RECIPIENTE DE VIDRO REVESTIDO, PROCESSO PARA PREPARAR UM RECIPIENTE DE VIDRO REVESTIDO, E USO DE UMA CAMADA DE PROTEÇÃO À BASE DE DIÓXIDO DE TITÂNIO DOPADO COM ESTANHO
A tin-doped titanium dioxide coating on glass containers addresses the issue of scratching and durability in reusable bottles by enhancing abrasion resistance and maintaining integrity through caustic washing cycles.
Patent Information
- Application Number
- BR112025020557
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2026-11-10
AI Technical Summary
Existing glass containers, particularly reusable bottles, suffer from scratching and surface damage during cleaning and transit due to inadequate coatings, with titanium oxide coatings failing to provide sufficient durability in caustic washing cycles.
A glass container coated with a protective layer based on tin-doped titanium dioxide, applied via chemical vapor deposition at high temperatures, providing enhanced abrasion resistance and durability.
The tin-doped titanium dioxide coating significantly improves the glass container's resistance to scratching and maintains integrity through multiple caustic washing cycles, ensuring longevity and aesthetic appeal.
Abstract
Description
1 / 25 Coated glass container, process for preparing a Coated glass container, and use of a protective layer. Based on tin-doped titanium dioxide
[00001] This invention relates to a coated glass container and a process for preparing a coated glass container.
[00002] In many applications, glass containers must be reusable. Bottles for milk, soda, and beer have been part of closed-loop cycles of use-return-clean-refill-reuse for many years. Bottles must be able to withstand the demands of these cycles while remaining aesthetically acceptable to consumers. In particular, bottles are susceptible to scratches and other surface damage that can occur when bottles move on conveyors and during transit.
[00003] In order to alleviate such scratching, after the container has been annealed, cold-end coatings have been routinely deposited at temperatures of about 21 to 80°C. Examples are stearate, oleic acid, and polyethylene coatings. Such coatings are suitable for single-use bottles, but are prone to being washed away during the cleaning and refilling process for reusable bottles. Therefore, any points of contact become scratched.
[00004] To reduce scratching of reusable bottles, hot-end coatings such as titanium oxide were used. Such coatings are applied at approximately 450 to 600 °C after the bottles are formed, but before a cooling annealing step.
[00005] However, it was discovered that the coatings of Petition 870250086816, dated 09 / 25 / 2025, p. 11 / 46 2 / 25 Titanium oxide still exhibits scratch problems as a result of container cleaning cycles. Therefore, it would be beneficial to provide a coated glass container that alleviates these problems.
[00006] According to a first aspect of the present invention, a coated glass container is provided comprising: a glass container coated with a protective layer based on tin-doped titanium dioxide.
[00007] The inventors surprisingly discovered that the composition of the protective layer provides the coated glass container with enhanced durability in abrasion tests and caustic washing cycles.
[00008] In the context of the present invention, where a layer is said to be based on a particular material or materials, this means that the layer consists predominantly of said material or materials, which typically means that it comprises at least 50% of said material or materials.
[00009] In the following discussion of the invention, unless otherwise indicated, the disclosure of alternative values for the upper or lower limit of the permitted range of a parameter, coupled with an indication that one of said values is more highly preferred than the other, shall be interpreted as an implicit statement that each intermediate value of said parameter, situated between the most preferred and the least preferred of said alternatives, is itself preferred to said least preferred value and also to each value situated between said least preferred value and the Petition 870250086816, dated 09 / 25 / 2025, p. 12 / 46 3 / 25 of the aforementioned intermediate value.
[00010] Throughout this descriptive report, the term comprising or includes means including the specified component(s), but not excluding the presence of other components. The expression consisting essentially of or essentially consists of means including the specified components, but excluding other components, except for materials present as impurities, unavoidable materials present as a result of processes used to provide the components, and components added for a purpose other than achieving the technical effect of the invention. Typically, when referring to compositions, a composition consisting essentially of a set of components will comprise less than 5% by weight, normally less than 3% by weight, more typically less than 1% by weight of unspecified components.
[00011] The expression “consisting of” or “consists of” means including the specified components, but excluding other components.
[00012] Whenever appropriate, depending on the context, the use of the term comprises or comprising may also be considered as including the meaning essentially consists of or consisting essentially of, and may also be considered as including the meaning “consists of” or “consisting of”.
[00013] References in this document, such as in the xay range, should include the interpretation of xaye, therefore, they include the xe y values.
[00014] In the context of the present invention, a transparent material or a transparent container is a material or a Petition 870250086816, dated 09 / 25 / 2025, page 13 / 46 4 / 25 a container that is capable of transmitting visible light in such a way that objects or images situated beyond or behind said material can be seen distinctly through said material or container.
[00015] In the context of the present invention, the thickness of a layer is, for any given location on a layer surface, represented by the distance through the layer, in the direction of the smaller dimension of the layer, from said location on a layer surface to a location on an opposite surface of said layer.
[00016] In the context of the present invention, a “derivative” is a chemical substance that is structurally related to another chemical substance and theoretically derivable from it.
[00017] In the context of the present invention, a container is a device suitable for containing, among other things, liquids, powders and gels.
[00018] When a container is completely filled with, for example, a liquid, only part of its surface is in contact with said liquid. In the context of the present invention, the “inner surface” of the container denotes the part of the container's surface that is in contact with the liquid when the container is completely full. In contrast, the remainder of the container's surface, which is not in contact with the liquid when the container is completely full, is referred to as the “outer surface”.
[00019] Preferably, the glass container is a bottle, jar, tube, can or jug.
[00020] Preferably, the protective layer is located on the outer surface of the container. In some embodiments, the protective layer may cover the entire surface. Petition 870250086816, dated 09 / 25 / 2025, page 14 / 46 5 / 25 outer surface of the container. In alternative embodiments, the protective layer may cover part of the outer surface of the container. Preferably, the protective layer covers at least 70%, more preferably at least 80%, even more preferably at least 90%, most preferably at least 95% of the outer surface of the container.
[00021] The glass container preferably comprises a closed base located at the first end of the glass container. Preferably, the glass container further comprises a body extending from the closed base and being circumferentially closed. Preferably, the glass container further comprises an open mouth (commonly called a finish). Preferably, the open mouth is located at a second end of the glass container. Said second end of the glass container is preferably an opposite end (i.e., further away) from said first end of the glass container. Preferably, the body extends axially from the base.
[00022] Preferably, the glass container further comprises a neck extending from the body and ending in the open mouth. Preferably, the neck extends axially from the body. Preferably, the neck is generally conical in shape.
[00023] Preferably, the protective layer does not cover the open mouth. This arrangement reduces the likelihood of problems arising from filling the glass container with a substance that then comes into contact with the protective layer. Preferably, the protective layer covers the entire outer surface of the container except for a region at least Petition 870250086816, dated 09 / 25 / 2025, p. 15 / 46 6 / 25 minus 0.5 cm from the open mouth, more preferably at least 1 cm from the open mouth, even more preferably at least 1.5 cm from the open mouth, more preferably at least 2 cm from the open mouth, but preferably at most 4 cm from the open mouth, more preferably at most 3.5 cm from the open mouth, even more preferably at most 3 cm from the open mouth.
[00024] Preferably, the protective layer consists essentially of tin-doped titanium dioxide. More preferably, the protective layer consists of tin-doped titanium dioxide.
[00025] Preferably, the protective layer has a bulk tin concentration of 0.01 to 8%, more preferably 0.1 to 6%, even more preferably 0.1 to 5%, most preferably 0.2 to 4.5%. In the context of the present invention, the term bulk means the portion of the protective layer that is at least 2 nm in the direction of the smaller dimension of the protective layer from the surface of the protective layer.
[00026] Preferably, the protective layer has a bulk tin dioxide concentration of less than 1%, more preferably less than 0.5%, even more preferably less than 0.1%, even more preferably less than 0.01%. Most preferably, the majority of the protective layer does not contain tin dioxide. Preferably, the entire protective layer has a tin dioxide concentration of less than 1%, more preferably less than 0.5%, even more preferably less than 0.1%, even more preferably less than 0.01%. Most preferably, the entire protective layer does not contain tin dioxide.
[00027] Preferably, the surface of the protective layer Petition 870250086816, dated 09 / 25 / 2025, page 16 / 46 7 / 25 exhibits a water droplet contact angle of at least 55°, more preferably at least 65°, even more preferably at least 70°, but preferably at most 90°, more preferably at most 80°, even more preferably at most 75°, where the contact angle is measured using a 5 microliter water droplet.
[00028] Preferably, the protective layer is based on tin-doped titanium dioxide, where the tin is in the 4+ oxidation state.
[00029] Preferably, the protective layer has a physical thickness of at least 5 nm, more preferably at least 15 nm, even more preferably at least 20 nm, more preferably at least 25 nm, but preferably at most 200 nm, more preferably at most 150 nm, even more preferably at most 100 nm, most preferably at most 70 nm.
[00030] Preferably, the protective layer is pyrolytic. As used in this document, the term pyrolytic refers to a coating or layer thereof that is chemically bonded to a glass container.
[00031] Preferably, the protective layer consists essentially of tin-doped titanium dioxide and has a bulk tin concentration of 0.1 to 5%, and the surface of the protective layer exhibits a water droplet contact angle of at least 60° but at most 90°, where the contact angle is measured using a 5 microliter water droplet.
[00032] Preferably, the glass container is transparent. The glass container can be transparent or colored. The glass container can be a glass-based container. Petition 870250086816, dated 09 / 25 / 2025, page 17 / 46 8 / 25 metal oxide. The glass container may be a clear or colored glass container. A typical soda-lime-silicate glass composition is (by weight), SiO2 69 - 74%; Al2O3 0.3%; Na2O 10 - 16%; K2O 0 - 5%; MgO 0 - 6%; CaO 5 - 14%; SO3 0 - 2% and Fe2O3 0.005 - 2%. The glass composition may also contain other additives, for example, refining aids, which would normally be present in an amount of up to 2%. Clear float glass is understood to be glass with the composition defined in BS EN 572-1 and BS EN 572-2 (2004). For clear float glass, the Fe2O3 level by weight is typically 0.11%. Float glass with an Fe2O3 content of less than about 0.05% by weight is typically referred to as low-iron float glass. This glass usually has the same basic composition as the other component oxides, that is, low-iron float glass is also a lime and soda silicate glass, as is clear float glass.Typically, colored float glass has at least 0.5% by weight of Fe2O3, for example, 1.0% by weight of Fe2O3. Alternatively, the glass container is a borosilicate-based glass container, an alkali-aluminosilicate-based glass container, or an aluminum oxide-based crystal glass container.
[00033] The protective layer may be in direct contact with the surface of the glass container. Alternatively, said protective layer may be in indirect contact with the surface of the glass container, that is, said protective layer may be deposited over one or more previously deposited layers.
[00034] According to a second aspect of the present invention, a process is provided for the preparation of a Petition 870250086816, dated 09 / 25 / 2025, p. 18 / 46 9 / 25 glass container coated according to the first aspect of the present invention, said process comprising the following steps: a) provide a glass container, b) distribute a titanium-containing precursor and a tin-containing precursor onto or adjacent to a surface of the glass container, and (c) react the aforementioned titanium-containing precursor with the aforementioned tin-containing precursor to deposit a protective layer of tin-doped titanium dioxide on the surface of the glass container.
[00035] Preferably, the protective layer is deposited by chemical vapor deposition (CVD). Alternatively, the coating can be deposited by a physical vapor deposition process, such as sputtering or pulsed laser deposition, or a sol-gel process or other solution-based process.
[00036] When the protective layer is deposited by CVD, preferably the container is at a temperature between 400°C and 700°C, more preferably between 450°C and 650°C, and even more preferably between 500°C and 650°C. This temperature is conveniently provided by the residual heat from the melting of a glass container when the process is incorporated into a continuous process for the manufacture of glass containers. Thus, preferably, the process is incorporated into a continuous process for the manufacture of glass containers and, more preferably, the temperature of the glass container is provided by the residual heat from the melting of the glass container.
[00037] Preferably, the titanium-containing precursor Petition 870250086816, dated 09 / 25 / 2025, page 19 / 46 10 / 25 comprises one or more titanium alkoxides, titanium acetylacetonate, titanium acetate, such as titanium tetraacetate, and a titanium alkyl. Preferably, the titanium-containing precursor comprises a titanium alkoxide. The titanium alkoxide may be selected from one or more titanium tetraisopropoxide (TTIP), titanium ethoxide (TET), n-butoxide, t-butoxide, di(ipropoxide)bis(2,2,6,6-tetramethyl-3,5heptanedionate)titanium(IV), pentamethylcyclopentadienyltitanium trimethoxide, titanium (di-i-propoxide)bis(acetylacetonate), and derivatives. Preferably, the titanium alkoxide is titanium tetraisopropoxide (TTIP). TTIP is beneficial in terms of volatility and stability at relatively high temperatures. It also has the advantages of being readily available and low cost.
[00038] Preferably, the tin-containing precursor comprises one or more of a tin alkoxide, such as tin isopropoxide; tin acetylacetonate; a tin acetate, such as tin diacetate, tin tetraacetate, methyl tin diacetate or dibutyltin diacetate (DBTA); a tin alkyl, such as tetramethyl tin, tetraethyl tin, tetraisobutyl tin and derivatives. The tin alkoxide may be selected from one or more of tin methoxide, tin ethoxide, n-butoxide, t-butoxide, n-propoxide, tin isopropoxide and derivatives. Preferably, the tin alkoxide is tin isopropoxide. Preferably, the tin-containing precursor comprises DBTA.
[00039] Preferably, step b) includes the formation of one or more gases and / or gas mixtures, most preferably by Petition 870250086816, dated 09 / 25 / 2025, p. 20 / 46 11 / 25 Heating of the titanium-containing precursor and the tin-containing precursor. The precursor compounds may, at some point, be a liquid or a solid, but they may be volatile so that they can be vaporized or sublimed for use in a gaseous mixture. Once in a gaseous state, the precursor compounds can be included in a gas stream and used in a CVD process. Preferably, the formation of the gas and / or gaseous mixture comprises heating the titanium-containing precursor, the tin-containing precursor, and / or any other precursor compound using a bubbler system or a thin-film evaporator system. Thin-film evaporator systems are particularly suitable for production-scale processes.
[00040] The gas mixture(s) may further comprise an oxygen-containing precursor that is different from the titanium-containing precursor and the tin-containing precursor. Preferably, the oxygen-containing precursor is selected from one or more oxygen-containing organic compounds or oxygen-containing inorganic compounds. Preferably, the one or more oxygen-containing precursors is one or more oxygen-containing organic compounds.
[00041] The oxygen-containing organic compound may be one or more carbonyl compounds. Preferably, the carbonyl compound is an ester. More preferably, the carbonyl compound is an ester with an alkyl group with a β-hydrogen. Alkyl groups with a β-hydrogen containing two to ten carbon atoms are preferred. Preferably, the ester is selected from one or more of ethyl acetate (EtoAc), ethyl formate, ethyl propionate, isopropyl formate, isopropyl acetate, n-butyl acetate, and t-butyl acetate. More Petition 870250086816, dated 09 / 25 / 2025, page 21 / 46 12 / 25 preferably, one or more oxygen-containing compounds are a mixture of t-butyl acetate and ethyl acetate.
[00042] In another embodiment, the oxygen-containing precursor may be supplied as part of a gaseous composition, such as air. Alternatively, the oxygen is supplied in a substantially purified form. In either of these two embodiments, the oxygen is supplied in the form of molecular oxygen. The inorganic oxygen-containing compound may be selected from one or more of water (H2O), carbon dioxide (CO2), nitric oxide (NO), nitrogen dioxide (NO2), and nitrous oxide (N2O).
[00043] The gas mixture(s) may further comprise one or more carrier or diluent gases, for example, nitrogen, air and / or helium, preferably nitrogen. Thus, the process may also comprise providing a source of one or more carrier or diluent gases from which separate supply lines may extend.
[00044] Preferably, the gas mixture is distributed to a coating apparatus. In certain embodiments, the gas mixture is fed through a coating apparatus and discharged from the coating apparatus using one or more gas distribution beams before the protective layer is deposited. In certain embodiments, the gas mixture is formed before being fed through the coating apparatus. For example, the titanium-containing precursor, the tin-containing precursor, and preferably a carrier or diluent gas, such as nitrogen, may be mixed in a feed line connected to an inlet of the coating apparatus. In other embodiments, the gas mixture may be formed within the coating apparatus. In one embodiment Petition 870250086816, dated 09 / 25 / 2025, p. 22 / 46 Preferred method 13 / 25, the titanium-containing precursor and the tin-containing precursor are kept separate until they are distributed onto or adjacent to a surface of the glass container.
[00045] The process is preferably a dynamic process in which the glass container is moving during steps b) and c). Preferably, the container moves at a predetermined rate of, for example, greater than 3 m / min, more preferably between 3 m / min and 20 m / min.
[00046] Preferably, CVD is performed during a continuous process for the manufacture of glass containers, preferably at a substantially atmospheric pressure (APCVD). Alternatively, CVD can be performed using low-pressure CVD or ultra-high vacuum CVD. CVD can be performed using aerosol-assisted CVD or liquid-direct injection CVD. In addition, CVD can be performed using microwave plasma-assisted CVD, plasma-intensified CVD, remote plasma-intensified CVD, atomic layer CVD, combustion CVD (flame pyrolysis), hot wire CVD, metal-organic CVD, fast thermal CVD, vapor phase epitaxy, or photo-initiated CVD.
[00047] Preferably, the process further comprises: providing a tunnel in a conveyor belt prior to step a) such that the conveyor belt transports the glass container from an upstream end, where the glass container enters the tunnel, to a downstream end, where the glass container exits the tunnel, the tunnel having: an upper section and first and second side walls; Petition 870250086816, dated 09 / 25 / 2025, p. 23 / 46 14 / 25 one or more nozzles, arranged on at least one side wall to distribute jets of gas, which jets traverse a path of the glass container transported through the tunnel; where the titanium-containing precursor and the tin-containing precursor are distributed onto or adjacent to the surface of the glass container in the form of gas jets.
[00048] Preferably, a linear array of nozzles is arranged in at least one side wall of the tunnel. Preferably, at least one exhaust opening is arranged in a side wall, more preferably wherein the exhaust opening is located closer to the downstream end than the nozzles. Preferably, the tunnel further comprises means for applying negative pressure to the exhaust opening, for example, an extractor fan. Preferably, the tunnel further comprises an evaporator, preferably wherein the evaporator comprises a heatable tube. Preferably, a carrier gas stream is directed through the evaporator to one or more of the nozzles. Preferably, the titanium-containing precursor and the tin-containing precursor are introduced into the carrier gas stream in the evaporator.Preferably, a diluent gas is introduced into the carrier gas stream, preferably after passing through the evaporator and before reaching one or more nozzles.
[00049] According to a third aspect of the present invention, the use of a tin-doped titanium dioxide-based protective layer is provided to improve the durability of a glass container.
[00050] Any characteristic defined above in relation to the first and second aspects of the present invention may also Petition 870250086816, dated 09 / 25 / 2025, p. 24 / 46 15 / 25 may be used in relation to any other aspect of the present invention. Any invention described in this document may be combined with any feature of any other invention described in this document mutatis mutandis. It will be understood that optional features applicable to one aspect of the invention may be used in any combination and in any number. Furthermore, they may also be used with any of the other aspects of the invention in any combination and in any number. This includes, but is not limited to, dependent claims of any claim being used as dependent claims for any other claim in the claims of this application.
[00051] The reader's attention is drawn to all works and documents that are filed concurrently with or prior to this descriptive report relating to this application and that are open to public inspection with this descriptive report, and the contents of all such works and documents are incorporated herein by reference.
[00052] All features disclosed in this descriptive report (including any attached claims, abstract and drawings), and / or all steps of any method or process so disclosed, may be combined in any combination, except combinations where at least some of the features and / or steps are mutually exclusive.
[00053] Each feature disclosed in this descriptive report (including any attached claims, summary and drawings) may be replaced by alternative features serving the same, equivalent or similar purpose, unless expressly indicated otherwise. Therefore, unless expressly indicated otherwise, each feature Petition 870250086816, dated 09 / 25 / 2025, p. 25 / 46 16 / 25 disclosed is just one example of a generic series of equivalent or similar characteristics.
[00054] The invention will now be described by means of the following specific embodiments, which are given by way of illustration and not limitation, with reference to the accompanying drawings, in which: Fig. 1 is a schematic diagram of an APCVD system used to prepare samples according to the invention, and Fig. 2 shows images demonstrating the angle of contact with water for samples according to the invention and for comparative samples before and after caustic washing treatments. Examples
[00055] A custom-built APCVD 1 system, as shown in Figure 1, was used to prepare comparative samples (samples B). The two precursors detailed below were contained in separate stainless steel bubblers 2,3 and subsequently heated in order to generate the vapor pressure required to be carried through system 1 and into a mixing chamber 4. The gas flow through system 1 was directed by stainless steel tubes 5 connected to the mixing chamber 4 and through stainless steel valves (6 = two-way valve, 7 = three-way valve) fitted to bubblers 2, 3 and tube segments 5. All components of the CVD 1 system (e.g., tubes 5, mixing chamber 4, bubblers 2, 3) were connected to RS type k thermocouples that measured the temperature of the individual parts of system 1 and were further connected to Eurotherm™ temperature controllers.The vapor generated from the precursors was transported through the system by oxygen-free N2 gas (BOC™ 99.99%) 8 along a range of. Petition 870250086816, dated 09 / 25 / 2025, page 26 / 46 17 / 25 flow rates. Flow meters were installed in each tube 5 to control the flow of carrier gas 8 before it reached system 1. The gases were transported from mixing chamber 4 to a quartz tube reactor 9 via a double baffle distributor. The substrates 10 were contained in reactor 9 and heated in a graphite block (320 mm long) 11 containing three Whatman™ heater cartridges. An exhaust pipe 12 was installed in reactor 9 to transport the byproducts generated during deposition. Other exhaust pipes 13 were indirectly connected to bubblers 2, 3 and mixing chamber 4. To prepare samples according to the invention (samples A), the same method was used, except that the two precursors were transported to two separate mixing chambers before being combined in the reactor.
[00056] Using the APCVD system described above, a range of Sn-doped TiO2 films according to the invention (samples A) and comparative titania:tin oxide films (samples B) were deposited on standard uncoated soda-calsilicate glass (80 x 225 x 3.2 mm3) used to effectively mimic container glass sections. The glass substrates were washed with acetone (99%), isopropanol (99.9%) and distilled water prior to coating in order to avoid environmental or handling contamination and were subsequently dried in an oven. Titanium(IV) isopropoxide (TTIP, 97%, Sigma-AldrichTM) was used as a single-source precursor of titanium and oxygen. Dibutyltin diacetate (DBTDA, 99.5%, Sigma-Aldrich™) was used as the tin source in the deposition alongside TTIP. The choice of precursors was primarily governed by industrial relevance. The non-chlorinated titanium precursors are... Petition 870250086816, dated 09 / 25 / 2025, page 27 / 46 18 / 25 are preferred in the glass bottle industry in order to reduce the effects of Na+ migration from the glass substrate and the chemical washing process that is part of the recycling cycle.
[00057] The bubbler temperature was set to 110°C for the TTIP line to achieve the desired vapor pressure, while the bubbler containing DBTDA was set to 130°C. The mixing chamber temperature was set to 200°C, while the TTIP and DBTDA lines were heated to 180°C. All samples were prepared for a deposition time of 60-180 seconds with a total gas flow of 18.5 L min-1 at a substrate temperature of 550°C. In a typical deposition, all parts of the system were heated to the appropriate temperatures and allowed to stabilize in the presence of a constant flow of carrier gas. The carbon block containing the glass substrate was heated to the target deposition temperature. The precursors, transported by the appropriate N2 flow, were then released from the bubblers with sufficient vapor pressure to reach the mixing chamber and the reactor.The precursor flow was redirected to an escape route after the deposition time had elapsed, which was subsequently closed. The samples were then removed from the reactor after cooling under a flow of N2 carrier gas at ambient temperature and were further handled and stored in air. After coating, the samples were cut into 30 x 30 mm pieces for characterization. The samples used for analysis were selected from similar regions of the reactor, thus ensuring that the gas flow and temperature at the characterization sites were constant throughout the process. Petition 870250086816, dated 09 / 25 / 2025, page 28 / 46 19 / 25 Sample Characterization: Raman Spectroscopy Measurements
[00058] The optical properties of the samples were investigated using a Perkin Elmer Lambda 950 UV / Vis / NIR double-beam, double-chromium spectrophotometer. Transmission spectra were recorded for all samples of interest over a wavelength range of 0-2500 nm. All measurements were performed over a number of 10 scans, with 60 s per scan. X-ray Photoelectron Spectroscopy (XPS) Measurements
[00059] Selected samples of primitive and Sn-doped TiO2 thin films (20 x 20 mm2) were analyzed with a Thermo Scientific K-α spectrometer using monochromatic Al Ka radiation and a dual-beam charge compensation system. Spectra were recorded under a constant pass energy of 50 eV and a spot size of 400 μm. The acquisition time was 25 s over a combination of 100 scans in order to ensure optimal peak definition and reduce background errors. The instrument produces binding energy values with an error of less than ± 0.2 eV. Both surface and depth profiles were obtained for the samples. For the latter, the recording time was 500 s for all samples. All survey spectra were recorded in the 0-1200 eV range.High-definition profiles were obtained for the Ti 2p (449-475 eV), Sn 3d (480-500 eV), O 1s (526-545 eV), and C 1s (280-299 eV) orbitals for surface and depth profile scans. After recording, all spectra were calibrated relative to the C 1s orbital. Petition 870250086816, dated 09 / 25 / 2025, page 29 / 46 20 / 25 using a standard value of 284.8 eV. The peaks were further modeled using XPSCasa software to account for different environments, as well as to calculate the film composition. This was achieved by dividing the areas below the peak by the respective Relative Sensitivity Factor (RSF) value (NIST database), as this refers to the relative concentrations of elements in the material. Water Contact Angle (WCA) Measurements
[00060] The hydrophilicity of the samples was investigated by WCA measurements in various regions of each sample. This was achieved using an FTA (First Ten Angstroms Inc.) 1000 B surface analyzer configuration. The droplet size in all measurements was 5 μL. Images of the water droplet in contact with the sample surface were recorded for all samples, in accumulations of 40 images per sample. Raman Spectroscopy Analysis
[00061] Raman spectra were recorded for four samples according to the invention (samples A) comprising tin-doped titania films with bulk tin concentrations in the range of 0.1-5 to % Sn. All four samples show well-defined vibrational bands at approximately 143 cm-1, 199 cm-1, 398 cm-1, 518 cm-1 and 640 cm-1, which are consistent with the TiO2 space group in the anatase phase and suggest that the deposited films are found primarily in the anatase phase. Other less intense vibrational modes were observable in samples with relatively higher bulk tin concentration (in % Sn > 3) at 250 cm-1, 325 cm-1e and 366 cm-1e are consistent with small traces of the brookite phase, which is in agreement with previous studies of Petition 870250086816, dated 09 / 25 / 2025, pp. 30 / 46 21 / 25 Tin-doped TiO2 films prepared via a sol-gel method. No SnO2 was identified via Raman spectroscopy, suggesting that the incorporation of Sn4+ ions was achieved substitutionally. A shift in the Raman frequency of the anatase main Raman peak at approximately 143 cm-1 and in the full-width half-maximum (FWHM) values appears to confirm this, as a trend was identified as a result of increasing tin mass concentrations, which is consistent with previous work on similar materials and acts as a general trend in the case of doped thin films.
[00062] Raman spectra were also recorded for five comparative samples (samples B) comprising mixed titania:tin oxide films with bulk tin concentrations between 8 and 17% in % Sn. All spectra showed the characteristic anatase peak at a frequency of approximately 143 cm⁻¹, while peaks consistent with the other five fundamental anatase vibrations were significantly less intense. No other titanium dioxide phases were observed, suggesting that no phase transition occurred as the bulk tin concentration increased. The characteristic peaks of the SnO₂ vibrational modes were identified at 636 cm⁻¹. These results suggest that the incorporation of Sn₄⁺ into the films was in the form of SnO₂. The overall weak spectral characteristics further suggest the presence of SnO₂ rather than tin-doped titania, since SnO₂ is known to be a poor Raman scatterer.The lack of a change in the Raman frequency of the main anatase Raman peak with increasing tin mass concentrations further supports the incorporation of Sn4+ into the system. Petition 870250086816, dated 09 / 25 / 2025, page 31 / 46 22 / 25 material in the form of SnO2, forming a composite film of anatase and tin oxide, and not as a dopant. Furthermore, increasing the bulk concentrations of tin did not induce any significant change in the calculated FWHM values. This finding further suggests that the anatase structure in samples B was not disturbed by the presence of tin. In turn, the characteristic anatase Raman features are weak compared to samples A, which is consistent with the presence of a mixed-phase material. X-ray Photoelectron Spectroscopy (XPS) Analysis: Surface scans of tin 3d orbitals Samples A
[00063] The binding energies corresponding to the 3d Sn doublet are shown in Table 1. The error associated with these values is ±0.2 eV. All values within their error ranges are consistent with Sn only in the 4+ oxidation state. Sample Name A1 A2 A3 A4 A5 Sn 3d5 / 2 BE / eV 486.5 486.4 486.7 486.8 486.8 Sn 3d3 / 2 BE / eV 494.9 494.8 495.1 495.2 495.2 Table 1. Binding energies of the 3d Sn orbital doublet of selected samples A with the Sn surface concentration decreasing from left to right across the table.
[00064] A trend of decreasing binding energy with increasing Sn surface concentration for both components of the 3d doublet can be identified in Table 1. This further confirms the environmental change in the film after the Petition 870250086816, dated 09 / 25 / 2025, pp. 32 / 46 23 / 25 incorporation of tin. Samples B
[00065] The binding energies corresponding to the Sn 3d doublet are shown in Table 2. The error associated with these values is ±0.2 eV. All values within their error ranges are consistent with Sn only in the 4+ oxidation state. There is no change in binding energy across the table, showing that there are no changes induced by a range of tin concentrations. This further suggests that tin oxide is the form of tin incorporation in the samples and not a dopant. Sample Name Comparative B1 Comparative B2 Comparative B3 Comparative B4 Comparative B5 Sn 3d5 / 2 BE / eV 486.7 486.8 486.8 486.8 486.9 Sn 3d3 / 2 BE / eV 495.3 495.2 495.2 495.2 495.3 Table 2. Binding energies of the 3d Sn orbital doublet of selected B samples with the Sn surface concentration decreasing from left to right across the table. Concentration Calculations from XPS Profiles
[00066] The relative concentration of Sn to Ti was calculated for surface and bulk XPS profiles for a sample range A. This was achieved by converting the gross area of the peaks of interest to effective areas using the Relative Sensitivity Factor (RSF). The RSF values used for the Ti 2p and Sn 3d orbitals are 7.81 and 25.1, respectively. The relative concentrations of Sn and Ti were obtained and, therefore, different values for x were determined for the proposed ternary oxide formula SnxTi1-xO2. At the surface, x varies from Petition 870250086816, dated 09 / 25 / 2025, pp. 33 / 46 24 / 25 0.35 to 0.50, while in bulk this decreases considerably, becoming as low as 0.03. Abrasion tests and caustic washing cycle
[00067] The film integrity of the samples was tested by simulating the industrial process of washing reusable glass bottles. All samples tested had film thicknesses between 30 and 150 nm. The samples were introduced to a 2% NaOH solution at 80°C for 15-minute cycles. Between any two cycles, the surface of the films was abraded with 150-grit fine sandpaper. Samples A underwent 10 caustic washing cycles without scratch marks and maintained film integrity throughout.
[00068] In contrast, samples B showed scratch marks when worn after 5 cycles, with the effect becoming more pronounced after 7 cycles. The integrity of the films in locations where the material did not show scratches was not visibly affected.
[00069] Thus, samples A comprising tin-doped titania films performed much better in these tests than comparative samples B comprising mixed titania:tin oxide films.
[00070] Water contact angles (WCAs) were measured before and after caustic washing tests. Samples A showed an average contact angle of 70-75°, as measured before caustic treatment, while comparative samples B showed a lower average WCA of approximately 50-55°. This further illustrates that the two sets of films have distinct compositions. WCA measurements were taken after 5 caustic washing cycles for all samples. The films of samples A exhibited minimal or no change in WCA (see Petition 870250086816, dated 09 / 25 / 2025, pages 34 / 46 25 / 25 Figure 2a), where the top line shows an image of a water droplet in the sample before the 5 cycles and the bottom line shows an analogous image after the five cycles). In contrast, samples B showed a decreasing trend in WCA after the caustic treatment (see Figure 2b), where the top and bottom lines again represent the before and after images).
[00071] The invention is not limited to the details of the foregoing embodiments. The invention extends to any novel, or any novel combination of, the features disclosed in this descriptive report (including any appended claims, abstract and drawings), or to any novel, or any novel combination of, the steps of any method or process disclosed herein. Petition 870250086816, dated 09 / 25 / 2025, pp. 35 / 46
Claims
1 / 4 - CLAIMS - 1. COATED GLASS CONTAINER, characterized by the suit comprising: a glass container coated with a protective layer based on tin-doped titanium dioxide.
2. A coated glass container, according to claim 1, characterized in that the protective layer consists essentially of tin-doped titanium dioxide, preferably in which the protective layer consists of tin-doped titanium dioxide.
3. A coated glass container, according to any one of claims 1 and 2, characterized in that the protective layer has a bulk tin concentration of 0.01 to 8%, preferably 0.1 to 6%, more preferably 0.1 to 5%, most preferably 0.2 to 4.5%.
4. A coated glass container, according to any one of claims 1 to 3, characterized in that the protective layer has a bulk tin dioxide concentration of less than 1%, preferably less than 0.5%, more preferably less than 0.1%, and even more preferably less than 0.01%.
5. A coated glass container, according to any one of claims 1 to 4, characterized in that the entire protective layer has a tin dioxide concentration of less than 1%, preferably less than 0.5%, more preferably less than 0.1%, and even more preferably less than 0.01%.
6. Coated glass container, according to any one of claims 1 to 5, characterized by the fact that the entire protective layer does not contain tin dioxide.
7. A coated glass container, according to any one of claims 1 to 6, characterized in that the surface of the protective layer exhibits a water droplet contact angle of at least 55°, preferably at least 65°, more preferably at least 70° but at most 90°, preferably at most 80°, most preferably at most 75°, wherein the contact angle is measured using a 5 microliter water droplet.
8. A coated glass container, according to any one of claims 1 to 7, characterized in that the protective layer has a physical thickness of at least 5 nm, preferably at least 15 nm, more preferably at least 20 nm, more preferably at least 25 nm but at most 200 nm, preferably at most 150 nm, more preferably at most 100 nm, most preferably at most 70 nm.
9. A coated glass container, according to any one of claims 1 to 8, characterized in that the protective layer is pyrolytic.
10. A coated glass container, according to any one of claims 1 to 9, characterized in that the protective layer consists essentially of tin-doped titanium dioxide and has a bulk tin concentration of 0.1 to 5%, and the surface of the protective layer exhibits a water droplet contact angle of at least 60° but at most 90°, where the contact angle is measured using a 5 microliter water droplet.
11. PROCESS FOR PREPARING A COATED GLASS CONTAINER according to one of claims 1 to 10, Petition 870250086816, dated 09 / 25 / 2025, p. 38 / 46 3 / 4 said process characterized in that it comprises the following steps: a) providing a glass container, b) distributing a titanium-containing precursor and a tin-containing precursor onto or adjacent to a surface of the glass container, and c) reacting said titanium-containing precursor and said tin-containing precursor to deposit a tin-doped titanium dioxide-based protective layer onto the surface of the glass container.
12. Process according to claim 11, characterized in that the protective layer is deposited by chemical vapor deposition (CVD) and in that the titanium-containing precursor and the tin-containing precursor are kept separate until they are distributed onto or adjacent to the surface of the glass container.
13. Process according to claim 12, characterized in that the container is at a temperature between 400°C and 700°C, preferably between 450°C and 650°C, more preferably between 500°C and 650°C.
14. Process, according to any one of claims 11 to 13, characterized in that the titanium-containing precursor comprises one or more of a titanium alkoxide, titanium acetylacetonate, titanium acetate, such as titanium tetraacetate, and a titanium alkyl, preferably the titanium-containing precursor comprises a titanium alkoxide, more preferably the titanium alkoxide is titanium tetraisopropoxide (TTIP).
15. Process, according to any of the claims 11 to 14, characterized in that the tin-containing precursor comprises one or more of a tin alkoxide, such as tin isopropoxide; tin acetylacetonate; a tin acetate, such as tin diacetate, tin tetraacetate, methyl tin diacetate or dibutyltin diacetate (DBTA); a tin alkyl, such as tetramethyl tin, tetraethyl tin, tetraisobutyl tin and derivatives, preferably the tin-containing precursor comprises a tin alkoxide, more preferably the tin-containing precursor is DBTA.
16. USE OF A PROTECTIVE LAYER BASED ON TIN-DOPED TITANIUM DIOXIDE, characterized by the fact that it improves the durability of a glass container. Petition 870250086816, dated 09 / 25 / 2025, pp. 40 / 46