Double-sided shingled solar cell module and preparation method thereof

Through double-sided stacking technology, the front main gate electrode is connected and sintered to form a connection, which solves the area occupation and stability of traditional welding tape connections, and realizes efficient and reliable manufacturing of solar cell modules, simplifies the process flow and reduces the cost.

CN108987509BActive Publication Date: 2024-11-01ZHEJIANG AIKO SOLAR ENERGY TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN201810879880.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-08-03
Publication Date
2024-11-01
Estimated Expiration
2038-08-03

AI Technical Summary

Technical Problem

The metal welding tape connection method of traditional crystalline silicon module battery cell occupies the light-receiving area on the front of the module, and there are fractures and corrosion caused by line loss and temperature changes, which affects the conversion efficiency and performance stability. The bonding connection of the stacking technology is complex and unstable. , increasing resistance loss and process complexity.

Method used

A double-sided stacked tiled solar cell module is used to pretreat and cut the front and back electrodes of the solar cell to form a stacked tiled battery string, and the front main gate electrodes are connected and connected by sintering, which simplifies the process flow and reduces costs.

Benefits of technology

It realizes solar cell modules with simple structure, simplified process, low cost, high reliability and high photoelectric conversion efficiency, reduces the line loss and resistance loss of traditional metal welding tapes, and improves the connection force and reliability of the components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN108987509B_ABST
    Figure CN108987509B_ABST
Patent Text Reader

Abstract

The present invention discloses a double-sided shingled solar cell assembly, comprising at least two solar cells, the solar cells are stacked and arranged in sequence to form a shingled cell string, the solar cell comprises a front electrode and a back electrode, the front electrode comprises a front main grid and a front sub-grid, the back electrode comprises a back sub-grid, the long sides of adjacent solar cells overlap to form a surface contact; the adjacent solar cells are connected by the front main grid electrode, and a shingled cell string is formed by sintering. Correspondingly, the present invention also provides a method for preparing a double-sided shingled solar cell assembly. The present invention has a simple structure, a simplified process flow, reduced process steps, and reduced costs, and the reliability of the cell assembly is high and the photoelectric conversion efficiency is high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solar cells, and in particular to a double-sided shingled solar cell assembly and a preparation method thereof. Background Art

[0002] Traditional crystalline silicon module cells are basically connected by metal welding ribbons. This connection method has three obvious defects: first, the gap between the metal welding ribbon and the cell occupies the light-receiving area on the front of the module; second, the metal welding ribbon has line loss; third, the welding ribbon is prone to breakage and corrosion due to thermal expansion and contraction due to temperature changes. All three methods have a great impact on the conversion efficiency and performance stability of the module.

[0003] In order to overcome the above problems, a technology using shingling technology to connect solar cells into modules has emerged. Conventional shingled modules are made by slicing the cells and then bonding the cells into strings using special conductive adhesive materials.

[0004] For example, Chinese patent publication number CN106489211A discloses a shingled solar cell module, which comprises: a plurality of super cells arranged in two or more parallel rows, each super cell comprising a plurality of rectangular or substantially rectangular silicon solar cells arranged in a straight line, wherein long sides of adjacent silicon solar cells overlap and are directly conductively bonded to each other to electrically connect the silicon solar cells in series; and a hidden tap contact pad located on a back surface of a first solar cell, the hidden tap contact pad not conducting a large current during normal operation; wherein the first solar cell is located in the middle of a first super cell in the first row of super cells, and the hidden tap contact pad is electrically connected in parallel to at least a second solar cell in the second row of super cells.

[0005] The adjacent solar cells are connected by conductive adhesive, which has a complex process, an unstable connection effect, increases resistance loss, and affects the overall photoelectric conversion efficiency.

[0006] Furthermore, it is required that the conductive adhesive used for the conductive bonding between the overlapping adjacent solar cells in a super cell be different from the conductive adhesive used for the conductive bonding between the super cell and the flexible electrical interconnect, which further increases the complexity of the process operation, the number of process steps, the chance of error, and the reliability of the product cannot be guaranteed. Summary of the invention

[0007] The technical problem to be solved by the present invention is to provide a double-sided shingled solar cell module with a simple structure, simplified process flow, reduced process steps, and lower costs. The cell module has high reliability and high photoelectric conversion efficiency.

[0008] The technical problem to be solved by the present invention is also to provide a method for preparing a double-sided shingled solar cell module, which simplifies the process flow, reduces the process steps, has low cost, is easy to promote, and has high photoelectric conversion efficiency.

[0009] In order to solve the above technical problems, the present invention provides a double-sided shingled solar cell assembly, comprising at least two solar cells, wherein the solar cells are stacked and arranged in sequence to form a shingled cell string, wherein the solar cell comprises a front electrode and a back electrode, wherein the front electrode comprises a front main grid and a front auxiliary grid, and the back electrode comprises a back auxiliary grid, and the long sides of the adjacent solar cells overlap to form a surface contact;

[0010] The adjacent solar cells are connected via the front main grid electrode and are sintered to form a shingled cell string.

[0011] As a preferred embodiment of the above scheme, the solar cell is a slice formed by cutting a silicon wafer after pretreatment, and each slice is provided with a front main grid and a plurality of front sub grids on the front side.

[0012] As a preferred embodiment of the above solution, the adjacent solar cells are connected via a front main grid electrode, and the front main grid of each solar cell is arranged on the back side of the previous solar cell.

[0013] As a preferred embodiment of the above solution, the solar cell comprises a first solar cell and a second solar cell;

[0014] The front electrode of the first solar cell comprises a front main grid and a front auxiliary grid, and the back electrode comprises a back auxiliary grid;

[0015] The front electrode of the second solar cell comprises a front main grid and a front sub-grid, and the back electrode comprises a back main grid and a back sub-grid;

[0016] The first solar cells are stacked and arranged in sequence, and finally connected with the second solar cells in a stacked manner.

[0017] As a preferred embodiment of the above solution, the shingled battery string is configured as one or more rows of shingled battery strings;

[0018] Each row of shingled cell strings includes one or more first solar cells and one second solar cell;

[0019] One or more first solar cells are stacked and arranged in sequence, and finally are stacked and connected with second solar cells, and the second solar cells are arranged at the outermost side.

[0020] As a preferred embodiment of the above scheme, the shingled cell string is configured as multiple rows of shingled cell strings, the solar cells of a single row of shingled cell strings are connected in series, and different rows of shingled cell strings are connected in parallel or in series via welding strips.

[0021] As a preferred embodiment of the above solution, the area of ​​the overlapping regions of adjacent solar cells is 0.5-20% of the area of ​​a single solar cell.

[0022] Correspondingly, the present invention also discloses a method for preparing a double-sided shingled solar cell module, comprising:

[0023] (1) Pre-treating the silicon wafer and printing the front electrode and the back electrode on the surface of the silicon wafer;

[0024] (2) Cutting silicon wafers to form solar cells;

[0025] (3) stacking the solar cells one by one, with the long sides of adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying;

[0026] (4) sintering the shingled battery string at high temperature to solidify the slurry;

[0027] (5) The shingled cell strings are subjected to anti-LID annealing, and after grading testing, they are packaged into shingled modules.

[0028] Correspondingly, the present invention also discloses another method for preparing a double-sided shingled solar cell module, comprising:

[0029] (1) Pre-processing the silicon wafer and then cutting it to form a solar cell;

[0030] (2) Printing front and back electrodes on the surface of solar cells;

[0031] (3) stacking the solar cells one by one, with the long sides of the adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying;

[0032] (4) sintering the shingled battery string at high temperature to solidify the slurry;

[0033] (5) The shingled cell strings are subjected to anti-LID annealing, and after grading testing, they are packaged into shingled modules.

[0034] As a preferred embodiment of the above scheme, the silicon wafer is pretreated, and the pretreatment includes:

[0035] (1.1) Forming a velvet surface on the front and back sides of the silicon wafer;

[0036] (1.2) High square resistance diffusion is performed on the front side of the silicon wafer to form a PN junction;

[0037] (1.3) Selective laser doping of the front side of the silicon wafer;

[0038] (1.4) Remove the byproducts and surrounding PN junctions formed during the diffusion process and polish the back of the silicon wafer;

[0039] (1.5) Depositing a passivation film and a protective film on the back of the silicon wafer;

[0040] (1.6) Depositing passivation film and anti-reflection film on the front side of the silicon wafer;

[0041] (1.7) Laser groove the passivation film and protective film on the back of the silicon wafer.

[0042] The implementation of the present invention has the following beneficial effects:

[0043] The present invention provides a double-sided shingled solar cell assembly, comprising at least two solar cells, wherein the long sides of the adjacent solar cells overlap to form a surface contact; and the adjacent solar cells are connected through a front main grid electrode and sintered to form a shingled cell string, which has the following advantages:

[0044] 1. The present invention adopts a connection method of sharing the front main grid slurry between adjacent slices, replacing the conductive adhesive bonding between conventional shingled cells, integrating laser cutting and shingled connection of slices into the battery manufacturing process, eliminating the back main grid slurry, and greatly simplifying the manufacturing process of double-sided shingled modules, reducing equipment costs and production costs;

[0045] 2. The connection method of the shared front main grid paste between adjacent slices of the present invention also simplifies the design requirements of the double-sided shingled battery pattern. It is no longer necessary to consider the symmetry of the slice pattern, and there is no need to increase the design of the slice positioning points and welding positioning points, which increases the flexibility of the design of the front and back electrode patterns;

[0046] 3. The adjacent slices of the present invention are connected by a common front main grid slurry, which reduces the series resistance and resistance loss compared with the conductive glue connection method, and significantly improves the power of the double-sided shingled module;

[0047] 4. The adjacent slices of the present invention share the front main grid paste, and can form a shingled battery string by sintering, that is, the preparation process of the shingled battery string is integrated into the ordinary solar cell manufacturing process, further simplifying the process flow, reducing the process steps, and reducing costs. The prior art is to first prepare the product according to the ordinary solar cell, then slice it, and then prepare it into a shingled module according to the shingling technology. The two preparation processes of the prior art are independent of each other;

[0048] 5. The process flow of the present invention is relatively simple, each process step is relatively mature, and is integrated into the ordinary solar cell manufacturing process, reducing the probability of errors in the manufacturing process and increasing the reliability of the product;

[0049] 6. The solar cells of the present invention are connected by front and back shingles, with no metal welding strips on the surface and no gaps between the cells, which fully utilizes the available area of ​​the component surface and reduces the line loss of traditional metal welding strips, thereby greatly improving the conversion efficiency of the component;

[0050] 7. The traditional metal welding strip connection method is line connection, while the shingled assembly of the present invention is surface connection, which effectively improves the connection strength between battery cells and makes the assembly more reliable. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram of the segmentation of the front side of the silicon wafer of the present invention;

[0052] Figure 2 is a schematic diagram of the segmentation of an embodiment of the back side of a silicon wafer of the present invention;

[0053] Figure 3 is a schematic diagram of segmentation of another embodiment of the back side of a silicon wafer of the present invention;

[0054] Figure 4 is a schematic diagram of the shingled assembly of the present invention during the stacking arrangement process;

[0055] Figure 5 yes Figure 4 A schematic structural diagram of the front side of the manufactured shingled assembly;

[0056] Figure 6 yes Figure 4 A schematic structural diagram of the back side of the manufactured shingled assembly;

[0057] Figure 7 yes Figure 4 A cross-sectional view of the produced shingled assembly;

[0058] Figure 8 is a schematic diagram of the shingled assembly of the present invention in another stacking arrangement process;

[0059] Fig. 9 yes Figure 8 A schematic structural diagram of the front side of the manufactured shingled assembly;

[0060] Fig.10 yes Figure 8 A schematic structural diagram of the back side of the manufactured shingled assembly;

[0061] Fig.11 yes Figure 8 A cross-sectional view of the produced shingled assembly;

[0062] Fig.12 It is a flow chart of the method for preparing a double-sided shingled solar cell module of the present invention;

[0063] Fig.13 It is a flow chart of another method for preparing a double-sided shingled solar cell module of the present invention. DETAILED DESCRIPTION

[0064] In order to make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings.

[0065] The present invention provides a double-sided shingled solar cell assembly, comprising at least two solar cells 1, wherein the solar cells 1 are stacked in sequence to form a shingled cell string 10. The solar cell 1 comprises a front electrode and a back electrode, wherein the front electrode comprises a front main grid 11 and a front auxiliary grid 12, and the back electrode comprises a back auxiliary grid 13.

[0066] like Figure 1 , Figure 2 and Figure 3 As shown, the solar cell 1 is a slice formed by cutting a silicon wafer after pretreatment, and each slice is provided with a front main grid 11 and a plurality of front auxiliary grids 12 (such as Figure 1 A plurality of back side secondary grids 13 and back side main grids 14 are provided on the back side of each slice (as shown in FIG. Figure 2 Alternatively, a plurality of back side sub-grids 13 are provided on the back side of each slice (as shown in FIG. Figure 3 shown). Figure 1 , Figure 2 and Figure 3 The dotted lines in the figure are the cutting lines of the silicon wafer.

[0067] It should be noted that the main grid and the auxiliary grid of the present invention can be in the form of straight lines, segments, curves, etc., and the laser cutting line can also be a straight line or a curve, and is not limited to this. Moreover, in addition to the main grid and the auxiliary grid, the present invention can also be provided with a spine. The implementation methods of the solar cell assembly are diverse, and the implementation methods of the present invention are not limited to the examples given.

[0068] like Figure 4 As shown, in the stacking arrangement process of the present invention, the adjacent solar cells 1 are connected via the front main grid 11 electrodes, and the front main grid 11 of each solar cell is arranged on the back of the previous solar cell. Figure 5 , Figure 6 and Figure 7 As shown, in the assembled shingled cell string, the long sides of the adjacent solar cells 1 overlap to form a surface contact; the adjacent solar cells 1 are connected via the front main grid electrode and are sintered to form a shingled cell string 10.

[0069] and Figure 8-11 FIG. 1 is a schematic diagram of another embodiment of a solar cell string 10 composed of solar cells 1. Figure 4-7 The difference between the shingled cell string shown is that Figure 8-11 Another solar cell shape is selected, which is similar to a trapezoid and is the outer slice of the silicon wafer.

[0070] It should be noted that the present invention can use solar cells of various shapes, preferably rectangular, trapezoidal, or similar to rectangular or trapezoidal, but not limited thereto.

[0071] The present invention pre-processes and cuts traditional silicon wafers into solar cells. The solar cells are connected in a front-to-back shingled manner. There is no metal welding strip on the surface and no gap between the cells. The available area of ​​the component surface is fully utilized, and the line loss of the traditional metal welding strip is reduced, thereby greatly improving the conversion efficiency of the component.

[0072] Furthermore, the conventional metal welding strip connection method is line connection, while the shingled assembly of the present invention is surface connection, which effectively improves the connection strength between the battery cells and makes the assembly more reliable.

[0073] Most importantly, the adjacent slices of the present invention are connected by a common front main grid paste, replacing the conductive adhesive bonding between conventional shingled cells, integrating laser cutting and shingled connection of the slices into the cell manufacturing process, eliminating the back main grid paste, and greatly simplifying the manufacturing process of double-sided shingled components, reducing equipment costs and production costs.

[0074] The invention adopts a connection method of sharing the front main grid paste between adjacent slices, which also simplifies the design requirements of the double-sided shingled battery pattern. It no longer needs to consider the symmetry of the slice pattern, and there is no need to add the design of slice positioning points and welding positioning points, which increases the flexibility of the front and back electrode pattern design.

[0075] The adjacent slices of the present invention are connected by a common front main grid slurry, which reduces the series resistance and resistance loss compared with the conductive adhesive connection method, and significantly improves the power of the double-sided shingled component.

[0076] Preferably, Figure 7 and Fig.11As shown, the area of ​​the overlapping region 2 of adjacent solar cells 1 is 0.5-20% of the area of ​​a single solar cell 1, which can ensure the stability of the adjacent solar cells connected by the front main grid electrode, reduce the series resistance and resistance loss, and significantly improve the power of the single-sided shingled component. Moreover, it can also simplify the difficulty of the preparation process, save silicon materials in the overlapping area, and implement it at a lower cost. When the area of ​​the overlapping area of ​​adjacent solar cells is 0.5-20% of the area of ​​a single solar cell, the series resistance and resistance loss can be reduced by an additional 10% under the premise of the basic scheme of the present invention. If the area of ​​the overlapping area of ​​adjacent solar cells is less than 0.5% of the area of ​​a single solar cell, the width of the shared main grid is smaller, which affects the transmission of current; if the area of ​​the overlapping area of ​​adjacent solar cells is greater than 20% of the area of ​​a single solar cell, the series resistance and resistance loss are not significantly reduced, and the photoelectric conversion efficiency of solar energy cannot be significantly improved. Moreover, the larger the area of ​​the overlapping area, the more silicon material is used. Therefore, the overlapping area needs to take a balance value. Further preferably, the area of ​​the overlapping region 2 of adjacent solar cells 1 is 1-10% of the area of ​​a single solar cell 1. More preferably, the area of ​​the overlapping region 2 of adjacent solar cells 1 is 2-8% of the area of ​​a single solar cell 1.

[0077] The shingled battery string 10 of the present invention can be set as one or more rows of shingled battery strings, and the solar cells 1 of each row of shingled battery strings 10 are connected in series. When the shingled battery string 10 is set as multiple rows, the solar cells 1 of a single row of shingled battery strings 10 are connected in series; different rows of shingled battery strings 10 are connected in parallel or in other ways, and the connection methods are various, which are not limited by the present invention. Preferably, different rows of shingled battery strings 10 are connected in parallel or in series through welding strips.

[0078] In each row of shingled cell strings 10, the front main grid 11 located at the front side serves as the negative electrode, and the back main grid 14 located at the back side serves as the positive electrode. Generally speaking, the front main grid 11 located at the front side is arranged on one side of the row of shingled cell strings 10, and the back main grid 14 located at the back side is arranged on the other side of the row of shingled cell strings 10. At this time, the back electrode of the solar cell arranged on the other side of the row of shingled cell strings is provided with not only a back auxiliary grid but also a back main grid.

[0079] In order to better describe this technical solution, the present invention divides the solar cell 1 into a first solar cell and a second solar cell; the front electrode of the first solar cell includes a front main grid 11 and a front auxiliary grid 12, and the back electrode includes a back auxiliary grid 13; the front electrode of the second solar cell includes a front main grid 11 and a front auxiliary grid 12, and the back electrode includes a back main grid 14 and a back auxiliary grid 13; the first solar cells are stacked and arranged in sequence, and finally stacked and connected with the second solar cells.

[0080] Preferably, each row of shingled cell strings 10 includes one or more first solar cells and one second solar cell; the one or more first solar cells are stacked and arranged in sequence, and finally connected to the second solar cells in a stacked manner, and the second solar cells are arranged at the outermost side.

[0081] Correspondingly, the present invention also discloses a method for preparing a double-sided shingled solar cell module, such as Fig.12 As shown, including:

[0082] S101, pre-treating the silicon wafer and printing the front electrode and the back electrode on the surface of the silicon wafer.

[0083] Specifically, according to the pattern design of the electrode, the front main grid and the front auxiliary grid are printed on the front side of the silicon wafer, and the back auxiliary grid and the back main grid are printed on the back side of the silicon wafer. It should be noted that 1-2 back main grids are sufficient.

[0084] S102, cutting the silicon wafer to form a solar cell;

[0085] The cut solar cell comprises a first solar cell and a second solar cell; the front electrode of the first solar cell comprises a front main grid 11 and a front auxiliary grid 12, and the back electrode comprises a back auxiliary grid 13; the front electrode of the second solar cell comprises a front main grid 11 and a front auxiliary grid 12, and the back electrode comprises a back main grid 14 and a back auxiliary grid 13.

[0086] The cutting is preferably performed by laser cutting, which is less likely to cause fragments and can ensure the accuracy of size.

[0087] S103, stacking the solar cells one by one, with the long sides of the adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying;

[0088] Specifically, each row of shingled cell strings 10 includes one or more first solar cells and one second solar cell; the one or more first solar cells are stacked and arranged in sequence, and finally connected to the second solar cells in a stacked manner, and the second solar cells are arranged at the outermost side.

[0089] The solar cells 1 of different rows of shingled cell strings 10 are connected in parallel or in other ways. The connection methods are various and are not limited in the present invention.

[0090] S104, sintering the shingled battery string at high temperature to solidify the slurry;

[0091] S105, perform anti-LID annealing on the shingled cell strings, perform grading tests, and then package them into shingled modules.

[0092] It should be noted that anti-LID annealing refers to light induced degradation annealing.

[0093] After the grading test, batteries of the same grading level are packaged into the same component to ensure the maximum power output of the component and the stability of the power output.

[0094] The present invention can adopt another method for preparing a double-sided shingled solar cell module, such as Fig.13 As shown, including:

[0095] S201, pre-processing the silicon wafer, and then cutting it to form a solar cell;

[0096] The cutting is preferably performed by laser cutting, which is less likely to cause fragments and can ensure the accuracy of size.

[0097] S202, printing a front electrode and a back electrode on the surface of the solar cell;

[0098] The solar cell comprises a first solar cell and a second solar cell; the front electrode of the first solar cell comprises a front main grid 11 and a front auxiliary grid 12, and the back electrode comprises a back auxiliary grid 13; the front electrode of the second solar cell comprises a front main grid 11 and a front auxiliary grid 12, and the back electrode comprises a back main grid 14 and a back auxiliary grid 13. The present invention performs printing according to the pattern design of the first solar cell and the second solar cell.

[0099] S203, stacking the solar cells one by one, with the long sides of the adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying;

[0100] Specifically, each row of shingled cell strings 10 includes one or more first solar cells and one second solar cell; the one or more first solar cells are stacked and arranged in sequence, and finally connected to the second solar cells in a stacked manner, and the second solar cells are arranged at the outermost side.

[0101] The solar cells 1 of different rows of shingled cell strings 10 are connected in parallel or in other ways. The connection methods are various and are not limited in the present invention.

[0102] S204, sintering the shingled battery string at high temperature to solidify the slurry;

[0103] S205, performing anti-LID annealing on the shingled cell strings, and packaging them into shingled modules after grading tests.

[0104] It should be noted that anti-LID annealing refers to light induced degradation annealing.

[0105] After the grading test, batteries of the same grading level are packaged into the same component to ensure the maximum power output of the component and the stability of the power output.

[0106] The present invention integrates laser cutting and shingled connection of slices into the battery manufacturing process. Adjacent slices share the front main grid paste, and a shingled battery string can be formed by sintering, which further simplifies the process flow, reduces the process steps, and reduces the cost. The prior art first prepares the product according to ordinary solar cells, then slices them, and then prepares them into shingled components according to the shingling technology. The two preparation processes of the prior art are independent of each other.

[0107] Furthermore, the process flow of the present invention is relatively simple, each process step is relatively mature, and is integrated into the ordinary solar cell manufacturing process, thereby reducing the probability of errors in the manufacturing process and increasing the reliability of the product.

[0108] Fig.12 and Fig.13 The manufacturing method shown differs in that the cutting is performed before or after printing the front and back electrodes.

[0109] Further, the preprocessing includes:

[0110] (1.1) Forming a velvet surface on the front and back sides of the silicon wafer;

[0111] The silicon wafer may be P-type silicon or N-type silicon.

[0112] (1.2) High square resistance diffusion is performed on the front side of the silicon wafer to form a PN junction;

[0113] The square resistance is generally preferably 80-200Ω / □, but is not limited thereto.

[0114] (1.3) Selective laser doping of the front side of the silicon wafer;

[0115] The laser doping pattern needs to correspond to the subsequent front electrode sub-grid pattern, which can be designed using existing technology.

[0116] (1.4) Remove the byproducts and surrounding PN junctions formed during the diffusion process and polish the back of the silicon wafer;

[0117] If phosphorus diffusion is used to form N-type silicon on the front side of the silicon wafer, the byproduct is phosphorus silicon glass;

[0118] If boron diffusion is used to form P-type silicon on the front side of the silicon wafer, the by-product is borosilicate glass.

[0119] (1.5) Depositing a passivation film and a protective film on the back of the silicon wafer;

[0120] The passivation film is preferably a silicon dioxide film, an aluminum oxide film or a silicon nitride film, and the protective film is preferably a silicon nitride film, a silicon oxynitride film, a silicon dioxide film or a composite film composed of the above films, but is not limited thereto.

[0121] (1.6) Depositing passivation film and anti-reflection film on the front side of the silicon wafer;

[0122] The passivation film is preferably a silicon dioxide film, an aluminum oxide film or a silicon nitride film; the anti-reflection film is preferably a silicon nitride film or a silicon dioxide film, but is not limited thereto.

[0123] (1.7) Laser groove the passivation film and protective film on the back of the silicon wafer.

[0124] The laser groove pattern corresponds to the subsequent back sub-grid line pattern, which is generally a straight line or line segment type.

[0125] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A double-sided shingled solar cell assembly, comprising at least two solar cells, wherein the solar cells are stacked in sequence to form a shingled cell string, It is characterized in that The solar cell comprises a front electrode and a back electrode, the front electrode comprises a front main grid and a front sub-grid, the back electrode comprises a back sub-grid, and the long sides of adjacent solar cells overlap to form a surface contact; The adjacent solar cells are connected via the front main grid and the back auxiliary grid electrode, and are dried and sintered to form a shingled cell string; The area of ​​the overlapping region of adjacent solar cells is 0.5-20% of the area of ​​a single solar cell; The solar cell comprises a first solar cell and a second solar cell; The front electrode of the first solar cell comprises a front main grid and a front auxiliary grid, and the back electrode comprises a back auxiliary grid; The front electrode of the second solar cell comprises a front main grid and a front sub-grid, and the back electrode comprises a back main grid and a back sub-grid; The first solar cells are stacked and arranged in sequence, and finally connected with the second solar cells in a stacked manner.

2. The double-sided shingled solar cell module according to claim 1, It is characterized in that The solar cell slices are slices formed by cutting silicon slices after pretreatment, each slice has a front main grid and a plurality of front auxiliary grids on the front side, and a plurality of back auxiliary grids on the back side.

3. The double-sided shingled solar cell module according to claim 1, It is characterized in that The adjacent solar cells are connected via a front main grid electrode, and the front main grid of each solar cell is arranged on the back of the previous solar cell.

4. The double-sided shingled solar cell module according to claim 1, It is characterized in that The shingled battery string is arranged as one or more rows of shingled battery strings; Each row of shingled cell strings includes one or more first solar cells and one second solar cell; One or more first solar cells are stacked and arranged in sequence, and finally are stacked and connected with second solar cells, and the second solar cells are arranged at the outermost side.

5. The double-sided shingled solar cell module according to claim 4, It is characterized in that The shingled cell string is configured as a plurality of rows of shingled cell strings, wherein the solar cells of a single row of the shingled cell string are connected in series, and different rows of the shingled cell strings are connected in parallel or in series via welding strips.

6. A method for preparing a double-sided shingled solar cell module according to any one of claims 1 to 5, It is characterized in that include: (1) Pre-treating the silicon wafer and printing the front electrode and the back electrode on the surface of the silicon wafer; (2) Cutting silicon wafers to form solar cells; (3) stacking the solar cells one by one, with the long sides of adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying; (4) sintering the shingled battery string at high temperature to solidify the slurry; (5) The shingled cell strings are subjected to anti-LID annealing, and after grading testing, they are packaged into shingled modules.

7. A method for preparing a double-sided shingled solar cell module according to any one of claims 1 to 5, It is characterized in that include: (1) Pre-processing the silicon wafer and then cutting it to form a solar cell; (2) Printing front and back electrodes on the surface of solar cells; (3) stacking the solar cells one by one, with the long sides of adjacent solar cells overlapping and connected through the front main grid to form a shingled cell string, and drying; (4) sintering the shingled battery string at high temperature to solidify the slurry; (5) Anti-LID annealing is performed on the shingled cell strings, and after grading testing, they are packaged into shingled modules.

8. A method for preparing a double-sided shingled solar cell module according to claim 6 or 7, It is characterized in that The silicon wafer is pre-processed, and the pre-processing includes: (1.1) Forming a velvet surface on the front and back sides of the silicon wafer; (1.2) High square resistance diffusion is performed on the front side of the silicon wafer to form a PN junction; (1.3) Selective laser doping of the front side of the silicon wafer; (1.4) Remove the byproducts and surrounding PN junctions formed during the diffusion process and polish the back of the silicon wafer; (1.5) Depositing a passivation film and a protective film on the back of the silicon wafer; (1.6) Depositing passivation film and anti-reflection film on the front side of the silicon wafer; (1.7) Laser groove the passivation film and protective film on the back of the silicon wafer.

Citation Information

Cited By

  • Preparation method of solar cell and solar cell

    CN121013468A