COLETOR DE CORRENTE PARA ÂNODO, ÂNODO PARA CÉLULA ELETROQUÍMICA, CÉLULA ELETROQUÍMICA, DISPOSITIVO DE ARMAZENAMENTO DE ENERGIA, MÉTODO DE FABRICAÇÃO DE COLETOR DE CORRENTE PARA O ÂNODO E MÉTODO DE FABRICAÇÃO DE ÂNODO PARA UMA CÉLULA ELETROQUÍMICA

The current collector with a controlled roughness interface layer addresses the mechanical instability of silicon-based anodes by improving adhesion and reducing electrical resistance, enhancing the electrochemical performance and lifespan of electrochemical cells.

BR112022019877B1Active Publication Date: 2026-11-10ARMOR BATTERY FILMS
View PDF -1 Cites 0 Cited by

Patent Information

Application Number
BR112022019877
Authority / Receiving Office
BR · BR
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-01
Filing Date
2021-03-31
Publication Date
2026-11-10
Estimated Expiration
2041-03-31

AI Technical Summary

Technical Problem

Existing anodes in electrochemical cells, particularly those using silicon as the active material, face issues with mechanical damage and fragmentation due to significant volume changes during lithium ion intercalation and deintercalation, leading to reduced lifespan and increased electrical resistance.

Method used

A current collector for anodes is designed with an interface layer having a thickness of less than 10 micrometers and a controlled roughness, enhancing adhesion and reducing electrical resistance by improving electron exchange and mechanical stress management.

Benefits of technology

The interface layer improves the adhesion and electrical contact between the substrate and electrode, reducing mechanical stresses and enhancing the electrochemical performance, thereby extending the anode's lifespan and cycle capacity.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

CURRENT COLLECTOR FOR ANODE, ANODE FOR ELECTROCHEMICAL CELL, ELECTROCHEMICAL CELL, ENERGY STORAGE DEVICE, METHOD FOR MANUFACTURING A CURRENT COLLECTOR FOR THE ANODE AND METHOD FOR MANUFACTURING AN ANODE FOR AN ELECTROCHEMICAL CELL. The present invention relates to a current collector (23) for an anode (16), wherein the current collector (23) includes: - a substrate (20) with first face (201); and - at least one interface layer (22) with a thickness of less than 10 micrometers, preferably less than 6 micrometers, in contact with the first face (201) of the substrate (20), wherein the interface layer (22) has a roughness whose depth is from 0.5 micrometers to 10 micrometers.
Need to check novelty before this filing date? Find Prior Art

Description

1 / 44 “CURRENT COLLECTOR FOR ANODE, ANODE FOR ELECTROCHEMICAL CELL, ELECTROCHEMICAL CELL, DEVICE OF "ENERGY STORAGE, METHOD FOR MANUFACTURING A CURRENT COLLECTOR FOR THE ANODE AND METHOD FOR MANUFACTURING AN ANODE FOR AN ELECTROCHEMICAL CELL" Field of Invention

[001] The present invention relates to a current collector for an anode. The present invention also relates to an electrochemical cell and an energy storage device comprising such current collector. The present invention also relates to a method of manufacturing such current collector.

[002] The present invention also relates to an anode for an electrochemical cell. The present invention also relates to an electrochemical cell and to an energy storage device comprising said anode. The present invention further relates to a method of manufacturing said anode. Background of the Invention

[003] An electrochemical cell conventionally comprises a positive electrode, a negative electrode, an electrolyte, and current collectors for each electrode. The combination of a negative electrode and a current collector forms an anode, where the combination of a positive electrode and a current collector forms a cathode.

[004] The operating principle of these cells is based on the reversible storage of electrical energy in the form of chemical energy, using two separate and coupled electrochemical reactions. The positive and negative electrodes are immersed in the electrolyte and serve as the site for the so-called Faraday-type electrochemical reactions. In particular, the electrodes are made of active materials to store and remove ions by Petition 870240061031, dated 07 / 19 / 2024, page 16 / 117 2 / 44 means of oxidation and reduction reactions.

[005] The electrodes are produced according to a composition, in which the composition mainly includes one or more active materials (>70% by weight), conductive particles that provide good electron transport towards all active materials, and a binder that ensures the cohesion of the particles, in addition to adhesion to the current collector.

[006] The two electrodes, positive and negative, are then ionically linked by an electrolyte. The electrolyte can be liquid, gel, or solid.

[007] Due to the intrinsic ionic migration function of electrochemical cells, the electrodes require materials that are capable of inserting and / or removing ions. Lithium technologies have better characteristics in terms of volume and mass energy densities. These technologies are therefore preferentially selected for mobile applications, such as mobile telephony or laptop computers, as well as for the development of new electric vehicles and stationary systems that require large storage capacities and long service life.

[008] Silicon, as the active material of the anode, has a greater lithium ion storage capacity than graphite. During the first cycles of use, liquid electrolyte and lithium are deposited on the surface of the active material and decompose to form a layer called the solid electrolyte interface (SEI). The lithium deposited at this location is no longer available for the transport of lithium ions between the electrodes.

[009] Silicon anodes can, however, be damaged by deformation and fragmentation of the active material, caused by volume changes that can reach 300%. In fact, during cell operation, when lithium ions are intercalated, the active material of the anode expands. Petition 870240061031, dated 07 / 19 / 2024, page 17 / 117 3 / 44 and, when lithium ions are removed, the active material contracts. These volume changes can further result in stripping, peeling of the SEI and new electrolyte decomposition, accompanied by further lithium deposition, generating the formation of a new SEI. Brief Description of the Invention

[0010] There is therefore a need for an anode for an electrochemical cell that can be used to produce an electrochemical cell with a longer lifespan.

[0011] There is also a need for a current collector for anodes that provides enhanced properties, particularly better adhesion to the electrode and / or reduced electrical resistance between the substrate and the electrode.

[0012] For this purpose, a current collector for anodes is proposed, in which the current collector includes: - a substrate with a first face; and - at least one interface layer with a thickness of less than 10 micrometers, preferably less than 6 micrometers, in contact with the first face of the substrate, wherein the interface layer has a roughness whose depth is from 0.5 micrometers to 10 micrometers.

[0013] This collector has improved properties in terms of adhesion and / or reduced electrical resistance.

[0014] It should be noted that these performances are better if one or more interface layers are added between a substrate and an electrode layer to enhance adhesion between the two elements and / or reduce mechanical stresses within the electrode. This method is known, for example, from documents US 2012 / 107684, WO 2009 / 054987, US 2009 / 0061319 and US 2017 / 271678.

[0015] Even if an interface layer provides good adhesion Petition 870240061031, dated 07 / 19 / 2024, page 18 / 117 4 / 44 of the electrode to the substrate and, with it, a better electrical interface; however, it adds electrical resistance inside due to the conductivity limit of its components.

[0016] The roughness of the collector interface layer of the present device solves this technical problem, particularly by generating better electrical percolation inside the electrode and increasing the electron exchange surface with the current collector.

[0017] It should be noted that the present invention does not refer to a coating layer whose surface state merely reproduces the state of the substrate on which it is deposited, as described in US patent 2013 / 011510, but a layer with its own surface state. This surface state is controlled and can be modulated, for example, by means of the layer composition, in order to obtain the best electrochemical performance.

[0018] According to specific embodiments, the current collector comprises one or more of the following features, taken individually or in all technically possible combinations: - The interface layer has a second face in contact with the first face of the substrate. The second face of the interface layer has an extension, and the first face of the substrate has an extension, where the ratio between the extension of the second face of the interface layer and the extension of the first face of the substrate is 0.1 to 1; - The interface layer is prepared by means of a second-composition coating, wherein the second composition comprises a second binder material and a second conductive additive; The interface layer consists of a set that includes a series of elements arranged on the first face of the substrate, where each element is separated from an adjacent element by a distance of Petition 870240061031, dated 07 / 19 / 2024, page 19 / 117 5 / 44 200 micrometers to 2500 micrometers, and the distance separating two adjacent elements is the shortest distance between a point on one element and a point on a second element adjacent to the first element; - the interface layer is produced by coating with a third composition, wherein the third composition comprises a third conductive additive and, if appropriate, a third binder material; - each element has a base, where the base of each element is a polygon, disk, or oval; - the base of the interface layer elements has a first-face coverage level of 0.1 to 0.9, preferably 0.2 to 0.5; - each element has a height less than or equal to 10 micrometers; and - The current collector comprises at least one first interface layer, wherein the first interface layer has a second face in contact with the first face of the substrate, the second face of the interface layer has an extension, and the first face of the substrate has an extension, wherein the ratio between the extension of the second face of the interface layer and the extension of the first face of the substrate is from 0.1 to 1.The current collector comprises at least a second interface layer, wherein the second interface layer consists of an assembly comprising a series of elements arranged on the first face of the substrate, each element being separated from another adjacent element by a distance of 200 micrometers to 2500 micrometers, the distance separating two adjacent elements being the shortest distance between a point on a first element and a point on a second element adjacent to the first element, and the first interface layer and the second interface layer are superimposed on each other. Petition 870240061031, dated 07 / 19 / 2024, page 20 / 117 6 / 44 yes.

[0019] The present invention also relates to an electrochemical cell comprising a current collector, as described above.

[0020] The present invention also relates to a method of manufacturing a current collector for an anode, wherein the method comprises: - a step in supplying a substrate with a first face; and - a deposition step, by coating the first face of the substrate with at least one interface layer, wherein the interface layer is less than 10 micrometers thick, preferably less than 6 micrometers, and the interface layer has a roughness with a depth of 0.5 micrometers to 10 micrometers.

[0021] An anode for an electrochemical cell is further proposed, wherein the anode includes a substrate with a first face, an electrode produced according to a first composition, wherein the first composition includes an intercalation material, a first binder material and a first conductive additive, wherein the intercalation material comprises silicon. The electrode has one face, wherein the first face of the substrate and the face of the electrode are opposite each other. The anode includes at least one interface layer with a thickness of less than 10 micrometers, preferably less than 6 micrometers, disposed between the substrate and the electrode and in contact with the first face of the substrate and the face of the electrode.

[0022] According to other specific realizations, the anode comprises one or more of the following features, taken individually or in all technically possible combinations: - the interface layer has its first face in contact with Petition 870240061031, dated 07 / 19 / 2024, page 21 / 117 7 / 44 the electrode face, where the first face of the interface layer has a roughness with a depth of 10 nanometers to 10 micrometers; - The interface layer has a second face in contact with the first face of the substrate. The second face of the interface layer has an extension, and the first face of the substrate has an extension, where the ratio between the extension of the second face of the interface layer and the extension of the first face of the substrate is 0.1 to 1; - The interface layer is prepared by means of a second-composition coating, wherein the second composition comprises a second binder material and a second conductive additive; - The interface layer consists of an assembly that includes a series of elements arranged on the first face of the substrate, where each element is separated from another adjacent element by a distance of 200 micrometers to 2500 micrometers, and the distance separating two adjacent elements is the shortest distance between a point on one element and a point on a second element adjacent to the first element; - the interface layer that is produced by coating with a third composition, wherein the third composition comprises a third conductive additive and, if appropriate, a third binder material; - each element has a base, where the base of each element is a polygon, disk, or oval; - the base of the interface layer elements has a first-face coverage level of 0.1 to 0.9, preferably 0.2 to 0.5; - each element has a height less than or equal to 10 micrometers; - the anode comprises at least a first layer of Petition 870240061031, dated 07 / 19 / 2024, page 22 / 117 8 / 44 interface, wherein the first interface layer has its first face in contact with the electrode face and the first face of the interface layer has a roughness with a depth of 10 nanometers to 10 micrometers; the anode comprises at least a second interface layer, wherein the second interface layer consists of an assembly comprising a series of elements arranged on the first face of the substrate, each element is separated from another adjacent element by a distance of 200 micrometers to 2500 micrometers and the distance separating two adjacent elements is the shortest distance between a point of a first element and a point of a second element adjacent to the first element; and the first interface layer and the second interface layer are superimposed on one another; - the silicon content of the intercalation material is greater than or equal to 30%, preferably greater than or equal to 60% by weight; and The intercalation material is silicon.

[0023] The present invention also relates to an electrochemical cell that includes an anode as described above.

[0024] The present invention further describes an energy storage device that includes at least one electrochemical cell as described above.

[0025] The present invention also relates to a method for manufacturing anodes for an electrochemical cell, wherein the method comprises a step of providing a first-face substrate, a step of depositing by coating at least one interface layer onto the first face of the substrate, wherein the interface layer has a thickness of less than 10 micrometers, preferably less than 6 micrometers. The method further includes a step of preparing a first composition which includes an intercalation material, first material Petition 870240061031, dated 07 / 19 / 2024, page 23 / 117 9 / 44 binder and first conductive additive, wherein the intercalation material comprises silicon, and a deposition step by coating the first composition onto the interface layer to produce a single-faced electrode, wherein the first face of the substrate and the face of the electrode are opposite and the interface layer is in contact with the first face of the substrate and the face of the electrode. Brief Description of the Figures

[0026] Other features and advantages of the present invention will become apparent from reading the following description of embodiments of the present invention, provided only by way of example, with reference to the following drawings: Figure 1 is a schematic representation of an electrochemical cell that includes an anode; Figure 2 is a schematic side view of a section of the anode of the electrochemical cell, including an interface layer; Figure 3 is a schematic side view of a section of another example of an electrochemical cell anode, which includes another example of an interface layer; Figure 4 is a schematic representation of the top of a section of a part of the interface layer of an example anode; Figure 5 is a schematic representation of the top of a section of a part of the interface layer of another example of an anode; Figure 6 is a schematic representation of the top of a section of a part of the interface layer of yet another example of an anode; Figure 7 is a schematic representation of the top of a section of a part of the interface layer of yet another example of an anode; Petition 870240061031, dated 07 / 19 / 2024, page 24 / 117 10 / 44 Figure 8 is a schematic side view of a section of another example of an electrochemical cell anode, which includes two interface layers; and Figure 9 is a schematic side view of a section of another example of an electrochemical cell anode, which includes two interface layers. Detailed Description of the Invention

[0027] An electrochemical cell 10 is shown in Figure 1.

[0028] Cell 10 is intended to be connected to other electrochemical cells to form an energy storage device, particularly an electric generator with the desired capacity and voltage.

[0029] This generator is called a battery pack or, simply, a battery.

[0030] The electrochemical cell 10 uses a reversible energy conversion method to store energy and retrieve it later.

[0031] The described electrochemical cell 10 uses an electrochemical reaction, where the electrochemical cell 10 is an electrochemical cell.

[0032] According to the example described, electrochemical cell 10 is a lithium-ion battery intended for a lithium-ion battery pack.

[0033] The electrochemical cell 10 comprises an electrolyte 12, a cathode 14 and an anode 16.

[0034] The electrochemical cell 10 functions as an electrochemical cell thanks to the interaction between the electrolyte 12, the cathode 14 and the anode 16.

[0035] Electrolyte 12 consists of different ionic salts that provide the ions used for charge storage reactions or Faraday-type carbonate reactions and a solvent or mixture of solvents to allow the solubilization of the ions. Petition 870240061031, dated 07 / 19 / 2024, page 25 / 117 11 / 44

[0036] The ionic salts are selected from lithium hexafluorophosphate (LiPF6), lithium bis(trifluoromethanesulfonyl)imide salt (LiTFSI), lithium tetrafluoroborate (LiBF4), lithium bisoxalatoborate (LiBOB), lithium nitrate (LiNO3) and lithium difluorooxalatoborate (LiDFOB).

[0037] Carbonates include, for example, propylene carbonate (PC), ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC).

[0038] Also carbohydrates, in smaller proportions, are fluoroethylene carbonate (FEC), vinylene carbonate (VC), methyl acetate, methyl formate, acetonitrile, tetrahydrofuran, gamma-butyrolactone and their binary, ternary or even quaternary mixtures, as well as ionic liquids.

[0039] Cathode 14 includes an active material.

[0040] The active material of cathode 14 conventionally consists of lithium sulfur (LIS) and / or at least one lithiated metal oxide, wherein the lithiated metal oxide is selected, for example, from lithium cobalt oxide LiCoO2 (LCO), lithium-nickel-cobalt-manganese oxide LiNiMnCoO2 (NMC), lithium-nickel-cobalt-aluminum oxide LiNiCoAlO2 (NCA), lithium manganese oxide LiMnO4 (LMO), lithium-iron-phosphorus oxide LiFePO4 (LFP), lithium-nickel-manganese oxide Li(LiNiMn)O2, lithium-manganese-iron phosphate (LMFP) and lithium-nickel-manganese oxide LiNiMnO (LNMO).

[0041] Other examples of active cathode material 14 are possible, such as those adapted to sodium-ion batteries.

[0042] Anode 16 is shown in more detail in Figure 2.

[0043] The anode 16 includes a substrate 20, an electrode 21 and an interface layer 22.

[0044] The substrate 20, the electrode 21, and the interface layer 22 form a stack of layers along a stacking direction indicated by Z, where the interface layer 22 is arranged between the substrate Petition 870240061031, dated 07 / 19 / 2024, page 26 / 117 12 / 44 and electrode 21.

[0045] The substrate 20, the interface layer 22 and the electrode 21 are superimposed.

[0046] The substrate 20 and the interface layer 22 form a current collector for the anode 16.

[0047] The substrate 20 and the interface layer 22 form the current collector 23.

[0048] Throughout this descriptive report, each feature or embodiment refers, without distinction, to anode 16 or current collector 23.

[0049] Substrate 20 has first face 201 perpendicular to the stacking direction Z.

[0050] Substrate 20 has a thickness e20 of 1 to 20 micrometers (µm), preferably 10 µm, where the thickness e20 is measured along the Z stacking direction.

[0051] Next, “value from A to B” indicates that the value is greater than or equal to A and less than or equal to B.

[0052] Next, the thickness value of a layer is measured along the Z stacking direction.

[0053] Substrate 20 includes a metal sheet 35.

[0054] Metal sheet 35 is made, for example, of iron, copper, aluminum, nickel, titanium or stainless steel.

[0055] Electrode 21 is in contact with electrolyte 12 of electrochemical cell 10.

[0056] Electrode 21 has a face 212 perpendicular to the Z stacking direction.

[0057] Face 212 of electrode 21 is opposite to the first face 201 of substrate 20. Petition 870240061031, dated 07 / 19 / 2024, p. 27 / 117 13 / 44

[0058] Electrode 21 is placed on the interface layer 22.

[0059] Electrode 21 has a thickness e21 of 10 μm to 150 μm.

[0060] Electrode 21 is formed by depositing first composition C1 onto the interface layer 22. Preferably, electrode 21 is formed by coating first composition C1 onto the interface layer 22.

[0061] The first composition C1 includes an intercalation material MI, first binder material ML1 and first conductive additive AC1.

[0062] The intercalation material is additionally indicated by the expression “active material”.

[0063] The MI intercalation material comprises at least silicon. The silicon concentration in the MI intercalation material is greater than or equal to 30% by weight of the MI intercalation material, preferably greater than or equal to 60% by weight of the MI intercalation material, and is conveniently equal to 100% by weight of the MI intercalation material.

[0064] The silicon in the MI intercalation material is in the form of generally spherical particles with a diameter of 5 nanometers (nm) to 500 nm, preferably 10 nm to 200 nm. Alternatively, the silicon in the MI intercalation material is in the form of flakes or fibers. The silicon in the MI intercalation material may be coated with carbon. When the silicon concentration in the first MI1 intercalation material is strictly less than 100%, the MI intercalation material further comprises a material selected from mesophase microspheres, commonly referred to as “MesoCarbon MicroBeads” (MCMB), natural or artificial graphites, graphitic materials such as soft carbon or hard carbon, lithium titanate-based compounds such as Li4Ti5O12 (also referred to as LTO), and compounds containing silicon, tin, or Petition 870240061031, dated 07 / 19 / 2024, page 28 / 117 14 / 44 their leagues.

[0065] The first composition C1 comprises a weight concentration of intercalation material MI greater than or equal to 50%, preferably greater than or equal to 60%, conveniently 60% to 93%, relative to the weight of composition C1.

[0066] The silicon of electrode 21 is in the form of a dispersion of pure silicon particles and / or silicon oxide SiOx in the anode material 16 (where x is an integer equal to 1 or 2). The silicon and / or silicon oxide particles of electrode 21 are not covalently bonded to another chemical element, such as hydrogen. If the silicon has been oxidized, the silicon particles are mainly composed of pure Si and coated with SiOx.

[0067] Whenever mentioned below, the weight content of an element in a composition is calculated in relation to the weight of the total composition.

[0068] The choice of the first binder material ML1 varies considerably, provided that the first binder material ML1 is inert with respect to the other electrode materials 21.

[0069] The first binder material ML1 is a material, preferably a polymer, that can be used to facilitate the handling of electrodes during their manufacture.

[0070] The first binder material ML1 comprises one or more polymers selected from thermoplastic polymers, heat-shrinkable polymers, elastomers and mixtures thereof.

[0071] Examples of thermoplastic polymers include, without limitation, polymers resulting from the polymerization of aliphatic or cycloaliphatic vinyl monomers, such as polyolefins (including polyethylenes or polypropylenes), polymers resulting from the polymerization of vinyl monomers Petition 870240061031, dated 07 / 19 / 2024, page 29 / 117 15 / 44 aromatics, such as polystyrenes, polymers resulting from the polymerization of acrylic monomers and / or (meth)acrylates, polyamides, polyether ketones and polyimides.

[0072] Examples of heat-shrinkable polymers include, but are not limited to, heat-shrinkable resins (such as epoxy resins and polyester resins) possibly mixed with polyurethanes or polyether polyols.

[0073] Examples of elastomeric polymers include, but are not limited to, natural rubbers, synthetic rubbers, styrene-butadiene copolymers (also known by the abbreviation “SBR”), ethylene-propylene copolymers (also known by the abbreviation “EPM”), and silicones.

[0074] According to a specific embodiment, the first ML1 binder material is a mixture of thermoplastic polymer(s), heat-shrinkable polymer(s) and / or elastomeric polymer(s).

[0075] Other suitable early binder materials ML1 comprise crosslinked polymers, such as those produced with polymers containing carboxyl groups and crosslinking agents.

[0076] Other suitable primary ML1 binders comprise cellulose derivatives.

[0077] The first composition C1 comprises a weight concentration of the first binder material ML1 of less than or equal to 30%, preferably less than or equal to 20%.

[0078] The first conductive additive AC1 includes one or more types of conductive elements, in order to increase electronic conductivity.

[0079] Examples of conductive elements include, but are not limited to, conductive carbons, graphites, graphenes, carbon nanotubes, activated carbon fibers, non-activated carbon nanofibers, metal flakes, metal powders, metallic fibers and electrically conductive polymers.

[0080] A nanofiber is defined as a fiber with a diameter Petition 870240061031, dated 07 / 19 / 2024, page 30 / 117 16 / 44 with a maximum dimension of 1 nm to 200 nm and extending along a direction normal to the aforementioned diameter.

[0081] A nanotube is defined as a tube with an outer diameter with a maximum dimension of 1 nm to 100 nm and extending along a direction normal to the said diameter.

[0082] The first composition C1 comprises a weight concentration of the first conductive additive AC1 of less than or equal to 20%, preferably below 10%.

[0083] The thickness e21 of electrode 21 varies depending on the amount of silicon contained in electrode 21.

[0084] The higher the amount of silicon contained in electrode 21, the smaller the thickness e21 of electrode 21. A higher amount of silicon, therefore, allows for an increase in the energy density of anode 16.

[0085] In the example described, electrode 21 is separated from substrate 20 by interface layer 22.

[0086] The interface layer 22 has a first face 221 in contact with the face 212 of electrode 21 and a second face 22 in contact with the first face 201 of substrate 20.

[0087] The first face 221 and the second face 222 of the interface layer 22 are perpendicular to the Z stacking direction and parallel to each other.

[0088] The interface layer 22 has a thickness e22 less than or equal to 10 pm. Preferably, the thickness e22 is greater than or equal to 10 nm. More preferably, the thickness e22 is greater than or equal to 100 nm.

[0089] Conveniently, the e22 thickness is 10 nm to 3 pm.

[0090] The interface layer 22 is produced by depositing a second composition C2 onto the substrate. Preferably, the interface layer 22 is produced by coating the second Petition 870240061031, dated 07 / 19 / 2024, page 31 / 117 17 / 44 composition C2 on the first face 201 of substrate 20.

[0091] The second composition C2 includes second binder material ML2 and second conductive additive AC2.

[0092] The second conductive additive AC2 comprises one or more types of conductive elements that allow for increased electronic conductivity.

[0093] The second conductive additive AC2 is selected, for example, from carbon, carbon black, graphite, graphene, carbon nanotubes, activated carbon fibers, non-activated carbon nanofibers, metal flakes, metal powders, metal fibers and electrically conductive polymers.

[0094] Preferably, the second conductive additive AC2 is selected, but not limited to, carbon nanofibers and carbon nanotubes.

[0095] The second composition C2 comprises a weight concentration of the second conductive additive AC2 greater than or equal to 20%.

[0096] Preferably, the second composition C2 comprises a weight concentration of the second conductive additive AC2 of less than or equal to 70%.

[0097] Conveniently, the second composition C2 comprises a weight concentration of the second conductive additive AC2 of 30% to 60%.

[0098] The choice of the second binder material ML2 is not particularly limited, provided that the second binder material ML2 is inert with respect to the other materials of the second composition C2.

[0099] The second binder material ML2 comprises one or more polymers selected from thermoplastic polymers, heat-shrinkable polymers, elastomers and mixtures thereof. Petition 870240061031, dated 07 / 19 / 2024, page 32 / 117 18 / 44

[00100] Examples of thermoplastic polymers include, without limitation, polymers resulting from the polymerization of aliphatic or cycloaliphatic vinyl monomers, such as polyolefins (including polyethylenes or polypropylenes), polymers resulting from the polymerization of aromatic vinyl monomers, such as polystyrenes, polymers resulting from the polymerization of acrylic and / or (meth)acrylate monomers, polyamides, polyether ketones and polyimides.

[00101] Examples of heat-shrinkable polymers include, but are not limited to, heat-shrinkable resins (such as epoxy resins and polyester resins) possibly mixed with polyurethanes or polyether polyols.

[00102] Examples of elastomeric polymers include, but are not limited to, natural rubbers, synthetic rubbers, styrene-butadiene copolymers (also known by the abbreviation “SBR”), ethylene-propylene copolymers (also known by the abbreviation “EPM”), and silicones.

[00103] Other suitable secondary ML2 binder materials comprise cross-linked polymers, such as those produced with polymers containing carboxyl groups and cross-linking agents.

[00104] Other suitable secondary ML2 binder materials comprise cellulose derivatives.

[00105] The second composition C2 comprises a weight concentration of the second binder material ML2 greater than or equal to 30%.

[00106] Preferably, the second composition C2 comprises a weight concentration of the second binder material ML2 of less than or equal to 80%.

[00107] Conveniently, the second composition C2 Petition 870240061031, dated 07 / 19 / 2024, page 33 / 117 19 / 44 comprises a weight concentration of the second binder material ML2 of 40% to 70%.

[00108] Interface layer 22 is characterized by the roughness of the first face 221 of interface layer 22.

[00109] By definition, the roughness of the first face 221 of the interface layer 22 represents the amplitude of the reliefs of the first face 221 of the interface layer 22. The amplitude of the reliefs of the first face 221 of the interface layer 22 corresponds to the distance between the highest point and the lowest point of said reliefs, also called the peak-to-valley distance and indicated as Rt.

[00110] The reliefs of the first face 221 of the interface layer 22 may also be incorrectly defined as defects of the first face 221 of the interface layer 22.

[00111] The amplitude of the reliefs of the first face 221 of the interface layer 22 has a depth of 10 nm to 10 pm, preferably 2 pm to 9 pm. The amplitude of the reliefs of the first face 221 of the interface layer 22 may also have a depth of 0.5 pm to 9 pm, preferably 0.5 pm to 8 pm, more preferably 0.5 pm to 6 pm, conveniently 1 pm to 6 pm.

[00112] The reliefs on the first face 221 of the interface layer 22 are a consequence of the mixture of the components of the second composition C2. The second conductive additive AC2 and the second binder material ML2 are selected so that the interlacing of the components generates reliefs in a random and relatively homogeneous way over the entire surface of the first face 221 of the interface layer 22.

[00113] The weight quantities of the second conductive additive AC2 and the second binder material ML2 allow modulating the roughness of the first face 221 of the interface layer 22. Petition 870240061031, dated 07 / 19 / 2024, page 34 / 117 20 / 44

[00114] The size and shape of the particles of the second conductive additive AC2 also allow modulating the roughness of the first face 221 of the interface layer 22. The smaller the surface area of ​​the particles of the second conductive additive AC2, the smaller the amplitude of the reliefs of the first face 221 of the interface layer 22.

[00115] In addition, particles in the form of flakes or fibers are used to generate greater amplitude of the reliefs.

[00116] In one variant, the roughness of the first face 221 of the interface layer 22 is modified by a surface treatment.

[00117] The roughness of the interface layer 22 is modified, for example, by using a plasma torch on the surface of the first face 221 of the interface layer 22.

[00118] The roughness of the first face 221 of the interface layer 22 is determined by means of white light interferometry measurement, for example, by a nanometric non-contact surface survey station (OptoSurf brand). The survey station allows the first face 221 of the interface layer 22 to be reconstructed in 2D and 3D and then its roughness to be calculated.

[00119] The roughness of the first face 221 of the interface layer 22 is defined from at least two distinct zones of the first face 221 of the interface layer 22.

[00120] The roughness of the first face 221 of the interface layer 22 is equal to the average of at least two relief amplitude values, where each relief amplitude value corresponds to a distinct zone of the first face 221 of the interface layer 22. The relief amplitude of a distinct zone of the first face 221 of the interface layer 22 indicates the distance between the upper and lower points of said zone. The extent of each distinct zone of the first face 221 of the interface layer 22 is, therefore Petition 870240061031, dated 07 / 19 / 2024, p. 35 / 117 21 / 44 example, of 40,000 pm2.

[00121] In the proposed example, the interface layer 22 completely covers the surface.

[00122] In one variant, the interface layer 22 is perforated. The first face 201 of the substrate 20 is therefore not fully covered by the interface layer 22.

[00123] The second face 222 of the interface layer 22 has an extension A22.

[00124] The first face 201 of substrate 20 has an extension A201.

[00125] The interface layer 22 is characterized by a coverage level R(i / s) of face 201 of substrate 20.

[00126] The coverage ratio R(i / s) corresponds to the ratio between the extent A22 of the second face 222 of the interface layer 22 and the extent A201 of the first face 201 of the substrate 20 and is calculated according to the following formula: R(i / s) = A22 / A201

[00127] The coverage ratio R(i / s) is from 0.1 to 1. Preferably, the coverage ratio R(i / s) is 0.3 to 1. Conveniently, the coverage ratio R(i / s) is 0.7 to 1. Even more preferably, the coverage ratio R(i / s) is strictly less than 1, preferably 0.1 to 0.9 and, conveniently, 0.7 to 0.9.

[00128] The operation of anode 16 is in accordance with the operation of an anode according to the state of the art.

[00129] Interface layer 22 improves the interface between substrate 20 and electrode 21.

[00130] In particular, a thickness of less than 10 pm of the 22-layer interface conveniently enhances the interface between the Petition 870240061031, dated 07 / 19 / 2024, p. 36 / 117 22 / 44 substrate 20 and electrode 21 and reduce the electrical resistance between substrate 20 and electrode 21.

[00131] The presence of the interface layer 22 between the substrate 20 and the electrode 21 allows for improved adhesion between the different layers of the anode 16, which significantly increases its efficiency.

[00132] Furthermore, the perforated appearance of the interface layer 22 and the roughness of the second face 222 of the interface layer 22 allow for a reduction in electrical resistance between the substrate 20 and the electrode 21. The high resistance acts, however, as a barrier against electron transfer during the electrochemical cell cycle 10.

[00133] The interface layer 22 therefore has an important effect on the electronic conductivity of the anode 16, as it provides a better interface between the substrate 20 and the electrode 21 and preserves good electrical contact between the substrate 20 and the electrode 21.

[00134] The presence of interface layer 22 also increases the conduction path.

[00135] The electrochemical performance of anode 16 is therefore significantly enhanced by the presence of the interface layer 22.

[00136] The improved interface resulting from the perforated appearance of the interface layer 22 and the roughness of the second face 222 of the interface layer 22 disposed between the substrate 20 and the electrode 21 also limits the deterioration and delamination of the anode 16, caused by the volume expansion of silicon particles during the charging and discharging cycles of the electrochemical cell 10. The cycle capacity retention and service life of the anode 16 are therefore improved.

[00137] According to a variant shown in Figure 3, the interface layer 22 consists of a set 38 comprising a series Petition 870240061031, dated 07 / 19 / 2024, page 37 / 117 23 / 44 of elements 40.

[00138] Elements 40 are distributed uniformly over the entire surface of the first face 201 of the substrate 20.

[00139] The number of elements 40 is indicated by n.

[00140] According to the example described, each element 40 is identical.

[00141] Each element 40 of the interface layer 22 is in contact with the first face 201 of the substrate and with the face 212 of the electrode 21.

[00142] Each element 40 of the interface layer 22 has a base 401.

[00143] The base 401 of each element 40 is in contact with the first face 201 of the substrate 20.

[00144] Each 401 base is a disk that has a larger diameter with length d1. The diameter d1 varies from 200 pm to 1000 pm, preferably 500 pm to 900 pm.

[00145] Each base 401 has a center.

[00146] Each base 401 has an extension A401.

[00147] The A401 extension of each 401 base is 0.03 mm2a 0.8 mm2.

[00148] Each element 40 is a volume generated from its base 401.

[00149] In the example described, elements 40 are domes.

[00150] Each element 40 of the interface layer 22 has a height H40 less than or equal to 10 pm. Preferably, each element 40 of the interface layer 22 has a height H40 less than or equal to 6 pm. More preferably, each element 40 of the interface layer 22 has a height H40 greater than or equal to 10 nm. More preferably, each element 40 Petition 870240061031, dated 07 / 19 / 2024, page 38 / 117 24 / 44 of the 22 interface layer has an H40 height greater than or equal to 0.5 pm. Conveniently, each 40 element of the 22 interface layer has an H40 height of 10 nm to 3 pm.

[00151] This height H40 of the elements 40 allows for an increase in the contact surface with the electrode 21 and therefore improves the electrical contact between the substrate 20 and the electrode 21. This height H40 of the elements also makes it possible to limit the mechanical stresses associated with volume variations of the intercalation material MI of the electrode 21.

[00152] As can be seen in Figure 3, the interface layer 22 is formed by n discrete elements 40 that form the set 38. The first face 201 of the substrate 20, therefore, is not completely covered by the various elements 40.

[00153] The interface layer 22 is characterized by a coverage ratio R(r / s) of the first face 201 of the substrate 20.

[00154] The coverage ratio R(r / s) corresponds to the ratio between the extent A22 of the interface layer 22 and the extent A201 of the first face 201 of the substrate 20.

[00155] The A22 extent of interface layer 22 is defined as the sum of the A401 extents of the base 401 of the n elements 40 of interface layer 22. The A22 extent of interface layer 22 is calculated according to the following formula: A 22 = ΣΛ 401i where i indicates the area A401.

[00156] According to the example described, the 401 bases are all identical and the A22 extent of the interface layer is calculated according to the following formula: A22 = nx A401

[00157] The coverage ratio R(r / s) is calculated according to Petition 870240061031, dated 07 / 19 / 2024, p. 39 / 117 25 / 44 using the following formula: R(r / s) = A22 / A201

[00158] Preferably, the coverage ratio R(r / s) is 0.1 to 0.9.

[00159] Conveniently, the coverage ratio R(r / s) is 0.2 to 0.5.

[00160] The fact that the first face 201 of the substrate 20 is not fully covered by the interface layer 22 can be used to generate a relief on the first face 201 of the substrate 20, which makes it possible to increase the contact surface with the electrode 21 and, therefore, improve the electrical contact between the substrate 20 and the electrode 21. In this way, the mechanical stresses generated by the volume variations of the active material of the electrode 21 during the operation of the electrochemical cell 10 can also be limited. Modulating the coverage ratio R(r / s) also allows reducing the electrical resistance between the substrate 20 and the electrode 21 compared to the case where the coverage ratio is equal to 1.

[00161] The 40 elements of the interface layer 22 are produced by depositing a third composition C3 onto the first face 201 of the substrate 20. Preferably, the 40 elements of the interface layer 22 are produced by coating the first face 201 of the substrate 20 with the third composition C3.

[00162] The third composition C3 includes the third conductive additive AC3 and, if appropriate, the third binder material ML3. Conveniently, the third composition C3 consists of the third conductive additive AC3 and the third binder material ML3.

[00163] The third conductive additive AC3 includes one or more conductive elements to increase electronic conductivity.

[00164] The third conductive additive AC3 is selected, by Petition 870240061031, dated 07 / 19 / 2024, page 40 / 117 26 / 44 example, from carbon, carbon black, graphite, graphene, carbon nanotubes, activated carbon fibers, non-activated carbon nanofibers, metal flakes, metal powders, metallic fibers and electrically conductive polymers.

[00165] The third composition C3 comprises a weight concentration of the third conductive additive AC3 greater than or equal to 20%.

[00166] Preferably, the third composition C3 comprises a weight concentration of the third conductive additive AC3 of less than or equal to 90%.

[00167] Conveniently, the weight concentration of the third conductive additive AC3 included in the third composition C3 is 40% to 70%.

[00168] The third binder material ML3 consists of one or more polymers selected from thermoplastic polymers, heat-shrinkable polymers, elastomers and mixtures thereof.

[00169] Thermoplastic polymers, heat-shrinkable polymers and elastomers are as defined above.

[00170] The third composition C3 comprises a weight concentration of the third binder material ML3 greater than or equal to 10%.

[00171] Preferably, the third composition C3 comprises a weight concentration of the third binder material ML3 of less than or equal to 80%.

[00172] Conveniently, the weight concentration of the third binding material ML3 included in composition C3 is 30% to 60%.

[00173] The n elements 40 of the interface layer 22 are arranged according to different variants.

[00174] According to the examples shown in Figures 4, 5 and 6, Petition 870240061031, dated 07 / 19 / 2024, page 41 / 117 27 / 44 the n elements 40 of the interface layer 22 are arranged in corresponding elementary meshes, where each elementary mixture is identical. According to the example shown in Figure 7, the n elements 40 of the interface layer are randomly distributed over the first face 201 of the substrate 20.

[00175] According to the variant shown in Figure 4, the elementary mesh 50 of the interface layer 22 is provided by four bases 401 arranged in a square.

[00176] In this way, the four vertices of the elementary grid form a square, where each vertex is the center of a base 401.

[00177] The elementary mesh 50 has one side defined by a segment that connects the center of two adjacent bases 401.

[00178] The side of the elementary mesh 50 has a length c1 of 400 pm to 3500 pm, preferably 600 pm to 2000 pm.

[00179] Set 38 corresponds to the periodic repetition of elementary grid 50 along the X and Y directions, where the X and Y directions are normal to each other and to the Z direction.

[00180] The operation of anode 16 according to the variant shown in Figures 3 and 4 is in accordance with the operation of anode 16 as shown in Figure 2.

[00181] The advantages of anode 16 according to this variant are similar to the advantages of anode 16 as shown in Figure 2.

[00182] Furthermore, the organization of the interface layer into a series of 40 elements arranged in an elementary mesh provides a homogeneous anode across its entire dimension. The pattern repeatability provides better anode reproducibility and better electrochemical performance reproducibility.

[00183] According to the variant shown in Figure 5, the bases Petition 870240061031, dated 07 / 19 / 2024, page 42 / 117 28 / 44 401 of the 40 elements in interface layer 22 are square.

[00184] Each base 401 is defined by a diagonal with length d2. The length d2 varies from 200 pm to 1200 pm, preferably 500 pm to 1000 pm.

[00185] The elementary mesh 60 of the interface layer 22 is provided by five bases 401 that form a centered square.

[00186] In this way, the four vertices of the elementary grid form a square, where each vertex is the center of a 401 base, and the center of the fifth 401 base is located at the center of the aforementioned square.

[00187] The elementary mesh 60 has a side defined by a segment that connects the center of two adjacent bases 401 selected from the four bases 401 that form the square.

[00188] The side of the elementary mesh 60 is defined by the length c2. The length c2 varies from 400 pm to 3,700 pm, preferably 600 pm to 2,200 pm.

[00189] The set 38 therefore corresponds to the periodic repetition of the elementary grid 60 along the X and Y directions, where the X and Y directions are normal to each other and to the Z direction.

[00190] The operation of anode 16 according to the variant shown in Figure 5 is in accordance with the operation of anode 16 as shown in Figures 3 and 4.

[00191] The advantages of anode 16 according to this variant are similar to the advantages of anode 16 as shown in Figures 3 and 4.

[00192] Furthermore, the arrangement of the n staggered elements 40 allows for an increase in the coverage ratio R(r / s) and, therefore, an increase in the contact surface with the electrode 21. The fact that the bases 401 of the elements 40 are squares also allows for an increase in the coverage ratio. Petition 870240061031, dated 07 / 19 / 2024, page 43 / 117 29 / 44 coverage R(r / s).

[00193] In another example shown in Figure 6, the elementary mesh consists of an elementary mesh 70 corresponding to the elementary mesh 60 according to Figure 5, where the bases 401 are disks.

[00194] Each 401 base is defined by a diameter with length d3. The length d3 varies from 200 pm to 1200 pm, preferably 500 pm to 1000 pm.

[00195] The elementary mesh 70 has one side defined by the length c3. The length c3 varies from 400 pm to 3500 pm, preferably 600 pm to 2000 pm.

[00196] Set 38 therefore corresponds to the periodic repetition of elementary grid 70 along the X and Y directions, where the X and Y directions are normal to each other and to the Z direction.

[00197] The operation of anode 16 according to the variant shown in Figure 6 is in accordance with the operation of anode 16 as shown in Figures 3 and 4.

[00198] The advantages of anode 16 according to this variant are similar to those of anode 16 as shown in Figures 3 and 4.

[00199] Furthermore, the staggered arrangement of the n elements 40 allows for an increase in the coverage ratio R(r / s) and, therefore, an increase in the contact surface with electrode 21.

[00200] According to the example shown in Figure 7, the n elements 40 of the interface layer 22 are randomly distributed over the first face 201 of the substrate 20.

[00201] Two adjacent elements 40 are separated by a distance Dadj, where the distance Dadj is the shortest distance between two points of the two adjacent elements 40.

[00202] Two adjacent elements 40 form a pair of Petition 870240061031, dated 07 / 19 / 2024, page 44 / 117 30 / 44 adjacent 40 elements, where the pair of adjacent 40 elements consists of the first 40 element and the second 40 element. Each 40 element of the 22 interface layer is comprised within at least one pair of adjacent 40 elements. The Dadj distance represents the shortest distance between a point on the 401 base of the first 40 element of the pair of adjacent 40 elements and a point on the 401 base of the second 40 element of the pair of adjacent 40 elements.

[00203] The Dadj distance of each pair of adjacent 40 elements of the 22 interface layer is 200 pm to 2,500 pm, preferably 400 pm to 1,000 pm.

[00204] In other words, each element 40 of the interface layer 22 is separated from the set of adjacent elements 40 by a distance Dadj of 200 pm to 2500 pm, preferably 400 pm to 1000 pm.

[00205] Each 401 base has the same shape, where the shape is selected from one of the 401 bases according to Figures 4, 5 and 6.

[00206] The operation of anode 16 according to the variant shown in Figure 7 is in accordance with the operation of anode 16 as shown in Figure 3.

[00207] The advantages of anode 16 according to this variant are similar to those of anode 16 as shown in Figure 3.

[00208] Furthermore, organizing the interface layer into a series of 40 elements arranged in a set provides a homogeneous anode across its entire dimension.

[00209] As a result of the examples according to the In Figures 3, 4, 5, 6, and 7, the base 401 of each element 40 of the interface layer 22 is a polygon or oval.

[00210] The geometry of the base 401 of the elements 40 allows Petition 870240061031, dated 07 / 19 / 2024, page 45 / 117 31 / 44 adjust the coverage ratio R(r / s).

[00211] Each base 401 of the elements 40 of the interface layer 22 is in contact with the first face 201 of the substrate 20. Each element 40 additionally has a surface 402. The surfaces 402 of the elements 40 are not in contact with the first face 201 of the substrate 20.

[00212] Preferably, the surface 402 of each element 40 has roughness.

[00213] The surface roughness 402 of each element 40 indicates the amplitude of surface release 402 of each element 40.

[00214] The surface roughness 402 of each element 40 is determined according to the same method described above for determining the roughness of the second face 222 of the interface layer 22.

[00215] Preferably, the surface roughness 402 of each element 40 is 10 nm to 10 pm, preferably 0.5 pm to 9 pm, preferably 0.5 pm to 8 pm, most preferably 0.5 pm to 6 pm, conveniently 1 pm to 6 pm, most conveniently 2 pm to 6 pm.

[00216] The surface roughness 402 of each element 40 is modulated by the size, shape and quantity of the components of the composition C3.

[00217] According to another variant shown in Figure 8, the anode comprises two interface layers 22.

[00218] The two interface layers 22 are superimposed on each other along the Z stacking direction.

[00219] The first interface layer 22 is in contact with the first face 201 of the substrate and the second interface layer 22 is in contact with the first face 212 of the electrode.

[00220] The first interface layer 22 corresponds to Petition 870240061031, dated 07 / 19 / 2024, page 46 / 117 32 / 44 interface layer 22 according to Figure 2.

[00221] The second interface layer 22 corresponds to the interface layer 22 according to Figures 3 to 6.

[00222] More generally, the example of anode 16 according to Figure 8 demonstrates that anode 16 comprises a number p of interface layers 22, where p is an integer greater than or equal to 2. Preferably, p is 2 to 4.

[00223] The p interface layers 22 of anode 16 are superimposed on each other along the Z stacking direction.

[00224] The p interface layers 22 of anode 16 are successively deposited on top of each other by means of deposit, preferably by coating, of the second composition C2 or the third composition C3.

[00225] The second composition C2 and the third composition C3 are different for each of the 22 interface layers.

[00226] The operation of anode 16 according to this variant is in accordance with the operation of anode 16 as shown in Figures 2 to 7.

[00227] The advantages of anode 16 are similar to those of anode 16 as shown in Figures 2 and 7.

[00228] Furthermore, the presence of at least two interface layers 22 allows for greater relief than with a single interface layer 22, which makes it possible to increase the contact area with the electrode 21 and, therefore, improve the electrical contact between the substrate 20 and the electrode 21. By modulating the compositions, in addition to the coverage ratio of the at least two interface layers, it is possible to shape the interfaces between the different layers and increase the electrochemical performance of the anode 16. The composition of the first interface layer 22 can, for example, increase the adhesion of the electrode 21 to the substrate 20, while the composition of the Petition 870240061031, dated 07 / 19 / 2024, page 47 / 117 33 / 44 The second interface layer 22 would allow for a significant increase in conductivity inside anode 16. It is therefore possible to add the benefits provided by each interface layer 22 and maximize the performance of anode 16 thanks to their interactions.

[00229] Preferably, in all embodiments, interface layer 22 has roughness.

[00230] The interface layer 22 has a face that is not in contact with the first face 201 of the substrate 20.

[00231] The face of the interface layer 22 that is not in contact with the first face 201 of the substrate 20 corresponds to face 221 shown in Figure 2 or to all faces 402 of the discrete elements 40 shown in Figure 3.

[00232] The roughness of the interface layer 22 represents the relief amplitude of the face of the interface layer 22 that is not in contact with the first face 201 of the substrate 20.

[00233] The roughness of the interface layer face 22 that is not in contact with the first face 201 of the substrate 20 is determined by measuring white light interferometry, for example, using a nanometric non-contact surface survey station (OptoSurf brand). The survey station allows the reconstruction, in 2D and 3D, of the interface layer face 22 that is not in contact with the first face 201 of the substrate 20, in order to determine its roughness.

[00234] The roughness of interface layer 22 is defined from at least two distinct zones of the face of interface layer 22 that is not in contact with the first face 201 of substrate 20. For each zone, the relief amplitude Rt is determined, that is, the distance between the highest point and the lowest point of the said zone.

[00235] The roughness of interface layer 22 is equal to Petition 870240061031, dated 07 / 19 / 2024, p. 48 / 117 34 / 44 average value, indicated by Rtm, of at least two relief amplitude values ​​Rt, where each relief amplitude value Rt corresponds to a distinct zone of the face of the interface layer 22 that is not in contact with the first face 201 of the substrate 20.

[00236] The advantage of dividing the surface of the face of the interface layer 22 that is not in contact with the first face 201 of the substrate 20 into at least two distinct zones to measure the average amplitude of the reliefs is the limitation of the uncertainty associated with the possible lack of homogeneity of the face of the interface layer 22 that is not in contact with the first face 201 of the substrate 20.

[00237] The surface area of ​​each distinct zone of the interface layer face 22 that is not in contact with the first face 201 of the substrate 20 defined to determine the roughness of the interface layer 22 measures, for example, 40,000 pm2.

[00238] Preferably, the surface roughness 22 is from nm to 10 pm, preferably 0.5 pm to 9 pm, more preferably 0.5 pm to 8 pm, even more preferably 0.5 pm to 6 pm, conveniently 1 pm to 6 pm, most conveniently 2 pm to 6 pm.

[00239] The roughness of the interface layer 22 allows for better electrical percolation inside the electrode 21 and increases the electron exchange surface with the current collector 23.

[00240] Preferably, in all embodiments, the interface layer 22 has a coverage ratio R(ci / s) of the first face 201 of the substrate 20 strictly less than 1. The first face 201 of the substrate 20 is therefore not fully covered by the interface layer 22.

[00241] The interface layer 22 has one face in contact with the first face 201 of the substrate 20.

[00242] The face of interface layer 22 in contact with the Petition 870240061031, dated 07 / 19 / 2024, page 49 / 117 35 / 44 first face 201 of substrate 20 corresponds, for example, to face 222 shown in Figure 2 or to the set of bases 401 of discrete elements 40 shown in Figure 3.

[00243] The face in contact with the first face 201 of the substrate 20 has an extension of A22.

[00244] The first face 201 of substrate 20 has an extension A201.

[00245] The coverage ratio R(ci / s) of the first face 201 of substrate 20 corresponds to the ratio between the extent A22 of the face in contact with the first face 201 of substrate 29 and the extent 201 of the first face 201 of substrate 20 and is calculated according to the following formula: R(ci / s) = A22 / A201

[00246] The coverage ratio R(ci / s) is preferably greater than or equal to 0.1.

[00247] Preferably, the coverage ratio R(ci / s) is 0.1 to 0.9, conveniently 0.2 to 0.9.

[00248] Modulation of the coverage ratio of the first face 201 of substrate 20 makes it possible to reduce the electrical resistance between substrate 20 and electrode 21 compared to the case where substrate 20 is completely covered by the interface layer 22 (coverage ratio equal to 1).

[00249] According to a variant shown in Figure 9, the current collector 23 associated with the electrode 21 to form the anode 16 comprises two interface layers 22.

[00250] The first and second interface layers 22 have thickness as defined above and a coverage ratio of the first face 201 of the substrate 20 which is strictly less than 1.

[00251] Without wishing to restrict any theory, the inventors believe that, since electrons have at least four Petition 870240061031, dated 07 / 19 / 2024, page 50 / 117 36 / 44 possible paths from electrode 21 to substrate 20 (moving directly from electrode 21 to substrate 20 without crossing any interface layer, crossing only the first interface layer 22, crossing only the second interface layer 22, or crossing both interface layers 22, as shown in Figure 9), where each path has different conductivity characteristics, allowing electrons to follow one or more paths in a preferred way, electron transmission is enhanced.

[00252] The first face 201 of the substrate 20 is preferably substantially soft. “Substantially soft” means that the surface roughness of the substrate 20, measured with a profilometer, is less than or equal to 500 nm, preferably less than or equal to 200 nm, preferably less than or equal to 80 nm, most preferably less than or equal to 50 nm, conveniently less than or equal to 20 nm.

[00253] The thickness e22 of the 22 interface layer is preferably from 10 nm to 10 pm. If the thickness of the 22 interface layer is greater than 10 pm, the interface layer occupies too much volume and weight to the detriment of the materials that form the electrode, which would induce a loss of energy density in the electrochemical cell. On the other hand, the minimum thickness of the 22 interface layer is controlled by the application method and / or the composition from which it is obtained. An interface layer produced by liquid coating, for example, may have a thickness greater than or equal to 100 nm.

[00254] Preferably, the thickness e22 of the 22 interface layer is greater than or equal to 100 nm.

[00255] Conveniently, the thickness e22 of the interface layer 22 is preferably from 0.5 pm to 6 pm.

[00256] Throughout this descriptive report, the thickness of the interface layer 22 corresponds to the maximum thickness of Petition 870240061031, dated 07 / 19 / 2024, page 51 / 117 37 / 44 mentioned interface layer 22.

[00257] In addition to increasing the exchange surface of the current collector 23 with the electrode 21, the presence of at least one interface layer 22 makes it possible to limit the deterioration and delamination of the anode 16, caused by the volume expansion of the intercalation material of the electrode 21. This phenomenon is particularly very present in silicon anodes, where the active material can reach volume changes of 300%.

[00258] Concrete, but by no means exhaustive, examples illustrate collector achievements and will be provided below. Examples Example 1 Measuring the roughness of the interface layer according to its COMPOSITION

[00259] The roughness of three different interface layers was measured. The composition of the three interface layers differs because the proportion of fibers among the conductive additives is different in each layer, which makes it possible to assess the impact of the shape of the additives on the roughness of the interface layers. The compositions of the three interface layers were as follows: - Formulation A: 0% by weight of fibers to 100% by weight of carrying additives; - Formulation B: 23% by weight of fibers to 100% by weight of carrying additives; - Formulation C: 29% by weight of fibers to 100% by weight of conducting additives; and - the remainder of the driving additives consists of ovoid particles. [ 00260] Five Rtm measurements were performed on each Petition 870240061031, dated 07 / 19 / 2024, page 52 / 117 38 / 44 interface layer, using the method detailed in the descriptive report. The Rtm measurement corresponds to the average of the Rt measurements of each zone, with the analysis surface of each interface layer divided into 25 zones.

[00261] The results obtained are presented in the following table. Rtm (pm) Formulation A Formulation B Formulation C Analysis 1 3.272 6.338 7.017 Analysis 2 3.289 6.853 7.322 Analysis 3 3.241 6.895 7.959 Analysis 4 2.938 6.899 7.899 Analysis 5 3.421 7.425 7.643 Average value 3.232 6.882 7.568 Standard deviation 0.178 0.385 0.398

[00262] These results demonstrate that it is possible to modulate the roughness of the interface layer by selecting the components of the composition and, particularly, by means of conductive additives. It is shown here that particles in the form of fibers generate greater amplitude of the reliefs and, the higher the amount of fiber mass in the composition, the greater the amplitude. Example 2 Evaluation of the adhesion of the interface layer to the substrate.

[00263] A characterization method was developed to evaluate the adhesion quality of the interface layer to the substrate. For this purpose, peel resistance characterization was conducted on a substrate coated with one or more interface layers using an adhesive. The protocol was as follows: - application of the adhesive to the surface of the interface layer that has a peel-off adhesion strength at 180° of 7.5 N / cm (ASTM D3330); - applying adhesive pressure to the interface layer with a roller 2.6 kg; to ensure that the application pressure of the adhesive to the coating Petition 870240061031, dated 07 / 19 / 2024, p. 53 / 117 39 / 44 was the same for the different samples analyzed and to allow for better reproducibility of the test; - removal of the adhesive from the interface layer by peeling at 180°; and - Analysis of the appearance of the interface layer and the adhesive face in contact with the coating. If the interface layer has been completely removed from the substrate in certain areas and is present on the adhesive, delamination is present: the adhesion of the interface layer to the substrate is considered to be of poor quality.

[00264] Three current collector configurations were studied: - Sample A (EchA): interface layer formed from a C2 composition with a binder concentration by weight of 60% to 65% and a conductive additive concentration by weight of 35% to 40%, deposited on a copper plate with a coverage ratio of 0.9; - Sample B (EchB): interface layer formed from a C3 composition with a binder concentration by weight of 50% to 55% and a conductive additive concentration by weight of 45% to 50%, deposited on a copper plate with a coverage ratio of 0.27; and - Sample C (EchC): first interface layer formed from a C2 composition identical to that of sample EchA, deposited on a copper plate, and formation of a second interface layer formed with a C3 composition identical to sample EchB deposited on the interface layer with composition C2, in order to form an overlap of interface layers.

[00265] The nature of the binder material and the conductive additive are the same between composition C2 and composition C3.

[00266] The peeling resistance of the layers of Petition 870240061031, dated 07 / 19 / 2024, page 54 / 117 The 40 / 44 interface of the different samples was characterized using the protocol detailed above.

[00267] The results obtained are presented in the following table. Current collector EchA EchB EchC Interface layer appearance after stripping No delamination Delamination No delamination

[00268] No delamination was found for the sample. EchA, unlike sample EchB, has a higher concentration of binder material in composition C2 than in composition C3 of sample EchB. This results in better adhesion of the interface layer to the copper plate. Sample EchC, however, did not exhibit delamination. The interface layer with composition C3 therefore has good adhesion quality to the C2 interface layer. The overlapping of different interface layers allows the use of a C3 composition, which has a higher concentration of conductive additive than composition C2 and therefore generates better interface quality and better electrical percolation in contact with the electrode. It can be considered that this overlapping provides good electrode-substrate adhesion quality through C2 and increased electrical performance through the layer obtained from composition C3.It is therefore demonstrated that the overlapping of interface layers allows the introduction of a new interface or even an interface with a controlled conductivity gradient, which is more conductive, something that would not have been possible without this arrangement. In the case of the EchC sample, the benefits provided by each interface layer are then accumulated, making it possible to maximize the anode's performance thanks to their interactions.

[00269] It can also be considered that a similar result would be obtained if the nature of the binder material in composition C3 were different from composition C2. In fact, the choice of binder material Petition 870240061031, dated 07 / 19 / 2024, page 55 / 117 41 / 44 of composition C3 can be adapted for better compatibility with the electrode composition, and the adhesion of the metal plate assembly is provided by composition C2. In this way, this arrangement allows for a wider choice of the binder material and / or conductive additive and its weight concentration in the composition of the interface layer in contact with the electrode, since the latter is not limited by its ability to adhere to the metal plate.

[00270] The Applicant has further demonstrated that the geometry of the bases of the interface layer formed with composition C3 does not have a significant impact on the adhesion test results. Example 3 Impedance measurement of electrochemical cells comprising different interface layers.

[00271] The electrochemical cells were produced by the following successive layers: - a current collector; - an electrode deposited on the first current collector, in which the intercalation material is S'tile silicon, the binder material ML1 is PAA (ThermoFisher Scientific) and the conductive additive AC1 is SUPER P®-Li carbon (Imerys Graphite & Carbon); - a separator, a polypropylene membrane (Celgard® type), impregnated with LiPF6 EC DMC 2% FEC electrolyte; and - a lithium metallic counter electrode.

[00272] All these elements have a multilayer system assembled in a coin cell battery, forming the electrochemical cell. In this assembly, the electrode containing silicon cannot be considered "negative" because the counter electrode is metallic lithium.

[00273] Five electrochemical cells were produced, comprising five different current collectors: Petition 870240061031, dated 07 / 19 / 2024, page 56 / 117 42 / 44 - a reference current collector (CCREF1), as a comparative example, consisting of a copper plate (circuit board) with a thickness of 10 pm, without an interface layer; - a reference current collector 2 (CCREF2), as a second comparative example, consisting of a copper plate (circuit board) with a thickness of 10 µm and an interface layer with a coverage ratio of 1 (100%), composed of 45% conductive additive and 55% binder material, with a thickness of 3 µm and a roughness of 0.5 µm; - a current collector (CC1) according to the embodiment shown in Figure 5, composed of a copper plate (Circuit Board) with a thickness of 10 pm, as well as an interface layer structured in a set of a series of elements in a staggered arrangement, where the base of each element is a square, the coverage ratio of 0.27 (i.e., 27% over the substrate surface), composed of 45% conductive additive and 55% binder material, with an element height of 3 pm; - a current collector (CC2) according to the embodiment shown in Figure 4, composed of a copper plate (Circuit Board) with a thickness of 10 µm, as well as an interface layer structured in a series of elements, wherein the base of each element is a disc, the coverage ratio of 0.21 (i.e., 21% over the substrate surface), composed of 45% conductive additive and 55% binder material, with an element height of 3 µm; and - a current collector (CC3) according to the embodiment shown in Figure 6, composed of a copper plate (Circuit Board) with a thickness of 10 µm, as well as an interface layer structured in a series of staggered elements, where the base of each element is a disc, the coverage ratio of 0.27 (i.e., 27% over the substrate surface), composed of 45% conductive additive and 55% Petition 870240061031, dated 07 / 19 / 2024, page 57 / 117 43 / 44 of binder material, with an element height of 2 µm.

[00274] The electrical performance of the cells was characterized by a VMP3 multipotentiostat (Biologic).

[00275] A formation cycle between 1.2 V and 10 mV x Li / Li+ at a rate of C / 20 (calculated based on theoretical capacitance) was conducted in order to form the solid electrolyte interface (SEI) layer on the silicon electrode, to ensure that the electrode was functional.

[00276] Impedance Spectroscopy Spectra Electrochemical signals (EIS) were subsequently recorded across the frequency range of 500 kHz to 10 MHz, with an amplitude of 5 mV.

[00277] Electrochemical impedance spectroscopy is a useful method for studying physical and electrochemical phenomena at the current collector / electrode / electrolyte interfaces of the electrochemical cell. It is based on studies of the transfer function of electrochemical systems in steady-state and linear regimes. For nonlinear systems to be placed under these conditions, a small amplitude perturbation is applied around the operating point considered quasi-steady (system in equilibrium). In the present work, impedance measurements were performed by applying a sinusoidal perturbation with a potential amplitude of 5 mV near the equilibrium voltage of the system.

[00278] The representation of impedance in the Nyquist plane (not shown) made it possible to emphasize the different phenomena involved in the cells studied.

[00279] In fact, the impedance spectra obtained (not shown) correspond to the different contributions in an electrochemical cell: contact resistances that may result from the assembly of the electrochemical cell and the current collector, resistance to charge transfer, diffusion of Li+ ions in the electrodes, etc. In order to compare the Petition 870240061031, dated 07 / 19 / 2024, page 58 / 117 44 / 44 resulting resistances from the current collector, the difference between two points of different frequencies was measured, corresponding to the width of the semicircle obtained by all the contributions mentioned above, allowing the determination of the resistance “R EIS”, also called impedance.

[00280] The results obtained are presented in the table below. Current collector CCREF1 CCREF2 CC1 CC2 CC3 Impedance (Ωηιπ) 1.90 1.90 1.67 1.74 1.73

[00281] The results above illustrate the fact that the impedance differences for the current collectors can be related to the coverage ratio. In fact, lower impedance was found for the current collectors with a coating that has a coverage ratio of 0.27 (CC1 and CC3) compared to the current collector that has a coverage ratio of 0.21 (CC2).

[00282] These differences may also be related to the height of the elements that form the interface layer, since the height of the DC1 current collector elements is greater than the height of the DC3 current collector elements and therefore generates a larger electrical contact surface with the electrode. In addition, the geometry and extent of each element that forms the interface layer may contribute to variations in the measured impedances. Petition 870240061031, dated 07 / 19 / 2024, p. 59 / 117

Claims

1 / 5 Claims 1. CURRENT COLLECTOR (23) FOR ANODE (16), characterized in that the current collector (23) includes: - a substrate (20) with first face (201); and - at least one interface layer (22) having a first face (221) and a second face (222) in contact with the first face (201) of the substrate (20), the interface layer (22) having a thickness of less than 10 micrometers, and having roughness whose depth is from 0.5 micrometers to 10 micrometers, the roughness being equal to the average value (Rtm) of at least two relief amplitude values ​​(Rt), determined by means of white light interferometry measurement, each relief amplitude value (Rt) corresponding to a distinct zone of the face of the interface layer (22).

2. CURRENT COLLECTOR (23), according to claim 1, characterized in that the interface layer (22) has the second face (222) in contact with the first face (201) of the substrate (20), the second face (222) of the interface layer (22) has an extension (A22) and the first face (201) of the substrate (20) has an extension (A201), wherein the ratio between the extension (A22) of the second face (222) of the interface layer (22) and the extension (A201) of the first face (201) of the substrate (20) is from 0.1 to 1, preferably from 0.3 to 1, more preferably from 0.7 to 1.

3. CURRENT COLLECTOR (23), according to any one of claims 1 to 2, characterized in that the interface layer (22) is formed by coating with a second composition (C2), wherein the second composition (C2) comprises a second binder material (ML2) and a second conductive additive (AC2).

4. CURRENT COLLECTOR (23), according to claim 1, characterized in that the interface layer (22) consists of an assembly (38) which includes a series of elements (40) arranged on the first Petition 870240061031, dated 19 / 07 / 2024, page 60 / 117 2 / 5 face (201) of the substrate (20), wherein each element (40) is separated from another adjacent element (40) by a distance (Dadj) of 200 micrometers to 2500 micrometers and the distance (Dadj) separating two adjacent elements (40) is the shortest distance between a point of a first element (40) and a point of a second element (40) adjacent to the first element (40).

5. CURRENT COLLECTOR (23), according to claim 4, characterized in that the interface layer (22) is formed by coating with a third composition (C3), wherein the third composition (C3) comprises a third conductive additive (AC3) and, optionally, a third binder material (ML3).

6. CURRENT COLLECTOR (23), according to any one of claims 4 to 5, characterized in that each element (40) has a base (401) and the base (401) of each element (40) is a polygon, disk or oval.

7. CURRENT COLLECTOR (23), according to claim 6, characterized in that the base (401) of the elements (40) of the interface layer (22) has a coverage ratio of the first face (201) of the substrate (20) of 0.1 to 0.9, preferably between 0.2 and 0.

5.

8. CURRENT COLLECTOR (23), according to any one of claims 4 to 7, characterized in that each element (40) has a height (H40) less than or equal to 10 micrometers, preferably less than or equal to 6 micrometers, and / or preferably greater than or equal to 10 nanometers, more preferably between 10 nanometers and 3 micrometers.

9. CURRENT COLLECTOR (23), according to any one of claims 1 to 8, characterized in that the interface layer (22) has a coverage ratio of the first face (201) of the substrate (20) strictly less than 1, preferably 0.1 to 0.9 and, more preferably, 0.7 to 0.

9. Petition 870240061031, dated 19 / 07 / 2024, p. 61 / 117 3 / 5 10. CURRENT COLLECTOR (23), according to any one of claims 2 to 3, characterized by further comprising at least a second interface layer (22), wherein the second interface layer (22) consists of an assembly (38) which includes a series of elements (40) arranged on the first face (201) of the substrate (20), each element (40) is separated from another adjacent element (40) by a distance (Dadj) of 200 micrometers to 2,500 micrometers and the distance (Dadj) between two adjacent elements (40) is the shortest distance between a point of a first element (40) and a point of a second element (40) adjacent to the first element (40) and the first interface layer (22) and the second interface layer (22) are superimposed on each other.

11. CURRENT COLLECTOR (23), according to any one of claims 1 to 10, characterized in that the first face (201) of the substrate (20) is preferably soft, wherein the roughness of the substrate surface (20) is less than or equal to 500 nm, preferably less than or equal to 200 nm, preferably less than or equal to 80 nm, preferably less than or equal to 50 nm, more preferably less than or equal to 20 nm.

12. CURRENT COLLECTOR (23), according to any one of claims 1 to 11, characterized in that the interface layer (22) has a thickness (e22) less than 6 micrometers, preferably between 10 nanometers and 3 micrometers.

13. CURRENT COLLECTOR (23), according to any one of claims 1 to 12, characterized in that the roughness of the interface layer (22) has a depth of 0.5 pm to 9 pm, preferably 0.5 pm to 6 pm, more preferably between 1 pm and 6 pm.

14. ANODE (16) FOR ELECTROCHEMICAL CELL (10), characterized in that the anode (16) includes: - a current collector (23) as defined in any of claims 1 to 13; and - an electrode (21) produced according to first composition (C1), wherein the first composition (C1) includes an intercalation material (MI), first binder material (ML1) and first conductive additive (AC1), wherein the intercalation material (MI) comprises silicon, the electrode (21) has a face (212), the first face (201) of the substrate (20) and the face (212) of the electrode (21) are opposite and the interface layer (22) is disposed between the substrate (20) and the electrode (21) and in contact with the first face (201) of the substrate (20) and the face (212) of the electrode (21).

15. ANODE (16), according to claim 14, characterized in that the silicon content of the intercalation material (IM) is greater than or equal to 30% by weight.

16. ANODE (16), according to any one of claims 14 to 15, characterized in that the intercalation material (IM) is silicon.

17. ELECTROCHEMICAL CELL (10), characterized by comprising a collector (23) as defined in any one of claims 1 to 13 or an anode as defined in any one of claims 14 to 16.

18. ENERGY STORAGE DEVICE, characterized by including at least one electrochemical cell as defined in claim 17.

19. METHOD FOR MANUFACTURING A CURRENT COLLECTOR (23) FOR THE ANODE (16), characterized by the method including: - a step of supplying a substrate (20) with a first face (201); and - a step of depositing at least one interface layer (22) by coating on the first face (201) of the substrate (20), wherein the interface layer (22) has a thickness of less than 10 micrometers and the interface layer (22) has a roughness whose depth is from 0.5 micrometers to 10 micrometers.

20. METHOD FOR MANUFACTURING AN ANODE (16) FOR AN ELECTROCHEMICAL CELL (10), characterized by the method comprising: - a step for implementing the steps of the method for manufacturing a current collector (23) for the anode (16) as defined in claim 19; - a step for preparing a first composition (C1) that includes an intercalation material (MI), first binder material (ML1) and first conductive additive (AC1), wherein the intercalation material (MI) comprises silicon; and - a deposition step by coating the first composition (C1) onto the interface layer (22) in order to obtain an electrode (21) with a face (212), wherein the first face (201) of the substrate (20) and the face (212) of the electrode (21) are opposite and the interface layer (22) is in contact with the first face (201) of the substrate (20) and the face (212) of the electrode (21). Petition 870240061031, dated 19 / 07 / 2024, page 64 / 117