A method for evaluating the corrosion rate of the bottom plate of a petroleum storage tank

By calculating the corrosion rate and correction coefficient on the soil and oil storage sides, combined with climate and oil tank design factors, the problem that the existing technology cannot accurately evaluate the corrosion rate of the bottom plate of the oil storage tank without opening the tank is solved, and the petroleum is achieved Accurate prediction of the corrosion rate of the tank base plate supports tank maintenance management and reduces maintenance costs.

CN111382490BActive Publication Date: 2024-11-08CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201811627229.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2018-12-28
Publication Date
2024-11-08
Estimated Expiration
2038-12-28

AI Technical Summary

Technical Problem

The prior art cannot accurately evaluate the corrosion rate of the bottom plate of the petroleum storage tank without opening the tank, affecting the tank maintenance management and production efficiency.

Method used

Based on the basic corrosion rate and correction coefficient calculation on the soil and oil storage side, combined with climate, environment and oil tank design factors, the corrosion rate of the petroleum storage tank bottom plate is judged and calculated, and uniform corrosion and local corrosion are distinguished to achieve unopening. Accurate evaluation in case of tanks.

Benefits of technology

It provides accurate prediction of the corrosion rate of the in-service storage tank base plate, supports tank maintenance management, reduces maintenance costs and production shutdown time, and is suitable for the actual situation of my country's petroleum storage tanks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111382490B_ABST
    Figure CN111382490B_ABST
Patent Text Reader

Abstract

The embodiment of the present invention provides a method for evaluating the corrosion rate of the bottom plate of a petroleum storage tank, including: obtaining the corrosion rate of the soil side of the bottom plate based on the basic corrosion rate of the soil side of the bottom plate, the first correction coefficient of the oil tank and the environmental correction coefficient; obtaining the corrosion rate of the oil storage side of the bottom plate based on the basic corrosion rate of the oil storage side of the bottom plate, the second correction coefficient of the oil tank and the correction coefficient of the stored oil; judging whether the corrosion of the oil storage side of the bottom plate is uniform corrosion or local corrosion; if the corrosion of the oil storage side is uniform corrosion, the corrosion rate of the bottom plate is the sum of the corrosion rate of the soil side and the corrosion rate of the oil storage side; if the corrosion of the oil storage side is local corrosion, the corrosion rate of the bottom plate is the maximum value of the corrosion rate of the soil side and the corrosion rate of the oil storage side. The method proposes the main factors and correction coefficients that affect the corrosion rate of the bottom plate, and can accurately predict the corrosion rate of the bottom plate of the in-service storage tank without opening the tank, providing technical support for the maintenance and management of the tank.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The embodiments of the present invention relate to the field of storage tank safety evaluation, and in particular to a method for evaluating the bottom plate corrosion rate of a petroleum storage tank. Background Art

[0002] Oil storage tanks are containers for storing crude oil or other oil products, and are used in refineries, oil fields, oil depots, and other industries. Oil tanks usually include three types: steel oil tanks, reinforced concrete oil tanks, and brick oil tanks. Steel oil tanks have three structures: vertical oil tanks, spherical shell oil tanks, and horizontal oil tanks. Vertical oil tanks are divided into vertical dome oil tanks and vertical floating roof oil tanks. Vertical dome oil tanks are composed of a spherical crown tank top and a vertical cylindrical tank wall, and are mainly used to store oil products that are not volatile. The vertical floating roof oil tank is composed of a floating roof (floating plate) floating on the surface of the oil and a vertical cylindrical tank wall. The floating roof rises and falls with the increase or decrease of the oil storage in the tank. There is an annular sealing device between the outer edge of the floating roof and the tank wall. The oil in the tank is always directly covered to reduce the volatilization of the oil. It is mainly used to store volatile oil products. Floating roofs are divided into single-disc floating roofs, double-disc floating roofs, and float-type floating roofs.

[0003] The corrosion of the bottom plate of oil storage tanks is one of the main causes of oil leakage. The determination of the corrosion rate of the bottom plate of the tank usually requires the use of offline detection technologies such as ultrasound and magnetic leakage after the tank is opened. However, the production must be stopped for the maintenance of the tank, and the maintenance operation is time-consuming and expensive, which affects the oil storage production of the oil depot. Therefore, how to predict the corrosion rate of the bottom plate of the in-service tank and provide a technical reference for the reasonable determination of the maintenance cycle has become the focus of petrochemical enterprises.

[0004] At present, the prediction of the bottom plate corrosion rate of in-service tanks is mostly carried out by introducing foreign risk-based tank corrosion rate evaluation models. However, the actual structure and operation management of oil storage tanks in my country are different from those in foreign countries, such as the design of anti-corrosion in the tank, oil quality requirements, and the bottoming of the floating plate. Therefore, the determination of the corrosion rate should not only consider the structure of the tank, but also focus on the climate environment in which the tank is located and the influence of correction factors such as actual operation, maintenance, online detection and management on the corrosion rate. In particular, how to achieve a scientific evaluation of the bottom plate corrosion rate without opening the tank is a difficult problem that oil depot companies urgently need to solve.

[0005] The prior art (application number CN201710028586.6) discloses a method for evaluating the corrosion of the bottom of a steel oil storage tank, including step 1: establishing a composite fuzzy matter-element matrix R; step 2: constructing a composite fuzzy matter-element matrix of correlation coefficients Step 3: Determine the weighted composite element of each feature index Step 4: Determine the composite fuzzy matter-element with correlation degree It can be seen that this technical solution uses a model to qualitatively evaluate the corrosion state of the bottom plate. In addition, to accurately evaluate the corrosion condition of the bottom of the oil tank, it is necessary to use a magnetic flux leakage detector and an ultrasonic detector to simultaneously detect the corrosion condition of the front and back sides of the tank bottom plate after opening the tank. It is impossible to accurately evaluate the corrosion rate of the tank bottom plate without opening the tank. Summary of the invention

[0006] In view of the problems existing in the prior art, an embodiment of the present invention provides a method for evaluating the corrosion rate of the bottom plate of a petroleum storage tank, which realizes accurate evaluation of the corrosion rate of the bottom plate without opening the tank.

[0007] The embodiment of the present invention relates to a method for evaluating the bottom plate corrosion rate of a petroleum storage tank, which is characterized by comprising:

[0008] Based on the soil side basic corrosion rate of the bottom plate, and the first correction factor and the environmental correction factor of the oil tank, the soil side corrosion rate of the bottom plate is obtained;

[0009] Based on the basic corrosion rate of the oil storage side of the bottom plate, the second correction factor of the oil tank and the correction factor of the stored oil, the corrosion rate of the oil storage side of the bottom plate is obtained;

[0010] Determining whether the corrosion on the oil storage side of the bottom plate is uniform corrosion or local corrosion;

[0011] If the corrosion on the oil storage side is uniform corrosion, the corrosion rate of the bottom plate is the sum of the corrosion rate on the soil side and the corrosion rate on the oil storage side; or

[0012] If the corrosion on the oil storage side is local corrosion, the corrosion rate of the bottom plate is the maximum value between the corrosion rate on the soil side and the corrosion rate on the oil storage side.

[0013] Furthermore, the first correction coefficient of the oil tank includes: a correction coefficient of the oil tank foundation, a correction coefficient of the cathodic protection of the bottom plate, a correction coefficient of the oil tank heating temperature, a correction coefficient of the tank bottom sealing effect, and a correction coefficient of the external corrosion of the bottom plate edge.

[0014] Furthermore, the environmental correction factor includes: a climate correction factor, a soil resistivity correction factor, and a drainage correction factor around the oil tank foundation.

[0015] Furthermore, the calculation formula for obtaining the soil side corrosion rate of the oil tank bottom plate is:

[0016] CR S =CR SB ×F HJ ×F SR ×F PA ×F TD ×F CP ×FST ×F PE ×F OU

[0017] Among them, CR S is the soil side corrosion rate of the bottom plate, CR SB is the basic corrosion rate on the soil side of the bottom plate, F HJ is the climate correction factor, F SR is the soil resistivity correction factor, F PA is the correction factor of the oil tank foundation, F TD is the drainage correction factor around the oil tank foundation, F CP is the cathodic protection correction factor of the bottom plate, F ST is the oil tank heating temperature correction factor, F PE is the tank bottom sealing effect correction factor, F OU Correction factor for external corrosion at the edge of the base plate.

[0018] Furthermore, the second correction coefficient of the oil tank includes: a correction coefficient for the pumping condition at the bottom of the tank, a correction coefficient for the bottoming of the floating plate, and a correction coefficient for the heating temperature of the oil tank.

[0019] Furthermore, the correction coefficients of the stored oil products include: a correction coefficient for the water content of the oil products and a correction coefficient for the oil product turnover.

[0020] Furthermore, the calculation formula for obtaining the corrosion rate of the oil storage side of the oil tank bottom plate is:

[0021] CR P =CR PB ×F PC ×F WD ×F OT ×F SD ×F PT

[0022] Among them, CR P is the corrosion rate of the oil storage side of the bottom plate, CR PB is the basic corrosion rate of the oil storage side of the bottom plate, F PC is the oil water content correction factor, F WD is the correction factor for tank bottom pumping, F OT is the oil turnover correction factor, F SD is the floating plate bottoming correction factor, F PT Correction factor for tank heating temperature.

[0023] Furthermore, if the corrosion on the oil storage side is uniform corrosion, the calculation formula for the bottom plate corrosion rate is CR = CR S +CR P , where CR is the corrosion rate of the bottom plate, CR Sis the soil side corrosion rate of the bottom plate, CR P is the corrosion rate on the oil storage side of the base plate.

[0024] Furthermore, if the corrosion on the oil storage side is localized corrosion, the calculation formula for the bottom plate corrosion rate is CR = max [CR S , CR P ], where CR is the corrosion rate of the bottom plate, CR S is the soil side corrosion rate of the bottom plate, CR P is the corrosion rate on the oil storage side of the base plate.

[0025] The method for evaluating the bottom plate corrosion rate of a petroleum storage tank provided in an embodiment of the present invention proposes the main factors affecting the bottom plate corrosion rate and the correction coefficients based on the actual situation of petroleum storage tanks in my country. The corrosion rate of the bottom plate of an in-service storage tank can be accurately predicted without opening the tank, thus providing technical support for the maintenance management of the storage tank. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A flow chart of a method for evaluating the corrosion rate of a bottom plate provided by an embodiment of the present invention;

[0028] Figure 2 A flow chart for obtaining the soil side corrosion rate of a bottom plate provided by an embodiment of the present invention;

[0029] Figure 3 A flow chart for obtaining the corrosion rate of the oil storage side of the bottom plate provided by an embodiment of the present invention;

[0030] Figure 4 The present invention is a schematic diagram of a system for detecting corrosion on the oil storage side of an oil tank bottom plate in the prior art. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Figure 1The flowchart of the bottom plate corrosion rate evaluation method of the petroleum storage tank provided by the embodiment of the present invention is shown. Figure 1 As shown,

[0033] Step 101, based on the soil side basic corrosion rate of the bottom plate, and the first correction coefficient and the environmental correction coefficient of the oil tank, the soil side corrosion rate of the bottom plate is obtained;

[0034] Step 102, based on the basic corrosion rate of the oil storage side of the bottom plate, the second correction coefficient of the oil tank and the correction coefficient of the stored oil, the corrosion rate of the oil storage side of the bottom plate is obtained;

[0035] Step 103, determining whether the corrosion on the oil storage side of the bottom plate is uniform corrosion or local corrosion;

[0036] Step 104, if the corrosion on the oil storage side of the bottom plate is uniform corrosion, the corrosion rate of the bottom plate is the sum of the corrosion rate on the soil side and the corrosion rate on the oil storage side; or

[0037] Step 105, if the corrosion on the oil storage side of the bottom plate is local corrosion, the corrosion rate of the bottom plate is the maximum value between the corrosion rate on the soil side and the corrosion rate on the oil storage side.

[0038] According to the actual situation of petroleum storage tanks in my country, the embodiment of the present invention proposes oil tank design factors, environmental factors and oil product factors that affect the bottom plate corrosion rate, as well as corresponding correction coefficients. The corrosion rate of the bottom plate of the in-service tank can be accurately predicted without opening the tank, providing technical support for the maintenance management of the tank.

[0039] Figure 2 A flow chart for obtaining the soil-side corrosion rate of a bottom plate of a petroleum storage tank provided by an embodiment of the present invention is shown.

[0040] In the embodiment of the present invention, considering that the actual structure and operation management of oil storage tanks in my country are different from those in foreign countries, for example, factors such as the anti-corrosion design inside the tank, the oil quality requirements, and the tank placement environment all have their own characteristics, the first correction coefficient of the oil tank in the embodiment of the present invention includes: the correction coefficient F of the oil tank foundation PA , cathodic protection correction factor F of the bottom plate CP , Oil tank heating temperature correction factor F ST , tank bottom sealing effect correction factor F PE , Correction factor F for external corrosion of bottom plate edge OU The environmental correction factors include: climate correction factor F HJ , soil resistivity correction factor F SR , Drainage correction factor F around the oil tank foundation TD Those skilled in the art may select other factors and correction coefficients that affect corrosion according to the actual conditions of the oil tank, and are not subject to the above limitations.

[0041] In the embodiment of the present invention, the calculation formula of the soil side corrosion rate of the bottom plate of the petroleum storage tank is:

[0042] CR S =CR SB ×F HJ ×F SR ×F PA ×F TD ×F CP ×F ST ×F PE ×F OU

[0043] Among them, CR S is the soil side corrosion rate of the bottom plate, CR SB is the basic corrosion rate on the soil side of the base plate.

[0044] Next, we will combine the attached Figure 2 The corresponding relationship between various factors affecting the corrosion rate of the soil side of the bottom plate and the correction coefficient is described in detail. Those skilled in the art can select a specific correction coefficient to obtain the corrosion rate of the soil side of the bottom plate according to the actual situation of the oil tank.

[0045] like Figure 2 As shown, step 201, determine the basic corrosion rate CR of the soil side of the bottom plate of the oil storage tank SB Generally, the basic corrosion rate of the bottom plate soil side can be determined based on actual conditions, or the basic corrosion rate of the bottom plate soil side can be determined as 0.13 mm / year based on historical statistical data.

[0046] Step 202, obtaining the climate correction factor F HJ Since oil storage tanks will corrode in the air, air humidity is an important indicator that affects the degree of bottom plate corrosion. my country is a vast country with different regions in different climate zones, so the degree of corrosion of oil storage tanks in different climate zones is different. Table 1 shows the corresponding relationship between different climate environments and correction coefficients.

[0047] Table 1

[0048]

[0049] In Table 1, the characteristics of high mountain and plateau climate are low temperature throughout the year and less precipitation; the characteristics of temperate continental climate are hot summer and cold winter, with little rain throughout the year; the characteristics of temperate monsoon climate are high temperature and heavy rain in summer and cold and little rain in winter; the characteristics of subtropical monsoon climate are high temperature and heavy rain in summer and mild and little rain in winter; the characteristics of tropical monsoon climate are high temperature throughout the year and two seasons of dry and rainy seasons. It can be seen that as the climate environment becomes hotter and hotter, the correction factor for calculating the corrosion rate becomes higher and higher.

[0050] Step 203, obtaining soil resistivity correction factor F SR . Since the oil storage tank is placed directly on the foundation surface, the soil's corrosiveness to the tank bottom plate must be considered. The corrosion of metal materials in the soil is electrochemical corrosion. In many cases, the lower the soil resistivity, the greater the metal corrosion rate. Because the salt content of various soils is relatively stable, the resistivity mainly decreases with the increase of water content. Within a fairly large range, as the soil water content increases, the amount of oxygen dissolved increases and the diffusion rate increases, the metal ionization rate increases, and the metal corrosion rate in the soil increases. Therefore, the resistivity of the soil under the oil tank bottom plate will directly affect the corrosion rate of the bottom plate. Table 2 shows the correction factor F corresponding to different soil resistivities. SR .

[0051] Table 2

[0052]

[0053] Step 204, obtaining the correction factor F of the oil tank foundation PA . In order to ensure stability, good drainage and sufficient bearing capacity, the foundation (base) of the oil tank must be built. Large oil tanks often need to have a concrete foundation to enclose the entire foundation and increase stability. The oil tank foundation, depending on the type of oil tank, is easy to meet the production and use requirements, terrain, landform, foundation conditions, and construction technical conditions. The following are the common types of oil tank foundations that are reasonably selected: slope protection foundation, ring wall foundation, outer ring wall foundation, and special structure foundation. The materials used to build the oil tank foundation usually include sand with high resistance and low chloride, oil sand, concrete, asphalt, construction grade sand, local soil, crushed limestone and high salt soil. Since the weight of the oil and the oil tank itself acts directly on the oil tank foundation through the bottom plate, the outer surface of the bottom plate is in close contact with the oil tank foundation and is easily corroded by moisture. Therefore, the type of oil tank foundation also affects the corrosion rate of the bottom plate. Table 3 shows the correction coefficients corresponding to different types of oil tank foundations (bases).

[0054] Table 3

[0055]

[0056] Step 205, obtaining the drainage correction factor F around the oil tank foundation TD . Since the oil tank bottom plate is in direct contact with the oil tank foundation, when rainwater falls and gathers around the oil tank foundation, it will accelerate the corrosion of the bottom plate. If the drainage slope of the oil tank foundation is damaged, it will be unfavorable for the discharge of rainwater and will lead to an accelerated corrosion rate. Therefore, the corrosion rate of the bottom plate is related to the drainage conditions around the oil tank foundation. In the process of obtaining the corrosion rate of the soil side of the bottom plate, the influence of the drainage conditions needs to be considered. Table 4 shows the corresponding relationship between the drainage conditions around the oil tank foundation and the correction coefficient.

[0057] Table 4

[0058]

[0059]

[0060] Step 206, obtaining the cathodic protection correction factor F of the bottom plate of the oil storage tank CP . Usually, the oil tank foundation material under the oil tank bottom plate will gradually age with the growth of time, and cracks will appear in the oil tank foundation. In this way, the underground moisture will contact the oil tank bottom plate through the cracks and cause corrosion to the bottom plate. Therefore, more and more attention is paid to the cathodic protection of oil storage tanks. The principle of cathodic protection is to add a large amount of electrons to the metal so that the protected metal is in a state of excess electrons as a whole, and each point on the metal surface reaches a uniform negative potential. There is no potential difference between the points on the metal surface, and there is no flow of electrons, so that the metal atoms no longer lose electrons and become ions to merge into the environment. The cathodic protection system not only requires correct installation and maintenance, but also in daily operation, it is necessary to ensure that the system protection potential is within the allowable value range to ensure that the cathodic protection system works effectively. Table 5 shows the corresponding relationship between the operation of cathodic protection on the bottom plate and the correction coefficient.

[0061] Table 5

[0062]

[0063] Step 207, obtaining the correction factor F of the heating temperature of the oil storage tank ST When the oil is needed, it will be discharged from the oil tank. When the oil temperature is low and becomes viscous and difficult to flow, the oil cannot be discharged smoothly from the tank. At this time, the oil tank needs to be heated to make the oil flow easily. If the temperature is too high during the heating process, the oil will carbonize and coke, and if the temperature is too low, the oil will easily condense, which will affect the corrosion of the bottom plate. Table 6 shows the corresponding relationship between the heating temperature of the oil tank and the correction factor.

[0064] Table 6

[0065]

[0066]

[0067] Step 208, obtaining the correction factor F of the sealing effect of the oil tank bottom PE The sealing system at the bottom of the oil tank is an important means to prevent corrosion of the tank bottom plate. Once the tank bottom seal is damaged, moisture impurities in the air will enter the bottom plate, accelerating the corrosion of the tank bottom plate. Therefore, the integrity of the tank bottom seal structure is used as the value condition of the correction coefficient. Table 7 shows the corresponding relationship between the tank bottom seal and the correction coefficient.

[0068] Table 7

[0069]

[0070] Step 209, obtaining the correction factor F of the external corrosion of the bottom plate edge of the oil storage tank OU There are three reasons for the corrosion of the outer edge of the oil tank bottom plate. First, the part where the oil tank foundation and the tank bottom plate are combined causes the bottom plate to expand and contract radially with the change of ambient temperature. Second, the oil tank is deformed due to the load change of the oil storage volume in the oil tank, causing the oil tank to have horizontal displacement in the radial direction. The edge plate cannot expand outward because it is firmly welded to the bottom plate, resulting in deformation at the edge plate, thereby generating edge stress. This stress and the resistance of the oil tank foundation to the edge plate work together to cause plastic deformation of the outer ring of the bottom plate. Third, due to the uneven settlement of the oil tank foundation, cracks are formed between the outer edge of the oil tank bottom plate and the oil tank foundation, causing the invasion of external corrosive media.

[0071] The corrosion outside the edge of the oil tank bottom plate includes the corrosion of the outer edge plate of the bottom plate and the corrosion outside the corner weld of the tank bottom. The corrosion damage of the outer edge plate will cause bending deformation, causing the generation of edge stress, which will further cause stress corrosion. The welding point between the tank wall plate and the bottom edge plate is prone to corrosion due to gradual damage by rainwater. Table 8 shows the corresponding relationship between the external corrosion of the bottom plate edge and the correction factor.

[0072] Table 8

[0073]

[0074]

[0075] In step 210, during the specific operation, the staff selects a specific correction coefficient from the above list according to the actual situation of the oil storage tank and calculates it according to the following formula:

[0076] CR S =CR SB ×F HJ ×F SR ×F PA ×F TD ×F CP ×F ST ×F PE ×F OU

[0077] Obtain the soil side corrosion rate of the petroleum storage tank bottom plate.

[0078] The method for obtaining the corrosion rate of the soil side of the bottom plate provided in the embodiment of the present invention comprehensively considers various factors affecting the corrosion of the soil side of the bottom plate according to the actual construction and operation conditions of crude oil storage tanks in China, and proposes corresponding correction coefficients, which effectively solves the problem of online evaluation of the corrosion condition of the soil side of the tank bottom plate and provides a basis for tank maintenance.

[0079] Figure 3 A flow chart for obtaining the corrosion rate of the oil storage side of the bottom plate of a petroleum storage tank provided by an embodiment of the present invention is shown.

[0080] In the embodiment of the present invention, considering that the actual structure and operation management of oil storage tanks in my country are different from those in foreign countries, such as the anti-corrosion design inside the tank, the oil quality requirements, the tank placement environment and other factors all have their own characteristics, the second correction coefficient of the oil tank in the embodiment of the present invention includes: the correction coefficient F for the water pumping condition at the bottom of the tank WD , Floating plate bottoming correction factor F SD , Oil tank heating temperature correction factor F PT The correction factors for stored oil products include: Oil water content correction factor F PC , Oil turnover correction factor F OT Those skilled in the art may select other factors and correction coefficients that affect corrosion according to the actual conditions of the oil tank, and are not subject to the above limitations.

[0081] In the embodiment of the present invention, the corrosion rate calculation formula of the oil storage side of the bottom plate of the oil storage tank is:

[0082] CR P =CR PB ×F PC ×F WD ×F OT ×F SD ×F PT

[0083] Among them, CR P is the corrosion rate of the oil storage side of the bottom plate, CR PB is the basic corrosion rate on the oil storage side of the bottom plate.

[0084] Next, we will combine the attached Figure 3 The corresponding relationship between various factors affecting the corrosion rate of the oil storage side of the bottom plate and the correction coefficient is described in detail. Those skilled in the art can select a specific correction coefficient to obtain the corrosion rate of the oil storage side of the bottom plate according to the actual situation of the oil tank.

[0085] like Figure 3 As shown, step 301, determine the basic corrosion rate CR of the oil storage tank bottom plate oil storage side PBUsually, the basic corrosion rate of the bottom plate oil storage side can be determined according to the actual situation, or the basic corrosion rate of the bottom plate oil storage side can be determined as 0.05 mm / year based on historical statistical data.

[0086] Step 302: Obtain the correction factor F of the water content of the oil in the oil tank PC There is usually a certain amount of water in oil, especially in large crude oil storage tanks. Due to the large storage capacity, there may be a lot of sediment water at the bottom of the tank, which increases the degree of corrosion at the bottom of the tank. Therefore, the water content of the oil is an important factor affecting the corrosion rate of the bottom plate oil storage side. Table 9 shows the corresponding relationship between the water content of the oil and the correction factor.

[0087] Table 9

[0088]

[0089] Step 303, obtaining the correction factor F of the oil tank bottom pumping condition WD Due to the large storage volume of crude oil in large crude oil storage tanks, there may be a lot of water deposited in the oil at the bottom of the tank. Pumping water from the bottom of the tank can minimize the corrosion of the deposited water on the bottom plate. Frequent pumping operations and draining the water from the bottom of the tank can effectively reduce the corrosion of the bottom plate. Table 10 shows the corresponding relationship between the pumping situation at the bottom of the oil storage tank and the correction factor.

[0090] Table 10

[0091]

[0092] Step 304, obtaining the correction factor F of the stored oil turnover OT During the oil product turnover process, impurities such as air and water will be introduced. The turnover frequency of oil storage tanks will have a certain impact on the corrosion inside the tanks. Table 11 shows the corresponding relationship between the turnover of stored oil products and the correction coefficient.

[0093] Table 11

[0094]

[0095] Step 305, obtaining the correction factor F of the bottoming condition of the floating plate in the oil storage tank SD . The main function of the floating plate in the oil tank is to reduce the volatilization of oil. There is an annular sealing device between the outer edge of the floating plate and the tank wall. The oil in the tank is always directly covered by the floating plate. The floating plate will rise and fall with the increase or decrease of the oil storage in the tank. The floating plate of the oil storage tank will fall to the bottom due to deformation of the floating plate, uneven force, inflexible up and down of the central drainage pipe or other reasons. Once the floating plate falls to the bottom, the contact points between the pillars on the floating plate and the bottom plate are prone to pitting, dents and other damage, which will increase the corrosion of the inner side of the bottom plate. Table 12 shows the corresponding relationship between the floating plate falling to the bottom and the correction coefficient.

[0096] Table 12

[0097]

[0098] Step 306, obtaining the correction factor F of the heating temperature of the oil storage tank PT When oil is needed, it will be discharged from the oil tank. If the oil temperature is low and becomes viscous and difficult to flow, the oil cannot be discharged smoothly from the tank. At this time, the oil tank needs to be heated to make the oil flow easily. If the temperature is too high during the heating process, the oil will carbonize and coke, and if the temperature is too low, the oil will easily condense, which will affect the corrosion of the bottom plate. Table 13 shows the corresponding relationship between the heating temperature of the oil tank and the correction coefficient.

[0099] Table 13

[0100]

[0101] Step 307, during the specific operation, the staff selects a specific correction coefficient from the above list according to the actual situation of the oil storage tank, and calculates it according to the following formula:

[0102] CR P =CR PB ×F PC ×F WD ×F OT ×F SD ×F PT

[0103] Obtain the corrosion rate of the oil storage side of the oil storage tank bottom plate.

[0104] The method for obtaining the corrosion rate of the oil storage side of the bottom plate provided in the embodiment of the present invention comprehensively considers various factors affecting the corrosion of the oil storage side of the bottom plate according to the actual construction and operation conditions of crude oil storage tanks in China, and proposes corresponding correction coefficients, which effectively solves the problem of online evaluation of the corrosion condition of the oil storage side of the bottom plate of the tank and provides a basis for tank maintenance.

[0105] For the soil side corrosion and oil storage side corrosion of the bottom plate of the oil storage tank, usually, the soil side corrosion is mostly local corrosion, while the oil storage side corrosion is divided into uniform corrosion and local corrosion. If the detection finds uniform corrosion on the oil storage side, the corrosion rate of the bottom plate of the oil storage tank is the sum of the corrosion rate of the soil side of the bottom plate and the corrosion rate of the oil storage side of the bottom plate, that is, CR = CR S +CR P ;

[0106] If the oil storage side is locally corroded, the corrosion rate of the bottom plate is the maximum value of the corrosion rate of the soil side and the corrosion rate of the oil storage side, that is, CR = max[CR S , CR P ].

[0107] Figure 4 The schematic diagram of the system for detecting the corrosion of the oil storage side of the oil tank bottom plate in the prior art is shown. Figure 4 As shown, the detection system includes an acoustic detector, a sensor and an oil tank. When corrosion occurs on the oil storage side of the bottom plate of the oil tank, the corrosion point will generate an acoustic signal, and the corrosion point can be regarded as a sound source. The sensor is placed on the outside of the oil tank wall and located at the bottom of the oil tank near the bottom plate to collect the acoustic signal generated by the corrosion point and transmit the acoustic signal to the acoustic detector through a signal cable. The acoustic detector analyzes the signal frequency and the signal peak frequency. When the signal frequency is 20-70KHz or the signal peak frequency is 40-45KHz, the corrosion on the oil storage side of the bottom plate is judged to be uniform corrosion; when the signal frequency is 80-140KHz or the signal peak frequency is 110-120KHz, the corrosion on the oil storage side of the bottom plate is judged to be local corrosion (local pitting).

[0108] The bottom plate corrosion rate assessment method provided in the embodiment of the present invention distinguishes the actual construction and operation conditions of crude oil storage tanks at home and abroad, comprehensively considers factors such as the crude oil turnover frequency of the tank, the tank bottom seal, the crude oil composition, the tank bottom pumping, the floating plate bottom, and the cathodic protection, and proposes a corresponding correction coefficient. It is more targeted at my country's storage tanks, effectively solves the problem of online assessment of the bottom plate corrosion of the tank, and provides a basis for the maintenance of the tank.

[0109] Next, a 100,000 cubic meter crude oil storage tank in a certain oil depot in my country is used as an example to illustrate the specific application of the bottom plate corrosion rate assessment method provided by the embodiment of the present invention. In this embodiment, the crude oil storage tank is numbered 22 (22#), no tank corrosion detection has been performed, and the stored oil product is crude oil.

[0110] First, according to the actual situation of tank No. 22, Figure 2 The corrosion rate on the soil side of the base plate was obtained using the method shown in Table 14.

[0111] Table 14

[0112]

[0113] The second step is to follow the actual situation of tank No. 22. Figure 3 The corrosion rate of the oil storage side of the base plate was obtained by the method shown in Table 15.

[0114] Table 15

[0115]

[0116]

[0117] By adopting Figure 4It can be seen from the detection method shown that the corrosion on the oil storage side of the bottom plate is uniform corrosion. Therefore, according to the method provided by the embodiment of the present invention, the corrosion rate of the bottom plate is the sum of the corrosion rate on the soil side and the corrosion rate on the oil storage side, that is, the corrosion rate evaluation value of the bottom plate of the No. 22 oil storage tank is CR = CR S +CR P =0.305 mm / year.

[0118] If the corrosion on the oil storage side of the bottom plate is found to be local corrosion through testing, the corrosion rate of the bottom plate is the maximum value of the corrosion rate on the soil side and the corrosion rate on the oil storage side, that is, CR = max[CR S , CR P ]=0.16 mm / year.

[0119] In order to verify the effect of the evaluation method provided by the embodiment of the present invention, the No. 22 tank was opened for inspection, and it was found that the actual value of the bottom plate corrosion rate was 0.3, and the error was within an acceptable range. The bottom plate corrosion rate evaluation method provided by the embodiment of the present invention takes into account more comprehensive factors, and the prediction results are in line with reality. It can accurately predict the bottom plate corrosion rate of the tank without opening the tank, providing strong support for the prediction of the tank overhaul cycle.

[0120] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for evaluating the corrosion rate of the bottom plate of a petroleum storage tank, characterized in that: include: Based on the soil side basic corrosion rate of the bottom plate, and the first correction factor and the environmental correction factor of the oil tank, the soil side corrosion rate of the bottom plate is obtained; Based on the basic corrosion rate of the oil storage side of the bottom plate, the second correction factor of the oil tank and the correction factor of the stored oil, the corrosion rate of the oil storage side of the bottom plate is obtained; Determining whether the corrosion on the oil storage side of the bottom plate is uniform corrosion or local corrosion; If the corrosion on the oil storage side is uniform corrosion, the corrosion rate of the bottom plate is the sum of the corrosion rate on the soil side and the corrosion rate on the oil storage side; or If the corrosion on the oil storage side is local corrosion, the corrosion rate of the bottom plate is the maximum value between the corrosion rate on the soil side and the corrosion rate on the oil storage side; The first correction factor of the oil tank includes: a correction factor of the oil tank foundation, a correction factor of the cathodic protection of the bottom plate, a correction factor of the oil tank heating temperature, a correction factor of the tank bottom sealing effect, and a correction factor of the external corrosion of the bottom plate edge; The calculation formula for the soil side corrosion rate of the oil tank bottom plate is: CR S =CR SB ×F HJ ×F SR ×F PA ×F TD ×F CP ×F ST ×F PE ×F OU Among them, CR S is the soil side corrosion rate of the bottom plate, CR SB is the basic corrosion rate on the soil side of the bottom plate, F HJ is the climate correction factor, F SR is the soil resistivity correction factor, F PA is the correction factor of the oil tank foundation, F TD is the drainage correction factor around the oil tank foundation, F CP is the cathodic protection correction factor of the bottom plate, F ST is the oil tank heating temperature correction factor, F PE is the tank bottom sealing effect correction factor, F OU Correction factor for external corrosion at the bottom plate edge; The second correction coefficient of the oil tank includes: a correction coefficient for the pumping condition at the bottom of the tank, a correction coefficient for the bottoming of the floating plate, and a correction coefficient for the heating temperature of the oil tank; The calculation formula for the corrosion rate of the oil storage side of the oil tank bottom plate is: CR P =CR PB ×F PC ×F WD ×F OT ×F SD ×F PT Among them, CR P is the corrosion rate of the oil storage side of the bottom plate, CR PB is the basic corrosion rate of the oil storage side of the bottom plate, F PC is the correction factor for oil water content, F WD is the correction factor for tank bottom pumping, F OT is the oil turnover correction factor, F SD is the floating plate bottom correction factor, F PT Correction factor for tank heating temperature.

2. The method according to claim 1, characterized in that: The environmental correction factors include: climate correction factor, soil resistivity correction factor, and drainage correction factor around the oil tank foundation.

3. The method according to claim 1, characterized in that The correction coefficients of the stored oil products include: a correction coefficient for the water content of the oil products and a correction coefficient for the oil product turnover.

4. The method according to claim 1, characterized in that: If the corrosion on the oil storage side is uniform corrosion, the calculation formula for the bottom plate corrosion rate is CR = CR S +CR P , where CR is the corrosion rate of the bottom plate, CR S is the soil side corrosion rate of the bottom plate, CR P is the corrosion rate on the oil storage side of the base plate.

5. The method according to claim 1, characterized in that If the corrosion on the oil storage side is localized corrosion, the calculation formula for the bottom plate corrosion rate is CR = max [CR S , CR P ], where CR is the corrosion rate of the bottom plate, CR S is the soil side corrosion rate of the bottom plate, CR P is the corrosion rate on the oil storage side of the base plate.