High photoelectric conversion efficiency solar cell and method for manufacturing high photoelectric conversion efficiency solar cell
By using a protective film composed of a compound containing aluminum oxide in a back electrode type solar cell, the problems of high manufacturing cost and poor protection effect are solved, and high photoelectric conversion efficiency and low-cost solar cell manufacturing are achieved.
Patent Information
- Application Number
- CN201680090602.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2016-11-07
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2036-11-07
Smart Images

Figure CN110073498B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a solar cell with high photoelectric conversion efficiency and a method for manufacturing the solar cell with high photoelectric conversion efficiency. Background Art
[0002] As a method for improving the photoelectric conversion efficiency of crystalline silicon solar cells, so-called back electrode type solar cells that eliminate the electrodes on the light-receiving surface and avoid optical losses due to the shadows of the electrodes have been widely studied in recent years.
[0003] Fig.10 This is a cross-sectional schematic diagram showing the basic structure of a back electrode type solar cell. Fig.10 In the back electrode type solar cell 1000, a p-type region 1002 of an additive imparting p-type conductivity by high-concentration diffusion is formed on the non-light-receiving surface of the substrate 1001, and an n-type region 1003 of an additive imparting n-type conductivity by high-concentration diffusion is formed adjacent thereto.
[0004] The p-type region 1002 and the n-type region 1003 are covered with protective films 1004 and 1005 respectively to reduce the loss caused by the recombination of carriers excited by light. Then, the positive electrode 1006 and the negative electrode 1007 are formed by penetrating the protective film 1004. In addition, Fig.10 Although not shown, a texture having projections and depressions of several micrometers is formed on the light-receiving surface of the substrate 1001 for confining light.
[0005] In the back electrode type solar cell, since there is no electrode on the light receiving surface, it is necessary to prevent the charge carriers excited by the short wavelength light from recombination and reaching the back side. Since the dangling bonds (unbonded electron pairs of silicon) that become the recombination centers of the charge carriers are actually present at a high density on the substrate surface, the protective film 1005 is required to have very high protection performance.
[0006] However, the recombination ratio of charge carriers is the sum of the bulk recombination ratio of the crystal bulk and the surface recrystallization ratio on the crystal surface. Generally speaking, when the concentration of added impurities (charge carrier concentration at room temperature) is increased in crystalline silicon, bulk recombination increases. This is due to the crystal defects of the added impurities or the direct recombination of the Auger process that becomes significant as the carrier concentration increases. Therefore, in general, in high concentration regions such as the p-type region 1002 and the n-type region 1003, the maximum added impurity concentration in the depth direction of the substrate is controlled to, for example, 10 18 atoms / cm 3In the first half of the degree, its surface is covered with an effective protective film to suppress the carrier recombination loss on the back side.
[0007] In addition, the surface protective layer has two elements: chemical termination and field effect. The field effect is an effect that uses the fixed charges embedded in the protective film to generate an electric field on the substrate surface, reduce the concentration of charge carriers near the surface, and reduce the recombination on the surface. In solar cells, positively charged silicon nitride or negatively charged aluminum oxide is generally used as a field effect protective layer.
[0008] In principle, the protective effect of the field effect type protective layer can be obtained regardless of the conductivity type of the substrate surface to which it is applied. However, when a film having a fixed charge of the same polarity as the majority carriers on the substrate surface is applied and electrodes are formed on the same surface, it is known that a minority of carriers will flow into the electrode of the opposite polarity to the electrode where they are supposed to be collected, thereby reducing the output of the solar cell.
[0009] Regarding this problem, Patent Document 1 describes an example in which an aluminum oxide film is formed on the surface of the p-type region of a back electrode type solar cell, silicon oxide is applied to the surface of the n-type region, and silicon nitride is applied to the light-receiving surface.
[0010] On the other hand, silicon oxide is a representative example of chemical termination type protective layers. Silicon oxide has a positive charge, and although it varies depending on the manufacturing method, it is considered to be a material that can be used on both p-type and n-type surfaces because its fixed charge density is 1 to 2 digits lower than that of general silicon nitride and its defect density at the interface with crystalline silicon is relatively low. In the example of non-patent document 1 (Mulligan), silicon oxide is applied to both the light-receiving surface and the back surface of a solar cell using an n-type substrate.
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2008-010746
[0014] Non-patent literature
[0015] Non-patent document 1: William P. Mulligan et al., Proceedings of 19th EU PVSEC pp. 387-390 (2004). Summary of the invention
[0016] Problems to be solved by the invention
[0017] However, the back structure of the solar cell of Patent Document 1 has a high protective effect, but on the other hand, the steps are complicated due to the need for patterning, resulting in a problem of high cost. In addition, silicon nitride, which is suitable for the protective layer of the light-receiving surface, can be expected to have a field effect due to its high positive fixed charge density, but on the other hand, the dangling bond termination ability is generally not high. Therefore, the problem is that the field effect can be used to obtain a sufficient protective effect on a substrate with a high resistivity, but the protective effect is significantly reduced on a low-resistance substrate where a higher output voltage can be expected.
[0018] In addition, in the formation of silicon oxide film, generally speaking, heat treatment at 700℃ to 1100℃ is necessary, so there is a problem that the added impurities in the high-concentration diffusion layer are diffused again, or redistributed due to segregation to the thermal oxide film, which reduces the characteristics of the solar cell. On the other hand, there is also a method of forming a silicon oxide film by immersing the substrate in a nitric acid solution at room temperature and exposing it to an ozone atmosphere at about 200℃ to 450℃, but there is a problem that the protection effect is not sufficient and the quality is unstable.
[0019] Therefore, when a silicon oxide protective layer is applied, as can be seen in the solar cell described in Non-Patent Document 1, a method has been adopted to improve the performance of the solar cell by further forming a surface electric field layer (FSF: Front Surface Field) toward the light-receiving side to impart a field effect to the light-receiving surface.
[0020] However, in order to suppress the loss of long-wavelength light due to free carrier absorption, FSF is formed by thermally diffusing boron or phosphorus so that the impurity concentration is one to two digits lower than that of the high-concentration layer formed on the back side. Therefore, it is necessary to add a FSF formation step, which increases the manufacturing cost of the solar cell.
[0021] The present invention is made in view of the above problems, and aims to provide a solar cell with high photoelectric conversion efficiency and low cost. In addition, the present invention aims to provide a method for manufacturing a solar cell with high photoelectric conversion efficiency, which is simple to manufacture and has high protection effect.
[0022] Provide a means to solve the problem
[0023] In order to achieve the above object, the present invention provides a solar cell, wherein a p-type region having a p-type conductivity and an n-type conductivity region having an impurity added to impart n-type conductivity are arranged on a first main surface of a crystalline silicon substrate, and the maximum concentration in the depth direction of the substrate is 5×10 18 atoms / cm 3The above n-type region is configured with a first protective film in a manner covering the aforementioned p-type region and the aforementioned n-type region, and a second protective film is configured on the surface on the opposite side of the aforementioned first main surface, i.e., the second main surface, in a manner covering the second main surface. The back electrode type solar cell is characterized in that the aforementioned first protective film and the aforementioned second protective film are solar cells composed of compounds containing aluminum oxide.
[0024] In this way, since the first and second protective films are composed of a compound containing aluminum oxide, the protective effect is improved on both the first and second main surfaces, so a solar cell with high photoelectric conversion efficiency can be made. In addition, a cheap solar cell can be made due to its simple manufacture.
[0025] At this time, at least a portion of the second main surface preferably has the same conductivity type and conductivity as those of the bulk of the crystalline silicon substrate.
[0026] If at least a portion of the second main surface has the same conductivity type and conductivity as the bulk of the substrate, there is no need to provide a diffusion layer on the second main surface, and a simple and inexpensive solar cell can be made.
[0027] Furthermore, it is preferable to further arrange an antireflection film on the second protective film.
[0028] In this manner, by disposing an antireflection film on the second protective film, reflection on the light-receiving surface can be suppressed, and a solar cell with higher photoelectric conversion efficiency can be produced.
[0029] Furthermore, it is preferable to further arrange a reflective film on the first protective film.
[0030] By disposing the reflective film on the first protective film in this manner, it is possible to produce a solar cell in which the reflection on the back surface is promoted and the photoelectric conversion efficiency is higher.
[0031] Furthermore, the antireflection film and the reflective film preferably include at least any one of silicon oxide, magnesium fluoride, silicon nitride, tin oxide, and titanium oxide.
[0032] In this way, if the reflective film and anti-reflective film contain at least any one of silicon oxide, magnesium fluoride, silicon nitride, tin oxide, and titanium oxide, it is suitable as a reflective film and anti-reflective film for a back electrode type solar cell, and a solar cell with better characteristics can be made.
[0033] Furthermore, it is preferable that an area occupied by the p-type region of the first main surface is larger than an area occupied by the n-type region.
[0034] Since the protective effect of aluminum oxide is greater for the p-type region than for the n-type region, a solar cell with higher photoelectric conversion efficiency can be produced if the p-type region occupies a larger area.
[0035] Furthermore, the present invention provides a solar cell module, characterized in that the solar cells described above are electrically connected to form the solar cell module.
[0036] In this manner, the solar cells of the present invention can be electrically connected to form a solar cell module.
[0037] Furthermore, the present invention provides a solar cell power generation system, characterized in that the solar cell power generation system is formed by electrically connecting a plurality of the above-mentioned solar cell modules.
[0038] In this manner, a plurality of solar cell modules electrically connected to the solar cells of the present invention can be electrically connected to form a solar cell power generation system.
[0039] In order to achieve the above object, the present invention provides a method for manufacturing a solar cell, comprising: forming a p-type region having a p-type conductivity on a first main surface of a crystalline silicon substrate, forming an n-type conductivity region having an n-type conductivity and an impurity added to impart the n-type conductivity with a maximum concentration of 5×10 18 atoms / cm 3 The method for manufacturing a back electrode type solar cell comprises the steps of forming the above n-type region, forming a first protective film in a manner covering the above-mentioned p-type region and the above-mentioned n-type region, forming a second protective film on the surface on the opposite side of the above-mentioned first main surface, i.e., the second main surface, in a manner covering the second main surface, forming a positive electrode connected to the surface of the above-mentioned p-type region, and forming a negative electrode connected to the surface of the above-mentioned n-type region, and is characterized in that the above-mentioned first protective film and the above-mentioned second protective film are formed using a compound containing aluminum oxide.
[0040] In this way, by forming the first protective film and the second protective film using a compound containing aluminum oxide, the protective effect is improved on both the first and second main surfaces, so that a solar cell with high photoelectric conversion efficiency can be manufactured. In addition, since the manufacturing steps are simple, the productivity is high and a cheap solar cell can be manufactured.
[0041] In this case, it is preferable to include a step of further forming an anti-reflection film on the second protective film.
[0042] By forming the antireflection film on the second protective film in this manner, it is possible to manufacture a solar cell in which reflection on the light-receiving surface is suppressed and the photoelectric conversion efficiency is higher.
[0043] Furthermore, it is preferable to include a step of further forming a reflective film on the first protective film.
[0044] By forming the reflective film on the first protective film in this manner, it is possible to manufacture a solar cell in which reflection on the back surface is promoted and the photoelectric conversion efficiency is higher.
[0045] In addition, the step of forming the aforementioned positive electrode and the step of forming the aforementioned negative electrode preferably include: a sub-step of coating a conductive paste on the aforementioned first protective film or the aforementioned reflective film, and a sub-step of heat-treating the aforementioned crystalline silicon substrate coated with the aforementioned conductive paste at a temperature of not less than 700°C and not more than 890°C for not less than 1 second and not more than 10 minutes.
[0046] If the positive electrode and the negative electrode are formed in this way, the electrodes can be formed simply, the productivity can be improved, and inexpensive solar cells can be manufactured.
[0047] Effects of the Invention
[0048] The solar cell of the present invention can be made into a cheap solar cell with high photoelectric conversion efficiency. In addition, the manufacturing method of the solar cell of the present invention can improve the protective effect of the protective film and can be manufactured simply, thereby making it possible to manufacture a solar cell with high photoelectric conversion efficiency cheaply. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 It is a schematic cross-sectional view showing an embodiment of a back electrode type solar cell according to the present invention.
[0050] Figure 2 It is a schematic cross-sectional view showing another embodiment of the back electrode type solar cell of the present invention.
[0051] Figure 3 It is a schematic cross-sectional view showing still another embodiment of the back electrode type solar cell of the present invention.
[0052] Figure 4 It is a schematic cross-sectional view showing still another embodiment of the back electrode type solar cell of the present invention.
[0053] Figure 5 This is a flowchart showing an example of a method for manufacturing a back electrode type solar cell according to the present invention.
[0054] Figure 6 FIG. 1 is a diagram showing an example of the concentration distribution of impurities in the depth direction of the substrate.
[0055] Figure 7 This is a schematic diagram showing the back surface structure of a back electrode type solar cell according to the present invention.
[0056] Figure 8 This is a schematic diagram showing an example of a solar cell module according to the present invention.
[0057] Fig. 9 This is a schematic diagram of a solar cell power generation system according to the present invention.
[0058] Fig.10 This is a schematic cross-sectional view of a general back electrode type solar cell. DETAILED DESCRIPTION
[0059] As described above, in recent years, it has become a problem to easily obtain a high protection effect in the manufacture of a back electrode type solar cell. The present inventors have made intensive studies on a measure for obtaining such a high protection effect and have completed the present invention.
[0060] Hereinafter, the present invention will be described in detail with reference to the drawings, but the present invention is not limited thereto.
[0061] Below, use Figure 1 The solar cell of the present invention is specifically described. The solar cell of the present invention has a p-type region 102 having a p-type conductivity type and an n-type conductivity type and an impurity additive having a maximum concentration of 5×10 18 atoms / cm 3 The back electrode type solar cell 100 is characterized in that the first protective film 104 is arranged on the n-type region 103 so as to cover the p-type region 102 and the n-type region 103, and the second protective film 105 is arranged on the surface on the opposite side of the first main surface, i.e., the second main surface, so as to cover the second main surface, wherein the first protective film 104 and the second protective film 105 are protective films composed of a compound containing aluminum oxide. In addition, a positive electrode 106 and a negative electrode 107 are arranged on the p-type region 102 and the n-type region 103, respectively.
[0062] In this way, since the first protective film 104 and the second protective film 105 are composed of a compound containing aluminum oxide, the protective effect is improved on both the first and second main surfaces, so a solar cell with high photoelectric conversion efficiency can be made. In addition, a cheap solar cell can be made due to the simplicity of manufacturing.
[0063] At this time, at least a portion of the second main surface preferably has the same conductivity type and conductivity as the bulk of the crystalline silicon substrate 101. If at least a portion of the second main surface has the same conductivity type and conductivity as the bulk of the substrate in this way, it is not necessary to provide a diffusion layer (FSF layer, etc.) on the second main surface, and a solar cell with a simple structure and low cost can be produced.
[0064] Reference Figure 2 to Figure 4 , illustrating a further aspect of the present invention. Figure 2 to Figure 4 ,and Figure 1 The same components of the solar cell are denoted by the same reference numerals.
[0065] like Figure 2 As shown, the solar cell 200 of the present invention is preferably provided with an anti-reflection film 108 on the second protective film 105. In this way, by providing the anti-reflection film 108 on the second protective film 105, reflection on the light receiving surface can be suppressed and a solar cell with higher photoelectric conversion efficiency can be produced.
[0066] In addition, if Figure 3 As shown, the solar cell 300 of the present invention is preferably provided with a reflective film 109 on the first protective film 104. By providing the reflective film 109 on the first protective film 104, a solar cell with enhanced back reflection and higher photoelectric conversion efficiency can be produced.
[0067] In addition, if Figure 4 As shown, the solar cell 400 of the present invention may be configured such that the anti-reflection film 108 is disposed on the second protective film 105, and the reflective film 109 is disposed on the first protective film 104. By configuring in this way, a solar cell with higher photoelectric conversion efficiency can be obtained.
[0068] In addition, the anti-reflection film 108 and the reflective film 109 preferably contain at least any one of silicon oxide, magnesium fluoride, silicon nitride, tin oxide, and titanium oxide. If it is such a reflective film and anti-reflection film, it is suitable as a reflective film and anti-reflection film of a back electrode type solar cell, and a solar cell with better characteristics can be made.
[0069] In addition, Figure 1 to Figure 4 In any form of solar cell, it is also preferable that the area occupied by the p-type region 102 of the first main surface is larger than the area occupied by the n-type region 103. Since the protective effect formed by aluminum oxide is greater for the p-type region than for the n-type region, if the area occupied by the p-type region is larger, a solar cell with higher photoelectric conversion efficiency can be made.
[0070] Next, the manufacturing method of the solar cell of the present invention is described. The manufacturing method of the solar cell of the present invention comprises: a step of forming a p-type region having a p-type conductivity on the first main surface of the crystalline silicon substrate, a step of forming an n-type region having an n-type conductivity on the first main surface, a step of forming a first protective film in a manner covering the p-type region and the n-type region, a step of forming a second protective film in a manner covering the second main surface on the surface opposite to the first main surface, a step of forming a positive electrode connected to the surface of the p-type region, and a step of forming a negative electrode connected to the surface of the n-type region. The manufacturing method of the back electrode type solar cell is characterized in that the first protective film and the second protective film are formed using a compound containing aluminum oxide.
[0071] Below, refer to Figure 5 , illustrating the solar cell ( Figure 1 The present invention is an example of a manufacturing method of the present invention, but the present invention is not limited thereto.
[0072] Figure 5 The substrate 101 of (a) is, for example, crystalline silicon having a p-type or n-type conductivity with a resistivity of 0.1 to 10 Ω·cm. Although not shown in the figure, it is preferable to form a concave-convex structure (texture) on the surface of the substrate to confine light. The concave-convex structure can be obtained by immersing the substrate 101 in an acidic or alkaline solution for a certain period of time. The acidic solution generally uses a mixed acid solution of fluoronitric acid and acetic acid, phosphoric acid, sulfuric acid, water, etc. When the substrate 101 is immersed in the solution, the fine grooves on the surface of the cracks during substrate processing are preferentially etched, etc., to form a concave-convex structure. In addition, an alkaline solution uses an aqueous solution of potassium hydroxide or sodium hydroxide, or an aqueous solution of tetramethylammonium hydroxide. Alkaline etching etches by forming a Si-OH bond, so the etching rate depends on the orientation of the crystal surface, and a concave-convex structure is obtained in which the surface with a slow etching rate is exposed.
[0073] The non-light-receiving surface of the substrate 101 does not necessarily require a concavo-convex structure. Rather, the effect of reducing the carrier recombination loss can be expected by reducing the surface area through flattening. In this case, a spin etching process using a chemical solution containing fluorine nitric acid or an in-line type single-side cleaning machine can be used.
[0074] After the concavoconvex structure is formed, it is best to clean it in an acidic aqueous solution of hydrochloric acid, sulfuric acid, nitric acid, fluoric acid, etc., or a mixture of these. From the perspective of cost and characteristics, cleaning in hydrochloric acid is preferred. In order to improve the cleanliness, 0.5-5% hydrogen peroxide can be mixed in the hydrochloric acid solution and heated to 60-90°C for cleaning.
[0075] Secondly, if Figure 5As shown in (b), a p-type region 102 is formed on one side (first main surface) of the substrate 101. A diffusion source containing a group III element can be used to form the p-type region, but in terms of electrical properties and simplicity of the device, it is preferred to use, for example, boron bromide and perform vapor phase diffusion at 900-1000°C. The solar cell of the present invention must form the p-type region only on the back side. To achieve this, it is best to perform diffusion while the two substrates are stacked together, or to form a diffusion barrier such as silicon nitride on the light-receiving side so that boron does not diffuse to the light-receiving surface. In addition to vapor phase diffusion, the p-type region 102 can also be formed by applying a boron compound to the substrate 101 and drying it, and then performing thermal diffusion at 900-1000°C. According to this method, it is relatively easy to suppress the diffusion of boron to the non-coated surface.
[0076] The concentration of the added impurities in the p-type region 102 is set to 5×10 18 atoms / cm 3 Above 5×10 20 atoms / cm 3 The following is preferred, and it is better to set it at 8×10 18 atoms / cm 3 Above 5×10 19 atoms / cm 3 When less than 5×10 18 atoms / cm 3 When the contact resistance between the substrate 101 and the electrode increases, when it exceeds 5×10 20 atoms / cm 3 When the charge carriers are recombinated due to defects in the p+ region and Auger recombination, the output of the solar cell decreases.
[0077] Secondly, if Figure 5 As shown in (c), a diffusion barrier 510 is formed on the p-type region 102. Here, a silicon nitride film or a silicon oxide film obtained by chemical vapor deposition or physical evaporation can be appropriately used. Although it also varies depending on the film manufacturing method, it is best to form a film with a thickness of approximately 50 to 400 nm. In addition to these, a silicon oxide film obtained by heat treatment can also be used. In this case, the substrate 101 is heat-treated in an oxygen or water vapor atmosphere at 700 to 1100°C to grow silicon oxide by 20 to 200 nm.
[0078] Then, if Figure 5As shown in (d), the diffusion barrier 510 where the n-type region is formed is partially removed to form an opening 511, exposing the p-type region 102. The diffusion barrier 510 can be removed by, for example, screen printing an etching paste at a designated location and performing a heat treatment at 100 to 400° C. Alternatively, laser ablation, which has a simpler procedure, can be used.
[0079] In addition, the opening area at this time seeks the most suitable design according to the different conductivity types of the substrate 101, and generally the area of the high concentration layer that becomes the emitter is proportional to the solar cell characteristics. The aluminum oxide used in the present invention can also be applied to the n-type region, but it is more effective for the p-type region. In terms of this property, the present invention can expect a higher effect in the back electrode type solar cell using an n-type substrate.
[0080] Secondly, if Figure 5 As shown in (e), an n-type region 103 is formed in the opening 511 of the diffusion barrier. In this way, an n-type region having n-type conductivity is formed on the first main surface of the substrate 101. The n-type region 103 can be formed if the diffusion source contains a V group element, but in terms of electrical characteristics and simplicity of the device, it is preferred to use, for example, phosphorus oxychloride and perform gas phase diffusion at 800-980°C. The solar cell of the present invention must form the n-type region 103 only on the back side (first main surface). To achieve this, it is best to perform diffusion in a state where two substrates are stacked together, or to form a diffusion barrier such as silicon nitride on the light-receiving surface (not shown) to prevent phosphorus from diffusing to the light-receiving surface. In addition to gas phase diffusion, the n-type region 103 can also be formed by applying a phosphorus compound to the substrate and drying it, and then performing thermal diffusion at 800-980°C. According to this method, it is relatively easy to suppress the diffusion of phosphorus to the non-coated surface.
[0081] Phosphorus diffusion may be performed after etching away the p-type region 102 exposed in the opening 511 of the diffusion barrier (e.g., oxide film) in addition to the above method. In this case, by immersing the substrate 101 in, for example, an aqueous sodium hydroxide solution or an aqueous potassium hydroxide solution, the oxide film formed on the surface acts as a shield, and only the exposed portion of the p-type region 102 can be removed.
[0082] The impurity concentration of the n-type region 103 is preferably set to 5×10 18 atoms / cm 3 above.
[0083] The protection ability formed by the field effect is determined by the fixed charge density of aluminum oxide and the carrier density on the substrate surface.18 atoms / cm 3 When the surface of the n-type region has a negative fixed charge, the positive holes of the minority carriers will gather on the surface and tend to be inverted. This will reduce the carrier recombination ratio on the surface of the n-type region. However, on the other hand, the minority carriers that recombine with the electrode will increase, resulting in a decrease in the characteristics of the solar cell. 18 atoms / cm 3 Although the field effect is reduced in the above region, the protective effect is maintained due to the high chemical termination ability of aluminum oxide on the surface of crystalline silicon. This effect is believed to be due to the formation of a silicon oxide film of several atomic layers at the interface between silicon and aluminum oxide when aluminum oxide is formed.
[0084] On the other hand, when the concentration of impurities exceeds 1×10 21 atoms / cm 3 When the impurity concentration is 1×10 21 atoms / cm 3 the following.
[0085] The impurity concentrations of the p-type region 102 and the n-type region 103 can be easily measured by secondary ion mass spectrometry. Figure 6 The boron concentration distribution measured by this method ( Figure 6 (a)) and phosphorus concentration distribution ( Figure 6 The concentration distribution has different shapes depending on the added impurities or diffusion conditions, and the value indicated by the arrow in the figure is the maximum concentration of the added impurities in the depth direction of the substrate.
[0086] The formation pattern of the p-type region and the n-type region may also be, for example, Figure 7 (a) shows a form in which the p-type region 102 and the n-type region 103 are adjacent to each other in a straight line. Figure 7 (b) shows a form in which an island-shaped n-type region 703 is formed in a p-type region 702, or as shown in Figure 7 (c) shows a form in which an island-shaped p-type region 712 is formed in an n-type region 713.
[0087] Furthermore, the order of the step of forming the p-type region and the step of forming the n-type region may be reversed.
[0088] After phosphorus diffusion, the boron glass, diffusion barrier, and phosphorus glass formed on the diffusion surface are removed with fluoric acid or the like. In order to keep the surface of the substrate 101 clean, it is better to mix ammonia water or tetramethylammonium hydroxide aqueous solution with 0.5-5% hydrogen peroxide, and heat it to 60-90°C for cleaning. In addition, hydrochloric acid, sulfuric acid, nitric acid, or a mixture thereof, or a mixture thereof with 0.5-5% hydrogen peroxide, and heat it to 60-90°C for cleaning. In addition, it is best to remove the oxide film on the surface of the substrate with fluoric acid aqueous solution at the last stage of cleaning.
[0089] Secondly, if Figure 5 As shown in (f), a first protective film 104 is formed on the p-type region 102 and the n-type region 103, and further, a second protective film 105 is formed on the opposite surface (the second main surface). Any protective film is a film formed by a compound containing aluminum oxide. In the film formation method of aluminum oxide, in addition to the atomic layer deposition method, chemical vapor deposition methods such as plasma CVD, atmospheric pressure CVD, or reduced pressure CVD are mainly used. In these methods, tetramethylaluminum is used as a precursor. In addition, hydrogen, argon or nitrogen is generally used when a carrier gas is introduced into the precursor. As an oxidant for aluminum, oxygen, carbon dioxide, nitrous oxide, water or ozone can be used.
[0090] Furthermore, the protective film made of aluminum oxide may be formed by vacuum deposition or sputtering, or by a sol-gel method using a compound such as aluminum alkoxide.
[0091] The first protective film 104 and the second protective film 105 may be formed on both sides at the same time, or may be formed on one side or the other. In the case of forming them at the same time, the atomic layer deposition method is applicable. In this case, the substrate 101 is placed in a reaction chamber maintained at about 100 to 350° C. so that both sides are exposed to the reaction gas, and the oxidizing gas and the precursor are alternately introduced thereto and the gas is replaced, thereby forming an aluminum oxide film.
[0092] It is also possible to change the composition of the first protective film 104 and the second protective film 105. In such a single-piece film formation, conventional flat-plate plasma CVD, sputtering, sol-gel method, etc. are applicable.
[0093] The thickness of the first protective film 104 and the second protective film 105 is greater than 0.5 nm, preferably 3 nm to 30 nm. By making the thickness of the first and second protective films within this thickness range, the coverage and protection effect of the protective film on the substrate 101 can be obtained simultaneously.
[0094] In addition, when the first protective film 104 is used as a reflective film for reflecting the light reaching the back of the solar cell back into the substrate, the film thickness is preferably 70 nm to 200 nm, more preferably 80 nm to 100 nm. If the film thickness is 70 nm to 200 nm, the reflective film can be used appropriately.
[0095] In order to improve the light reflection from the back of the substrate, Figure 3 As shown in the figure, a reflective film 109 composed of a compound other than aluminum oxide is further formed on the first protective film 104. Silicon oxide, magnesium fluoride, silicon nitride, tin oxide, titanium oxide, etc. can be used for the reflective film 109. Such films can be formed by chemical vapor deposition, sputtering, vacuum evaporation, etc. The film thickness of the reflective film 109 will also vary depending on the film thickness of the first protective film 104 or the refractive index of the reflective film 109, but can be made to be approximately 80 to 250 nm.
[0096] On the other hand, when the second protective film 105 also functions as an anti-reflection film, the film thickness is preferably 70 nm to 200 nm, more preferably 80 nm to 150 nm. If the film thickness of the second protective film 105 is 70 nm to 200 nm, it can function appropriately as a reflection film.
[0097] In addition, in order to improve the reflection prevention effect of the light receiving surface, it is also possible to Figure 2 As shown in the figure, an anti-reflection film 108 made of a compound other than aluminum oxide is further formed on the second protective film 105. Silicon oxide, magnesium fluoride, silicon nitride, tin oxide, titanium oxide, etc. can be used for the anti-reflection film 108. Such films can be formed by chemical vapor deposition, sputtering, vacuum evaporation, etc. The film thickness of the anti-reflection film 108 will also vary depending on the film thickness of the second protective film 105 or the refractive index of the anti-reflection film, but can be made to be approximately 50 to 120 nm.
[0098] In addition, if Figure 4 As shown, it is also possible to merge Figure 2 and Figure 3 The characteristics of the solar cell are formed by forming a laminate of a protective film 104 and a reflective film 109 on the back side, and a laminate of a protective film 105 and an anti-reflection film 108 on the light-receiving side.
[0099] The aluminum oxide film varies depending on the manufacturing method, but it is known that the protective effect can be improved by applying a heat treatment at 300 to 600° C. In the case where the film forming temperature is lower than the above temperature range, it is preferable to perform a heat treatment for 5 to 20 minutes in an inert gas atmosphere in the above temperature range or a hydrogen-mixed nitrogen atmosphere with a hydrogen concentration of 2 to 10% after the aluminum oxide film is formed and before the reflection film or anti-reflection film is laminated.
[0100] Secondly, if Figure 5 As shown in (g), a positive electrode 106 is formed on the p-type region 102, and a negative electrode 107 is formed on the n-type region 103. The step of forming the positive electrode 106 and the step of forming the negative electrode 107 preferably include a sub-step of applying a conductive paste on the first protective film 104 or the reflective film 109, and a sub-step of heat-treating the crystalline silicon substrate 101 coated with the conductive paste at a temperature of 700° C. to 890° C. for 1 second to 10 minutes. Here, there is no particular limitation on the method of forming the electrodes, but from the viewpoint of productivity, it is preferred to form the electrodes by screen printing or dispenser of the conductive paste. Specifically, the positive electrode 106 and the negative electrode 107 are formed by applying a silver paste of a mixture of silver powder, glass frit and an organic binder to the p-type region 102 and the n-type region 103 via the protective film 104, drying the mixture, and then firing the mixture for a period of 1 second to 30 minutes, preferably 1 second to 10 minutes, at a temperature of about 700° C. to 890° C. The protective film 104 or the protective film 104 and the reflective film are eroded by the silver paste by the heat treatment, and the electrodes are in electrical contact with silicon.
[0101] Electroplating may also be applied to the formation of electrodes. In this case, since it is necessary to expose the substrate surface where the electrodes are to be formed, the protective film 104 at that location may be removed by, for example, laser ablation.
[0102] A solar cell module can be obtained by electrically connecting a plurality of the solar cells of the present invention described above. Figure 8 This is an overview diagram showing an example of the structure of the non-light-receiving surface of a solar cell module 16 formed by electrically connecting the solar cells of the present invention. The positive electrode 26 of the solar cell is electrically connected to the negative electrode 27 of the adjacent solar cell using the ear piece 12, and the number of solar cells 11 required for the specified output is connected. The connected solar cells 11 are not shown in the figure, and are sealed using cover glass and a filler, and then a backplane. Soda-lime glass is widely used as the cover glass. In addition, ethylene vinyl acetate, polyolefin, or polysilicone is used as the filler. For the backplane, a functional film using polyethylene terephthalate is generally used. In addition, the positive electrode 26 of one solar cell is connected to the positive terminal 13 of the solar cell module 16, and the negative electrode 27 of another solar cell is connected to the negative terminal 14 of the solar cell module 16.
[0103] Fig. 9 1 is a diagram showing the basic structure of a solar cell power generation system that connects the solar cell modules 16 of the present invention. The solar cell power generation system of the present invention is a solar cell power generation system that electrically connects a plurality of the solar cell modules 16 of the present invention. Fig. 9As shown, a plurality of solar cell modules 16 are connected in series by wiring 15, and supply generated power to an external load circuit 18 via an inverter 17. Although not shown in the figure, the system may further include a secondary battery for storing the generated power.
[0104] Example
[0105] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited thereto.
[0106] (Example 1)
[0107] A phosphorus-doped <100> n-type as-cut silicon substrate with a square size of 150 mm, a thickness of 200 μm and a resistivity of 1 Ω·cm was immersed in a 5% potassium hydroxide aqueous solution at 80°C for 20 minutes to form a random conical texture, and then cleaned in a hydrochloric acid / hydrogen peroxide mixed solution after the damaged layer was removed using a hot concentrated potassium hydroxide aqueous solution.
[0108] Next, a mixture of a boron compound and a binder is spin-coated on the back of the substrate, and a heat treatment is performed at 1000°C for 30 minutes to diffuse the boron and form a p-type region. After that, an oxidation heat treatment is performed at 1000°C for 2 hours to form an oxide film (silicon oxide film). After the oxide film is formed, the oxide film at the location where the n-type region on the back of the substrate is formed is removed linearly by irradiation with a laser of a wavelength of 532nm.
[0109] Next, two substrates were placed in a quartz boat facing the light-receiving surface and heat-treated with phosphorus oxychloride at 820°C for 30 minutes to form an n-type region. After this step, the peak impurity concentrations in the substrate depth direction of the p-type region and the n-type region were measured by secondary ion mass spectrometry for samples randomly extracted. The p-type region was 5×10 19 atoms / cm 3 , n-type region is 3×10 19 atoms / cm 3 .
[0110] The substrate was immersed in a 10% HF aqueous solution to remove the glass layer and the oxide film, and then immersed in a mixed solution of 80° C. hydrochloric acid water and hydrogen peroxide water and a 2% HF aqueous solution in this order to be cleaned, and then washed with pure water and dried.
[0111] Aluminum oxide with a thickness of 100 nm was formed on the light-receiving surface of the cleaned substrate by atomic layer deposition, and aluminum oxide with a thickness of 10 nm was formed on the back side. After that, the substrate was heat treated at 450°C in a nitrogen atmosphere for 15 minutes. On the back side of the substrate, a silicon nitride film with a thickness of 90 nm was formed by plasma CVD.
[0112] Silver paste was applied to the p-type region and n-type region by screen printing, and then hardened by heat treatment at 800°C for 3 seconds to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0113] (Example 2)
[0114] On the back side of the substrate where the p-type region and the n-type region were formed in Example 1, aluminum oxide with a thickness of 100 nm was formed by atomic layer deposition, and aluminum oxide with a thickness of 10 nm was formed on the light-receiving surface. After that, the substrate was heat-treated at 450° C. in a nitrogen atmosphere for 15 minutes. On the light-receiving surface of the substrate, a silicon nitride film with a thickness of 90 nm was further formed by plasma CVD.
[0115] Silver paste was applied to the p-type region and n-type region by screen printing, and then hardened by heat treatment at 800°C for 3 seconds to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0116] (Example 3)
[0117] Aluminum oxide with a thickness of 10 nm was formed on both sides of the substrate on which the p-type region and the n-type region were formed in Example 1 by atomic layer deposition, and then the substrate was heat treated at 450° C. in a nitrogen atmosphere for 15 minutes. A silicon nitride film with a thickness of 90 nm was further formed on both sides of the substrate by plasma CVD.
[0118] Silver paste was applied to the p-type region and n-type region by screen printing, and then hardened by heat treatment at 800°C for 3 seconds to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0119] (Example 4)
[0120] A solar cell similar to Example 1 was prepared using a boron-doped <100> p-type as-cut silicon substrate of 150 mm square, 200 μm thick, and 1 Ω·cm specific resistance. Then, the output characteristics of the solar cell were measured using simulated sunlight of a xenon lamp light source.
[0121] (Example 5)
[0122] A phosphorus-doped <100> n-type as-cut silicon substrate with a square size of 150 mm, a thickness of 200 μm and a resistivity of 1 Ω·cm was immersed in a 5% potassium hydroxide aqueous solution at 80°C for 20 minutes to form a random conical texture, after the damaged layer was removed using a hot concentrated potassium hydroxide aqueous solution, and then cleaned in a hydrochloric acid / hydrogen peroxide mixed solution.
[0123] Next, a mixture of a boric acid compound and a binder is spin-coated on the back of the substrate, and a heat treatment is performed at 1000°C for 30 minutes to diffuse boron and form a p-type region. After that, an oxidation heat treatment is performed at 1000°C for 2 hours to form an oxide film. After the oxide film is formed, the oxide film at the location where the n-type region on the back of the substrate is formed is removed in an island shape by irradiation with a laser of a wavelength of 532nm. In addition, the area occupied by the n-type region at this time is reduced by 25% compared to Example 1.
[0124] Next, two substrates were placed in a quartz boat facing the light-receiving surface and heat-treated with phosphorus oxychloride at 820°C for 30 minutes to form an n-type region. After this step, the peak impurity concentrations in the substrate depth direction of the p-type region and the n-type region were measured by secondary ion mass spectrometry for samples randomly extracted. The p-type region was 5×10 19 atoms / cm 3 , n-type region is 3×10 19 atoms / cm 3 .
[0125] The substrate was immersed in a 10% HF aqueous solution to remove the glass layer and the oxide film, and then immersed in a mixed solution of 80° C. hydrochloric acid water and hydrogen peroxide water and a 2% HF aqueous solution in this order to be cleaned, and then washed with pure water and dried.
[0126] Aluminum oxide was deposited on both sides of the substrate by atomic layer deposition to a thickness of 10 nm, and then the substrate was heat treated at 450° C. in a nitrogen atmosphere for 15 minutes. Silicon nitride was further deposited on both sides of the substrate by plasma CVD to a thickness of 90 nm.
[0127] Silver paste was applied to the p-type region and n-type region by screen printing, and then heat treated at 800°C for 3 seconds to harden the silver paste to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0128] (Comparative Example 1)
[0129] On the back side of the substrate where the p-type region and the n-type region are formed in Example 1, an aluminum oxide film with a thickness of 10 nm is formed by atomic layer deposition. Next, the p-type region is covered with an acid registant by screen printing and dried, and then the aluminum oxide on the exposed n-type region is removed with a 2% fluoric acid aqueous solution. After the acid registant is removed and the substrate is cleaned, the substrate is heat treated at 450°C in a nitrogen atmosphere for 15 minutes. On both sides of the substrate, a silicon nitride film with a thickness of 90 nm is further formed by plasma CVD.
[0130] Silver paste was applied to the p-type region and n-type region by screen printing, and then heat treated at 800°C for 3 seconds to harden the silver paste to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0131] (Comparative Example 2)
[0132] A phosphorus diffusion source of a mixed phosphorus compound and a binder was coated on the light-receiving surface of the substrate on which the p-type region and the n-type region were formed in Example 1, and a heat treatment was performed at 820°C for 10 minutes with the coated surface facing each other to form a FSF layer on the light-receiving surface. Next, the substrate was immersed in a 10% HF aqueous solution to remove the glass layer, and then immersed in a mixed solution of 80°C hydrochloric acid water and hydrogen peroxide water and a 2% HF aqueous solution in sequence to be cleaned, and then washed with pure water and dried.
[0133] After that, an aluminum oxide film with a thickness of 10 nm was formed on both sides of the substrate by atomic layer deposition. Next, the p-type region was covered with an acid registant by screen printing and dried, and then the aluminum oxide on the exposed n-type region was removed with a 2% fluoric acid aqueous solution. After the acid registant was removed and the substrate was cleaned, the substrate was heat treated at 450°C in a nitrogen atmosphere for 15 minutes. On both sides of the substrate, a silicon nitride film with a thickness of 90 nm was formed by plasma CVD.
[0134] Silver paste was applied to the p-type region and n-type region by screen printing, and then heat treated at 800°C for 3 seconds to harden the silver paste to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0135] (Comparative Example 3)
[0136] A phosphorus diffusion source of a mixed phosphorus compound and a binder was coated on the light-receiving surface of the substrate on which the p-type region and the n-type region were formed in Example 1, and a heat treatment was performed at 820°C for 10 minutes with the coated surface facing each other to form a FSF layer on the light-receiving surface. Next, the substrate was immersed in a 10% HF aqueous solution to remove the glass layer, and then immersed in a mixed solution of 80°C hydrochloric acid water and hydrogen peroxide water and a 2% HF aqueous solution in sequence to be cleaned, and then washed with pure water and dried.
[0137] Then, the substrate was heat treated at 900° C. in an oxygen atmosphere for 10 minutes to form a silicon oxide film (thickness of about 10 nm) on both sides of the substrate. A silicon nitride film with a thickness of 90 nm was further formed on both sides of the substrate by plasma CVD.
[0138] Silver paste was applied to the p-type region and n-type region by screen printing, and then heat treated at 800°C for 3 seconds to harden the silver paste to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0139] (Comparative Example 4)
[0140] The solar cell was produced in the same manner as in Example 3, and the phosphorus diffusion conditions were adjusted so that the peak impurity concentration in the depth direction of the substrate in the n-type region was set to 3×10 18 atoms / cm 3 Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0141] (Comparative Example 5)
[0142] In Example 4, aluminum oxide with a thickness of 10 nm was formed on the light-receiving surface of the substrate where the p-type region and the n-type region were formed by atomic layer deposition, and the substrate was heat treated at 450° C. in a nitrogen atmosphere for 15 minutes. A silicon nitride film with a thickness of 90 nm was further formed on both sides of the substrate by plasma CVD.
[0143] Silver paste was applied to the p-type region and n-type region by screen printing, and then heat treated at 800°C for 3 seconds to harden the silver paste to obtain a solar cell. Finally, the output characteristics of the solar cell were measured using simulated sunlight using a xenon lamp as a light source.
[0144] The characteristics of the solar cells of the above-mentioned Examples 1 to 5 and Comparative Examples 1 to 5 are summarized and shown in the following Table 1. In Table 1, Jsc is the short-circuit current, Voc is the open voltage, FF is the curve element, and Eff. is the conversion efficiency. The conversion efficiency of the solar cells according to the present invention is all above 22.0%, showing a higher conversion efficiency than the comparative examples. In addition, the results of Example 5 show that the present invention is particularly effective in a solar cell structure in which the p-type region occupies a larger area.
[0145] Table 1
[0146] <![CDATA[Jsc[mA / cm 2 ]]]> Voc[mV] FF Eff.[%] Example 1 39.7 0.688 0.805 22.0 Example 2 40.3 0.689 0.802 22.3 Example 3 40.8 0.688 0.803 22.5 Example 4 40.8 0.688 0.805 22.6 Example 5 41.1 0.692 0.800 22.8 Comparative Example 1 38.8 0.682 0.805 21.3 Comparative Example 2 39.5 0.682 0.807 21.7 Comparative Example 3 38.5 0.686 0.803 21.2 Comparative Example 4 39.6 0.653 0.794 20.5 Comparative Example 5 39.9 0.679 0.807 21.9
[0147] Furthermore, the present invention is not limited to the above-mentioned embodiments. The above-mentioned embodiments are merely examples, and those having substantially the same structure and having the same effects as the technical concept described in the scope of the claims of the present invention are all included in the technical scope of the present invention.
Claims
1. A method for manufacturing a solar cell, It is characterized in that The method comprises: forming a p-type region having a p-type conductivity on a first main surface of a crystalline silicon substrate, wherein the p-type region is formed by vapor-diffusing boron bromide in a state where two substrates are overlapped with each other, or by applying a boron compound and then thermally diffusing the boron compound at 900 to 1000° C.; The maximum concentration in the depth direction of the substrate of the added impurity diffused into the crystalline silicon substrate and having n-type conductivity formed on the first main surface and imparting the n-type conductivity is 5×10 18 atoms / cm 3 The above steps of the n-type region, wherein the two substrates are overlapped with each other or a diffusion barrier is formed on the surface opposite to the first main surface, that is, the second main surface side, and gas phase diffusion is performed at 800 to 980° C. using phosphorus oxychloride; forming a first protective film so as to cover the p-type region and the n-type region; A step of forming a second protective film on a second main surface, which is a surface opposite to the first main surface, so as to cover the second main surface; A step of further forming a silicon nitride film as a reflective film on the first protective film; forming a positive electrode connected to the surface of the p-type region; A method for manufacturing a back electrode type solar cell having a step of forming a negative electrode connected to the surface of the aforementioned n-type region, in, The first protective film and the second protective film are aluminum oxide films, and the maximum concentration of the added impurities in the substrate depth direction of the p-type region is set to 5×10 18 atoms / cm 3 Above and 5×10 20 atoms / cm 3 the following, The steps of forming the positive electrode and the steps of forming the negative electrode include: A sub-step of coating a conductive paste on the first protective film; and a sub-step of heat-treating the crystalline silicon substrate coated with the conductive paste at a temperature of 700° C. to 890° C. for 1 second to 10 minutes. The conductive paste was made into Ag paste.
2. The method for manufacturing a solar cell according to claim 1, in, The method comprises the step of further forming an anti-reflection film on the second protective film.