Method for making semiconductor structure

By using a chemical vapor deposition method to form a titanium silicide layer and a titanium nitride layer in a single reaction chamber in a semiconductor integrated circuit, the problem of reduced compliance in the high aspect ratio contact area is solved, and lower parasitic capacitance and better performance are achieved. High circuit efficiency.

CN110504170BActive Publication Date: 2024-10-11TAIWAN SEMICONDUCTOR MANUFACTURING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN201910085896.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-18
Filing Date
2019-01-29
Publication Date
2024-10-11
Estimated Expiration
2039-07-14

AI Technical Summary

Technical Problem

In semiconductor integrated circuits, as the process size shrinks, the compliance of titanium silicide films and titanium nitride films in high aspect ratio contact areas decreases, resulting in an increase in parasitic capacitance and affecting circuit performance and speed.

Method used

Using chemical vapor deposition and in-situ treatment methods in a single reaction chamber, by adjusting the flow rate ratio of hydrogen and titanium tetrachloride, a titanium silicide layer and a titanium nitride layer are formed, improving their compliance and consistency, and controlling the thickness ratio to reduce parasitic capacitance.

Benefits of technology

The compliance and coverage of the titanium silicide layer and the titanium nitride layer are improved, the film formation quality is improved, the parasitic capacitance of the source/drain region is reduced, and the performance of the integrated circuit is enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110504170B_ABST
    Figure CN110504170B_ABST
Patent Text Reader

Abstract

The disclosed embodiments relate to a method for manufacturing a semiconductor structure. The method includes providing a substrate having a gate structure, an insulating structure on the gate structure, and a source / drain region. A titanium silicide layer is deposited on the source / drain region by a first chemical vapor deposition process. The first chemical vapor deposition process includes a first hydrogen gas flow. The method also includes depositing a titanium nitride layer on the insulating structure by a second chemical vapor deposition process. The second chemical vapor deposition process includes a second hydrogen gas flow. The first chemical vapor deposition process and the second chemical vapor deposition process are performed in a single reaction chamber, and the flow rate of the first hydrogen gas flow is greater than the flow rate of the second hydrogen gas flow.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to deposition methods and related parameters of titanium silicide layers and titanium nitride layers. Background Art

[0002] The semiconductor integrated circuit industry has experienced exponential growth. Technological advances in integrated circuit materials and design have enabled each generation of integrated circuits to have smaller and more complex circuits than the previous generation. In the evolution of integrated circuits, functional density (such as the number of interconnect devices per unit chip area) generally increases as geometric size (such as the smallest component or circuit that can be produced by the manufacturing process) decreases. The reduction in process size generally helps increase production capacity and reduce related costs. Summary of the invention

[0003] One embodiment of the present invention provides a method for manufacturing a semiconductor structure, which includes providing a substrate having a gate structure, an insulating structure on the gate structure, and a source / drain region. A titanium silicide layer is deposited on the source / drain region by a first chemical vapor deposition process. The first chemical vapor deposition process includes a first hydrogen gas flow. The method also includes depositing a titanium nitride layer on the insulating structure by a second chemical vapor deposition process. The second chemical vapor deposition process includes a second hydrogen gas flow. The first chemical vapor deposition process and the second chemical vapor deposition process are performed in a single reaction chamber, and the flow rate of the first hydrogen gas flow is greater than the flow rate of the second hydrogen gas flow. BRIEF DESCRIPTION OF THE DRAWINGS

[0004] Figure 1A is an isometric diagram of an exemplary semiconductor structure in some embodiments.

[0005] Figure 1B yes Figure 1A A top view of an exemplary transistor region in a semiconductor structure is shown.

[0006] Figures 2 to 7 is a cross-sectional view of a partially fabricated FinFET after each series of process steps in some embodiments.

[0007] Figure 8 In some embodiments, Figure 7 An enlarged cross-sectional view of a portion of the source / drain region circled in FIG.

[0008] Fig. 9 is a cross-sectional view of a merged fin structure in some embodiments.

[0009] Fig.10 is a flow chart of an exemplary production method in some embodiments.

[0010] Description of reference numerals:

[0011] H F , HG , H L , 913 height

[0012] L Gate length

[0013] L S length

[0014] W, 912 width

[0015] 100 Semiconductor Structure

[0016] 102, 904 substrate

[0017] 104, 902, 902' Fins

[0018] 106 Isolation Structure

[0019] 108, 117 Gate structure

[0020] 110, 901 source / drain region

[0021] 110 D Drain region

[0022] 110 S Source Region

[0023] 111 Spacer layer

[0024] 112 Channel Area

[0025] 113 Lightly doped drain region

[0026] 114, 118, 910 upper surface

[0027] 115 gate dielectric layer

[0028] 116 Deviation Spacer

[0029] 118 dotted line

[0030] 119, 119', 122 Titanium layer

[0031] 120 Hard Mask

[0032] 121,907 Titanium silicide layer

[0033] 123, 906 Titanium nitride layer

[0034] 124, 905 contact layer

[0035] 125 Contact area

[0036] 131 Section Line

[0037] 150 Transistor Area

[0038] 801, 802 Arc length

[0039] 803 Maximum length

[0040] 804 Minimum length

[0041] 900 Merged fin structure

[0042] 903 Shallow Trench Isolation Layer

[0043] 908, 909 side surface

[0044] 911 Angle

[0045] 912 Source / Drain Width

[0046] 914 Fin Spacing

[0047] 1000 Methods

[0048] Steps 1001, 1002, 1003 DETAILED DESCRIPTION

[0049] The following content provides different embodiments or examples that can implement different structures of the present invention. The embodiments of specific components and arrangements are used to simplify the present invention and are not intended to limit the present invention. For example, the description of forming a first component on a second component includes direct or physical contact between the two, or there are other additional components between the two instead of direct contact. In addition, the numbering can be repeated in various examples of the present disclosure.

[0050] In addition, spatially relative terms such as "below," "beneath," "below," "above," "upper," or similar terms may be used to simplify the description of the relative relationship of one element to another element in a diagram. Spatially relative terms may be extended to elements used in other orientations, not limited to the orientation shown in the diagram. Elements may also be rotated 90° or other angles, so directional terms are only used to describe the orientation shown in the diagram.

[0051] An example of a field effect transistor is a metal oxide semiconductor field effect transistor. For example, a metal oxide semiconductor field effect transistor can be (i) a planar structure built in or on a planar surface of a substrate such as a semiconductor wafer, or (ii) a vertical structure.

[0052] The term “FinFET” refers to a field effect transistor formed on a fin, wherein the fin is oriented perpendicular to the planar surface of the wafer.

[0053] “Source / drain” refers to the source and / or drain junctions that form the terminals of a field effect transistor.

[0054] The term "vertical" herein means approximately perpendicular to the substrate surface.

[0055] "Epitaxial layer" refers to a doped or undoped layer or structure.

[0056] The term "nominal" refers to a desired target, characteristic value or parameter for a component or process step that is set during the design phase of the product, along with a range of upper and lower limits for the desired value. The range of values ​​is generally derived from slight variations or tolerances in the process.

[0057] Metal interconnects (also called interconnects) transmit electronic signals between different components of an integrated circuit. Electronic connections between the interconnects and semiconductor devices (such as fin field effect transistors) can be formed at the source / drain regions of the semiconductor device. The parasitic capacitance between the interconnects and the semiconductor device can be related to the resistance and capacitance delay of the integrated circuit and affect the performance and speed of the integrated circuit.

[0058] To improve electrical contacts and reduce parasitic capacitance, titanium silicide can be formed at the interface between the interconnect and the source / drain region. A titanium nitride layer can be formed on the sidewalls of the gate structure adjacent to the source / drain region as a barrier layer to prevent the diffusion of interconnect material into the gate structure. The thickness of titanium silicide and titanium nitride is an important parameter for the material function in the integrated circuit process, so the thickness of these two materials needs to be controlled.

[0059] A titanium layer is formed before forming the titanium silicide layer and the titanium nitride layer, and the titanium layer can be formed by a physical vapor deposition process. Titanium silicide and titanium nitride are then formed from the titanium layer, and the formation method can be a chemical vapor deposition process. Since the physical vapor deposition process and the chemical vapor deposition process can be performed in two different reaction chambers, the process may produce undesirable results when placing the wafer in the reaction chamber and moving the wafer between the reaction chambers, such as contaminating the wafer or increasing the production time.

[0060] In addition, as the size of semiconductor devices such as fin field effect transistors decreases, the space between adjacent gate structures also decreases, and the contact region (such as the region where the interconnection forms an electrical connection with the source / drain region, including the upper surface of the source / drain region and two adjacent gate structures) can have a high aspect ratio. In this high aspect ratio setting, the width of the bottom of the contact region (such as the source / drain region) can be considered to be smaller than the height of the sidewall (such as the adjacent gate structure), resulting in a decrease in the compliance of the titanium silicide film and the titanium nitride film deposited in the contact region.

[0061] In various embodiments of the present invention, the method of forming a titanium silicide layer and a titanium nitride layer in a semiconductor structure using a deposition and in-situ treatment process has the following advantages over other methods: (i) the titanium silicide layer and the titanium nitride layer have improved conformity and consistency; (ii) the coverage of the titanium silicide on the source / drain region is increased; (iii) the film quality of the titanium silicide layer and the titanium nitride layer is improved; and (iv) the thickness control of the titanium silicide layer and the titanium nitride layer is improved.

[0062] As shown in Figure 1 to Fig. 9 As shown, chemical vapor deposition and in-situ processing are used to form titanium silicide and titanium nitride in various semiconductor devices. The titanium silicide layer and titanium nitride layer formed by the process have a compliant and controlled thickness. The thickness ratio between the titanium silicide layer and the titanium nitride layer can be controlled during the process. Although the fin field effect transistor in the accompanying drawings has a contact area with a high aspect ratio, the method described herein can be used for other devices and structures. For example, the method disclosed herein can be used to form titanium silicide layers and titanium nitride layers on a planar device surface, in grooves and / or gaps with a high aspect ratio or a low aspect ratio, or in a fin field effect transistor with multiple fins. The process provided here is for example only, and other embodiments of the present invention may perform other processes (not shown).

[0063] Figure 1A 1 is an isometric view of a semiconductor structure 100 in some embodiments of the present invention. The semiconductor structure 100 includes a fin field effect transistor. The semiconductor structure 100 includes a substrate 102, a plurality of fins 104, a plurality of isolation structures 106, and a gate structure 108 located on the sidewalls and upper surface of each fin 104. The fins 104 and the isolation structures 106 each have an upper surface 114 and 118. The gate structure 108 includes a gate dielectric layer 115 and a gate structure 117. In other embodiments, the gate structure 108 may include one or more additional layers or structures. For illustration purposes, Figure 1A Only a single gate structure 108 is shown. In the following description, more than one gate structure 108 is used to illustrate the embodiments of the present invention. Figure 1A As shown, the hard mask 120 is located on the upper surface of the gate structure 117. The hard mask 120 is used to pattern the gate structure 108, and the patterning method thereof may be etching. In some embodiments, the hard mask 120 includes a dielectric material such as silicon nitride. Figure 1A The isometric view is a diagram showing the gate structure 108 formed after the gate dielectric layer and the gate layer are patterned (eg, etched). Figure 1A Only a single gate structure 108 is shown. An integrated circuit may include multiple gate structures.

[0064] Figure 1A Each fin 104 shown includes a pair of source / drain terminals. For ease of illustration, the source / drain terminals include a source region 110S The drain region 110 D , and the source / drain terminals are formed in, on, and / or around the fin 104. The channel region 112 of the fin 104 is located under the gate structure 108. The gate structure 108 has a gate length L and a gate width (2×H F +W), such as Figure 1A In some embodiments, the gate length L is between about 10 nm and about 30 nm. In some embodiments, the gate length L is between about 3 nm and about 10 nm. In some embodiments, the width W of the fin is between about 6 nm and about 12 nm. In some embodiments, the width W of the fin is between about 4 nm and about 6 nm. In some embodiments, the height H of the gate structure 108 from the upper surface of the fin 114 to the top of the gate structure 108 is G , is between about 50 nm and about 80 nm. In some embodiments, the height H of the fin 104 from the upper surface 118 of the isolation structure to the upper surface 114 of the fin 104 is F , between about 25 nm and about 35 nm.

[0065] The substrate 102 may be a silicon substrate. Alternatively, the substrate 102 may include other saturated elements such as germanium; semiconductor compounds such as silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; semiconductor alloys such as silicon germanium, gallium arsenide phosphide, aluminum indium arsenide, aluminum gallium arsenide, gallium indium arsenide, gallium indium phosphide, and / or gallium indium arsenide phosphide; or combinations thereof. In some embodiments, the substrate 102 is a semiconductor on an insulator. In some embodiments, the substrate 102 may be an epitaxial material.

[0066] The isolation structure 106 includes a dielectric material such as silicon oxide, spin-coated glass, silicon nitride, silicon oxynitride, fluorine-doped silicate glass, a low-k dielectric material, any other suitable insulating material, or any combination thereof. The isolation structure 106 may be a shallow trench isolation structure. In some embodiments, the isolation structure 106 and the shallow trench isolation structure are formed by etching a trench in the substrate 102. The insulating material may then be filled into the trench, followed by chemical mechanical polishing and back etching of the insulating material. Other manufacturing techniques may also be used to form the isolation structure 106 and / or the fin 104. The isolation structure 106 may include a multilayer structure, such as one or more liner layers.

[0067] The fin 104 is an active region for forming one or more transistors. The fin 104 may include silicon or another semiconductor element such as germanium, a semiconductor compound (including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide), a semiconductor alloy (including silicon germanium, gallium arsenide phosphide, aluminum indium arsenide, aluminum gallium arsenide, gallium indium arsenide, gallium indium phosphide, and / or gallium indium arsenide phosphide), or a combination thereof. The method for making the fin 104 may adopt a suitable process, including photolithography and etching processes. The photolithography process may include forming a photoresist (photoresist) layer on a substrate (such as a silicon layer), exposing the photoresist with a pattern, performing a post-exposure baking process, and developing the photoresist to form a mask unit containing the photoresist. The mask unit may then be used to protect some areas of the substrate, and an etching process may be performed to form a recess into the isolation structure 106 to retain the raised fin. The step of etching the recess may adopt reactive ion etching and / or other suitable processes. Various other methods are also suitable for forming the fin 104 on the substrate 102. In some embodiments, the fin 104 may include epitaxial material.

[0068] The gate structure 108 may include a gate dielectric layer 115, a gate structure 117, a spacer layer 111, and / or one or more additional layers. For ease of description, Figure 1A The spacer layer 111 is not shown. In some embodiments, the gate structure 108 uses polysilicon as the gate structure 117. Figure 1A As shown, the hard mask 120 is located on the upper surface of the gate structure 117. The hard mask 120 is used to pattern the gate structure 108, and the patterning method may be etching. In some embodiments, the hard mask 120 and the spacer layer 111 include dielectric materials such as silicon nitride, silicon oxide, any other suitable insulating material, or any combination thereof.

[0069] Although Figure 1A The isometric view of FIG. 1 shows that the gate structure 108 uses polysilicon as the gate structure 117, but in some embodiments, the gate structure 108 may be a sacrificial gate structure, which will be replaced by a metal gate structure in a replacement gate process. The replacement gate process is not shown in the figure. The metal gate structure may include a barrier layer, a gate dielectric layer, a work function layer, a fill metal layer, any other suitable material for a metal gate structure, or any combination of the above. In some embodiments, the metal gate structure may also include a cap layer, an etch stop layer, other suitable layers, or any combination of the above.

[0070] Exemplary p-type work function metals included in the metal gate structure may include titanium nitride, tantalum nitride, ruthenium, molybdenum, aluminum, tungsten nitride, zirconium silicide, molybdenum silicide, tantalum silicide, nickel silicide, other suitable p-type work function materials, or combinations thereof. Exemplary n-type work function metals included in the metal gate structure include titanium, silver, tantalum aluminum, tantalum aluminum carbide, titanium aluminum nitride, tantalum carbide, tantalum carbonitride, tantalum silicon nitride, manganese, zirconium, other suitable n-type work function materials, or combinations thereof. The work function is related to the material composition of the work function layer, so the material of the first work function layer can adjust its work number to achieve the threshold voltage required for the device to be formed in the respective area. The deposition method of the work function layer can be chemical vapor deposition, plasma enhanced chemical vapor deposition, atomic layer deposition, any other suitable process, or any combination thereof. The fill metal layer can include aluminum, tungsten, copper, any other suitable material, or any combination thereof. The filling metal may be formed by chemical vapor deposition, physical vapor deposition, electroplating, any other suitable process, or any combination thereof. The filling metal may be deposited on the work function metal layer to fill the remaining portion of the trench or opening formed by removing the sacrificial gate structure.

[0071] The semiconductor structure includes a fin 104 and a gate structure 108. To simplify the description, Figure 1A Other structures such as lightly doped drain regions and doped source / drain structures are not shown. The lightly doped drain region is a lightly doped region located between the transistor channel region and at least one transistor source / drain region. An example of a doping process for forming the lightly doped drain region is ion implantation.

[0072] Figure 1B show Figure 1A FIG. 1 is a top view of a transistor region 150 having one or more fins 104 flush with the upper surface 118 of the isolation structure 106. The transistor region 150 includes a source / drain region 110. S With 110 D The transistor region 150 also includes a channel region 112 which is part of the fin 104 and a gate structure 108 surrounding three sides of the channel region 112. Figure 1A 1. The channel region 112 is located below the gate structure 108 and has a width (fin width) W. The length of the channel region 112 may be different from the gate length L, depending on process conditions and device design. For ease of description, the length of the channel region 112 is labeled as the gate length L. The transistor region 150 also includes a gate dielectric layer 115 and a gate structure 117. Figure 1B Also shown is a spacer layer 111 formed on the gate structure 108. A lightly doped drain region 113 is formed on the upper surface and sidewalls of the fin 104. The lightly doped drain region 113 has a width W and a length L. S . Figure 1BAnother gate structure 108 is also shown in dashed lines. The other gate structure 108 has been described above, which is similar to and parallel to the gate structure 108 and is not shown in the figure. Figure 1A In. In combination Figures 2 to 7 In the following description, Figure 1B Two gate structures 108 are shown to illustrate an embodiment of the present invention.

[0073] Figures 2 to 7 Detailed Description of the Invention Various perspective views and cross-sectional views of a partially fabricated fin field effect transistor at various fabrication stages in various embodiments of the present invention. Figures 2 to 7 This will be described in detail below.

[0074] Figure 2 Along Figure 1A The cross-section line 131 is shown to show that two adjacent gate structures 108 are formed on the fin 104. Figure 1A A single gate structure 108 is shown, but the section line 131 of the present invention is along two gate structures (eg Figure 1B ) to show the structure of an embodiment of the present invention. Each gate structure 108 includes a gate structure 117 and a gate dielectric layer 115. A hard mask 120 is located on the gate structure 117. In some embodiments, the hard mask 120 is used to define the patterned gate structure 117. The hard mask 120 includes silicon nitride, silicon oxynitride, silicon carbide, silicon oxycarbide, spin-on glass, a low dielectric constant film, silicon oxide, any other suitable material, or any combination of the foregoing. In some embodiments, the hard mask 120 includes silicon oxide, which may be formed by any suitable method, including but not limited to chemical vapor deposition using tetraethoxysilane as a source gas, plasma enhanced chemical vapor deposition, or a high aspect ratio process. The channel region 112 is located under the gate structure 108 (e.g., directly under the gate structure 108). The dotted line 118 refers to the surface height of the isolation structure 106, such as the upper surface or boundary.

[0075] like Figure 2 As shown, the offset spacer 116 exposes a portion of the source / drain region 110 and the lightly doped drain region 113 between the two gate structures 108. In some embodiments, the thickness of the offset spacer 116 can provide an offset distance from the lightly doped drain region 113 and prevent dopants from being implanted into the channel region 112. For illustration purposes, Figure 2 Other spacers (such as the main spacer covering the offset spacer 116 and the gate structure 108 ) are not shown.

[0076] The offset spacer 116 may be formed by any suitable method. For example, to form the offset spacer, a compliant offset spacer layer may be first deposited on the substrate 102. An etch-back process may be used to remove a portion of the compliant offset spacer layer and expose a portion of the channel region for ion implantation. The retained compliant offset spacer layer may form an offset spacer 116 on the sidewall of the gate structure 117. The offset spacer 116 may include a dielectric material such as silicon oxide, silicon oxynitride, silicon nitride, or any combination of the foregoing. In some embodiments, the process for depositing the offset spacer may be a plasma enhanced chemical vapor deposition process. Other suitable deposition processes may also be used to form the offset spacer 116. In some embodiments, the thickness of the offset spacer 116 is between about 2 nm and about 4 nm.

[0077] Any suitable process may be used to form a lightly doped drain region 113 in the fin 104 between adjacent offset spacers 116. For example, an ion implantation process is performed to form the lightly doped drain region 113, which may use any suitable dopant species. Although the lightly doped drain region 113 in the accompanying drawings is adjacent to the upper surface of the fin 104, the lightly doped drain region 113 may be adjacent to the upper surface and sidewalls of the fin 104. The lightly doped drain implantation may be performed vertically, or diagonally toward the sidewalls of the fin 104. The lightly doped drain region 113 may extend downward from the surface of the fin 104 to a certain depth. Figure 2 For example, the lightly doped drain region 113 may extend downward from the upper surface of the fin 104 to a depth H L The lightly doped drain region 113 may extend from the sidewall surface of the fin 104 to the interior of the fin 104. The substrate 102 may include p-type devices and n-type devices. Additional processes such as lithographic patterning processes may be used to separate the p-type device region and the dopant ions for the n-type device.

[0078] After implanting the dopant ions, a thermal anneal may be performed to drive in and activate the dopants. The thermal anneal may be a rapid thermal annealing process, spike annealing, millisecond annealing, or laser annealing. The spike annealing may be on the order of seconds at the peak annealing temperature. The millisecond annealing may be on the order of milliseconds at the peak annealing temperature. The laser annealing may be on the order of nanoseconds to microseconds at the peak annealing temperature.

[0079] In addition, any suitable process may be used to form the source / drain region 110 in the lightly doped drain region 113 in the fin 104 between adjacent offset spacers 116. For example, ion implantation using any suitable dopant species is used to form the source / drain region 110. In another example, a portion of the lightly doped drain region 113 between adjacent offset spacers 116 is removed, and an epitaxial process is performed to grow a suitable source / drain material between adjacent offset spacers 116. In-situ doping using any suitable dopant may be used to dope the source / drain region 110 to any suitable doping level. Depending on different applications or embodiments, the depth of the source / drain region 110 from the upper surface 114 downward may be greater or less than the depth H of the lightly doped drain region 113. L The lateral width of the source / drain region 110 may be less than, equal to, or greater than the lateral width of the lightly doped drain region 113, depending on the application. The upper surface of the source / drain region 110 may be higher than, substantially flush with, or lower than the upper surface of the gate dielectric layer 115. In some embodiments, the source / drain region 110 is formed by an epitaxial process, and the upper surface of the source / drain region 110 is higher than the upper surface of the gate dielectric layer 115, such as Figure 2 shown.

[0080] In some embodiments, a main spacer (not shown) may be formed. Figure 2 ) on the transistor region 150. The main spacer may cover the upper surface of the gate structure 108 and the offset spacer 116. The thickness of the main spacer may be between about 5 nm and about 10 nm, which is sufficient to protect the gate structure 108 and the offset spacer 116 when the fin 104 is subsequently processed. The main spacer may be formed using an etch-back technique. For example, to form the main spacer, a compliant main spacer layer may be first deposited on the substrate 102 (including the gate structure 108 with the hard mask 120 on the structure). Then, a etch-back process is used to remove a portion of the compliant main spacer layer to form an opening and expose a portion of the lightly doped drain region 113 (for subsequent formation of the source / drain region 110). The retained compliant main spacer layer forms a main spacer. The main spacer may include a dielectric material such as silicon oxynitride, silicon nitride, carbon-doped silicon nitride (silicon carbonitride), or any combination of the above. Silicon carbonitride has a lower etch rate to etchants such as phosphoric acid or hydrofluoric acid than silicon nitride or silicon oxynitride. In some embodiments, the deposition process for forming the main spacers is plasma enhanced chemical vapor deposition. Other suitable deposition processes may also be used. A material removal process may be performed to remove the main spacer material on the hard mask 120 and other portions of the surface of the substrate 102. For example, the material removal process may be a reactive ion etching process and / or any other suitable process.

[0081] In some embodiments, after exposing the lightly doped drain region 113, the source / drain region 110 may be formed. Any suitable doping process such as ion implantation may be used to increase the doping of the source / drain region 110. In another example, the source / drain region 110 may be partially etched, and then a semiconductor material may be epitaxially grown. The semiconductor material may be the same as or different from the substrate 102. For example, the semiconductor material may include one or more of germanium, silicon, silicon germanium, other semiconductor alloys, or any combination of the foregoing. In addition, a titanium silicide layer may be formed on the source / drain region 110 (or the interface between the source / drain region 110 and a subsequently formed metal interconnect) to reduce contact resistance. A titanium nitride layer may be further formed on the titanium silicide layer as a barrier layer to prevent metal atoms of the interconnect from diffusing into the gate structure 108. The method for forming the titanium silicide layer and the titanium nitride layer is as follows. Figures 3 to 7 As shown. In some embodiments, a titanium silicide layer is formed before forming the titanium nitride layer. In some embodiments, both the titanium silicide layer and the titanium nitride layer can be formed from a titanium layer, and the formation method is chemical vapor deposition. In the following content, the formation method of the titanium silicide layer is first described, and then the formation method of the titanium nitride layer is described.

[0082] Figures 3 to 5 It is a process for forming a titanium silicide layer in some embodiments of the present invention. For ease of description, the steps for forming titanium and titanium silicide will be described separately. In some embodiments, titanium and titanium silicide can be formed simultaneously or sequentially. For example, when titanium is formed on the source / drain region 110, a portion of the titanium contacting the source / drain region 110 will be converted into titanium silicide, and the other portion of the titanium will be etched back. In some embodiments, reactions (1) to (4) do not limit the order of the chemical reactions. The formation process will be described in detail below. The contact region 125 refers to the area filled with metal interconnects and contacting the source / drain region 110. For ease of description, only the reactions and processes occurring in the contact region 125 are described.

[0083] Figure 3 An initial titanium layer 119 is shown formed over and between adjacent gate structures 108. The initial titanium layer 119 may be formed over source / drain regions 110. In some embodiments, the fin 104 comprises silicon. The titanium layer 119 and subsequently formed titanium silicide layer may be formed by any suitable method, such as plasma enhanced chemical vapor deposition. In some embodiments, other deposition methods such as chemical vapor deposition and / or atomic layer deposition may also be used. An exemplary plasma enhanced chemical vapor deposition process for forming the initial titanium layer 119 may include reactions (1) and (2) as follows.

[0084] 2TiCl4+H2→2TiCl x (x=2-3)+2HCl+Cl2 (1)

[0085] TiClx (x=2-3)+H2→Ti+2HCl+Cl x (2)

[0086] In some embodiments, a precursor gas such as titanium tetrachloride may flow into a plasma enhanced chemical vapor deposition chamber and react with hydrogen to form an initial titanium layer. Argon may be used to generate and stabilize plasma in a plasma enhanced chemical vapor deposition process under RF power to form a titanium silicide layer. The generated plasma may enhance the chemical reaction in the plasma enhanced chemical vapor deposition chamber. In some embodiments of reactions (1) and (2), the flow rate of titanium tetrachloride may be between about 1 standard cubic centimeter per minute (sccm) and 20 sccm, the flow rate of hydrogen may be between about 500 sccm and about 1500 sccm, the ratio of the flow rate of hydrogen to the flow rate of titanium tetrachloride may be between about 25 and about 1500, and the flow rate of argon may be between about 500 sccm and about 2500 sccm. In some embodiments, the RF power used in the plasma enhanced chemical vapor deposition process is between about 200 watts and about 750 watts. In some embodiments, the flow rate of argon is between about 40 sccm and about 1200 sccm. The station temperature of the plasma enhanced chemical vapor deposition process may be between about 400° C. and about 450° C. The deposition time may depend on the desired thickness of the titanium silicide layer in the subsequent process. In some embodiments, the desired thickness of the titanium silicide is between about 7 nm and about 10 nm, and the deposition time is between about 110 seconds and about 190 seconds.

[0087] In some embodiments, a higher hydrogen flow rate, a lower titanium tetrachloride flow rate, and / or a higher ratio between the hydrogen flow rate and the titanium tetrachloride flow rate can be used to selectively form titanium silicide. In some embodiments, the titanium tetrachloride flow rate is about 3.5 sccm, the hydrogen flow rate is about 1000 sccm, the RF power is about 300 watts, the chamber pressure is about 2 Torr, the station temperature is about 420°C, the deposition time is about 10 seconds, and the argon flow rate is about 800 sccm. The ratio between the hydrogen flow rate and the titanium tetrachloride flow rate can be about 286.

[0088] In some embodiments, the method of forming the initial titanium layer 119 begins with reaction (1). Titanium tetrachloride can react with hydrogen to form TiCl x (x=2-3), which further reacts with hydrogen to form titanium as shown in reaction (2). The hydrogen flow rate in reactions (1) and (2) affects the formation rate and amount of titanium. In some embodiments, when the initial titanium layer 119 is thicker, a thicker titanium silicide layer can be substantially formed in the source / drain region 110. The thicker titanium silicide layer can further reduce the contact resistance of the source / drain region 110.

[0089] When the initial titanium layer 119 is formed, the initial titanium layer 119 is also etched back and reacts with the source / drain region 110 to form titanium silicide. The deposition process shown in reactions (1) and (2), and the etch back process shown in reaction (3) can result in the titanium layer 119' being formed on the gate structure 108. Figure 4 The titanium layer 119' is shown. In some embodiments, due to the reaction between the precursor gas titanium tetrachloride and the initial titanium layer 119', the back etching can occur simultaneously with the step of forming the titanium layer. In some embodiments, the deposition rate of titanium is higher than the back etching rate of titanium, so the titanium layer 119' is formed. At the same time, while the initial titanium layer 119 is consumed to form TiCl x (x=2-3), TiCl x (x=2-3) can react with silicon in the source / drain region 110 in the presence of hydrogen to form titanium silicide in and / or on the source / drain region 110. In some embodiments, the thickness of the titanium layer 119' on the source / drain region 110 is less than the thickness of the titanium layer 119' on other locations of the contact region 125 (such as the sidewalls of the gate structure 108). In some embodiments, the initial titanium layer 119 on the source / drain region is completely consumed, and a little titanium remains on the source / drain region 110. For illustration purposes, Figure 4 The titanium layer 119 ′ is located on the source / drain region 110 .

[0090] The reaction to form the titanium layer 119' is now described in detail. In some embodiments, as titanium is formed and titanium tetrachloride continues to flow into the chamber, at least a portion of the initial titanium layer 119 reacts with titanium tetrachloride to form TiCl x (x=2-3). TiCl formed on the source / drain region 110 x (x=2-3) can react with the substrate material (such as silicon) in the source / drain region 110 to form titanium silicide (TiSi x (x=2-3)) on the fin 104 (e.g., as part of the source / drain region). At the same time, portions of the initial titanium layer 119 on other portions of the contact region 125 (e.g., the sidewalls of the gate structure 108) may be partially or completely etched. The chemical reactions for etching back the initial titanium layer 119 and forming the titanium silicide layer 121 are shown as reactions (3) and (4), which may occur simultaneously with reactions (1) and (2), or after reactions (1) and (2).

[0091] Ti+TiCl4→TiCl x (x=2-3) (3)

[0092] TiCl x (x=2-3)+2Si+H2→TiSi x (x=2-3)+Cl x+2HCl (4)

[0093] According to reactions (3) and (4), the portion of the initial titanium layer 119 contacting the source / drain region 110 can be converted into titanium silicide in the presence of silicon and hydrogen. In reaction (3), the initial titanium layer 119 reacts with titanium tetrachloride to form TiCl x (x=2-3) to etch back the initial titanium layer 119. In reaction (4), TiCl x (x=2-3) reacts with hydrogen and silicon in the source / drain region 110 to form titanium silicide on the source / drain region 110. Reaction (4) may be referred to as a "nitridation" process. In some embodiments, the sidewalls of the gate structure 108 and the initial titanium layer 119 on the source / drain region 110 may be partially or completely etched back to form TiCl x (x=2-3). In some embodiments, the results of reactions (3) and (4) only leave a small amount of titanium layer 119' or even no titanium layer 119'. In some embodiments, the TiCl generated in reactions (1) and / or (3) x (x=2-3) may react with a portion of the initial titanium layer 119 in the source / drain region 110 to form a titanium silicide layer 121 with a desired thickness (eg, between about 7 nm and about 10 nm) on and / or in the source / drain region 110 .

[0094] In some embodiments, the hydrogen flow rate in reactions (3) and (4) is about 1000 sccm, the titanium tetrachloride flow rate is about 3.5 sccm, the RF power is about 300 watts, the argon flow rate is about 800 sccm, and the chamber pressure is about 2 Torr. In some embodiments, the time of reactions (3) and (4) depends on or is related to the hydrogen flow rate, the ratio between the hydrogen flow rate and the titanium tetrachloride flow rate, the deposition rate of the titanium layer 119, the etching rate of the titanium layer 119, and / or the RF power. The time of reaction (4) can be changed to form a titanium silicide layer 121 of a desired thickness in the source / drain region 110. In some embodiments, the thickness of the titanium silicide is between about 7 nm and about 10 nm.

[0095] In some embodiments, the thickness of the titanium silicide layer 121 depends on or is related to the hydrogen flow rate and the ratio of the hydrogen flow rate to the titanium tetrachloride flow rate in reactions (1) and (3). In some embodiments, a relatively high hydrogen flow rate (e.g., 1000 sccm) in reactions (1) and (3) can result in a high titanium deposition rate (e.g., between about 1000 sccm and about 2000 sccm). / second to about / second). In summary, a texture of titanium-rich silicide can be formed in the source / drain region 110. In some embodiments, a high hydrogen flow rate can be used to form a desired thick titanium silicide layer 121. In some embodiments, a relatively high hydrogen flow rate (e.g., between about 500 sccm and about 1500 sccm) and a relatively low titanium tetrachloride flow rate (e.g., between about 1 sccm and about 20 sccm) can be used to selectively form titanium silicide on and / or in the source / drain region 110. In some embodiments, the hydrogen flow rate can be adjusted so that the titanium silicide layer 121 formed in the source / drain region 110 has a desired thickness. In some embodiments, the upper surface of the titanium silicide layer 121 can be higher than the upper surface of the gate dielectric layer 115. The lower surface of the titanium silicide layer 121 can be higher than, substantially flush with, or lower than the gate dielectric layer 115, depending on the thickness of the titanium silicide layer 121. The bottom surface of the titanium silicide layer 121 may be higher than, substantially flush with, or lower than the gate dielectric layer 115 , depending on the thickness of the titanium silicide layer 121 .

[0096] like Figure 5 As shown, another titanium layer 122 is formed between and on adjacent gate structures 108. The titanium layer 122 may be deposited for subsequent formation of titanium nitride. For illustration purposes, Figure 5 The titanium layer 119' shown is formed from the titanium silicide layer 121, and the titanium layer 122 is formed on the titanium layer 119'. In some embodiments, the titanium remaining on the contact region 125 (such as the titanium layer 122 and the titanium layer 119') is used to form titanium nitride. The titanium layer 122 can be formed by reactions (1) and (2), and the titanium layer 122 is formed by the titanium nitride layer 119'. Figure 3 The reaction for forming the initial titanium layer 119 is similar.

[0097] In some embodiments, in order to reduce the formation of titanium silicide and increase the formation of titanium nitride in the presence of titanium tetrachloride, titanium, and hydrogen, the hydrogen flow rate is reduced and the titanium tetrachloride flow rate is increased when forming titanium nitride. A lower hydrogen flow rate and a higher titanium tetrachloride flow rate can inhibit the formation of titanium silicide and promote the formation of titanium nitride. In some embodiments, a relatively low hydrogen flow rate (e.g., between about 5 sccm and about 50 sccm), a relatively high titanium tetrachloride flow rate (e.g., between about 1 sccm and about 20 sccm), and a ratio between the hydrogen flow rate and the titanium tetrachloride flow rate of about 0.25 to about 50 can be used to selectively form titanium nitride on titanium silicide. To selectively form titanium nitride in a "nitridation" process, the combination Figure 6The description is as follows. In some embodiments, the deposition time for forming the titanium layer 122 is between about 150 seconds and about 5000 seconds. In some embodiments, the deposition time for the titanium layer 122 is about 150 seconds, the chamber pressure is about 1 Torr, the flow rate of titanium tetrachloride is about 10 sccm, the flow rate of hydrogen is about 10 sccm, the ratio of the flow rate of hydrogen to the flow rate of titanium tetrachloride is about 1, and the flow rate of argon is about 600 sccm.

[0098] Figure 6 The titanium nitride layer 123 is shown formed on and between adjacent gate structures 108. In some embodiments, the titanium nitride layer 123 is formed on the source / drain regions 110 and on the offset spacers 116 adjacent to the gate structures 108. In some embodiments, the titanium nitride layer 123 is formed from the retained titanium (e.g., titanium layers 122 and 119') by chemical formulas (1) to (4). In some embodiments, the chemical reaction to form the titanium nitride layer 123 includes reaction (5) described below.

[0099] 2Ti+2NH3→2TiN+3H2 (5)

[0100] In some embodiments, reaction (5) is referred to as a "nitridation" process. Argon is used to generate and stabilize the nitridation process. The reaction time of reaction (5) (also referred to as "nitridation time") may depend on or be related to the amount of titanium deposited and the flow rate of the reaction gas (e.g., ammonia). In some embodiments, a thicker titanium layer (e.g., a thicker total thickness of titanium layers 122 and 119') may result in a longer nitridation time to form the titanium nitride layer 123. In some embodiments, nitrogen is flowed into the plasma enhanced chemical vapor deposition chamber before and during reaction (5) as part of the nitridation process. In the presence of nitrogen, ammonia and titanium may form nitrogen-passivated titanium nitride, which may improve the barrier function between the contact region 125 and a subsequently formed contact layer. The ammonia gas flow rate may be between about 500 sccm and about 5000 sccm, the argon gas flow rate may be between about 500 sccm and about 2500 sccm, and the RF power may be between about 200 watts and 750 watts. In some embodiments, the ammonia gas flow rate is about 4000 sccm, the argon gas flow rate may be about 1000 sccm, and the RF power may be about 500 watts. The nitridation time may be about 64 seconds. In some embodiments, the titanium nitride layer 123 on the offset spacer 116 of the gate structure 108 may have a thickness between about 1 nm and about 4 nm.

[0101] Compared to the hydrogen flow rate and titanium tetrachloride flow rate used to form the titanium silicide layer 121, a relatively low hydrogen flow rate and a relatively high titanium tetrachloride flow rate can be used to selectively form a nitrogen-rich titanium texture on the offset spacer 116 of the gate structure 108 through reaction (5). In some embodiments, by providing the aforementioned hydrogen flow rate and titanium tetrachloride flow rate, a nitridation process (such as reaction (5)) rather than a silicide process (such as reaction (4)) is more likely to occur when forming the titanium nitride layer 123. Therefore, the flow rates of hydrogen and titanium tetrachloride can be controlled so that the formed titanium nitride layer 123 has a desired thickness. The formed titanium nitride layer 123 can serve as a barrier layer and prevent the subsequently formed contact layer from diffusing into the offset spacer 116 and the gate structure 117.

[0102] In some embodiments, the selectivity between titanium silicide and titanium nitride is defined by the ratio of the total thickness of the titanium silicide layer 121 on the source / drain region 110 to the total thickness of the titanium nitride layer 123 on the offset spacer 116. In some embodiments, the selectivity is between about 3 and about 7.

[0103] Figure 7 Along Figure 1A The cross-sectional line 131 shown shows the titanium silicide layer 121 and the titanium nitride layer 123 formed by reactions (1) to (5), as well as the contact layer 124 (e.g., a portion of an internal connection) formed in the contact region 125. The contact layer 124 can form a contact with the titanium nitride layer 123, and the titanium nitride layer 123 can prevent metal atoms in the contact layer 124 from diffusing into the offset spacer 116, the gate structure 108, and / or the source / drain region 110. The titanium silicide layer 121 can reduce the parasitic capacitance between the contact layer 124 and the source / drain region 110. In some embodiments, the contact layer 124 includes cobalt. In other embodiments, the contact layer 124 includes other metals or metal alloys such as aluminum, copper, or the like. The method for forming the contact layer 124 can use a suitable deposition method such as chemical vapor deposition. To simplify the description, Figure 7 Omit other by-products such as residual titanium and Cl x The source / drain region 110 is partially enclosed and matched with Figure 8 Describe in detail.

[0104] Figure 8 show Figure 7 An enlarged cross-sectional view of the source / drain region 110 in the dashed circle. Figure 8 As shown, the titanium silicide layer 121 covers the source / drain region 110, and the titanium nitride layer 123 covers the titanium silicide layer 121. The contact layer 124 further covers the titanium nitride layer 123 and the titanium silicide layer 121.

[0105] Along the horizontal direction (or x-axis) in the cross-sectional view, the titanium silicide layer 121 covers the source / drain region 110 by its arc length 801, while the titanium silicide layer 121 does not cover the source / drain region 110 by its arc length 802. The total arc length of the cross section along the x-axis is the sum of the arc lengths 801 and 802. The pad coverage of the titanium silicide layer 121 on the source / drain region can be defined by the ratio between the arc length 801 and the sum of the arc lengths 801 and 802. The pad coverage of the embodiment of the present invention can be between about 65% and about 81%. In some embodiments, the pad coverage of the embodiment of the present invention is about 72%.

[0106] In addition, the length (or thickness) of the titanium silicide layer 121 along the vertical direction (or y-axis) may be between about 1.3 nm and about 19 nm. In some embodiments, the length of the titanium silicide layer 121 is between about 7 nm and about 10 nm. The titanium silicide layer 121 has a maximum length 803 and a minimum length 804. In some embodiments of the present invention, the ratio between the minimum length of the titanium silicide layer 121 along the y-axis and the maximum length of the titanium silicide layer 121 along the y-axis may be between about 35% and about 59%. In some embodiments of the present invention, the ratio between the minimum length of the titanium silicide layer 121 along the y-axis and the maximum length of the titanium silicide layer 121 along the y-axis is about 47%.

[0107] Through plasma enhanced chemical vapor deposition, the embodiment of the present invention can form a titanium silicide layer 121 with improved coverage and consistency on the source / drain region 110. The titanium silicide layer 121 has improved coverage and controlled thickness, which can reduce the parasitic capacitance between the source / drain region 110 and the contact layer 124. At the same time, the improved consistency of the titanium silicide layer 121 can further prevent the contact layer 124 from diffusing into the source / drain region 110.

[0108] In the n-type fin field effect transistor formed by the embodiment of the present invention, the general distribution of the parasitic capacitance of the source / drain region 110 may be between about 3795Ω / fin and 3980Ω / fin. In some embodiments, the parasitic capacitance is about 3823Ω / fin, which is lower than the parasitic capacitance of the interface formed by physical vapor deposition (e.g., about 3991Ω / fin). In the p-type fin field effect transistor formed by the embodiment of the present invention, the general distribution of the parasitic capacitance of the source / drain region 110 may be between about 3794Ω / fin and 3990Ω / fin. In some embodiments, the parasitic capacitance in the p-type fin field effect transistor is about 3830Ω / fin, which is lower than the parasitic capacitance of the interface formed by physical vapor deposition (e.g., about 3987Ω / fin).

[0109] Fig. 9is an exemplary cross-sectional view of a merged fin structure 900 in some embodiments. The merged fin structure 900 may include a titanium silicide layer 907 , a titanium nitride layer 906 on the titanium silicide layer 907 , and a contact layer 905 on the titanium nitride layer 906 .

[0110] like Fig. 9 As shown, fins 902 and 902' share source / drain region 901. Source / drain region 901 can be an n-type region or a p-type region. In some embodiments, source / drain region 901 combines two source / drain regions, each of which is grown on fins 902 and 902'. In some embodiments, source / drain region 901 can have Fig. 9 In some embodiments, the fin spacing 914 may be between 10 nm and 40 nm. In some embodiments, the source / drain region 901 has a partial hexagon having an upper surface 910 and a plurality of side surfaces 908 and 909. In some embodiments, the angle 911 of the side surfaces 908 and 909 may be between approximately 45° and 65°. The source / drain region 901 has a width 912 and a height 913, which may be optimized to improve device performance. In some embodiments, the width 912 may be between approximately 50 nm and 90 nm, and the height 913 may be between 40 nm and 80 nm. Those skilled in the art will appreciate that these dimensions are not intended to limit embodiments of the present invention.

[0111] In addition, the merged fin structure 900 includes a substrate 904. In some embodiments, the substrate 904 may be a semiconductor wafer, or a top layer of a semiconductor wafer on an insulating layer. For example (but not limited to), the composition of the semiconductor substrate may be silicon or another semiconductor element. For example, the substrate 904 may be (i) a semiconductor element may be germanium; (ii) a semiconductor compound including silicon carbide, gallium arsenide, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; (iii) a semiconductor alloy including silicon germanium, gallium arsenide phosphide, aluminum indium arsenide, aluminum gallium arsenide, gallium indium arsenide, gallium indium phosphide, and / or gallium indium arsenide phosphide; or (iv) any combination of the above. In addition, the composition of the fins 902 and 902' and the composition of the substrate 904 may be the same material or a different material. For example (but not limited to), the composition of the fins 902 and 902' may be silicon.

[0112] The fins 902 and 902' of the merged fin structure 900 are electrically isolated from each other by a shallow trench isolation layer 903. The shallow trench isolation layer 903 may be silicon oxide, silicon nitride, silicon oxynitride, fluorine-doped silicate glass, a dielectric material with a low dielectric constant, and / or other suitable dielectric materials with appropriate gap-filling properties. The shallow trench isolation layer 903 may be formed after the fins are formed on the substrate 904, but before the source / drain region 901 is formed. For example, the space between the fins may be filled with a dielectric material, and then the dielectric material may be partially chemically mechanically polished and etched back to expose the fins 902 and 902'. Other manufacturing methods may be used to form the shallow trench isolation layer 903. In addition, the shallow trench isolation layer 903 may be a multi-layer structure, which may include more than one layer of the aforementioned materials.

[0113] In some embodiments, the source / drain region 901 may be an epitaxial stack having two or more epitaxial layers grown in series and having the same or different dopant types and / or concentrations. Variations in these layers may be required depending on device performance requirements. In some embodiments, the merged fin structure 900 includes a third epitaxial layer (e.g., a cap layer). For example, the thickness of the first epitaxial layer may be between 10nm and 20nm. The thickness of the second epitaxial layer may be between 30nm and 60nm, and the thickness of the third epitaxial layer (e.g., a cap layer) may be less than 10nm. In some embodiments, the source / drain region 901 may have Fig. 9 A partial hexagon is shown, which is the result of the merger of two diamond-shaped source / drain regions, each grown on fins 902 and 902'. The source / drain width 912 can be monitored by in-line measurement.

[0114] In some embodiments, the epitaxial growth process of the epitaxial layer can be performed at a high wafer temperature (e.g., between 450°C and 740°C). During epitaxial growth, the process pressure can be between 1 Torr and 100 Torr, and the reactant gas can include silane, disilane, germane, diborane, hydrogen chloride, hydrogen, nitrogen, and / or argon. The above ranges and gas types are only used for illustration and are not intended to limit the embodiments of the present invention. The size and shape of the source / drain region 901 may depend on the growth conditions of each individual epitaxial layer, such as gas flow, wafer temperature, and / or process pressure.

[0115] The titanium silicide layer and the titanium nitride layer described herein may be formed on the source / drain region 901 of the merged fin structure 900, and the formation method thereof may adopt the same or similar process. Fig. 9In some embodiments shown, the merged fin structure 900 has a partial hexagonal shape, and the upper surface 910 is formed on one side of the source / drain region 901. A titanium silicide layer 907 may be formed on the upper surface 910, a titanium nitride layer 906 may be formed on the titanium silicide layer 907, and a contact layer 905 may be formed on the titanium nitride layer 906. In some embodiments, Fig. 9 The layers in the graph (including the length and coverage along the y-axis) and the interfaces between the layers can be compared with Figure 8 The layers and interfaces shown are similar. For example, the contact layer 905 can be similar to the contact layer 124, the titanium nitride layer 906 can be similar to the titanium nitride layer 123, the titanium silicide layer 907 can be similar to the titanium silicide layer 121, and the source / drain region 901 can be similar to the source / drain region 110. In another example, the ratio between the minimum length and the maximum length of the titanium silicide layer 907 along the y-axis of the merged fin structure 900 is calculated in the same manner as Figure 8 In some embodiments, the merged fin structure 900 has a hexagonal shape, and the upper surface of the merged fin structure 900 may be substantially horizontal. The titanium silicide layer and the titanium nitride layer described herein may be formed on the upper surface, and the configuration thereof is similar to that of FIG. Figure 8 and 9 Similar to that shown.

[0116] Fig.10 1 is a flow chart of a method 1000 for forming a contact region 125 with improved parasitic capacitance. Other processes may be performed between various steps of the method 1000, but the related description is omitted for clarity. For the purpose of illustration, steps 1001 to 1003 are described using a plasma enhanced chemical vapor deposition process.

[0117] In step 1001, a substrate is provided. The substrate may be any suitable semiconductor substrate such as silicon. The substrate may include a fin field effect transistor, which includes a gate structure formed on a fin. The fin is perpendicular or approximately perpendicular to the substrate surface and may be rectangular or trapezoidal. In some embodiments, the upper surface and sidewall interface of the fin may be rounded corners. The fin may be formed by a variety of dry etching techniques, such as reactive ion etching or inductively coupled plasma etching. The fin may include a source / drain region of the fin field effect transistor. The source / drain region is located on both sides of the gate structure. Figure 1A and Figure 1B As shown, step 1001 provides an exemplary substrate.

[0118] A pre-cleaning process may be performed on the substrate. The pre-cleaning process may include any suitable cleaning process such as etching to remove contamination and / or impurities on the substrate. For example, the pre-cleaning process removes oxides on the substrate. In some embodiments, the pre-cleaning process includes a dry etching process to remove silicon oxide and other particles on the surface of the substrate.

[0119] In step 1002, a relatively high flow rate of hydrogen gas and a relatively low flow rate of titanium tetrachloride are used to selectively form a titanium silicide layer.

[0120] In some embodiments, the method of forming the titanium silicide layer begins with a preheat-preflow process. The preheat-preflow process allows the reaction gas to flow into the chamber, stabilize the chamber pressure, and heat the station to the desired reaction temperature. The reaction gas may include titanium tetrachloride and hydrogen. In some embodiments, argon gas flows into the chamber to generate and stabilize the plasma in the subsequent deposition process. In some embodiments, the preheat-preflow process lasts for about 31 seconds, which includes preflowing a precursor gas such as titanium tetrachloride for about 3 seconds. In some embodiments, the gas flow rate may be the same as the flow rate in the subsequent deposition process. In some embodiments, a high ratio between the hydrogen flow rate and the titanium tetrachloride flow rate (e.g., between about 25 and about 1500) can be used to form the titanium silicide layer. In some embodiments, the titanium tetrachloride flow rate is about 3.5 sccm and the hydrogen flow rate is about 1000 sccm, resulting in a flow rate ratio of about 286. In some embodiments, the argon flow rate is about 800 sccm, the chamber pressure is about 2 Torr, and the station carrying the substrate is heated to about 420°C. In some embodiments, the time for the preheat-preflow process may be different from the time for stabilizing chamber conditions. For example, the time for the gas to flow into the chamber to reach a stable pressure may be different from the time for the heating station to reach a desired temperature. The specific parameters of the preheat-preflow process are not limited to the embodiments described herein.

[0121] In some embodiments, step 1002 includes a deposition process after a preheat-preflow process. Through the above-mentioned reactions (1) and (2), a titanium layer can be formed during the deposition process. At the same time, through the above-mentioned reaction (4), the titanium layer can react with the silicon in the source / drain region to form a titanium silicide layer on the source / drain region. In some embodiments, a portion of the titanium layer on the gate structure is partially or completely etched through the above-mentioned reaction (3). Reactions (1) to (4) can occur simultaneously or continuously, that is, a titanium silicide layer is formed in the source / drain region. In some embodiments, byproducts such as titanium and / or Cl are also formed. x In the contact area. Deposition process parameters Figure 3 and 4 As described above. In some embodiments, the hydrogen flow rate is about 1000 sccm, which can be used to achieve a high deposition rate of the titanium layer and the titanium-rich silicide texture in the source / drain region. By controlling the deposition time, a titanium silicide layer of a desired thickness can be formed in the source / drain region.

[0122] In some embodiments, step 1002 further includes a cleaning process after the deposition process. The cleaning process may evacuate the reaction chamber to remove unwanted or unused particles / gases. In some embodiments, argon gas is used in the cleaning process. In some embodiments, the cleaning process lasts for about 60 seconds and the argon gas flow rate is about 2000 sccm.

[0123] In some embodiments, step 1002 further includes a hydrogen treatment process after the purge process. The hydrogen treatment process allows hydrogen to flow into the chamber to further remove residual gases (such as titanium tetrachloride and TiCl x , x is between 2 and 3) to remove dangling bonds and unwanted residues on the surface of the substrate. In some embodiments, during the hydrogen treatment process, hydrogen is first flowed into the chamber in a first period, and then the RF power is turned on in a second period. In some embodiments, the hydrogen flow rate in the hydrogen treatment process is about 1000 sccm, and the chamber pressure is about 2 Torr. In some embodiments, the total time of the hydrogen treatment process is about 50 seconds, which includes about 30 seconds for the hydrogen flow and about 20 seconds for the plasma treatment. In some embodiments, the RF power used for the plasma treatment is about 300 watts.

[0124] In some embodiments, the deposition process, the purge process, and the hydrogen treatment process may be repeated multiple times before the subsequent step of forming silicon nitride. "Number of cycles" refers to the number of repetitions. In some embodiments, for given chamber parameters, a higher number of cycles results in a more compliant and more consistent titanium silicide layer. For example, a titanium silicide layer formed at a cycle number of 4 is more compliant and more consistent than a titanium silicide layer formed at a cycle number of 2. In some embodiments, for given chamber parameters, a higher number of cycles results in a reduced selectivity between titanium silicide and a titanium nitride layer (formed in a subsequent process). For example, the selectivity at a cycle number of 3 is lower than the selectivity at a cycle number of 1. For example, a lower number of cycles may correspond to a longer deposition time to form a titanium silicide layer formed at a higher number of cycles. In some embodiments, the number of cycles is between about 1 and 5, and the selectivity is between about 3 and 7.

[0125] In step 1003, a relatively low flow rate of hydrogen and a relatively high flow rate of titanium tetrachloride are used to selectively form a titanium nitride layer. In some embodiments, a conversion step (such as a hydrogen treatment process) is performed after the titanium silicide layer is formed to set the chamber environment for forming titanium nitride. For example, the conversion step may include a purge process to remove hydrogen from the chamber, and a reflow process to allow the reaction gas to flow in. In some embodiments, the temperature may be maintained at about 420°C. In some embodiments, the purge process includes flowing argon to remove hydrogen. In some embodiments, the argon flow rate is about 1200sccm, and the purge time is about 2 seconds. In some embodiments, a preflow process flows titanium tetrachloride gas and hydrogen. In some embodiments, the preflow time is about 6 seconds, the chamber pressure is about 1Torr, the titanium tetrachloride flow rate is about 10sccm, the argon flow rate is about 1200sccm, and the hydrogen flow rate is about 10sccm. In some embodiments, the conversion step may include other number of processes to obliquely increase the gas flow in the chamber and stabilize the chamber environment.

[0126] In some embodiments, step 1003 includes a deposition process after the conversion step. Through reactions (1) and (2), a titanium layer may be formed during the deposition process. In some embodiments, reaction (3) is performed to partially or completely etch a portion of the titanium layer on the gate structure. Reactions (1) to (3) may occur simultaneously or sequentially to form a titanium layer in the contact region. In some embodiments, byproducts (such as Cl) are also formed. x ) in the contact region. In some embodiments, the byproducts in the contact region (such as Cl x ) concentration can be between about 1×10 16 amu is about 1×10 21 amu. Deposition process parameter matching Figure 5 As described above. In some embodiments, a low ratio of hydrogen flow rate to titanium tetrachloride flow rate (e.g., between about 0.25 and about 50) can be used to form a titanium silicide layer. In some embodiments, the hydrogen flow rate is about 10 sccm and the titanium tetrachloride flow rate is about 10 sccm (i.e., the flow rate ratio of the two is about 1) to form a titanium nitride layer with high selectivity. For example, a lower hydrogen flow rate and a higher titanium tetrachloride flow rate can inhibit the formation of titanium silicide and control the thickness of the titanium layer to be formed for subsequent formation of a titanium nitride layer. By controlling the deposition time, a titanium layer of a desired thickness can be formed on and / or in the contact region.

[0127] In some embodiments, step 1003 further includes a hydrogen treatment process after the deposition process. In some embodiments, hydrogen is used to drive off any unreacted gases (such as titanium tetrachloride and TiCl x(x=2 to 3)), i.e., removing dangling bonds and residues on the substrate. In some embodiments, the chamber pressure is about 1 Torr, the processing time is about 3 seconds, and the hydrogen flow rate is about 10 sccm. In some embodiments, argon gas is used to generate and stabilize the plasma, which can be used to remove dangling bonds. In some embodiments, the argon flow rate is about 600 sccm, and the RF power is about 300 watts.

[0128] In some embodiments, step 1003 further includes a nitridation process after the hydrogen treatment process. A conversion step may be performed at the beginning of the nitridation process to remove hydrogen and stabilize chamber conditions. In some embodiments, the conversion step includes a purge sub-step and a vacuum sub-step. In some embodiments, the purge sub-step begins after the hydrogen treatment process to flow in argon and hydrogen. In some embodiments, the argon flow rate is about 1800 sccm, the hydrogen flow rate is about 10 sccm, the chamber pressure is about 0 Torr, and the time of the purge sub-step is about 10 seconds. In some embodiments, a vacuum sub-step is performed after the purge sub-process, which lasts for about 2 seconds. In some embodiments, the chamber pressure in the conversion step is about 0 Torr. In some embodiments, the conversion step removes hydrogen that is not used in subsequent reactions of the nitridation process. In some embodiments, the hydrogen used in step 1002 and the hydrogen used in step 1003 flow into the reaction chamber through different gas inlets. Therefore, the flow rates of the two steps can be controlled separately to achieve higher control accuracy. In summary, the flow rate accuracy of each step is improved.

[0129] In some embodiments, the nitridation process includes a nitrogen pre-flow process. The nitrogen pre-flow process allows nitrogen to flow into the chamber to produce a nitrogen-rich atmosphere used in a subsequent nitrogen treatment sub-process. The nitrogen can react with ammonia (such as ammonia that flows into the chamber later) to form a nitrogen-passivated titanium nitride layer. The nitrogen-passivated nitride layer can improve the barrier between the contact layer and the gate structure. At the same time, argon flows into the chamber to generate and stabilize the plasma in subsequent sub-processes. In some embodiments, the argon flow rate is about 2000 sccm, the ammonia flow rate is about 4000 sccm, the chamber pressure is about 3 Torr, and the pre-flow time is about 12 seconds.

[0130] In some embodiments, the nitridation process further includes a nitrogen treatment sub-step (or nitrogen pretreatment) after the nitrogen pre-flow step. In the nitrogen treatment sub-step, the nitrogen gas flowing into the chamber can be ionized to produce a nitrogen-rich atmosphere and a nitrogen plasma. In some embodiments, the ionization process is combined with a subsequent ammonia flow and / or ammonia treatment to form a nitrogen-passivated titanium nitride layer. In some embodiments, the RF power is about 500 watts, the nitrogen flow rate is about 4000 sccm, the nitrogen treatment time is about 20 seconds, the argon flow rate is about 2000 sccm, the chamber pressure is about 3 Torr, and the ammonia flow rate is about 4000 sccm.

[0131] In some embodiments, the nitridation process further includes an ammonia flow step after the nitrogen pre-flow step. The ammonia flow step can use hydrogen as a carrier gas to flow ammonia into the chamber and establish chamber conditions for the subsequent reaction between ammonia and titanium. In some embodiments, the ammonia flow time is about 12 seconds, the argon flow rate is about 2000 sccm, the chamber pressure is about 3 Torr, the hydrogen flow rate is about 4500 sccm, and the ammonia flow rate is about 4000 sccm.

[0132] In some embodiments, the nitridation process further includes an ammonia treatment sub-step after the ammonia gas flow step. In some embodiments, the ammonia treatment sub-step can react ammonia (using hydrogen as a carrier gas) with the titanium layer formed on the contact region (such as the titanium layer formed by the deposition process of step 1002 and step 1003) to form a titanium nitride layer on the contact region. In some embodiments, Figure 6 The reaction (5) is carried out in the presence of nitrogen plasma to form a nitrogen-passivated titanium nitride layer on the contact layer. In some embodiments, the ammonia flow time is about 20 seconds, the argon flow rate is about 2000 sccm, the chamber pressure is about 3 Torr, the hydrogen flow rate is about 4500 sccm, the RF power is about 500 watts, and the ammonia flow rate is about 4000 sccm.

[0133] In some embodiments, a pull-back process is performed after forming the titanium nitride layer and before depositing the contact layer in the contact region. The pull-back process can remove excess thickness of the titanium nitride and make the titanium nitride layer have a desired thickness and smoothness. In some embodiments, the pull-back process includes rinsing the substrate with hydrogen peroxide.

[0134] In some embodiments, after forming the titanium nitride layer and / or the pull-back process, a contact layer is formed in the contact region. The contact layer may form a contact with the titanium nitride. The contact layer may include any suitable metal or metal alloy, and the formation method may be any suitable deposition method. For example, the contact layer may include aluminum, copper, cobalt, any other suitable metal, or any combination of the above. In some embodiments, the contact layer includes cobalt.

[0135] Chemical vapor deposition is performed sequentially in the same reaction chamber to form a titanium silicide layer and a titanium nitride layer. The thickness of the titanium silicide layer and the titanium nitride layer can be controlled by adjusting the flow rate of hydrogen and the precursor titanium tetrachloride. In other words, the appropriate flow rate of hydrogen and titanium tetrachloride (or the ratio between the hydrogen flow rate and the titanium tetrachloride flow rate) can be selected to selectively form or deposit a titanium silicide layer or a titanium nitride layer. The above method can simultaneously control the thickness ratio between the titanium silicide layer and the titanium nitride layer. Before forming the above two layers, the gas in the reaction chamber can be driven away to remove potential contamination and establish the conditions of the reaction chamber for subsequent chemical vapor deposition. In addition, the benefit of not having to switch the reaction chamber is to improve the film quality and compliance of the titanium silicide layer and the titanium nitride layer, and to reduce the production time. The structure thus formed has a reduced parasitic capacitance between the contact layer and the source / drain region, and improves the barrier between the contact layer and the gate structure.

[0136] In some embodiments, a method for making a semiconductor structure includes providing a substrate having a gate structure, an insulating structure on the gate structure, and a source / drain region, and depositing a titanium silicide layer on the source / drain region by a first chemical vapor deposition process. The first chemical vapor deposition process includes a first hydrogen gas flow. The method also includes depositing a titanium nitride layer on the insulating structure by a second chemical vapor deposition process. The second chemical vapor deposition process includes a second hydrogen gas flow. The first chemical vapor deposition process and the second chemical vapor deposition process are performed in a single reaction chamber, and the flow rate of the first hydrogen gas flow is greater than the flow rate of the second hydrogen gas flow.

[0137] In some embodiments, the step of forming the titanium silicide layer includes: depositing a first titanium layer on the source / drain region based on a first hydrogen flow; and converting at least a portion of the first titanium layer on the source / drain region into a titanium silicide layer based on the first hydrogen flow.

[0138] In some embodiments, the step of forming the titanium nitride layer includes: depositing a second titanium layer on the sidewall of the insulating structure based on a second hydrogen flow; and converting at least a portion of the second titanium layer on the sidewall of the insulating structure into the titanium nitride layer.

[0139] In some embodiments, the first CVD process and the second CVD process each include a plasma enhanced CVD process.

[0140] In some embodiments, the flow rate of the first hydrogen gas flow is between about 500 sccm and about 1500 sccm, and the flow rate of the second hydrogen gas flow is between about 5 sccm and about 50 sccm; the power of the first chemical vapor deposition process and the second chemical vapor deposition process is between about 200 watts and about 750 watts; the flow rate of argon gas in the first chemical vapor deposition process is between about 40 sccm and about 2500 sccm, and the flow rate of argon gas in the second chemical vapor deposition process is between about 500 sccm and about 2200 sccm; and the flow rate of titanium tetrachloride gas for the first chemical vapor deposition process and the second chemical vapor deposition process is between about 1 sccm and about 20 sccm.

[0141] In some embodiments, the flow rate of the first hydrogen gas flow is about 1000 sccm, and the flow rate of the second hydrogen gas flow is about 10 sccm; and the flow rate of the titanium tetrachloride gas for the first chemical vapor deposition process is about 3.5 sccm, and the flow rate of the titanium tetrachloride gas for the second chemical vapor deposition process is about 10 sccm.

[0142] In some embodiments, the thickness of the titanium silicide layer on the source / drain region is between about 7 nm and about 10 nm; the thickness of the titanium nitride layer on the sidewall of the insulating structure is between about 1 nm and about 4 nm; and the ratio between the thickness of the titanium silicide layer on the source / drain region and the thickness of the titanium nitride layer on the sidewall of the insulating structure is between about 3 and about 7.

[0143] In some embodiments, the step of converting at least a portion of the second titanium layer on the sidewall of the insulating structure into a titanium nitride layer includes nitriding the second titanium layer using ammonia gas, wherein a flow rate of the ammonia gas is between about 500 sccm and about 5000 sccm.

[0144] In some embodiments, the first chemical vapor deposition process includes at least one cycle, and each cycle includes a first deposition sub-process to form at least a portion of the titanium silicide layer, a purge sub-process to remove residual gas, and a first hydrogen treatment sub-process to clean the substrate.

[0145] In some embodiments, the first chemical vapor deposition process includes 1 to 5 cycles.

[0146] In some embodiments, the second chemical vapor deposition process includes a second deposition sub-process to form at least a portion of the second titanium layer and a nitridation sub-process to form the titanium nitride layer, and wherein the deposition time of the second deposition sub-process is between about 150 seconds and about 5000 seconds.

[0147] In some embodiments, a method for making a semiconductor structure includes providing a substrate having a source / drain region; depositing a titanium silicide layer on the source / drain region by a first deposition process having a first flow rate ratio of hydrogen gas to a precursor; and depositing a titanium nitride layer on the titanium silicide layer by a second deposition process having a second flow rate ratio of hydrogen gas to a precursor, wherein the first flow rate ratio of hydrogen gas to a precursor is greater than the second flow rate ratio of hydrogen gas to a precursor.

[0148] In some embodiments, the flow rate of hydrogen gas in the first deposition process is between about 500 sccm and about 1500 sccm, the flow rate of the precursor is between about 1 sccm and about 20 sccm, and the flow rate ratio of the first hydrogen gas to the precursor is between about 25 and about 1500; and the flow rate of hydrogen gas in the second deposition process is between about 5 sccm and about 50 sccm, the flow rate of the precursor is between about 1 sccm and about 20 sccm, and the flow rate ratio of the second hydrogen gas to the precursor is between about 0.25 and about 50.

[0149] In some embodiments, the precursor includes titanium tetrachloride.

[0150] In some embodiments, the semiconductor structure includes a substrate, and the substrate includes a first gate structure, a first insulating structure on the first gate structure, a second gate structure, a second insulating structure on the second gate structure, and a source / drain region between the first gate structure and the second gate structure. The semiconductor structure also includes a titanium nitride layer located on the sidewalls of the first insulating structure and the second insulating structure; a titanium silicide layer located on the source / drain region; and a contact layer located on the titanium silicide layer and between the first insulating structure and the second insulating structure. The ratio between the thickness of the titanium silicide layer and the thickness of the titanium nitride layer is between about 3 and about 7.

[0151] In some embodiments, the contact layer includes cobalt, the source / drain region includes n-type dopants, and the parasitic capacitance between the contact layer and the source / drain region is between about 3795Ω / fin and about 3980Ω / fin.

[0152] In some embodiments, the contact layer includes cobalt, the source / drain regions include p-type dopants, and the parasitic capacitance between the contact layer and the source / drain regions is between about 3794Ω / fin and about 3990Ω / fin.

[0153] In some embodiments, the liner coverage between the cross-sectional length of the titanium silicide and the cross-sectional length of the source / drain regions is between about 65% and about 81%.

[0154] In some embodiments, a ratio between the minimum thickness and the maximum thickness of the titanium silicide layer is between about 35% and about 59%.

[0155] In some embodiments, the thickness of the titanium nitride layer is between about 1 nm and about 4 nm; and the thickness of the titanium silicide layer is between about 7 nm and about 10 nm.

[0156] It should be understood that the purpose of the detailed description (not the abstract) is to illustrate the claims. The abstract may be one or more (but not all) exemplary embodiments, and thus is not intended to limit the claims.

[0157] The features of the above embodiments or examples are helpful for those skilled in the art to understand the embodiments of the present invention. Those skilled in the art should understand that the embodiments of the present invention can be used as a basis to design and change other processes and structures to achieve the same purpose and / or the same advantages of the above embodiments. Those skilled in the art should also understand that these equivalent substitutions do not depart from the spirit and scope of the present invention, and can be changed, replaced, or modified without departing from the spirit and scope of the present invention.

Claims

1. A method for manufacturing a semiconductor structure, include: forming a fin having a source / drain region on a substrate; forming a gate structure on the fin; forming an insulating structure on the gate structure; forming a spacer on the sidewall of the gate structure and the upper surface of the fin; wherein the upper surface of the source / drain region is vertically higher than the upper surface of the fin; Depositing a titanium silicide layer on the source / drain region by a first chemical vapor deposition process, wherein the first chemical vapor deposition process includes a first hydrogen gas flow, wherein an upper surface of the titanium silicide layer is formed on a first surface plane vertically higher than an upper surface of the fin, and a lower surface of the titanium silicide layer is formed on a second surface plane vertically lower than an upper surface of the fin; and A titanium nitride layer is deposited on the insulating structure by a second chemical vapor deposition process, and the second chemical vapor deposition process includes a second hydrogen flow, wherein the first chemical vapor deposition process and the second chemical vapor deposition process are performed in a single reaction chamber, and the flow rate of the first hydrogen flow is greater than the flow rate of the second hydrogen flow.

2. The method for manufacturing a semiconductor structure as claimed in claim 1, wherein the step of forming the titanium silicide layer include: Depositing a first titanium layer on the source / drain region using the first hydrogen flow; as well as A portion of the first titanium layer is converted into the titanium silicide layer using the first hydrogen flow.

3. The method for manufacturing a semiconductor structure as claimed in claim 2, wherein the step of forming the titanium nitride layer include: Depositing a second titanium layer on the sidewall of the insulating structure using the second hydrogen flow; as well as A portion of the second titanium layer is converted into the titanium nitride layer. 4 . The method for fabricating a semiconductor structure as claimed in claim 3 , wherein the first chemical vapor deposition process and the second chemical vapor deposition process each comprise a plasma enhanced chemical vapor deposition process.

5. The method for manufacturing a semiconductor structure according to claim 1, wherein The flow rate of the first hydrogen gas flow is between 500 sccm and 1500 sccm, and the flow rate of the second hydrogen gas flow is between 5 sccm and 50 sccm; The power of the first chemical vapor deposition process and the second chemical vapor deposition process is between 200 watts and 750 watts; The argon gas flow rate in the first chemical vapor deposition process is between 40 sccm and 2500 sccm, and the argon gas flow rate in the second chemical vapor deposition process is between 500 sccm and 2200 sccm; and The flow rate of the titanium tetrachloride gas in the first chemical vapor deposition process and the second chemical vapor deposition process is between 1 sccm and 20 sccm.

6. The method for manufacturing a semiconductor structure according to claim 1, wherein The flow rate of the first hydrogen gas flow is 1000 sccm, and the flow rate of the second hydrogen gas flow is 10 sccm; and The flow rate of the titanium tetrachloride gas in the first chemical vapor deposition process is 3.5 sccm, and the flow rate of the titanium tetrachloride gas in the second chemical vapor deposition process is 10 sccm.

7. The method for manufacturing a semiconductor structure according to claim 1, in: The step of forming the titanium silicide layer includes depositing the titanium silicide layer to a thickness between 7 nm and 10 nm; and The step of forming the titanium nitride layer includes depositing the titanium nitride layer with a thickness between 1 nm and 4 nm.

8. The method for manufacturing a semiconductor structure as claimed in claim 3, wherein the step of converting the portion of the second titanium layer into the titanium nitride layer comprises nitriding the second titanium layer with ammonia gas, wherein the flow rate of the ammonia gas is between 500 sccm and 5000 sccm.

9. The method for manufacturing a semiconductor structure according to claim 1, wherein the first chemical vapor deposition process comprises at least one cycle, and the at least one cycle include: a first deposition subprocess forming at least a portion of the titanium silicide layer; A purification sub-process to remove residual gas; as well as A first hydrogen treatment sub-process is performed to clean the substrate. 10 . The method for fabricating a semiconductor structure as claimed in claim 9 , wherein the first chemical vapor deposition process comprises 1 to 5 cycles.

11. The method for manufacturing a semiconductor structure according to claim 1, wherein the second chemical vapor deposition process include: a second deposition subprocess forming at least a portion of a second titanium layer; as well as A nitridation sub-process is used to form the titanium nitride layer, wherein the deposition time of the second deposition sub-process is between 150 seconds and 5000 seconds. 12 . The method for fabricating a semiconductor structure as claimed in claim 1 , wherein the step of forming the titanium silicide layer and the titanium nitride layer comprises making the ratio between the thickness of the titanium silicide layer and the thickness of the titanium nitride layer be between 3 and 7.

13. A method for manufacturing a semiconductor structure, include: forming a source / drain region on a fin on a substrate; forming a spacer on the upper surface of the fin adjacent to the source / drain region; Depositing a titanium silicide layer on the source / drain region by a first deposition process having a first flow rate ratio of hydrogen gas to precursor, wherein an upper surface of the titanium silicide layer is formed on a first horizontal plane vertically higher than an upper surface of the fin, and a lower surface of the titanium silicide layer is formed on a second horizontal plane vertically lower than an upper surface of the fin; and A titanium nitride layer is deposited on the titanium silicide layer by a second deposition process having a second hydrogen to precursor flow rate ratio, wherein the first hydrogen to precursor flow rate ratio is greater than the second hydrogen to precursor flow rate ratio.

14. The method for manufacturing a semiconductor structure according to claim 13, wherein The flow rate of hydrogen gas in the first flow rate ratio of hydrogen gas to precursor is between 500 sccm and 1500 sccm, the flow rate of the precursor in the first flow rate ratio of hydrogen gas to precursor is between 1 sccm and 20 sccm, and the flow rate ratio of the first hydrogen gas to precursor is between 25 and 1500; and The flow rate of hydrogen in the second flow rate ratio of hydrogen gas to precursor is between 5 sccm and 50 sccm, the flow rate of the precursor in the second flow rate ratio of hydrogen gas to precursor is between 1 sccm and 20 sccm, and the flow rate ratio of the second hydrogen gas to precursor is between 0.25 and 50.

15. The method for fabricating a semiconductor structure as claimed in claim 14, wherein the precursor comprises titanium tetrachloride.

16. A method of manufacturing a semiconductor structure, include: forming a fin on a substrate; forming a gate structure on the fin; forming a spacer on the sidewall of the gate structure and the upper surface of the first portion of the fin; forming a source / drain region on the second portion of the fin, wherein an upper surface of the source / drain region is vertically higher than an upper surface of the first portion of the fin; Depositing a silicide layer on the source / drain region and the first portion of the spacer by a first deposition process including a first precursor gas flow, wherein an upper surface of the silicide layer is formed on a first surface plane vertically higher than an upper surface of the first portion of the fin, and a lower surface of the silicide layer is formed on a second surface plane vertically lower than an upper surface of the first portion of the fin; and Depositing a nitride layer on the second portion of the spacer by a second deposition process comprising a second precursor gas flow, The first deposition process and the second deposition process are performed in a single reaction chamber, and the flow rate of the second precursor gas flow is greater than the flow rate of the first precursor gas flow.

17. The method for manufacturing a semiconductor structure according to claim 16, wherein the step of depositing the silicide layer include: Depositing a first metal layer on the source / drain region and the spacer using the first precursor gas flow and a first hydrogen gas flow; as well as The first hydrogen flow is used to convert a portion of the first metal layer into the silicide layer.

18. The method for manufacturing a semiconductor structure according to claim 17, wherein the step of depositing the nitride layer include: Depositing a second metal layer along the sidewall of the spacer using the second precursor gas flow and a second hydrogen gas flow; as well as A portion of the second metal layer is nitrided into the nitride layer by using an ammonia flow. 19 . The method for fabricating a semiconductor structure as claimed in claim 18 , wherein a flow rate of the first hydrogen gas flow is greater than a flow rate of the second hydrogen gas flow.

20. The method for manufacturing a semiconductor structure according to claim 18, wherein the step of depositing the silicide layer comprises depositing a first metal layer on the source / drain region and converting a first portion of the first metal layer into the silicide layer; and The step of depositing the nitride layer includes depositing a second metal layer on the second portion of the first metal layer.

21. A semiconductor structure, include: a substrate; A first gate structure and a second gate structure are located on the substrate; A first insulating structure and a second insulating structure are respectively located on the first gate structure and the second gate structure; a source / drain region located between the first gate structure and the second gate structure; a titanium silicide layer located on the source / drain region, wherein an upper surface of the titanium silicide layer is located at a first surface plane vertically higher than an upper surface of a channel region under the first gate structure, and a lower surface of the titanium silicide layer is located at a second surface plane vertically lower than an upper surface of the channel region; a titanium nitride layer, located on the titanium silicide layer and on the sidewalls of the first insulating structure and the second insulating structure; and A contact layer is located on the titanium silicide layer and between the first insulating structure and the second insulating structure. 22 . The semiconductor structure of claim 21 , wherein a ratio of a thickness of the titanium silicide layer to a thickness of the titanium nitride layer is 3 to 7. 23 . The semiconductor structure of claim 21 , further comprising a first spacer and a second spacer respectively located on sidewalls of the first gate structure and the second gate structure, wherein the titanium nitride layer is located on the sidewalls of the first spacer and the second spacer. 24 . The semiconductor structure of claim 21 , further comprising a first spacer and a second spacer respectively disposed on sidewalls of the first gate structure and the second gate structure, wherein the titanium silicide layer is disposed on sidewalls of the first spacer and the second spacer.

25. The semiconductor structure as described in claim 21 further includes a first spacer and a second spacer respectively located on the sidewalls of the first gate structure and the second gate structure, wherein the thickness of the titanium silicide layer on the source / drain region is greater than the thickness of the titanium nitride layer on the sidewalls of the first spacer and the second spacer.

26. The semiconductor structure of claim 21, wherein The thickness of the titanium nitride layer is between 1 nm and 4 nm; and The thickness of the titanium silicide layer is between 7 nm and 10 nm.

27. The semiconductor structure of claim 21, wherein a layer coverage between a cross-sectional length of the titanium silicide and a cross-sectional length of the source / drain region is 65% to 81%.

28. The semiconductor structure of claim 21, wherein a thickness ratio of a minimum thickness to a maximum thickness of the titanium silicide layer is between 35% and 59%.

29. The semiconductor structure of claim 21, wherein the contact layer comprises cobalt and the source / drain regions comprise n-type dopants.

30. The semiconductor structure of claim 21, wherein the contact layer comprises cobalt and the source / drain regions comprise p-type dopants.

31. A semiconductor structure, include: a substrate; a fin-shaped structure located on the substrate; a source / drain region located on the first portion of the fin structure; a gate structure having a gate dielectric layer located on the second portion of the fin structure; a titanium silicide layer located on the source / drain region, wherein an upper surface of the titanium silicide layer is located at a first surface plane vertically higher than an upper surface of the gate dielectric layer, and a lower surface of the titanium silicide layer is located at a second surface plane vertically lower than an upper surface of the gate dielectric layer; and A titanium nitride layer is located on the titanium silicide layer. 32 . The semiconductor structure of claim 31 , wherein a ratio of a thickness of the titanium silicide layer to a thickness of the titanium nitride layer is 3 to 7.

33. The semiconductor structure of claim 31, further comprising a spacer disposed on a sidewall of the gate structure, wherein the titanium nitride layer is disposed on the spacer.

34. The semiconductor structure of claim 31, further comprising a spacer disposed on a sidewall of the gate structure, wherein the titanium silicide layer is disposed on the spacer.

35. The semiconductor structure of claim 31, wherein a thickness of the titanium silicide layer on the source / drain region is greater than a thickness of the titanium nitride layer on the sidewall of the gate structure. 36 . The semiconductor structure of claim 31 , further comprising another fin structure located on the substrate, wherein the source / drain region is a merged source / drain region located on the fin structure and the other fin structure.

37. A semiconductor structure, include: a substrate; a source / drain region located on the substrate; A gate structure having a gate dielectric layer is located on the substrate; a titanium silicide layer located on the source / drain region, wherein an upper surface of the titanium silicide layer is located at a first horizontal plane vertically higher than an upper surface of the gate dielectric layer, and a lower surface of the titanium silicide layer is located at a second horizontal plane vertically lower than an upper surface of the gate dielectric layer; and A titanium nitride layer is located on the titanium silicide layer.

38. The semiconductor structure of claim 37, wherein a thickness of the titanium silicide layer on the source / drain regions is greater than a thickness of the titanium nitride layer on the sidewalls of the gate structure. 39 . The semiconductor structure of claim 37 , wherein a ratio of a thickness of the titanium silicide layer to a thickness of the titanium nitride layer is 3 to 7.

40. The semiconductor structure of claim 37, further comprising a contact plug on the titanium silicide layer.

Citation Information

Patent Citations

  • Methods of producing integrated circuit devices utilizing tantalum amine derivatives

    US20040235285A1

  • Densification process for titanium nitride layer for submicron applications

    US20100151676A1

  • Method for fabricating a thin-film transistor

    US5470768A

  • Method of forming a hole in the sub quarter micron range

    US6090674A