COMPOSIÇÃO ADITIVA PARA AUMENTO DE RESISTÊNCIA DE COMPOSIÇÕES CIMENTÍCIAS
The additive composition of EDIPA, a hardening retarder, and accelerator enhances both early and late compressive strength of cement, addressing the limitations of existing additives by improving strength and reducing clinker content while maintaining setting time.
Patent Information
- Application Number
- BR112025024281
- Authority / Receiving Office
- BR · BR
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-05-08
- Filing Date
- 2024-05-09
- Publication Date
- 2026-11-10
Abstract
Description
1 / 39 Additive composition for increasing the strength of cementitious compositions. BACKGROUND OF THE INVENTION
[001] The present invention relates to additive compositions for enhancing the strength of cementitious compositions. In particular, the present invention relates to the use of the disclosed additive compositions in cement compositions such that the early and late age compressive strength of the cement when cured is improved compared to a cement composition without the disclosed additive compositions.
[002] The term cement is used to designate many different types of materials useful as binders or adhesives. Hydraulic cements are powdered materials that, when mixed with water, form a paste that hardens slowly. If further mixed with sand, it forms a mortar, and if mixed with sand and coarse aggregate, such as rock, it forms concrete, which are rock-hard products. These products are commonly referred to as hydraulic cement mixtures. Portland cement is distinguished from other cements by the different components of which it is composed and by the requirement that it meet specific standard specifications established in each country.For example, in the United States, the American Society for Testing and Materials (ASTM), the American Association of State Highway and Transportation Officials, as well as other government agencies, have established certain basic standards for cement that are based on the main chemical composition requirements of the clinker and the main physical property requirements of the final hardened mortar or concrete. For the purposes of this disclosure, the term Portland cement is intended to include all cementitious compositions that meet the requirements of ASTM (as designated by ASTM Specification C150) or the established standards of other countries. Portland cement clinker is prepared by sintering a mixture of components, including carbonate. Petition 870250101994, dated 07 / 11 / 2025, page 12 / 76 2 / 39 calcium (as limestone), aluminum silicate (as clay or shale), silicon dioxide (as sand), and various iron oxides. During the sintering process, chemical reactions occur that form hardened nodules, commonly called clinkers. Portland cement clinker is formed by the high-temperature reaction of raw materials containing calcium, silicon, aluminum, and iron, resulting mainly in tricalcium silicate, dicalcium silicate, tricalcium aluminate, and a solid solution phase of ferrite that approximates tetracalcium aluminoferrite.
[003] After the clinker has cooled, it is ground into a fine powder along with a small amount of gypsum (calcium sulfate) in a finishing mill to provide a fine, homogeneous powder product known as Portland cement. Grinding the clinker and other cement components into a fine powder is the final step in the cement production process. There are two broad purposes for using a cement additive during grinding. One is to improve the grinding process to make it more efficient. Such improvements can be quantified as, for example, reduced grinding time, reduced grinding energy, and increased production rate. The second broad objective is to improve or alter the performance of the cement when it is used to make concrete.In this case, the chemicals remain on the surface of the ground cement particles until the cement is mixed with water, at which point they modify the cement hydration process, often by first redissolving in the mixing water. While many performance changes can be achieved with cement admixtures, a particularly common and desirable attribute is an increase in compressive strength at various (or all) ages. In general, cement admixtures that improve concrete performance also improve grinding efficiency. They therefore represent a class of higher-performance (and more expensive) cement admixtures (known as quality improvers) compared to admixtures that only affect the grinding process. Petition 870250101994, dated 07 / 11 / 2025, page 13 / 76 3 / 39
[004] Due to the hardness of clinkers, a large amount of energy is required to properly grind them into a suitable powder form. Energy requirements for finishing grinding can vary from about 33 to 77 kW h / ton, depending on the nature of the clinker. Several materials, such as glycols, alkanolamines, amine acetates, aromatic acetates, etc., have been shown to reduce the amount of energy required and thus improve the grinding efficiency of hard clinkers. These materials, commonly known as grinding aids or grinding additives, are processing additives that are introduced into the mill in small dosages and ground with the clinker to obtain a uniform powder mixture. In addition to reducing grinding energy, the commonly used processing additives listed above are often used to improve the powder's ability to flow easily and reduce its tendency to form lumps during storage.
[005] Some cement additive compositions can be used to improve or alter the performance of cement when it is used to make concrete. Similarly, chemicals to increase strength can also be added when the concrete is being mixed. Typically, the chemicals will be added to the mixing water when the concrete ingredients are being combined.
[006] Due to the very high temperature processing required to form suitable Portland cement clinker, clinker becomes a relatively expensive and carbon-intensive feedstock. For certain applications, it is possible to substitute less expensive fillers, such as limestone or clinker substitutes, like granulated blast furnace slag, natural or artificial pozzolan, calcined clay, pulverized fuel ash and the like, for a portion of the clinker. As used herein, the term filler refers to an inert material that does not possess subsequent age-strengthening attributes; the term clinker substitute Petition 870250101994, dated 07 / 11 / 2025, p. 14 / 76 4 / 39 refers to a material that can contribute to increased long-term compressive strength beyond 28 days. The addition of these fillers or clinker substitutes to form blended cements is limited in practice by the fact that such addition generally results in a decrease in the physical strength properties of the resulting cement. For example, when a filler, such as limestone, is mixed in quantities greater than 5%, the resulting cement exhibits a marked reduction in strength, particularly in relation to the strength achieved after 28 days of wet curing (28-day strength). As used herein, the term blended cements or cementitious compositions refers to hydraulic cement compositions containing between 2 and 90%, more conventionally between 5 and 60%, fillers or clinker substitute materials.
[007] Reducing the amount of clinker in concrete (known as the clinker factor) is currently the most effective way to reduce the CO2 footprint of concrete. This is because most of the CO2 associated with the use of concrete is emitted during the manufacture of clinker in high-temperature kilns. Recently, there has been an increase in demand for cement additives that increase strength, driven by regulations aimed at limiting CO2 emissions.
[008] Several other additives can be added to cement to alter the physical properties of the final cement. For example, alkanolamines such as monoethanolamine, diethanolamine, triethanolamine, and the like are known to shorten the hardening time (hardening accelerators) as well as increase the one-day compressive strength (initial strength) of cements. These additives, however, have little beneficial effect on the 28-day hardening strength of the finished cement and, in some cases, may actually decrease it. This behavior is described by V. Dodson, in Concrete Admixtures, Van Reinhold, New York, 1990, who states that calcium chloride, the hardening time accelerator of Petition 870250101994, dated 07 / 11 / 2025, page 15 / 76 5 / 39 hardening, a well-known and early-age strength enhancer, reduces compressive strength at later ages.
[009] U.S. Patents 4,990,190, 5,017,234, 5,084,103, 6,048,393, and 6,290,772, disclosures of which are incorporated herein by reference, describe the discovery that certain superior trihydroxyalkylamines, such as triisopropanolamine (hereinafter referred to as tipa) and N,N-bis(2-hydroxyethyl)-2-hydroxypropylamine (hereinafter referred to as DEIPA), will improve the late strength (strength after 7 and 28 days of wet cement mix preparation) of Portland cement, especially Portland cements containing at least 4 percent C4AF. The superior strength-enhancing trihydroxyalkylamine additives described in these patents are said to be particularly useful in blended cements. For example, tipa has been found to improve the late strength properties of cement compositions more than the early strength. Even more surprising is the observation that it tends to increase the amount of air trapped in the cement.In order to improve the initial strength, hardening, and air entrainment properties of the hardened cement composition containing tipa, the state of the art has taught the incorporation of known early strength enhancers and hardening accelerators, such as TEA or alkali metal salts, and a known air entrainment agent (ADA), such as those illustrated in US patent 5,156,679.
[010] Such strength-enhancing compositions, however, should not significantly shorten or lengthen the hardening time of the concrete. Consequently, there remains a need for additive compositions that improve strength properties in both early and late stages to a greater degree than is currently possible, in order to reduce the clinker content of the concrete as much as possible without significantly affecting the setting time. Petition 870250101994, dated 07 / 11 / 2025, page 16 / 76 6 / 39 hardening of the concrete to which the strength-enhancing compound was added. BRIEF SUMMARY OF THE INVENTION
[011] In one aspect, a composition for use as an additive to increase the strength of a cementitious composition is disclosed in this document, the composition comprising: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10.
[012] In another aspect, a method for enhancing the strength of a cement composition is disclosed in this document, the method comprising the steps of: (i) grinding a solid comprising Portland cement clinker in the presence of an additive, thereby preparing the cement composition, or (ii) making concrete from a mixture of a solid comprising Portland cement clinker, sand, coarse aggregate, water and an additive, wherein the additive comprises: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, Petition 870250101994, dated 07 / 11 / 2025, p. 17 / 76 7 / 39 corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10, and wherein the cement composition, when cured, has a compressive strength at 2 days and at 28 days that is at least 10% greater than a cement composition without the additive.
[013] In yet another aspect, a strength-enhanced hydraulic cement powder composition comprising Portland cement clinker and an additive is disclosed in this document, wherein the additive comprises: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10.
[014] In yet another aspect, a hydraulic composition of Portland cement comprising: 20 to 64 percent by mass of clinker is disclosed in this document; 5 to 60 percent by mass of calcined clay; 0 to 35 percent by mass of limestone; 0 to 10 percent by mass of calcium sulfate; an additive comprising: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of Petition 870250101994, dated 07 / 11 / 2025, p. 18 / 76 8 / 39 triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10.
[015] In yet another aspect, a cementitious composition comprising: cement; and a means for increasing the strength of the cement composition by hardening the cement composition in an aqueous environment without substantially increasing the hardening time of the cement composition is disclosed in this document.
[016] The embodiments and features of the present invention can be used individually or in combination with each other. BRIEF DESCRIPTION OF THE DRAWINGS
[017] The precedent will be evident from the following more particular description of exemplary embodiments of the invention, as illustrated in the accompanying drawings.
[018] Figure 1A is a graph showing the day 1 mortar strength results of US commercial cements as received without added limestone with and without EXP-1 and EXP-2 additives normalized to the strength of the blank without additive;
[019] Figure 1B is a graph showing the day 2 mortar strength results of US commercial cements as received without added limestone with and without EXP-1 and EXP-2 additives normalized to the strength of the blank without additive; Petition 870250101994, dated 07 / 11 / 2025, page 19 / 76 9 / 39
[020] Figure 1C is a graph showing the 28-day mortar strength results of US commercial cements as received without added limestone with and without additives EXP-1 and EXP-2 normalized to the strength of the blank without additive;
[021] Figure 1D is a graph showing the changes in setting time of various commercial North American cements without added limestone with additives EXP-1 and EXP-2 compared to blank cement without additive;
[022] Figure 1E is a graph showing the day 1 mortar strength results of US commercial cements as received with added limestone at 22% by weight with and without EXP-1 and EXP-2 additives normalized to the strength of the blank without additive;
[023] Figure 1F is a graph showing the day 2 mortar strength results of US commercial cements as received with added limestone at 22% by weight with and without EXP-1 and EXP-2 additives normalized to the strength of the blank without additive;
[024] Figure 1G is a graph showing the 28-day mortar strength results of US commercial cements as received with added limestone at 22% by weight with and without EXP-1 and EXP-2 additives normalized to the strength of the blank without additive;
[025] Figure 1H is a graph showing the changes in setting time of various North American commercial cements with added limestone at 22% with additives EXP-1 and EXP-2 compared to blank cement without additive;
[026] Figure 2 is an isothermal calorimetry graph illustrating the estimated initial hardening time of the S7 cement composition as received and with an additive; Petition 870250101994, dated 07 / 11 / 2025, page 20 / 76 10 / 39
[027] Figure 3A is a pie chart showing the day 1 strength of cement S2 resulting from variations in the ratios of the components of an additive as disclosed herein, wherein the size of the circle is proportional to the change in the raw material;
[028] Figure 3B is a pie chart showing the day 2 strength of cement S2 resulting from variations in the ratios of the components of an additive as disclosed herein, wherein the size of the circle is proportional to the change in the raw material;
[029] Figure 3C is a pie chart showing the 28-day strength of S2 cement resulting from variations in the ratios of the additive components, as disclosed in this document, where the size of the circle is proportional to the change in the raw material;
[030] Figure 3D is a circle graph showing the changes in the setting time of cement S2 resulting from variations in the component ratios of an additive as disclosed herein, wherein the size of the circle is proportional to the change in the raw material;
[031] Figure 4A is a graph of the isothermal calorimetry results for cement S1 prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2;
[032] Figure 4B is a graph of the isothermal calorimetry results for S2 cement prepared for strength testing and comparison of the effects of EXP-1 and EXP-2 additives;
[033] Figure 4C is a graph of the isothermal calorimetry results for the S3 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2; Petition 870250101994, dated 07 / 11 / 2025, page 21 / 76 11 / 39
[034] Figure 4D is a graph of the isothermal calorimetry results for the S4 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2;
[035] Figure 4E is a graph of the isothermal calorimetry results for S5 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2;
[036] Figure 4F is a graph of the isothermal calorimetry results for S6 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2;
[037] Figure 4G is a graph of the isothermal calorimetry results for the S7 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2; and
[038] Figure 4H is a graph of the isothermal calorimetry results for the S8 cement prepared for strength testing and comparison of the effects of additives EXP-1 and EXP-2. DETAILED DESCRIPTION OF THE INVENTION
[039] As used in this document, the terms a, an, the, and similar terms refer to both the singular and the plural, unless the context clearly indicates otherwise. A bottle, for example, refers to a single bottle or more than one bottle.
[040] Also as used herein, the description of one or more steps of the method does not preclude the presence of additional steps of the method before or after the combined recited steps. Additional steps may also be intervening steps to those described. Furthermore, it is understood that the letters of the steps or ingredients of the process are a convenient means of identifying discrete activities or ingredients and the recited letters may be arranged in any sequence. Petition 870250101994, dated 07 / 11 / 2025, p. 22 / 76 12 / 39
[041] When a range of numbers is presented in the application, it is understood that the range includes all whole numbers and fractions thereof between the stated range limits. A range of numbers expressly includes numbers less than the stated endpoints and those between the stated range. A range of 1-3, for example, includes the whole numbers one, two, and three, as well as any fractions that lie between those whole numbers.
[042] Conventional cement chemist notation uses the following abbreviations: CaO = C SiO2 = S A12O3 = A Fe2O3 = F Under this notation, the following abbreviations are used: tricalcium silicate = C3S dicalcium silicate = C2S tricalcium aluminate = C3A tetracalcium aluminoferrite = C4AF
[043] As used herein, “alkyl” means a saturated, linear or branched aliphatic monovalent hydrocarbon radical optionally substituted having the specified number of carbon atoms. Thus, (C1-C4) alkyl means a radical having 1-4 carbon atoms in a linear or branched arrangement. (C1-C4) alkyl includes methyl, ethyl, propyl, isopropyl, n-butyl and tert-butyl.
[044] As used herein, alkanolamine means an alkyl, typically a C1-C6 alkyl, functionalized with at least one amino group and at least one hydroxyl group. A tertiary alkanolamine includes an amino group in which all three hydrogens are replaced by a substituent, typically an optionally substituted C1-C6 alkyl, and at least one hydroxyl group for each alkyl group. Petition 870250101994, dated 07 / 11 / 2025, p. 23 / 76 13 / 39
[045] As used herein, sucrose refers to a combination of the disaccharide glucose and the monosaccharide fructose with the formula C12H22O11.
[046] As used herein, corn syrup refers to syrup made from corn starch, consisting of dextrose, maltose and dextrins.
[047] As used herein, molasses refers to thick, dark brown syrup obtained from raw sugar during the refining process.
[048] As used herein, a chloride salt refers to an alkali metal (Group I of the periodic table, for example, sodium or potassium) or an alkaline earth metal (Group II of the periodic table, for example, calcium) salt of hydrochloric acid.
[049] As used herein, thiocyanate salts refers to an alkali metal (Group I of the periodic table, for example, sodium or potassium) or an alkaline earth metal (Group II of the periodic table, for example, calcium) salt of thiocyanic acid.
[050] The content of all components in the compositions described below is indicated in relation to the dry weight of the composition.
[051] The terms cementitious composition or cementitious powder are used in this document to designate a binder or adhesive that includes a material that will solidify upon the addition of water (hydraulic cementitious material) and an optional additive. When mixed with water and sand, hydraulic cementitious materials form a mortar. When mixed with sand, coarse aggregate (stones or gravel) and water, cementitious materials form concrete. The terms cementitious material, cementitious powder and cement may be used interchangeably.
[052] Cement compositions can be mixtures composed of a cementitious material, for example, Portland cement, alone or in combination with other finely ground components, such as fly ash, silica fume, blast furnace slag, limestone, natural pozzolans or artificial pozzolans.
[053] As used herein, the term clinker refers to a material made by heating limestone (calcium carbonate) with other materials (such as clay) to Petition 870250101994, dated 07 / 11 / 2025, p. 24 / 76 14 / 39 approximately 1450 °C in a furnace, to form calcium silicates and other cementitious compounds.
[054] As used in this document, the term Portland cement includes all cement compositions that meet the requirements of ASTM (as designated by ASTM Specification C150) or the established standards of other countries. Portland cement is prepared by sintering a mixture of components, including calcium carbonate (such as limestone), aluminum silicate (such as clay or shale), silicon dioxide (such as sand), and various iron oxides. During the sintering process, chemical reactions occur that form hardened nodules, commonly called clinkers. Portland cement clinker is formed by the reaction of calcium oxide with acidic components, resulting primarily in tricalcium silicate, dicalcium silicate, tricalcium aluminate, and a solid solution phase of ferrite that approximates tetracalcium aluminoferrite.The additive compositions disclosed in this document are not limited to use in Portland cement and may be used with any cement composition, including blended cements.
[055] As used herein, the term fine aggregate refers to particulate material used in construction that is less than 4.75 mm in size. The term coarse aggregate refers to particulate material used in construction that is larger than about 2 / 16 inch.
[056] The expressions % by weight, % by weight, mass percentage, and weight percentage of a compound are synonymous and refer to the dry weight (mass) percentage of that compound. Unless otherwise specified, the weight (mass) percentage of a compound present in a composition is calculated as the weight of that compound divided by the total mass of the composition comprising the compound multiplied by 100%. The weight (mass) percentage of a compound may also refer to the % by weight of a compound. Petition 870250101994, dated 07 / 11 / 2025, page 25 / 76 15 / 39 added to a composition and is calculated as the weight of that compound divided by the total mass of the composition without the compound multiplied by 100%. The composition percentages indicated here refer to the total active quantities of the alkanolamine, retarder and accelerator chemicals, not including water, glycol or other inactive components.
[057] The additive compositions disclosed herein provide improved strength to a cementitious composition when hydrated and hardened. The additive composition can also be used as a grinding aid, for example, in the grinding process of cement clinker and therefore can be added to a cement composition immediately before or during a grinding process or the additive can be added to a cement composition before hydration.
[058] The additive composition for increasing the strength of a cementitious composition comprises an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10.
[059] In some embodiments, the additive composition further comprises at least one of an antifoaming agent, a biocide, and a dye. Antifoaming agents are typically used to reduce the air content in a cementitious composition. Examples of antifoaming agents that can be used in the present invention include, Petition 870250101994, dated 07 / 11 / 2025, page 26 / 76 16 / 39 but are not limited to octyl alcohol, water-insoluble esters of carbonic and boric acid, acetylenic diols, ethylene oxide-propylene oxide block or random copolymers and silicones. Triisobutyl phosphate (TiBP) is a preferred antifoaming agent.
[060] In some embodiments, the additive is a liquid. The additive compositions disclosed in this document may be supplied in a pure concentrated form or diluted in aqueous or organic solvents and may also be used in combination with other chemical mixtures.
[061] The alkanolamine component of the additive composition disclosed herein comprises ethanoldiisopropanolamine (EDIPA) as an essential element and may be present in 100% of the alkanolamine component. In embodiments, however, EDIPA is optionally blended with other alkanolamines such as triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA), and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED). The alkanolamine component of the additive composition functions as a strength-enhancing agent.
[062] In embodiments, the alkanolamine component of the additive composition is a mixture of EDIPA and TIPA. In other embodiments, the alkanolamine component of the additive composition is a mixture of EDIPA and DEIPA. In embodiments where the alkanolamine comprises a mixture of EDIPA and at least one other alkanolamine, preferably the EDIPA is at least 10%, more preferably at least 20%, and most preferably at least 30% by weight of the total amount of the alkanolamine mixture. Thus, the EDIPA may be present in the additive composition from 10% to 100%, from 10% to 50%, from 10% to 30%, from 10% to 25%, or from 10% to 20% by weight of the total amount of the alkanolamine mixture. Petition 870250101994, dated 07 / 11 / 2025, p. 27 / 76 17 / 39
[063] Preferably, the alkanolamine is present in the additive composition from 9 to 79 percent by mass, more preferably from 23.0 to 62.0 percent by mass, and most preferably from 35.5 to 48.5 percent by mass of the additive composition.
[064] The hardening retarder component of the additive composition disclosed in this document is preferably at least one selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses. Preferably, the hardening retarder is present in the additive composition from 2.0 to 46.0 percent by mass, more preferably from 4 to 19.5 percent by mass, and most preferably from 7.0 to 13.0 percent by mass of the additive composition.
[065] Adjust the function of the retarders to prolong the setting time of the cement to allow time for the cement to be pumped into place. In some embodiments, the hardening retarder component of the additive composition is sodium gluconate and is present in 50% to 100% of the hardening retarder component of the additive composition.
[066] The hardening accelerator component of the admixture composition disclosed in this document functions to reduce the hardening times of concrete. The hardening accelerator component of the admixture composition disclosed in this document is preferably at least one selected from the group consisting of a thiocyanate salt (e.g., sodium, potassium, calcium) or a chloride salt (e.g., sodium, potassium, calcium). Preferably, the hardening accelerator is present in the admixture composition from 16 to 77 percent by mass, more preferably from 31.5 to 66.0 percent by mass, and most preferably from 42.5 to 54.6 percent by mass of the admixture composition.
[067] In some embodiments, the hardening accelerator component of the additive composition is sodium thiocyanate and is present in 50% to 100% of the hardening accelerator component of the additive composition. Petition 870250101994, dated 07 / 11 / 2025, page 28 / 76 18 / 39
[068] The additive compositions disclosed in this document (and therefore the resulting cement compositions) may also comprise additional ingredients that may be included for a desired purpose, including, for example, decorative or aesthetic purposes, or to alter the performance and / or one or more characteristics of the cement. For example, the aqueous compositions disclosed herein optionally comprise from about 0.1 to about 25% by weight, preferably from about 1 to 15%, more preferably from about 1 to about 10%, even more preferably from about 2 to about 8% by weight and, most preferably, from about 3 to 5% by weight of at least one polyacrylic acid (“PAA”), which includes the acid, partial or complete neutralization of the acids to form polyacrylic acid salts, such as, for example, alkali metal salts and / or ammonium salts.The term polyacrylic acid, as used in the present invention, means acrylic acid homopolymers and acrylic acid copolymers with ethylenically copolymerizable monomers, such as, for example, ethylene propylene, butadiene, styrene, methacrylic acid and the like. The copolymerizable monomers are normally present in up to 30 mole percent, preferably up to 20 mole percent. Preferred agents are acrylic acid homopolymers and acrylic acid homopolymers that are partially to totally neutralized with an alkali metal base, such as the sodium salt of polyacrylic acid.
[069] The optional polyacrylic acid component of the additive composition disclosed herein preferably has a weight-average molecular weight of at least about 1,500 to 500,000 g / mol, determined by gel permeation chromatography (GPC). In some embodiments, the weight-average molecular weight of the polyacrylic acid polymer is in the range of 100,000 to 500,000 g / mol. In other embodiments, the molecular weight of the polyacrylic acid polymer is in the range of 40,000 to 100,000 g / mol. In still other embodiments, the molecular weight of the polyacrylic acid polymer is in the range of 1,500 to 75,000 g / mol. In still other embodiments, the weight-average molecular weight Petition 870250101994, dated 07 / 11 / 2025, page 29 / 76 The molecular weight of the 19 / 39 polyacrylic acid polymer is in the range of 1500 to 50000 g / mol, and preferably 1500 to 25000 g / mol. Lower molecular weights (e.g., 1500 to 50000 g / mol) are preferable due to cost and control of the liquid additive viscosity. When used, polyacrylic acid functions to modify the flow properties of the resulting ground cement.
[070] The additive composition disclosed in this document provides enhanced strength to a cement composition when hydrated, both at an early age (e.g., 1 day or 2 days) and at a later age (e.g., 28 days) without significantly altering the hardening time of the concrete. The inventors surprisingly discovered that the increased strength at early and late ages is not the result of the alkanolamines alone, but rather the result of the presence of all three components (alkanolamine, retarder, and accelerator) present in the composition. In particular, without intending to be limited by any particular theory, it is believed that the presence of both the accelerator and retarder components increases strength without causing undesirable changes in hardening times.In preferred embodiments, the alkanolamine and hardening accelerator are present in the additive composition at a mass ratio of 0.2 to 4.0, and the hardening accelerator and retarder are present at a mass ratio of 1 to 10. In more preferred embodiments, the alkanolamine and hardening accelerator are present in the additive at a mass ratio of 0.4 to 1.8, and the hardening accelerator and retarder are present at a mass ratio of 3 to 8. In even more preferred embodiments, the alkanolamine and hardening accelerator are present in the additive at a mass ratio of 0.7 to 1.1, and the hardening accelerator and retarder are present at a mass ratio of 4 to 6.5. Petition 870250101994, dated 07 / 11 / 2025, p. 30 / 76 20 / 39
[071] In another aspect, the present disclosure is directed to a method for increasing the strength of a cement composition, the method comprising the steps of (i) grinding a solid comprising cement clinker in the presence of an additive, thereby preparing the cement composition, or (ii) making concrete from a mixture of a solid comprising Portland cement clinker, sand, coarse aggregate, water and an additive, wherein the additive comprises: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses;and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10, and wherein the cement composition, when cured, has a compressive strength at 2 days and at 28 days that is at least 10% greater than a cement composition without the additive. Preferably, the cement composition, when cured, has a compressive strength at 2 days and at 28 days that is at least 10% to 50% greater than a cement composition without the additive.
[072] Clinker production involves the release of CO2 from the calcination of limestone. It is estimated that for every ton of clinker produced, up to one ton of CO2 is released into the atmosphere. The use of fillers, as substitutes for limestone or clinker, such as granulated blast furnace slag, natural or artificial pozzolans, pulverized fuel ash and the like, for a portion of the clinker allows a reduction in the levels of CO2 emitted per ton of Petition 870250101994, dated 07 / 11 / 2025, p. 31 / 76 21 / 39 finished cement. As used herein, the term filler refers to an inert material that does not possess subsequent age-strengthening attributes; the term clinker substitute refers to a material that can contribute to increased long-term compressive strength beyond 28 days. The addition of these fillers or clinker substitutes to form blended cements is limited in practice by the fact that such addition generally results in a decrease in the physical strength properties of the resulting cement. For example, when a filler, such as limestone, is mixed in amounts greater than 5%, the resulting cement exhibits a marked reduction in strength, particularly with respect to the strength achieved after 28 days of wet curing (28-day strength).As used herein, the term blended cements refers to hydraulic cement compositions containing between 2 and 90%, more conventionally between 5 and 70%, fillers or clinker substitute materials. The additive composition disclosed in this document increases the early and later stage strength of a ground cement powder composition comprising the additive.
[073] In some embodiments, the additive disclosed in this document is used to manufacture a Type 1L cement, as defined by ASTM C595 (“Standard Specification for Blended Hydraulic Cements”).
[074] In embodiments, the method disclosed in this document further includes the step of adding to the cement clinker at least one supplementary cementitious material selected from the group consisting of fly ash, granulated blast furnace slag, limestone, calcined clay and a pozzolan (including natural pozzolans and artificial pozzolans). In some embodiments, at least one selected from the group consisting of limestone, fly ash, slag and calcined clay is added to the clinker.
[075] In embodiments, the clinker solid to be ground with the additive disclosed in this document further comprises at least 5% added limestone by mass. Petition 870250101994, dated 07 / 11 / 2025, p. 32 / 76 22 / 39 In other embodiments, the clinker solid to be ground with the additive disclosed in this document further comprises at least 10% added limestone by mass. In still other embodiments, the clinker solid to be ground with the additive disclosed in this document further comprises at least 20% added limestone by mass and, more preferably, at least 22% added limestone by mass. In still other embodiments, the clinker solid to be ground with the additive disclosed in this document further comprises from 22% to 75% or more added limestone by mass and, more preferably, from 22% to 55% added limestone by mass. Limestone may also be added to the clinker powder once the clinker has been ground so that the finished cement product can reflect the aforementioned concentrations of added limestone.
[076] In some embodiments, the clinker solid to be milled with the additive disclosed in this document further comprises at least 4% by mass of tricalcium aluminate (C3A). In other embodiments, the clinker solid to be milled with the additive disclosed in this document further comprises from about 4% to about 20% by mass of tricalcium aluminate (C3A).
[077] The method includes the grinding step with the additive composition disclosed herein. The composition as disclosed herein may be added to the clinker composition immediately before or during the grinding step. In one embodiment, for example, the additive composition is aqueous and may be sprayed onto the clinker composition before, during, or after grinding. In another embodiment, the additive may be sprayed onto limestone or SCM material (e.g., blast furnace slag, fly ash, natural pozzolan, and calcined clay) that will be used to make cement or concrete, before, during, or after grinding.
[078] In one embodiment, the additive as disclosed herein is added to the clinker in an amount of 0.01% to 0.5% based on the dry weight of the hydraulic cementitious powder. In another embodiment, the additive is present in an amount of at least Petition 870250101994, dated 07 / 11 / 2025, p. 33 / 76 23 / 39 0.04% based on the dry weight of the hydraulic cementitious powder. In yet another embodiment, the additive is present in an amount of at least 0.1% based on the dry weight of the hydraulic cementitious powder. In yet another embodiment, the additive is present in an amount of approximately 0.1% to approximately 1.0% based on the dry weight of the hydraulic cementitious powder.
[079] In some embodiments, the additive composition comprises EDIPA. In other embodiments, the additive composition comprises a mixture of EDIPA and TIPA.
[080] A particular advantage of the additive disclosed in this document is that it can be interleaved or mixed with the cement. As used in this document, the terms interleaving and mixing refer to the particular stage of cement processing in which the additives described in this document are added. They can be added to the clinker during the finishing grinding stage and thus buried to help reduce energy requirements and provide a uniform free-flowing cement powder with a reduced tendency to form lumps during storage. It is also possible to add the additives in question as a mixture to the cement powder before, in conjunction with, or after the addition of water to cause hydraulic hardening of the cement.
[081] In terms of modalities, the method disclosed in this document also includes the step of hydrating the cement composition by adding water.
[082] The method for enhancing the strength of a cement composition disclosed in this document increases the strength of the cement composition preferably without increasing the cement setting time by more than 35 minutes (0.58 h), more preferably without increasing the cement setting time by more than 30 minutes (0.50 h), even more preferably without increasing the cement setting time by more than 25 minutes (0.42 h), and Petition 870250101994, dated 07 / 11 / 2025, p. 34 / 76 24 / 39 more preferably without increasing the cement setting time by more than 20 minutes (0.33 h), compared to the same cement composition without the additive.
[083] As used herein, the term setting time refers to the period of time between the initial mixing of mortar or concrete and the times when the mortar or concrete loses its ability to flow easily (initial setting) and then begins to gain strength (final setting). Initial setting time is a critical parameter for the industrial use of concrete because the concrete must remain fluid and flowable while it is transported to a construction site, placed in forms, and finished. If the setting time is too short, these steps cannot be completed and the concrete may need to be discarded. Conversely, if the final setting time is too long, it can cause undesirable and costly delays in the construction process.Manipulating the amounts of accelerators and retarders in response to defined time changes, however, can add expense and requires additional testing of the concrete to determine if strength increases have been sacrificed. It is preferable that the additive composition strikes a consistent balance of performance – including strength enhancement and setting times – and cost to allow concrete manufacturers to accurately predict the setting time of the concrete they are making based on their prior experience with a particular cement. Therefore, it would be undesirable for a cement additive to significantly alter the setting time of the cement, because the cement manufacturer would then have difficulty maintaining a consistent setting time for their product when starting or stopping the use of that additive, or when altering the dosage of that additive.
[084] To measure the defined times, several different methods can be used. One commonly used method is to measure the penetration of a needle into a mortar under a fixed amount of force. As the mortar sets, the penetration distance decreases, allowing the setting times to be determined. Petition 870250101994, dated 07 / 11 / 2025, page 35 / 76 25 / 39 quantified. An example of this type of test is ASTM C 403 (Test for Time of Setting of Concrete Mixtures by Penetration Resistance). Another approach is to measure the heat output of the mortar using isothermal calorimetry. Since the increase in penetration resistance and the increase in heat output arise from the same chemical reactions between cement and water, the setting times estimated from the two approaches will be closely correlated.
[085] As stated above, the additive disclosed in this document can be used with cement mixtures, such as Portland cements, to improve the compressive strength of the resulting mortar or concrete composition. One way to determine compressive strength is found, for example, in ASTM C109: Standard Test Method for Compressive Strength of Hydraulic Cement Mortars. Another standard method is described in EN 196-1: Cement Test Methods.Hydrated cement compositions comprising the additives as disclosed herein have a significantly higher compressive strength, preferably a 2-day compressive strength of at least 10% and, more preferably, at least 20% higher than the product cured with cement without the addition of the additive as disclosed herein, and / or a 28-day compressive strength of at least 10% and preferably at least 15% higher than the product cured with cement without the addition of the additive as disclosed herein.
[086] In yet another aspect, the present disclosure is directed to a hydraulic cement composition, such as, for example, a Portland cement, comprising: 20 to 64 percent by mass of clinker; 5 to 60 percent by mass of calcined clay; 0 to 35 percent by mass of limestone; 0 to 10 percent by mass of calcium sulfate; an additive comprising: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetraquis-(2 Petition 870250101994, dated 07 / 11 / 2025, p. 36 / 76 26 / 39 hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10.
[087] In addition to clinker, the composition of hydraulic cement, in some embodiments, comprises at least one supplementary cementitious material chosen from ground granulated blast furnace slag, fly ash, natural pozzolan and calcined clay.
[088] The hydraulic cement composition disclosed in this document comprises 20 to 64 percent by mass of clinker; 5 to 60 percent by mass of calcined clay; 0 to 35 percent by mass of limestone; 0 to 10 percent by mass of calcium sulfate; and the additive as disclosed in this document.
[089] In some embodiments, the hydraulic cement composition comprises from 5% to 15% limestone by mass. In other embodiments, the hydraulic cement composition comprises from 5% to 35% limestone by mass. In still other embodiments, the hydraulic cement composition comprises from 20% to 35% limestone by mass. In still other embodiments, the hydraulic cement composition comprises at least 5% limestone by mass. In still other embodiments, the hydraulic cement composition comprises at least 10% limestone by mass. In still other embodiments, the hydraulic cement composition comprises at least 20% limestone by mass. In still other embodiments, the hydraulic cement composition comprises at least 22% limestone by mass. Petition 870250101994, dated 07 / 11 / 2025, page 37 / 76 27 / 39
[090] In some forms, the hydraulic composition of Portland cement also comprises at least 4% by mass of C3A.
[091] In embodiments, the composition of hydraulic cement has a total oxide composition comprising, in relation to a sum of dry weights of clinker, calcined clay, limestone and calcium sulfate: 5 to 25% by mass of Al2O3; 25 to 55% by mass of CaO; 20 to 40% by mass of SiO2; 2 to 10% by mass of SO3; and 0.1 to 10% by mass of Fe2O3.
[092] In other embodiments, the composition of hydraulic cement has a total oxide comprising, in relation to a sum of dry weights of clinker, calcined clay, limestone and calcium sulfate: 6 to 20% by mass of AbO3; 40 to 50% by mass of CaO; 22 to 35% by mass of SiO2; 2 to 5% by mass of SO3; and 0.5 to 8% by mass of Fe2O3.
[093] In another embodiment, a cementitious composition comprising: cement; and a means for increasing the strength of the cementitious composition by hardening the cementitious composition in an aqueous environment without substantially increasing the hardening time of the cementitious composition. In some embodiments, the hardening time is not increased by more than 35 minutes (0.58 h), preferably not more than 30 minutes (0.50 h), and more preferably not more than 25 minutes (0.42 h) and, most preferably, not more than 20 minutes (0.33 h) in relation to the same cementitious composition without the aforementioned means.
[094] One skilled in the art, using the preceding detailed description, may utilize the present invention to its full extent. The following examples are provided to illustrate the invention, but should not be construed as limiting the invention in any way, except as indicated in the appended claims. Petition 870250101994, dated 07 / 11 / 2025, page 38 / 76 28 / 39 Examples Example 1: Screening of effects on defined strength and time.
[095] The performance of an additive composition according to the present disclosure was evaluated using eight commercial North American cements, both as received and with limestone added in the amount necessary to achieve 22% of each cement. The mineral compositions of the cements tested as measured by quantitative x-ray diffraction (QXRD) are given in Table 1 for the received cement compositions. Table 1: Mineral composition of the cements (as received) tested for Example 1, as determined by QXRD. Cement C3S (% by weight) C2S (% by weight) C3A (% by weight) C4AF (% by weight) Limestone (% by weight) S1 56.6 11.9 4.8 9.4 4.8 S2 56.1 16.2 9.6 4.2 2.6 S3 44.8 21.9 5.0 6.4 10.8 S4 51.8 18.9 4.5 8.6 9.7 S5 49.4 18.2 6.9 4.9 12.0 S6 56.7 16.6 3.4 9.3 4.9 S7 65.3 9.9 3.1 8.1 5.0 S8 55.7 11.4 2.6 8.5 7.9
[096] To measure compressive strengths, mortar samples were prepared and tested according to EN 196-1. For each cement, mortar samples were prepared with and without the additive composition to measure the effect on compressive strength. The compositions of the additives evaluated are provided in Table 2, where composition EXP-1 represents a prior art composition as a reference and composition EXP-2 represents an exemplary composition of the present invention. Petition 870250101994, dated 07 / 11 / 2025, page 39 / 76 29 / 39 Table 2: Composition of the Evaluated Additives (Benchmark EXP-1) and (Inventive EXP-2)., Quantity in formulation (% by weight) Proportions EDIPA DEIPA TIPA Sodium Gluconate Sodium Thiocyanate Ratio r1 Amine / accelerator Ratio r2 Accelerator / retarder EXP-1 0.00 6.20 6.21 10.47 16.50 0.75 1.58 EXP-2 8.86 0.00 12.32 4.92 23.62 0.90 4.80
[097] One objective in developing a strength-enhancing composition is the successful use of the composition across a range of cements with varying compositions. Consequently, a performance screening was conducted using the eight commercial North American cements identified above, both as received and with lime added in an amount necessary to achieve 22% of the cement composition. For this screening, one dose of an inventive formulation EXP-2 and two doses of the reference formulation EXP-1 were tested. The resulting dosages and active concentrations of both additives are given in Table 3. Note that the ppm (parts per million) units refer to the mass of additive or chemical divided by the mass of cement being treated. Table 3: Dosages of additives and concentrations of active chemicals for the screening experiment of reference additives (EXP-1) and (EXP-2).________ Dose (ppm) Active quantity in the given dose (ppm) EDIPA DEIPA TIPA Sodium Gluconate Sodium Thiocyanate EXP-1 Dose 1 1500 0 93 93 157 248 Petition 870250101994, dated 07 / 11 / 2025, page 40 / 76 30 / 39 EXP-1 Dose 2 2500 0 155 155 262 413 EXP-2 2540 225 0 313 125 600
[098] The parameters that were measured were the mortar strength at 1 day, 2 days and 28 days and the initial hardening time. The mortar strengths were measured according to the EN 196-1 standard. Increasing strength at different ages is the main objective of the revealed additive compositions, therefore, in all cases, what is reported is the change in strength between a blank cement and the same cement made with the additive added to the mixing water at the dosage given in Table 3. Screening results
[099] Individual screening performance results are shown in Figures 1A-1H. Average results, in terms of change in resistance and adjustment time caused by the presence of additives, are summarized below in Table 4. Table 4: Average changes (compared to the control sample without additive) in 1D strength, 2D strength, 28D strength, and setting time from screening of North American cements. Cements as received Limestone added at 22% 1D (MPa) 2D (MPa) 28D (MPa) Set time (hours) 1D (MPa) 2D (MPa) 28D (MPa) Set time (hours) EXP-1 Dose 1 +3.88 +3.81 +4.48 +0.49 +3.76 +4.48 +6.51 +0.36 EXP-1 Dose 2 +5.55 +5.33 +6.12 +0.88 +4.35 +5.49 +7.01 +0.92 EXP-2 +6.22 +6.62 +9.18 +0.32 +4.99 +6.47 +9.45 +0.38 Petition 870250101994, dated 07 / 11 / 2025, page 41 / 76 31 / 39
[0100] Screening resulted in several notable differences between the performances of EXP-1 and EXP-2 in the cement compositions identified above. The reference additive EXP-1 was effective in increasing strength and showed a modest dose response (higher strengths at the higher dose).
[0101] The EXP-2 additive gave higher average strengths than the highest dose of EXP-1, and the dose response based on changing from the highest dose of EXP-1 (2500 ppm) to EXP-2 (2540) was very good, especially on 28D. This indicates that the EXP-2 additive is giving a surprisingly positive strength benefit based on its composition.
[0102] Tables 5 to 7 show the results of the change in mortar strength at 1 day, 2 days and 28 days, respectively. Table 5: Results of the change in mortar strength (compared to the blank without additive) in 1 day for commercial cements as received and supplemented with limestone. Cements as received (MPa) Limestone added at 22% Cement EXP-1 dose 1 EXP-1 dose 2 EXP-2 EXP-1 dose 1 EXP-1 dose 2 EXP-2 S1 +4.51 +5.08 +6.01 +3.07 +3.63 +3.33 S2 +4.39 +5.77 +7.27 +4.03 +5.13 +5.86 S3 +3.58 +5.50 +6.46 +3.65 +4.77 +6.47 S4 +4.42 +5.70 +5.82 +4.36 +5.03 +5.18 S5 +2.84 +4.54 +6.14 — — — S6 -- -- -- +2.23 +2.43 +2.90 S7 +1.96 +5.86 +5.10 +4.43 +4.36 +5.18 S8 +5.47 +6.37 +6.77 +4.54 +5.07 +6.02 Average +3.88 +5.55 +6.22 +3.76 +4.35 +4.99 Petition 870250101994, dated 07 / 11 / 2025, page 42 / 76 32 / 39 Table 6: Results of mortar strength change (compared to unadditived white mortar) over 2 days for commercial cements as received and supplemented with lime. Cements as received (MPa) Limestone added at 22% Cement EXP-1 dose 1 EXP-1 dose 2 EXP-2 EXP-1 dose 1 EXP-1 dose 2 EXP-2 S1 +4.56 +5.43 +6.05 +5.00 +6.28 +6.70 S2 +2.05 +2.88 +5.76 +3.85 +5.35 +6.52 S3 +2.90 +5.03 +6.37 +3.50 +5.13 +7.18 S4 +4.87 +5.89 +7.05 +4.74 +5.57 +6.40 S5 +2.99 +3.74 +6.40 -- -- -- S6 -- -- -- +4.46 +5.25 +6.16 S7 +3.34 +7.64 +8.27 +5.40 +5.50 +5.92 S8 +5.99 +6.70 +6.44 +4.42 +5.32 +6.40 Average +3.81 +5.33 +6.62 +4.48 +5.49 +6.47 Table 7: Results of mortar strength change (compared to unadditived white mortar) at 28 days for commercial cements as received and supplemented with lime. Cements as received (MPa) Limestone added at 22% Cement EXP-1 dose 1 EXP-1 dose 2 EXP-2 EXP-1 dose 1 EXP-1 dose 2 EXP-2 S1 +12.35 +13.08 +16.33 +9.60 +9.55 +11.92 S2 -0.25 +1.25 +5.18 +1.40 +1.30 +5.07 S3 +3.92 +6.07 +7.92 +4.15 +7.05 +7.55 S4 +5.08 +6.63 +6.80 +3.55 +3.75 +5.35 S5 +4.33 +4.28 +6.80 -- -- -- Petition 870250101994, dated 07 / 11 / 2025, p. 43 / 76 33 / 39 S6 -- -- -- +11.80 +10.85 +14.55 S7 +4.60 +6.35 +11.65 +9.25 +10.05 +11.78 S8 +4.10 +5.15 +9.55 +5.80 +6.55 +9.93 Average +4.88 +6.12 +9.18 +6.51 +7.01 +9.45
[0103] Screening results show that the inventive additive composition is very effective in increasing early and late age strength development for as-received cements and cements with added limestone. This indicates that the EXP-2 additive will be effective in allowing higher levels of limestone replacement in cements without loss of performance.
[0104] The primary compositional differences between EXP-2 and EXP-1 can be summarized as follows (see also Table 2): EXP-2 contains the alkanolamine EDIPA instead of DEIPA. The ratio of accelerator (sodium thiocyanate) to retarder (sodium gluconate) is higher in EXP-2 (4.80) than in EXP-1 (1.58). This is important for the time-defined stability of EXP-2, as discussed below. The importance of the component ratios is also discussed further below. Set schedules
[0105] For the screening described here, a calorimetry approach was used to estimate the initial hardening time of mortars made with and without additives. For all calorimetry results presented in this publication, a TAM-Air calorimeter was used and the temperature was fixed at 21°C. The approach to estimating the hardening time is illustrated in Figure 2, which shows the heat output rate (per gram of cement) of two mortar samples as a function of time since mixing. The hardening time is estimated as the time required for the heat output rate to reach a fixed value of 1.5 mW / g of cement. This fixed value is shown as a horizontal line in Figure 2. The time estimates defined for the two samples are the times in Petition 870250101994, dated 07 / 11 / 2025, page 44 / 76 34 / 39 that the rate curves cross this fixed horizontal line. The times are shown in Figure 2 as time T1 (for White) and T2 (for EXP-1 Dose 2).
[0106] Table 8 lists the absolute setting times and setting time changes for the as-received cements S1-S8 with and without the additives EXP-1 and EXP-2. Table 8: Define the time results for the received commercial cements. Absolute defined time (hours) Define time change (hours) Cement Blank EXP-1 dose 1 EXP-1 dose 2 EXP-2 EXP-1 dose 1 EXP-1 dose 2 EXP-2 S1 3.44 3.96 4.42 3.97 +0.52 +0.98 +0.53 S2 3.70 4.12 4.40 3.76 +0.42 +0.70 +0.06 S3 2.34 2.93 3.09 2.72 +0.59 +0.75 +0.38 S4 2.47 2.85 3.15 2.87 +0.38 +0.68 +0.40 S5 2.77 3.30 3.60 3.19 +0.53 +0.83 +0.42 S6 -- -- -- -- -- -- -- S7 2.61 3.21 3.63 2.95 +0.60 + 1.02 +0.34 S8 4.22 4.62 5.41 4.32 +0.40 + 1.19 +0.10 Average 3.08 3.57 3.96 3.40 +0.49 +0.88 +0.32
[0107] Table 9 lists the absolute setting times and the change in setting time for the as-received cements S1-S8 after the addition of powdered limestone to achieve 22% limestone - with and without the additives EXP-1 and EXP-2. Petition 870250101994, dated 07 / 11 / 2025, page 45 / 76 35 / 39 Table 9: Define time results for commercial cements with supplemental limestone totaling 22% by weight. Absolute defined time (hours) Define time change (hours) Cement Blank EXP-1 dose 1 EXP-1 dose 2 EXP-2 EXP-1 dose 1 EXP-1 dose 2 EXP-2 S1 3.45 3.93 4.56 4.09 +0.48 +1.11 +0.64 S2 3.39 4.19 4.69 3.89 +0.80 +1.30 +0.50 S3 2.53 3.14 3.33 2.81 +0.61 +0.80 +0.28 S4 2.57 3.05 3.14 2.85 +0.48 +0.57 +0.28 S5 — — — — — — — S6 3.10 3.58 3.70 3.15 +0.48 +0.60 +0.05 S7 2.49 3.34 3.54 3.16 +0.85 + 1.05 +0.67 S8 4.22 4.72 5.26 4.45 +0.50 + 1.04 +0.23 Average 3.11 3.71 4.03 3.49 +0.60 +0.92 +0.38
[0108] The increase in defined time was much smaller for the EXP-2 additive than for the highest dose of EXP-1 and slightly smaller than the lowest dose of EXP-1. This is a strong positive attribute, as it means that the EXP-2 additive can be used in high dosages without causing performance problems with the cement. Hydration kinetics
[0109] During the screening of North American cements described earlier, isothermal calorimetry was used to measure the rate of heat release from mortar samples at 21°C. As previously described, calorimetry was used to estimate the initial hardening time of mortars made with and without additives. Isothermal calorimetry is widely used as a way to investigate the hydration kinetics of cement in the early stages (generally up to a few days). Petition 870250101994, dated 07 / 11 / 2025, page 46 / 76 36 / 39 The shape of the heat release curves can provide information about the cement composition, including the sulfate level. The effects of any chemical additives or mixtures can also be observed. In this case, the calorimetry results reflect, to some extent, the previous screening conclusions. Figures 4A-4H show the calorimetry data for each of the cements tested – without an additive (White) and with the additives. The following discussion will highlight the calorimetry data for two of the screened cements, S2 and S7.
[0110] Notably, the S7 cement (Figure 4G) from screening did not show a large difference in initial strength between the reference EXP-1 additive and the EXP-2 additive according to the present invention. This is reflected by the similarity in the size and shape of the calorimetry curves. On the other hand, the S2 cement (Figure 4B) shows a more dramatic difference. The mortar sample made with EXP-2 has a larger secondary peak that actually has two peaks, while the sample made with EXP-1 has a single, slightly smaller secondary peak. This difference is reflected in a much larger difference in initial strength for the S2 cement, with the EXP-2 additive giving more strength intensification. The inventors believe that the change in peak shape illustrated by the calorimetry graph for S2 cement is caused by the presence of EDIPA in the EXP-2 formulation, which is a key factor in its performance relative to the reference formulation.Thus, calorimetry can provide a useful way to determine whether an additive formulation will provide improved strength performance for a given cement, compared to other available formulations. Example 2: Importance of the Relative Proportions of Additive Components
[0111] The relative mass ratios of the alkanolamine, retarder, and accelerator components of the additive compositions disclosed in this document are significant with respect to the performance of the compositions. To illustrate this, the following were Petition 870250101994, dated 07 / 11 / 2025, page 47 / 76 37 / 39 experiments were carried out in which the amine / accelerator and accelerator / retarder ratios, referred to as r1 and r2, respectively, were varied, maintaining the total active concentrations of these components at a constant value of 1000 ppm. Three r1 values (0.27, 0.82, and 2.46) and three r2 values (1.07, 3.20, and 9.60) were tested. The amine, retarder, and accelerator chemicals were the same as for the EXP-2 additive (see Table 2). Mortar samples were made with each combination of the two ratios, as well as the ratios in the EXP-2 formulation. The results, for mortars made with S2 cement, are shown in Figures 3A to 3D, where the size of the circle is proportional to the change in the raw material and where the EXP-2 formulation is shown as a shaded circle near the center.
[0112] As can be seen in Figures 3A to 3D, the changes in strength and setting time depend strongly on the component ratios. The EXP-2 formulation (shaded circle) provides an optimized result of high initial strength, high late strength, and minimal change in setting time. The EXP-1 additive is not graphically represented as it has a different amine chemical (DEIPA). However, the screening experiment showed that it gives less strength gain and longer setting time compared to EXP-2. The results of this experiment show that the surprisingly optimal performance of the inventive EXP2 additive arises not only from its individual chemical components but also from the specific balance of these components within the formulation. Example 3: Strength Test
[0113] A sample of industrial cement from a factory in North America manufactured using a glycol-based additive without strength-enhancing chemicals was used for this test. The mortar strength test was performed following the ASTM C109 standard using additive compositions as per this disclosure. The additive compositions tested are shown in Table 1. Petition 870250101994, dated 07 / 11 / 2025, page 48 / 76 38 / 39 10. All additives contain alkanolamine, accelerator, and retarder components. Additive A contains a mixture of DIEPA and tipa as the alkanolamine component and was used in two dosages. Additives B, C, and D contain EDIPA as the alkanolamine component. Table 10: Composition of additives used for Example 2 in ppm (mass of chemical product per mass of cement). Additive Type A (low dose) A (high dose) BCD DIEPA Amine 83 152 TIPA Amine 83 152 EDIPA Amine 164 164 164 Sodium Gluconate Retarder 59 109 109 Corn Syrup Retarder 60 60 Sodium Thiocyanate Accelerator 248 456 456 325 236 Total Actives 472 870 729 549 460
[0114] Resistance results are shown in Table 11. All additives significantly increased resistance. However, the additive compositions with EDIPA (additives B, C, and D) performed better than the additive compositions containing DEIPA and tipa, even when the dosage of Additive A was higher. For example, Additive D, with 460 ppm of active chemicals, gives +17% and +10% in 1D and 28D, respectively, while the high dose of additive A (870 ppm of active chemicals) gives +14% and +7% in 1D and 28D. Petition 870250101994, dated 07 / 11 / 2025, p. 49 / 76 39 / 39 respectively. This illustrates the particular advantage of using EDIPA in revealed additive formulations. Table 11: Strength results for Example 3, showing the increase in strength at two ages compared to a control mortar without additive. Additive 1D 28D A (low dose) + 10% +8% A (high dose) + 14% +7% B + 17% + 10% C + 19% + 10% D + 17% + 10%
[0115] Although this invention has been particularly shown and described with references to exemplary embodiments thereof, it will be understood by those skilled in the art that various alterations in form and details may be made to it without departing from the scope of the invention covered by the appended claims. Petition 870250101994, dated 07 / 11 / 2025, p. 50 / 76
Claims
1 / 4 CLAIMS 1. Composition for use as an additive to enhance the strength of a cementitious composition, the composition being CHARACTERIZED by comprising: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses; and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, the alkanolamine and the hardening accelerator being present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder being present in a mass ratio of 1 to 10.
2. Composition according to claim 1, CHARACTERIZED in that the alkanolamine and the hardening accelerator are present in a mass ratio of 0.4 to 1.8 and the hardening accelerator and the hardening retarder are present in a mass ratio of 3 to 8.
3. Composition according to claim 2, CHARACTERIZED in that the alkanolamine and the hardening accelerator are present in a mass ratio of 0.7 to 1.1 and the hardening accelerator and the hardening retarder are present in a mass ratio of 4 to 6.
5.
4. Composition according to claim 1, CHARACTERIZED by an alkanolamine comprising EDIPA and THEED.
5. Composition according to claim 1, CHARACTERIZED by further comprising from about 2 to about 8% by weight of at least one polyacrylic acid. Petition 870250101994, dated 07 / 11 / 2025, p. 51 / 76 2 / 4 6. Composition, according to claim 1, CHARACTERIZED in that the alkanolamine is present in 35.5 to 48.5 percent by mass, the hardening accelerator is present in 42.5 to 54.6 percent by mass and the hardening retarder is present in 7.0 to 13.0 percent by mass.
7. Composition according to claim 1, CHARACTERIZED by an alkanolamine comprising a mixture of EDIPA and tipa.
8. Composition, according to claim 1, CHARACTERIZED in that EDIPA is at least 30% of the total amount of alkanolamine.
9. Composition, according to claim 1, CHARACTERIZED by further comprising water.
10. Method for enhancing the strength of a cement composition, the method being CHARACTERIZED by comprising the steps of: (i) grinding a solid comprising Portland cement clinker in the presence of an additive, thereby preparing the cement composition, or (ii) making concrete from a mixture of a solid comprising Portland cement, sand, coarse aggregate, water and an additive, the additive comprising: an alkanolamine comprising ethanoldiisopropanolamine (EDIPA) and optionally at least one selected from the group consisting of triisopropanolamine (TIPA), diethanolisopropanolamine (DEIPA), triethanolamine (TEA) and tetrakis-(2-hydroxyethyl)ethylenediamine (THEED); at least one hardening retarder selected from the group consisting of a gluconate salt, sucrose, corn syrup and molasses;and at least one hardening accelerator selected from the group consisting of a thiocyanate salt, sodium chloride and calcium chloride, wherein the alkanolamine and the hardening accelerator are present in a mass ratio of 0.2 to 4.0 and the hardening accelerator and the hardening retarder are present in a mass ratio of 1 to 10, and wherein the cement composition, when cured, has a compressive strength at 2 days and at 28 days that is at least 10% greater than a cement composition without the additive.
11. Method according to claim 10, CHARACTERIZED in that the alkanolamine and the settled accelerator are present in a mass ratio of 0.7 to 1.1 and the settled accelerator and the settled retarder are present in a mass ratio of 4 to 6.
5.
12. Method according to claim 10, CHARACTERIZED in that the alkanolamine is EDIPA and THEED.
13. Method according to claim 12, CHARACTERIZED in that the alkanolamine is present in 23.0 to 62.0 percent by mass, the hardening accelerator is present in 31.5 to 66.0 percent by mass and the hardening retarder is present in 4.0 to 19.5 percent by mass.
14. Method according to claim 10, CHARACTERIZED in that the alkanolamine is present in 35.5 to 48.5 percent by mass, the hardening accelerator is present in 42.5 to 54.6 percent by mass and the hardening retarder is present in 7.0 to 13.0 percent by mass.
15. Method according to claim 10, CHARACTERIZED by the alkanolamine comprising a mixture of EDIPA and tipa.
16. Method according to claim 12, CHARACTERIZED in that EDIPA is at least 30% of the total amount of alkanolamine.
17. Method according to claim 10, CHARACTERIZED in that the solid further comprises at least one selected from the group consisting of limestone, fly ash, slag, pozzolan and calcined clay.
18. Method according to claim 10, CHARACTERIZED in that the solid further comprises at least 22% limestone by mass. Petition 870250101994, dated 07 / 11 / 2025, page 53 / 76 4 / 4 19. Strength-enhanced hydraulic cement powder composition CHARACTERIZED by comprising cement and the additive composition as defined in claim 1.
20. Composition according to claim 19, CHARACTERIZED in that the alkanolamine and the hardening accelerator are present in a mass ratio of 0.4 to 1.8 and the hardening accelerator and the hardening retarder are present in a mass ratio of 3 to 8.
21. Composition, according to claim 19, CHARACTERIZED in that the cement powder comprises at least 22% limestone by mass.
22. Composition, according to claim 19, CHARACTERIZED in that the cement powder comprises at least one selected from the group consisting of ground granulated blast furnace slag, fly ash, a pozzolan and calcined clay.
23. Composition, according to claim 19, CHARACTERIZED in that the cement powder composition has a setting time that is not increased by more than 35 minutes compared to the same cement powder composition without the additive.
24. Method according to claim 12, CHARACTERIZED in that the cement composition has a setting time that is not increased by more than 25 minutes compared to the same cement composition without the additive. Petition 870250101994, dated 07 / 11 / 2025, pp. 54 / 76