Type 1900 Hot Plate, manufactured by Barnstead) were placed side by side, spaced approximately 18 cm apart, and a rectangular parallelepiped metal rod (made of stainless steel) measuring 1.5 cm wide, 22 cm long, and 0.5 cm thick was placed on the hot plates so that each end rested approximately 2 cm above the rod. Then, only one of the hot plates was heated to a temperature of 200°C. After about 30 minutes, the temperature of the metal rod on the heated hot plate was measured with a contact thermometer (MC1000 manufactured by Chino Corporation) and confirmed to be above 100°C. Similarly, the temperature of the metal rod on the unheated hot plate was confirmed to be about 25°C. Inorganic-coated sand was then quickly sprinkled onto the metal rod, and after 60 seconds, the metal rod was rotated 180° around its longitudinal axis so that the inorganic-coated sand-sprinkled surface was facing downwards. The temperature of the hottest part at the boundary between the remaining and non-remaining inorganic-coated sand sections was measured with a contact thermometer. This procedure was repeated three times, and the average of the measured temperatures was taken as the fusion point of the inorganic-coated sand. The measurement results are shown in Table 2.

[0105] <Mold Strength> Using each inorganic-coated sand, a mold was prepared according to the following procedure, and the mold strength was measured. The evaluation results are shown in Table 2. (Procedure) A mold for 22.3 mm x 22.3 mm x 180 mm test pieces (5 pieces) was heated to 180°C. Each inorganic-coated sand from the above Examples and Comparative Examples was filled into the mold heated to 180°C at a blow pressure of 0.3 MPa using a CSR-43 blow molding machine. The inorganic-coated sand was left to harden in the mold for 150 seconds, yielding a mold test piece. (Measurement) The mold strength (MPa) of each obtained mold test piece was measured using a George Fischer PFG universal strength testing machine equipped with a PBV flexural attachment. The mold test pieces were removed from the mold and then left in a constant temperature and humidity chamber at 25°C / 55% RH for 1 hour.

[0106] <Storage> Immediately after preparing each of the inorganic-coated sands of the above Examples and Comparative Examples, 2 kg of the inorganic-coated sand was placed in a plastic bag, sealed, and stored at 25°C for 12 hours. Immediately after that, mold test pieces were prepared in the same manner as in <Mold strength> above, and the mold strength was measured. The measurement results are shown in Table 2.

[0107]

Claims

1. A dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 The inorganic coated sand contains fine particles, and the melt viscosity at 80°C of the inorganic binder constituting the inorganic binder layer is 32 mPa·s or more and 150 mPa·s or less.

2. A dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 An inorganic coated sand containing fine particles, the amount of water of hydration of the metasilicate hydrate being 6 or more and 8 or less.

3. A dry inorganic coated sand having a refractory aggregate and an inorganic binder layer covering the surface of the refractory aggregate, wherein the inorganic binder layer is a mixture of metasilicate hydrate and amorphous SiO 2 Inorganic coated sand containing fine particles and having a fusion point of 40°C or higher and 60°C or lower according to JACT test method C-1 fusion point test method.

4. The inorganic coated sand according to any one of claims 1 to 3, wherein the inorganic binder layer contained in the inorganic coated sand is 0.2 parts by mass or more and 15 parts by mass or less per 100 parts by mass of the fire-resistant aggregate.

5. The inorganic coated sand according to any one of claims 1 to 4, wherein the amorphous SiO 2 The inorganic coated sand has a content of fine particles of 0.1 parts by mass or more and 10 parts by mass or less per 100 parts by mass of the refractory aggregate.

6. A casting mold using the inorganic coated sand according to any one of claims 1 to 5.

7. An inorganic coated sand composition comprising the inorganic coated sand according to any one of claims 1 to 5.

8. A casting mold using the inorganic coated sand composition according to claim 7.

9. A method for producing inorganic coated sand according to any one of claims 1 to 5, comprising: a step (1) of mixing the refractory aggregate, metasilicate nonahydrate and metasilicate pentahydrate to obtain a mixture; and a step (2) of cooling the mixture, wherein the step (1) comprises mixing at a temperature equal to or higher than the melting point of a mixture of the metasilicate nonahydrate and the metasilicate pentahydrate, and the step (2) comprises cooling to a temperature lower than the melting point of the mixture of the metasilicate nonahydrate and the metasilicate pentahydrate.

10. A method for producing the inorganic coated sand according to any one of claims 1 to 5, comprising a step (3) of mixing the refractory aggregate with a solution containing water glass, caustic alkali, and water to obtain a mixture containing metasilicate hydrate.

Citation Information

Patent Citations

  • JP1973053929A

  • JP1975020543A

  • JP1975026498A

  • Coil dismantling method in core of rotary machine

    JP1978025803A

  • Surface coating material for tundish

    JP2000176612A