A lithium ion battery negative electrode sheet and preparation method thereof and a lithium ion battery

By alternating strips of carbon-based materials with low expansion rates and strips of silicon-based materials with high expansion rates in the negative electrode sheet of lithium-ion batteries, the cracking problem caused by expansion and contraction of silicon-based negative electrode materials during charging and discharging is solved, thereby improving the energy density and cycle stability of the battery.

CN110233240BActive Publication Date: 2024-11-01SHENZHEN UTILITY ENERGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201910496355.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-06-10
Publication Date
2024-11-01
Estimated Expiration
2039-06-10

AI Technical Summary

Technical Problem

The mechanical stress caused by the expansion and contraction of existing silicon-based anode materials in lithium-ion batteries during charging and discharging leads to cracks inside the electrode, affecting electronic pathways and conductivity.

Method used

The negative electrode material layer uses alternating carbon-based and silicon-based material strips. The low expansion rate of the carbon material strips interrupts the continuous stress transmission of the high expansion rate of the silicon-based material strips, preventing crack generation and propagation, and improving electron pathways and conductivity.

Benefits of technology

It improves the energy density of lithium-ion batteries, enhances their cycle performance and rate performance, and extends their cycle life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110233240B_ABST
    Figure CN110233240B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of lithium-ion batteries, and in particular to a negative electrode sheet of a lithium-ion battery, comprising: a negative current collector and a negative electrode material layer arranged on the negative current collector, wherein the negative electrode material layer is composed of carbon material strips and silicon-based material strips alternately distributed from left to right, i.e., carbon material strips-silicon-based material strips-carbon material strips-silicon-based material strips-carbon material strips. The negative electrode sheet of a lithium-ion battery provided by the present invention not only effectively improves the energy density of the battery, but also enables the battery to have excellent capacity retention and rate performance during the cycle process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a lithium ion battery negative electrode sheet and a preparation method thereof, and a lithium ion battery. Background Art

[0002] Lithium-ion batteries are recognized as ideal chemical energy sources in today's society due to their high voltage, high energy density, long cycle life, low self-discharge, no memory effect, wide operating temperature range, and environmental friendliness. They are commonly used energy storage and conversion devices in modern life and are widely used in portable electronic devices such as mobile phones and laptops, large-scale energy storage power stations, and electric vehicles. In order to achieve high energy density, existing lithium-ion batteries increase the surface density of the positive electrode, and at the same time, the negative electrode needs to use a higher gram capacity of active materials or increase the surface density of the negative electrode. At present, the negative electrode material of lithium-ion batteries mainly uses graphite carbon negative electrode materials, which have excellent conductivity and high cycle stability, but their theoretical specific capacity is only 372mAh / g, which cannot meet the requirements of the development of lithium-ion batteries with higher specific energy and high power density in the future. With the increasing market demand for the energy density of lithium-ion batteries, finding high specific capacity negative electrode materials to replace carbon has become an important development direction.

[0003] Silicon-based negative electrode materials have a high theoretical specific capacity, with the highest theoretical specific capacity reaching 4200mAh / g. They are high-specific-capacity negative electrode materials that can replace carbon-based negative electrode materials, and they are rich in resources and are considered to be the most promising negative electrode materials for future lithium-ion batteries. However, due to the volume expansion and large volume changes of silicon negative electrode materials during the lithium insertion / extraction process, this means that the electrode needs to withstand greater mechanical stress, which comes from the stacking pressure of the electrode materials on the one hand, and the stress generated by the expansion and contraction of the electrodes during the charge and discharge process on the other hand. The expansion and contraction of the electrodes cause internal strain, which ultimately causes the separation of the active material from the foil and the active material, interrupting the electronic conduction, thereby affecting the battery cycle performance of the electrode.

[0004] Is there any practical solution to the problem that the mechanical stress caused by the expansion and contraction of the existing silicon-based negative electrode materials of lithium-ion batteries during the charge and discharge process causes cracks inside the electrode, affecting the overall electronic path and conductivity of the electrode? Summary of the invention

[0005] The purpose of the present invention is to provide a negative electrode plate for a lithium-ion battery, aiming to solve the technical problems that mechanical stress caused by expansion and contraction of silicon-based negative electrode materials of existing lithium-ion batteries during charging and discharging leads to cracks inside the electrode plate, affecting the overall electronic path and conductivity of the electrode plate.

[0006] Another object of the present invention is to provide a method for preparing a negative electrode sheet of a lithium ion battery.

[0007] Another object of the present invention is to provide a lithium ion battery.

[0008] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention is as follows:

[0009] A negative electrode sheet for a lithium-ion battery comprises a negative current collector and a negative electrode material layer arranged on the negative current collector, wherein the negative electrode material layer is composed of carbon material strips and silicon-based material strips alternately distributed from left to right.

[0010] Preferably, the thickness of the negative electrode material layer is 50 micrometers to 110 micrometers.

[0011] Preferably, the width of the silicon-based material strip is 5 cm to 10 cm.

[0012] Preferably, the width of the carbon material strip is 2 cm to 5 cm.

[0013] Preferably, the carbon-based material strip and the silicon-based material strip are in conductive contact with each other, and the contact surface between the carbon-based material strip and the silicon-based material strip is a plane or a curved surface.

[0014] Preferably, the silicon-based material strip contains silicon negative electrode active material, and the silicon negative electrode active material is selected from at least one of silicon, silicon alloy, silicon oxide, silicon-carbon composite, and silicon-carbon oxide.

[0015] Preferably, the carbon material strips contain carbon negative electrode active substances, and the carbon negative electrode active substances are selected from at least one of artificial graphite, natural graphite, carbon fiber, and carbon microspheres.

[0016] Preferably, the silicon-based material strips and the carbon-based material strips contain: a conductive agent, a binder and a thickener.

[0017] A method for preparing a negative electrode sheet of a lithium ion battery comprises the following steps:

[0018] Obtaining copper foil as a negative electrode current collector;

[0019] A silicon-based material and a carbon-based material are obtained, and the silicon-based material and the carbon-based material are deposited on the copper foil so that the copper foil forms carbon-based material strips and silicon-based material strips that are alternately distributed from left to right, and the carbon-based material strips and the silicon-based material strips are in conductive contact with each other to obtain a deposition product; the deposition product is dried and rolled to obtain a negative electrode sheet for a lithium-ion battery.

[0020] A lithium ion battery comprises: a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is the above-mentioned lithium ion battery negative electrode sheet or the lithium ion battery negative electrode sheet prepared by the above-mentioned method.

[0021] The negative electrode sheet of a lithium ion battery provided by the present invention comprises a copper foil negative current collector and a negative electrode material layer. In view of the mechanical stress caused by the expansion and contraction of the existing silicon-based negative electrode material during the charging and discharging process, cracks are generated inside the electrode sheet, affecting the problem of the electron path and conductivity in the electrode sheet, the negative electrode material layer of the present invention is composed of carbon material strips and silicon-based material strips alternately distributed from left to right, that is, carbon material strips-silicon-based material strips-carbon material strips-silicon-based material strips-carbon material strips. By using carbon material strips with low expansion rate and silicon-based material strips with high specific capacity and high expansion rate to be arranged alternately, on the one hand, the carbon material strips with low expansion rate cut off the continuous stress conduction generated when the silicon-based material strips with high expansion rate expand, so that the continuity of crack generation is interrupted, preventing the generation and diffusion of cracks in the electrode sheet, reducing the failure of the electron path caused by the expansion and contraction process of the electrode sheet, improving the overall electronic conductivity of the electrode sheet, and improving the capacity retention rate of the active material of the electrode sheet after multiple cycles, thereby ensuring the rate performance and cycle performance of the battery; on the other hand, the silicon-based material strips have a high specific capacity, ensuring that the lithium ion battery has a high energy density. Therefore, the lithium ion battery negative electrode provided by the present invention not only effectively improves the energy density of the battery, but also enables the battery to have excellent capacity retention and rate performance during the cycle process.

[0022] The method for preparing a negative electrode sheet of a lithium ion battery provided by the present invention comprises the following steps: after obtaining copper foil, silicon-based material and carbon-based material, carbon-based material strips and silicon-based material strips are sequentially deposited on the copper foil from left to right to form alternatingly distributed carbon-based material strips and silicon-based material strips, and then the strips are dried and rolled to obtain a negative electrode sheet of a lithium ion battery. The method is simple and can realize industrial production and application.

[0023] The lithium ion battery provided by the present invention comprises the above-mentioned lithium ion battery negative electrode sheet which can improve the battery energy density, capacity retention rate, rate performance and cycle stability. Therefore, the lithium ion battery provided by the present invention not only has a higher energy density, but also has excellent capacity retention rate and rate performance during the cycle process, and has a long cycle life. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a plan view of a negative electrode sheet of a lithium-ion battery provided in an embodiment of the present invention.

[0025] Figure 2 It is a cross-sectional schematic diagram of a negative electrode sheet of a lithium-ion battery provided in an embodiment of the present invention.

[0026] Figure 3 It is a plan view of a negative electrode sheet of a lithium-ion battery with a curved contact surface provided by an embodiment of the present invention.

[0027] Figure 4 It is a plan view of a negative electrode sheet of a lithium-ion battery provided by an embodiment of the present invention, wherein the contact surface forms a certain angle with the electrode sheet coating direction.

[0028] Figure 5 It is a cross-sectional schematic diagram of the lithium-ion battery negative electrode sheet, positive electrode sheet and separator after being assembled according to an embodiment of the present invention.

[0029] Figure 6 It is a schematic diagram of stress diffusion after expansion of a negative electrode sheet of a lithium-ion battery provided by an embodiment of the present invention.

[0030] Among them, the reference numerals in the figure are:

[0031] 1——Carbon material strip 2——Silicon-based material strip 3——Negative current collector 4——Negative electrode material layer 5——Separator 6——Cathode material strip 7——Positive current collector DETAILED DESCRIPTION

[0032] In order to make the purpose, technical scheme and technical effect of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention is described clearly and completely. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. In combination with the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] In the description of the present invention, it should be understood that the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0034] The weight of the relevant components mentioned in the description of the embodiments of the present invention may not only refer to the specific content of each component, but also indicate the weight ratio between the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the description of the embodiments of the present invention, it is within the scope disclosed in the description of the embodiments of the present invention. Specifically, the weight described in the description of the embodiments of the present invention may be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.

[0035] As attached Figure 1 As shown, an embodiment of the present invention provides a negative electrode sheet for a lithium-ion battery, comprising: a negative current collector 3 and a negative electrode material layer 4 arranged on the negative current collector 3, wherein the negative electrode material layer 4 is composed of carbon-based material strips 1 and silicon-based material strips 2 alternately distributed from left to right, that is, carbon-based material strips 1-silicon-based material strips 2-carbon-based material strips 1-silicon-based material strips 2-carbon-based material strips 1.

[0036] The negative electrode sheet of a lithium-ion battery provided in an embodiment of the present invention includes a copper foil negative current collector and a negative electrode material layer. In order to solve the problem that the mechanical stress caused by the expansion and contraction of the existing silicon-based negative electrode material during the charging and discharging process causes cracks inside the electrode sheet, affecting the electron path and conductivity in the electrode sheet, the negative electrode material layer of the present invention is composed of carbon material strips and silicon-based material strips alternately distributed from left to right, that is, carbon material strips-silicon-based material strips-carbon material strips-silicon-based material strips-carbon material strips. By alternately arranging carbon material strips with low expansion rate and silicon-based material strips with high specific capacity and high expansion rate, on the one hand, as shown in the attached Figure 6 As shown, the carbon material strip with low expansion rate cuts off the continuous stress conduction generated when the silicon-based material strip with high expansion rate expands, so that the continuity of crack generation is interrupted, preventing the generation and diffusion of cracks in the pole piece, reducing the failure of the electronic path caused by the expansion and contraction of the pole piece, improving the overall electronic conductivity of the pole piece, and improving the capacity retention rate of the active material of the pole piece after multiple cycles, ensuring the rate performance and cycle performance of the battery; on the other hand, the silicon-based material strip has a higher specific capacity, ensuring that the lithium-ion battery has a higher energy density. Therefore, the lithium-ion battery negative electrode provided by the embodiment of the present invention not only effectively improves the energy density of the battery, but also enables the battery to have excellent capacity retention rate and rate performance during the cycle process.

[0037] As a preferred embodiment, the negative electrode material layer is provided with alternating carbon material strips and silicon-based material strips in the lateral direction along the coating direction of the negative electrode sheet from left to right, that is, carbon material strips-silicon-based material strips-carbon material strips-silicon-based material strips-carbon material strips. The alternating carbon material strips and silicon-based material strips in the embodiment of the present invention are arranged in sequence from left to right along the lateral direction of the coating direction of the negative electrode sheet, which is more conducive to coating and manufacturing the negative electrode material layer.

[0038] As attached Figure 2 As shown, as a preferred embodiment, the thickness of the negative electrode material layer 4 is 50 microns to 110 microns. The thickness of the negative electrode material layer 4 in the embodiment of the present invention is 50 microns to 110 microns. The negative electrode material layer 4 of this thickness is most conducive to simultaneously improving the overall energy density of the battery and ensuring the cycle performance of the battery. If the negative electrode material layer 4 is less than 50 microns, the content of active substances in the negative electrode material layer 4 is too small, which reduces the energy density of the battery. If the negative electrode material layer 4 is higher than 110 microns, the resistance of lithium ions to embedding or escaping in the negative electrode sheet increases, the internal resistance of the battery increases, and the battery charging and discharging efficiency is affected.

[0039] In some embodiments, the thickness of the negative electrode material layer 4 is 50 micrometers, 60 micrometers, 70 micrometers, 80 micrometers, 90 micrometers, 100 micrometers and 110 micrometers.

[0040] As a preferred embodiment, the width of the silicon-based material strip 2 is 5 cm to 10 cm. The silicon-based material strip 2 of the embodiment of the present invention has a high specific capacity and a high expansion rate. When the width is 5 cm to 10 cm, it can not only improve the overall energy density of the battery, but also reduce the mechanical stress caused by the expansion of the silicon-based material strip through the alternately arranged carbon material strip layers, thereby improving the overall cycle life and rate performance of the battery.

[0041] In some embodiments, the width of the silicon-based material strip 2 is 5 cm, 6 cm, 7 cm, 8 cm, 9 cm and 10 cm.

[0042] As a preferred embodiment, the width of the carbon material strip 1 is 2 cm to 5 cm. The carbon material strip 1 of the embodiment of the present invention has a low expansion rate and a relatively low specific capacity. When the width is 2 cm to 5 cm, it can not only cut off the stress conduction of the high expansion rate silicon-based material strip 2 and prevent crack propagation, but also avoid the risk of reducing the overall energy density of the battery due to the low specific capacity carbon material strip 1 being too wide.

[0043] In some embodiments, the width of the carbon-based material strip 1 is 2 cm, 3 cm, 4 cm and 5 cm.

[0044] As a preferred embodiment, the carbon material strip 1 and the silicon-based material strip 2 are in conductive contact with each other, and the contact surface of the carbon material strip 1 and the silicon-based material strip 2 is a plane or a curved surface. The carbon material strip 1 and the silicon-based material strip 2 in the embodiment of the present invention are in conductive contact with each other, and the contact surface is a curved surface or a plane, which is conducive to the conduction between electrons and ions in the battery, ensuring the electrochemical performance of the battery, and the continuous stress conduction generated by the high-expansion silicon-based material strip 2 is cut off by the alternating arrangement of the carbon material strips 1, so that the continuity of the crack generation is interrupted, thereby improving the capacity retention rate of the active material of the electrode after multiple cycles.

[0045] As attached Figure 3 As shown, as a more preferred embodiment, the carbon material strip 1 and the silicon-based material strip 2 are in conductive contact with each other, and the contact surface of the carbon material strip 1 and the silicon-based material strip 2 is a curved surface. The contact surface of the carbon material strip 1 and the silicon-based material strip 2 in the embodiment of the present invention is a curved surface, so that the carbon material strip 1 and the silicon-based material strip 2 have a larger contact area, which is more conducive to the low-expansion carbon material strip 1 cutting off the continuous stress conduction generated by the high-expansion silicon-based material strip 2, further improving the electrical performance and cycle life of the battery.

[0046] As a more preferred embodiment, the contact surface between the carbon-based material strip 1 and the silicon-based material strip 2 is a plane, and the plane may be parallel to the coating direction, as shown in the attached Figure 1 As shown, it can also be at a certain angle with the coating direction, as shown in the attached Figure 4As shown, the carbon material strip 1 and the silicon-based material strip 2 have a larger contact area, which is more conducive to the low-expansion carbon material strip 1 cutting off the continuous stress conduction generated by the high-expansion silicon-based material strip 2, further improving the electrical performance and cycle life of the battery.

[0047] As a preferred embodiment, the silicon-based material strip 2 contains a silicon negative electrode active material, and the silicon negative electrode active material is selected from at least one of silicon, silicon alloy, silicon oxide, silicon carbon composite, and silicon carbon oxide. It also contains a conductive agent, a binder and a thickener, or a solvent. In some embodiments, the solvent is deionized water; the conductive agent is at least one of conductive carbon black, carbon nanotubes, acetylene black, and graphene; the binder is at least one of styrene butadiene rubber (SBR) and a water dispersion of acrylonitrile multipolymer (LA133); the thickener is carboxymethyl cellulose (CMC), etc.

[0048] As a preferred embodiment, the carbon material strip 1 contains a carbon negative electrode active material, and the carbon negative electrode active material is selected from at least one of artificial graphite, natural graphite, carbon fiber, and carbon microspheres. It also contains a solvent, a conductive agent, a binder, and a thickener. In some embodiments, the solvent is deionized water; the conductive agent is at least one of conductive carbon black, carbon nanotubes, acetylene black, and graphene; the binder is at least one of styrene butadiene rubber (SBR) and a water dispersion of acrylonitrile multipolymer (LA133); the thickener is carboxymethyl cellulose (CMC), etc.

[0049] The negative electrode sheet of the lithium-ion battery provided in the embodiment of the present invention can be prepared by the following method.

[0050] The present invention also provides a method for preparing a negative electrode sheet of a lithium-ion battery, comprising the following steps:

[0051] S10. Obtaining copper foil as a negative electrode current collector;

[0052] S20. Obtain a silicon-based material and a carbon-based material, and deposit the silicon-based material and the carbon-based material on the copper foil, so that carbon-based material strips 1 and silicon-based material strips 2 are alternately distributed on the copper foil from left to right, and the carbon-based material strips 1 and the silicon-based material strips 2 are in conductive contact with each other, to obtain a deposition product;

[0053] S30. Drying and rolling the deposited product to obtain a negative electrode sheet for a lithium-ion battery.

[0054] The method for preparing a negative electrode sheet for a lithium-ion battery provided in an embodiment of the present invention comprises obtaining copper foil, silicon-based material and carbon-based material, depositing carbon-based material strips and silicon-based material strips alternatingly distributed on the copper foil from left to right, and then drying and rolling to obtain a negative electrode sheet for a lithium-ion battery. The preparation method is simple and can be industrialized for production and application.

[0055] Specifically, in the above step S10 , the embodiment of the present invention uses copper foil as the negative current collector 3 .

[0056] Specifically, in the above step S20, a silicon-based material and a carbon-based material are obtained, and the silicon-based material and the carbon-based material are deposited on the copper foil, so that carbon-based material strips 1 and silicon-based material strips 2 are formed on the copper foil from left to right in sequence, and the carbon-based material strips 1 and the silicon-based material strips 2 are in conductive contact with each other to obtain a deposition product. In the embodiment of the present invention, the silicon-based material and the carbon-based material are deposited on the copper foil to obtain a deposition product in which carbon-based material strips 1 and silicon-based material strips 2 are formed on the copper foil in sequence from left to right in sequence. Among them, the silicon-based material contains at least one silicon negative electrode active material selected from silicon, silicon alloy, silicon oxide, silicon-carbon composite, and silicon-carbon oxide; the carbon-based material strip 1 contains at least one carbon negative electrode active material selected from artificial graphite, natural graphite, carbon fiber, and carbon microspheres. In addition, the silicon-based material and the carbon-based material also contain a solvent, a conductive agent, a binder, and a thickener. In some embodiments, the solvent is deionized water; the conductive agent is at least one of conductive carbon black, carbon nanotubes, acetylene black, and graphene; the binder is at least one of styrene butadiene rubber (SBR) and an aqueous dispersion of acrylonitrile multipolymer (LA133); the thickener is carboxymethyl cellulose (CMC), etc.

[0057] In some embodiments, the raw material components of the silicon-based material and the carbon-based material are dispersed into a uniform and stable material at a high speed through emulsification and homogenization, and then the silicon-based material and the carbon-based material are coated on the copper foil by co-extrusion coating, so that the copper foil forms alternating carbon-based material strips 1 and silicon-based material strips 2 in the lateral direction of the coating from left to right to obtain a deposition product.

[0058] Specifically, in the above step S30, the deposition product is dried and rolled to obtain a negative electrode sheet for a lithium-ion battery. In the embodiment of the present invention, the deposition product is dried and rolled to obtain a prepared negative electrode sheet for a lithium-ion battery.

[0059] Accordingly, as attached Figure 5 As shown, a lithium ion battery comprises: a positive electrode sheet, a negative electrode sheet, a separator 5 and an electrolyte, wherein the negative electrode sheet is the above-mentioned lithium ion battery negative electrode sheet or the lithium ion battery negative electrode sheet prepared by the above-mentioned method.

[0060] The lithium-ion battery provided by the embodiment of the present invention includes the above-mentioned lithium-ion battery negative electrode sheet that can improve the battery energy density, capacity retention rate, rate performance and cycle stability. Therefore, the lithium-ion battery provided by the embodiment of the present invention not only has a higher energy density, but also has excellent capacity retention rate and rate performance during the cycle process, and has a long cycle life.

[0061] Specifically, the lithium-ion battery positive electrode sheet provided by the embodiment of the present invention includes a positive current collector 7 and a positive electrode material strip 6 .

[0062] In order to make the above implementation details and operations of the present invention clearly understood by those skilled in the art, and to demonstrate the significant improvement in performance of the lithium-ion battery negative electrode sheet and lithium-ion battery of the embodiments of the present invention, the above technical solution is illustrated by multiple embodiments below.

[0063] Example 1

[0064] A lithium-ion battery, comprising:

[0065] Negative electrode sheet: 2 cm carbon material strips 1 of artificial graphite HSG and 5 cm silicon-based material strips 2 of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 80 microns. The contact surface of the carbon material strips 1 and the silicon-based material strips 2 is flat;

[0066] The negative electrode sheet, the positive electrode sheet and the separator are assembled to form a 053048 model soft-pack battery.

[0067] Example 2

[0068] A lithium-ion battery, comprising:

[0069] Negative electrode sheet: 5 cm carbon material strips 1 of artificial graphite HSG and 5 cm silicon-based material strips 2 of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 80 microns. The contact surface of the carbon material strips 1 and the silicon-based material strips 2 is flat.

[0070] The negative electrode sheet and the positive electrode sheet and the separator which are the same as those in Example 1 are assembled into a 053048 model soft-pack battery.

[0071] Example 3

[0072] A lithium-ion battery, comprising:

[0073] Negative electrode sheet: 2 cm carbon material strips of artificial graphite HSG and 10 cm silicon-based material strips of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 80 microns. The contact surface of the carbon material strips and the silicon-based material strips is flat;

[0074] The negative electrode sheet and the positive electrode sheet and the separator which are the same as those in Example 1 are assembled into a 053048 model soft-pack battery.

[0075] Example 4

[0076] A lithium-ion battery, comprising:

[0077] Negative electrode sheet: 2 cm carbon material strips of artificial graphite HSG and 10 cm silicon-based material strips of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 50 μm. The contact surface between the carbon material strips and the silicon-based material strips is flat.

[0078] The negative electrode sheet and the positive electrode sheet and the separator which are the same as those in Example 1 are assembled into a 053048 model soft-pack battery.

[0079] Example 5

[0080] A lithium-ion battery, comprising:

[0081] Negative electrode sheet: 2 cm carbon material strips of artificial graphite HSG and 10 cm silicon-based material strips of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 110 μm. The contact surface between the carbon material strips and the silicon-based material strips is flat.

[0082] The negative electrode sheet and the positive electrode sheet and the separator which are the same as those in Example 1 are assembled into a 053048 model soft-pack battery.

[0083] Example 6

[0084] A lithium-ion battery, comprising:

[0085] Negative electrode sheet: 2 cm carbon material strips of artificial graphite HSG and 10 cm silicon-based material strips of silicon-oxygen composite material SO450 are alternately coated on the copper foil from left to right along the coating direction of the negative electrode sheet, and the material coating thickness is 80 microns. The contact surface between the carbon material strips and the silicon-based material strips is a curved surface.

[0086] The negative electrode sheet and the positive electrode sheet and the separator which are the same as those in Example 1 are assembled into a 053048 model soft-pack battery.

[0087] Comparative Example 1

[0088] A lithium-ion battery comprises: a negative electrode sheet with a thickness of 80 microns coated with a silicon-based material of a silicon-oxygen composite material SO450, and a positive electrode sheet and a separator the same as those in the above embodiment 1, assembled into a 053048 model soft-pack battery.

[0089] Furthermore, in order to verify the advancement of the lithium ion batteries provided by Examples 1 to 6 of the present invention and Comparative Example 1, the present invention was subjected to electrochemical performance tests, and the test results are shown in Table 1 below:

[0090] Table 1

[0091]

[0092] From the test results in Table 1 above, it can be seen that the cycle performance of the lithium-ion batteries of Examples 1 to 6 is better than that of Comparative Example 1, and the capacity retention rate of the lithium-ion batteries of Examples 1 to 6 is substantially higher than that of Comparative Example 1, and the volume energy density of the lithium-ion batteries of Examples 1 to 6 is slightly lower than that of Comparative Example 1. Among them, the volume energy density of the lithium-ion battery of Example 5 is closest to that of Comparative Example 1, but its cycle performance is relatively the worst among Examples 1 to 6, mainly due to its high coating thickness, so the coating thickness should not exceed 110 μm. The good cycle performance of the lithium-ion battery of Example 4 is mainly due to the thin coating thickness, but it affects its volume energy density; in general, the volume energy density, cycle performance and rate performance of Example 3 are better; the contact surface of the lithium-ion battery of Example 6 is a curved surface, which mainly improves the rate performance of the battery cell.

[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode sheet for a lithium-ion battery, characterized in that: The negative electrode sheet is composed of a negative current collector and a negative electrode material layer arranged on the negative current collector. The negative electrode material layer is composed of carbon material strips and silicon-based material strips alternately distributed from left to right in the transverse direction along the coating direction of the negative electrode sheet. The thickness of the negative electrode material layer is 50 microns to 110 microns, the width of the silicon-based material strip is 5 centimeters to 10 centimeters, and the width of the carbon material strip is 2 centimeters to 5 centimeters.

2. The negative electrode sheet of a lithium-ion battery according to claim 1, characterized in that: The carbon-based material strip and the silicon-based material strip are in conductive contact with each other, and a contact surface between the carbon-based material strip and the silicon-based material strip is a plane or a curved surface.

3. The negative electrode sheet of a lithium-ion battery according to claim 2, characterized in that: The silicon-based material strip contains silicon negative electrode active material, and the silicon negative electrode active material is selected from at least one of silicon, silicon alloy, silicon oxide, silicon-carbon composite, and silicon-carbon oxide.

4. The negative electrode sheet for a lithium-ion battery according to any one of claims 1 to 3, characterized in that: The carbon material strip contains carbon negative electrode active material, and the carbon negative electrode active material is selected from at least one of artificial graphite, natural graphite, carbon fiber, and carbon microspheres.

5. The negative electrode sheet of a lithium-ion battery according to claim 4, characterized in that: The silicon-based material strips and the carbon-based material strips contain: a conductive agent, a binder and a thickener.

6. A method for preparing a negative electrode sheet for a lithium ion battery according to any one of claims 1 to 5, characterized in that: The following steps are involved: Obtaining copper foil as a negative electrode current collector; Obtaining a silicon-based material and a carbon-based material, and depositing the silicon-based material and the carbon-based material on the copper foil, so that the copper foil forms alternatingly distributed carbon-based material strips and silicon-based material strips from left to right, and the carbon-based material strips and the silicon-based material strips are in conductive contact with each other, to obtain a deposition product; The deposited product is dried and rolled to obtain a negative electrode sheet for a lithium-ion battery.

7. A lithium ion battery, characterized in that: include: A positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, wherein the negative electrode sheet is a lithium ion battery negative electrode sheet as described in any one of claims 1 to 5 or a lithium ion battery negative electrode sheet prepared by the method as described in claim 6.