Cation-disordered rock salt lithium metal oxides and oxyfluorides and methods for preparing the same
By using lithium metal oxide or oxyfluoride with the general formula LixM'aM"bO2-yFy in lithium-ion batteries, combined with a combination of low- and high-valent transition metals and fluorine substitution, a cationic disordered rock salt structure is formed, solving the problem of cationic Disordered oxides address oxygen loss and resistivity issues in lithium-ion batteries, enabling high-capacity and high-energy-density electrochemical performance.
Patent Information
- Application Number
- CN201880059794.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-03-23
- Filing Date
- 2018-09-18
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2038-09-18
AI Technical Summary
Existing cationically disordered lithium transition metal oxides suffer from high oxygen loss and resistive surface layers in lithium-ion batteries, resulting in poor cyclability and low energy density, limiting their performance in high-capacity energy storage applications.
Using lithium metal oxide or oxyfluoride with the general formula LixM'aM"bO2-yFy, through the combination of low-valent transition metals (such as Mn2+, Fe2+, Co2+) and high-valent transition metals (such as V3+, V4+, Mo4+), combined with fluorine Substitution, forming a cationic disordered rock salt structure, and preparing it through high-energy ball milling technology, optimizing the ratio of lithium to transition metal to improve the electrochemical performance of the material.
Achieved high discharge capacity (about 250mAh/g to 400mAh/g) and high energy density (about 700Wh/kg to 900Wh/kg), and significantly improved the electrochemical reversibility and cycle stability of the material, surpassing traditional disorder Performance Limitations of Rock Salt Materials.
Smart Images

Figure CN111225877B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to cationically disordered lithium metal oxides and oxyfluorides, and includes disordered rock salt vanadium and molybdenum based lithium metal oxides and oxyfluorides for high capacity lithium ion battery electrodes and methods of making the same. In addition, the present invention relates to disordered rock salt lithium manganese-vanadium oxides and oxyfluorides and methods of making the same, the disordered rock salt lithium manganese-vanadium oxides and oxyfluorides being optimized to provide high capacity and energy density for use in lithium ion batteries and related applications. Background Art
[0002] Lithium-ion ("Li-ion") batteries are one of the most studied energy storage devices due to their relatively high energy and high power performance. The growing demand for cheap, portable, high-density energy storage for personal devices, transportation, and power grids has driven the development of advanced lithium-ion battery systems. See B. Kang, G. Ceder, Nature 458, 190-193 (2009); P. Barpanda, et al. Nature materials 10, 772-779 (2011) and K. Kang, YS Meng, J. Breger, CP Grey, G. Ceder, Science 311, 977-980 (2006).
[0003] With the growing demand for high-performance lithium-ion batteries, cathode materials with high-density energy storage have been sought from various chemical spaces. In particular, oxide materials have attracted the most attention because they easily provide the highest energy density among all cathode materials.
[0004] More specifically, layered lithium transition metal oxides, such as LiCoO 2 , has become one of the most important categories of cathode materials for rechargeable lithium batteries. Currently, the most advanced high-density energy storage battery systems are based on high-voltage redox-active layered oxides for Co, Mn and Ni. In these materials, lithium ions and transition metal ions are well separated, forming different layers with alternating crystal structures. In these ordered compounds, Li sites and pathways (2D thick sheets in layered oxides) are separated from transition metal sublattices, providing stability and electron storage capacity. Figure 1 provides a schematic diagram of the layered rock salt structure Li-MO. It is generally believed that a well-organized structure with little or no mixing between lithium and transition metal sublattices is important for obtaining high-capacity cathode materials with good cycle life. In fact, it has been believed that good stratification in their structure is necessary for high lithium mobility in the material, and cation mixing has been found to lead to poor cyclability by slowing lithium diffusion. These findings may lead researchers to ignore cation-disordered lithium transition metal oxides as promising cathode materials.
[0005] Recently, important insights have been gained in the oxide space, which has expanded the search space for high-density energy storage cathode materials. Specifically, if sufficient lithium excess (i.e., the number of Li sites is greater than the number of TM sites (Li 1+ x TM 1-x O 2 In the case of x>0.09), cation-disordered lithium transition metal oxides ("Li-TM oxides") are generally considered to be electrochemically inactive and promising cathode materials because the disordered structure of lithium restricts the diffusion of lithium. In fact, once a sufficient excess of Li is introduced, easy Li diffusion is possible in the disordered structure, which in turn introduces a percolation network of convenient Li diffusion channels (0-TM channels) through which the activated Li can diffuse into the cathode due to the lack of repelling TM ions. + Due to the weak electrostatic repulsion on ions, Li diffusion is easy in the disordered structure.
[0006] However, there are still many difficulties and challenges in cation disorder / cation mixing in cathode materials that provide high-density energy storage. For example, oxygen oxidation is usually required to obtain high capacity from disordered materials, but this oxygen oxidation triggers oxygen loss through lattice densification, which reduces O-TM percolation (and thus Li diffusion) in disordered materials by reducing excess lithium content, especially near the surface. As a result, almost all of its TM redox (e.g., Fe 2+ / 4+ 、Ni 2+ / 4+ 、Co 2+ / 4+ ) Cation-disordered Li-TM oxides that overlap with oxygen redox suffer large polarization after oxygen loss and show limited cyclability. In addition, oxygen loss can also lead to a resistive surface layer, such as Li 2 CO 3 layers, which can further add impedance to the cathode. In addition, the performance of early disordered cathode materials was limited by the necessary presence of heavy, inert metals in the system and the low voltage of the active redox couple.
[0007] A previously reported strategy for improving the stability of layered (rock salt) materials is described in U.S. Patent No. 7,205,072 to Kang et al. Kang describes a fluorine substitution strategy based on layered lithium nickel-manganese-cobalt based oxide materials that is said to improve the structural stability of layered (rock salt) materials against disorder. The structural choice between layered rock salt and cationic disordered rock salt structures depends largely on the composition of the material. The fluorine-substituted lithium nickel-manganese-cobalt oxides discussed in Kang specifically form layered rock salt structures based on the composition configuration and the oxidation states of the elements contained in the composition. For example, Kang does not discuss the role of fluorine substitution or the use of divalent transition metals with vanadium or molybdenum on the structural integrity of the cationic disordered structure.
[0008] Thus, unlike approaches using layered lithium transition metal oxides, disordered rock salt systems have been identified as potential high-capacity cathodes because they offer flexibility in composition and redox behavior if at least 55% of the cation sublattice is occupied by Li (see, for example, J. Lee, A Urban, X. Li, D. Su, G. Hautier, G. Ceder, Science 343, 519-522 (2014) and J. Lee, A Urban, X. Li, D. Su, G. Hautier, G. Ceder, Science 343, 519-522 (2014). However, the performance of disordered cathodes is limited by the presence of heavy, inert metals in the system, low voltage of active redox couples, and poor reversibility (due to oxygen loss and electrochemical unavailability of some lithium during charging) (e.g., see J. Lee, D.-H. Seo, M. Balasubramanian, N. Twu, X. Li, G. Ceder, Energy Environ. Sci. 8, 3255 (2014) and N. Yabuuchi et al. Proc. Natl Acad. Sci. 112, 7650-7655 (2015)).
[0009] Therefore, there remains a need for cation-disordered lithium transition metal oxides with improved electrochemical properties for use as, for example, cathode materials. Summary of the invention
[0010] According to aspects of the present invention, there are particular lithium metal oxides or oxyfluorides having the general formula: Li x M' a M” b O 2-y F y; comprising a lithium metal oxide or oxyfluoride having a cation disordered rock salt structure, wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7; M' is a low-valent transition metal; M" is a high-valent transition metal. A particular feature of one aspect of the present invention is that M' is selected from Mn 2+ , Fe 2+ 、Co 2+ 、Ni 2+ A group consisting of a combination thereof. For example, M' can be Mn 2 + In addition, M" is selected from V 3+ 、V 4+ 、Mo 4+ 、Mo 5+ and their combinations. For example, M" can be V 4+ Or Mo 5+ In yet another embodiment, the lithium metal oxide or oxyfluoride has the formula: Li x M' a V b O 2-y F y , where 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7, or the formula: Li x M' a Mo b O 2-y F y , wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7. In yet another embodiment, the general formula: Li x M' a M” b O 2-y F y , in particular, 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6 and 0≤y≤0.3.
[0011] The lithium metal oxide or oxyfluoride of the present invention may have a crystal space group The embodiments of the present invention are also characterized by a lithium metal oxide or oxyfluoride having a discharge capacity of about 250 mAh / g to about 400 mAh / g and an energy density of about 700 Wh / kg to about 900 Wh / kg.
[0012] The present invention also includes a compound having the general formula Li x M' a M” b O 2-y F yA method for preparing cation-disordered lithium metal oxides and oxyfluorides, wherein the lithium metal oxides or oxyfluorides have a cation-disordered rock salt structure, wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7; M' is a low-valent transition metal; M" is a high-valent transition metal, comprising the following steps: providing at least one lithium-based precursor; providing at least one low-valent transition metal-based precursor; providing at least one high-valent transition metal-based precursor; optionally providing at least one fluorine-based precursor; mixing at least one lithium-based precursor, at least one low-valent transition metal-based precursor, at least one high-valent transition metal-based precursor and optionally at least one fluorine-based precursor to form a mixture; and then grinding the mixture.
[0013] In this regard, M' is selected from Mn 2+ , Fe 2+ 、Co 2+ 、Ni 2+ and combinations thereof, and M" is selected from V 3+ 、V 4+ 、Mo 4+ 、Mo 5+ and a group consisting of and combinations thereof. In addition, embodiments of methods for preparing cation-disordered lithium metal oxides and fluoride oxides include mixing stoichiometric amounts of at least one lithium-based precursor, at least one low-valent transition metal-based precursor, at least one high-valent transition metal-based precursor, and at least one optional fluorine-based precursor, such as those described in this paragraph. Embodiments of the present invention also include a grinding step by high-energy ball milling (e.g., grinding the mixture as described above). In yet another embodiment, the mixed at least one low-valent transition metal-based precursor comprises MnO, CoO, FeO, NiO or a combination thereof, and the mixed at least one high-valent transition metal-based precursor comprises VO 2 、MoO 2 、MoO 3 or a combination thereof. An embodiment of the present invention further comprises the step of grinding for about 40 hours to about 80 hours.
[0014] The present invention also relates to a positive electrode material, which includes the lithium metal oxide or oxyfluoride according to the present invention. The present invention also relates to a lithium ion battery, which includes a negative electrode material; an electrolyte; and a positive electrode material including the lithium metal oxide or oxyfluoride according to the present invention. The lithium ion battery of the present invention can be used in portable electronic devices, automobiles or energy storage systems.
[0015] Another aspect of the present invention is characterized by a lithium metal oxide or oxyfluoride having a cation disordered rock salt structure, the general formula of which is: Li x M' a M” b O 2-yF y , where 1.10≤x≤1.33, 0.1≤a≤0.41, 0.39≤b≤0.67 and 0≤y≤0.3, where M' is a low-price Mn 2+ , and M" is a redox active high-valent V 3+ or V 4+ Or Mo 4+ Or Mo 5+ , where the ratio of M' and M" balances the available Li capacity with the transition metal capacity within the target window voltage. The available Li capacity is considered to be defined as the total Li capacity minus the Li that is electrochemically unavailable through the formation of stable tetrahedral Li and Li strongly bound to F (if any). The transition metal capacity is defined as the theoretical transition metal electron capacity, assuming that the maximum average oxidation state of Mn is Mn 4+ , the maximum average oxidation state of V is V 5+ , the maximum average oxidation state of Mo is Mo 6+ . Balanced transition metal fluorides can improve cathodes for lithium-ion batteries. In particular, the lithium content in the cathode exceeds the transition metal capacity by up to 30% (inclusive) to offset the lithium that is unavailable due to F-Li binding (in the presence of F) and tetrahedral Li formation. The resulting compounds, made with a disordered rock salt structure, achieve large reversible energy density during charge / discharge cycles.
[0016] Compound LR-LMVO(Li 1.2 Mn 0.2 V 0.6 O 2 ) and LR-LMVF20(Li 1.23 Mn 0.255 V 0.515 O 1.8 F 0.2 ) represent embodiments of the present invention, which is based on designs derived from empirical studies aimed at achieving a desired balance, and the recognition that the mechanism limiting the available Li capacity involves a Li capacity that is exactly matched to the transition metal capacity. In other words, in this aspect of the invention, studies were conducted involving the computational identification of the mechanisms limiting the available Li capacity in the previously disclosed family of Li-Mn-V oxides and Li-Mn-V oxyfluorides, which, by design, have Li capacities that exactly match the transition metal capacity. The purpose of the experimental studies was to determine the source of the limited capacity and to design materials that overcome the limitations. The aforementioned compounds LR-LMVO and LR-LMVF20 are illustrative of some of the embodiments from this empirical study that exhibit beneficial properties, as described in more detail below.
[0017] In summary, aspects of the present invention include lithium metal oxides or oxyfluorides having the general formula: Li x M'a M” b O 2-y F y , the lithium metal oxide or oxyfluoride has a cation-disordered rock salt structure of one of (a) or (b), wherein
[0018] (a) 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7; M' is a low-valent transition metal, and M" is a high-valent transition metal; and
[0019] (b) 1.1≤x≤1.33, 0.1≤a≤0.41, 0.39≤b≤0.67 and 0≤y≤0.3; M' is Mn; M" is V or Mo.
[0020] With respect to the above formula (a), the present invention also includes: 2+ , Fe 2+ 、Co 2+ 、Ni 2 and the group consisting of M', for example, where M' is Mn 2+ .
[0021] With respect to the above formula (a), the present invention also includes: having a compound selected from V 3+ 、V 4+ 、Mo 4+ 、Mo 5+ and combinations thereof, such as M" wherein V 4+ Or Mo 5+ Another example of the above general formula (a) is the following general formula: Li x M' a V b O 2-y F y , wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7, and 0≤y≤0.7; or wherein 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6, and 0≤y≤0.3.
[0022] The embodiment of the present invention is also special in that the cation disordered rock salt structure is characterized by a crystal space group and a lithium metal oxide or oxyfluoride having a discharge capacity of about 250 mAh / g to about 400 mAh / g and an energy density of about 700 Wh / kg to about 900 Wh / kg.
[0023] In another embodiment of the present invention, the lithium metal oxide or oxyfluoride has formula (b), and M' is Mn; M" is V or Mo. As an example of formula (b), the lithium metal oxide is Li1.2 Mn 0.2 V 0.6 O 2 (LR-LMVO); or as an example of an oxyfluoride embodiment, the lithium metal oxyfluoride is Li 1.23 Mn 0.255 V 0.515 O 1.8 F 0.2 (LR-LMVF20).
[0024] The present invention is also special in that the preparation method of lithium metal oxide or oxyfluoride having the general formula: Li x M' a M” b O 2-y F y , the lithium metal oxide or oxyfluoride has a cation-disordered rock salt structure of one of (a) or (b), wherein
[0025] (a) 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7; M' is a low-valent transition metal, and M" is a high-valent transition metal; and
[0026] (b) 1.1≤x≤1.33, 0.1≤a≤0.41, 0.39≤b≤0.67 and 0≤y≤0.3; M' is Mn; M" is V or Mo. The method comprises the following steps:
[0027] providing at least one lithium-based precursor;
[0028] providing at least one low-valent transition metal-based precursor;
[0029] providing at least one high-valent transition metal-based precursor;
[0030] optionally providing at least one fluorine-based precursor;
[0031] At least one lithium-based precursor, at least one low-valent transition metal-based precursor, at least one high-valent transition metal-based precursor, and optionally at least one fluorine-based precursor are mixed to form a mixture; final mixing is optionally achieved by grinding the mixture (eg, high-speed ball milling).
[0032] In one embodiment of the method of the present invention, wherein the rock salt structure is (a), M' is selected from Mn 2+ , Fe 2+ 、Co 2+ 、Ni 2+ In one embodiment of the method of the present invention, relative to formula (a), M" is selected from V 3+ 、V 4+ 、Mo 4+、Mo 5+ and the group consisting of combinations thereof (including when the M' group is as described in this paragraph).
[0033] The method of the present invention also includes mixing stoichiometric amounts of at least one lithium-based precursor, at least one low-valent transition metal-based precursor, at least one high-valent transition metal-based precursor, and at least one and at least one optional fluorine-based precursor, wherein the lithium-based precursor can be added in an excess of up to 10% over the desired Li stoichiometry, and the mixture can also be ground as in a grinding involving high-energy ball milling.
[0034] An embodiment of the method of the present invention, wherein the rock salt structure is (a), comprises mixing at least one low-valent transition metal-based precursor and at least one high-valent transition metal-based precursor together, in which embodiment, the low-valent transition metal-based precursor comprises MnO, CoO, FeO, NiO or a combination thereof, and in which embodiment, the high-valent transition metal-based precursor comprises VO 2 、MoO 2 、MoO 3 or a combination thereof.
[0035] In an embodiment of the method of the present invention, the grinding step is performed for about 40 hours to about 80 hours.
[0036] In an embodiment of the method of the present invention, wherein the rock salt structure is (b), M' is Mn; M" is V or Mo. For example, under structure (b), the lithium metal oxide Li 1.2 Mn 0.2 V 0.6 O 2 (LR-LMVO); or lithium metal oxyfluoride is Li 1.23 Mn 0.255 V 0.515 O 1.8 F 0.2 (LR-LMVF20).
[0037] One aspect of the present invention also includes a positive electrode material including a lithium metal oxide or an oxyfluoride having any one of the aforementioned compositions.
[0038] Another aspect of the invention comprises a lithium ion battery comprising:
[0039] Anode material;
[0040] Electrolytes and
[0041] The above-mentioned positive electrode material.
[0042] Yet another aspect of the present invention is a portable electronic device, a vehicle or an energy storage system, comprising:
[0043] The above-mentioned lithium-ion battery.
[0044] The product of the present invention can be synthesized using solid state techniques, wherein lithium-based transition metal precursors are mixed and ground. Fluorine-based precursors are an optional ingredient that is introduced prior to mixing. For example, the product is used in the preparation of a positive electrode, for example, the positive electrode is used in the construction of a lithium ion battery, which is typically used in electronic devices, energy storage devices or automobiles. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Other features and advantages of the present invention may be ascertained from the following detailed description provided in conjunction with the accompanying drawings described below:
[0046] FIG1 is a schematic diagram of a layered rock salt structure.
[0047] Figure 2 is a schematic diagram of a disordered rock salt structure according to an embodiment of the present invention.
[0048] Figure 3 is a phase diagram of a disordered rock salt vanadium-based oxyfluoride system according to one embodiment of the present invention.
[0049] Figure 4 is a phase diagram of a disordered rocksalt molybdenum-based oxyfluoride system according to another embodiment of the present invention.
[0050] Figure 5 is a schematic diagram of a rechargeable lithium-ion battery.
[0051] Figure 6 Shown Li 1.143 Mn 0.286 V 0.572 O 2 ("LMV1 of the present invention"); Li 1.156 Mn 0.315 V 0.528 O 1.9 F 0.1 ("LMV2 of the present invention"); Li 1.171 Mn 0.343 V 0.486 O 1.8 F 0.2 ("LMV3 of the present invention"); and Li 1.186 Mn 0.371 V 0.443 O 1.7 F 0.3 X-ray diffraction ("XRD") pattern of ("inventive LMV4").
[0052] Fig. 7A shows the first cycle electrochemical performance of LMV1 of the present invention, LMV2 of the present invention, LMV3 of the present invention, and LMV4 of the present invention; and
[0053] Figure 7B and7C The multiple charge / discharge cycle performance of the LMV3 of the present invention is shown.
[0054] Figure 8 The average amount of Li at 4.6 V that cannot be achieved by high voltage F binding is shown as a function of fluorine level and Li capacity relative to transition metal capacity, where "stoichiometric" refers to the total Li capacity (x) equal to the transition metal capacity (2a+b), while 20% Li and TM rich refers to compositions with excess Li or TM capacity (x=1.2(2a+b) and 1.2x=(2a+b), respectively).
[0055] Fig. 9 The expected fraction of Li that migrates to tetrahedral sites when charged to 4.6 V is shown. Given experimental trends in electrolyte stability and cell reversibility, 4.6 V is a practical voltage limit.
[0056] Fig.10 shows that the Mn mixed at low F 2+ / V 4+ Predicted first charge capacity between 1.5 V and 4.6 V in oxyfluorides, accounting for the unavailable Li due to F incorporation and the formation of tetrahedral Li. The experimentally tested LR-LMVO and LR-LMVF20 compounds are labeled.
[0057] Fig.11A and 11B The X-ray diffraction patterns and scanning electron microscope images of the synthesized (a) LR-LMVO and (b) LR-LMVF20 materials are shown, respectively, indicating that the products are phase-pure disordered rock salts.
[0058] Fig. 12A and 12B Shown are the galvanostatic charge / discharge voltage curves of (a) LR-LMVO and (b) LR-LMVF20, respectively, obtained in the first five cycles in the window voltage from 1.5 V to 4.6 V. The inset shows the drop in charge and discharge capacity in the first 20 cycles. DETAILED DESCRIPTION
[0059] The present invention relates to cationically disordered lithium metal oxides. In one aspect of the invention, there are particular cationically disordered rock salt vanadium and molybdenum based lithium metal oxides and oxyfluorides. Without being bound by any particular theory, it is believed that by using low valent transition metals with two electron redox capability (e.g., Mn 2+ , Fe 2+ 、Co 2+ and Ni 2+ ) and a high-valent transition metal having at least one electron redox capability (e.g. V 3+ 、V 4+ 、Mo4+ and Mo 5+ ) and optionally associated with partial fluorine substitution of oxygen on the anion lattice, a high capacity disordered rock salt material can be obtained. In some embodiments of the present invention, the lithium metal oxide may not include fluorine substitution. In some embodiments, the specific combination of valence states used in the present invention allows fluorine substitution to be avoided. In other embodiments, the lithium metal oxide can be fluorine substituted. The combination of the different valence states described and fluorine substitution provides a high-performance composition. In this regard, fluorine-substituted lithium metal oxides are referred to as fluoride oxides in this article.
[0060] Due to the reliance on high voltage transition metal redox pairs (e.g., Mn 2+ / 4+ , Fe 2+ / 4+ 、Co 2+ / 4+ , or Ni 2 + / 4+ and V 4+ / 5+ Or Mo 5+ / 6+ ), the disordered rock salt lithium metal oxides and oxyfluorides of the present invention are designed to eliminate redox-inert transition metals from the system, optimize active transition metal redox pairs to maximize voltage and balance lithium with transition metal components to eliminate irreversible oxygen loss. In fact, the disordered rock salt lithium metal oxides and oxyfluorides of the present invention are designed to maximize the capacity of the transition metal to minimize the amount of oxygen redox used in the electrochemical cycle of the material. Therefore, the disordered lithium metal oxide and oxyfluoride materials of the present invention provide high-density energy storage and excellent reversibility of electrochemical behavior, which is not achievable with previously reported disordered rock salt materials. In fact, previously reported disordered rock salt materials lose a large portion of their energy density in the first few charge / discharge cycles.
[0061] In this aspect of the invention, disordered rock-salt vanadium and molybdenum based lithium metal oxides and oxyfluorides are provided. In one embodiment, the oxides and oxyfluorides include cationically disordered rock-salt structures. In fact, the oxides and oxyfluorides discussed herein only form disordered rock-salt structures. As used herein, cationically disordered rock-salt structures refer to structures with a crystallographic space group A structure characterized by. In the cation-disordered rock salt structure of the present invention, lithium and transition metals can randomly occupy empty octahedral sites in the face-centered cubic ("FCC") framework of oxygen, and fluorine can replace oxygen. When present, the substituted fluorine is randomly distributed in the FCC framework together with oxygen. In another embodiment, the cation-disordered rock salt structure may include interwoven FCC structures: one made of anions (such as oxygen and fluorine) and the other made of randomly distributed lithium and transition metals. However, regardless of the design of the structure, the present invention contemplates a disordered rock salt structure in which lithium occupies at least 55% of the cation sublattice. For example, lithium may occupy 55% to 100% of the cation sublattice.
[0062] In some embodiments, the cation-disordered rock salt structure of the present invention provides a method for replacing fluorine with oxygen. As described above, the substituted fluorine shares the FCC framework of oxygen and is randomly distributed with oxygen. However, regardless of whether fluorine is present in the lithium metal oxide, the disordered oxides and oxyfluorides of the present invention are completely cation-mixed, that is, 100% cation mixing. In the process of forming the cation-disordered rock salt structure, minimal non-cationic mixing may occur. However, any minimal non-cationic mixing that occurs is unintentional and is still understood by those of ordinary skill in the art to refer to complete cation mixing. Figure 2 The cation disordered rock salt structure expected by the present invention is shown. Figure 2 It can be seen that the distribution of oxygen / fluorine, lithium and transition metals in the rock salt structure is completely random.
[0063] The disordered rock salt oxides and oxyfluorides of the present invention contemplate the use of specific combinations of low-valent transition metals and high-valent transition metals: for example, optionally with partial substitution of fluorine for oxygen. According to aspects of the present invention, the oxides and oxyfluorides have the general formula (1):
[0064] Li x M' a M” b O 2-y F y (1)
[0065] Wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7. It will be apparent to one of ordinary skill in the art that the general formulas for oxides and oxyfluorides described herein refer to discharged systems. In another embodiment, the general formula (1) may be defined as 1.10≤x≤1.30, 0.1≤a≤0.5, 0.2≤b≤0.6 and 0≤y≤0.5. In yet another embodiment, the general formula (1) may be defined as 1.10≤x≤1.25, 0.2≤a≤0.4, 0.3≤b≤0.6 and 0≤y≤0.4. In yet another embodiment, the general formula (1) may be defined as 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6 and 0.1≤y≤0.3.
[0066] According to aspects of the present invention, M' of general formula (1) is a low-valent transition metal. The term "low-valent transition metal" refers to a transition metal having an oxidation state of less than +3, and more preferably, having an oxidation state of +2 or less. In this regard, the low-valent transition metal considered by the present invention has a two-electron redox capability. In one embodiment, M' can be Mn, Fe, Co, Ni, or any combination thereof, wherein the oxidation state of each metal is +2. For example, M' can be Mn with an oxidation state of +2. According to the present invention, M" of general formula (1) is a high-valent transition metal. The term "high-valent transition metal" refers to a transition metal having an oxidation state of +3 or greater, and more preferably, having an oxidation state of +4 or greater. In this regard, the high-valent transition metal considered by the present invention has at least one electron redox capability. In one embodiment, M" can be V, Mo, or any combination thereof, wherein V has an oxidation state of +3 or +4, and Mo has an oxidation state of +4 or +5. In another embodiment, M" can be V with an oxidation state of +4 or Mo with an oxidation state of +5.
[0067] In another embodiment, the disordered rock salt oxides and oxyfluorides of the present invention may be vanadium-based. That is, M" of formula (1) may be V. For example, the oxides and oxyfluorides may have formula (2):
[0068] Li x M' a V b O 2-y F y (2)
[0069] Wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7. In another embodiment, the general formula (2) can be defined as 1.10≤x≤1.25, 0.1≤a≤0.5, 0.2≤b≤0.6 and 0≤y≤0.5. In another embodiment, the general formula (2) can be defined as 1.10≤x≤1.25, 0.2≤a≤0.4, 0.3≤b≤0.6 and 0≤y≤0.4. In another embodiment, the general formula (2) can be defined as 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6 and 0.1≤y≤0.3. According to the present invention, M' of the general formula (2) can be defined as the general formula (1). That is, M' may be a low-valent transition metal selected from Mn, Fe, Co, Ni, or any combination thereof, wherein the oxidation state of each metal is +2.
[0070] In one embodiment, M' of general formula (2) may be Mn. For example, the disordered rock salt material of the present invention may include oxides and oxyfluorides of lithium manganese vanadium. That is, the oxides and oxyfluorides of the present invention may have general formula (3):
[0071] Li x Mn a V b O 2-y F y (3)
[0072] Wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7. For example, the general formula (3) may be defined as 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6 and 0≤y≤0.3. In one embodiment, the oxide of the general formula (3) may include the compound Li 1.143 Mn 0.286 V 0.572 O 2 , wherein x=1.143, a=0.286, b=0.572 and y=0. In another embodiment, the fluorine oxide of formula (3) may include the compound Li 1.156 Mn 0.315 V 0.528 O 1.9 F 0.1 , wherein x=1.156, a=0.315, b=0.528 and y=0.1. In yet another embodiment, the fluorine oxide of formula (3) may include the compound Li 1.171 Mn 0.343 V 0.486 O 1.8 F 0.2 , wherein x=1.171, a=0.343, b=0.486 and y=0.2. In yet another embodiment, the fluorine oxide of formula (3) may include the compound Li 1.186 Mn 0.371 V 0.443 O 1.7 F 0.3 , where x=1.186, a=0.371, b=0.443 and y=0.3.
[0073] In another embodiment, the disordered rock salt oxides and oxyfluorides of the present invention may be molybdenum-based. That is, M" of formula (1) may be Mo. For example, the oxides and oxyfluorides may have formula (4):
[0074] Li x M' a Mo b O 2-y F y (4)
[0075] Wherein 1.09≤x≤1.35, 0.1≤a≤0.7, 0.1≤b≤0.7 and 0≤y≤0.7. In another embodiment, the general formula (4) can be defined as 1.10≤x≤1.25, 0.1≤a≤0.5, 0.2≤b≤0.6 and 0≤y≤0.5. In another embodiment, the general formula (4) can be defined as 1.10≤x≤1.25, 0.2≤a≤0.4, 0.3≤b≤0.6 and 0≤y≤0.4. In another embodiment, the general formula (4) can be defined as 1.1≤x≤1.2, 0.25≤a≤0.4, 0.4≤b≤0.6 and 0.1≤y≤0.3. According to the present invention, M' of the general formula (4) can be defined as the general formula (1). That is, M' may be a low-valent transition metal selected from Mn, Fe, Co, Ni, or any combination thereof, wherein the oxidation state of each metal is +2.
[0076] The disordered rock salt oxides and oxyfluorides according to aspects of the present invention may have to The α-lattice constants of LMV1, LMV2, LMV3 and LMV4 are respectively and The particle size of the compounds of the present invention is between 100 and 200 nm.
[0077] The present invention also includes methods for preparing disordered rock salt oxides and oxyfluorides of the present invention. Various methods can be used to prepare oxides and oxyfluorides of the present invention, including but not limited to solid state reaction methods, aqueous solution methods or mechanochemical synthesis. In one embodiment, before the preparation method, a phase diagram showing the thermal stability of the relevant system can be constructed to determine the composition region of the target disordered rock salt phase that can be entered by the desired preparation method. That is, a phase diagram showing thermal stability can be constructed to determine the composition region of the target disordered rock salt phase that can be entered by solid state synthesis or mechanochemical synthesis (such as high energy ball milling). The thermal stability of the composition well indicates whether the compound can be formed at a specific temperature by solid state synthesis or high energy ball milling.
[0078] For example, Figure 3 and Figure 4 The compositional space and thermal stability of the system contemplated under aspects of the present invention are shown. Figure 3 It shows that based on Mn 2+ , Fe 2+ 、Co 2+ or Ni 2+ and V 4+ Compositional space of the mixed transition metal disordered Li-excess oxyfluoride rocksalt structure. Figure 4 It shows that based on Mn2+ , Fe 2+ 、Co 2+ or Ni 2+ and Mo 5+ The composition space of the mixed transition metal disordered Li-excess oxyfluoride rock salt structure. It can be seen that Figure 3 and Figure 4 The synthetic availability of these systems is defined by solid-state synthesis and high-energy ball milling at a given temperature. The contours in the phase diagram represent the composition region that is stable at the temperature associated with the contour, starting from the endpoint phase. In the case of solid-state synthesis, the contour temperature is the minimum annealing temperature required to form the target composition. In the case of high-energy ball milling, any composition that is stable at 1750°C or lower can be synthesized.
[0079] In addition, the phase diagram can also show compositions that fall above the Li percolation threshold of disordered rock salt (i.e., Li occupies at least 55% of the cation sublattice). For example, Figure 3 and Figure 4 shows compositions that satisfy the disordered rock salt Li percolation threshold. In fact, the present invention contemplates compositions that fall above the Li percolation threshold. In addition, the phase diagram can also show the reversible capacity available from all transition metals in the system. For example, Figure 3 and 4 Shows Mn 2+ / 4+ , Fe 2+ / 4+ 、Co 2+ / 4+ or Ni 2+ / 4+ and V 4+ / 5+ Redox couple and Mn 2 + / 4+ , Fe 2+ / 4+ 、Co 2+ / 4+ 、Ni 2+ / 4+ and Mo 5+ / 6+ Expected total capacity of the redox couple.
[0080] In one embodiment, mechanochemical synthesis can be used to prepare disordered rock salt oxides and oxyfluorides of the present invention. In this regard, the method for preparing disordered rock salt oxides and oxyfluorides of the present invention includes the step of providing the necessary precursors for producing oxides and oxyfluorides. For example, the method may include the step of providing at least one lithium-based precursor, at least one low-valent transition metal precursor, at least one high-valent transition metal precursor and optionally at least one fluorine-based precursor. In this regard, the low-valent transition metal precursor can be a manganese-based precursor, a cobalt-based precursor, an iron-based precursor or a nickel-based precursor. Similarly, the high-valent metal precursor can be a vanadium-based precursor or a molybdenum-based precursor.
[0081] It will be apparent to one of ordinary skill in the art that any precursor that provides the desired elemental composition of the disordered oxide or oxyfluoride may be used in the present invention. However, in one embodiment, the lithium-based precursor may include Li 2 CO 3 , Li 2 O or LiOH. In another embodiment, the low-valent transition metal precursor may include MnO, CoO, FeO, NiO or a combination thereof. In yet another embodiment, the high-valent transition metal precursor may include VO 2 、MoO 2 、MoO 3 Or a combination thereof. Similarly, preferred fluorine-based precursors include LiF.
[0082] After selecting the desired precursor, a stoichiometric amount of lithium-based, low-valent transition metal-based, high-valent transition metal-based and fluorine-based precursors are mixed, wherein a lithium-based precursor exceeding the desired lithium content by 10% can be added at most. Any mechanical means for fully mixing the precursors can be used. The duration of mixing will depend on the type of mechanical means used and the speed of mixing the precursors. For example, in one embodiment, the precursors can be mixed in a ball mill (according to the present invention, mixing can include a separate mixing stage before the grinder receives, or mixing can be considered as: providing the material to be ground to form an initial mixture in the grinder, and then grinding the received mixture into a final mixture state). In this regard, the precursors can be mixed in a ball mill at about 300rpm over a period of time between 6 and 12 hours.
[0083] In yet another embodiment, the mixed precursor can be subjected to high energy ball milling. In this regard, high energy ball milling is carried out at a higher speed (rpm) than ball milling. For example, high energy ball milling can be carried out at a speed of 450rpm to 550rpm. In addition, according to the present invention, the grinding step can be carried out at room temperature and under an argon atmosphere.
[0084] The mixed precursor can be subjected to grinding for 20 to 200 hours. In another embodiment, the mixed precursor can be subjected to grinding for about 40 hours to about 80 hours. In yet another embodiment, the mixed precursor can be subjected to grinding for about 50 hours to about 70 hours. For example, the mixed precursor can be subjected to grinding for about 60 hours. After the grinding step, disordered rock salt oxides and oxyfluorides of the present invention are formed. The resulting oxides and oxyfluorides can be ground into fine powders and prepared as cathode films.
[0085] In embodiments of the present invention, solid-state reaction synthesis can be used to prepare disordered rock salt oxides and oxyfluorides of the present invention. For example, solid-state synthesis can be used to prepare molybdenum-based oxides and oxyfluorides of the present invention. Solid-state synthesis can also be used to prepare vanadium-based metal oxides of the present invention.
[0086] The disordered rock salt oxides and oxyfluorides of the present invention provide improved electrochemical performance. For example, the disordered rock salt oxides and oxyfluorides of the present invention include three active transition metal pairs, two of which are from low-valent metals (e.g., Mn 2+ / 4+ ), the other from a high-valent metal, provides a highly reversible and high-density energy storage cathode. For example, after repeated cycling profiles at high cut-off voltages, the disordered rock salt oxides and oxyfluorides of the present invention show minimal changes in capacity and voltage. In other words, the oxides and oxyfluorides of the present invention are highly reversible, in contrast to other reported lithium-excess cathodes, which typically lose a lot of capacity due to oxygen loss after the first few cycles, or are only reversible at low voltages. Without being bound by any particular theory, it is believed that the high transition metal content demonstrated in the oxides and oxyfluorides of the present invention (whose capacity is balanced to perfectly match the Li content) eliminates the need for oxygen capacity on charge / discharge. This, in turn, promotes reversible electrochemical performance.
[0087] In addition, the disordered rock salt oxides and oxyfluorides of the present invention achieve high discharge capacity and high-density energy storage. In an embodiment of the present invention, the oxide and oxyfluoride reach a discharge capacity of about 250mAh / g to about 400mAh / g. The embodiment of the present invention is characterized by an oxide and achieves a discharge capacity of about 275mAh / g to about 380mAh / g. In other embodiments, the oxide and oxyfluoride of the present invention reach a discharge capacity of about 290mAh / g to about 350mAh / g. For example, the oxide and oxyfluoride of the present invention can achieve a discharge capacity of about 310mAh / g. The oxide and oxyfluoride of the present invention can obtain these discharge capacities at an average voltage of about 2.5V to about 3V. In another embodiment, the oxide and oxyfluoride of the present invention can achieve these discharge capacities at an average voltage of about 2.6V to about 2.75V.
[0088] Therefore, the embodiments of the disordered rock salt oxide and oxyfluoride of the present invention achieve an energy density of about 700Wh / kg to about 900Wh / kg. The embodiments of the disordered rock salt oxide and oxyfluoride of the present invention also achieve an energy density of about 740Wh / kg to about 875Wh / kg. In other embodiments, the disordered rock salt oxide and oxyfluoride of the present invention reach an energy density of about 760Wh / kg to about 860Wh / kg. For example, the disordered rock salt oxide and oxyfluoride can reach an energy density of 781Wh / kg at a cut-off voltage of 4.6V and an energy density of 862Wh / kg at a cut-off voltage of 4.8.
[0089] The present disclosure also provides lithium batteries and lithium ion batteries, which include electrode materials, such as cathodes composed of disordered rock salt oxides and oxyfluorides as described herein. In one embodiment, the disordered rock salt oxides and oxyfluorides produced according to the present invention can be used as cathodes in lithium ion rechargeable batteries. Figure 5 A schematic diagram of a rechargeable lithium-ion battery is shown. Figure 5 As shown, the reversible shuttling of Li ions between the cathode 10 and the anode 20 enables a rechargeable lithium-ion battery 30. The disordered rock salt oxides and oxyfluorides described herein (above and below) can be used as cathodes in lithium-ion rechargeable batteries, which are suitable for products such as portable electronic devices, automobiles including electric vehicles and hybrid electric vehicles, and energy storage systems. The disordered rock salt oxides and oxyfluorides described herein (above and below) can also be used as cathode materials for lithium-ion cathode batteries for high-density energy storage, where cathode energy density is an important factor for overall battery performance. For example, the disordered rock salt oxides and oxyfluorides of the present invention can be used in long-life secondary lithium-ion batteries, where reversibility is a desirable feature for achieving stable performance over many charge / discharge cycles.
[0090] Another aspect of the present invention is directed to disordered rock salt lithium manganese-vanadium oxides and oxyfluorides, aimed at optimizing the maximum utilization of lithium capacity, and in particular, a mixture of the following materials: a low-valent transition metal (Mn) having a two-electron redox ability 2+ , Fe 2+ 、Co 2+ 、Ni 2+ ), a high-valent transition metal charge compensator having at least one electron redox capability ((V 3+ 、V 4 + 、Mo 4+ 、Mo 5+ ), and O 2- and F - In these mixtures, it is possible to obtain a series of synthetically accessible, high-capacity disordered rock-salt materials that rely mainly on high-voltage transition metal redox couples that provide high-density energy storage and reversibility.
[0091] Two compounds Li in the Li-Mn-VOF space 1.143 Mn 0.286 V 0.572 O 2 and Li 1.171 Mn 0.343 V 0.486 O 1.8 F 0.2 In the performance process and Li1.171 Mn 0.343 V 0.486 O 1.8 F 0.2 During the performance of first-principles models of the electrochemical behavior of the materials, two mechanisms were identified that limit the exploitable Li capacity in these materials: the formation of strong Li-F bonds and the migration of Li to very stable tetrahedral sites at high charge states. After quantifying these mechanisms, a map of the practically exploitable Li capacity was calculated in the Li-Mn-VOF space and used to design two new compounds (LR-LMVO) and (LR-LMVF20) described below, which offer higher capacity and energy density than previously reported compounds.
[0092] For example, the chemical formula is Li x Mn a V b O 2-y Compounds with (1.10≤x≤1.33, 0.1≤a≤0.41, 0.39≤b≤0.67, 0≤y≤0.30) will have 0.4y-0.8yLi-difficult-to-use sites due to binding with F (if present), and 0.10x-0.12xLi-difficult-to-use sites due to tetrahedral Li formation, where the above two effects are not additive but act independently of each other, that is, the two effects limit the available Li capacity in parallel rather than superposition. Based on these findings, it can be concluded that disordered rock-salt oxide Li 1.2 Mn 0.2 V 0.6 O 2 (LR-LMVO) is a method to balance the practically available Li capacity and the theoretical transition metal capacity (in Li x Mn a V b O 2-y F y The material 2a+b) in the above diagram can provide the largest available capacity of this space. Similarly, a similar disordered rock salt fluoride oxide Li 1.23 Mn 0.255 V 0.515 O 1.8 F 0.2 (LR-LMVF20) as a compound that similarly balances the available lithium capacity with the transition metal capacity, but exhibits slightly better cycling stability due to surface passivation by F.
[0093] The two compounds, LR-LMVO and LR-LMVF20, were experimentally realized, confirming their synthetic availability and superior performance. These results illustrate the benefits provided by the optimization rules to maximize the available Li capacity developed according to the present invention. As a result of our studies, it has been determined that the high oxidation state transition metal state (Mn 4+ and V 5+ ) is not the limiting mechanism in these materials. Therefore, we believe that the origin of the limited capacity must lie in the Li availability related to the Li configuration in the material, which is avoided by introducing excess total Li capacity.
[0094] With reference to the aforementioned advantageous LR-LMVO and LR-LMVF20 pertaining to the second aspect of the present invention, Figure 8 The average amount of Li at 4.6 V that cannot be achieved by high voltage F binding is shown as a function of fluorine level and Li capacity relative to transition metal capacity, where "stoichiometric" refers to the total Li capacity (x) equal to the transition metal capacity (2a+b), while 20% Li and TM rich refers to compositions with excess Li or TM capacity (x=1.2(2a+b) and 1.2x=(2a+b), respectively).
[0095] Fig. 9 The expected fraction of Li that migrates to tetrahedral sites when charged to 4.6 V is shown. Given experimental trends in electrolyte stability and cell reversibility, 4.6 V is a practical voltage limit.
[0096] Fig.10 shows that the Mn mixed at low F 2+ / V 4+ The predicted first charge capacity between 1.5 V and 4.6 V in the oxyfluoride accounts for the unavailable Li due to F incorporation and the formation of tetrahedral Li. Fig.10 Mark in.
[0097] Example
[0098] The following non-limiting examples illustrate disordered rock salt lithium metal oxides and oxyfluorides. The first group of examples (Example Class 1) is directed to the first aspect of the invention, in particular disordered rock salt vanadium and molybdenum based lithium metal oxides and oxyfluorides, and the second group of examples (Example Class 2) is directed to the second aspect of the invention, in particular disordered rock salt lithium manganese-vanadium oxides and oxyfluorides having the above-mentioned advantageous properties. The examples are merely illustrative of preferred embodiments of the invention and are not to be construed as limitations of the invention, the scope of which is defined by the appended claims.
[0099] Example Category 1
[0100] The following disordered rock salt vanadium and molybdenum based oxides and oxyfluorides of the present invention were synthesized:
[0101] With the general formula Li x Mn a V b O 2-y F y Li-Mn-VOF type, 1.1≤x≤1.2, 0.3≤a≤0.4, 0.4≤b≤0.6, 0≤y≤0.3, where x=1.143, a=0.286, b=0.572, y=0(Li 1.143 Mn 0.286 V 0.572 O 2 ) (“LMV1 of the present invention”);
[0102] With the general formula Li x Mn a V b O 2-y F y Li-Mn-VOF type, 1.1≤x≤1.2, 0.3≤a≤0.4, 0.4≤b≤0.6, 0≤y≤0.3, where x=1.156, a=0.315, b=0.528, y=0.1(Li 1.156 Mn 0.315 V 0.528 O 1.9 F 0.1 ) (“LMV2 of the present invention”);
[0103] With the general formula Li x Mn a V b O 2-y F y Li-Mn-VOF type, 1.1≤x≤1.2, 0.3≤a≤0.4, 0.4≤b≤0.6, 0≤y≤0.3, where x=1.171, a=0.343, b=0.486, y=0.2(Li 1.171 Mn 0.343 V 0.486 O 1.8 F 0.2 ) (“LMV3 of the present invention”); and
[0104] With the general formula Li x Mn a V b O 2-y F yLi-Mn-VOF type, 1.1≤x≤1.2, 0.3≤a≤0.4, 0.4≤b≤0.6, 0≤y≤0.3, where x=1.186, a=0.371, b=0.443, y=0.3(Li 1.186 Mn 0.371 V 0.443 O 1.7 F 0.3 ) (“LMV4 of the present invention”).
[0105] When preparing the compounds of the present invention under Example Class 1, Li 2 O (Sigma-Aldrich, minimum 97%), MnO (Sigma-Aldrich, 99.99%), VO 2 (Sigma-Aldrich, 99.9%) and LiF (Alfa Aesar, 99.99%) were used as precursors. The stoichiometric precursors were mixed at 300 rpm for 12 h using a Retsch PM 200 planetary ball mill, except for Li 2 O (the added lithium was 10% higher than the desired Li content). The mixed precursors (1 g in total) were then ball milled using a Retsch PM 200 planetary ball mill at 500 rpm under argon. LMV1 of the present invention was ball milled for 40 hours. LMV2 of the present invention was ball milled for 50 hours. LMV3 of the present invention was ball milled for 60 hours. LMV4 of the present invention was ball milled for 80 hours. The compounds obtained from the ball milling process were fine powders.
[0106] To prepare the cathode membrane, the powders of each of the present invention LMV1, the present invention LMV2, the present invention LMV3 and the present invention LMV4 were manually mixed with carbon black (Timcal, Super P) in a weight ratio of 70:20. Polytetrafluoroethylene (PTFE, DuPont, Teflon 8C) ("PTFE") was added to each mixture as a binder. Each resulting cathode membrane included the respective present invention LMV1, the present invention LMV2, the present invention LMV3 or the present invention LMV4; the weight ratio of carbon black to PTFE was 70:20:10. The components were manually mixed for 30 minutes and rolled into a film in an argon-filled glove box. In order to assemble the battery for conventional cycle testing, 1M LiPF6 in ethylene carbonate ("EC") and dimethyl carbonate ("DMC") solutions (1:1, Techno Semichem), glass microfiber filters (GE Whatman) and lithium metal foil (FMC) were used as electrolyte, separator and counter electrode, respectively. 2032 button cells were assembled in an argon-filled glove box and tested on a battery tester (Arbin) at room temperature in constant current mode. The loading density of the cathode film was about 5 mg / cm2 Based on the fluoride oxide (Li x Mn a V b O 2-y F y ) (i.e. 70 wt %) to calculate the specific capacity.
[0107] X-ray diffraction ("XRD") patterns of the prepared compounds were collected on a Rigaku MiniFlex (copper source) in the 2-theta range of 5-85°. Figure 6 XRD patterns of the compounds LMV1 of the present invention, LMV2 of the present invention, LMV3 of the present invention, and LMV4 of the present invention are shown. Figure 6 It was confirmed that each of the target compositions, inventive LMV1, inventive LMV2, inventive LMV3 and inventive LMV4, was a phase pure product. In other words, these compounds were successfully prepared by high energy ball milling.
[0108] The electrochemical properties of the inventive LMV1, inventive LMV2, inventive LMV3 and inventive LMV4 cathodes were also tested. Fig. 7A The first cycle electrochemical performance of the compounds of the present invention LMV1, LMV2, LMV3 and LMV4 is shown at a cutoff voltage of 4.8 V. Each compound of the present invention exhibits similar high capacity and high voltage, approaching 90% of the theoretical transition metal capacity.
[0109] Figure 7B and 7C The multiple charge / discharge cycle performances of the LMV3 compound of the present invention at 4.6V and 4.8V cut-off voltages are shown respectively. Figure 7B As shown, the LMV3 compound of the present invention achieves a discharge capacity of up to about 290 mAh / g at an average voltage of 2.69 V, and an energy density of 781 Wh / kg at a cut-off voltage of 4.6 V. Figure 7B The energy density obtained at a cutoff voltage of 4.6 V is highly reversible, as demonstrated by the repeated cycling curves of , with the variation of discharge capacity and average voltage being less than 2% within the first 5 cycles. Figure 7C As shown, the LMV3 compound of the present invention achieved a discharge capacity of about 317 mAh / g at an average voltage of 2.72 V, and obtained an energy density of 862 Wh / kg at a cut-off voltage of 4.8 V.
[0110] Example Category 2
[0111] Under example category 2, examples are provided for the above-mentioned disordered rock-salt lithium manganese-vanadium oxides and oxyfluorides LR-LMVO and LR-LMVF prepared using mechanochemical synthesis. 2 O (Sigma-Aldrich, 99%), MnO (Sigma-Aldrich 99.99%), VO 2 (Sigma-Aldrich 99.99%), and LiF in the case of oxyfluoride (AlfaAesar, 99.99%) were used as precursors and stoichiometrically mixed (10% excess Li 2 The mixed precursors were then ball milled using a Retsch PM200 planetary ball mill at a speed of 500 rpm under argon for 50 hours.
[0112] To prepare the cathode film, Li x Mn a V b O 2-y F y The powders of Mn and carbon black (Timcal, Super P) were manually mixed in a weight ratio of 70:20 for 40 minutes. Then, polytetrafluoroethylene (PTFE, DuPont, Teflon 8C) was added to the mixture as a binder so that the cathode film was composed of Mn in a weight ratio of 70:20:10. a V b O 2-y F y , carbon black and PTFE. The components were manually mixed for another 30 minutes and then rolled into a film in an argon glove box. In order to assemble the battery for conventional cycle testing, 1M LiPF6 in ethylene carbonate (EC) and dimethyl carbonate (DMC) solution (1:1, Techno Semichem), glass microfiber filter (GE Whatman) and lithium metal foil (FMC) were used as electrolyte, separator and counter electrode, respectively. 2032 buttons were placed in an argon-filled glove box and tested on a battery tester (Arbin) in constant current mode at room temperature. The loading density of the cathode film is about 5 mg / cm 2 The specific capacity was calculated based on the amount of LixMnaVbO2-yFy (70 wt%) in the cathode film. The X-ray diffraction (XRD) patterns of the prepared compounds were collected on a RigakuMiniFlex (copper source) in the 2θ range of 5-85 degrees.
[0113] The development and experimental confirmation of design rules for Li capacity relative to transition metal capacity yielded a series of optimal compounds for high charge capacity, where the Li 4+Similarly, Mo, a redox-active high-valent transition metal, 5+ Included, as we have previously disclosed: Li x Mn a V b O 2-y F y , where 0.1≤a≤0.7, 0.1≤b≤0.7, 0.1≤y≤0.7, (2a+b)≤x≤1.3*(2a+b); and Li x Mn a Mo b O 2-y F y , where 0.1≤a≤0.7, 0.1≤b≤0.7, 0.1≤y≤0.7, (2a+b)≤x≤1.3*(2a+b).
[0114] Using a subset of these compositions, experiments demonstrated that these compounds can indeed produce high-performance lithium-ion cathodes. Fig.11A and Fig. 11B As shown, the diffraction patterns clearly show the pure phase disordered rock salt structure of LR-LMVO and LR-LMVF20. That is, Fig.11A and 11B The X-ray diffraction patterns and scanning electron microscope images of the synthesized (a) LR-LMVO and (b) LR-LMVF20 materials are shown, respectively, indicating that the products are phase-pure disordered rock salts.
[0115] The electrochemical performance of these cathodes is Fig. 12A and 12B That is, Fig. 12A and 12B Shown are the galvanostatic charge / discharge voltage curves of (a) LR-LMVO and (b) LR-LMVF20, respectively, obtained in the first five cycles in the window voltage from 1.5 V to 4.6 V. The inset shows the drop in charge and discharge capacity in the first 20 cycles.
[0116] As shown in the figure, at a cut-off voltage of 4.6 V, the first charge and discharge capacity of LR-LMVO is as high as 312 mAh / g (824 Wh / kg), and the first charge and discharge capacity of LR-LMVF20 reaches 296 mAh / g (786 Wh / kg). Importantly, the energy density obtained at a cut-off voltage of 4.6 is highly reversible, as shown in Fig. 12A and Fig. 12B The charge and discharge capacity decreases very slowly during the first 20 cycles, as evidenced by the repeated cycling curves shown in the inset. This reversibility of the material is consistent with other reported lithium-excess cathodes. 1This is in stark contrast to the latter, which typically lose a lot of capacity after the first few cycles due to oxygen loss or are only reversible at low voltages. 2 The high transition metal content (balancing its capacity to match the available Li content) of the compositions reported here eliminates the need for O charge / discharge capacity, thereby improving reversible electrochemical performance.
[0117] Although previous patents and 3 The patents have space for the cathode of lithium fluoride batteries, but these patents do not cover the divalent transition metal (Mn 2+ , Fe 2+ 、Co 2+ 、Ni 2+ ) and V or Mo. The present invention specifically focuses on combining the electrochemical activity of these divalent metals with the limited activity from V or Mo, and optionally using F substitution to achieve additional degrees of freedom in the Li component, and balancing the available Li capacity with the capacity of the redox active transition metal in the material. Thus, the present invention provides the ability to design compositions that are intended to provide optimal electrochemical performance.
[0118] An example of a direct application of aspects of the present invention is a lithium ion cathode battery cathode material for high density energy storage, where cathode energy density is a key limiting factor affecting overall battery performance. In particular, embodiments of various aspects of the present invention are well suited for use in long life secondary lithium ion batteries, where the reversibility of the compounds of the present invention represents a desirable feature for achieving stable performance over charge / discharge cycles.
[0119] Although the numerical ranges and parameters setting forth the broad scope of the present invention are approximate, the numerical values listed in the specific examples should be reported as accurately as possible. However, any numerical value inherently contains certain errors, which must be caused by the standard deviation in their respective test measurements. In addition, when setting forth the numerical ranges of varying ranges herein, it is contemplated that any combination of these values, including the recited values, may be used. In fact, all ranges disclosed herein are inclusive and combinable. For example, all ranges include endpoints and all intermediate values of the ranges.
[0120] The scope of the invention described and claimed herein is not limited by the specific embodiments disclosed herein, as these embodiments are intended to serve as illustrations of several aspects of the invention. Several aspects of the invention include all available, non-contradictory sub-combinations of the claims set forth below. Any equivalent embodiments are within the scope of the invention. In fact, various modifications of the invention will become apparent to those skilled in the art, based on the foregoing description, in addition to those shown and described herein. Such modifications also fall within the scope of the appended claims. All patents and patent applications cited above are expressly incorporated herein by reference in their entirety.
Claims
1. A lithium metal fluorine oxide having the general formula: Li x M’ a M” b O 2-y F y , wherein the lithium metal fluorine oxide has a cation - disordered rock - salt structure of either (a) or (b), where (a) 1.09 ≤ x ≤ 1.35, 0.1 ≤ a ≤ 0.7, 0.1 ≤ b ≤ 0.7 and 0 < y ≤ 0.7; M’ is Mn 2+ , and M” is selected from the group consisting of V 3+ , V 4+ , Mo 4+ , Mo 5+ and combinations thereof, and (2a + b) ≤ x ≤ 1.3(2a + b); and (b) 1.1 ≤ x ≤ 1.33, 0.1 ≤ a ≤ 0.41, 0.39 ≤ b ≤ 0.67 and 0 < y ≤ 0.3; M’ is Mn 2+ ; M” is selected from the group consisting of V 3+ , V 4+ , Mo 4+ , Mo 5+ and combinations thereof, and (2a + b) ≤ x ≤ 1.3(2a + b).
2. The lithium metal fluorine oxide according to claim 1, wherein M” is V 4+ or Mo 5+ .
3. The lithium metal fluorine oxide according to claim 1, having the formula: Li x M’ a V b O 2-y F y , wherein 1.09 ≤ x ≤ 1.35, 0.1 ≤ a ≤ 0.7, 0.1 ≤ b ≤ 0.7 and 0 < y ≤ 0.
7.
4. The lithium metal fluorine oxide according to claim 1, wherein the rock - salt structure is 1.1 ≤ x ≤ 1.2, 0.25 ≤ a ≤ 0.4, 0.4 ≤ b ≤ 0.6 and 0 < y ≤ 0.
3.
5. The lithium metal fluorine oxide according to claim 1 is Li 1.23 Mn 0.255 V 0.515 O 1.8 F 0.2 (LR - LMVF20).
6. The lithium metal fluorine oxide according to any one of claims 1 to 5 has a cation - disordered rock - salt structure characterized by the crystallographic space group Fm - 3m. 7 . The lithium metal oxyfluoride according to claim 1 , having a discharge capacity of 250 mAh / g to 400 mAh / g.
8. The lithium metal oxyfluoride according to any one of claims 1 to 5, which has an energy density of 700 Wh / kg to 900 Wh / kg.
9. A positive electrode material comprising: The lithium metal oxyfluoride according to claims 1 to 5.
10. A lithium ion battery comprising: Anode material; Electrolytes; and The positive electrode material according to claim 9.
11. A portable electronic device, a vehicle or an energy storage system comprising: The lithium ion battery according to claim 10.