Method for etching film and plasma processing device

By forming a monomolecular layer on the organic film and using oxidative species to etch to form a protection area, the problem of uneven protection on the side wall of the film opening in the prior art is solved, and uniform protection and etching protection on the high aspect ratio opening are achieved. .

CN110544628BActive Publication Date: 2024-10-11TOKYO ELECTRON LTD
View PDF 18 Cites 0 Cited by

Patent Information

Application Number
CN201910444639.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-05-28
Filing Date
2019-05-27
Publication Date
2024-10-11
Estimated Expiration
2039-05-27

AI Technical Summary

Technical Problem

The existing technology makes it difficult to uniformly form a protective area on the opening side wall of the film, and the protective area cannot effectively prevent the influence of etching chemical species, especially when a high aspect ratio opening is formed.

Method used

A monomolecular layer of the precursor is formed on the organic film and etched from the plasma using oxidative species to form a protective area, ensuring that the protective area and etching process are carried out simultaneously to avoid closing the openings while being evenly distributed on the high aspect ratio sidewall surface .

Benefits of technology

It achieves a uniform protection area that does not close the membrane opening, preventing etching chemicals from affecting the side wall surface, and at the same time forming a protection area on the high aspect ratio opening, effectively suppressing the expansion of the opening.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN110544628B_ABST
    Figure CN110544628B_ABST
Patent Text Reader

Abstract

The present invention provides a method for uniformly forming a protective region in a surface to protect a side wall surface from a chemical species used to etch the film without closing the opening of the film. In the method for etching the film of the illustrated embodiment, a monomolecular layer of a precursor is formed on the film. The film has a side wall surface and a bottom surface for forming an opening. The film is etched using a chemical species that comes from a plasma formed from a process gas. During the etching of the film, a protective region is formed from a monomolecular layer using a chemical species from the plasma or other chemical species from the plasma.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Illustrated embodiments of the present invention relate to a method of etching a film and a plasma processing apparatus. Background Art

[0002] In the manufacture of electronic devices, films are subjected to plasma etching. In plasma etching, plasma is generated from a gas in a chamber. A substrate placed in the chamber is etched by chemical species from the plasma.

[0003] In plasma etching, in order to suppress the expansion of the opening formed in the film in the lateral direction (i.e., in the direction perpendicular to the film thickness direction), a protective region is sometimes formed on the side wall surface of the film used to form the opening. The technology including the process of forming the protective region and the process of etching the film is described in, for example, Patent Documents 1 to 3.

[0004] In the techniques described in Patent Documents 1 to 3, an organic film is etched. In the techniques described in Patent Documents 1 and 2, a protective region containing silicon is formed on a side wall surface by sputtering. The protective region protects the organic film from the influence of oxidative species that etches the organic film. In the technique described in Patent Document 3, the organic film is etched by plasma etching using a gas containing carbonyl sulfide, oxygen, and chlorine. When plasma is generated, sulfur species and silicon chloride species are generated. The sulfur species and silicon chloride species form a protective region on the side wall surface. In the technique described in Patent Document 3, the protective region is formed simultaneously with the etching of the organic film.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2012-204668

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-049141

[0009] Patent Document 3: Japanese Patent Application Publication No. 2015-012178 Summary of the invention

[0010] Technical problem to be solved by the invention

[0011] It is required to form a protective region uniformly in the surface without closing the opening of the film, and the protective region is used to protect the side wall surface from the chemical species that etch the film. In addition, it is required that the protective region can be formed on the side wall surface for forming an opening with a high aspect ratio.

[0012] Technical solutions for solving technical problems

[0013] According to an exemplary embodiment, a method for etching a film is provided. The film is an organic film. The organic film has a sidewall surface and a bottom surface for forming an opening. The method includes: (i) a process of forming a monomolecular layer of a precursor on the organic film; and (ii) a process of etching the organic film using an oxidizing chemical species, the oxidizing chemical species coming from a plasma formed from an oxygen-containing gas. In the process of etching the organic film, the monomolecular layer is oxidized using the oxidizing chemical species from the plasma to form a protective region.

[0014] Effects of the Invention

[0015] According to a method for etching a film in an exemplary embodiment, a protective region can be formed uniformly in the surface without closing the opening of the film, and the protective region is used to protect the side wall surface from the chemical species used to etch the film. In addition, the protective region can be formed on the side wall surface used to form an opening with a high aspect ratio. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a flow chart showing a method of etching a film according to an exemplary embodiment.

[0017] Figure 2 This is a partially enlarged cross-sectional view of an example of a substrate.

[0018] Figure 3 FIG. 1 is a diagram schematically showing a plasma processing apparatus according to an exemplary embodiment.

[0019] Figure 4 (a) is used to illustrate Figure 1 FIG. 1 shows an example of step STa of the method shown in FIG. Figure 4 (b) is a partially enlarged cross-sectional view of an example of a substrate in a state after step STa is performed.

[0020] Figure 5 yes Figure 1 FIG. 1 is a partially enlarged cross-sectional view of an example of a substrate in a state after step ST1 of the method shown in FIG.

[0021] Figure 6 (a) is used to illustrate Figure 1 FIG. 1 is a diagram showing an example of step ST3 of the method shown in FIG. Figure 6 (b) is a partially enlarged cross-sectional view of an example of a substrate in a state after step ST3 is performed.

[0022] Figure 7 Yes Execution Figure 1 A partially enlarged cross-sectional view of an example of a substrate in a state after the method shown.

[0023] Description of Reference Numerals

[0024] MT...Method for etching a film

[0025] EF…membrane

[0026] OP...open your mouth

[0027] SS...Side wall

[0028] BS... bottom

[0029] ML...monolayer

[0030] PR... Protected Area

[0031] PL3...Plasma. DETAILED DESCRIPTION

[0032] Various exemplary embodiments are described below.

[0033] In an exemplary embodiment, a method for etching a film is provided. The film is an organic film. The organic film has a sidewall surface and a bottom surface for forming an opening. The method includes: (i) a process of forming a monomolecular layer of a precursor on the organic film; and (ii) a process of etching the organic film using an oxidizing chemical species, wherein the oxidizing chemical species is from a plasma formed from an oxygen-containing gas. In the process of etching the organic film, the monomolecular layer is oxidized using the oxidizing chemical species from the plasma to form a protective region.

[0034] In the method of an exemplary embodiment, the protection region is formed from a monomolecular layer. Therefore, it is possible to suppress the situation where the protection region closes the opening of the organic film. In addition, the protection region can be formed uniformly in the surface. In addition, the protection region can also be formed on the side wall surface for forming an opening with a high aspect ratio. In this method, the protection region is formed by oxidizing the monomolecular layer using oxidizing chemical species, and the above-mentioned oxidizing chemical species comes from the plasma generated for etching the organic film. Therefore, the treatment for converting the monomolecular layer into the protection region is carried out simultaneously with the etching of the organic film.

[0035] In a method of an exemplary embodiment, the precursor may contain silicon. In a method of an exemplary embodiment, the precursor may contain a metal. The metal may be tungsten or titanium.

[0036] In the method according to an exemplary embodiment, the step of forming the opening in the organic film may be further included.

[0037] In the method of one exemplary embodiment, the step of forming a monomolecular layer and the step of etching the organic film may be repeated alternately.

[0038] In a method of an exemplary embodiment, the steps of forming a monomolecular layer and etching the organic film may be performed in a space continuously maintained at a reduced pressure in a chamber of a plasma processing apparatus without removing a substrate having an organic film from the chamber.

[0039] In a method of an exemplary embodiment, the plasma processing apparatus may be a capacitively coupled plasma processing apparatus. The plasma processing apparatus may include: a chamber, a support table, a gas supply unit, a first high-frequency power supply, and a second high-frequency power supply. The support table includes a lower electrode configured to support a substrate in the chamber. The gas supply unit is configured to supply a precursor gas containing a precursor and an oxygen-containing gas into the chamber. The upper electrode is disposed above the support table. The first high-frequency power supply is configured to supply a first high-frequency power for generating plasma to the upper electrode. The second high-frequency power supply is configured to supply a second high-frequency power for introducing ions into the substrate to the lower electrode.

[0040] In another exemplary embodiment, a method for etching a film is provided. The film has a sidewall surface and a bottom surface for forming an opening. The method includes: (i) forming a monomolecular layer of a precursor on the film; and (ii) etching the film using a chemical species, wherein the chemical species is from a plasma formed from a process gas. In the step of etching the film, a protective region is formed from the monomolecular layer using a chemical species from the plasma or another chemical species from the plasma.

[0041] In the method of an illustrative embodiment, the protection region is formed from a monomolecular layer. Therefore, it is possible to suppress the situation where the protection region closes the opening of the film. In addition, the protection region can be formed uniformly in the surface. In addition, the protection region can also be formed on the side wall surface for forming an opening with a high aspect ratio. In this method, chemical species from the plasma generated for etching the film or other chemical species from the plasma degenerate the monomolecular layer, resulting in the formation of the protection region. Therefore, the treatment for converting the monomolecular layer into the protection region is carried out simultaneously with the etching of the organic film.

[0042] In an exemplary embodiment, the film may be a low dielectric constant film containing silicon, carbon, oxygen and hydrogen. The precursor may contain silicon. The chemical species used to etch the film may include fluorine species and nitrogen species. In the method of this embodiment, the precursor is nitrided using nitrogen species.

[0043] In an exemplary embodiment, the film may be a low dielectric constant film containing silicon, carbon, oxygen and hydrogen. The precursor may contain a metal. The chemical species used to etch the film may include fluorine species and nitrogen species. In the method of this embodiment, the other chemical species may include an oxygen species. In the method of this embodiment, the precursor is nitrided using an oxygen species. The metal may be tungsten or titanium.

[0044] In an exemplary embodiment, the film may be a polysilicon film. The precursor may contain silicon or metal. The chemical species used to etch the film may contain halogen chemical species. The other chemical species may contain oxidative chemical species. In the method of this embodiment, the precursor is nitrided using oxidative chemical species. The metal may be tungsten or titanium.

[0045] In an exemplary embodiment, the film may be a silicon oxide film. The precursor may contain silicon or metal. The chemical species used to etch the film may include chemical species formed from hydrofluorocarbons in the process gas. The other chemical species may include oxidative chemical species. In the method of this embodiment, the precursor is nitrided using oxidative chemical species. The metal may be tungsten or titanium.

[0046] In addition, in another exemplary embodiment, a plasma processing device is provided. The plasma processing device includes: a chamber, a support table, a gas supply unit, a plasma generating unit, and a control unit. The support table is configured to support a substrate in the chamber. The gas supply unit is configured to supply a precursor gas containing a precursor and a processing gas into the chamber. The plasma generating unit is configured to generate plasma of the processing gas. The control unit is configured to control the gas supply unit so that the precursor gas is supplied into the chamber in order to form a monomolecular layer of the precursor on the film of the substrate supported on the support table. In addition, the control unit is configured to control the gas supply unit and the plasma generating unit so that the processing gas is supplied into the chamber and the plasma of the processing gas is generated in order to etch the film and denature the monomolecular layer to form a protective area.

[0047] Hereinafter, various exemplary embodiments will be described in detail with reference to the accompanying drawings. In addition, in each of the drawings, the same reference numerals are given to the same or corresponding parts.

[0048] Figure 1 is a flow chart showing a method of etching a film according to an exemplary embodiment. Figure 1 The method MT shown is performed for etching a film of a substrate. Figure 2 This is a partially enlarged cross-sectional view of an example of a substrate. Figure 2 The substrate W shown has a film EF. The substrate W may have a base region UR and a mask MK.

[0049] The film EF is provided on the base region UR. The mask MK is provided on the film EF. A pattern is formed on the mask MK. That is, the mask MK provides one or more openings. The film EF is partially exposed from the openings of the mask MK. The film EF can be formed of any material. The mask MK can be formed of any material as long as the film EF can be selectively etched relative to the mask MK in the step ST3 described later.

[0050] In the first example of the substrate W, the film EF is an organic film. In the first example of the substrate W, the mask MK is a silicon-containing film. The silicon-containing film is, for example, an antireflection film containing silicon.

[0051] In the second example of the substrate W, the film EF is a low dielectric constant film containing silicon, carbon, oxygen and hydrogen. That is, in the second example of the substrate W, the film EF is a SiCOH film. In the second example of the substrate W, the mask MK is formed of a metal-containing film such as a tungsten-containing film or a titanium-containing film. In the second example of the substrate W, the mask MK can be formed of an organic film such as a photoresist film, a silicon oxide film or a polysilicon film.

[0052] In the third example of the substrate W, the film EF is a polysilicon film. In the third example of the substrate W, the mask MK is formed of a metal-containing film such as a tungsten-containing film. In the third example of the substrate W, the mask MK can be formed of an organic film such as a photoresist film or a silicon nitride film.

[0053] In the fourth example of the substrate W, the film EF is a silicon oxide film. In the fourth example of the substrate W, the mask MK is formed of a metal-containing film such as a tungsten-containing film or a titanium-containing film. In the fourth example of the substrate W, the mask MK can be formed of an organic film such as a photoresist film or a polysilicon film.

[0054] like Figure 1 As shown, method MT includes step ST1 and step ST3. In one embodiment, method MT is performed using a plasma processing device. Figure 3 FIG. 1 is a diagram schematically showing a plasma processing apparatus according to an exemplary embodiment. Figure 3 The plasma processing apparatus 1 shown is a capacitive coupling type plasma processing apparatus.

[0055] The plasma processing apparatus 1 has a chamber 10. The chamber 10 provides an internal space 10s therein. The chamber 10 includes a chamber body 12. The chamber body 12 has a substantially cylindrical shape. The internal space 10s is located inside the chamber body 12. The chamber body 12 is formed of, for example, aluminum. A corrosion-resistant film is provided on the inner wall surface of the chamber body 12. The corrosion-resistant film may be a film formed of ceramics such as aluminum oxide and yttrium oxide.

[0056] A passage 12p is formed in the side wall of the chamber body 12. When the substrate W is transported between the internal space 10s and the outside of the chamber 10, the substrate W passes through the passage 12p. The passage 12p can be opened and closed by a gate valve 12g. The gate valve 12g is provided along the side wall of the chamber body 12.

[0057] A support portion 13 is provided on the bottom of the chamber body 12. The support portion 13 is formed of an insulating material. The support portion 13 has a substantially cylindrical shape. The support portion 13 extends upward from the bottom of the chamber body 12 in the internal space 10s. The support portion 13 supports a support table 14. The support table 14 is provided in the internal space 10s. The support table 14 is configured to be able to support the substrate W in the chamber 10, that is, in the internal space 10s.

[0058] The support platform 14 has a lower electrode 18 and an electrostatic chuck 20. The support platform 14 may also have an electrode plate 16. The electrode plate 16 is formed of a conductor such as aluminum and has a substantially disc shape. The lower electrode 18 is disposed on the electrode plate 16. The lower electrode 18 is formed of a conductor such as aluminum and has a substantially disc shape. The lower electrode 18 is electrically connected to the electrode plate 16.

[0059] The electrostatic chuck 20 is disposed on the lower electrode 18. The substrate W is placed on the upper surface of the electrostatic chuck 20. The electrostatic chuck 20 has a main body and an electrode. The main body of the electrostatic chuck 20 has a substantially disc shape and is formed of a dielectric. The electrode of the electrostatic chuck 20 is a film-shaped electrode and is disposed in the main body of the electrostatic chuck 20. The electrode of the electrostatic chuck 20 is connected to a DC power supply 20p via a switch 20s. When a voltage from the DC power supply 20p is applied to the electrode of the electrostatic chuck 20, an electrostatic attraction is generated between the electrostatic chuck 20 and the substrate W. The substrate W is adsorbed to the electrostatic chuck 20 by the generated electrostatic attraction and is held by the electrostatic chuck 20.

[0060] A focus ring FR is disposed on the periphery of the lower electrode 18 so as to surround the edge of the substrate W. The focus ring FR is provided to improve the in-plane uniformity of plasma processing on the substrate W. The focus ring FR is not limited and may be formed of silicon, silicon carbide or quartz.

[0061] A flow path 18f is provided inside the lower electrode 18. A heat exchange medium (e.g., a refrigerant) is supplied to the flow path 18f from a cooling unit 22 provided outside the chamber 10 via a pipe 22a. The heat exchange medium supplied to the flow path 18f returns to the cooling unit 22 via a pipe 22b. In the plasma processing apparatus 1, the temperature of the substrate W placed on the electrostatic chuck 20 is adjusted by heat exchange between the heat exchange medium and the lower electrode 18.

[0062] The plasma processing apparatus 1 is provided with a gas supply line 24. The gas supply line 24 supplies a heat transfer gas (eg, He gas) from a heat transfer gas supply mechanism to a space between the upper surface of the electrostatic chuck 20 and the back surface of the substrate W.

[0063] The plasma processing apparatus 1 further includes an upper electrode 30. The upper electrode 30 is disposed above the support table 14. The upper electrode 30 is supported on the upper portion of the chamber body 12 via a member 32. The member 32 is formed of an insulating material. The upper electrode 30 and the member 32 close the upper opening of the chamber body 12.

[0064] The upper electrode 30 may include a top plate 34 and a support 36. The lower surface of the top plate 34 is the lower surface on the side of the internal space 10s, and is used to form the internal space 10s. The top plate 34 may be formed of a low-resistance conductor or semiconductor with little Joule heat. A plurality of gas exhaust holes 34a are formed in the top plate 34. The plurality of gas exhaust holes 34a penetrate the top plate 34 in the plate thickness direction.

[0065] The support body 36 supports the top plate 34 in a manner that the top plate 34 can be detached. The support body 36 can be formed of a conductive material such as aluminum. A gas diffusion chamber 36a is provided inside the support body 36. A plurality of gas holes 36b are formed in the support body 36. The plurality of gas holes 36b extend downward from the gas diffusion chamber 36a. The plurality of gas holes 36b are respectively connected to the plurality of gas exhaust holes 34a. A gas inlet 36c is formed in the support body 36. The gas inlet 36c is connected to the gas diffusion chamber 36a. A gas supply pipe 38 is connected to the gas inlet 36c.

[0066] The gas supply pipe 38 is connected to the gas source group 40 via the valve group 41, the flow controller group 42 and the valve group 43. The gas source group 40, the valve group 41, the flow controller group 42 and the valve group 43 constitute the gas supply part GS. The gas source group 40 includes a plurality of gas sources. The plurality of gas sources of the gas source group 40 include a plurality of gas sources used in the method MT. The valve group 41 and the valve group 43 respectively include a plurality of opening and closing valves. The flow controller group 42 includes a plurality of flow controllers. The plurality of flow controllers of the flow controller group 42 are respectively mass flow controllers or pressure-controlled flow controllers. The plurality of gas sources of the gas source group 40 are respectively connected to the gas supply pipe 38 via the corresponding opening and closing valve of the valve group 41, the corresponding flow controller of the flow controller group 42 and the corresponding opening and closing valve of the valve group 43.

[0067] In the plasma processing apparatus 1, a shield 46 is detachably provided along the inner wall surface of the chamber body 12. The shield 46 is also provided on the outer periphery of the support portion 13. The shield 46 prevents the byproducts of etching from adhering to the chamber body 12. The shield 46 is formed by forming a corrosion-resistant film on the surface of a base material formed of aluminum, for example. The corrosion-resistant film may be a film formed of ceramics such as yttrium oxide.

[0068] A baffle 48 is provided between the support portion 13 and the side wall of the chamber body 12. The baffle 48 is formed by, for example, forming a corrosion-resistant film on the surface of a base material formed of aluminum. The corrosion-resistant film may be a film formed of ceramics such as yttrium oxide. A plurality of through holes are formed in the baffle 48. An exhaust port 12e is provided below the baffle 48 and at the bottom of the chamber body 12. The exhaust port 12e is connected to an exhaust device 50 via an exhaust pipe 52. The exhaust device 50 includes a pressure regulating valve and a vacuum pump such as a turbomolecular pump.

[0069] The plasma processing device 1 also includes a first high-frequency power supply 62 and a second high-frequency power supply 64. The first high-frequency power supply 62 is a power supply that generates a first high-frequency power. The first high-frequency power has a frequency suitable for generating plasma. The frequency of the first high-frequency power is, for example, a frequency in the range of 27 MHz to 100 MHz. The first high-frequency power supply 62 is connected to the upper electrode 30 via a matcher 66 and an electrode plate 16. The matcher 66 has a circuit for matching the output impedance of the first high-frequency power supply 62 to the impedance of the load side (upper electrode 30 side). In addition, the first high-frequency power supply 62 can also be connected to the lower electrode 18 via the matcher 66. The first high-frequency power supply 62 constitutes an example of a plasma generating unit.

[0070] The second high-frequency power supply 64 is a power supply for generating a second high-frequency power. The second high-frequency power has a frequency lower than that of the first high-frequency power. When the first high-frequency power and the second high-frequency power are used together, the second high-frequency power is used as a high-frequency power for biasing ions introduced into the substrate W. The frequency of the second high-frequency power is, for example, a frequency in the range of 400kHz to 13.56MHz. The second high-frequency power supply 64 is connected to the lower electrode 18 via a matcher 68 and an electrode plate 16. The matcher 68 has a circuit for matching the output impedance of the second high-frequency power supply 64 with the impedance of the load side (lower electrode 18 side).

[0071] In addition, the second high-frequency power may be used instead of the first high-frequency power, that is, only one high-frequency power may be used to generate plasma. In this case, the frequency of the second high-frequency power may be a frequency greater than 13.56 MHz, for example, 40 MHz. In this case, the plasma processing device 1 may not have the first high-frequency power supply 62 and the matching device 66. In this case, the second high-frequency power supply 64 constitutes an example of a plasma generating unit.

[0072] When plasma is generated in the plasma processing device 1, gas is supplied from the gas supply unit GS to the internal space 10s. In addition, by supplying the first high-frequency power and / or the second high-frequency power, a high-frequency electric field is generated between the upper electrode 30 and the lower electrode 18. The gas is excited by the generated high-frequency electric field. As a result, plasma is generated.

[0073] The plasma processing device 1 also includes a control unit 80. The control unit 80 can be a computer including a processor, a storage unit such as a memory, an input device, a display device, a signal input and output interface, etc. The control unit 80 controls each unit of the plasma processing device 1. In the control unit 80, an operator can use the input device to input instructions for managing the plasma processing device 1. In addition, in the control unit 80, a display device can be used to visualize the working status of the plasma processing device 1. In addition, a control program and scheme data are stored in the storage unit of the control unit 80. In order to perform various processes in the plasma processing device 1, the control program is executed by the processor of the control unit 80. The processor of the control unit 80 executes the control program to control each unit of the plasma processing device 1 according to the scheme data, thereby executing the method MT in the plasma processing device 1.

[0074] Refer again Figure 1 In the following description, the method MT is described in detail. Figure 2 The method MT is described by taking the case where the substrate W shown is processed as an example. In addition, the method MT can also be performed using other plasma processing apparatuses. The method MT can also be performed on other substrates.

[0075] The method MT is performed in a state where the substrate W is placed on the support table 14. In one embodiment, the method MT starts in a step STa. In the step STa, the film EF is etched by plasma etching.

[0076] In step STa, plasma PLa is generated from a processing gas in the chamber 10. In the case where the first instance of the substrate W is processed, that is, when the film EF of the substrate W is an organic film, the processing gas used in step STa may contain an oxygen-containing gas. The oxygen-containing gas contains, for example, oxygen, carbon monoxide gas, or carbon dioxide gas. Alternatively, in the case where the first instance of the substrate W is processed, the processing gas used in step STa may also contain nitrogen and / or hydrogen.

[0077] When the second example of the substrate W is processed, that is, when the film EF of the substrate W is a low dielectric constant film, the processing gas used in step STa may include a fluorine-containing gas. The fluorine-containing gas is, for example, a fluorocarbon gas. The fluorocarbon gas is, for example, C4F8 gas.

[0078] When the third example of the substrate W is processed, that is, when the film EF of the substrate W is a polysilicon film, the processing gas used in step STa may contain a halogen-containing gas, such as HBr gas, Cl2 gas or SF6 gas.

[0079] When the fourth example of the substrate W is processed, that is, when the film EF of the substrate W is a silicon oxide film, the processing gas used in the step STa may contain a hydrofluorocarbon gas. The hydrofluorocarbon gas is, for example, CH3F gas.

[0080] In step STa, if Figure 4 As shown in (a) of FIG. 1 , chemical species from plasma PLa are irradiated on film EF, and the chemical species are used to etch film EF. In step STa, film EF is etched to a position between the lower surface of film EF and the upper surface of film EF. The lower surface of film EF is the surface of film EF that contacts base region UR. The upper surface of film EF is the surface of film EF that is exposed from the opening of mask MK. When step STa is performed, as shown in FIG. Figure 4 As shown in (b), an opening OP is formed in the film EF. The opening OP is formed by the side wall surface SS and the bottom surface BS of the film EF.

[0081] In step STa, the control unit 80 controls the exhaust device 50 so that the pressure in the internal space 10s is set to a specified pressure. In step STa, the control unit 80 controls the gas supply unit GS so that the processing gas is supplied to the internal space 10s. In step STa, the control unit 80 controls the plasma generating unit to generate plasma from the processing gas. In step STa of one embodiment, the control unit 80 controls the first high-frequency power source 62 and / or the second high-frequency power source 64 so that the first high-frequency power and / or the second high-frequency power are supplied.

[0082] The plasma etching in step STa may be the same as the plasma etching in step ST3 described later. For details of the plasma etching in step STa in this case and the control performed by the control unit 80 in step STa, refer to the description of step ST3.

[0083] Furthermore, the method MT may not include the step STa. In this case, the opening OP is previously provided in the film EF of the substrate to which the method MT is applied.

[0084] In method MT, step ST1 is performed. In step ST1, if Figure 5 As shown, a monomolecular layer ML of a precursor is formed on the substrate W. The monomolecular layer ML is formed on the side wall surface SS and the bottom surface BS. The monomolecular layer ML is also formed on the mask MK. The precursor constituting the monomolecular layer ML is degraded during the execution of the step ST3 described later to form a protective region PR, and any precursor may be used as long as the protective region PR can protect the side wall surface SS from the active species that etch the film EF.

[0085] In step ST1, a precursor gas containing a precursor is supplied to a substrate W having an opening OP. In one embodiment, the precursor gas is supplied to the inner space 10s. In step ST1, a carrier gas may be supplied together with the precursor gas. The carrier gas may be an inactive gas. The inactive gas may be, for example, a rare gas or nitrogen. During the execution of step ST1, plasma is not generated in the chamber 10.

[0086] In the case where any of the first to fourth examples of the above-mentioned substrate W is processed, the precursor gas used in step ST1 is a silicon-containing gas or a metal-containing gas. The silicon-containing gas contains a silicon-containing substance as a precursor. The silicon-containing gas is, for example, an aminosilane gas. The metal-containing gas contains a metal-containing substance as a precursor. The metal-containing substance contains, for example, tungsten or titanium. The metal-containing gas is, for example, a tungsten-containing gas or a titanium-containing gas. The tungsten-containing gas can be a tungsten halogenated gas such as tungsten hexafluoride gas and tungsten hexachloride gas. The titanium-containing gas can be a titanium halogenated gas such as titanium tetrafluoride gas and titanium tetrachloride gas.

[0087] In step ST1, the control unit 80 controls the exhaust device 50 so that the pressure in the internal space 10s is set to a specified pressure. In step ST1, the control unit 80 controls the gas supply unit GS so that the precursor gas is supplied to the internal space 10s. In step ST1, a carrier gas may be supplied together with the precursor gas. The carrier gas is an inert gas. The inert gas is, for example, a rare gas or nitrogen.

[0088] In method MT, step ST2 can be performed between step ST1 and step ST3. In step ST2, the internal space 10s is purged. In step ST2, the control unit 80 controls the exhaust device 50 so that the internal space 10s is exhausted. In step ST2, the control unit 80 can also control the gas supply unit GS so that an inactive gas is supplied to the internal space 10s. By performing step ST2, the precursor gas in the internal space 10s is replaced with an inactive gas. By performing step ST2, excess precursor adsorbed on the substrate W can also be removed. In this case, the supply of the precursor gas in step ST1 and the purging in step ST2 result in the formation of a monolayer ML.

[0089] In step ST3, the film EF is etched by plasma etching. In step ST3, plasma PL3 is generated from the processing gas in the chamber 10. In step ST3, as shown in FIG. Figure 6 As shown in (a), the active species from the plasma of the processing gas are irradiated to the film EF, as shown in Figure 6 The film EF is etched as shown in (b). In step ST3, the chemical species that etches the film EF or other chemical species from the plasma PL3 react with the precursor in the monomolecular layer ML, and the protection region PR is formed from the monomolecular layer ML.

[0090] In the case where the first example of the substrate W is processed, that is, when the film EF of the substrate W is an organic film, the processing gas used in step ST3 may include an oxygen-containing gas. The oxygen-containing gas includes, for example, oxygen, carbon monoxide gas or carbon dioxide gas. In step ST3, the processing gas may also include carbonyl sulfide gas. In the case where the first example of the substrate W is processed, the film EF is etched using oxidative species from the plasma PL3. In addition, the protective region PR is formed by the reaction of the oxidative species from the plasma PL3 with the precursor in the monolayer ML. In the case where the precursor in the monolayer ML is a silicon-containing substance, the protective region PR is formed of silicon oxide. In the case where the precursor in the monolayer ML is a metal-containing substance, the protective region PR is formed of a metal oxide (for example, tungsten oxide or titanium oxide).

[0091] In the case where the second example of the substrate W is processed, that is, in the case where the film EF of the substrate W is a low dielectric constant film, the processing gas used in step ST3 contains fluorine and nitrogen. For example, the processing gas contains a fluorocarbon gas and a nitrogen-containing gas. The fluorocarbon gas is, for example, C4F8 gas. The nitrogen-containing gas is, for example, nitrogen gas (N2 gas). The processing gas may also contain a rare gas (such as Ar gas) and oxygen (O2 gas). In the case where the second example of the substrate W is processed, the film EF is etched using fluorine chemical species and nitrogen chemical species from the plasma PL3. In the case where the precursor in the monolayer ML is a silicon-containing substance, in the step ST3, the protective region PR is formed by the reaction of the nitrogen chemical species from the plasma PL3 with the silicon-containing substance in the monolayer ML. In this case, the protective region PR is formed by silicon oxide. In the case where the precursor in the monolayer ML is a metal-containing substance, in the step ST3, the protective region PR is formed by the reaction of the oxygen chemical species from the plasma PL3 with the metal-containing substance in the monolayer ML. In this case, the protection region PR is formed of a metal oxide (eg, tungsten oxide or titanium oxide). In addition, the oxidizing species from the plasma PL3 reduce the amount of carbon-containing deposits formed on the substrate W in step ST3.

[0092] In the case where the third example of the substrate W is processed, that is, in the case where the film EF of the substrate W is a polysilicon film, the processing gas used in step ST3 may include a halogen-containing gas and an oxygen-containing gas. The halogen-containing gas is HBr gas, Cl2 gas or SF6 gas. The oxygen-containing gas may include, for example, oxygen, carbon monoxide gas or carbon dioxide gas. In the case where the third example of the substrate W is processed, the film EF is etched using halogen chemical species from the plasma PL3. In addition, the protective region PR is formed by the reaction of the oxygen chemical species from the plasma PL3 with the precursor in the monolayer ML. In the case where the precursor in the monolayer ML is a silicon-containing substance, the protective region PR is formed of silicon oxide. In the case where the precursor in the monolayer ML is a metal-containing substance, the protective region PR is formed of a metal oxide (for example, tungsten oxide or titanium oxide).

[0093] In the case where the fourth example of the substrate W is processed, that is, in the case where the film EF of the substrate W is a silicon oxide film, the processing gas used in step ST3 may include a hydrofluorocarbon gas and an oxygen-containing gas. The hydrofluorocarbon gas is, for example, CH3F gas. The oxygen-containing gas may include, for example, oxygen, carbon monoxide gas, or carbon dioxide gas. The processing gas used in step ST3 may also contain a rare gas (for example, Ar gas). In the case where the fourth example of the substrate W is processed, the film EF is etched using chemical species formed from the hydrofluorocarbon gas in the processing gas. In addition, the protective region PR is formed by the reaction of the oxidative species from the plasma PL3 with the precursor in the monolayer ML. In the case where the precursor in the monolayer ML is a silicon-containing substance, the protective region PR is formed by silicon oxide. In the case where the precursor in the monolayer ML is a metal-containing substance, the protective region PR is formed by a metal oxide (for example, tungsten oxide or titanium oxide). In addition, the oxidative species from the plasma PL3 reduce the amount of carbon-containing deposits formed on the substrate W in step ST3.

[0094] In step ST3, the control unit 80 controls the exhaust device 50 so that the pressure in the internal space 10s is set to a specified pressure. In step ST3, the control unit 80 controls the gas supply unit GS so that the processing gas is supplied to the internal space 10s. In step ST3, the control unit 80 controls the plasma generation unit so that plasma is generated from the processing gas. In step ST3 of one embodiment, the control unit 80 controls the first high-frequency power supply 62 and / or the second high-frequency power supply 64 so that the first high-frequency power and / or the second high-frequency power are supplied.

[0095] In method MT, step ST4 may be performed after step ST3 is performed. In step ST4, the internal space 10s is purged. Step ST4 is the same as step ST2.

[0096] In the next step ST5, it is determined whether the stop condition is satisfied. When the number of times the steps ST1 and ST3 are repeated alternately reaches a predetermined number of times, it is determined that the stop condition is satisfied. In step ST5, when it is determined that the stop condition is not satisfied, the processing from step ST1 is performed again. As a result of the alternate repetition of steps ST1 and ST3, the depth of the opening OP increases. For example, Figure 7 As shown, the opening OP is formed to reach the surface of the base region UR. In step ST5, when it is determined that the stop condition is satisfied, the method MT ends. The flow including steps ST1 and ST3 may be performed only once. In this case, step ST5 does not need to be performed.

[0097] In the method MT, during the etching of the film EF (i.e., during the execution of step ST3), the side wall surface SS is protected by the protection region PR. Therefore, it is possible to suppress the side wall surface SS from being etched by the chemical species that etches the film EF and the opening OP from expanding in the lateral direction (i.e., in the direction perpendicular to the film thickness direction of the film EF). In addition, during the execution of step ST3, the region extending on the film EF and the region extending on the upper surface of the mask MK in the entire region of the monomolecular layer ML have a large ion flow to these regions, and are therefore etched.

[0098] As described above, in the method MT, the protection region PR is formed from the monomolecular layer ML. Therefore, it is possible to suppress the protection region PR from closing the opening of the film EF. In addition, the protection region PR can be formed uniformly in the plane. In addition, the protection region PR can also be formed on the side wall surface for forming the opening OP with a high aspect ratio. In the method MT, the chemical species from the plasma PL3 generated for etching the film EF or other chemical species from the plasma PL3 degenerates the monomolecular layer, resulting in the formation of the protection region PR. Therefore, the process for converting the monomolecular layer ML into the protection region PR is performed simultaneously with the etching of the film EF.

[0099] In one embodiment, as described above, step ST1 and step ST3 may be performed in the internal space 10s without removing the substrate W from the chamber 10. That is, method MT may be performed in a space continuously maintained at reduced pressure in a chamber of a plasma processing apparatus without removing the substrate W from the chamber.

[0100] Various exemplary embodiments have been described above, but the present invention is not limited to the exemplary embodiments described above, and various omissions, substitutions, and changes may be made. In addition, elements of different exemplary embodiments may be appropriately combined to form other exemplary embodiments.

[0101] For example, the apparatus used in step ST1 and the plasma processing apparatus used in step ST3 may be different apparatuses. The plasma processing apparatus used in step STa may be different from the apparatus used in step ST1 and the plasma processing apparatus used in step ST3.

[0102] In addition, the plasma processing apparatus used in the method MT may be any type of plasma processing apparatus. For example, the plasma processing apparatus used in the method MT may be an inductively coupled plasma processing apparatus or a plasma processing apparatus that uses surface waves such as microwaves to generate plasma.

[0103] According to the above description, various embodiments of the present invention are described in this specification for the purpose of illustration, and it should be understood that various changes can be made without departing from the scope and spirit of the present invention. Therefore, the various embodiments disclosed in this specification are not intended to be limiting, and the true scope and spirit are as shown in the attached patent claims.

Claims

1. A method for etching a film in a chamber, Features: The film is an organic film having a side wall surface and a bottom surface for forming an opening, The method includes: A step of supplying a precursor gas containing a precursor in a state where no plasma is generated in the chamber, thereby forming a monomolecular layer of the precursor on the organic film; and The step of etching the organic film using oxidative species, wherein the oxidative species is derived from a plasma formed from an oxygen-containing gas, In the step of etching the organic film, the monomolecular layer is oxidized by the oxygen species from the plasma to form a protection region.

2. The method according to claim 1, Features: The precursor contains silicon.

3. A method for etching a film, Features: The film is an organic film having a side wall surface and a bottom surface for forming an opening, The method includes: forming a monomolecular layer of a precursor on the organic film; and The step of etching the organic film using oxidative species, wherein the oxidative species is derived from a plasma formed from an oxygen-containing gas, In the step of etching the organic film, the monomolecular layer is oxidized by the oxidizing species from the plasma to form a protective region. The precursor contains a metal.

4. The method according to claim 3, Features: The metal is tungsten or titanium.

5. The method according to any one of claims 1 to 3, Features: The method also includes a step of forming the opening.

6. The method according to any one of claims 1 to 4, Features: The step of forming a monomolecular layer of the precursor and the step of etching the organic film are repeated alternately.

7. The method according to any one of claims 1 to 4, Features: In a space continuously maintained at a reduced pressure in a chamber of a plasma processing apparatus, the step of forming a monomolecular layer of a precursor and the step of etching the organic film are performed without removing the substrate having the organic film from the chamber.

8. The method according to claim 7, Features: The plasma processing device is a capacitively coupled plasma processing device, which includes: the chamber; a support table including a lower electrode and configured to support the substrate in the chamber; a gas supply unit configured to supply a precursor gas containing the precursor and the oxygen-containing gas into the chamber; an upper electrode disposed above the support platform; a first high-frequency power source configured to supply a first high-frequency power for generating plasma to the upper electrode; and The second high-frequency power source is configured to supply a second high-frequency power for introducing ions into the substrate to the lower electrode.

9. A method of etching a film, Features: The film has a side wall surface and a bottom surface for forming an opening, The method comprises: forming a monomolecular layer of a precursor on the film; and the step of etching the film using chemical species from a plasma formed from a process gas, In the step of etching the film, a protection region is formed from the monomolecular layer using the chemical species from the plasma or other chemical species from the plasma, The film is a low dielectric constant film containing silicon, carbon, oxygen and hydrogen, The precursor contains silicon, The chemical species for etching the film includes a fluorine chemical species and a nitrogen chemical species, The precursor is nitrided using the nitrogen species.

10. A method of etching a film, Features: The film has a side wall surface and a bottom surface for forming an opening, The method comprises: forming a monomolecular layer of a precursor on the film; and the step of etching the film using chemical species from a plasma formed from a process gas, In the step of etching the film, a protection region is formed from the monomolecular layer using the chemical species from the plasma or other chemical species from the plasma, The film is a low dielectric constant film containing silicon, carbon, oxygen and hydrogen, The precursor contains a metal, The chemical species for etching the film includes a fluorine chemical species and a nitrogen chemical species, The other chemical species include oxygen chemical species.

11. The method according to claim 10, Features: The metal is tungsten or titanium.

12. A method of etching a film, Features: The film has a side wall surface and a bottom surface for forming an opening, The method comprises: forming a monomolecular layer of a precursor on the film; and the step of etching the film using chemical species from a plasma formed from a process gas, In the step of etching the film, a protection region is formed from the monomolecular layer using the chemical species from the plasma or other chemical species from the plasma, The film is a polysilicon film, The precursor contains silicon or metal, The chemical species that etches the film comprises a halogen chemical species, The other chemical species include oxygen chemical species.

13. The method according to claim 12, Features: The metal is tungsten or titanium.

14. A method of etching a film, Features: The film has a side wall surface and a bottom surface for forming an opening, The method comprises: forming a monomolecular layer of a precursor on the film; and the step of etching the film using chemical species from a plasma formed from a process gas, In the step of etching the film, a protection region is formed from the monomolecular layer using the chemical species from the plasma or other chemical species from the plasma, The film is a silicon oxide film, The precursor contains silicon or metal, the chemical species that etches the film comprises a chemical species formed from a hydrofluorocarbon in the process gas, The other chemical species include oxygen chemical species.

15. The method of claim 14, Features: The metal is tungsten or titanium.

16. A plasma processing device, It is characterized in that include: Chamber; a support table configured to support a substrate within the chamber; a gas supply unit configured to supply a precursor gas containing a precursor and a processing gas into the chamber; a plasma generating unit configured to generate plasma of the processing gas; and a control unit configured to control the gas supply unit and the plasma generation unit, The control unit is composed of: In order to form a monomolecular layer of the precursor on the film of the substrate supported on the support table, the gas supply unit is controlled so that the precursor gas is supplied into the chamber, In order to etch the film and modify the monomolecular layer to form a protective region, the gas supply unit and the plasma generation unit are controlled so that the process gas is supplied into the chamber and plasma of the process gas is generated.

Citation Information

Patent Citations

  • Manufacturing method of semiconductor device, and storage medium

    JP2009049141A

  • Plasma etching method, plasma etching apparatus, control program and computer-readable storage medium

    CN101241859A

  • Method of manufacturing semiconductor device and storing medium

    CN101369537A

  • Etching method

    CN105474368A

  • Plasma etch apparatus with conductive coating on inner metal surfaces of chamber to provide protection from chemical corrosion and method of forming same