Fuel cell stack and method for manufacturing the same
By using high density and thin thickness controlled metal porous components and partitions in fuel cells, the problem of large-scale fuel cells caused by thickening of partitions is solved, miniaturization and improvement of mechanical strength is achieved, and it is suitable for Vibration environments such as cars.
Patent Information
- Application Number
- CN201911172576.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-11-28
- Filing Date
- 2019-11-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-11-26
AI Technical Summary
When the existing fuel cell partitions are made by stamped steel plates, the partitions become thicker, which makes the fuel cell larger and difficult to be mounted in a vibrating environment such as automobiles.
A partition made of a metal material is adopted, and a first metal porous part and a second metal porous part are provided thereon. An internal connection structure is formed through printing technology and integrated firing technology, so that the density of the partition is more than 90%. , the thickness is controlled below 100μm to ensure the mechanical strength and durability of the fuel cell.
The miniaturization of fuel cells and the improvement of mechanical strength are achieved, and it can operate stably in vibrating environments such as cars, and prevent structural rupture during rapid temperature rise and fall.
Smart Images

Figure CN111244520B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a fuel cell stack and a method for manufacturing the same. Background Art
[0002] In order to develop a solid oxide fuel cell system that can be used in automobiles, etc., it is desired to develop a unit cell that can withstand vibration and will not break even if the temperature rises rapidly. For example, a fuel cell in which the internal connection structure is formed of a ceramic material is disclosed (for example, refer to Patent Document 1). However, in this fuel cell, mechanical strength and tolerance to rapid temperature rise and fall are lacking, so it is difficult to be installed in automobiles, etc. Therefore, a fuel cell using a separator is disclosed, and the separator is made by stamping a steel plate (for example, refer to Patent Document 2).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: International Publication No. 2018 / 042476
[0006] Patent Document 2: Japanese Patent Application Publication No. 2016-39099 Summary of the invention
[0007] Technical problem to be solved by the invention
[0008] However, when the separator is produced by pressing a steel plate, the separator becomes thicker, resulting in an increase in the size of the fuel cell.
[0009] Technical solutions for solving technical problems
[0010] The fuel cell stack of the present invention is characterized in that it includes: a first fuel cell and a second fuel cell in which a solid oxide electrolyte layer having oxygen ion conductivity is sandwiched by two electrode layers; a separator made of a metal material, which is arranged between the above-mentioned first fuel cell and the above-mentioned second fuel cell; and an internal connection structure, which has a first metal porous portion and a first gas flow path on the above-mentioned first fuel cell side of the above-mentioned separator, and a second metal porous portion and a second gas flow path on the above-mentioned second fuel cell side of the above-mentioned separator.
[0011] In the above fuel cell stack, the density of the separator may be 90% or more.
[0012] In the above fuel cell stack, the separator may have a thickness of 100 μm or less.
[0013] In the above fuel cell stack, the density of the first porous metal portion and the second porous metal portion may be 30% or more and 80% or less.
[0014] In the above-mentioned fuel cell stack, the above-mentioned first metal porous part, the above-mentioned separator and the above-mentioned second metal porous part can be stacked in sequence, and the total thickness of the above-mentioned first metal porous part, the above-mentioned dense metal layer and the above-mentioned second metal porous part in the stacking direction is less than 300μm.
[0015] In the above-mentioned fuel cell stack, the above-mentioned internal connection structure can be composed of the following material, that is, when the above-mentioned first gas flow path is supplied with hydrogen-containing fuel gas and the above-mentioned second gas flow path is supplied with oxygen-containing oxidant gas, the electron conductivity on the above-mentioned first fuel cell side becomes higher than the electron conductivity on the above-mentioned second fuel cell side.
[0016] In the above fuel cell stack, the internal connection structure may be formed of a material capable of forming an oxide film on the surface when in contact with oxygen.
[0017] The manufacturing method of the fuel cell stack of the present invention is characterized in that it includes: the steps of preparing a stack, in which a plurality of first patterns having a disappearing material and a metal powder are arranged on a metal powder layer at predetermined intervals, a first electrode layer is stacked on the plurality of first patterns, an electrolyte layer is arranged on the first electrode layer, a plurality of second patterns having a disappearing material and a metal powder are arranged under the metal powder layer at predetermined intervals, and a second electrode layer is stacked under the plurality of second patterns; and the step of firing the stack.
[0018] Effects of the Invention
[0019] According to the present invention, it is possible to provide a fuel cell stack that can be miniaturized and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a three-dimensional diagram of the appearance of a fuel cell stack.
[0021] Figure 2 It is a perspective view illustrating details of the internal connection structure.
[0022] Figure 3 A diagram schematically showing a cross-sectional photograph of an internal connection structure.
[0023] Figure 4A and Figure 4B The diagram illustrates a method for manufacturing a fuel cell stack.
[0024] Figure 5A to Figure 5C The diagram illustrates a method for manufacturing a fuel cell stack.
[0025] Description of Reference Numerals
[0026] 10 Solid Oxide Electrolyte Layer
[0027] 20 Cathode
[0028] 21 Box
[0029] 30 First porous metal layer
[0030] 31 Frame
[0031] 40 Anode
[0032] 41 Frame
[0033] 50 Second metal porous layer
[0034] 51 Frame
[0035] 60 Dividers
[0036] 71 PET film
[0037] 72 Metal powder layer
[0038] 73 Frame
[0039] 74 Metal Powder Pattern
[0040] 75 PET film
[0041] 76 Electrolyte layer
[0042] 77 Frame
[0043] 78 electrode layer
[0044] 79 Gas flow path forming material
[0045] 91 first stack
[0046] 92 Second stack
[0047] 93 Third stack
[0048] 94 Fourth stack
[0049] 95 Molding
[0050] 100 Fuel Cell
[0051] 200 fuel cell stack. DETAILED DESCRIPTION
[0052] Hereinafter, embodiments will be described with reference to the drawings.
[0053] like Figure 1As shown in the example, the fuel cell stack 200 has a structure in which a plurality of fuel cells 100 are stacked. The fuel cell 100 has a structure in which a cathode 20 (first electrode layer), a first metal porous layer 30 including a first metal porous portion 30a and a gas flow path 30b, and a separator 60 are stacked in the following order on the upper surface (first surface) of the solid oxide electrolyte layer 10, and an anode 40 (second electrode layer), a second metal porous layer 50 including a second metal porous portion 50a and a gas flow path 50b, and a separator 60 are stacked in the following order on the lower surface (second surface) of the solid oxide electrolyte layer 10. In addition, the separator 60 is a common component in adjacent fuel cells 100. Sometimes the combination of the first metal porous layer 30, the separator 60 and the second metal porous layer 50 is referred to as an internal connection structure. The internal connection structure is a portion for electrically connecting the unit cells consisting of the solid oxide electrolyte layer 10, the cathode 20 and the anode 40 in series. In addition, a combination of the solid oxide electrolyte layer 10 , the cathode 20 , the first metal porous layer 30 , the anode 40 , and the second metal porous layer 50 may be referred to as a unit SOFC unit.
[0054] The solid oxide electrolyte layer 10 is a dense layer of a solid oxide electrolyte having oxygen ion conductivity. The cathode 20 is an electrode having electrode activity as a cathode, having electron conductivity and oxygen ion conductivity. The anode 40 is an electrode having electrode activity as an anode, having electron conductivity and oxygen ion conductivity. The first metal porous layer 30 and the second metal porous layer 50 are components having gas permeability and capable of supporting a unit cell portion consisting of the solid oxide electrolyte layer 10, the cathode 20 and the anode 40. The separator 60 is a dense metal layer having gas impermeability. The gas flow paths 30b and 50b are pores made of a disappearing material.
[0055] The fuel cell 100 generates electricity through the following actions. In the first metal porous part 30a and the gas flow path 30b, an oxidant gas containing oxygen such as air is supplied as a reaction gas. The oxidant gas reaches the cathode 20 via the first metal porous part 30a and the gas flow path 30b. In the cathode 20, the oxygen reaching the cathode 20 reacts with the electrons supplied from the external circuit to become oxygen ions. The oxygen ions are conducted in the solid oxide electrolyte layer 10 and move to the anode 40 side. On the other hand, in the second metal porous part 50a and the gas flow path 50b, a fuel gas containing hydrogen such as hydrogen gas and reformed gas is supplied as another reaction gas. The fuel gas reaches the anode 40 via the second metal porous part 50a and the gas flow path 50b. The hydrogen reaching the anode 40 releases electrons in the anode 40, and reacts with the oxygen ions conducted from the cathode 20 side in the solid oxide electrolyte layer 10 to form water (H2O). The released electrons are taken out to the outside by the external circuit. The electrons extracted to the outside are electrically processed and then supplied to the cathode 20. Electricity is generated by the above-described actions.
[0056] The solid oxide electrolyte layer 10, the cathode 20, the first metal porous layer 30, the anode 40 and the second metal porous layer 50 have a roughly rectangular shape of roughly the same size. Therefore, the solid oxide electrolyte layer 10, the cathode 20, the first metal porous layer 30, the anode 40 and the second metal porous layer 50 constitute a roughly rectangular parallelepiped shape. In the rectangular parallelepiped shape, a pair of two sides facing each other among the four sides other than the upper surface and the lower surface are called the first side and the second side. The remaining pair of two sides facing each other are called the third side and the fourth side. Let the direction in which the first side faces the second side face is the X-axis. Let the direction in which the third side faces the fourth side face is the Y-axis. Let the stacking direction of each layer be the Z-axis. The X-axis, the Y-axis and the Z-axis are, for example, orthogonal to each other.
[0057] A frame 21 is provided on the third side and the fourth side of the cathode 20, respectively. A frame 31 is provided on the third side and the fourth side of the first metal porous layer 30, respectively. The frame 21 and the frame 31 function as sealing members. Therefore, a flow path of the oxidant gas is formed by the frame 21, the frame 31, and the separator 60 in contact with the first metal porous layer 30. Thus, the oxidant gas flows from any one of the first side and the second side to the other in the first metal porous layer 30. That is, the oxidant gas flows in the X-axis direction.
[0058] A frame 41 is provided on the first side and the second side of the anode 40, respectively. A frame 51 is provided on the first side and the second side of the second metal porous layer 50, respectively. The frame 41 and the frame 51 function as sealing members. Therefore, a flow path of the fuel gas is formed by the frame 41, the frame 51, and the separator 60 in contact with the second metal porous layer 50. Thus, the fuel gas flows from any one of the third side and the fourth side to the other in the second metal porous layer 50. That is, the fuel gas flows in the Y-axis direction.
[0059] Figure 2 is a perspective view illustrating the details of the internal connection structure. Figure 2 As shown in the example, the internal connection structure has a structure in which a first metal porous layer 30 is provided on a separator 60 and a second metal porous layer 50 is provided under the separator 60. The separator 60 has a function of blocking the permeation of the reaction gas and has a function of connecting two adjacent fuel cells 100 in series.
[0060] In the first metal porous layer 30, a plurality of first metal porous portions 30a extend in a strip shape along the X-axis direction. Each first metal porous portion 30a is arranged at a predetermined interval in the Y-axis direction. Therefore, a gas flow path 30b extending in the X-axis direction is formed between two adjacent first metal porous portions 30a. The interval in the Y-axis direction of each first metal porous portion 30a is, for example, 500 μm to 3000 μm. The oxidant gas supplied to the first metal porous layer 30 is mainly supplied to the cathode 20 while flowing in the gas flow path 30b. A portion of the oxidant gas is supplied to the cathode 20 while diffusing from the first metal porous portion 30a. The first metal porous portion 30a is in contact with the cathode 20, and therefore acts as a current collector and also as a support.
[0061] In the second metal porous layer 50, a plurality of second metal porous portions 50a extend in a strip shape along the Y-axis direction. Each second metal porous portion 50a is arranged at a predetermined interval in the X-axis direction. Therefore, a gas flow path 50b extending in the Y-axis direction is formed between two adjacent second metal porous portions 50a. The interval in the X-axis direction of each second metal porous portion 50a is, for example, 500 μm to 5000 μm. The fuel gas supplied to the second metal porous layer 50 is mainly supplied to the anode 40 while flowing in the gas flow path 50b. A portion of the fuel gas is supplied to the anode 40 while diffusing from the second metal porous portion 50a. The second metal porous portion 50a is in contact with the anode 40, and therefore acts as a current collector and also as a support.
[0062] Figure 3 It is a figure which shows schematically a cross-sectional photograph of the internal connection structure. Figure 3 The cross section of is a cross section of the portion where the first porous metal portion 30a and the second porous metal portion 50a sandwich the separator 60. Figure 3 As shown, the metal is densely formed in the separator 60. In the first metal porous part 30a and the second metal porous part 50a, the parts where the metal is densely formed and the parts where the metal is not formed and become voids exist in a mixed manner. In this way, the reaction gas can be diffused even in the first metal porous part 30a and the second metal porous part 50a.
[0063] The separator 60 is preferably dense enough to block the oxidant gas and the fuel gas. Therefore, the separator 60 preferably has a higher density. For example, the density of the separator 60 is preferably 90% or more, and more preferably 98% or more. The density is based on an image obtained by observing the cross section using a SEM (scanning electron microscope) or the like, and the area of the dense portion and the total area of the void portion and the dense portion are measured, and the ratio of the two (area of the dense portion / total area of the void portion and the dense portion) can be calculated. The porosity can be calculated by calculating (area of the void portion / total area of the void portion and the dense portion).
[0064] When the separator 60 is formed thicker, the distance between two adjacent fuel cells 100 becomes longer and the resistance becomes higher. Therefore, it is preferred to form the separator 60 thinner. For example, the thickness of the separator 60 is preferably less than 100μm, and more preferably less than 60μm. On the other hand, when the separator 60 is too thin, the continuity of the separator 60 is reduced, and undesirable conditions such as holes that are prone to gas leakage may occur. Therefore, it is preferred to set a lower limit for the thickness of the separator 60. For example, the thickness of the separator 60 is preferably more than 10μm, and more preferably more than 40μm. By forming the separator 60 thinner, the fuel cell stack 200 can also be miniaturized.
[0065] The first porous metal part 30a and the second porous metal part 50a preferably have a density that can supply the reaction gas to the electrode. For example, the density of the first porous metal part 30a and the second porous metal part 50a is preferably 80% or less, and more preferably 60% or less. On the other hand, when the density of the first porous metal part 30a and the second porous metal part 50a is too low, the adhesion (closed contact force) between the layers is reduced during firing, and the separator 60 and the anode 40 and the cathode 20 may peel off. Therefore, it is preferred to set a lower limit for the density of the first porous metal part 30a and the second porous metal part 50a. For example, the density of the first porous metal part 30a and the second porous metal part 50a is preferably 30% or more, and more preferably 50% or more.
[0066] In addition, when the internal connection structure is formed thicker as a whole, the distance between two adjacent fuel cells 100 becomes longer and the resistance becomes higher. Therefore, it is preferred to form the internal connection structure thinner as a whole. For example, the total thickness of the first metal porous layer 30, the separator 60 and the second metal porous layer 50 is preferably 400 μm or less, and more preferably 250 μm or less. By forming the internal connection structure thinner as a whole, the fuel cell stack 200 can be miniaturized.
[0067] The material of the internal connection structure is not particularly limited as long as it is a metal, but it is preferably composed of a material that makes the electron conductivity of the anode 40 side higher than that of the cathode 20 side when the oxidant gas is supplied to the gas flow path 30b and the fuel gas is supplied to the gas flow path 50b. For example, it is preferred that the first metal porous layer 30, the separator 60, and the second metal porous layer 50 are composed of a material that can form an oxide film on the surface when exposed to oxygen. For example, the first metal porous layer 30, the separator 60, and the second metal porous layer 50 can use a metal such as Ni. Alternatively, it is preferred to use an alloy containing one or more of the elements such as C, Si, Al, Nb, Mo, Y, Ce, Cr, Fe, Ti, Cu, Mn, La, W, Ni, and Zr, and containing 10 wt% to 95 wt% of Cr, making the trace additive elements other than Fe and Cr less than 10 wt%, and the rest being Fe components. For example, Fe-18 to 22Cr alloys can be used. By forming an oxide film on the surface, it is possible to suppress oxidation from progressing to the inside.
[0068] In addition, the fuel cell 100 of the present embodiment has a structure that can suppress cracking during firing. Specifically, in the cathode 20 and the anode 40, it is preferred that the main component of the material having electron conductivity is the same (common) as the main component of the material having oxygen ion conductivity. In this structure, since the materials of the cathode 20 and the anode 40 are similar, when the adhesive is removed during the firing process of the cathode 20 and the anode 40, the imbalance (bias) of the shrinkage stress of the two layers can be suppressed, and cracking can be suppressed. Thus, a unit cell portion consisting of a solid oxide electrolyte layer 10, a cathode 20, and an anode 40 can be formed by printing technology and integrated firing technology. Thus, it is possible to achieve both an increase in the number of stacking layers and miniaturization. As a result, it is possible to ensure the desired power generation and achieve miniaturization.
[0069] For example, there is no particular limitation on the main component of the electron and oxygen ion mixed conductive material used in the cathode 20 and the anode 40. For example, as the cathode 20 and the anode 40, it is considered to use a material having both electron conductivity and oxygen ion conductivity (electron and oxygen ion mixed conductive material). For example, LaMnO3 series, LaCoO3 series, etc. can be used as the electron and oxygen ion mixed conductive material. However, in the integral firing, the metal powder is fired at the same time to form the first metal porous layer 30 and the second metal porous layer 50, so it is desirable to make the atmosphere a reducing atmosphere. When LaMnO3 series, LaCoO3 series, etc. are used as the main component of the electron and oxygen ion mixed conductive material, good power generation performance can be obtained, but on the other hand, firing in a reducing atmosphere is difficult. Therefore, the main component of the electron and oxygen ion mixed conductive material preferably has reduction resistance. For example, it is preferred to use a CeO2 series material doped with Gd.
[0070] As another method, different materials are used as the electron conductive material and the oxygen ion conductive material, respectively, and mixed conductivity of electrons and oxygen ions can also be achieved as a whole. For example, the main component of the oxygen ion conductive material is not particularly limited, and scandium oxide-yttria stabilized zirconia (ScYSZ) is preferably used. For example, it is preferred to use ScYSZ having a composition range of 5 mol% to 16 mol% of scandium oxide (Sc2O3) and 1 mol% to 3 mol% of yttria (Y2O3). It is more preferred to use ScYSZ in which the addition amount of scandium oxide and yttria is 6 mol% to 15 mol% in total. Because in this composition range, the oxygen ion conductivity becomes the highest. In addition, the oxygen ion conductive material is, for example, a material having an oxygen ion transport number of 99% or more.
[0071] Next, there is no particular limitation on the electron conductive material, and metals such as Ni can be used. Alternatively, an alloy containing one or more elements such as C, Si, Y, Ce, Cr, Fe, Ti, Cu, Mn, La, W, Ni, and Zr is preferably used, and contains 10wt% to 95wt% of Cr, and an alloy in which other elements are less than 30wt%. Specifically, Fe-18 to 22Cr alloys can be used. By using metal and alloy materials, the mechanical strength of the SOFC system becomes higher, and it can cope with rapid temperature rise and temperature drop. This characteristic is fully utilized and can be installed in a car. In addition, with respect to the composition of the alloy, by increasing Cr, the thermal expansion coefficients of the cathode 20 and the anode 40 are close to the thermal expansion coefficient of the solid oxide electrolyte layer 10, so that the unit cell becomes less likely to break. In addition, alloys with more Cr have excellent heat resistance and can suppress the degradation of the unit cell during power generation. However, in order to suppress costs and Cr poisoning on the cathode side, it is preferred that the Cr content is less. Among the above contents, the composition of Fe-18 to 22Cr is a relatively balanced composition, and is therefore preferred.
[0072] In addition, ceramics can be used as the main component of the electron conductive material used in the cathode 20 and the anode 40. For example, LaCrO3 doped with Sr, SrTiO3 doped with La, etc. can be used. These materials are stable substances in a wide partial pressure range of reducing atmosphere and oxidizing atmosphere, and have low reactivity with other materials (electrolytes), and are materials suitable for manufacturing processes. In addition, the high-temperature stability of ceramic materials is better than that of metals and alloy materials, so if it is a SOFC system with good durability, ceramic materials are preferred. In addition, for example, the conductivity of the electron conductive material at a temperature above 400°C is 10S·cm -1 The above materials have conductivity substantially the same as that of metals.
[0073] In addition, when different materials are used for the oxygen ion conductive material and the electron conductive material, when a plurality of oxygen ion conductive materials are mixed and used, it is sufficient that the main component of the oxygen ion conductive material is common to the cathode 20 and the anode 40, and it is preferred that the plurality of oxygen ion conductive materials are common to each other. In addition, when different materials are used for the oxygen ion conductive material and the electron conductive material, when a plurality of electron conductive materials are mixed and used, it is sufficient that the main component of the electron conductive material is common to the cathode 20 and the anode 40, and it is preferred that the plurality of electron conductive materials are common to each other.
[0074] The thickness of the cathode 20 and the anode 40 is preferably 50 μm or less, more preferably 30 μm or less. When the reformed gas is used as a fuel, the thickness of the electrode that can effectively contribute to the electrochemical reaction is usually about 30 μm, because when the hydrocarbon fuel is used directly, the effective electrode thickness becomes thicker, usually about 50 μm.
[0075] The cathode 20 and the anode 40 may also contain a catalyst. For example, Ni compounds such as Ni(NO3)3 and NiCl3 can be used as catalysts for the cathode 20 and the anode 40. As a method of adding Ni, a method of impregnating the solution with Ni(NO3)3, NiCl3, etc. after firing can be used.
[0076] The solid oxide electrolyte layer 10 preferably has 6 mol% to 15 mol% of ZrO2 or the like doped in scandium oxide (Sc2O3) and yttrium oxide (Y2O3) as the main component. The concentration of scandium oxide (Sc2O3) + yttrium oxide (Y2O3) is between 6 mol% and 15 mol% and the oxygen ion conductivity is the highest, and it is preferred to use a material of this component. In addition, the thickness of the solid oxide electrolyte layer 10 is preferably less than 20 μm, and more preferably less than 10 μm. The thinner the electrolyte, the better, but in order to manufacture it in a way that the gas on both sides does not leak, a thickness of 1 μm or more is preferably used.
[0077] The first metal porous layer 30 and the second metal porous layer 50 are not particularly limited. For example, metals such as Ni can be used. In addition, it is preferred to use an alloy containing one or more elements such as C, Si, Al, Nb, Mo, Y, Ce, Cr, Fe, Ti, Cu, Mn, La, W, Ni, and Zr, and containing 10wt% to 95wt% of Cr, with trace elements other than Fe and Cr being less than 10wt%, and the rest being Fe. Specifically, Fe-18 to 22Cr alloys can be used.
[0078] In addition, the porosity of the first metal porous part 30a and the second metal porous part 50a is preferably 30% to 70%, and more preferably 40% to 60%. Because when the porosity is less than 30%, gas diffusion is inhibited, which may reduce the power generation. On the other hand, because the strength of the metal porous part is insufficient when the porosity is greater than 70%, it may not be able to play the function of supporting the gas flow path. In addition, the thickness of the first metal porous part 30a and the second metal porous part 50a is preferably 150μm to 50μm, and more preferably 100μm or less. Becoming thinner and reducing the volume of the entire SOFC system is beneficial for miniaturization, but in order to ensure the necessary gas flow rate, a thickness of 50μm or more is required. In addition, the first metal porous layer 30 and the second metal porous layer 50 are supports for forming a gas flow path, and the thickness of the flow path is roughly the same as the thickness of the first metal porous layer 30 and the second metal porous layer 50. The gas flow paths 30b and 50b are made of a material that disappears at a temperature range of 200 to 600°C, and the paste is printed in line and space. The disappearing material is not particularly limited, and organic substances such as acrylic resins can be used.
[0079] In the fuel cell stack 200 of the present embodiment, an internal connection structure such as one made by stamping a steel plate is not used, but the following internal connection structure is used, that is, a first metal porous portion 30a (first metal porous portion) and a gas flow path 30b (first gas flow path) are provided on one surface of the separator 60 (dense metal layer), and a second metal porous portion 50a (second metal porous portion) and a gas flow path 50b (second gas flow path) are provided on the other surface of the separator 60. If it is such an internal connection structure, the internal connection structure can be made by sintering using printing technology and integrated firing technology. As a result, the internal connection structure can be made thinner. As a result, the fuel cell stack 200 can be miniaturized.
[0080] In addition, in the fuel cell 100 manufactured using the printing technology and the integrated firing technology, the proportion of the metal part becomes higher. Because the ceramic NiO is used as a support in the unit cell of the prior art, unlike this, since it is manufactured by integral firing with the internal connection structure in this embodiment, a support is not required, and the volume ratio of the metal can be increased. For example, the volume ratio of the metal part relative to the fuel cell stack 200 is more than 70%. In such a structure, the Young's modulus of the metal material is high and it is less likely to break.
[0081] The first porous metal part 30a and the second porous metal part 50a are sintered on both sides of the separator 60, and the first porous metal part 30a and the second porous metal part 50a are in close contact with the separator 60. As a result, the deformation of the structure during rapid temperature rise and fall can be effectively suppressed. In addition, the first porous metal part 30a is sintered with the cathode 20, and the second porous metal part 50a is sintered with the anode 40, thereby improving the close contact between the internal connection structure and the unit cell part.
[0082] Next, a method for manufacturing the fuel cell stack 200 will be described.
[0083] (Manufacturing steps of dense metal material)
[0084] As a dense metal material, metal powder (for example, with a particle size of 1 μm to 10 μm), a plasticizer (for example, adjusted to 1wt% to 6wt% in order to adjust the adhesion of the sheet), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20wt% to 30wt% depending on the viscosity), and a binder (PVB (polyvinyl butyral), acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. In order to form a dense body by sintering, no material is mixed and lost. The dense metal material is used as a material for forming the partition 60, the frame 31 and the frame 51. The volume ratio of the organic component (the solid part of the binder and the plasticizer) to the metal powder is, for example, in the range of 1:4 to 1:1.
[0085] (Steps for producing porous metal materials)
[0086] As a porous metal material, metal powder (for example, with a particle size of 10 μm to 100 μm), a plasticizer (for example, adjusted to 1 wt% to 6 wt% in order to adjust the adhesion of the sheet), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a vanishing material (organic matter), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The porous metal material is used as a material for forming the first metal porous part 30a and the second metal porous part 50a. The volume ratio of the organic component (vanishing material, binder solid part, plasticizer) to the metal powder is set in the range of 1:1 to 20:1, for example, and the amount of the organic component is adjusted according to the porosity.
[0087] (Steps for producing electrode layer material)
[0088] As materials for the electrode layer, an electron conductive material powder (e.g., with a particle size of 100 nm to 10 μm), an oxygen ion conductive material powder (e.g., with a particle size of 100 nm to 10 μm), a catalyst (e.g., a Ni compound with a particle size of 10 nm to 1 μm), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a plasticizer (e.g., adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), a vanishing material (organic matter), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. As a method for adding Ni, a method of impregnating the sintered material with a solution of Ni(NO3)3, NiCl3, etc. can be used. The volume ratio of the organic component (vanishing material, binder solid part, plasticizer) to the electron conductive material powder is set to, for example, a range of 1:1 to 5:1, and the amount of the organic component is adjusted according to the porosity. The volume ratio of the electron conductive material powder to the oxygen ion conductive material powder is set in a range of, for example, 3:7 to 7:3.
[0089] (Steps for preparing the material for the dense mixed layer)
[0090] As materials for the dense mixed layer, electronic conductive material powder (e.g., particle size of 1 μm to 10 μm), oxygen ion conductive material powder (e.g., particle size of 10 nm to 10 μm), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on viscosity), plasticizer (e.g., adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet) and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. Since it is a layer for blocking gas, no catalyst or disappearing material is mixed.
[0091] (Steps for preparing electrolyte layer material)
[0092] As a material for the electrolyte layer, an oxygen ion conductive material powder (e.g., ScYSZ, YSZ, etc., with a particle size of 10nm to 1000nm), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20wt% to 30wt% depending on the viscosity), a plasticizer (e.g., adjusted to 1wt% to 6wt% to adjust the adhesion of the sheet), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (binder solid part, plasticizer) to the oxygen ion conductive material powder is, for example, in the range of 6:4 to 3:4.
[0093] (Steps for producing gas flow path forming material)
[0094] Using a disappearing material (organic substances such as acrylic resin, polyimide resin, etc.), a plasticizer (for example, adjusted to 1wt% to 6wt% in order to adjust the adhesion of the sheet), a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20wt% to 30wt% depending on the viscosity), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry.
[0095] First, if Figure 4A As shown in the above figure, a dense metal material is applied to a PET (polyethylene terephthalate) film 71 to form a roughly rectangular shape by 20 μm to 35 μm, thereby forming a metal powder layer 72. For example, the metal powder layer 72 has a roughly rectangular shape, and as an example, has a square shape with a side length of 60 mm to 70 mm. Next, two frames 73 are formed by printing the dense metal material at the ends of the two opposite side surfaces of the metal powder layer 72. Regarding the frame 73, according to the accuracy of stacking and cutting, for example, the width is in the range of 1 mm to 10 mm, and the length is in the range of 60 mm to 70 mm. Next, on the metal powder layer 72, a porous metal material is printed between the two frames 73, thereby forming a metal powder pattern 74. For example, as Figure 4A As shown in the following figure, a plurality of band-shaped metal powder patterns 74 are formed at predetermined intervals. Next, the gas flow path forming material 79 is printed in the reverse pattern of the metal powder pattern 74 to fill the empty space. Thus, the first stack 91 is formed. The thickness of the frame 73 is, for example, 100 μm to 200 μm. The thickness of the metal powder pattern 74 is, for example, ±10 μm of the thickness of the frame 73. In addition, Figure 4A The lower right picture is a top view.
[0096] Then, if Figure 4B As shown in the above figure, the electrolyte layer material is applied to the PET film 75 to form a shape roughly the same as the metal powder layer 72 with a thickness of 5μm to 15μm, thereby forming an electrolyte layer 76. Next, the dense electrode layer material is printed on the ends of the two opposite side surfaces of the electrolyte layer 76, thereby forming two frames 77. Regarding the frame 77, according to the accuracy of stacking and cutting, for example, the width is in the range of 1mm to 10mm, and the length is in the range of 60mm to 70mm. Next, the electrode layer material is printed between the two frames 77 on the electrolyte layer 76, thereby forming an electrode layer 78 (the reverse pattern layer opposite to the frame 77). In this way, the second stack 92 can be formed. The thickness of the frame 77 is, for example, 15μm to 40μm. The thickness of the electrode layer 78 is, for example, the thickness of the frame 77 ±3μm. Among them, Figure 4B The lower right picture is a top view.
[0097] Then, if Figure 5A As illustrated in FIG. 1 , the first stack 91 is stacked on the second stack 92. In this case, the second stack 92 is turned over so that the electrode layer 78 is stacked on the metal powder pattern 74. In addition, the frame 77 is stacked on the frame 73. Thus, the third stack 93 is formed. In addition, the PET 75 is peeled off.
[0098] Then, if Figure 5B As shown in the example, another third stack 93 is stacked on the third stack 93. In this case, the other third stack 93 is stacked in a manner that the electrolyte layer 76 is stacked on the electrolyte layer 76. In addition, the other third stack 93 is rotated 90 degrees in a state where two electrolyte layers 76 are opposite to each other. That is, in the third stack 93 and the other third stack 93, the side surfaces of the arrangement frame 73 and the frame 77 are different. Thus, the fourth stack 94 is formed.
[0099] Then, if Figure 5C As shown in the example, a plurality of (e.g., 200) fourth stacks 94 are stacked in a state where the PET film 71 is peeled off. Thus, a molded body 95 is formed. In the molded body 95, the electrolyte layer 76 corresponds to the solid oxide electrolyte layer 10 after firing, the electrode layer 78 on the upper surface (first surface) of the electrolyte layer 76 corresponds to the cathode 20 after firing, the metal powder pattern 74 on the electrode layer 78 corresponds to the first metal porous portion 30a after firing, the electrode layer 78 under the lower surface (second surface) of the electrolyte layer 76 corresponds to the anode 40 after firing, the metal powder pattern 74 under the electrode layer 78 corresponds to the second metal porous portion 50a after firing, and the metal powder layer 72 corresponds to the separator 60 after firing.
[0100] The molded body 95 is subjected to hydrostatic pressing at a pressure of, for example, 100 MPa. The molded body 95 with each layer tightly attached is cut into a square with a side length of 60 mm to 65 mm. Thereafter, a debinding treatment is performed in an atmospheric atmosphere. Organic components slowly decompose between 200°C and 700°C, so in order to suppress the adverse conditions of the debinding treatment, the temperature is slowly raised within a temperature range of 200°C to 700°C over a period of about 1 week. Thereafter, the temperature is maintained at 700°C for about 1 hour.
[0101] Next, the molded body 95 from which the binder has been removed is moved to a reduction firing furnace and fired in a reducing atmosphere such as 100% H2, 0.1-4% H2-Ar atmosphere. The method for manufacturing a sintered integrated SOFC stack can be carried out in accordance with the known method. That is, it is implemented in a manner such that at least a portion of the constituent metal and ceramic materials is sintered to obtain a desired sintered body of dense or porous quality. It is preferred to sinter all the elements together. For example, the heat treatment can be performed at a temperature of 1200°C to 1550°C, and more preferably at a temperature of 1250°C to 1400°C. In addition, the firing time at the above-mentioned firing temperature is not particularly limited, but since the slow firing method can suppress the shrinkage difference of each layer, for example, several hours to tens of hours can be used. In addition, the gas flow path forming material 79 can disappear in any heat treatment.
[0102] Afterwards, the cathode 20 and the anode 40 are impregnated with catalysts as needed, thereby completing the fuel cell stack 200. For example, when impregnating the anode 40 with a catalyst, the cathode 20 is sealed with a masking tape and impregnated in a solution of Ni nitrate or Ni chloride, and then dried. On the other hand, the cathode 20 is impregnated in a nitrate precursor solution such as Ag nitrate, Pr nitrate, or LSM, LSC, or LSCF, and then dried. Afterwards, heat treatment is performed at 300°C to 850°C in an air atmosphere to decompose and react the impregnated reagent to form a desired catalyst.
[0103] In the manufacturing method of the present embodiment, a stacked body is prepared and then fired, wherein in the stacked body, on a metal powder layer 72, a plurality of gas flow path forming materials 79 and a metal powder pattern 74 (first pattern) having metal powder are arranged at predetermined intervals, an electrode layer 78 (first electrode layer) is stacked on the plurality of metal powder patterns 74, an electrolyte layer 76 is arranged on the electrode layer 78, and under the metal powder layer 72, a plurality of gas flow path forming materials 79 and a metal powder pattern 74 (second pattern) having metal powder are arranged at predetermined intervals, and an electrode layer 78 (second electrode layer) is stacked under the plurality of metal powder patterns 74.
[0104] According to the manufacturing method, the internal connection structure can be made using printing technology and integrated firing technology. As a result, the internal connection structure can be formed thinner. As a result, the fuel cell stack 200 can be miniaturized. In addition, by sintering the first metal porous part 30a and the second metal porous part 50a on both sides of the separator 60, the close contact between the first metal porous part 30a and the second metal porous part 50a and the separator 60 can be improved. As a result, the deformation of the structure during rapid temperature rise and fall can be effectively suppressed. In addition, the first metal porous part 30a is sintered with the cathode 20, and the second metal porous part 50a is sintered with the anode 40, which can also improve the close contact between the internal connection structure and the unit cell part.
[0105] [Example]
[0106] According to the above embodiment, a fuel cell stack 200 is manufactured. As a dense metal material, a Fe-Cr alloy powder with a particle size of 20 μm is used. As a porous metal material, a Fe-Cr alloy powder with a particle size of 20 μm is used. As an electrode layer material, a Fe-Cr alloy powder with a particle size of 5 μm and a 10Sc1YSZ powder with a particle size of 100 nm are used. As a dense mixed layer material, a Fe-Cr alloy powder with a particle size of 5 μm and a 10Sc1YSZ powder with a particle size of 100 nm are used. As an electrolyte material, a 10Sc1YSZ powder with a particle size of 100 nm is used. As a gas flow path forming material, an acrylic resin is used. In the internal connection structure after integral firing, the separator 60 is a 98% dense body with a thickness of 40 μm. The width of the gas flow path 30b is 1 mm. Since it is designed to be relatively thick in order to allow air to flow, the thickness of the gas flow path 30b is 95 μm. In addition, the width of the gas flow path 50b is 1 mm, and since it is designed to be relatively thin in order to allow the fuel gas to flow, the thickness of the gas flow path 50b is 70 μm. In addition, the width of the first metal porous part 30a is 1 mm, the same height as the gas flow path 30b, and the density is about 70 vol%. The width of the second metal porous part 50a is 1 mm, the same height as the gas flow path 50b, and the density is about 70 vol%. The total thickness of the internal connection structure composed of the separator 60, the first metal porous layer 30 and the second metal porous layer 50 is 205 μm.
[0107] As mentioned above, although the embodiment of the present invention was described in detail, the present invention is not limited to the above-mentioned specific embodiment, and various deformation|transformation and changes are possible within the scope of the summary of the present invention described in the claims.
Claims
1. A fuel cell stack, characterized in that: include: A first fuel cell and a second fuel cell in which a solid oxide electrolyte layer having oxygen ion conductivity is sandwiched between two electrode layers; as well as An internal connection structure, comprising a separator disposed between the first fuel cell and the second fuel cell, wherein a first metal porous portion and a first gas flow path are provided on the first fuel cell side of the separator, and a second metal porous portion and a second gas flow path are provided on the second fuel cell side of the separator, wherein the separator is a sintered body of metal powder and has a thickness of 100 μm or less, One of the two electrode layers includes a first material having oxygen ion conductivity and a second material having electron conductivity that is different from the first material. The other electrode layer of the two electrode layers includes a third material having oxygen ion conductivity and a fourth material having electron conductivity that is different from the third material. The main component of the first material is the same as the main component of the third material, The main component of the second material is the same as the main component of the fourth material, The two electrode layers and the solid oxide electrolyte layer are sintered bodies.
2. The fuel cell stack according to claim 1, characterized in that: The density of the separator is above 90%.
3. The fuel cell stack according to claim 1 or 2, characterized in that: The density of the first porous metal part and the second porous metal part is 30% or more and 80% or less.
4. The fuel cell stack according to claim 1 or 2, characterized in that: The first porous metal part, the separator, and the second porous metal part are stacked in this order, and the total thickness of the first porous metal part, the separator, and the second porous metal part in the stacking direction is 300 μm or less.
5. The fuel cell stack according to claim 1 or 2, characterized in that: The internal connection structure is made of a material that causes electron conductivity on the first fuel cell side to be higher than electron conductivity on the second fuel cell side when the first gas flow path is supplied with a fuel gas containing hydrogen and the second gas flow path is supplied with an oxidant gas containing oxygen.
6. The fuel cell stack according to claim 5, characterized in that: The internal connection structure is made of a material capable of forming an oxide film on the surface when in contact with oxygen.
7. A method for manufacturing a fuel cell stack, characterized in that: include: A step of preparing a stacked body, wherein a plurality of first patterns having a disappearing material and a metal powder are arranged at predetermined intervals on a metal powder layer, a first electrode layer is stacked on the plurality of first patterns, an electrolyte layer is arranged on the first electrode layer, a plurality of second patterns having a disappearing material and a metal powder are arranged at predetermined intervals under the metal powder layer, and a second electrode layer is stacked under the plurality of second patterns; and a step of firing the laminate, By firing the laminate, a separator having a thickness of 100 μm or less is obtained from the metal powder by sintering. The first electrode layer includes a first material having oxygen ion conductivity and a second material having electron conductivity that is different from the first material. The second electrode layer includes a third material having oxygen ion conductivity and a fourth material having electron conductivity that is different from the third material, The main component of the first material is the same as the main component of the third material, The main component of the second material is the same as the main component of the fourth material.
Citation Information
Patent Citations
Interconnector, solid oxide fuel cell stack, and method for manufacturing solid oxide fuel cell stack
WO2018042476A1
Fuel cell stack and fuel cell system
CN101821891A
Stack structure for solid oxide fuel cell stack, solid oxide fuel cell stack, and production method for the same
CN103647100A
Wet grinding and warm-pressing sintering method for metal bipolar plate of proton exchange membrane fuel cell
CN107146898A
Fuel cell
JP1988146363A