Electrodes for electrochemical sensors
By using palladium metal layer and palladium oxide-containing layer in the biosensor electrode, the reduction in conductivity caused by atmospheric aging and mechanical instability of electrons to mobility are solved, and the durability and measurement accuracy of the electrode are improved.
Patent Information
- Application Number
- CN201880011289.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-02-10
- Filing Date
- 2018-01-30
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-01-30
AI Technical Summary
Existing biosensor electrodes are prone to physical and chemical changes in atmospheric aging, resulting in reduced conductivity and mechanical instability of electron-to-movement, affecting measurement accuracy.
Using an electrode containing a palladium metal layer and a palladium oxide-containing layer, the oxide-containing layer is sputtered by sputtering the palladium metal layer in an inert atmosphere and sputtering the palladium oxide-containing layer in an atmosphere containing an oxidant, the oxide surface coverage is controlled to form a stable electrode surface. .
It improves the atmospheric aging resistance and electrochemical performance of the electrode, maintains the consistency and accuracy of measurement, and extends the service life of the electrode.
Smart Images

Figure CN110249225B_ABST
Abstract
Description
Background of the Invention
[0001] 1. Field of the Invention
[0002] The present invention generally relates to electrodes for use in electrochemical sensors, such as for use in biosensors. More particularly, the present invention relates to an electrode comprising a palladium metal layer and a palladium oxide-containing layer.
[0003] 2. Description of related technologies
[0004] Biosensors for analyzing biological samples are becoming increasingly common. For example, with the increase in cases of diabetes in the world population, the demand for biosensors that measure blood sugar has grown significantly. Such biosensors are commonly referred to as blood glucose meters and operate by having the user place a drop of blood on a test strip associated with the blood glucose meter. The test strip is configured to be reactive to the amount of glucose in the drop of blood so that the blood glucose meter can detect and display the glucose level of the user's blood.
[0005] The test strips for biosensors of the blood glucose meter type are usually composed of two or more electrodes (e.g., a working electrode and a counter electrode) formed on a substrate. In addition, biological reactants that react with the biological sample, such as enzymes (e.g., glucose oxidase, glucose dehydrogenase, etc.) and mediators (e.g., ferrocyanide, ruthenium complexes, osmium complexes, quinones, phenothiazines, phenoxazines, etc.) are formed on at least one of the electrodes (e.g., the working electrode). In operation, a drop of blood is applied to the test strip. Subsequently, an electrochemical reaction proportional to the amount of glucose in the blood occurs on the working electrode. In more detail, glucose first reacts with biological reactants, such as enzymes (glucose oxidase, glucose dehydrogenase, etc.) and sometimes enzyme cofactors (PQQ, FAD, etc.), and is oxidized to gluconic acid. The biological reactants, such as enzymes, cofactors, or enzyme-cofactor complexes are temporarily reduced by two electrons transferred from glucose to the enzyme, cofactor, or enzyme-cofactor complex. Next, in the case where the mediator is reduced in a single electron process, the reduced enzyme, cofactor or enzyme-cofactor complex reacts with the mediator, transferring a single electron to each of the two mediator species (molecules or complexes). When the mediator species is reduced, the enzyme, cofactor or enzyme-cofactor complex thereby returns to its original oxidation state. Subsequently, the reduced mediator diffuses to the electrode surface, where a predetermined and sufficient oxidation potential is applied to the biosensor to oxidize the reduced mediator back to its original oxidation state. The current generated by the oxidation of the mediator species by the biosensor is measured and is proportional to the amount of glucose in the blood.
[0006] The quality of the working electrode plays an important role in accurately measuring blood glucose levels. Specifically, each of the following factors contributes to improved accuracy of blood glucose test strips: (1) the reproducibility of the electroactive surface area of the electrode, (2) the batch-to-batch reproducibility of the electrode's electron transfer kinetics in a specific glucose measurement configuration, and (3) the long-term stability of the electrode material during storage.
[0007] Many metal-based electrode compositions are somewhat unstable in that they are susceptible to atmospheric aging. Such electrode aging due to exposure to the environment may change the physical and chemical properties of the electrode. As a result, the electrochemical performance and accuracy of the electrode may be degraded.
[0008] To mitigate such aging issues, many commercially available biosensors use electrode materials that are noble in nature, such as gold, palladium, platinum, iridium, etc. Such noble metals are generally considered to be minimally reactive with interfering substances (e.g., the atmosphere), and therefore are considered to provide enhanced chemical resistance for consistent and accurate measurements. However, it has been found that even noble metals (such as palladium) are subject to atmospheric aging and thereby undergo physical and chemical changes over time.
[0009] Therefore, there is a need for electrodes for electrochemical sensors, such as biosensors, that provide consistent and accurate measurements throughout the useful life of the sensor. In particular, there is a need for electrodes that can withstand the negative effects of atmospheric aging without experiencing a significant decrease in electrode conductivity and / or without experiencing significant changes in heterogeneous electron transfer kinetics when used with commonly used redox mediators. SUMMARY OF THE INVENTION
[0010] One or more embodiments of the present invention relate to an electrochemical electrode for a biosensor. The electrode comprises a substrate, a palladium metal layer fabricated on the substrate, and a palladium oxide-containing layer fabricated on the palladium metal layer. The palladium metal layer has a thickness of no more than 90 nm, and the palladium oxide-containing layer has a thickness of no more than 40 nm.
[0011] One or more additional embodiments of the present invention are directed to an electrochemical electrode for a biosensor. The electrode comprises a substrate, a palladium metal layer fabricated on the substrate, and a palladium oxide-containing layer fabricated on the palladium metal layer. The ratio of the thickness of the palladium oxide-containing layer to the thickness of the palladium metal layer is no more than 3:5.
[0012] One or more additional embodiments of the present invention are directed to a method of making an electrochemical electrode for a biosensor. The method includes an initial step of providing a substrate. An additional step includes sputtering a palladium metal layer on the substrate in a first atmosphere consisting essentially of an inert gas. An additional step includes sputtering a palladium oxide-containing layer on the palladium metal layer in a second atmosphere comprising a mixture of an inert gas and an oxidant, wherein the oxidant constitutes 0.5 to 40% of the second atmosphere by partial pressure.
[0013] One or more additional embodiments of the present invention are directed to an electrochemical electrode for a biosensor. The electrode comprises a substrate, a palladium metal layer formed on the substrate, and a palladium oxide-containing layer formed on the palladium metal layer. Within 10 days of forming the palladium metal layer and the palladium oxide-containing layer, when the electrode is plated with MESA via a mercaptoethanesulfonate (MESA) plating procedure, the electrode is configured to receive a specific partial surface coverage (partial coverage A) of MESA on the outer surface of the electrode. Between 10 and 90 days after forming the palladium metal layer and the palladium oxide-containing layer, when the electrode is plated with MESA via a MESA plating procedure, the electrode is configured to receive a separate partial surface coverage (partial coverage B) of MESA on the outer surface of the electrode. The partial coverage A deviates from the partial coverage B by no more than 30%.
[0014] One or more additional embodiments of the present invention relate to an electrochemical electrode for a biosensor. The electrochemical electrode comprises a substrate, a palladium metal layer formed on the substrate, and a palladium oxide-containing layer deposited on the palladium metal layer. When the electrochemical electrode is plated with MESA via a mercaptoethanesulfonate (MESA) plating procedure, the electrochemical electrode is configured to receive a specific partial surface coverage of MESA on the outer surface of the electrode. When a baseline electrode is immersed in MESA via a MESA plating procedure, the baseline electrode is configured to receive a baseline partial surface coverage of MESA on the outer surface of the baseline electrode. The electrochemical electrode is configured so that when the electrochemical electrode receives a specific partial coverage of MESA within 10 days of forming the palladium metal layer and the palladium oxide-containing layer, the specific partial surface coverage of MESA on the electrochemical electrode deviates by no more than 25% higher and / or 50% lower than the baseline partial surface coverage of MESA on the baseline electrode.
[0015] One or more additional embodiments of the present invention are directed to an electrochemical electrode for a biosensor. The electrochemical electrode comprises a substrate, a palladium metal layer formed on the substrate, and a palladium oxide-containing layer formed on the palladium metal layer. The electrochemical electrode is configured to have a reduction peak determined by a Type 1 cyclic voltammetry test that is at least 10 mV more cathode-biased than a reduction peak determined by a Type 1 cyclic voltammetry test for a baseline electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Embodiments of the present invention are described herein with reference to the following drawings, in which:
[0017] Figure 1 is a schematic cross-sectional view of an electrode according to an embodiment of the present invention, particularly showing a conductive film on a substrate;
[0018] Figure 2 yes Figure 1 A more detailed cross-sectional schematic diagram of an electrode, particularly showing a conductive film including a conductive layer and an oxide-containing layer;
[0019] Figure 3 is a schematic diagram of a test strip biosensor including electrodes according to an embodiment of the present invention;
[0020] Figure 4 is a graph depicting polarization scans of three electrodes subjected to a Type 1 cyclic voltammetry test;
[0021] Figure 5 is a graph depicting polarization scans of four electrodes subjected to a Type 1 cyclic voltammetry test;
[0022] Figure 6 is a graph depicting polarization scans of four electrodes subjected to a type 2 cyclic voltammetry test;
[0023] Figure 7 is a graph depicting polarization scans of two electrodes subjected to a Type 1 cyclic voltammetry test;
[0024] Figure 8 is a graph depicting cyclic voltammograms of three electrodes subjected to type 3 cyclic voltammogram testing;
[0025] Fig. 9 is a graph depicting cyclic voltammograms of four electrodes subjected to type 4 cyclic voltammogram testing;
[0026] Fig.10 is a graph depicting MESA coverage of electrodes subjected to a Type 1 MESA coverage test;
[0027] Fig.11 is a graph depicting the change in percentage of MESA coverage of electrodes subjected to the Type 1 MESA coverage test;
[0028] Fig.12 is a graph depicting MESA kinetics of an electrode subjected to a Type 1 MESA kinetics test;
[0029] Fig.13 is another graph depicting MESA kinetics of an electrode subjected to Type 1 MESA kinetics testing; and
[0030] Fig.14 is a graph depicting cyclic voltammograms of four electrodes subjected to type 3 cyclic voltammogram testing. DETAILED DESCRIPTION OF THE INVENTION
[0031] The present invention generally relates to the composition of electrodes for use in electrochemical sensors (such as biosensors). As used herein, the term "biosensor" refers to a device for analyzing biological samples. In some embodiments, such as Figure 1 As shown in , the electrode may be a layered thin film electrode (electrode 100), and may generally include a substrate 102 and a conductive film 104 coated on at least a portion of the substrate 102. Figure 2 As shown in , the conductive film 104 may include a conductive layer 106 and an oxide-containing layer 108. In such embodiments, the conductive layer 106 may be formed on the substrate 102, and the oxide-containing layer 108 may be formed on the conductive layer 106. Although the conductive film 104 includes the oxide-containing layer 106, the electrode 100 formed according to an embodiment of the present invention provides the conductive film 104 with sufficient conductivity and electrochemical response for use in an electrochemical sensor.
[0032] As described above, in some embodiments, the electrode 100 can be used in a biosensor. The biosensor can be a medical sensor, such as a blood glucose sensor or a blood glucose meter. The term "medical sensor" as used herein refers to a biosensor used for medical monitoring and / or diagnosis. In addition, the term "blood glucose sensor" refers to a medical sensor used to measure the concentration of glucose in the blood. Thus, the electrode 100 described herein can form part of a test strip used in a medical sensor (such as a blood glucose sensor). For example, Figure 3 As shown in , some embodiments contemplate that the medical sensor may include a test strip 110, which includes a first electrode 100 separated from a second electrode 100 by a reaction space 112. The first electrode 100 may include a working electrode, and the second electrode 100 may include a reference electrode or a counter electrode or a combined reference electrode and counter electrode. Thus, a biological sample (such as a drop of blood) can be placed in the reaction space 112 and electrically contacted with the first and second electrodes 100 for analysis.
[0033] Unlike conventional biosensor electrodes, which typically include and / or use only a conductive film substantially formed of a noble metal such as palladium and / or gold, the electrode 100 described herein may be formed to include a conductive film 104, which includes a conductive layer 106 formed of a noble metal such as palladium and an oxide-containing layer 108, which may be formed as a layer containing an oxide of the same noble metal such as palladium oxide. Although the electrode 100 includes the oxide-containing layer 108, the combination of the conductive layer 106 and the oxide-containing layer 108 described herein is configured to provide excellent consistency and accuracy when measuring a biological sample while simultaneously being subjected to atmospheric aging.
[0034] In more detail, embodiments of the present invention configure the substrate 102 of the electrode 100 to be formed of any type of material (flexible or rigid), which is generally non-conductive and chemically inert to the expected chemical reactions described herein. In certain embodiments, the substrate 102 may include a flexible non-conductive film, including a polymer, such as a polymer film, a polyester film, a polycarbonate film, and the like. In certain specific embodiments, the substrate 102 may include a polyethylene terephthalate (PET) film. Embodiments of the present invention contemplate that the substrate 102 may have a thickness of at least 25 μm, 125 μm, or 250 μm and / or no more than 800 μm, 500 μm, or 400 μm. In certain embodiments, substrate 102 can have a thickness of 25 to 800 µm, 25 to 500 µm, or 25 to 400 µm; 125 to 800 µm, 125 to 500 µm, or 125 to 400 µm; or 250 to 800 µm, 250 to 500 µm, or 250 to 400 µm.
[0035] As described above, the conductive film 104 plated on the substrate 102 may include a conductive layer 106 and an oxide-containing layer 108. In some embodiments, the conductive layer 106 may be substantially composed of palladium, and the oxide-containing layer 108 may include palladium oxide. However, in other embodiments, the conductive layer 106 may include other metals (e.g., gold) or non-metals, and the oxide-containing layer 108 may include oxides of such other metals, or may include oxides of other materials. The conductive layer 106 and the oxide-containing layer 108 may be manufactured on the substrate 102 via one or more physical vapor deposition techniques, such as sputtering coating (e.g., magnetron sputtering, unbalanced magnetron sputtering, facing target sputtering, etc.), thermal evaporation, electron beam evaporation, arc evaporation, co-evaporation, ion plating, etc. Specifically, the conductive layer 106 may be manufactured on the substrate 102 (e.g., via sputtering), and the oxide-containing layer 108 may be manufactured on the conductive layer 106 (e.g., via sputtering). The term "manufacture" used herein is used to refer to "intentional manufacture". Thus, when oxide-containing layer 108 is described as being fabricated, such description excludes the formation of naturally occurring oxide-containing layers, such as when the electrode is exposed to an ambient environment (e.g., an atmosphere-induced oxide-containing layer naturally formed on a metal electrode surface that has aged in an ambient environment).
[0036] Conductive film 104 may be formed to a thickness of at least 5, 10, 20, or 30 nm and / or no more than 110, 100, 90, or 80 nm on substrate 102. In certain embodiments, conductive film 104 may have a thickness of 5 to 110 nm, 5 to 100 nm, 5 to 90 nm, 5 to 80 nm; 10 to 110 nm, 10 to 100 nm, 10 to 90 nm, or 10 to 80 nm; 20 to 110 nm, 20 to 100 nm, 20 to 90 nm, or 20 to 80 nm; or 30 to 110 nm, 30 to 100 nm, 30 to 90 nm, or 30 to 80 nm.
[0037] As described above, the conductive film 104 may be a multilayer film including the conductive layer 106 and the oxide-containing layer 108. Thus, some embodiments of the present invention configure the conductive layer 106 to be formed on the substrate 102 to a thickness of at least 0.5, 1, 2, 3 nm, or 4 nm and / or not more than 90, 80, 40, 10, or 5 nm. In some embodiments, the conductive layer 106 can have a thickness of 0.5 to 90 nm, 0.5 to 80 nm, 0.5 to 40 nm, 0.5 to 10 nm, or 0.5 to 5 nm; 1 to 90 nm, 1 to 80 nm, 1 to 40 nm, 1 to 10 nm, or 1 to 5 nm; 2 to 90 nm, 2 to 80 nm, 2 to 40 nm, 2 to 10 nm, or 2 to 5 nm; 3 to 90 nm, 3 to 80 nm, 3 to 40 nm, 3 to 10 nm, or 3 to 5 nm; or 4 to 90 nm, 4 to 80 nm, 4 to 40 nm, 4 to 10 nm, or 4 to 5 nm. In other embodiments, the conductive layer 106 can have a thickness of 15 to 35 nm, 20 to 30 nm, or about 25 nm.
[0038] In addition, the oxide-containing layer 108 of the conductive film 104 can be formed on the conductive layer 106 to a thickness of at least 0.5, 1, 2, or 3 nm and / or no more than 20, 15, 10, or 5 nm. In certain embodiments, the oxide-containing layer 108 can have a thickness of 0.5 to 20 nm, 0.5 to 15 nm, 0.5 to 10 nm, or 0.5 to 5 nm; 1 to 20 nm, 1 to 15 nm, 1 to 10 nm, or 1 to 5 nm; 2 to 20 nm, 2 to 15 nm, 2 to 10 nm, or 2 to 5 nm; or 3 to 20 nm, 3 to 15 nm, 3 to 10 nm, or 3 to 5 nm. In other embodiments, the conductive layer 106 can have a thickness of 5 to 15 nm, 7 to 12 nm, or about 10 nm.
[0039] Thus, embodiments may configure oxide-containing layer 108 to have a thickness of no more than 70%, 60%, 50%, 40%, 30%, 20%, 10%, 5%, 4%, or 2% of the thickness of conductive layer 106. Similarly, the ratio of the thickness of oxide-containing layer 108 to the thickness of conductive layer 106 may be no more than 7:10, 3:5, 1:2, 2:5, 1:3, 1:5, 1:10, 1:20, 1:25, or 1:50.
[0040] Although the conductive film 104 may include individual, discrete layers in the form of the conductive layer 106 and the oxide-containing layer 108, in some embodiments, the individual layers may not be divided from each other by a clear boundary. For example, in some embodiments, the conductive layer 106 and the oxide-containing layer 108 may be connected by a connecting portion of material, and the connecting portion includes an oxide transition gradient from the conductive layer 106 to the oxide-containing layer 108. Therefore, the connecting portion may be substantially composed of a conductive material (e.g., palladium) at a location close to the conductive layer 106, and may contain a higher amount of oxide (e.g., palladium oxide) as the connecting portion transitions away from the conductive layer 106 to a location closer to the oxide-containing layer 108.
[0041] Conductive film 104 can be formed on substrate 102 so that the resulting electrode 100 can have a sheet resistance of at least 0.1, 0.5, 1, 5, or 10 ohms / square and / or no more than 200, 100, 50, 35, or 15 ohms / square as measured by ASTM F1711-96. In some embodiments, the resulting electrode 100 can have a sheet resistance of 0.1 to 200 ohms / square, 0.5 to 100 ohms / square, 1 to 50 ohms / square, 5 to 35 ohms / square, or 10 to 15 ohms / square.
[0042] Embodiments of the present invention configure the conductive layer 106 of the conductive film 104 to be substantially composed of metal. In some embodiments, the metal of the conductive layer 106 can be a noble metal, such as palladium. As readily understood by those skilled in the art, although the conductive layer 106 can be substantially composed of palladium, the conductive layer 106 can contain incidental impurities. As used herein, "incidental impurities" refers to any impurities that naturally occur in the ore used to produce the metal or are added unintentionally during the production process. The conductive layer 106 may contain less than about 0.1, 0.05, or 0.001% by weight of incidental impurities in some embodiments.
[0043] The oxide-containing layer 108 may include a material including an oxide of the metal forming the conductive layer 106. Thus, for example, the oxide-containing layer 108 may include palladium oxide. The amount of oxide in the oxide-containing layer 108 may vary. For example, in some embodiments, the amount of oxide in the oxide-containing layer 108 may be at least 40%, at least 50%, at least 60%, at least 70%, at least 80%, at least 90%, at least 95%, or at least 99% by weight of the oxide-containing layer 108. Additionally, the amount of oxide in the oxide-containing layer 108 may be 40 to 99%, 60 to 95%, or 80 to 90% by weight.
[0044] To form electrode 100, embodiments of the present invention generally provide conductive layer 106 and oxide-containing layer 108 to be formed on substrate 102 via physical vapor deposition by performing the following steps:
[0045] (a) providing a substrate;
[0046] (b) providing a target;
[0047] (c) depositing material from the target onto a substrate in an inert atmosphere, thereby forming a conductive layer on the substrate, the conductive layer consisting essentially of the material from the target; and
[0048] (d) depositing a material from the target onto the conductive layer in an atmosphere containing an oxidant, thereby forming an oxide-containing layer on the conductive layer, the oxide-containing layer comprising an oxide of the material from the target.
[0049] Step (a) providing the substrate can include providing any type of substrate material as described above, such as PET. In certain embodiments, the substrate will include a sheet of substrate material that can be placed in a high vacuum chamber. The sheet of substrate material can include a single fragment of material, such as a square sheet. In some other embodiments, the sheet of substrate material can include a roll of material that is passed through a high vacuum chamber via a roll-to-roll mechanism, as described in more detail below. In some embodiments, the substrate can remain fixed, and in other embodiments, the substrate can rotate during the deposition process.
[0050] Step (b) providing a target may include providing a physical vapor deposition target, which may include any of the previously described conductive materials. The target may be provided in a vacuum chamber in which a substrate is also provided. In some specific embodiments, the target may be substantially composed of palladium. Such a target may contain less than about 0.1, 0.05 or 0.001% by weight of incidental impurities. In some embodiments, the target will be contained in an electrode and / or will include an electrode, such as a sputtering cathode, during the physical vapor deposition process. In certain embodiments, the target may be circular, tubular, rectangular, and the like. However, it should be understood that embodiments of the present invention contemplate the use of targets of other shapes, such targets having various sizes as may be desired.
[0051] The depositing of step (c) generally comprises forming material from the target on the substrate in an inert atmosphere to form a conductive layer. Similarly, the depositing of step (d) generally comprises forming material from the target on the conductive layer in an oxidant-containing atmosphere to form an oxide-containing layer.
[0052] The term "physical vapor deposition" as used herein means depositing a thin film by setting a vaporized material to condense onto a surface (e.g., a substrate). Physical vapor deposition coating can be performed using any type of physical vapor deposition method, such as sputtering coating, thermal evaporation, electron beam evaporation, arc evaporation, co-evaporation, ion plating, and the like. For example, in some embodiments, the physical vapor deposition step will be performed via a sputtering method, wherein the substrate is plated with a conductive layer and the conductive layer is plated with an oxide-containing layer by sputtering a target in an inert atmosphere and in an oxidant-containing atmosphere, respectively, via a sputtering device. Although the oxide-containing layer 108 of the electrode 100 can be manufactured by physical vapor deposition (e.g., sputtering), embodiments can configure the oxide-containing layer 108 to be manufactured by other methods, such as corona treatment, oxygen plasma, chemical oxidation, ion-assisted oxidation, and the like. Therefore, when the oxide-containing layer 108 is described herein as being "manufactured", such manufacturing can be performed via the above methods and procedures (e.g., sputtering, corona treatment, oxygen plasma, chemical oxidation, ion-assisted oxidation, and the like).
[0053] In some embodiments, the deposition of steps (c) and (d) can be carried out in a single zone vacuum chamber. For example, for the deposition of step (c), the vacuum chamber can initially reach a vacuum and be filled with a rare gas such as argon so that the conductive layer can be deposited on the substrate by sputtering a palladium target. In some embodiments, the deposition of step (c) can be carried out by a sputtering system operating at a power of 2 to 70 kW, 7 to 35 kW, or about 8 kW. Then, after an oxidant is added to the chamber to generate a rare gas and an oxidant mixture, the deposition of step (d) can be carried out in the same vacuum chamber so that the oxide-containing layer can be deposited on the conductive layer. The oxidant used can be changed, but can include oxygen, water, ozone, etc. In certain embodiments, the oxidant can account for 0.5 to 40%, 1 to 20%, 2 to 10%, 4 to 6%, or about 5% of the second atmosphere by partial pressure. The amount of oxide contained in the electrode has been shown to be controllable by controlling the amount of the oxidant in the rare gas and oxidant mixture. It has also been determined that the amount of oxide contained in the electrode can be controlled by controlling the amount of time used to deposit the oxide-containing layer during the deposition process of step (d). In some embodiments, the deposition of step (d) can be performed by a sputtering system operating at a power of 2 to 70 kW, 7 to 35 kW, or about 8 kW. Certain embodiments can set the ratio of the sputtering power used during the sputtering of step (c) (i.e., for depositing the conductive layer) and the sputtering of step (d) (i.e., for depositing the oxide-containing layer) to about 2:1, about 3:1, about 4:1, about 5:1, about 6:1, about 7:1, about 8:1, about 9:1, or about 10:1.
[0054] As an alternative to a single-zone vacuum chamber, in some embodiments, the deposition of steps (c) and (d) can be performed in at least two different zones of a vacuum chamber (e.g., a dual-zone vacuum chamber). For example, such embodiments can be performed by a roll-to-roll physical vapor deposition method, which includes roll-to-roll magnetron sputtering. Initially, the substrate can be provided to a first vacuum chamber zone, which includes a first target placed therein. For the deposition of step (c), the first vacuum chamber zone can be filled with a rare gas such as argon so that the conductive layer can be deposited on the substrate by sputtering the substrate with the material from the first target in the first chamber zone. Subsequently, the substrate coated with the conductive layer deposited thereon can be transferred to a second vacuum chamber zone having a second target placed therein. In some embodiments, the first and second targets can be the same material. Subsequently, the deposition of step (d) can be performed in the second vacuum chamber zone, which is filled with a mixture of a rare gas and an oxidant so that an oxide-containing layer can be deposited on the conductive layer.
[0055] Whether a single zone vacuum chamber or a dual zone vacuum chamber is used, the resulting substrate having a conductive layer and an oxide-containing layer formed thereon can be prepared in the form of a thin film sheet that can be cut to a certain size and used as an electrochemical electrode, such as for a biosensor. Such electrodes can include a working electrode, a reference electrode, or a counter electrode. Specifically, the resulting thin film sheet can be cut to a suitable size to form an electrochemical electrode having a size particularly suitable for a biosensor. In other embodiments, an electrochemical electrode can be formed from a thin film sheet by etching such as chemical or laser etching (or ablation). In yet other embodiments, an electrochemical electrode can be formed using a patterned mask, which is laid on a substrate, and a conductive layer and an oxide-containing layer are physically vapor deposited thereon to form an electrode.
[0056] As previously described above, the electrode formed according to an embodiment of the present invention (which includes a conductive layer formed as a palladium metal layer and an oxide-containing layer formed as a palladium oxide-containing layer) can exhibit desirable electrochemical properties and can withstand the effects of atmospheric aging. Therefore, the electrode according to an embodiment of the present invention is particularly well suited as a replacement for biosensors incorporating pure precious metals (such as palladium and / or gold). In particular, it has been found that the palladium oxide-containing layer formed on the palladium metal layer can limit additional oxidation and surface modification of the electrode, so that the electrode can be formed to reduce or minimize the effects of atmospheric aging (such as further oxidation). It has been found that the extent to which the electrode can withstand atmospheric aging is related to the amount of palladium oxide formed on the electrode surface. For example, an electrode with a higher oxide surface coverage is more resistant to atmospheric aging than an electrode with a lower oxide surface coverage. However, it should be understood that there is a maximum beneficial amount of oxide surface coverage for the electrode, because too much oxide in the electrode may reduce the conductivity of the electrode to below an operable level. The embodiments of the present invention control the amount of palladium oxide on the electrode surface by controlling the amount of oxidant added to the deposition atmosphere during the deposition of the palladium oxide-containing layer and / or by controlling the deposition time for depositing the palladium oxide-containing layer. In other embodiments incorporating other methods for forming the palladium oxide-containing layer (e.g., corona treatment, oxygen plasma, chemical oxidation, ion-assisted oxidation, etc.), the amount of palladium oxide in the electrode can be controlled by controlling various parameters of such other methods (e.g., treatment time).
[0057] In view of the above, it has been determined that the stability of electrodes formed according to embodiments of the present invention (i.e., the ability to withstand the effects of atmospheric aging) can be quantified by the amount of oxide formed on the electrode surface. For palladium-based electrodes, the amount of palladium oxide on the electrode surface can be determined by measuring the amount and / or rate at which MESA remains on the electrode surface after the electrode is plated with mercaptoethanesulfonate (MESA). In particular, it has been determined that the rate at which MESA attaches to the electrode surface decreases with the oxide surface coverage of the electrode. Thus, a palladium electrode having a high amount of palladium oxide on its surface will allow a lower amount of MESA to attach to the electrode surface when plated with MESA over a given plating time period. In contrast, a palladium electrode having a low amount of palladium oxide on its surface will allow a higher amount of MESA to attach to the electrode when plated with MESA over a given time period. Thus, (1) the rate at which MESA is plated on the electrode (i.e., MESA kinetics) and (2) the surface coverage of MESA on the electrode after plating in MESA for a given time period (i.e., MESA coverage) are each inversely proportional to the surface oxidation of the electrode.
[0058] In order to make the electrode stable and withstand the influence of atmospheric aging, the electrode should have a consistent oxide surface coverage as the electrode life passes. Whenever such an electrode is coated with MESA, the electrode will have consistent MESA dynamics. On the other hand, when an electrode that is unstable and cannot withstand the influence of atmospheric aging is exposed to the atmosphere, the oxide surface coverage of the electrode will increase as the electrode life passes. As mentioned above, the MESA dynamics of the electrode are known to decrease with the electrode oxide surface coverage that is increased. Therefore, an electrode with unstable atmosphere will have a MESA dynamics that decreases as the electrode life passes. In contrast, an electrode with stable atmosphere will have a MESA dynamics that is substantially stable as the electrode life passes.
[0059] Electrodes formed according to embodiments of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) are shown to be atmospherically stable. For example, within 10 days of forming the palladium layer and the palladium oxide-containing layer, when the electrode is plated in MESA via a MESA coating procedure (as defined below), an electrode formed according to embodiments of the present invention can be configured to receive a specific fractional coverage (fractional coverage A) of MESA as determined by a Type 1 MESA Coverage Test (as defined below) on the outer surface of the electrode. In addition, between 10 and 90 days after forming the palladium metal layer and the palladium oxide-containing layer, when the electrode is plated in MESA via a MESA coating procedure, the electrode is configured to receive an additional fractional coverage (fractional coverage B) of MESA as determined by a Type 1 MESA Coverage Test on the outer surface of the electrode. Embodiments of the present invention set fractional coverage A to deviate from fractional coverage B by no more than 30%, 20%, 15%, 10%, 7%, 6%, 5%, 4%, 3, or 2%.
[0060] In various embodiments, when plated with MESA via a MESA coating procedure, an electrode formed according to embodiments of the present invention is configured to receive a specific fractional coverage of MESA on the outer surface of the electrode as determined by a Type 1 MESA Coverage Test. In contrast, when a baseline electrode (defined herein as an electrode formed substantially of a palladium metal layer sputtered to a thickness of at least 10 nm on a substrate in an inert atmosphere and aged for at least 90 days in an ambient atmosphere) is plated in MESA via a MESA coating procedure, the baseline electrode is configured to receive a baseline fractional coverage of MESA on the outer surface of the baseline electrode as determined by a Type 1 MESA Coverage Test. The electrodes of the present invention are configured such that within 10 days of forming the palladium metal layer and the palladium oxide-containing layer, the specific fractional coverage of MESA on the electrode deviates by no more than 25%, 20%, 15%, 10%, or 5% higher and / or 50%, 40%, 30%, 20%, or 10% lower than the baseline fractional coverage of MESA on the baseline electrode.
[0061] Although it is beneficial that the electrodes formed according to embodiments of the present invention are atmospherically stable so that they can withstand the effects of atmospheric aging, it is also important that the electrodes have suitable electrochemical performance. As will be shown in the following examples, electrodes formed according to embodiments of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) are shown to be electrochemically similar to electrodes formed essentially of noble metals (such as pure palladium electrodes). Specifically, electrodes formed according to embodiments of the present invention have heterogeneous electron transfer or conductivity similar to conventional electrodes (such as pure palladium electrodes). However, although the electrodes are electrochemically similar to other conventional electrodes, it has been found that the electrodes of the present invention have different oxide structures on their surfaces, so that the reduction wave of the electrode produces characteristics different from the reduction wave of the conventional electrode. For example, the electrode formed according to an embodiment of the present invention is configured to have a reduction peak determined by a Type 1 cyclic voltammetry test that is more biased toward the cathode by at least 10 mV than the reduction peak determined by a Type 1 cyclic voltammetry test for a baseline electrode.
[0062] The present invention may be further illustrated by the following examples of embodiments of the present invention, but it is to be understood that these examples are included for illustrative purposes only and are not intended to limit the scope of the present invention unless otherwise specifically stated. Example
[0063] Preparation of thin film electrodes
[0064] For each of the following examples, the electrode was formed by one of the following physical vapor deposition methods. Therefore, it is understood that the electrode of the present embodiment can be formed using the following method to include a conductive layer of palladium metal formed on a substrate, and an oxide-containing layer including palladium oxide formed on the conductive layer. The single-zone vacuum chamber method includes forming an electrode thin film sheet by performing the following steps:
[0065] (a) A palladium metal layer was deposited on a 10.16 cm x 10.16 cm square sheet of PET substrate using direct current ("DC") magnetron sputtering in a high vacuum chamber, the sputtering being performed using a Denton Vacuum Desktop Pro sputtering apparatus.
[0066] i. Evacuate the vacuum chamber to ~10 -5 Initial base pressure in mTorr;
[0067] ii. Introduce 10 sccm of argon gas into the high vacuum chamber to produce a deposition pressure of 5 mTorr;
[0068] iii. rotating the substrate sheet within the vacuum chamber at approximately two revolutions per minute;
[0069] iv. maintaining a 5.08 cm diameter palladium target in a pure argon atmosphere under a DC magnetron sputtering device at a constant power of 40 watts for a deposition time of 4 minutes to coat at least a portion of the substrate sheet with a conductive palladium metal layer (to initialize the target, the target was maintained under a DC magnetron sputtering device at a constant power of 40 watts for a pre-sputtering time of 5 minutes before the substrate was introduced into the vacuum chamber);
[0070] (b) depositing a palladium oxide-containing layer on the palladium metal layer by a sputtering device—
[0071] i. introducing a gas mixture of 10 sccm of oxygen and argon into the high vacuum chamber to produce a deposition pressure of 5 mTorr;
[0072] ii. rotating the substrate sheet within the vacuum chamber at approximately two revolutions per minute;
[0073] iii. sputtering the palladium target in an oxygen and argon atmosphere under a DC magnetron sputtering apparatus at a constant power of 40 watts for a deposition time of 1 minute to coat at least a portion of the palladium metal layer with a palladium oxide-containing layer; and
[0074] (c) All depositions were performed at room temperature (i.e., 25 °C).
[0075] In addition to the single zone vacuum chamber method, certain electrodes of embodiments of the present invention (which are described in the examples below) are formed using a roll-to-roll device via a dual zone vacuum chamber method. In more detail, the dual zone vacuum chamber method is similar to the above method, except that two palladium targets are used, one in each vacuum chamber zone. In addition, pure argon is pumped into the first zone to begin forming the electrode film sheet by depositing a palladium metal layer on a substrate. Subsequently, the electrode film sheet is transferred (roll-to-roll) to the second zone. Oxygen is supplied to the second zone to produce an argon / oxygen mixture for depositing a palladium oxide layer on the palladium metal layer.
[0076] Thus, an electrode film sheet comprising a palladium metal layer on a substrate and a palladium oxide-containing layer on the palladium metal layer is formed. Individual electrodes with a size of 5.08 cm × 7.62 cm are cut from the electrode film sheet, whether using a single-zone vacuum chamber method or a double-zone vacuum chamber method. As described in detail below, some electrodes have their electrochemical properties tested via a potentiostat. In addition, some electrodes are tested after further plating with 2-mercaptoethanesulfonate ("MESA") as described in more detail below.
[0077] The electrochemical experiments were performed using a Gamry Instruments Reference 600 potentiostat in a three-electrode configuration, and the electrochemical cell contained a thin film electrode membrane located inside a Gamry Instruments VistaShield Faraday cage. The thin film electrodes were each formed as working electrodes by partially masking the thin film electrodes with a plating tape having a single 3 mm diameter orifice punched into it. Thus, the unmasked portion of the thin film electrode provided a geometric working electrode surface area of 0.0707 square centimeters. The unmasked portion of the thin film electrode served as an electrical connection point with the working electrode lead of the potentiostat. The masked portion of the thin film electrode was placed on a flat support block of a non-conductive material such as plastic. The thin film electrode was then placed in the working electrode port of a glass electrochemical cell. The exposed 3 mm diameter portion of the thin film electrode was placed near the center of the bottom opening of the working electrode port of the electrochemical cell. The working electrode port of the electrochemical cell was sealed with a clamp and an O-ring. The electrochemical cell also contained a reference electrode, which included a saturated calomel reference electrode and a carbon auxiliary electrode. The reference electrode and the auxiliary electrode were placed in the reference electrode port and the auxiliary electrode port, respectively. Additionally, a reference electrode and an auxiliary electrode are connected to the reference lead and the auxiliary lead of the potentiostat, respectively. The electrochemical cell also includes a gas flow port whereby the test solution is degassed and blanketed with an inert gas such as nitrogen.
[0078] Description of Type 1 Cyclic Voltammetry Test
[0079] Some of the following embodiments were performed using a Type 1 cyclic voltammetry test defined as follows: 50 ml of a potassium phosphate buffer solution ("PBS") containing 145 mM sodium chloride at pH 7.1 was placed in an electrochemical cell and sealed with a stopper. Alternatively, 50 ml of 0.1 M potassium chloride can be used for the PBS. Using a medium porous filter stick, via a nitrogen flow, gas inlet and outlet fittings (which are associated with a gas flow port) enable the PBS to be bubbled with an inert gas (i.e., degassed). The gas flow port also enables the gas flow to be switched from the filter stick to a headspace cover setting. The gas outlet is connected to an oil bubbler to prevent external gases (e.g., air) from back-diffusion into the electrochemical cell. The PBS was stirred with a magnetic stirring bar while bubbling with nitrogen for at least 5 minutes, after which the gas flow was switched to a cover configuration. The solution was not stirred (from bubbling or otherwise) during the electrochemical test performed, that is, the PBS was stationary during the electrochemical test.
[0080] Cyclic voltammetry was performed on a thin film electrode forming the working electrode in the electrochemical cell. The initial voltage potential for type 1 cyclic voltammetry was 0 V relative to an open circuit (i.e., resting potential) as measured between the working electrode and a reference electrode (i.e., saturated calomel reference electrode) after a rest period of at least 10 seconds before the test. The voltage potential was first scanned cathodically at a scan rate of 25 mV per second, followed by a scan of the anodic potential.
[0081] Description of Type 2 Cyclic Voltammetry Test
[0082] Type 2 cyclic voltammetry tests were performed in the same manner as Type 1 cyclic voltammetry tests, except that 50 mL of 0.1 M sodium hydroxide was used instead of PBS.
[0083] Description of Type 3 Cyclic Voltammetry Test
[0084] The experimental setup for the Type 3 cyclic voltammetry test was similar to that for the Type 1 cyclic voltammetry test, except that 1 mM Fe[III](CN)6 was added to PBS as a redox mediator. In addition, the procedure for the Type 3 cyclic voltammetry test was as follows:
[0085] (1) The initial potential of the film electrode is 0 V relative to the open circuit potential (i.e., static potential);
[0086] (2) the potential of the film electrode is scanned cathodically at 25 mV per second to a potential of -0.3 V (relative to the reference electrode); and
[0087] (3) The potential of the thin film electrode was scanned anodically at 25 mV per second to a potential of approximately 1 V (relative to the reference electrode).
[0088] Description of Type 4 Cyclic Voltammetry Test
[0089] The experimental setup for type 4 cyclic voltammetry test was similar to that for type 1 cyclic voltammetry test, except that 2 mM 3(2',5'-disulfophenylimino)-3H-phenothiazine was added to PBS.
[0090] Application of Type 1 Cyclic Voltammetry
[0091] Figure 4 Test
[0092] Figure 4 Results of three electrodes subjected to a Type 1 cyclic voltammetry test are shown. The first electrode (pure Pd) and the second electrode (pure Pd11) were each formed by sputtering a palladium target in a pure argon atmosphere, without introducing oxygen during the sputtering process. Thus, the first electrode and the second electrode are substantially formed by a palladium metal layer on a substrate. The first electrode was not atmospherically aged and immediately subjected to a Type 1 cyclic voltammetry test. The second electrode was atmospherically aged for 11 months and then subjected to a Type 1 cyclic voltammetry test. Figure 4Also shown is a third electrode (PdO 10%), which is an electrode formed according to an embodiment of the present invention. In particular, the third electrode is formed by sputtering a palladium target in a pure argon atmosphere for four minutes to generate a palladium metal layer on a substrate. In addition, a third electrode having a palladium oxide layer on a palladium metal layer is formed by sputtering a palladium target in an argon / oxygen atmosphere mixture containing 10% oxygen for 1 minute. It should be understood that in the various examples described herein, the specific oxygen percentage is measured in partial pressure of the total pressure of the argon / oxygen atmosphere in the vacuum chamber. The third electrode was not atmospherically aged and was immediately subjected to a Type 1 cyclic voltammetry test.
[0093] Because the second electrode was atmospherically aged for 11 months, the second electrode reacted with the atmosphere to generate an atmospherically generated palladium oxide layer on the outer surface of the palladium metal layer. In contrast, because the first electrode was not aged, the first electrode did not include a palladium oxide layer (which contained as much oxide as the second electrode), as shown in FIG. Figure 4 As indicated in the electrochemical analysis shown in . Figure 4 As shown, the reduction wave of the second electrode is significantly larger than the reduction wave of the first electrode, thereby indicating that the palladium oxide layer on the surface of the palladium conductive layer changes the electrochemical response of the electrode when performing a type 1 cyclic voltammetry test. In addition, the reduction wave of the third electrode is shown to be significantly larger than that of the first electrode, and it is also found to have a peak that is significantly shifted in the cathode direction relative to the first electrode and the second electrode. Unexpectedly, the reduction wave of the third electrode (whose palladium oxide layer is generated during the sputtering process) is significantly different (i.e., has a cathode shift peak) from the reduction wave of the second electrode (whose palladium oxide layer is naturally generated during atmospheric aging). Such differences indicate different oxide structures on the surfaces of the corresponding electrodes.
[0094] Figure 5 Test
[0095] Figure 5 Again, as before Figure 4 The results of the three electrodes (i.e. pure Pd, pure Pd11 and PdO 10%) subjected to type 1 cyclic voltammetry are shown in FIG. Figure 5 Also shown is a fourth electrode (PdO EC) subjected to a Type 1 cyclic voltammetry test. The fourth electrode is formed by sputtering a palladium target in a pure argon atmosphere, without introducing oxygen during the sputtering process. Thus, the fourth electrode is initially substantially formed of a palladium metal layer on a substrate. However, before conducting a Type 1 cyclic voltammetry test, the fourth electrode is first anodic scanned to 1.1 V in order to electrochemically generate a palladium oxide-containing layer on the surface of the palladium metal layer.
[0096] like Figure 5As shown, the reduction wave of the fourth electrode is significantly larger than the reduction waves of the other electrodes. Unexpectedly, the reduction wave of the third electrode (PdO 10%) (whose palladium oxide layer is generated during sputtering) is significantly different from the characteristics of the reduction wave of the fourth electrode (whose palladium oxide layer is electrochemically generated during the anodic scanning process). Such differences indicate different oxide structures on the surfaces of the corresponding electrodes.
[0097] Figure 6 Test
[0098] Figure 6 The results of four electrodes subjected to type 2 cyclic voltammetry tests are shown. The first electrode (pure Pd) is formed in a roll-to-roll coating machine having a first zone and a second zone. The first electrode is passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode. Subsequently, the first electrode is passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. The first zone and the second zone are each filled with an atmosphere consisting essentially of argon (i.e., an inert gas) so that the first electrode is formed by sputtering a palladium target in each of the first and second zones, and oxygen is not introduced during the sputtering process. Thus, the first electrode is substantially formed by a palladium metal layer on a substrate. The second electrode (PdO 1%), the third electrode (PdO 5%), and the fourth electrode (PdO 10%) are each electrodes formed according to an embodiment of the present invention. Specifically, the second electrode, the third electrode, and the fourth electrode are formed in a roll-to-roll coating machine, wherein the first zone provides a pure argon atmosphere and the second zone provides a mixed atmosphere of argon / oxygen. Thus, the second electrode, the third electrode, and the fourth electrode are each passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode. Subsequently, the electrode is passed through the second district to deposit the remaining 20% of the conductive film thickness of the electrode. In more detail, the second electrode, the third electrode and the fourth electrode are each formed by sputtering a palladium target in the first district containing a pure argon atmosphere so as to deposit a palladium metal layer on a substrate. Then, each second electrode, the third electrode and the fourth electrode having a palladium oxide layer on the palladium metal layer are formed by sputtering a palladium target in the second district containing an atmosphere containing a mixture of argon and oxygen. Specifically, the second electrode is sputtered in an argon / oxygen atmosphere containing 1% oxygen. The third electrode is sputtered in an argon / oxygen atmosphere containing 5% oxygen. The fourth electrode is sputtered in an argon / oxygen atmosphere containing 10% oxygen. Each electrode is then aged for sixty days by atmosphere, and then a type 2 cyclic voltammetry test is performed.
[0099] Figure 6It is shown that the reduction wave of the electrode sputtered in an argon / oxygen atmosphere with a higher oxygen concentration is significantly different from that of the electrode sputtered in an argon / oxygen atmosphere with a lower oxygen concentration or no oxygen concentration. For example, the second electrode (i.e., PdO 1%) has a reduction wave similar to that of the first electrode (i.e., pure Pd). In contrast, the third electrode (i.e., PdO 5%) and the fourth electrode (i.e., PdO 10%) have reduction waves that are significantly larger than the first and second electrodes and have peaks that are shifted in a more cathodic direction. In addition, as described above, each of the electrodes was atmospherically aged for 60 days after sputtering. Figure 6 The results were unexpected because the reduction wave of the electrodes formed according to the embodiments of the present invention (e.g., PdO 1%, PdO 5%, and PdO 10%) did not convert back to the electrochemical response of the electrode substantially formed of a palladium metal layer (e.g., pure Pd) that was also subjected to atmospheric aging even after atmospheric aging.
[0100] Figure 7 Test
[0101] Figure 7 The results of two electrodes subjected to a Type 1 cyclic voltammetry test are shown. The first electrode (PdO 1m) and the second electrode (PdO 2m) are each electrodes formed according to an embodiment of the present invention. Specifically, the first electrode is formed by sputtering a palladium target in a pure argon atmosphere for four minutes to generate a palladium metal layer on a substrate. Subsequently, a first electrode having a palladium oxide layer on the palladium metal layer is formed by sputtering a palladium target in an atmosphere of an argon / oxygen mixture containing 10% oxygen for one minute. The second electrode is formed by sputtering a palladium target in a pure argon atmosphere for three minutes to generate a palladium metal layer on a substrate. Subsequently, a second electrode having a palladium oxide layer on the palladium metal layer is formed by sputtering a palladium target in an atmosphere of an argon / oxygen mixture containing 10% oxygen for two minutes. The electrodes were not allowed to undergo significant atmospheric aging before conducting a Type 1 cyclic voltammetry test. Figure 7 It is shown that the reduction waves of the electrodes are different, which indicates that the surface structures of the palladium oxide-containing layers on the electrodes are different. Specifically, Figure 7 It is shown that the thickness of the palladium oxide-containing layer on the electrode can be controlled by the deposition time in an argon / oxygen atmosphere.
[0102] Figure 8 Test
[0103] Figure 8Results of three electrodes subjected to a Type 3 cyclic voltammetry test are shown. The first electrode (pure Pd) is formed in a roll-to-roll coater having a first zone and a second zone. The first electrode is passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode. Subsequently, the first electrode is passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. The first zone and the second zone are each filled with an atmosphere consisting essentially of argon (i.e., an inert gas) so that the first electrode is formed by sputtering a palladium target in each of the first and second zones, without introducing oxygen during the sputtering process. Thus, the first electrode is essentially formed by a palladium metal layer on a substrate. The second electrode and the third electrode are each formed in a roll-to-roll coater, wherein the first zone provides a pure argon atmosphere and the second zone provides a mixed atmosphere of argon / oxygen. Thus, the second electrode and the third electrode are each passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode, and then passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. In more detail, the second electrode (PdO 1%) was formed by sputtering a palladium target in a first zone containing a pure argon atmosphere to generate a palladium metal layer on a substrate. In addition, a second electrode having a palladium oxide layer on the palladium metal layer was formed by sputtering a palladium target in a second zone containing an argon / oxygen atmosphere mixture containing 1% oxygen. The third electrode was formed by sputtering a palladium target in a first zone containing a pure argon atmosphere to generate a palladium metal layer on a substrate. In addition, a third electrode having a palladium oxide layer on the palladium metal layer was formed by sputtering a palladium target in a second zone containing an argon / oxygen atmosphere mixture containing 10% oxygen. None of the electrodes were atmospherically aged before performing a Type 3 cyclic voltammetry test.
[0104] Figure 8 It was shown that an electrode formed according to an embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) behaves electrochemically similar to a pure palladium electrode in the presence of a common redox mediator (e.g., FeIII / II(CN)6 in 0.1 M KCl). Because palladium oxide is a semiconductor and is relatively non-conductive, it is surprising that covering the electrode with a relatively semiconductor has no effect on the electrochemical performance of the electrode.
[0105] Fig. 9 Test
[0106] Fig. 9Results of four electrodes subjected to a Type 4 cyclic voltammetry test are shown. The first electrode (pure Pd10) is formed in a roll-to-roll coater having a first zone and a second zone. The first electrode is passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode. Subsequently, the first electrode is passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. The first zone and the second zone are each filled with an atmosphere consisting essentially of argon (i.e., an inert gas) so that the first electrode is formed by sputtering a palladium target in each of the first and second zones, and no oxygen is introduced during the sputtering process. Thus, the first electrode is substantially formed by a palladium metal layer on a substrate. The first electrode is then atmospherically aged for 90 days and then subjected to a Type 4 cyclic voltammetry test. The second electrode, the third electrode, and the fourth electrode are each formed in a roll-to-roll coater, wherein the first zone provides a pure argon atmosphere and the second zone provides a mixed atmosphere of argon / oxygen. Thus, the second electrode, the third electrode, and the fourth electrode are each passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode, and then passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. In more detail, the second electrode (PdO 1%) is formed by sputtering a palladium target in a first zone containing a pure argon atmosphere to generate a palladium metal layer on a substrate. In addition, a second electrode having a palladium oxide layer on a palladium metal layer is formed by sputtering a palladium target in a second zone containing an argon / oxygen atmosphere mixture containing 1% oxygen. The third electrode (PdO 5%) is formed by sputtering a palladium target in a first zone containing a pure argon atmosphere to generate a palladium metal layer on a substrate. In addition, a third electrode having a palladium oxide layer on a palladium metal layer is formed by sputtering a palladium target in a second zone containing an argon / oxygen atmosphere mixture containing 5% oxygen. The fourth electrode (PdO 10%) is formed by sputtering a palladium target in a first zone containing a pure argon atmosphere to generate a palladium metal layer on a substrate. In addition, a fourth electrode having a palladium oxide layer on a palladium metal layer is formed by sputtering a palladium target in a second zone containing an argon / oxygen atmosphere mixture containing 10% oxygen. None of the second, third, or fourth electrodes were atmospherically aged before performing a Type 4 cyclic voltammetry test.
[0107] Fig. 9 It was shown that an electrode formed according to an embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) behaved electrochemically similarly to a pure palladium electrode that had been atmospherically aged in the presence of a common redox mediator (e.g., 3(2',5'-disulfophenylimino)-3H-phenothiazine in PBS buffer. Because palladium oxide is a semiconductor and is relatively non-conductive, it is surprising that covering the electrode with a relatively semiconductor has no effect on the electrochemical performance of the electrode.
[0108] Description of the MESA coating process
[0109] In addition to the beneficial electrochemical properties, the electrodes formed according to the embodiments of the present invention are configured to withstand atmospheric aging due to the new oxide-containing layer formed on the electrode surface. As discussed above, the extent of the oxide surface coverage of the electrode can be quantified by measuring the MESA coating properties of the electrode. In order to measure the MESA coating properties, the electrode can be MESA-plated according to the following MESA coating procedure. It should be understood that the following MESA coating procedure is similar in some respects to the procedure described by Macfie et al.: Mechanism of 2-Mercaptoethanesulphonate Adsorption onto Sputtered Palladium Films: Influence of Surface Oxide Species, The Journal of Physical Chemistry C 2012, 116, 9930-9941 (hereinafter referred to as Macfie), the entire contents of which are incorporated herein by reference.
[0110] The first step of the MESA coating procedure involves providing a 500 ml beaker containing ~200 ml of a 0.3 mM MESA solution in Milli-Q water. The solution was gently stirred using a magnetic stirrer and a 10.16 cm × 10.16 cm electrode film was placed in the solution for 500 seconds. The electrode film was removed, immediately washed with water and ethanol, and air dried. The electrode was cut from the electrode film to a size of 5.08 cm × 7.62 cm. The electrode was then placed in a 1.0 mM 1-dodecanethiol solution in ethanol for 16 hours. The electrode was then removed, rinsed with ethanol, dried, and tested for analysis.
[0111] Description of Type 1 MESA Coverage Test
[0112] The extent of surface MESA coating was calculated using a method similar to that described in Macfie. In more detail, the electrodes coated with MESA were subjected to type 3 voltammetry. The voltage difference between the cathode peak and the anodic peak of the electrode was then measured. In particular, the voltage at the Fe III / II with Fe II / III Redox couple (∆E 峰值 ) between the peak currents (splitting). Therefore, ∆E is used in the following equation 峰值 The surface coverage of the MESA portion on the electrode (hereinafter defined as "MESA coverage") was determined.
[0113]
[0114] Description of the Type 1 MESA Kinetic Test
[0115] The rate of MESA uptake on the electrode surface (hereinafter defined as MESA kinetics) was calculated for each electrode by obtaining the MESA coverage as calculated from the Type 1 MESA Coverage Test and dividing the coverage value by the amount of time the electrode film was placed in the MESA solution for coating (i.e., 500 seconds as described in the MESA Coating Procedure).
[0116] Application of MESA Test
[0117] Fig.10 Test
[0118] Fig.10 Results of six groups of electrodes subjected to a Type 1 MESA coating test are shown. The first group (S1) of electrodes is formed in a roll-to-roll coater having a first zone and a second zone. Each of the electrodes in the first group is passed through the first zone to deposit 80% of the thickness of the conductive film of the electrode. Subsequently, each of the electrodes is passed through the second zone to deposit the remaining 20% of the thickness of the conductive film of the electrode. The first zone and the second zone are each filled with an atmosphere consisting essentially of argon (i.e., an inert gas) so that the first group of S1 electrodes is formed by sputtering a palladium target in each of the first and second zones, without introducing oxygen during the sputtering process. Thus, each electrode in group S1 is substantially formed by a palladium metal layer on a substrate. The remaining electrodes are formed in a roll-to-roll coater according to an embodiment of the present invention. In particular, each of the remaining electrodes is formed by sputtering a palladium target in a first zone containing a pure argon atmosphere so as to generate a palladium metal layer on a substrate. Each of such electrodes is sputtered in the first zone so that 80% of the thickness of the conductive film of the electrode is formed in the first zone. In addition, each of the remaining electrodes having a palladium oxide-containing layer on the palladium metal layer was formed by sputtering a palladium target in the second zone containing an argon / oxygen atmosphere mixture. Specifically, each of such electrodes was sputtered in the second zone so that the remaining 20% of the thickness of the conductive film of the electrode was formed in the second zone. For each of the remaining electrode groups, the oxygen percentage (by partial pressure) in the argon / oxygen atmosphere of the second zone was as follows:
[0119] S3 – 0.075%;
[0120] S5 – 0.25%;
[0121] S8 – 1.0%;
[0122] S9 – 2.0%;
[0123] S10 – 5.0%; and
[0124] S11 – 10.0%.
[0125] like Fig.10As shown in , electrodes from each group were subjected to the MESA coating procedure at different times between 7 days after sputtering and 90 days after sputtering. Subsequently, the electrodes were subjected to a Type 1 MESA coverage test to determine the MESA coverage on the electrodes. Fig.10 It is shown that the MESA coverage of the pure palladium electrode (i.e., S1) and the electrodes whose palladium oxide layer is formed at a low oxygen concentration (e.g., S3, S5, and S8) is significantly reduced over the first 90 days. In contrast, the electrodes whose palladium oxide layer is formed at a higher oxygen concentration (e.g., S9, S10, and S11) do not change significantly over the 90-day period after sputtering. Fig.10 The magenta line in the graph represents the MESA coverage of a separate, pure palladium electrode aged for 90 days prior to the MESA coating procedure and Type 1 MESA coverage test. As expected, the MESA coverage of the separate pure palladium electrode was consistent throughout the test period, and no further oxidation of the pure palladium electrode occurred during atmospheric aging. Unexpectedly, the electrode formed according to an embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) was more stable to atmospheric aging than a pure palladium film sputtered in a pure argon atmosphere.
[0126] Fig.11 Test
[0127] Fig.11 Shown from Fig.10 The same electrodes discussed in . However, Fig.11 Shown is the percent change in MESA coverage for each measurement obtained for a given electrode set, with such measurements starting at 7 days post-sputtering and ending at 90 days post-sputtering. Fig.11 It is shown that the pure palladium electrode group (i.e., S1) has a MESA coating reduction of about 50% between 7 days after sputtering and 90 days after sputtering. Such changes indicate a significant amount of surface oxidation of the pure palladium electrode during this period. In contrast, the MESA coating variation of the electrode formed according to the embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) is smaller. For example, the electrodes from groups S10 and S11 only changed by about 15% between 7 days after sputtering and 90 days after sputtering. Unexpectedly, the electrode formed according to the embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) is more stable to atmospheric aging than the pure palladium electrode sputtered in a pure argon atmosphere.
[0128] Fig.12 Test
[0129] Fig.12 Including from Fig.10 and 11 However, in Fig.12In the experiment, a type 1 MESA kinetic test was performed on the electrodes to obtain the MESA kinetic value of each electrode. Fig.12 It is shown that MESA dynamics change with electrode aging. Specifically, Fig.12 It is shown that the MESA kinetics of the pure palladium electrode (i.e., S1) and the electrodes whose palladium oxide layer is formed at low oxygen concentration (e.g., S3, S5, and S8) decrease within the first 90 days after sputtering. In contrast, the electrodes whose palladium oxide layer is formed at higher oxygen concentration (e.g., S9, S10, and S11) do not change significantly within 90 days after sputtering. The magenta line in the figure represents a separate palladium film that was aged for 90 days before measuring its MESA kinetics. Fig.12 It is shown that pure palladium electrodes and electrodes containing palladium oxide layers formed at low oxygen concentrations (e.g., S3, S5, and S8) achieve the same MESA kinetics as the palladium film alone aged for 90 days. Unexpectedly, electrodes formed according to embodiments of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) are more stable to atmospheric aging than pure palladium electrodes sputtered in a pure argon atmosphere.
[0130] Fig.13 Test
[0131] Fig.13 It is shown how the MESA kinetics of an electrode prepared according to an embodiment of the present invention (i.e., having a palladium metal layer formed by sputtering in an argon atmosphere and a palladium oxide-containing layer formed on the palladium metal layer by sputtering in an argon / oxygen mixture atmosphere) changes based on the concentration of oxygen in the argon / oxygen sputtering atmosphere. In particular, the electrodes were each subjected to a Type 1 MESA kinetic test 6 days after sputtering. Fig.13 It is shown that the MESA kinetics of the electrode can be adjusted by changing the oxygen concentration in the argon / oxygen atmosphere, and thus the degree of surface oxidation of the electrode. Unexpectedly, the degree of oxidation can be adjusted to control the kinetics of surface binding of molecules because the structure of the palladium oxide-containing layer is different from the structure of palladium oxide produced by the atmosphere.
[0132] Fig.14 Test
[0133] Fig.14Results of four electrodes subjected to type 3 cyclic voltammetry tests after MESA coating according to the MESA coating procedure are shown. The first electrode (pure Pd) and the second electrode (pure Pd10) are formed by sputtering a palladium target in a pure argon atmosphere, and no oxygen is introduced during the sputtering process. Thus, the first electrode and the second electrode are substantially formed by a palladium metal layer on a substrate. The first electrode is atmospherically aged for 1 day and then subjected to the MESA coating procedure. The second electrode is atmospherically aged for 90 days and then subjected to the MESA coating procedure. The third electrode (PdO 0.1%) is formed by sputtering a palladium target in a pure argon atmosphere for four minutes to generate a palladium metal layer on a substrate. In addition, a third electrode having a palladium oxide layer on a palladium metal layer is formed by sputtering a palladium target in an argon / oxygen atmosphere mixture containing 0.1% oxygen for one minute. The fourth electrode (PdO 10%) is formed by sputtering a palladium target in a pure argon atmosphere for four minutes to generate a palladium metal layer on a substrate. In addition, a fourth electrode having a palladium oxide layer on the palladium metal layer was formed by sputtering a palladium target in an argon / oxygen atmosphere mixture containing 10% oxygen for one minute. The third electrode and the fourth electrode were atmospherically aged for 1 day and subjected to a MESA coating procedure. Subsequently, each of the electrodes was subjected to a type 3 cyclic voltammetry test.
[0134] The MESA coating kinetics for each sample are shown in Table 1 below.
[0135] Table 1 – MESA coating dynamics
[0136] sample <![CDATA[MESA Coating Kinetics (s -1 )]]> Pd10 (90 days aging) <![CDATA[5.1×10 -6 ]]> <![CDATA[No O2]]> <![CDATA[6.2×10 -6 ]]> <![CDATA[0.1% O2]]> <![CDATA[5.2×10 -6 ]]> <![CDATA[10% O2]]> -
[0137] Fig.14 showed that the degree of oxidation on the electrode surface can be adjusted by changing the oxygen concentration in the argon / oxygen mixture atmosphere during sputtering. Fig.14 Table 1 demonstrates that an electrode formed according to an embodiment of the present invention (i.e., having a palladium metal layer formed on a substrate and a palladium oxide-containing layer formed on the palladium metal layer) can match the MESA plating kinetics of a pure palladium electrode aged for 90 days in the atmosphere. Unexpectedly, the palladium oxide-containing layer on the electrode of the present invention is indicative of the kinetics of small molecule surface binding to the surface because the structure of the palladium oxide-containing layer on the electrode of the present invention is different from the palladium oxide produced by the atmosphere.
[0138] The above detailed description of the embodiments of the present invention is intended to describe aspects of the present invention in sufficient detail to enable those skilled in the art to implement the present invention. Other embodiments may be adopted and may be changed without departing from the scope of the present invention. Therefore, the above detailed description should not be treated in a restrictive sense. The scope of the present invention is limited only by the claims presented in subsequent conventional utility applications and the full range of equivalents enjoyed by such claims.
[0139] In this specification, reference to "one embodiment", "an embodiment" or "an embodiment" means that one or more features mentioned are included in at least one embodiment of the technology. Separate references to "one embodiment", "an embodiment" or "an embodiment" in this specification do not necessarily refer to the same embodiment, and are not mutually exclusive unless so stated and / or unless it is obvious to a person skilled in the art from this specification. For example, features, steps, etc. described in one embodiment may also be included in other embodiments, but are not necessarily included. Thus, the technology can include various combinations and / or integrations of the embodiments described herein.
[0140] The inventors hereby declare their intention to rely on the doctrine of equivalents to determine and assess the fair and equitable scope of the present invention as it relates to any arrangements that do not materially depart from the present invention but are outside the literal scope of the present invention as set forth in the following claims.
[0141] definition
[0142] It should be understood that the following is not intended to be an exclusive list of defined terms.Other definitions may be provided in the foregoing specification, such as where context accompanies the use of a defined term.
[0143]
[0026] As used herein, the terms "a," "an," and "the" mean one or more.
[0144] As used herein, the term "and / or" when used with a list of two or more items means that any one of the listed items may be employed by itself, or any combination of two or more of the listed items may be employed. For example, if a composition is described as containing components A, B, and / or C, the composition may contain A alone; B alone; C alone; A and B in combination; A and C in combination, B and C in combination; or A, B, and C in combination.
[0145] As used herein, the term "comprising" is an open transition term used to transition from the subject matter described before the term to one or more elements described after the term, wherein the one or more elements listed after the transition term are not necessarily the only elements constituting the subject matter.
[0146] As used herein, the term "having" has the same open-ended meaning as "comprising" provided above.
[0147] As used herein, the term "comprising" has the same open-ended meaning as "including" provided above.
[0148] Numerical range
[0149] This specification uses numerical ranges to quantify certain parameters related to the present invention. It should be understood that when a numerical range is provided, such range is to be interpreted as providing literal support for claim limitations that only list the lower limit of the range and claim limitations that only list the upper limit of the range. For example, a disclosed numerical range of 10 to 100 provides literal support for a claim that lists "greater than 10" (with no upper limit) and a claim that lists "less than 100" (with no lower limit).
Claims
1. An electrochemical electrode for a biosensor, the electrode comprising: (a) substrate; (b) a palladium metal layer fabricated on said substrate, wherein said palladium metal layer has a thickness of not more than 90 nm; and (c) a palladium oxide-containing layer produced on the palladium metal layer, wherein the palladium oxide-containing layer has a thickness of not more than 40 nm; wherein the palladium oxide-containing layer has a thickness not exceeding 40% of the palladium metal layer, and The biosensor is a blood glucose sensor.
2. The electrochemical electrode of claim 1, wherein the electrode has a thickness of at least 5 nm and / or not more than 110 nm.
3. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium metal layer has a thickness of at least 4 nm and / or not more than 80 nm.
4. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium oxide-containing layer has a thickness of at least 0.5 nm and / or not more than 30 nm.
5. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium metal layer is sputter-coated on the substrate.
6. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium oxide-containing layer is sputter-coated on the palladium metal layer.
7. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium metal layer is sputter-coated on the substrate, and the palladium oxide-containing layer is sputter-coated on the palladium metal layer.
8. The electrochemical electrode of any one of claims 1 to 2, wherein the palladium metal layer is sputter-coated on the substrate in a first atmosphere consisting of an inert gas; wherein the palladium oxide-containing layer is sputtered onto the palladium metal layer in a second atmosphere comprising a mixture of an inert gas and an oxidant; and wherein the oxidant constitutes 0.5 to 50% of the second atmosphere by partial pressure.
9. The electrochemical electrode of claim 8, wherein the inert gas is argon.
10. The electrochemical electrode of claim 8, wherein the oxidant is selected from one or more of the following: oxygen, ozone and water.
11. The electrochemical electrode of claim 8, wherein the oxidant is oxygen, and wherein oxygen comprises 1 to 20% of the second atmosphere by partial pressure.
12. The electrochemical electrode of claim 8, wherein the ratio of sputtering power used during the sputtering of the palladium metal layer and the sputtering of the palladium oxide-containing layer is 4:
1.
13. The electrochemical electrode of any one of claims 1 to 2, wherein the substrate comprises a polymer film.
14. The electrochemical electrode of any one of claims 1 to 2, wherein the substrate comprises polyester or polycarbonate.
15. The electrochemical electrode according to any one of claims 1 to 2, wherein within 10 days of forming the palladium metal layer and the palladium oxide-containing layer, when the electrode is plated in mercaptoethanesulfonate via a mercaptoethanesulfonate plating procedure, the electrode is configured to receive a specific fractional surface coverage A of mercaptoethanesulfonate on the outer surface of the electrode as determined by a Type 1 Mercaptoethanesulfonate Coverage Test, wherein 90 days after forming the palladium metal layer and the palladium oxide-containing layer, when the electrode is plated in mercaptoethanesulfonate via a mercaptoethanesulfonate plating procedure, the electrode is configured to receive an additional partial surface coverage B of mercaptoethanesulfonate on the outer surface of the electrode as determined by a Type 1 Mercaptoethanesulfonate Coverage Test, The coverage A deviates from the coverage B by no more than 30%.
16. The electrochemical electrode of claim 15, wherein said coverage A deviates from said coverage B by no more than 20%.
Citation Information
Patent Citations
System and method for measuring an analyte in a sample
CN101598702A
Hydrogen gas sensor using hydrogen absorption membrane containing oxygen