Condensing gas boiler heat exchanger, alloy for heat exchanger and boiler
By adding heat dissipation protrusions and heat exchange enhancement columns to the heat exchanger of the condensing gas boiler, the flue gas condensation effect and heat exchange efficiency are improved, solving the problems of insufficient heat exchange efficiency and impact resistance in the existing technology, and achieving high efficiency. Heat absorbing and simple maintenance.
Patent Information
- Application Number
- CN201910427536.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-05-22
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-05-22
AI Technical Summary
The heat exchange efficiency of existing condensing gas boiler heat exchangers is not high enough, the latent heat absorption of flue gas is not efficient enough, and its tensile strength, yield strength and impact resistance are poor.
Design a condensing gas boiler heat exchanger, including setting a condensation water channel in the heat exchanger body, and setting heat dissipation protrusions and heat exchange enhancement columns on its outer surface to increase the heat exchange area, and the condensation water channel is more distributed near the combustion chamber. Dense, with a Z-shaped plate structure inside to enhance the heat exchange effect, and a neutralizer and secondary heat exchanger outside the boiler to recover and utilize the heat of the flue gas.
It significantly improves the heat exchange efficiency of the heat exchanger, ensures efficient absorption of latent heat of flue gas, simplifies maintenance, ensures water balance, and improves the quality of life and comfort of use.
Smart Images

Figure CN110260515B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a condensing gas boiler heat exchanger, an alloy for the heat exchanger and a boiler. Background Art
[0002] In traditional boilers, after the fuel is burned in the boiler, the exhaust gas temperature is relatively high, and the water vapor in the flue gas is still in a gaseous state, which will take away a lot of heat. Among all kinds of fossil fuels, natural gas has the highest hydrogen content, with a mass percentage of hydrogen of about 20% to 25%. Therefore, the exhaust gas contains a large amount of water vapor. According to calculations, the heat paper to be taken away by the steam generated by burning 1 square meter of natural gas is 4000KJ, which is about more than 10% of its high calorific value. Therefore, condensing boilers came into being. They recover the heat energy in the flue gas by condensing the flue gas, and use water or air with lower temperature to cool the flue gas to reduce the flue gas temperature. Near the heat exchange surface area, the water vapor in the flue gas condenses, and at the same time, the sensible heat release of the flue gas and the latent heat release of the water vapor condensation are realized, and the water or air in the heat exchanger absorbs heat and is heated, realizing heat recovery and improving the thermal efficiency of the boiler.
[0003] The fully premixed variable frequency condensing gas boiler is an efficient, environmentally friendly and energy-saving boiler that uses natural gas as fuel. The boiler has a thermal efficiency of up to 109.1%, which is 40% more energy-saving than conventional boilers. The boiler exhaust temperature can be as low as 30°C. It uses a very low-cost PVC chimney, and the flue gas pollution is very small. The nitrogen oxide emissions do not exceed 30ppm, meeting the European "blue sky use" standard and fully complying with Beijing's latest environmental emission standards. With the further improvement of the country's requirements for energy conservation and emission reduction and the gradual improvement of relevant policies, especially the increasingly stringent NO X Emission requirements will promote the rapid development of fully premixed variable frequency condensing gas boilers.
[0004] The "Clean Coal and Reduce Nitrogen" project is an important guarantee measure to achieve the target of an annual average concentration of PM2.5 of 60 micrograms per cubic meter. At the beginning of 2017, the municipal government issued the "Notice on the 2017 Air Pollution Prevention and Control Program in Beijing", which clearly stipulates that new natural gas boilers before October 2017 should adopt low-nitrogen combustion or flue gas recirculation technology, and nitrogen oxide emissions should be controlled below 30 mg / cubic meter. For Beijing alone, it is necessary to basically eliminate coal-fired boilers below 10 tons in the plain areas of remote suburbs and below 35 tons in built-up areas, and complete the clean energy transformation task of coal-fired boilers of about 4,000 tons. New gas boilers must meet the emission limit of 30 mg / cubic meter of nitrogen oxides. With the urgent need of the "coal to gas" project, fully premixed variable frequency condensing gas boilers will be the inevitable choice! However, the heat exchange efficiency of current condensing water gas boilers, including fully premixed variable frequency condensing gas boilers, is still not high enough, and the latent heat absorption of flue gas is not efficient.
[0005] At present, all countries are vigorously developing condensing gas boilers, and the development of their heat exchangers. The tensile strength and yield strength of the heat exchangers currently produced in my country are still not high enough, and the elongation and impact resistance are relatively poor. At present, this field mainly focuses on improving corrosion resistance and wear resistance, and the mechanical properties mainly focus on improving tensile strength and yield strength; Patent publication number CN109425241A: Heat exchanger, which has: a plurality of heat exchange tubes made of aluminum extrusion molding materials; and fins made of aluminum material, which are arranged between adjacent heat exchange tubes and connected to the heat exchange tubes by brazing material, and the tube wall of the heat exchange tube includes a heat exchange tube made of a shaped A main body composed of an Al alloy of the aluminum extrusion molding material, and a coating layer composed of Al-Si-Zn and covering the outer surface of the main body, a diffusion layer formed by diffusion of Zn and Si in the Al-Si-Zn alloy forming the coating layer is formed on the outer surface layer of the main body of the tube wall of the heat exchange tube, and within a range between the outermost surface of the tube wall of the heat exchange tube and the deepest part of the diffusion layer, a low potential portion with the lowest natural potential within the range and a high potential portion with a natural potential higher than that of the low potential portion by more than 60 mV exist in a manner such that the low potential portion is located on the outermost surface side of the tube wall. The tube wall of the heat exchange tube includes a main body composed of an Al alloy forming the aluminum extrusion molding material, and a cladding layer composed of an Al-Si-Zn alloy and covering the outer surface of the main body. A diffusion layer formed by diffusion of Zn and Si in the Al-Si-Zn alloy forming the cladding is formed on the outer surface layer of the main body of the heat exchange tube. In the range between the outermost surface of the tube wall of the heat exchange tube and the deepest part of the diffusion layer, a low-potential part with the lowest natural potential in the range and a high-potential part with a natural potential higher than 60 mV than the low-potential part exist in a manner such that the low-potential part is located on the outermost surface side of the tube wall. Therefore, corrosion starting from the outer surface of the tube wall of the heat exchange tube stops at the high-potential part. Therefore, the corrosion depth can be reduced and the corrosion resistance of the heat exchange tube can be improved. The corrosion resistance is high, but its elongation and impact resistance are still poor. No technical literature related to improving the elongation and impact resistance of the heat exchanger has been retrieved. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects existing in the prior art and provide a condensing gas boiler heat exchanger, which can enhance the condensation effect of the heat exchanger on the flue gas, can better absorb heat, greatly enhance the heat exchange efficiency of the heat exchanger, and ensure more efficient heat exchange; ensure efficient absorption of flue gas latent heat; the all-cast aluminum high-efficiency condensing heat exchanger is very simple to maintain; it can also ensure water balance and the working condition is close to perfect.
[0007] To achieve the above-mentioned purpose, the technical solution of the present invention is to design a condensing gas boiler heat exchanger, including a heat exchanger body, a combustion chamber and a smoke exhaust chamber connected to each other are arranged in the body, a condensation water channel is arranged between the combustion chamber and the smoke exhaust chamber, and the condensation water channel is arranged integrally with the body; the outer surface of the condensation water channel is integrally or fixedly provided with a heat dissipation protrusion, and the closer the condensation water channel is to the combustion chamber, the denser the arrangement. The heat dissipation protrusion is arranged on the outer surface of the heat exchanger, which increases the heat exchange area and enhances the condensation effect of the heat exchanger on the flue gas; the water channels closer to the combustion chamber are arranged more densely, which can better absorb heat, greatly enhancing the heat exchange efficiency of the heat exchanger and ensuring more efficient heat exchange.
[0008] A further technical solution is that a heat exchange enhancement column is fixedly arranged or integrally arranged in the condensation water channel, and both ends of the heat exchange enhancement column are connected to the inner wall of the condensation water channel, and the heat exchange enhancement column is cylindrical; the condensation water channel is also provided with an internal flow channel in the part close to the combustion chamber, and the internal flow channel is composed of a plurality of support plates, and a spacing is provided between each support plate, one end of the support plate is connected to the inner wall of the condensation water channel, and the other end is provided with a spacing from the inner wall of the condensation water channel; each support plate is composed of a plurality of Z-shaped plates connected end to end. In this way, in addition to the heat dissipation protrusions that enhance the specific surface area of the heat exchanger are arranged on the outer surface of the heat exchanger, a cylinder (i.e., a heat exchange enhancement column) that enhances heat exchange is also arranged on the inner surface of the heat exchanger, so that the heat exchange area of the inner and outer surfaces of the heat exchanger is greatly increased, and the heat exchange effect is greatly enhanced, so that the heat absorption effect of the water in the condensation water channel is enhanced, and the condensation effect on the flue gas is enhanced. The water channel closer to the combustion chamber is more densely arranged, and can absorb heat better, which greatly enhances the heat exchange efficiency of the heat exchanger and ensures more efficient heat exchange.
[0009] A further technical solution is that the condensation water channel includes a water channel main body and a water channel end part connected to the water channel main body, the water channel end part is an annular flow channel close to the inner wall of the combustion chamber, a water outlet is arranged at the end of the annular flow channel, the water channel main body is a plurality of sections of Z-shaped pipes connected end to end, one end of the water channel main body is connected to the water channel end part, and the other end of the water channel main body is provided with a water inlet; the combustion chamber and the smoke exhaust chamber are respectively located at the two ends of the body; the heat dissipation protrusions are needle-shaped or columnar, and the closer the heat dissipation protrusions are to the smoke exhaust chamber, the denser the arrangement. The setting of the water inlet and the water outlet cooperates with the setting of the combustion chamber and the smoke exhaust chamber so that the flow direction of the smoke is opposite to the flow direction of the condensed water, thereby enhancing the heat exchange effect and the condensation effect of the smoke; and the water channel end part before the water outlet is arranged in an annular shape in order to further enhance the full contact between the water channel and the combustion chamber (because the smoke temperature in the combustion chamber is the highest) and enhance the heat absorption effect of the water in the condensation water channel.
[0010] A further technical solution is that the spacing between the rotation axes of adjacent heat dissipation protrusions is 10mm or 12mm; the diameter of the heat dissipation protrusion is 6mm or 7mm. The body of the condensing gas boiler heat exchanger is made of cast aluminum, and the spacing of 10mm between the rotation axes of adjacent heat dissipation protrusions is the processing limit, and it cannot be processed any smaller. The closer the water channel is to the combustion chamber, the smaller the value, for example, the water channel widths are 59.5mm, 49.5mm, 41.5mm and 35.5mm respectively (the widths of the last few water channels close to the combustion chamber are all about 35.5mm, and the internal flow channel is built-in, and the spacing between adjacent support plates that constitute the internal flow channel is 1.5mm or 1.4mm or 1.7mm) The diameter of the heat exchange enhancement column is 9mm.
[0011] Another technical solution is that a condensate drain end is provided at the bottom of the heat exchanger body, a condensate collection pipe is provided on the condensate drain end, the other end of the condensate collection pipe is connected to the neutralizer, a water pipe is arranged around the surface of the neutralizer, the water inlet of the water pipe is connected to the cold water inlet pipe, and the water outlet of the water pipe is connected to the warm water outlet pipe. The neutralizer is made of pure aluminum or stainless steel with a purity of 99.5%. The warm water outlet pipe is used for washing water in the kitchen and dry area basin. In this way, a separate hot water outlet is provided (using the heat released during the neutralization reaction of the neutralizer to heat the cold water for washing or washing dishes, etc.), which can avoid the situation that the hot water outlet water pressure of the shower room is reduced when the condensing gas boiler heat exchanger on the market is used, if someone takes a bath and someone washes (or uses hot water in the kitchen), thereby avoiding mutual interference and improving the quality of life. The neutralizer is made of pure aluminum or stainless steel with a purity of 99.5%, which not only meets the need for corrosion protection of the neutralizer, but also meets the need for heat transfer from the neutralizer to the water inlet pipe. A secondary heat exchanger can also be set at the smoke exhaust pipe of the boiler. The secondary heat exchanger further utilizes the heat of the flue gas after the heat exchanger in the boiler body has absorbed a certain amount of sensible heat and latent heat of the post-combustion gas. The cold water introduced into the cold water inlet pipe of the secondary heat exchanger becomes warm water suitable for washing dishes and washing face and brushing teeth after heat exchange in the secondary heat exchanger. The cold water inlet pipe and hot water outlet pipe at the secondary heat exchanger are independent of the inlet and outlet pipes of the shower room (the inlet and outlet pipes of the shower room are connected to the cold water inlet pipe and hot water outlet pipe of the boiler heat exchanger <this is not the cold water inlet pipe and hot water outlet pipe of the secondary heat exchanger>) to avoid mutual influence.
[0012] The present invention also provides a technical solution, which is a condensing gas boiler including the heat exchanger, wherein a condensate drainage end is arranged at the bottom end of the heat exchanger body, a condensate collecting pipe is arranged on the condensate drainage end, the other end of the condensate collecting pipe is connected to the neutralizer, and a hydrogen recovery pipe is arranged on the upper end of the neutralizer. A cold water tank, a hydrogen purifier, a compressor, a hydrogen storage tank, a first solenoid valve and an excess hydrogen storage tank are sequentially connected to the hydrogen recovery pipe along the flow direction of hydrogen, a signal input end of the first solenoid valve is electrically connected to a signal output end of a PLC controller, a gas pressure detector for detecting the internal gas pressure of the hydrogen storage tank is arranged on the hydrogen storage tank, and a signal output end of the gas pressure detector is electrically connected to a signal input end of the PLC controller, a hydrogen gas transmission pipe is also connected to the hydrogen storage tank, a second solenoid valve is arranged on the hydrogen gas transmission pipe, a gas transmission port of the hydrogen gas transmission pipe is connected to the auxiliary burner, and the signal input end of the second solenoid valve is also electrically connected to the signal output end of the PLC controller. The excess hydrogen storage tank is also connected to a pressure relief valve, which is connected to a gas leak detection alarm. Once the solenoid valve or hydrogen gas pipeline is blocked and the hydrogen pressure in the excess hydrogen storage tank exceeds the warning value, the pressure relief valve can ensure that the hydrogen pressure in the excess hydrogen storage tank will not continue to rise. When gas is emitted from the pressure relief valve, it will trigger the gas leak detection alarm to sound an alarm, reminding relevant personnel to eliminate equipment failures in a timely manner. Among them, hydrogen storage tanks and excess hydrogen storage tanks are equipped with hydrogen purity analyzers, and the detection probes of the hydrogen purity analyzer are set inside the hydrogen storage tanks and excess hydrogen storage tanks. The hydrogen purity analyzer is used to detect and display the purity of the hydrogen in the hydrogen storage tanks and excess hydrogen storage tanks for reference by relevant staff.
[0013] A further technical solution is that the auxiliary burner is arranged in an auxiliary boiler shell on one side of the boiler body, the auxiliary boiler shell is fixedly connected to the outer wall of the boiler body, and a second heat exchanger is also provided in the auxiliary boiler shell. The water inlet pipe of the second heat exchanger is a cold water inlet pipe, and the water outlet pipe of the second heat exchanger is a warm water outlet pipe. The upper end of the auxiliary boiler shell is connected to a smoke exhaust pipe, and the lower end of the auxiliary boiler shell is connected to a condensate recovery pipe, and the condensate recovery pipe is connected to the neutralizer. Using the hydrogen released by the neutralization reaction (the condensate has a certain acidity and contains some harmful substances, magnesium is added to the neutralizer to change the water quality. The chemical reaction formula is as follows: Mg+2H2O=Mg(OH)2+H2↑, Mg(OH)2+2HNO3=Mg(NO3)2+2H2O, Mg(OH)2+H2SO4=MgS04+2H2O, Mg+2HNO3=Mg(NO3)2+H2↑, Mg+H2SO4=MgSO4+H2↑. The reaction products, magnesium nitrate and magnesium sulfate, are not corrosive and soluble in water and can be mixed with ) A secondary burner can be set up to recycle hydrogen. Although the amount of hydrogen produced in the neutralization reaction is not large, it can be used for secondary use to heat cold water to the temperature of warm water, which is suitable for the needs of warm water in the dry area basin and kitchen. In addition, since the secondary burner is independent of the main boiler, even if the hot water valve in the kitchen or dry area basin is opened when someone is bathing, it will not affect the water pressure of the shower room. This solves the common problem in the market that once someone in the house takes a bath, the hot water valve in other areas will cause the water temperature or water pressure to drop, thereby improving the comfort of home use.
[0014] The present invention also provides an alloy for a condensing gas boiler heat exchanger, comprising the following components in percentage by weight:
[0015] Silicon: 8%~11%, Magnesium: 0.2%~0.45%, Iron: ≤0.2%, Titanium: 0.02%~0.14%, Strontium: 0.01%~0.03%, and the balance is aluminum. After studying the fluidity of cast aluminum materials, it was found that when the Si content is 8-11%, it can not only maintain sufficient eutectic phase, but also leave room for further solid solution strengthening and dispersion strengthening; the addition of Mg element can form Mg2Si dispersion strengthening phase and improve the mechanical properties of the alloy; however, the selection of Mg content needs to balance the inverse relationship between strength and elongation, and the Mg content is selected to be 0.2% to 0.45%; the presence of Fe element in the alloy greatly weakens the matrix and reduces the mechanical properties of the alloy; therefore, the Fe content is controlled below 0.2% as much as possible; the Ti element can play a role in grain refinement, and the optimal content of Ti is 0.02% to 0.14%; after studying the influence of Sr on the metallographic structure, mechanical properties, air absorption, etc. of the material, it is determined that the optimal addition amount of Sr modifier is about 0.02%.
[0016] A further technical solution is: silicon: 9.5% to 10.5%, magnesium: 0.28% to 0.30%, iron: 0.13%, titanium: 0.09% to 0.11%, strontium: 0.02%, and the balance is aluminum.
[0017] The present invention also provides a method for preparing the alloy. According to the raw material ratio, a metal furnace charge for the alloy is prepared: industrial pure aluminum, high-purity Mg, Al-Si master alloy, Al-Ti master alloy and Al-Sr master alloy are weighed; the metal furnace charge is preheated before loading into the furnace, the preheating temperature is 350-450° C., and the temperature is kept at 350-450° C. for 2-4 hours; wherein the Mg metal is kept at 200-250° C. for 2-4 hours; hexachloroethane is weighed according to 0.5wt%-0.8wt%, and the hexachloroethane is stored in a sealed dryer, and the hexachloroethane is preheated beside the melting furnace before use; the weighed modifier is baked at 300-400° C. for 3-4 hours and preheated beside the furnace;
[0018] The crucible surface is cleaned and preheated, and the slag scoop and the bell jar are heated to 300°C in an oven; then the inner wall of the crucible and the smelting tool are evenly sprayed with a spray pot; the coating in the spray pot is prepared from zinc oxide, water glass and hot water, and the proportion is: 10% by mass of zinc oxide, 7% by mass of water glass and the balance, and the balance is water; the alloy prepared according to the predetermined composition is added to pure aluminum and aluminum-silicon master alloy, and smelted by electricity; the alloy liquid is heated to 680°C and pure magnesium is added, and when adding pure magnesium, it is pressed into the alloy liquid with a bell jar and kept until the magnesium is completely melted; then the alloy liquid is heated After reaching 750-780°C, the raw materials are refined and degassed: degassing and refining is carried out by rotating dry nitrogen or argon, and the degassing time is not less than 15 minutes; then standing for 15-20 minutes, and then skimming; then the alloy liquid is cooled to 730°C, and AlSr10 master alloy and AlTi5 master alloy are added in sequence; the master alloy is pressed into the alloy liquid with a bell jar and maintained until the alloy is completely melted; after refining again, the alloy liquid temperature is adjusted to 730°C, and chemical analysis samples are poured, and single casting tensile test bars are poured; the capacity of the melting furnace is 5kg, and the bulk density of the graphite crucible is 5kg. Among them, hexachloroethane is C2Cl6.
[0019] The advantages and beneficial effects of the present invention are as follows: heat dissipation protrusions are arranged on the outer surface of the heat exchanger to increase the heat exchange area and enhance the condensation effect of the heat exchanger on the flue gas; the water channels closer to the combustion chamber are arranged more densely, which can absorb heat better, greatly enhancing the heat exchange efficiency of the heat exchanger and ensuring more efficient heat exchange; the unique all-water cooling design ensures efficient absorption of flue gas latent heat; the wider water channels make the maintenance of the all-cast aluminum high-efficiency condensing heat exchanger very simple; the fewer parallel water channels inside the heat exchanger ensure hydraulic balance and a nearly perfect working state. In addition to the heat dissipation protrusions that enhance the specific surface area of the heat exchanger on the outer surface of the heat exchanger, a cylinder that enhances heat exchange (i.e., a heat exchange enhancement column) is also provided on the inner surface of the heat exchanger, so that the heat exchange area of the inner and outer surfaces of the heat exchanger is greatly increased, the heat exchange effect is greatly enhanced, and the heat absorption effect of the water in the condensation water channel is enhanced, which enhances the condensation effect on the flue gas. The setting of the water inlet and outlet cooperates with the setting of the combustion chamber and the smoke exhaust chamber so that the flow direction of the flue gas is opposite to the flow direction of the condensed water, thereby enhancing the heat exchange effect and the condensation effect of the flue gas; and the end part of the water channel in front of the water outlet is arranged in a ring shape to further enhance the full contact between the water channel and the combustion chamber (because the flue gas temperature in the combustion chamber is the highest) and enhance the heat absorption effect of the water in the condensation water channel.
[0020] The warm water outlet pipe is used for washing water in the kitchen and dry area basins. This separate hot water outlet method (using the heat released by the neutralization reaction of the neutralizer to heat cold water for washing or washing dishes, etc.) can avoid the situation where the condensing gas boiler heat exchanger on the market, when in use, if someone is taking a shower and someone is washing (or using hot water in the kitchen), the water pressure of the hot water outlet in the shower room will be reduced, avoiding mutual interference and improving the quality of life. The neutralizer is made of pure aluminum or stainless steel with a purity of 99.5%, which not only meets the need for corrosion protection of the neutralizer, but also meets the need for heat transfer from the neutralizer to the water inlet pipe.
[0021] An auxiliary burner can be set up using the hydrogen released by the neutralization reaction to recycle the hydrogen. Although the amount of hydrogen released by the neutralization reaction is not large, it can be used for secondary utilization to heat cold water to the temperature of warm water, which is suitable for the warm water needs of dry area basins and kitchens. Moreover, since the auxiliary burner is independent of the main boiler, even if the hot water valve in the kitchen or dry area basin is opened when someone is taking a bath, it will not affect the water pressure of the shower room. This solves the common problem in the market that once someone in the house takes a bath, opening the hot water valve in other areas will cause the water temperature or water pressure to drop, thereby improving the comfort of home use. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a cross-sectional view in the longitudinal direction of the middle part of the first embodiment of a condensing gas boiler heat exchanger of the present invention;
[0023] Figure 2 yes Figure 1 A partially enlarged schematic diagram of
[0024] Figure 3 yes Figure 1 The side view after the cut part is completed;
[0025] Figure 4 yes Figure 1 The side view of the longitudinal section after the sectioned part is completed;
[0026] Figure 5 yes Figure 4 A magnified schematic diagram of the upper middle part;
[0027] Figure 6 This is a graph showing the relationship between the amount of magnesium added and the tensile strength and elongation at break;
[0028] Figure 7 This is the relationship between the amount of iron added and the tensile strength and elongation at break;
[0029] Figure 8 This is the relationship between the amount of titanium added and the tensile strength and relative elongation;
[0030] Fig. 9 This is an electron microscope photo of the heat exchanger alloy material when the strontium element addition amount is 0.02%;
[0031] Fig.10 is a schematic diagram of a fourth embodiment of the present invention;
[0032] Fig.11 It is a schematic diagram of Embodiment 5 of the present invention.
[0033] In the figure: 1. heat exchanger body; 2. combustion chamber; 3. smoke exhaust chamber; 4. condensate water channel; 5. heat dissipation protrusion; 6. heat exchange enhancement column; 7. support plate; 8. water channel main part; 9. water channel end part; 10. water outlet; 11. water inlet; 12. condensate collecting pipe; 13. neutralizer; 14. water pipe; 15. cold water inlet pipe; 16. warm water outlet pipe; 17. hydrogen recovery pipe; 18. cold water tank; 19. hydrogen purifier; 20. compressor; 21. hydrogen storage tank; 22. first solenoid valve; 23. excess hydrogen storage tank; 24. gas pressure detector; 25. hydrogen gas pipeline; 26. second solenoid valve; 27. auxiliary burner; 28. auxiliary boiler shell; 29. second heat exchanger; 30. smoke exhaust pipe; 31. condensate recovery pipe. DETAILED DESCRIPTION
[0034] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and examples. The following examples are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0035] Embodiment 1:
[0036] like Figures 1 to 5 As shown ( Figure 4 The longitudinal section refers to Figure 4 yes Figure 1 along Figure 1 The present invention is a condensing gas boiler heat exchanger, including a heat exchanger body 1, a combustion chamber 2 and a smoke exhaust chamber 3 are arranged in the body, a condensation water channel 4 is arranged between the combustion chamber 2 and the smoke exhaust chamber 3, and the condensation water channel 4 is arranged integrally with the body; the outer surface of the condensation water channel 4 is integrally provided with a heat dissipation protrusion 5, and the closer the condensation water channel 4 is to the combustion chamber 2, the denser the arrangement. A heat exchange enhancement column 6 is fixedly arranged in the condensation water channel 4, and both ends of the heat exchange enhancement column 6 are connected to the inner wall of the condensation water channel 4, and the heat exchange enhancement column 6 is cylindrical. The condensation water channel 4 is also provided with an internal flow channel in the part close to the combustion chamber 2, and the internal flow channel is composed of a plurality of support plates 7, each of which is provided with a spacing, one end of the support plate 7 is connected to the inner wall of the condensation water channel 4, and the other end is provided with a spacing from the inner wall of the condensation water channel 4; each support plate 7 is composed of a plurality of Z-shaped plates connected end to end. The condensation water channel 4 includes a water channel main body 8 and a water channel end part 9 connected to the water channel main body 8. The water channel end part 9 is an annular flow channel close to the inner wall of the combustion chamber 2. A water outlet 10 is arranged at the end of the annular flow channel. The water channel main body 8 is a plurality of Z-shaped pipes connected end to end. One end of the water channel main body 8 is connected to the water channel end part 9, and the other end of the water channel main body 8 is provided with a water inlet 11. The combustion chamber 2 and the smoke exhaust chamber 3 are located at the two ends of the body respectively; the heat dissipation protrusion 5 is needle-shaped, and the closer the heat dissipation protrusion 5 is to the smoke exhaust chamber 3, the denser the arrangement. The spacing between the rotation axes of adjacent heat dissipation protrusions 5 is 10mm or 12mm (the spacing between the rotation axes of the heat dissipation protrusions 5 close to the smoke exhaust chamber is 10mm; the spacing between the rotation axes of the heat dissipation protrusions 5 close to the combustion chamber is 12mm).
[0037] The present invention also provides a method for preparing the alloy.
[0038] The smelting process is as follows:
[0039] Raw materials: industrial pure aluminum, high purity Mg, Al-Si master alloy, Al-Ti master alloy, Al-Sr master alloy
[0040] Refining and degassing process: Use rotary blowing of dry nitrogen or argon for degassing and refining, and the degassing time is not less than 15 minutes
[0041] Since the chemical elements in the new and old raw materials have different burnout rates in different smelting furnaces, the alloy
[0042] During the process, the initial content of each element must be calculated based on the data in Table 5.
[0043] Table 5 Burning rate of each element
[0044]
[0045] The data in the table are suitable for smelting working alloys with master alloys. When Mg is added in the form of pure metal, the burn-off amount increases, reaching 10-30% (except Al-Mg alloy) and 10-15% respectively.
[0046] Equipment used: 5Kg melting furnace, 5Kg graphite crucible, bell jar, slag ladle.
[0047] Melting process:
[0048] Various metal charges (including pure metals, intermediate alloys, and recycled materials) used to prepare alloys must be prepared in the following manner before loading into the furnace in order to ensure the quality of the alloy.
[0049] (1) The chemical composition, surface condition and other quality indicators of the charge must be tested to check whether they meet the requirements of the specified material grade and its technical standards.
[0050] (2) The size of the metal charge after crushing, breaking and cutting should meet the requirements for loading into the furnace.
[0051] (3) Metal charge must be clean and free from oxides, sand, core, oil, moisture, inlays and other impurities. It must be sandblasted or cleaned with a wire brush and stored in a dry and ventilated place.
[0052] (4) Metal charges must be preheated before loading into the furnace. The preheating temperature is generally 350-450℃ for 2-4 hours. Mg metal is kept at 200-250℃ for 2-4 hours.
[0053] Preparation of non-metallic auxiliary materials
[0054] ① Hexachloroethane
[0055] (1) Weigh according to the prescribed amount;
[0056] (2) Store in a sealed desiccator and preheat near a furnace before use.
[0057] ②Deteriorating agent
[0058] (1) Bake the weighed modifier at 300-400℃ for 3-4 hours
[0059] (2) Place on the stove to preheat.
[0060] Melting process
[0061] (1) Clean the crucible surface and preheat it, and heat the slag ladle and bell jar to 300°C in an oven. Then use a spray pot to evenly spray the inner wall of the crucible and the smelting tool. The coating is generally made of zinc oxide, water glass, and hot water. The commonly used ratio is: 10% zinc oxide; 7% water glass; the rest is water.
[0062] (2) Prepare the alloy according to the predetermined composition, add pure aluminum and aluminum-silicon master alloy, and melt it by electric current.
[0063] (3) Heat the alloy liquid to 680°C and add pure magnesium. When adding, press it into the alloy liquid with a bell jar and keep it there until the magnesium is completely melted.
[0064] (4) Heat the alloy liquid to 750-780°C and use rotary dry nitrogen or argon for degassing and refining for no less than 15 minutes. Let it stand for 15-20 minutes and skim the slag.
[0065] (5) The alloy liquid is cooled to 730°C, and AlSr10 (i.e., the weight percentage of Sr in the aluminum strontium alloy is 9.0% to 11.0%) master alloy and AlTi5 (i.e., the weight percentage of titanium in the aluminum titanium alloy is 4% to 6%) master alloy are added in sequence. The master alloy is pressed into the alloy liquid with a bell jar and maintained until the alloy is completely melted.
[0066] (6) After re-refining, the alloy liquid temperature is adjusted to 730°C, and chemical analysis samples and single-cast tensile test bars are cast.
[0067] Alloy for condensing gas boiler heat exchanger, comprising the following components in percentage by weight:
[0068] Silicon: 8.5%, magnesium: 0.28%, iron: 0.13%, titanium: 0.09%, strontium: 0.02%, and the balance is aluminum. The method for preparing the alloy is to preheat pure aluminum, pure silicon, pure magnesium, and pure iron at 125°C to 145°C according to the raw material ratio, then break the pure silicon into small pieces, wrap them with aluminum foil, and preheat them again at 200°C ± 5°C; then put the preheated pure aluminum ingot into a smelting furnace to heat it up, and keep it warm when the furnace temperature reaches 750°C until the metal aluminum is molten; after melting is complete, add the preheated pure silicon, pure titanium, and pure strontium into the molten state. The alloy is added to the melt, stirred until the added components are completely melted, heated to 950°C and kept warm for 20-25 minutes, and then cooled to 850°C, and the preheated blunt magnesium is added to the melt, stirred until it is completely melted, and kept warm for 5 minutes ± 2 minutes; when the alloy melt temperature drops to 760°C, 0.5wt% to 0.8wt% hexachloroethane is added for refining, and the surface scum is removed, and the slag is skimmed after keeping warm for 10 minutes ± 3 minutes; The temperature is then raised to 850° C., Al-P master alloy is added, the amount of P element added is 0.1%±0.05% of the total weight of the alloy, stirred, and kept warm for 15-20 minutes to fully melt the Al-P master alloy; then, the melt is heated from 850° C. to 1050° C., kept warm for 5 minutes, and then cooled to 850° C.; the melt is repeatedly overheated for three times, and finally kept warm at 850° C., slag is removed, kept warm for 5 minutes, and cast in a mold cavity of a metal mold, wherein the metal mold needs to be preheated to 250° C.-350° C. before pouring, to obtain a corresponding cast aluminum alloy; then the cast aluminum alloy is kept warm for 8 hours at a temperature of 495° C.-565° C. for solution treatment, and then placed in 50° C.-80° C. water for cooling; then placed in a temperature of 180° C.-200° C. for aging treatment and kept warm for 10 hours to obtain a corresponding aluminum alloy.
[0069] After the aging treatment, the following process steps are also performed: for the aluminum alloy ingot having the chemical composition of the aluminum alloy, a heat treatment process of performing heat treatment at a temperature of 450-550°C for more than 1 hour; after the heat treatment, a hot rolling process of performing hot rolling at a condition where the end temperature of the hot final rolling is above 250°C and below 300°C; after the hot rolling, a cold working process of cold working with a cold working rate of more than 96% is performed; after the cold working, a tempering annealing process of maintaining a temperature of 160°C to 260°C for 1 to 6 hours is performed.
[0070] Embodiment 2:
[0071] The difference from the first embodiment is that the alloy for the condensing gas boiler heat exchanger comprises the following components in weight percentage: silicon: 9.5%, magnesium: 0.30%, iron: 0.13%, titanium: 0.11%, strontium: 0.02%, and the balance is aluminum.
[0072] Embodiment three:
[0073] The difference from the first embodiment is that the alloy for the condensing gas boiler heat exchanger comprises the following components in weight percentage: silicon: 9%, magnesium: 0.29%, iron: 0.13%, titanium: 0.10%, strontium: 0.02%, and the balance is aluminum.
[0074] The heat exchangers made from the above three embodiments were tested with reference to GB T 6892-2006 General Industrial Aluminum and Aluminum Alloy Extruded Profiles. The results are as follows:
[0075]
[0076] The relationship between the amount of magnesium added and the tensile strength and elongation at break, such as Figure 6 As shown (the contents of the other elements are the proportions of Example 1), the addition of Mg element can form Mg2Si dispersion strengthening phase and improve the mechanical properties of the alloy; however, the selection of Mg content needs to balance the inverse relationship between strength and elongation, and the Mg content is selected to be 0.25% to 0.35%;
[0077] The relationship between the amount of iron added and the tensile strength and elongation at break, such as Figure 7 As shown (the contents of the other elements are the proportions of Example 1), the presence of Fe in the alloy greatly weakens the matrix and reduces the mechanical properties of the alloy; therefore, the Fe content is controlled to be below 0.2% as much as possible;
[0078] The relationship between the amount of titanium added and the tensile strength and relative elongation, such as Figure 8 As shown (the contents of the other elements are the proportions of Example 1), the Ti element can play a role in grain refinement, and the optimal content of Ti is 0.08% to 0.14%;
[0079] Fig. 9 This is an electron microscope photograph of a strontium element added in an amount of about 0.02% (the contents of the other elements are the proportions of Example 1). It can be seen that there is less air absorption and the metallographic structure is better.
[0080] Embodiment 4:
[0081] The difference from the first embodiment is that: Fig.10 As shown, a condensate drain end is arranged at the bottom end of the heat exchanger body 1, and a condensate collecting pipe 12 is arranged on the condensate drain end. The other end of the condensate collecting pipe 12 is connected to a neutralizer 13. A water pipe 14 is arranged around the surface of the neutralizer 13. The water inlet of the water pipe 14 is connected to a cold water inlet pipe 15, and the water outlet of the water pipe 14 is connected to a warm water outlet pipe 16. The material of the neutralizer 13 is pure aluminum or stainless steel with a purity of 99.5%.
[0082] Embodiment five:
[0083] The difference from the first embodiment is that: Fig.11 As shown, a condensing gas boiler including the heat exchanger is provided with a condensate drain end at the bottom end of the heat exchanger body 1, a condensate collecting pipe 12 is connected to the condensate drain end, the other end of the condensate collecting pipe 12 is connected to the neutralizer 13, and the upper end of the neutralizer 13 is connected to a hydrogen recovery pipe 17, and a cold water tank 18, a hydrogen purifier 19, a compressor 20, a hydrogen storage tank 21, a first solenoid valve 22 and an excess hydrogen storage tank 23 are sequentially connected to the hydrogen recovery pipe 17 along the flow direction of hydrogen. The signal of the first solenoid valve 22 The input end is electrically connected to the signal output end of the PLC controller. The hydrogen storage tank 21 is provided with a gas pressure detector 24 for detecting the internal gas pressure thereof. The signal output end of the gas pressure detector 24 is electrically connected to the signal input end of the PLC controller. The hydrogen storage tank 21 is also connected to a hydrogen gas pipeline 25. A second solenoid valve 26 is arranged on the hydrogen gas pipeline 25. The gas delivery port of the hydrogen gas pipeline 25 is connected to the auxiliary burner 27. The signal input end of the second solenoid valve 26 is also electrically connected to the signal output end of the PLC controller. The auxiliary burner 27 is arranged in an auxiliary boiler shell 28 on one side of the boiler body. The auxiliary boiler shell 28 is fixedly connected to the outer wall of the boiler body. A second heat exchanger 29 is also arranged in the auxiliary boiler shell 28. The water inlet pipe of the second heat exchanger 29 is a cold water inlet pipe 15, and the water outlet pipe of the second heat exchanger 29 is a warm water outlet pipe 16. The upper end of the auxiliary boiler shell 28 is connected to a smoke exhaust pipe 30, and the lower end of the auxiliary boiler shell 28 is connected to a condensate recovery pipe 31, and the condensate recovery pipe 31 is connected to the neutralizer 13.
[0084] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A condensing gas boiler, comprising a condensing gas boiler heat exchanger, characterized in that: The condensing gas boiler heat exchanger comprises a heat exchanger body, in which a combustion chamber and a smoke exhaust chamber are connected, a condensation water channel is arranged between the combustion chamber and the smoke exhaust chamber, and the condensation water channel is integrally arranged with the body; a heat dissipation protrusion is integrally arranged or fixedly arranged on the outer surface of the condensation water channel, and the closer the condensation water channel is to the combustion chamber, the denser the arrangement; A heat exchange enhancement column is fixedly arranged or integrally arranged in the condensation water channel, and both ends of the heat exchange enhancement column are connected to the inner wall of the condensation water channel, and the heat exchange enhancement column is cylindrical; the condensation water channel is also provided with an internal flow channel at a portion close to the combustion chamber, and the internal flow channel is composed of a plurality of support plates, and a spacing is provided between each support plate, one end of the support plate is connected to the inner wall of the condensation water channel, and the other end is provided with a spacing from the inner wall of the condensation water channel; each support plate is composed of a plurality of Z-shaped plates connected end to end; The condensation water channel includes a water channel main body and a water channel end part connected to the water channel main body. The water channel end part is an annular flow channel close to the inner wall of the combustion chamber. A water outlet is arranged at the end of the annular flow channel. The water channel main body is a plurality of Z-shaped pipes connected end to end. One end of the water channel main body is connected to the water channel end part, and the other end of the water channel main body is provided with a water inlet. The combustion chamber and the smoke exhaust chamber are respectively located at the two ends of the body. The heat dissipation protrusions are needle-shaped or columnar, and the closer the heat dissipation protrusions are to the smoke exhaust chamber, the denser the arrangement. The distance between the rotation axes of adjacent heat dissipation protrusions is 10mm or 12mm; the diameter of the heat dissipation protrusion is 6mm or 7mm; A condensate drain terminal is arranged at the bottom of the heat exchanger body, a condensate collecting pipe is arranged on the condensate drain terminal, the other end of the condensate collecting pipe is connected to the neutralizer, a water pipe is arranged around the surface of the neutralizer, the water inlet of the water pipe is connected to the cold water inlet pipe, the water outlet of the water pipe is connected to the warm water outlet pipe, and the neutralizer is made of pure aluminum or stainless steel with a purity of 99.5%; The upper end of the neutralizer is connected to a hydrogen recovery pipe, and a cold water tank, a hydrogen purifier, a compressor, a hydrogen storage tank, a first solenoid valve and an excess hydrogen storage tank are sequentially connected to the hydrogen recovery pipe along the flow direction of hydrogen. The signal input end of the first solenoid valve is electrically connected to the signal output end of the PLC controller. The hydrogen storage tank is provided with a gas pressure detector for detecting the internal gas pressure thereof, and the signal output end of the gas pressure detector is electrically connected to the signal input end of the PLC controller. The hydrogen storage tank is also connected to a hydrogen gas pipeline, and a second solenoid valve is arranged on the hydrogen gas pipeline. The gas delivery port of the hydrogen gas pipeline is connected to the auxiliary burner, and the signal input end of the second solenoid valve is also electrically connected to the signal output end of the PLC controller. The excess hydrogen storage tank is also connected to a pressure relief valve, and the pressure relief valve is connected to a gas leak detection alarm; The auxiliary burner is arranged in the auxiliary boiler shell on one side of the boiler body. The auxiliary boiler shell is fixedly connected to the outer wall of the boiler body. A second heat exchanger is also arranged in the auxiliary boiler shell. The water inlet pipe of the second heat exchanger is a cold water inlet pipe, and the water outlet pipe of the second heat exchanger is a warm water outlet pipe. The upper end of the auxiliary boiler shell is connected to a smoke exhaust pipe, and the lower end of the auxiliary boiler shell is connected to a condensate recovery pipe, and the condensate recovery pipe is connected to the neutralizer.
2. The alloy for condensing gas boiler heat exchanger as claimed in claim 1, characterized in that: Contains the following components in weight percentage: Silicon: 8%~11%, Magnesium: 0.2%~0.45%, Iron: ≤0.2%, Titanium: 0.02%~0.14%, Strontium: 0.01%~0.03%, and the balance is aluminum.
3. The alloy for condensing gas boiler heat exchanger according to claim 2, characterized in that: Silicon: 8.5%~9.5%, Magnesium: 0.28%~0.30%, Iron: 0.13%, Titanium: 0.09%~0.11%, Strontium: 0.02%, and the balance is aluminum.
4. A method for preparing the alloy as claimed in claim 2, characterized in that: According to the raw material ratio, a metal charge for the alloy is prepared: industrial pure aluminum, high-purity Mg, Al-Si master alloy, Al-Ti master alloy and Al-Sr master alloy are weighed; the metal charge is preheated before loading into the furnace, the preheating temperature is 350-450° C., and the temperature is kept at 350-450° C. for 2-4 hours; wherein the Mg metal is kept at 200-250° C. for 2-4 hours; hexachloroethane is weighed according to 0.5wt%-0.8wt%, and the hexachloroethane is stored in a sealed desiccator, and the hexachloroethane is preheated beside the furnace before use; the weighed modifier is baked at 300-400° C. for 3-4 hours and preheated beside the furnace; Clean the crucible surface and preheat it, and heat the slag scoop and bell jar to 300°C in the oven; then use a spray pot to evenly spray the inner wall of the crucible and the smelting tool; the coating in the spray pot is made of zinc oxide, water glass and hot water, and the proportion is: 10% by mass of zinc oxide, 7% by mass of water glass and the balance, and the balance is water; add the alloy prepared according to the predetermined composition to pure aluminum and aluminum-silicon master alloy, and smelt it by power; heat the alloy liquid to 680°C and add pure magnesium. When adding pure magnesium, press it into the alloy liquid with a bell jar and keep it until the magnesium is completely melted; then heat the alloy liquid to 750-780°C and perform a refining and degassing process on the raw materials: use rotary blown dry nitrogen or argon for degassing and refining, and the degassing time is not less than 15 minutes; then let it stand for 15-20 minutes, and then skim the slag; then cool the alloy liquid to 730°C, and add AlSr in turn 10 Master alloy, AlTi5 master alloy; the master alloy is pressed into the alloy liquid by a bell jar and maintained until the alloy is completely melted; after refining again, the temperature of the alloy liquid is adjusted to 730°C, a chemical analysis sample is poured, and a single cast tensile test bar is poured; the capacity of the melting furnace is 5kg, and the bulk density of the graphite crucible is 5kg.
Citation Information
Patent Citations
Heat exchanger
CN109425241A
Aluminum alloy for casting engine cylinder cover and preparation method of aluminum alloy
CN106086490A
Combined condensing heat exchanger
CN106352551A
Waste gas hydrogen recovery burner
CN206601044U
Condensation type gas boiler heat exchanger
CN210569227U