Device comprising a multilayer body and a LIDAR sensor
By using a multi-layer body covering of aromatic polycarbonate substrate layer and polysiloxane topcoat layer, the problem of signal attenuation and scratch resistance of LiDAR sensor is solved, high transmittance and weather resistance are achieved, and components are extended service life.
Patent Information
- Application Number
- CN201880080886.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2017-12-21
- Filing Date
- 2018-12-14
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2038-12-14
AI Technical Summary
Existing thermoplastic materials are not suitable for LiDAR sensors, resulting in signal attenuation, and lack scratch resistance and weathering stability, affecting the function and service life of the sensor.
A multi-layer body covering consisting of a base layer made of aromatic polycarbonate and a polysiloxane topcoat layer is combined with UV absorber and organically modified silane and silicon sol to ensure that it is in the range of 800nm to 1600nm. low signal attenuation and high weather resistance.
The high transmittance and scratch resistance of LiDAR sensors in the infrared range are achieved, extending the service life of the components and improving resistance to environmental impacts.
Smart Images

Figure 118954 
Figure 243400 
Figure FHA0000007708260000011
Abstract
Description
[0001] The invention relates to a sensor system comprising a LiDAR sensor emitting laser light with a wavelength in the range of 800 nm to 1600 nm and a covering body which completely or partially surrounds the LiDAR sensor and comprises a multilayer body. The multilayer body arranged in front of the LiDAR sensor comprises a substrate layer made of a thermoplastic composition and at least one topcoat layer. The invention also relates to a vehicle comprising such a sensor system and to the use of a specific topcoat as a coating layer of a multilayer LiDAR sensor covering body.
[0002] Driver assistance systems, such as emergency brake assist systems, lane departure warning systems, traffic sign recognition systems, adaptive speed control systems and distance controllers are known and used in today's vehicles. In order to perform the functions mentioned, environmental detection sensors, which usually rely on radar sensors, LiDAR sensors, ultrasonic sensors and camera sensors, are used. LiDAR sensors are particularly important for highly automated driving and autonomous driving, because they are able to provide high-resolution three-dimensional images of the vehicle's surroundings from near to far ranges. The substrate materials described in the present invention are particularly suitable for LiDAR sensors.
[0003] LiDAR (Light detection and ranging) or LaDAR is an optical distance and velocity measurement method related to radar. It uses an infrared laser beam instead of the radio waves or microwaves of radar. There are very different types of LiDAR systems, which are mainly distinguished by the horizontal detection range (e.g. 70° to 360°), the type of laser (e.g. continuous wave scanning laser or static pulsed laser), and the sensor technology (e.g. mechanical rotating mirror or semiconductor electronics). The present invention also covers infrared cameras that use their own infrared light source, which are technically related to LiDAR.
[0004] For use in the automotive sector, components based on thermoplastic materials offer many advantages over conventional materials such as glass. This includes, for example, increased crack resistance and / or weight savings, which in the case of automobiles allows for greater passenger safety in the event of road traffic accidents and lower fuel consumption. Finally, materials containing thermoplastic polymers allow for much greater design freedom as they can be more easily shaped.
[0005] Since thermoplastic materials are generally transparent to infrared (IR) radiation, they should in principle be suitable for such sensor systems. However, surprisingly, as found in the present invention, most conventional thermoplastics used in the exterior area of automobiles are not suitable for such sensors. For example, it can be found that in the case of many thermoplastics, a low wall thickness of less than 1 mm is sufficient to significantly reduce the signal strength of the LiDAR sensor, so that they are not suitable for such systems. This includes, for example, polyolefins, polyamides, ABS, PC / ABS blends and other thermoplastic materials commonly used in the exterior area of automobiles.
[0006] In addition to the substrate material itself, there are other factors that can lead to attenuation of the LiDAR sensor signal. This includes, for example, other components made of different materials, as well as protective layers and / or paint layers. Coverings made of thermoplastic materials should be used to hide the LiDAR sensor and also protect the delicate sensor electronics. However, the covering itself must be protected from weathering and environmental influences and its outer surface must be protected from wear. This can be considered, for example, with corresponding paint layers. Such protective layers are known in principle and are used, for example, for headlight coverings. However, it has been found that not just any paint layer and protective layer that is suitable for thermoplastic systems is suitable for coating a covering for a sensor system including a LiDAR sensor.
[0007] The functionality of the sensor system must be ensured; weathering and wear effects must not have a negative impact on the functionality of the sensor. For example, wear, scratches or even corrosion in the paint layer may lead to attenuation of the LiDAR sensor signal. The prior art does not provide any teaching on the effects of general use wear or weathered paint layers arranged on thermoplastic materials on LiDAR sensors.
[0008] The prior art describes various thermoplastic systems which in principle exhibit permeability to electromagnetic waves.
[0009] CN 105400189 A describes laser-transmissive opaque substrate materials based on polyurethane-polyester systems. Special colorant combinations suitable for these polyurethane-polyester-based systems and which are in principle transparent to laser beams are described in detail. Such compositions are particularly suitable for laser welding. No substrate materials based on polycarbonate are described. Likewise, no substrate materials suitable for sensors are described.
[0010] WO 2016 / 037865 A1 describes an automotive exterior component having a glass-like appearance. No substrate material suitable for a LiDAR system is described therein.
[0011] WO 2008 / 12775 A1 describes radar sensors for automotive applications. However, these sensors operate in the range of 20-25 GHz and no conclusions can be drawn about substrate materials suitable for laser-assisted systems in the infrared region.
[0012] WO 2008 / 149093 A1 describes a laminated and pigmented glass system which is particularly suitable for LiDAR sensors. Solutions based on polycarbonate substrate materials cannot be deduced from this document.
[0013] US2009 / 284603 A1 describes thermoplastic substrates containing colorants. It is believed that these substrate materials have good permeability to IR radiation. It describes specific colorant mixtures. It does not describe whether these mixtures are suitable for laser-assisted detectors. No specific colorant compositions for polycarbonate are described.
[0014] EP 1772667 A2 describes a plastic component containing a light element arranged to be covered. The plastic component covers the light element but is transparent or translucent to the corresponding radiation. To achieve this, the substrate contains effect pigments. Such pigments are not suitable for laser-assisted systems because they cause scattering.
[0015] JP 2003-004942 A describes multilayer bodies composed of various material layers with different refractive indices. These systems are transparent to IR radiation. However, significantly higher requirements are placed on the material of the cover body for laser-assisted IR sensors. Laser-assisted sensors are not described.
[0016] US2016 / 0291134 A1 reports that LiDAR sensors are used in the automotive industry for autonomous or semi-autonomous driving. The substrate material used to cover or accommodate the LiDAR sensor is not described in detail.
[0017] The scratch resistance of polycarbonate can still be improved; therefore, scratch-resistant coatings are often also used for coating molded parts.
[0018] For these reasons, thermoplastic substrates, such as polycarbonate moldings, are provided with protective coatings. These protective systems are particularly suitable for exterior use, where they provide both mechanical protection against abrasion and scratches and excellent protection against weathering influences, such as rainfall, temperature and, in particular, ultraviolet (UV) radiation.
[0019] Coating systems suitable for these purposes (e.g. for polycarbonate headlamp covers) can be roughly divided into two categories:
[0020] (a) Thermosetting coating systems based on polysiloxane lacquers, which can be single-layer and multi-layer (only a primer layer to promote adhesion between substrate and polysiloxane topcoat). They are described primarily in US 4,278,804 A, US 4,373,061 A, US 4,410,594 A, US 5,041,313 A and EP-A-1087001.
[0021] (b) Likewise, UV-curing coating systems, for example based on acrylates, urethane acrylates or acrylsilanes and optionally containing fillers for improving scratch resistance, can provide adequate weathering protection due to the relatively wide range of film thicknesses over which they can be applied. Such systems are known and are described, inter alia, in US 3,707,397 A or DE 69717959 T2, US 5,990,188 A, US 5,817,715 A, US 5,712,325 A and WO 2014 / 100300 A1.
[0022] The prior art describes systems that are permeable to IR radiation based on thermoplastic substrates. Such substrates are suitable, for example, for infrared cameras or for laser welding. However, no practical teaching can be derived from this, since laser-assisted sensor systems operating in the IR range have a significantly increased sensitivity. Therefore, even the slightest scattering causes deviations in the sensor element and thus renders the corresponding substrate material unusable.
[0023] Thus, there is no description of multilayer bodies having a substrate layer of thermoplastic material, in particular those based on aromatic polycarbonate, which can be used for exterior parts of motor vehicles, rail vehicles and aircraft and the like and are suitable for vehicle environment monitoring by means of LiDAR sensors.
[0024] External components used in the field of motor vehicles, rail vehicles and aircraft or in the field of infrastructure which contain (preferably consist of) multilayer bodies, wherein the multilayer body contains a substrate layer of thermoplastic material, should also have a long service life as far as possible and not become brittle during the service life, i.e. they should be as weather-stable as possible. The color and the surface (gloss effect) should also change only slightly as far as possible. Thermoplastic components should also have sufficient scratch resistance as far as possible. Lack of scratch resistance or weathering stability can adversely affect the service life of the component itself and the function of the sensor system.
[0025] The object of the present invention is therefore to provide a corresponding device, i.e. a system, having a combination for environmental monitoring, which comprises a covering body made of a suitable multilayer body, comprising a substrate layer made of a thermoplastic material and a topcoat layer, and a LiDAR sensor, which operates in the IR range of 800 nm to 1600 nm. At least one of the other requirements mentioned above should also be met here, or the corresponding disadvantages should be overcome.
[0026] The object of the present invention is to provide a device for a vehicle, such as a rail vehicle, an aircraft (such as an airplane, a helicopter or a drone) or a motor vehicle, which device has a combination of a LiDAR sensor and a suitable covering body, wherein the LiDAR sensor operates in a wavelength range of 800 to 1600 nm, the covering body produces the lowest possible signal attenuation effect and is weather-resistant and abrasion-resistant, and the covering body is made of a multilayer body with a substrate layer, which substrate layer is made of a thermoplastic composition.
[0027] Surprisingly, it has been found that this object is achieved by:
[0028] A sensor system comprising
[0029] a) a LiDAR sensor that emits laser light having a wavelength of 800 to 1600 nm, and
[0030] b) a covering body partially or completely surrounding the LiDAR sensor, the covering body comprising a multilayer body, the multilayer body comprising in turn i) a substrate layer comprising a thermoplastic composition based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10min), preferably 9 to 19cm 3 / (10min), measured according to ISO 1133-1:2012-03 (300°C, 1.2kg),
[0031] wherein the composition has a light transmittance in the range of 380 to 780 nm of less than 25.0%, preferably at most 20%, more preferably less than 15%, measured according to DIN ISO 13468-2:2006 (D65, 10°) at a layer thickness of 4 mm,
[0032] and wherein the substrate layer has a transmittance of at least 40%, preferably 45%, particularly preferably 55% and particularly preferably more than 65% for IR radiation in the range from 800 nm to 1600 nm at its respective thickness, determined in accordance with DIN ISO 13468-2:2006 (according to this standard, using a wavelength range as mentioned above), and
[0033] ii) optionally a primer layer based on polymethyl methacrylate (PMMA) and comprising at least one UV absorber,
[0034] iii) a polysiloxane-based topcoat layer comprising a combination of an organically modified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Other particles ≥0.50μm,
[0035] wherein the topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged, and wherein the topcoat layer preferably contains a UV absorber,
[0036] Or a vehicle, in particular a motor vehicle, comprising such a system.
[0037] Suitable covers made of dark, pigmented polycarbonate are attractive because they can hide the LiDAR sensor behind them, the parts can be produced by injection molding methods, and polycarbonate also has very good properties, such as high heat deformation resistance, high stiffness and other good properties.
[0038] In this context, a "system" is not only understood as a package (Paket) consisting of mechanically connected individual components in the narrow sense, such as a device, but also more broadly as a simple combination of individual components that are (only) functionally connected to form a unit. The LiDAR sensor can be installed individually in each vehicle and a covering can be provided for the required locations in the vehicle through which the pulses of the LiDAR sensor should be transmitted. However, it can also be a mechanically connected combination.
[0039] "Based on" in connection with a substrate layer means in this context that the composition of the substrate layer comprises the aromatic polymer as a main component, preferably in a respective polymer content of at least 70% by weight, preferably at least 80% by weight, more preferably at least 85% by weight, even more preferably at least 90% by weight, particularly preferably at least 95% by weight, based in each case on the total composition of the substrate layer. The same applies to primer layers in connection with polymethyl methacrylate, which likewise forms the basis for the primer layer, wherein the content of polymethyl methacrylate comprises preferably at least 50% by weight, more preferably at least 60% by weight, particularly preferably at least 65% by weight of polymethyl methacrylate.
[0040] D 90 The value is the particle size below which 90% of the particles are smaller than this value. 50The value is the average particle size. 50% of the particles have a particle size that is smaller than the given value. In the present invention, the following determination methods are suitable for the respective given particle sizes: The determination is carried out by TEM / STEM (scanning transmission electron microscopy) in accordance with DIN SPEC 52407:2015-03, wherein the sample preparation is carried out in the form of thin sections on the paint layer. A gray value image is obtained by the measurement, since the particles have a higher density than the matrix. By gray value analysis, the particles are separated from the matrix using image analysis methods; in this way the size can be determined. The diameter of the particles is determined by image analysis (preferably by analyzing the particle surface; the diameter is determined by means of an area equivalent circle (ECD method; equivalent circle diameter). Statistical analysis, for example d 90 ; Median, arithmetic mean are calculated in random samples. In the present invention, the arithmetic mean of the diameter (D(n)) is always given.
[0041] The "transmittance in the range of 800 nm to 1600 nm" refers to the average transmittance in this range (arithmetic mean) averaged over all wavelengths in this range.
[0042] According to the invention, "covering" or "for covering" means using a covering made of the thermoplastic composition or a covering containing a sub-area made of the thermoplastic composition to be placed in front of the LiDAR sensor to protect it from impacts, dirt, etc. or to cover it "relative to the outside". The purpose of the covering can also be aerodynamic reasons and / or design reasons. Here, the covering body in the present invention can therefore be a housing that completely or almost completely - except for cable ducts, etc. - encloses the LiDAR sensor. In addition to the vehicle's superordinate (übergeordnet) system, this combination of housing and LiDAR sensor is also the subject of the present invention. Of course, all embodiments and configurations described as preferred also apply to this combination alone. However, the covering body can also be the only element placed in front of the LiDAR sensor in the direction of the vehicle shell, preferably as a vehicle shell. Such a covering body is, for example, a front panel or a bumper, preferably a front panel. According to the invention, a front panel is understood to be a body part mounted on the vehicle as part of the shell. This can be a molded component part at the front of the vehicle or a design element mounted at the front of the vehicle. "Front panel" is also understood to be, for example, a substitute for the radiator grille. Due to new forms of mobility For example, an electric, radiator grille consisting of many openings is no longer necessary. The front panel is therefore preferably a closed front cover or a body part which optionally has only individual ventilation slots or contains the appearance of a radiator grille only for design reasons and combines various functions. Such a component can be seamlessly integrated. Here, the cover is an element penetrated by the laser (pulse or continuous wave) of the LiDAR sensor used to detect the environment. The cover of the invention is also a side panel, such as a door element, or a rear panel that can cover optionally required side sensors or sensors installed at the rear.
[0043] The covering body is preferably "composed" of a multilayer body. A "multilayer body" in the context of the present invention is a product having at least a substrate layer and a topcoat layer. The topcoat layer, which has the function of a scratch-resistant layer and / or a weathering protection layer, can itself be a single-layer or multilayer system. In addition, there can also be a primer layer between the topcoat layer and the substrate layer. Particularly preferred covering bodies are composed of a substrate layer and topcoat layers, which can be identical or different, located on one or both sides of the substrate layer, optionally with a primer layer between the substrate layer and the topcoat layer, respectively.
[0044] The covering can be installed not only on motor vehicles but also on other vehicles and mobile means, such as drones, airplanes, helicopters or rail vehicles; according to the invention, these are all encompassed by the term "vehicle".
[0045] A “substrate layer comprising a thermoplastic composition” is to be understood as meaning that the main part of the substrate layer, i.e. the part arranged in front of the LiDAR sensor, i.e. the part covering the LiDAR sensor relative to the vehicle environment, consists of such a thermoplastic composition, i.e. the substrate layer comprises an area consisting of such a thermoplastic composition, wherein this area is arranged in front of the LiDAR sensor. However, the substrate layer may also comprise other sub-areas consisting of other thermoplastic compositions that do not have the features according to the invention. In the case of a front panel, for example, this may be an area with high light transmittance for a headlight cover. Such a cover can in particular be manufactured in a two-component or multi-component injection molding process. The cover may likewise have sub-areas made of different compositions having the features according to the invention. However, it is preferred according to the invention that the substrate layer consists of the thermoplastic composition.
[0046] The topcoat layer can be implemented on one or both sides of the substrate layer. Preferably, at least one topcoat layer is applied on this side of the covering body, wherein this side is defined as on the outside of a vehicle, particularly a motor vehicle, i.e. on the side facing the environment. If the topcoat layer is applied on both sides, different coatings can also be used. For the side facing the outside, a layer that improves media resistance, weather resistance and / or wear resistance is particularly preferred. On the side facing the inside of the multilayer body, a coating can be used in particular to improve dustproof performance, antifogging performance and / or anti-reflection performance.
[0047] “Up to” is inclusive of the recited values. Thus, “up to 20%” also includes “20%” as well as values within the rounded range, such as “20.3%”.
[0048] In the context of the invention, “the substrate layer has a certain transmittance for IR radiation at its respective thickness” means that the IR permeability is determined on the respective molded part in the range of the LiDAR radiation path. The actual permeability of the component to IR radiation in the range of 800 to 1600 nm is taken into account here. The light transmittances specified in the VIS range apply analogously.
[0049] In the present invention, “multilayer” means “at least two layers”, namely a substrate layer and a topcoat layer on the side of the substrate layer opposite the LiDAR sensor, wherein in addition to the topcoat layer, a primer layer can also be present between the topcoat layer and the substrate. However, in particular, further protective or functional layers, in particular a second topcoat layer and an optional primer layer, and functional layers, such as antireflection layers, antifog layers and / or anti-dust layers, can also be present on the side of the multilayer body facing inwards, provided that these layers do not significantly attenuate the signal of the LiDAR sensor.
[0050] According to the invention, a “vehicle” is understood to be any means of transport for goods and / or persons, ie, by land, water or air.
[0051] The thickness of the substrate layer is the thickness of the thickest point of the substrate layer within the range of the LiDAR radiation path.
[0052] The described multilayer body is sufficiently transparent to the laser light of a LiDAR sensor.
[0053] The multilayer body with at least one topcoat layer is preferably such that the topcoat layer and any further layers present, such as a primer layer, do not significantly reduce the transmittance of the cover body for the radiation of the LiDAR sensor. “Not significantly” means that the intensity of the laser IR radiation penetrating the cover body in the range of 800 to 1600 nm, in particular in the range of 880 to 950 nm and / or in the range of 1520 to 1570 nm, is reduced by at most 15%, preferably at most 10%, particularly preferably at most 5%, compared to the same cover body without the topcoat layer. If, in addition to the at least one topcoat layer, further layers are present in addition to the substrate layer, these layers together, preferably together with the topcoat layer, also result in an intensity of the laser IR radiation penetrating the covering body in the range of 800 to 1600 nm, in particular in the range of 880 to 950 nm and / or in the range of 1520 to 1570 nm (determined by DIN ISO 13468-2:2006) compared to an identical covering consisting solely of the substrate layer (i.e. a covering which does not contain any further layers apart from the substrate layer) being reduced by preferably at most 15%, preferably at most 10%, particularly preferably at most 5%.
[0054] There is preferably no object between the LiDAR sensor and the covering that significantly attenuates the signal of the LiDAR sensor. Here, not "significantly" means at most an additional attenuation of up to 5%.
[0055] With regard to other preferred embodiments, the features described elsewhere apply. The present invention also provides for the use of a polysiloxane-based topcoat as a coating layer for a LiDAR sensor cover, the topcoat comprising a combination of an organically modified silane and a silica sol, wherein the topcoat comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Other particles ≥0.50μm.
[0056] The invention also relates to the use of a multilayer body for partially or completely covering a LiDAR sensor which emits laser light having a wavelength in the range of 800 to 1600 nm, in particular 880 to 950 nm and / or 1520 to 1570 nm, the multilayer body comprising
[0057] i) a substrate layer, which preferably has a thickness of 1.0 to 7.0 mm, more preferably 1.0 to 6.0 mm, the substrate layer comprising, preferably consisting of, a thermoplastic composition based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10min), preferably 9 to 19cm 3 / (10min), measured according to ISO1133-1:2012-03 (300°C, 1.2kg),
[0058] wherein the composition has a light transmittance in the range of 380 to 780 nm of less than 25.0%, preferably at most 20%, more preferably less than 15.0%, determined in accordance with DIN ISO 13468-2:2006 (D65, 10°) at a layer thickness of 4 mm, and wherein the substrate layer has a transmittance at its respective thickness for IR radiation in the range of 800 to 1600 nm, in particular 880 to 950 nm and / or 1520 to 1570 nm of at least 40%, preferably at least 65%,
[0059] and
[0060] ii) optionally a primer layer based on polymethyl methacrylate and comprising at least one UV absorber, and
[0061] iii) at least one topcoat layer based on polysiloxane,
[0062] The topcoat layer comprises a combination of an organically modified silane and a silica sol.
[0063] Wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Other particles ≥0.50μm,
[0064] The topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged.
[0065] It will be appreciated that feature variants described as being preferred for the sensor system also apply to the described use or vehicle.
[0066] Preferably, the cover, in particular the substrate layer, has a black color impression. Colored covers are also possible in principle, for example red, green or blue.
[0067] A covering made of the thermoplastic composition or comprising regions made of the thermoplastic composition also exhibits the following positive properties in these regions:
[0068] - Glassy appearance;
[0069] - low weight compared to steel or glass, which is important in order to keep the weight of the vehicle as low as possible;
[0070] - they meet the requirements for the safety of vehicle occupants and other road users, in particular pedestrians, and in this respect in particular exhibit sufficient elasticity and deformability and a low tendency to break;
[0071] - they enable the integration of electrical, electronic, electro-optical and optical functional elements without significantly limiting their functionality in relation to the vehicle and its occupants and to the external environment;
[0072] - they enable the covering of electrical, electronic, electro-optical and optical functional elements without significantly limiting their functionality in relation to the vehicle and its occupants and to the external environment;
[0073] - they can have an attractive design, in particular be designed to be continuous and seamless, and at the same time as far as possible be shaped in two, preferably all three dimensions;
[0074] - they can be produced simply, in particular with as few production steps as possible, wherein in particular all production steps can be carried out together with the integration of at least part of the functional elements in one mold and subsequent mounting and sealing of the functional elements can be omitted;
[0075] They can be post-injected with the thermoplastic composition in the region in front of the LiDAR sensor and also with a further thermoplastic composition in the region not in front of the LiDAR sensor;
[0076] - They can have, at least towards the outside of the vehicle, an attractive surface that is resistant to environmental influences, for example weathering and stone impacts.
[0077] A corresponding covering is also very easy to produce, wherein all production steps can be carried out together with the integration of the functional element in one mold and subsequent mounting and sealing of the functional element can be omitted.
[0078] In addition to LiDAR sensors, other functional elements and devices can also be covered, such as distance sensors as parking aids, motion sensors with which the bonnet can be opened, light strips, headlights, indicator lights, cameras and screens. As mentioned above, the cover as well as the substrate layer can also have transparent areas for this purpose. This solution is also applicable to radar-assisted sensors in principle.
[0079] The covering body is preferably a molded part used in the front or rear area of a vehicle, such as a bumper, a radiator grille, a front panel or a rear panel, in particular a front panel of a motor vehicle, but also a vehicle side part. However, the covering body can also be a roof or a roof module of a motor vehicle. It is particularly preferred that no other elements are present in the radiation path between the covering body and the LiDAR sensor that would impair the operation of the LiDAR sensor.
[0080] The LiDAR sensor used according to the invention emits laser light in the range of 800 to 1600 nm, preferably in the range of 820 to 1600 nm, particularly preferably in the range of 880 to 950 nm and / or 1520 to 1570 nm. Very particularly preferred LiDAR sensors operate at a nominal wavelength of about 905 nm (measured in air) or at a nominal wavelength of about 1550 nm (measured in air).
[0081] The distance from the LiDAR sensor to the cover is preferably ≤300 mm, more preferably ≤200 mm, even more preferably ≤100 mm, and particularly preferably ≤50 mm. The selected distance can be regarded as essentially structure-dependent, since the distance should be selected so that the sensor is adequately protected from impacts. In principle, the LiDAR sensor can also be placed directly on the cover and can optionally be joined thereto, for example glued or screwed.
[0082] Preferably, the positioning of the LiDAR sensor is selected so that the sensor is arranged centrally in the front area or in the rear area of the vehicle. However, the LiDAR sensor can also be arranged in a corner area of the vehicle or offset, for example.
[0083] The substrate layer of the covering described according to the invention in the region of the thermoplastic composition, preferably in the entire region of the substrate layer, preferably has a thickness of 1.0 to 7.0 mm, preferably 1.6 to 6.0 mm, particularly preferably 2.0 to 4.0 mm. Since the thickness of the topcoat layer present according to the invention is in the μm range, as is the thickness of the optionally present primer layer, the total thickness of the covering does not deviate substantially from these values, so that these values can be understood equally well as the total thickness of the covering.
[0084] The weight average molecular weight M of the aromatic polycarbonate selected according to the invention is w Preferably, the weight average molecular weight is 22000 to 29000 g / mol, wherein w In principle, a value of 10,000 to 50,000 g / mol, more preferably 14,000 to 40,000 g / mol, particularly preferably 16,000 to 32,000 g / mol is also suitable. w Determined by gel permeation chromatography, calibrated with bisphenol A polycarbonate standards using dichloromethane as eluent, calibrated with linear polycarbonates (made of bisphenol A and phosgene) with known molar mass distribution from PSS Polymer Standards Service GmbH, Germany, calibrated according to method 2301-0257502-09D (German version 2009) from Currenta GmbH & Co. OHG, Leverkusen. Eluent is dichloromethane. Column combination of crosslinked styrene-divinylbenzene resin. Diameter of the analytical column: 7.5 mm; length: 300 mm. Particle size of the column material: 3 μm to 20 μm. Concentration of the solution: 0.2 wt %. Flow rate: 1.0 ml / min, solution temperature: 30° C. Detection by means of a refractive index (RI) detector.
[0085] The preparation of the polycarbonates is preferably carried out by the interfacial process or the melt transesterification process, which has been described many times in the literature.
[0086] For the phase interface method, reference is made, for example, to H. Schnell, "Chemistry and Physics of Polycarbonates", Polymer Reviews, Vol. 9, Interscience Publishers, New York 1964, p. 33 et seq., to Polymer Reviews, Vol. 10, "Condensation Polymers by Interfacial and Solution Methods", Paul W. Morgan, Interscience Publishers, New York 1965, Chapter VIII, p. 325, to Dres. U. Grigo, K. Kircher and PR-Müller "Polycarbonate", Becker / Braun, Kunststoff-Handbuch, Vol. 3 / 1, Polycarbonate, Polyacetale, Polyester, Celluloseester, Carl Hanser Verlag München, Wien 1992, pp. 118-145, and to EP 0 517 044 A1.
[0087] The melt transesterification process is described, for example, in "Encyclopedia of Polymer Science", Vol. 10 (1969), Chemistry and Physics of Polycarbonates, Polymer Reviews, H. Schnell, Vol. 9, John Wiley and Sons, Inc. (1964) and in patent documents DE 1031512 A and US Pat. No. 6,228,973 B1.
[0088] The polycarbonates are preferably prepared by reaction of bisphenol compounds with carbonic acid compounds, in particular phosgene, or diphenyl carbonate or dimethyl carbonate in the melt transesterification process.
[0089] Particularly preferred here are homopolycarbonates based on bisphenol A and copolycarbonates based on the monomers bisphenol A and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, for example POLYCARBONATE® from Covestro Deutschland AG.
[0090] These and other bisphenol or diol compounds which can be used for the synthesis of polycarbonates are described, inter alia, in WO 2008 / 037364 A1 (page 7, line 21 to page 10, line 5), EP 1582549 A1 (
[0018] to
[0034] ), WO 2002 / 026862 A1 (page 2, line 20 to page 5, line 14) and WO 2005 / 113639 A1 (page 2, line 1 to page 7, line 20).
[0091] The polycarbonates may be linear or branched. Mixtures of branched and unbranched polycarbonates may also be used.
[0092] Suitable branching agents for preparing branched polycarbonates are known in the literature and are described, for example, in US Pat. No. 4,185,009 B and DE 2500092 A1 (3,3-bis(4-hydroxyaryloxindole), in each case see the entire document), DE 4240313 A1 (see page 3, lines 33 to 55), DE 19943642 A1 (see page 5, lines 25 to 34) and US Pat. No. 5,367,044 B and the literature cited therein.
[0093] The polycarbonates used may also be inherently branched, wherein no branching agents are added during the preparation of the polycarbonate. An example of inherent branching is the so-called Fries structure as described for melt polycarbonates in EP 1 506 249 A1.
[0094] Furthermore, chain terminators can be used in the preparation of the polycarbonates. The chain terminators used are preferably phenols, such as phenol, alkylphenols such as cresol and 4-tert-butylphenol, chlorophenol, bromophenol or cumylphenol or mixtures thereof.
[0095] In principle, the composition of the substrate layer can also contain, in addition to aromatic polycarbonates, mixtures, other thermoplastic polymers, i.e. thermoplastic polymers other than aromatic polyester carbonates. Such thermoplastic polymers are polystyrene, styrene copolymers, cyclic polyolefins, poly- or copolymerized polyacrylates and poly- or copolymerized methacrylates such as poly- or copolymerized methyl methacrylate (e.g. PMMA) and copolymers containing styrene such as transparent polystyrene acrylonitrile (PSAN), thermoplastic polyurethanes, polymers based on cyclic olefins (e.g. Commercial products from Ticona Corporation), polycarbonate blends containing olefin copolymers or grafted polymers such as styrene / acrylonitrile copolymers.
[0096] Here, it is only permissible to contain so much further thermoplastic polymer that the transmittance to the laser light of the LiDAR sensor is not seriously disturbed, so that the functionality of the system is no longer present. Preferably, the substrate layer therefore contains less than 5.0% by weight, more preferably less than 1.0% by weight, and very particularly preferably is completely free of further thermoplastic polymers. According to the invention, “less than” means that the individual components may also be completely absent.
[0097] Preferably, according to the present invention,
[0098] The sensor system includes
[0099] a) a LiDAR sensor that emits laser light having a wavelength of 800 to 1600 nm, and
[0100] b) a covering body partially or completely surrounding the LiDAR sensor, the covering body comprising a multilayer body which in turn comprises a substrate layer comprising a thermoplastic composition,
[0101] wherein the composition has a light transmittance in the range of 380 to 780 nm of less than 25.0%, preferably at most 20%, more preferably less than 15.0%, measured according to DIN ISO 13468-2:2006 (D65, 10°) at a layer thickness of 4 mm,
[0102] and wherein the substrate layer has a transmittance of at least 65% at its respective thickness for IR radiation in the range of 880 nm to 950 nm and / or 1520 to 1570 nm, determined in accordance with DIN ISO 13468-2:2006,
[0103] and wherein the thermoplastic composition comprises
[0104] i) at least 70% by weight of an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10min), measured according to ISO 1133-1:2012-03 (300°C, 1.2kg),
[0105] ii) at least one green and / or blue colorant, and
[0106] iii) at least one red and / or violet colorant,
[0107] iv) optionally other colorants,
[0108] and 0 to less than 5.0 wt. % of other thermoplastic polymers,
[0109] and 0 to less than 0.005% carbon black, wherein the sum of the colorants ii) to iv) in the thermoplastic composition is >0.005% by weight, preferably >0.05% by weight, and wherein the thickness of the substrate layer is 1.0 to 7.0 mm, preferably 1.5 to 6.0 mm, more preferably 2 to 5 mm, particularly preferably 2.0 to 5.0 mm,
[0110] and
[0111] At least one polysiloxane-based topcoat layer comprising a combination of an organomodified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles having a diameter of less than 0.50 μm, preferably less than 0.20 μm, more preferably less than 100 nm, particularly preferably less than 50 nm, very particularly preferably less than 30 nm, particularly preferably from 15 to 30 nm and containing no D 90 Other particles ≥0.50μm.
[0112] The composition comprises a green and / or blue colorant (component ii) and a red and / or violet colorant (component iii). Optionally, further colorants (component iv) can be used, with yellow colorants being particularly preferred.
[0113] Therefore, it is preferred to use at least one colorant selected from the group consisting of the colorants of formula (1), (2a-c), (3), (4), (5), (6), (7), (8) (group ii), particularly preferably (1), (2a-c), (3) or (4), and at least one colorant selected from the group consisting of the colorants of formula (9), (10), (11), (12), (13), (14a), (14b), (15) (group iii), preferably selected from the colorants of formula (10), (14a), (14b) or (15). The optional further colorants (group iv) are preferably selected from the colorants of formulae (16) to (20), particularly preferably selected from the colorants of formulae (16) and (17). The colorants to which these formulae relate are described in more detail below.
[0114] Green colorants are particularly preferably colorants of the formulae (1) and (2a / 2b / 2c):
[0115]
[0116]
[0117] The colorant of the formula (1) is known under the name Macrolex Grun 5B from the company Lanxess Deutschland GmbH, color index: 61565, CAS number: 128-90-3, and is an anthraquinone dye.
[0118] The colorants of the formulae (2a), (2b) and (2c) are primarily known under the name Macrolex Grun G (Solvent Green 28).
[0119] The blue colorant used is preferably a colorant of the formula (3) and / or (4a / 4b) and / or (5a / 5b):
[0120]
[0121] It is available under the name "Keyplast Blue KR", CAS No.: 116-75-6,
[0122]
[0123] in
[0124] - Rc and Rd independently of one another represent linear or branched alkyl or halogen, preferably methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl or Cl, more preferably methyl, Cl and particularly preferably Cl,
[0125] -n independently represents a natural number from 0 to 3 for each R, wherein for n=0, the radical is hydrogen.
[0126] In a preferred embodiment, Rc and / or Rd are Cl, and are in the ortho and / or para position relative to the carbon atom bearing the amine functional group, such as di-o-chloronaphtho, di-o-, mono-p-chloronaphtho and mono-o-naphtho. In addition, in a preferred embodiment, Rc and Rd represent tert-butyl, respectively, preferably in the meta position relative to the carbon atom bearing the nitrogen functional group.
[0127] In a particularly preferred embodiment, n=0 in all rings, so that all Rc and Rd=H.
[0128]
[0129] The radicals R(5-20) are each independently hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl, fluorine, chlorine, bromine, sulfone, CN.
[0130] Preferably, R(5-20) is the same at all positions. More preferably, R(5-20) is H at all positions. In an alternative embodiment, R(5-20) is Cl at all positions.
[0131] M is preferably aluminum (R=H: aluminum phthalocyanine, CAS: 14154-42-8), nickel (R=H: nickel phthalocyanine, CAS: 14055-02-8), cobalt (R=H: cobalt phthalocyanine, CAS: 3317-67-7), iron (R=H: iron phthalocyanine, CAS: 132-16-1), zinc (R=H: zinc phthalocyanine, CAS: 14320-04-08), copper (R=H: copper phthalocyanine, CAS: 147-14-8; R=H and Cl: polychlorinated copper phthalocyanine, CAS: 1328-53-6; R=Cl: hexadecanochlorophthalocyanine, CAS: 28888-81-5; R=Br: hexadecanobromophthalocyanine, CAS: 28746-04-5), manganese (R=H: manganese phthalocyanine, CAS: 14325-24-7).
[0132] The combination of M = Cu and R = H for all positions is particularly preferred. For example, compounds of structure (5b) with M = Cu and R(5-20) = H are available from BASF AG, Ludwigshafen as Blau K6911D or Blau K 7104LW was obtained.
[0133] The compound of structure (5a) is available, for example, from BASF AG, Ludwigshafen as Blau L7460 obtained.
[0134] As blue colorants you can also use:
[0135] A colorant of formula (6) available under the name "Macrolex Blue 3R Gran"
[0136]
[0137] and / or a colorant of formula (7) obtainable under the name "Macrolex Blue RR" (CAS 32724-62-2; Solvent Blue 97; CI 615290),
[0138]
[0139] As blue colorants you can also use:
[0140]
[0141] in
[0142] - R1 and R2 independently of one another represent linear or branched alkyl or halogen, preferably methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl or Cl, more preferably methyl, Cl and particularly preferably Cl,
[0143] -n represents a natural number from 0 to 4.
[0144] In a particularly preferred embodiment, n=0 in all rings, such that all R1 and R2=H.
[0145] Such colorants of structure (8) are commercially available from BASF AG in the Paliogen Blau series.
[0146] When using colorants of structure (8), particularly preferred pigments have a bulk volume (determined to DIN ISO 787-11:1995-10) of 2 l / kg to 10 l / kg, preferably 3 l / kg to 8 l / kg, 5 m 2 / g-60m 2 / g, preferably 10m 2 / g-55m 2 / g specific surface area (determined according to DIN 66132:1975-07), and a pH value of 4-9 (determined according to DIN ISO 787-9).
[0147] As red colorant, preference is given to using the colorant of the formula (9), which is available under the name “Macrolex Red 5B”, CAS No. 81-39-0:
[0148]
[0149] Also usable are colorants of formula (10), CAS number 71902-17-5, and colorants of formula (11), CAS number 89106-94-5:
[0150]
[0151] As violet colorants, preference is given to using colorants of the formula (12), which has the CAS number 61951-89-1, colorants of the formula (13), obtainable under the name "Macrolex Violet B" from Lanxess AG, which has the CAS number 81-48-1, or colorants of the formula (14a / 14b):
[0152]
[0153] Wherein R is selected from H and p-methylaniline; preferably, R=H;
[0154]
[0155] in
[0156] - Ra and Rb are independently of one another linear or branched alkyl or halogen, preferably methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl or Cl, more preferably methyl, Cl and particularly preferably Cl,
[0157] -n independently represents a natural number from 0 to 3 for each R, wherein for n=0, the radical is hydrogen.
[0158] In a preferred embodiment, Ra and / or Rb are Cl, and are in the ortho and / or para position relative to the carbon atom bearing the amine functional group, such as di-o-chloronaphtho, di-o-, mono-p-chloronaphtho and mono-o-naphtho. In addition, in a preferred embodiment, Ra and Rb each represent a tert-butyl group, which is preferably in the meta position relative to the carbon atom bearing the nitrogen functional group.
[0159] In a particularly preferred embodiment, n=0 in all rings, so that all Ra and Rb=H.
[0160] It is also possible to use a colorant corresponding to formula (15), which is available under the name "Macrolex Red Violet R", CAS No.: 6404-72-6:
[0161]
[0162] As yellow colorants, preference is given to using colorants of the formula (16), available under the name "Macrolex Gelb 3G", CAS No. 4702-90-3, and / or colorants of the formula (17), available under the name "Macrolex Orange 3G" (CAS No. 6925-69-5, CI 564100):
[0163]
[0164] It is also possible to use a colorant of formula (18), available under the name "Oracet Yellow 180", CAS No.: 13676-91-0; a colorant of formula (19), CAS No. 30125-47-4, and / or a colorant of formula (20), available under the name "Oracet Orange 220; Solvent Orange 116", CAS No.: 669005-94-1.
[0165]
[0166] The group iv) of further colorants preferably contains less than 0.10% by weight of colorants which do not belong to groups ii), iii) or to colorants of structures (16) to (20). Preferably, the group iv) of further colorants consists only of colorants of structures (16) to (20).
[0167] In principle, however, in addition to the abovementioned colorants, further colorants (component iv) may optionally be used in addition. Preference is given to those of the Heliogen Grun type (eg Heliogen Grun K 8730; CAS 1328-53-6; Pigment Green 7; CI 74260).
[0168] Preferably, however, the colorant of the composition of the substrate layer is selected exclusively from colorants of formulae (1) to (20).
[0169] The composition preferably comprises less than 0.005% by weight, more preferably less than 0.001% by weight, of carbon black, and particularly preferably it contains no carbon black.
[0170] Such low transmittance results, for example, in compositions comprising a combination of colorants.
[0171] Macrolex Violett 3R from Lanxess AG (CAS 61951-89-1, solvent violet 36, color index: 61102), anthraquinone dye:
[0172]
[0173] and Macrolex Grün 5B (CAS 128-80-3, Solvent Green 3, Color Index 61565) from Lanxess AG, also an anthraquinone dye:
[0174]
[0175] For example, the two colorants are each present in an amount of 0.1% by weight, based on the entire composition.
[0176] The total concentration of colorants, in particular of the colorants of the formula, is preferably at least 0.13% by weight, more preferably at least 0.15% by weight, particularly preferably at least 0.18% by weight.
[0177] The composition of the substrate layer material should be processable as far as possible at temperatures customary for thermoplastics, ie above 300° C., for example 350° C., without significant changes in the optical properties, such as deep gloss, or mechanical properties occurring during processing.
[0178] The composition forming the region of the substrate layer(s) and based on a thermoplastic polymer, preferably on an aromatic polycarbonate, preferably contains one or more other conventional additives in addition to the colorant. Such additives are described, for example, in EP-A 0839623, WO-A 96 / 15102, EP-A 0500496 or in "Plastics Additives Handbook", Hans Zweifel, 5th edition 2000, Hanser Verlag, München, for example mold release agents, UV absorbers, heat stabilizers, flame retardants, antistatic agents and / or flow improvers.
[0179] It applies here that in principle substances can also be added to the composition which do not significantly impair the functionality of the sensor system.
[0180] The composition particularly preferably contains less than 0.1% by weight of scattering additives, and the composition of the substrate layer very particularly preferably contains no scattering additives, such as those based on acrylates, polyethylene, polypropylene, polystyrene, glass, aluminum oxide and / or silicon dioxide. The composition also particularly preferably contains less than 0.1% by weight and very particularly preferably contains no white pigments or similar pigments, such as titanium dioxide, kaolin, barium sulfate, zinc sulfide, aluminum oxide, aluminum hydroxide, quartz powder, interference pigments and / or pearlescent pigments, i.e. flake-shaped particles, such as mica, graphite, talc, SiO2, chalk and / or titanium dioxide (coated and / or uncoated). The composition also particularly preferably contains less than 0.1% by weight and very particularly preferably contains no nanoparticle systems, such as carbon black, nanotubes, metal particles, metal oxide particles. The composition also preferably contains less than 0.1% by weight and particularly preferably contains no pigments based on insoluble pigments, such as described, for example, in DE 10057165 A1 and WO 2007 / 135032 A2.
[0181] The composition particularly preferably contains a release agent based on fatty acid esters, preferably stearates, particularly preferably on pentaerythritol. Preference is given to using pentaerythritol tetrastearate (PETS) and / or glycerol monostearate (GMS).
[0182] The region for the substrate layer or the composition for the substrate layer optionally further contains a UV absorber. Suitable UV absorbers are compounds having a transmittance as low as possible below 400 nm and a transmittance as high as possible above 400 nm. Such compounds and their preparation are known in the literature and are described, for example, in EP 0839623 A1, WO 1996 / 15102 A2 and EP 0500496 A1. UV absorbers particularly suitable for use in the composition of the invention are benzotriazoles, triazines, benzophenones and / or arylated cyanoacrylates.
[0183] In a particularly preferred embodiment, the composition for the substrate layer contains a UV absorber.
[0184] The following UV absorbers are suitable, for example: hydroxybenzotriazoles, such as 2-(3',5'-bis(1,1-dimethylbenzyl)-2'-hydroxyphenyl)benzotriazole ( 234, BASF AG, Ludwigshafen), 2-(2'-hydroxy-5'-(tert-octyl)phenyl)benzotriazole ( 329, BASF AG, Ludwigshafen), 2-(2'-hydroxy-3'-(2-butyl)-5'-(tert-butyl)phenyl)benzotriazole ( 350, BASF AG, Ludwigshafen), bis(3-(2H-benzotriazolyl)-2-hydroxy-5-tert-octyl)methane ( 360, BASF AG, Ludwigshafen), (2-(4,6-diphenyl-1,3,5-triazine-2-yl)-5-(hexyloxy)phenol ( 1577, BASF AG, Ludwigshafen), benzophenones, 2,4-dihydroxybenzophenone ( 22, BASF AG, Ludwigshafen) or 2-hydroxy-4-(octyloxy)benzophenone ( 81, BASF AG, Ludwigshafen), 2-cyano-3,3-diphenyl-2-propenoic acid, 2,2-bis[[(2-cyano-1-oxo-3,3-diphenyl-2-propenyl)oxy]methyl]-1,3-propanediyl ester (9CI) ( 3030, BASF AG, Ludwigshafen), 2-[2-hydroxy-4-(2-ethylhexyl)oxy]phenyl-4,6-di(4-phenyl)phenyl-1,3,5-triazine (CGX UVA 006, BASF AG, Ludwigshafen) or tetraethyl 2,2'-(1,4-phenylenedimethylene)bismalonate ( B-Cap, Clariant AG). Mixtures of these UV absorbers can also be used.
[0185] More preferably, the thermoplastic composition further comprises at least one further heat stabilizer or processing stabilizer.
[0186] In this context, preference is given to phosphites and phosphonites and to phosphines. Examples are triphenyl phosphite, diphenyl alkyl phosphites, phenyl dialkyl phosphites, tris(nonylphenyl) phosphite, trilauryl phosphite, tri(octadecyl) phosphite, distearyl pentaerythritol diphosphite, tris(2,4-di-tert-butylphenyl) phosphite, diisodecyl pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2,4-dicumylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methyl)-2-nitropropene diphosphite, bis(2,6-di-tert-butyl-4-nitropropene diphosphite) and bis(2,4-dicumylphenyl) pentaerythritol diphosphite. phenyl) pentaerythritol ester, diisodecyl pentaerythritol diphosphite, bis(2,4-di-tert-butyl-6-methylphenyl) pentaerythritol diphosphite, bis(2,4,6-tri(tert-butylphenyl) pentaerythritol diphosphite, tristearyl sorbitol triphosphite, tetrakis(2,4-di-tert-butylphenyl) 4,4'-biphenylene diphosphonite, 6-isooctyloxy-2,4,8,10-tetra-tert-butyl-12H-dibenzo[d,g]-1,3,2-dioxaphosphocyclooctadiene (di oxaphosphocin), bis(2,4-di-tert-butyl-6-methylphenyl)methyl phosphite, bis(2,4-di-tert-butyl-6-methylphenyl)ethyl phosphite, 6-fluoro-2,4,8,10-tetra-tert-butyl-12-methyl-dibenzo[d,g]-1,3,2-dioxaphosphocine, 2,2',2"-nitrilo[triethyltri(3,3',5,5'-tetra-tert-butyl-1,1'-biphenyl-2,2'-diyl)phosphite], 2-ethylhexane 1,2-diphenylphosphine, ... 168 (tris(2,4-di-tert-butyl-phenyl) phosphite) or tris(nonylphenyl) phosphite or mixtures thereof. Alkyl phosphates such as monohexyl phosphate, dihexyl phosphate and trihexyl phosphate, triisooctyl phosphate and trinonyl phosphate can also be used.
[0187] Phenolic antioxidants such as alkylated monophenols, alkylated sulfanylphenols, hydroquinones and alkylated hydroquinones may also be used. 1010 (pentaerythritol-3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate; CAS: 6683-19-8) and / or (2,6-di-tert-butyl-4-(octadecyloxycarbonylethyl)phenol).
[0188] Colorants and other additives can be introduced into the composition, for example, by mixing 2 to 5 wt % of a polycarbonate powder containing colorants and other additives, based on the total composition, with a polycarbonate base material, wherein the polycarbonate in powder form can have a different MVR than the base material. The molecular weight or MVR of the polycarbonate of the composition results from all polycarbonates contained in the composition.
[0189] Since coverings for infrastructure or transport can be relatively large and can have complex geometries, the thermoplastic composition used for the substrate layer should be sufficiently flowable to be able to be processed into corresponding moldings in an injection molding process, in particular, for example, injection-compression molding.
[0190] The multilayer body comprises one or more topcoat layers in addition to the substrate layer. In the present invention, these layers preferably fulfill the function of a scratch-resistant layer and / or a weathering protection layer. The topcoat layer can be applied on one or both sides, but at least on one side of the covering body, wherein this side is defined as the outer side of the covering body installed in a vehicle, in particular a motor vehicle, i.e., the side facing the environment. On the side of the covering body defined as facing the interior of the vehicle, further functional layers, such as anti-fog layers, anti-dust layers and / or anti-reflection layers, may optionally also be present, provided that they do not significantly attenuate the signal of the LiDAR sensor.
[0191] The topcoat layer a located on the side of the substrate layer facing the vehicle environment consists of a scratch-resistant paint (hard coat, topcoat). It is a polysiloxane paint produced by the sol-gel process. The D of the silicon dioxide contained in the topcoat layer determined by scanning transmission electron microscopy is 90 is less than 0.50 μm, preferably less than 0.20 μm, more preferably less than 100 nm, particularly preferably less than 50 nm, very particularly preferably less than 30 nm, and particularly preferably from 15 to 30 nm. Very particularly preferably, the D 100 The topcoat layer does not contain D 90 Particles ≥0.50, i.e. particles of other fillers, etc.
[0192] In this case, “on the side facing the vehicle surroundings” refers to that side of the substrate material which is opposite to the side on which the LiDAR sensor is arranged.
[0193] The topcoat layer located on the side of the substrate layer facing the vehicle environment particularly preferably also comprises at least one UV absorber.The topcoat layer is selected so that it is abrasion-resistant and scratch-resistant.
[0194] Different methods are known to manufacture topcoats on plastic articles. These systems can be applied, for example, by immersion, spin coating, spray coating or flow coating, preferably by immersion or flow coating. Curing can be carried out by heat or by UV radiation. The topcoat can be applied, for example, directly or after preparing the substrate surface with a primer (primer). The topcoat can also be applied by plasma-assisted polymerization methods, in particular by SiO2 plasma. Antifog coatings or antireflective coatings, in particular, coatings to be applied to the side determined to be toward the interior of the vehicle can also be manufactured by plasma methods. It is also possible to apply the topcoat to the resulting molded article by a specific injection molding method, for example, post-injection molding of the surface-treated foil. Various additives can be present in the topcoat, for example, UV absorbers derived from, for example, triazoles, triazines, resorcinols or benzophenones.
[0195] In a preferred embodiment which results in particularly good weathering stability, the covering comprises a polysiloxane-based topcoat layer which has the function of a scratch-resistant layer and / or a weathering protection layer (layer a') and which contains i. at least one UV absorber selected from the group consisting of benzophenones, resorcinols, 2-(2-hydroxyphenyl)benzotriazoles, hydroxyphenyl-s-triazines, 2-cyanoacrylates, oxalanilides
[0196] and / or a UV inhibitor selected from hindered amines (HALS), in particular hindered amines (HALS) based on 2,2,6,6-tetramethylpiperidine or its derivatives; particularly preferably, the topcoat layer comprises a UV absorber based on benzophenone or bis-benzophenone and having silyl side chains,
[0197] ii. at least one combination of an organo-modified silane and a silica sol, wherein the organo-modified silane is preferably a methyltrialkoxysilane or a dimethyldialkoxysilane, wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 ≥ 0.50 μm and optionally, in another preferred embodiment, a further primer layer based on polymethyl methacrylate (layer a") arranged on the substrate layer and serving as adhesion promoter between the topcoat layer based on polysiloxane and the substrate layer, which comprises at least one UV inhibitor selected from the group consisting of benzophenones, resorcinols, 2-(2-hydroxyphenyl)benzotriazoles, hydroxyphenyl-s-triazines, 2-cyanoacrylates, oxalanilides and / or from the group consisting of sterically hindered amines (HALS), in particular based on 2,2,6,6-tetramethylpiperidine or derivatives thereof,
[0198] in
[0199] The thickness of the primer layer is 0.3 μm to 8 μm, preferably 1.0 μm to 4.0 μm.
[0200] The content of UV absorber in the primer layer is up to 35% by weight. With respect to UV absorber, "based on X" means a compound whose structure is derived from the formula X, and optionally has one or more substitutions, ring fusions, etc.
[0201] Particularly preferably, the covering body comprises no further layers besides the substrate layer and one or more topcoat layers and optionally one or more primer layers.
[0202] The primer composition (primer solution) used to form the primer layer here is particularly preferably composed of the following substances:
[0203] a) one or more poly(meth)acrylate binders,
[0204] b) one or more solvents, preferably selected from glycol ethers,
[0205] c) one or more UV absorbers, and
[0206] d) optionally one or more hindered amines (HALS), and
[0207] e) Optional leveling additives. These are additives which serve to achieve better wetting of the substrate (ie the surface to be coated) and / or to improve the surface smoothness. Thus, the leveling additives in the primer layer serve for better wetting of the substrate layer.
[0208] The topcoat layer composition used here particularly preferably consists of:
[0209] a) one or more alkoxysilanes, preferably methyltrimethoxysilane or methyltriethoxysilane,
[0210] b) Silicate sols, preferably with an average particle size D as determined by scanning transmission electron microscopy. 50 less than 50 nm, in particular 15 to 30 nm,
[0211] c) one or more solvents, preferably selected from alcohols and water,
[0212] d) one or more UV absorbers, which are preferably based on benzophenone of structure (I) and / or benzophenone of structure (II) and / or (III) and have silyl side chains
[0213]
[0214]
[0215] Where n = 1 to 10, preferably 2 to 4; R = methyl, ethyl, propyl,
[0216] e) optionally one or more hindered amines (HALS), and
[0217] f) optionally one or more poly(meth)acrylate binders, and
[0218] g) Optional leveling additives.
[0219] According to the invention, "derivatives" are understood to be those compounds whose molecular structure has different atoms or different groups of atoms in place of H atoms or functional groups or in which one or more atoms / groups of atoms have been removed. The parent compound can thus still be identified.
[0220] Preferably, a primer containing a UV absorber is used to improve the adhesion of the scratch-resistant paint on the substrate layer. The primer preferably contains other stabilizers, such as HALS systems (stabilizers based on hindered amines), adhesion promoters and / or flow improvers. The respective resins that form the base material of the primer layer can be selected from a large number of materials and are described, for example, in Ullmann's Encylopedia of Industrial Chemistry, 5th edition, volume A18, pages 368-426, VCH, Weinheim 1991. Polyacrylates, polyurethanes, phenol-based systems, melamine-based systems, epoxy systems and alkyd systems or mixtures of these systems can be used. The resin is usually dissolved in a suitable solvent, usually in an alcohol. Depending on the selected resin, curing can be carried out at room temperature or at elevated temperatures. Preferably, temperatures of 20° C. (room temperature) to 130° C. are used - usually after a short time at room temperature to remove most of the solvent. Commercially available primer systems are, for example, SHP470, SHP470-FT2050 and SHP401 from Momentive Performance Materials. Such coatings are described, for example, in US Pat. No. 6,350,512 B1, US Pat. No. 5,869,185 A, EP 1 308 084 A1 and WO 2006 / 108520 A1.
[0221] The polysiloxane layer preferably contains n SiX 4-n Silicon-organic compounds and / or partial condensates thereof, wherein the R radicals are identical or different and represent linear or branched, saturated or mono- or polyunsaturated or aromatic hydrocarbon radicals, the X radicals are identical or different and represent hydrolyzable radicals or hydroxyl radicals, preferably halogen, in particular chlorine or bromine, alkoxy, alkylcarbonyl or acyloxy radicals, and
[0222] n is 0, 1, 2 or 3, preferably 1 or 2, very particularly preferably 1.
[0223] R preferably represents a saturated, branched or unbranched alkyl radical having 1 to 20 carbon atoms and / or represents a mono- or polyunsaturated branched or unbranched alkenyl radical having 2 to 20 carbon atoms or an aryl radical having 6 to 12 carbon atoms. The alkyl or alkenyl radical more preferably has a maximum of 12, even more preferably a maximum of 8 carbon atoms. Particularly preferably, all radicals are methyl and / or phenyl.
[0224] X particularly preferably denotes alkoxy, very particularly preferably C1- to C4-alkoxy, for example methoxy or ethoxy.
[0225] Silicon Compound R n SiX 4-n The X groups are hydrolyzable and condensable. Through these hydrolyzable and condensable groups, an inorganic network containing Si-O-Si units is constructed. Unlike the X groups, the R groups are stable to hydrolysis under common condensation conditions.
[0226] When using the above-mentioned siloxane-based topcoat systems, dry layer thicknesses of 3 μm to 20 μm are preferred, more preferably 3.5 μm to 15 μm, particularly preferably 4 μm to 12 μm. "Dry layer thickness" is understood to be the layer thickness of the lacquer after application, evaporation of the solvent and subsequent thermal or UV curing. Such layer thicknesses generally apply to the preferred topcoat layers. The layer thickness can be determined, for example, by white light interferometry (for example with the aid of a white light interferometer from Eta Optic; ETA-SST), which is preferred. The thickness can also be determined by material comparison using cross-sectional preparations of the layer and microscopic examinations (by means of AFM or scanning electron microscopy).
[0227] Optionally, if a primer layer is not required, the topcoat layer a' may comprise a poly(meth)acrylate adhesive as an adhesion-promoting component. Commercially available adhesives may be the Joncryl types from BASF.
[0228] As already mentioned above, instead of a primer / topcoat layer combination, it is also possible to use heat-curing or UV-curing one-component hybrid systems for the multilayer body forming the covering.
[0229] Heat-curing systems are primarily hybrid systems and are described, for example, in EP 0570165 A2, WO 2008 / 071363 A2 or DE 2804283 A. Hybrid systems are known, for example, as heat-curing systems and are commercially available. UV-curing systems, as they are currently also used on plastic cover sheets, are commercially available, for example, as UV-curing or heat-curing lacquer systems and are available, for example, from the companies Momentive Performance Materials and Redspot.
[0230] In a particularly preferred method for producing the covering body of the vehicle according to the invention, the topcoat layer and optionally the basecoat layer are applied by means of a flow coating method, since this produces coated components of high optical quality.
[0231] The flow coating method can be carried out manually with a hose or a suitable coating head or automatically in a continuous process with the aid of a flow coating robot nozzle and optionally a slot nozzle. In this case, the components can be coated either while suspended or arranged in appropriate racks. For larger and / or 3D components, i.e. components with three-dimensional surfaces (which therefore also have a different geometry than a sheet material), the components to be coated are suspended or arranged in suitable racks.
[0232] Other possible application methods are immersion, all spraying and injection methods, knife coating, roller coating or spin coating, preferably spraying and injection, for example with an injection gun, in a flat spraying device or by means of a high-speed rotating bell. In this case, the components can be suspended or placed in corresponding racks for coating.
[0233] Small parts can also be coated manually. Here, the liquid primer or lacquer solution to be coated for forming the protective layer is poured longitudinally over the sheet starting from the upper edge of the small part, with the starting point of the lacquer on the sheet extending from left to right across the width of the sheet. The painted sheets are dried and cured while hanging vertically in a fixture according to the respective manufacturer's instructions.
[0234] It has been found, completely surprisingly, that organic coating systems are less suitable for devices comprising LiDAR sensors. This includes, for example, UV-crosslinkable systems, such as urethane acrylates, with and without inorganic nanoparticles.
[0235] Particularly preferred is
[0236] Sensor systems and mainly in particular vehicles, which include
[0237] a) a LiDAR sensor emitting laser light having a wavelength in the range of 800 to 1600 nm, in particular 880 to 950 nm and / or 1520 to 1570 nm, and
[0238] b) a covering body partially or completely surrounding the LiDAR sensor, the covering body comprising a multilayer body, the multilayer body comprising in turn a substrate layer comprising a thermoplastic composition based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10 min), measured according to ISO 1133-1:2012-03 (300° C., 1.2 kg), wherein the light transmittance of the substrate layer in the range of 380 to 780 nm is less than 25.0%, preferably at most 20%, more preferably less than 15%, measured according to DIN ISO 13468-2:2006 (D65, 10°) at a layer thickness of 4 mm,
[0239] and wherein the substrate layer has a transmittance of at least 55%, preferably at least 60%, particularly preferably at least 65%, at its respective thickness, for IR radiation in the range of 800 to 1600 nm, in particular in the range of 880 to 950 nm and / or in the range of 1520 to 1570 nm, determined in accordance with DIN ISO 13468-2:2006,
[0240] and wherein the thermoplastic composition consists of:
[0241] i) at least 85% by weight, more preferably at least 95% by weight, of aromatic polycarbonate,
[0242] ii) at least one green and / or blue colorant selected from the colorants of formula (1), (2a-c), (3), (4a), (4b), (5), (6), (7) and / or (8), and
[0243] iii) at least one red and / or violet colorant selected from the colorants of formula (9), (10), (11), (12), (13), (14a), (14b) and / or (15),
[0244] iv) optionally further colorants, which are preferably selected from the colorants of formula (16), (17), (18), (19) and / or (20),
[0245] v) optionally heat stabilizers, mold release agents, UV absorbers, flame retardants, antistatic agents and / or flow improvers, preferably in an amount of 0 to 10% by weight, more preferably 0 to 3% by weight,
[0246] vi) 0 to less than 5.0% by weight of other thermoplastic polymers,
[0247] vii) 0 to less than 0.005 wt. % carbon black, wherein the sum of colorants ii) to iv) is > 0.001 wt. %, more preferably > 0.005 wt. %, even more preferably > 0.008 wt. %,
[0248] and wherein the substrate layer has a thickness of 1.0 to 6.0 mm, preferably 2 to 4 mm, more preferably 2.0 to 4.0 mm, an optional primer layer based on polymethyl methacrylate and comprising at least one UV absorber,
[0249] and
[0250] A polysiloxane-based topcoat layer comprising a combination of an organically modified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Particles ≥ 0.50 μm,
[0251] The topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged.
[0252] Very particularly preferably
[0253] Sensor systems, especially vehicles, include
[0254] a) a LiDAR sensor emitting laser light having a wavelength in the range of 800 to 1600 nm, in particular 880 to 950 nm and / or 1520 to 1570 nm, and
[0255] b) a covering body partially or completely surrounding the LiDAR sensor, the covering body comprising, preferably consisting of, a multilayer body, the multilayer body in turn comprising
[0256] - a substrate layer based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10 min), determined according to ISO 1133-1:2012-03 (300° C., 1.2 kg), a light transmittance in the range of 380 to 780 nm of less than 1.0%, determined according to DIN ISO 13468-2:2006 (D65, 10°) at a layer thickness of 4 mm, and a transmittance for IR radiation in the range of 800 to 1600 nm, in particular in the range of 880 to 950 nm and / or in the range of 1520 to 1570 nm of at least 60%, particularly preferably at least 65%, determined according to DIN ISO 13468-2:2006,
[0257] The thermoplastic composition is composed of the following substances:
[0258] i) at least 85% by weight, more preferably at least 95% by weight, of aromatic polycarbonate,
[0259] ii) at least one green and / or blue colorant selected from the colorants of formula (1), (2a-c), (3), (4a), (4b), (5), (6), (7) and / or (8), and
[0260] iii) at least one red and / or violet colorant selected from the colorants of formula (9), (10), (11), (12), (13), (14a), (14b) and / or (15),
[0261] iv) optionally further colorants, which are preferably selected from the colorants of formula (16), (17), (18), (19) and / or (20),
[0262] v) optionally heat stabilizers, mold release agents, UV absorbers, flame retardants, antistatic agents and / or flow improvers, preferably in an amount of 0 to 3% by weight,
[0263] vi) 0 to less than 5.0% by weight of other thermoplastic polymers,
[0264] vii) 0 to less than 0.005% by weight of carbon black,
[0265] The sum of the colorants ii) to iv) is >0.001 wt. %, more preferably >0.005 wt. %, even more preferably >0.008 wt. %,
[0266] and wherein the thickness of the substrate layer is 1.0 to 6.0 mm, preferably 2 to 4 mm, more preferably 2.0 to 4.0 mm, and
[0267] - an optional primer layer based on polymethyl methacrylate and comprising at least one UV absorber, and - a topcoat layer based on polysiloxanes, comprising a combination of an organomodified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles smaller than 50 nm, preferably smaller than 30 nm and do not contain D 90 Particles ≥ 0.50 μm,
[0268] The topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged, and the topcoat layer particularly preferably contains at least one UV absorber, preferably at least one UV absorber embedded in a siloxane network. The UV absorber embedded in the siloxane network contains alkoxysilane groups, which can be hydrolyzed in the siloxane lacquer (sol-gel system used) and chemically bonded to the siloxane network during curing.
[0269] On the side of the covering body intended to face the vehicle interior, a protective layer may be applied to improve the media resistance, ie, a protective layer having dustproof, anti-fog and / or anti-reflection properties.
[0270] Non-limiting examples of anti-fog and anti-dust coatings are particle-free MODIPER H5000 or MODIPER H9800-UV from NOF Corporation, GXC AFPC (polycarbonate) or a layer obtained by flame siliconization.
[0271] Suitable antireflection layers are all single-layer or multi-layer layer structures which have as outer layers a low-refractive-index layer (n D <1.5). By using the above-described composition based on aromatic polycarbonate for the substrate layer and the scratch-resistant layer provided according to the invention, a covering for LiDAR sensors is provided, with which, on the one hand, a wide variety of electrical, electronic, electro-optical and optical functional elements can be covered without significantly restricting their functions in relation to the vehicle and its occupants and the external environment (so that the functions are no longer performed as intended), and on the other hand, an attractive coloring in the human visible spectrum, in particular a glass-like black impression, can be achieved.
[0272] The substrate layer and the sheet layer of three-dimensional molding made by the above-mentioned polymer composition containing the above-mentioned components are carried out by merging, mixing and homogenizing by a common incorporation method, wherein homogenization is particularly preferably carried out in the melt under the action of shearing force. For this reason, thermoplastic polymers, preferably aromatic polycarbonates, and polymer molding compounds, preferably optional other components of polycarbonate molding compounds are mixed, extruded and granulated in the melt under normal conditions in a conventional melt mixing device, for example in a single screw or multi-screw extruder or kneader. Additives can be separately metered in with particles or pellets via a metering balance or a side feeder, or metered in a suitable position at an elevated temperature in the form of a melt by means of a metering pump in the solid conveying zone of the extruder or in the polymer melt. The masterbatch in the form of particles or pellets can also be combined with other granular compounds to provide a premix, which is then supplied to the solid conveying zone of the extruder or in the polymer melt in the extruder via a metering hopper or a side feeder together. The compounding device is preferably a twin-screw extruder, particularly preferably a twin-screw extruder with co-rotating screws, wherein the twin-screw extruder preferably has a screw length-diameter ratio of 20 to 44, particularly preferably 28 to 40. Such a twin-screw extruder comprises a melting zone and a mixing zone, or a combined melting and mixing zone, and optionally a degassing zone, in which an absolute pressure p of preferably up to 800 mbar, more preferably up to 500 mbar, particularly preferably up to 200 mbar is established. The average residence time of the mixture composition in the extruder is preferably limited to a maximum of 120 seconds, particularly preferably to a maximum of 80 seconds, particularly preferably to a maximum of 60 seconds. In a preferred embodiment, the temperature of the melt of the polymer or polymer alloy at the extruder outlet is 200° C. to 400° C.
[0273] In addition to extrusion, the composition for the substrate layer can be converted into the substrate layer by hot pressing, spinning, blow molding, deep drawing or injection molding. Injection molding or injection compression molding is preferred.
[0274] Injection molding is known to the person skilled in the art and is described, for example, in "Handbuch Spritzgieβen", Friedrich Johannaber / Walter Michaeli, München; Wien: Hanser, 2001, ISBN 3-446-15632-1 or "Anleitung zum Bau von Spritzgieβwerkzeugen", Menges / Michaeli / Mohren, München; Wien: Hanser, 1999, ISBN 3-446-21258-2.
[0275] Injection molding here includes all injection molding methods, including multi-component injection molding and injection-compression molding methods.
[0276] The difference between the injection compression molding method and the conventional injection molding method is that the injection molding and / or solidification process is carried out while the template is moving. In the known injection molding method, the template is slightly opened before the injection molding process to compensate for the shrinkage that occurs during the subsequent solidification process and to reduce the required injection pressure. Therefore, a pre-expanded cavity already exists at the beginning of the injection molding process. The overflow surface (Tauchkante) of the mold ensures that the pre-expanded cavity is leak-proof enough even when the template is slightly opened. The plastic material is injected into this pre-expanded cavity and compressed at the same time or subsequently when the mold moves toward the closed position. In particular, in the manufacture of large-area and thin-walled molded parts with long flow paths, more complex injection compression molding technology is preferred or, as required, mandatory. Only in this way can the reduction of the injection pressure required for large molded parts be achieved. In addition, stress or warping in the injection molded parts caused by high injection pressure can be avoided by injection compression molding.
[0277] The covering is preferably integrated into the vehicle body via the non-infrared transparent region. "Non-infrared transparent" is understood here to mean that the transmittance in the non-infrared transparent region at its respective thickness in the range of 800 to 1600 nm, in particular 880 nm to 950 nm and / or 1520 to 1570 nm is less than 65%, as determined according to DIN ISO 13468-2:2006. They are opaque layers, preferably made of polymer blends, more preferably made of polycarbonate blends, preferably containing polycarbonate as the main component present, very particularly preferably containing ABS (acrylonitrile-butadiene-styrene) or polyester as a blending partner. Such an opaque layer is in direct contact with the above-mentioned layer structure made of substrate layer and optionally present protective layer over a large area.
[0278] When the non-infrared transparent material is molded onto the covering body used according to the invention, the transition point of the material is preferably in the edge region to cover possible unevenness. In each case, there is a region where the substrate layer is located on the non-infrared transparent layer or the non-infrared transparent layer is located on the substrate layer. "Located on..." is understood here to mean that the layers overlap when the covering body is viewed perpendicular to the joining plane of the layers. It will be appreciated that the non-infrared transparent layer does not need to be in direct contact with the substrate layer, but can only be in direct contact with the substrate layer, because it can be arranged behind a further layer.
[0279] These non-infrared transparent materials serve in particular as reinforced frame parts.For the production of reinforced frame parts, thermoplastics containing fillers and / or reinforcing agents are preferably used.
[0280] The fillers and / or reinforcing agents used are generally fibers, flakes, tubes, rods or spheres or spheres or particles. Suitable fillers and reinforcing agents include, for example, talc, wollastonite, mica, kaolin, diatomaceous earth, calcium sulfate, calcium carbonate, barium sulfate, glass fibers, glass or ceramic balls, hollow glass or hollow ceramic balls, glass wool or mineral wool, carbon fibers or carbon nanotubes. Preferably, the filler is a filler that causes the isotropic shrinkage behavior of the composition.
[0281] Particular preference is given to using talc and short glass fibers.
[0282] Glass or ceramic spheres or hollow spheres can hereby increase the scratch resistance of this surface.
[0283] In the part of the substrate layer which is not arranged in front of the LiDAR sensor, i.e. does not cover the LiDAR sensor towards the environment, the substrate layer may also contain a material containing fillers and reinforcing agents. The content thereof is preferably 5% to 40% by weight, preferably 7% to 30% by weight, more preferably 8% to 25% by weight, wherein the weight data are based on the total composition of the substrate layer.
[0284] The covering, which comprises or consists of an opaque substrate layer, optionally with one or more primer layers and one or more topcoat layers, can be applied to any support system made of metal or plastic in vehicle construction. This can be achieved with the aid of special adhesive systems, for example based on polyurethane. The combination of LiDAR sensor and covering can be installed in the vehicle as a whole; however, LiDAR sensor and covering can also be installed separately. Preferably, the LiDAR sensor is installed first and the covering, in particular the front panel, is subsequently placed in front of the LiDAR sensor.
[0285] In the present invention, the preferred embodiments mentioned for the individual features may also be combined with each other as long as they are not contradictory.
[0286] Attached photos
[0287] Figure 1 A front panel is shown as an example of the cover of the present invention.
[0288] Figure 2 The experimental setup used in the Examples section is shown. Example
[0289] Hereinafter, the present invention is explained in detail with reference to specific examples.
[0290] Substrate material 1: for comparative example
[0291] Contains 99.99984% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 / 10 min and based on bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG. The composition also contained 0.00006 wt % Macrolex Violett 3R (colorant of formula (12)) and 0.0001 wt % Macrolex Blau RR (colorant of formula (7)).
[0292] Substrate material 2: for comparative example
[0293] Contains 99.8% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition having an MVR of 100 Å / 10 min and based on bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG. The composition also contained 0.1 wt. % of Solvent Blue 36 (further colorant) and 0.1 wt. % of Macrolex Grun G (colorant of formula (2)).
[0294] Substrate material 3: for comparative example
[0295] Contains 99.8000 wt. % of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition of a polycarbonate having an MVR of 10 min / 10 min and based on bisphenol A and phenol-terminated polycarbonate from Covestro Deutschland AG. The polycarbonate contained 0.134 wt. % of Solvent Blue 36 (another colorant), 0.044 wt. % of Macrolex Orange 3G (colorant of formula (17)) and 0.022 wt. % of Amaplast Yellow GHS (Solvent Yellow 163, colorant of formula (18)).
[0296] Substrate material 4: for comparative example
[0297] Contains 99.84% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 / (10 min) and is based on a composition of bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG. The material contains 0.16% by weight of carbon black.
[0298] Substrate material 5: for comparative example
[0299] Contains 93.195850 wt. % of a carbon steel having a thickness of about 18 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 / (10 min) and based on bisphenol A and a polycarbonate terminated with tert-butylphenol from Covestro Deutschland AG. The composition further contains 6.756 wt. % of Kronos 2230 (titanium dioxide), 0.00006 wt. % of Macrolex Gelb 3G (colorant of formula (16)), 0.00009 wt. % of Macrolex Violett 3R (colorant of formula (12)) and 0.054 wt. % of Tinopal (2,5-thienylbis(5-tert-butyl-1,3-benzoxazole); fluorescent whitening agent).
[0300] Substrate material 6: for comparative example
[0301] Contains 99.435% by weight of a polyol having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition having an MVR of 10 min and based on bisphenol A and a polycarbonate terminated with phenol from Covestro Deutschland AG. The polycarbonate contains 0.1% of Kronos 2230 (titanium dioxide), 0.03% of Sicotan Gelb K2107 (Pigment Brown 24, CAS 68186-90-3; other colorants), 0.022% of Heucodur Blau 2R from Heubach (Pigment Blue 28, cobalt-aluminate-blue spinel, CAS 1345-16-0; other colorants), 0.35% of Macrolex Rot EG (colorant of formula (10)) and 0.063% of Bayferrox 110M from Lanxess AG (Fe2O3; CAS 001309-37-1).
[0302] Substrate material 7: for comparative example
[0303] Polycarbonate / ABS blend from Covestro Deutschland AG having a hardness (according to ISO 1133-1:2012-03) of about 17 cm at 260° C. under a load of 5.0 kg. 3 / 10min MVR and has an ABS content of about 30 wt% and a SAN content of about 10 wt%. The material does not contain a colorant.
[0304] Substrate material 8: for comparative example
[0305] Contains 99.96% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition of an MVR of 1.5 % to 1.5 % of bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG. The composition contained 0.04% by weight of carbon black.
[0306] Substrate material 9: for comparative example
[0307] Contains 99.78% by weight of a polyol having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3A composition having an MVR of 10 min / 10 min and based on bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG. The composition contained 0.02% by weight of carbon black and 0.2% by weight of Macrolex Violet B (colorant of formula (13)).
[0308] Substrate material 10: used in embodiments of the present invention
[0309] Contains 99.874% by weight of a carbon steel having a diameter of about 18 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 / 10min and based on bisphenol A and a polycarbonate terminated with tert-butylphenol from Covestro Deutschland AG. The composition also contains 0.048 wt. % Macrolex Orange 3G (colorant of formula (17)), 0.01 wt. % Macrolex Violet B (colorant of formula (13)) and 0.068 wt. % of a colorant of formula (4a / 4b, 1:1).
[0310] Substrate material 11: used in embodiments of the present invention
[0311] Contains 99.8% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition having an MVR of 10 min and based on bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG and containing 0.1% by weight of Macrolex Violet 3R (colorant of formula (12)) and 0.1% by weight of Macrolex Grun 5B (colorant of formula (1)).
[0312] Substrate material 12: used in embodiments of the present invention
[0313] Contains 99.894% by weight of a carbon steel having a thickness of about 12 cm measured at 300° C. under a load of 1.2 kg (according to ISO 1133-1:2012-03). 3 A composition having an MVR of 10 min and based on bisphenol A and a phenol-terminated polycarbonate from Covestro Deutschland AG and containing 0.0360 wt. % Macrolex Blau RR (colorant of formula (7)) and 0.07 wt. % Macrolex Violet 3R (colorant of formula (12)).
[0314] Substrate material 13: for comparative example
[0315] Injection-molded, colorant-free and carbon black-free sheet made of polyamide 6,6 with a thickness of 3.0 mm.
[0316] Substrate material 14: for comparative example
[0317] Polyethersulfone from Solvay Solexis Inc. in the form of a 0.175 mm thick Ajedium film.
[0318] Substrate material 15: for comparative example
[0319] Siloxane-containing block cocondensates based on bisphenol A-containing polycarbonates having a siloxane content of 5% and prepared as described in EP 3 099 731 A1.
[0320] Substrate Material 16: A plate made of Altuglass brand polymethyl methacrylate (Arkema) for comparative example.
[0321] Test methods
[0322] Determination of solids content (method A for silicone paints and primers):
[0323] The solids content of the paint is determined using a Mettler Toledo HB43 solids tester, wherein a weighed sample of the paint is evaporated at 140° C. until a constant mass is reached. The solids content is then given as a percentage of the quotient of the mass after evaporation and the mass before evaporation. In the simplest case, the solids content of the paint after the paint has cured is the paint weight minus the weight of the solvent.
[0324] Determination of solid content (method B for UV paint systems):
[0325] The solids content of the paint is determined with the aid of a Mettler Toledo HB43 solids tester, wherein a weighed sample of the paint is evaporated at 110° C. until a constant mass is reached. The solids content is then given as a percentage of the quotient of the mass after evaporation and the mass before evaporation. In the simplest case, the solids content of the paint after the paint has cured is the paint weight minus the weight of the solvent.
[0326] Multilayer body 1: Comparative example
[0327] The multilayer body 1 is made of a substrate material 11 and has a topcoat layer comprising silicon dioxide particles with a particle size of 4 μm (Amosil FW600; calcined silicon dioxide Amosil FW 600 from Quarzwerke GmbH, Frechen, average particle size of about 4 μm, D 600 measured according to a Cilas particle sizer). 10 / D90 The ratio is about 1.5 / 10 [μm / μm]; ISO13320:2009 (particle measurement by laser scattering) and the specific surface area is about 6m 2 / g, determined according to DIN ISO 9277 (DIN-ISO 9277:2014-01)).
[0328] Preparation of paint:
[0329] In a flask equipped with a stirrer and a condenser, 27.5 g of methyltrimethoxysilane were mixed with 0.2 g of concentrated acetic acid.
[0330] In another container, 5.0 g of Joncryl 587 was dissolved in a mixture of 6.0 g each of isopropanol and n-butanol. Using a dissolver, 6.8 g of Amosil FW 600 was high shear dispersed for 30 minutes, after which 15.7 g of deionized water was added.
[0331] The previously prepared Joncryl 587 / Amosil FW 600 dispersion was slowly added to the acidified methyltrimethoxysilane with stirring.
[0332] The batch was diluted with 15.5 g each of isopropanol and n-butanol, and 0.1 g of tetra-n-butylammonium acetate (TBAA) was added.
[0333] The solids of the sol-gel lacquer were adjusted to a value of 1:1 using a solvent mixture of isopropanol and n-butanol. For silicon Method A for Oxygen Alkane Paints and Primers The solids content was measured to be 25%.
[0334] Solids: 25%
[0335] pH: 6.0
[0336] The topcoat layer was applied manually by means of a flow coating method. To form the protective layer, starting from the upper edge of a polycarbonate plate made of substrate 11 with dimensions of 250 mm x 105 mm x 3.2 mm, the paint was poured onto the plate in the length direction, while simultaneously guiding the starting point of the paint on the plate from left to right across the width of the plate.
[0337] The painted panels were hung vertically on a fixture and, after a drying period of 30 minutes at 23°C, were subsequently cured at 130°C for 60 minutes.
[0338] Multilayer body 2: Comparative example
[0339] The multilayer body is made of a substrate material 11 and has a topcoat layer, which contains particles of size D 90Silica particles with an average particle size of 1.2 μm (Amosil FW960-943 from Quarzwerke GmbH, Frechen, with an average particle size of 1.2 μm and a specific surface area of about 14 m 2 / g, determined according to DIN ISO 9277 (DIN-ISO 9277:2014-01)).
[0340] Preparation of the varnish: The preparation of the varnish was carried out as for the multi-layer body 1 , but in the present example Amosil FW 960-943 was used.
[0341] The solids of the sol-gel lacquer were adjusted to a value of 1:1 using a solvent mixture of isopropanol and n-butanol. For silicon Method A for Oxygen Alkane Paints and Primers The solids content was measured to be 25%.
[0342] Solids: 25%
[0343] pH: 5.5
[0344] As with the multi-layer body 1 , the lacquer was applied to a polycarbonate sheet made of the substrate 11 with dimensions of 250×105×3.2 mm.
[0345] Multilayer body 3: Embodiment of the present invention
[0346] The multilayer body is made of a substrate material 11 and has a topcoat layer containing silicon dioxide particles with a particle size of about 22 nm (Ludox AS-40 silicon dioxide, colloidal, specific surface area 140 m 2 / g; WR Grace & Co.-Conn. Maryland 21044 USA).
[0347] Preparation of paint:
[0348] In a flask equipped with stirring and a cooler, 27.5 g of methyltrimethoxysilane were mixed with 0.2 g of concentrated acetic acid.
[0349] In another container, 17 g of Ludox AS-40 (silica sol from Grace Corporation) was mixed with 5.5 g of deionized water.
[0350] The diluted silica sol was added to the acidified methyltrimethoxysilane under stirring and the stirring was continued at room temperature for 4 hours. After 4 hours, 1.7 g of concentrated acetic acid was added. In order to initiate the hydrolysis-condensation reaction, the mixture was stirred for another 3 hours at room temperature.
[0351] 21.5 g of isopropanol and n-butanol and 0.1 g of tetra-n-butylammonium acetate (TBAA) were added to the mixture under stirring at room temperature. 5.0 g of Joncryl 587 was then dissolved in the mixture.
[0352] The solids of the sol-gel lacquer were adjusted to a value of 1:1 using a solvent mixture of isopropanol and n-butanol. For silicon Method A for Oxygen Alkane Paints and Primers The solids content was measured to be 25%.
[0353] Solids: 25%
[0354] pH: 5.0
[0355] As for the multilayer body 1 , the lacquer was applied to a polycarbonate sheet made of the substrate 11 with dimensions of 250 mm×105 mm×3.2 mm.
[0356] Multilayer body 4: Embodiment of the present invention
[0357] A commercially available primer solution was used, which had a solids content of 10.5% (Method A). The primer was based on polymethyl methacrylate and glycol ether and contained 1-methoxy-2-propanol and diacetone alcohol as solvents and dibenzoylresorcinol as UV absorber.
[0358] In order to be within the manufacturer's layer thickness specifications, the paint needs to be diluted with a solvent mixture of diacetone alcohol and 1-methoxy-2-propanol (1:1). For this purpose, a solution of Tinuvin 479 (hydroxyphenyl triazine-UV absorber) in methoxy-2-propanol / diacetone alcohol (1:1) is added to the above primer, resulting in a primer solution containing 5.00% by weight of Tinuvin 479 and a solids content of 5.9%. The paint is subsequently filtered through a pressure filter (2-4 μm cellulose filter).
[0359] Preparation of hard coating solution (for topcoat layer):
[0360] A topcoat solution is used which contains Ludox AS particles with a particle diameter of about 22 nm. The solid content is about 20% by weight and the UV absorber content is about 11% by weight. As UV absorber, a UV absorber of structure (III) (wherein n=3) is used. The preparation method of the topcoat solution is described in US 5,041,313 A.
[0361] To 24.5 g of this solution was added 0.88 g of glacial acetic acid (100% acetic acid) under stirring to obtain a hard coating solution with 3.5 wt% acetic acid addition based on the total amount of paint.
[0362] The application is carried out manually. To form the layer, starting from the upper edge of the small part, the liquid primer solution is poured in the length direction onto a polycarbonate plate made of substrate 11 with dimensions of 250 mm x 105 mm x 3.2 mm, while at the same time guiding the starting point of the paint on the plate from left to right over the width of the plate. The painted plate is suspended vertically on a fixture and, after a drying time of 30 minutes at 23° C., is subsequently cured at 130° C. for 60 minutes. After the application of the primer layer, a topcoat (scratch-resistant layer) is applied as a topcoat layer in a similar manner and, after drying at 23° C. for 30 minutes, is cured at 130° C. for 60 minutes.
[0363] Multilayer body 5: according to the invention
[0364] The multilayer body 5 corresponds to the multilayer body 4 , with the only difference being that the substrate layer thickness given below is 4 mm instead of 3.2 mm.
[0365] The preparation and application of the primer and topcoat material are carried out as described for the multi-layer body 4 .
[0366] Multilayer body 6: Multilayer body according to the invention made of substrate material 11 corresponds to multilayer body 3, differing only in the changed substrate layer thickness (4 mm) instead of 3.2 mm. The lacquer was prepared and applied as described for example multilayer body 3.
[0367] Multilayer body 7: Comparative example Multilayer body made from substrate material 11 and UV-curing urethane acrylate lacquer system.
[0368] 100 g of Desmolux VP LS2308 (ALLNEX, unsaturated aliphatic urethane acrylate), 61.0 g of Ebecryl 8301 (Cytec, hexafunctional aliphatic urethane acrylate), 4.86 g of Irgacure 814 (BASF), 1.62 g of BYK 306 (BYK), 3.78 g of Hostavin 3206 LIQ (Clariant), 1.70 g of A coating solution consisting of 3058 LIQ (Clariant), 160 g of methoxypropanol and 160 g of diacetone alcohol was applied by flow coating to one side of a plate made of substrate 11 with dimensions of 10.5 cm×15 cm×0.4 cm.
[0369] The coating was done manually. Starting from the upper edge of the small part, the coating solution was poured onto the board in the length direction while guiding the starting point of the primer on the board from left to right across the width of the board. After an evaporation time of 5 minutes, the board was pre-cured at 75°C for 6 minutes. A mercury-doped UV lamp (80 W / cm2) was then used to cure the board at 75°C for 6 minutes. 2 UV curing is performed at a dosage of .
[0370] Compounding
[0371] The components were compounded in the amounts given in the examples in a twin-screw extruder of the KraussMaffei Berstorff ZE25 type at a barrel temperature of 260° C. or a material temperature of about 280° C. and a rotation speed of 100 rpm to produce a composition for the substrate layer. The color composition was processed into injection-molded rectangular polycarbonate plates with a thickness of 5 mm, 4 mm or 3.2 mm.
[0372] Pretreatment / cleaning of panels before coating
[0373] The coating was carried out in a controlled atmosphere coating room at 23 to 25° C. and 40 to 48% relative humidity in accordance with the respective specifications of the paint manufacturer.
[0374] Use so-called iso-wipes (LymTech Scientific The sample plate was cleaned with 70% isopropanol and 30% deionized water saturated), rinsed with isopropanol, dried in air for 30 minutes, and purged with ionized air.
[0375] LiDAR sensor used
[0376] A Velodyne Ty Puck VLP 16 LiDAR sensor was used. The sensor operates within a wavelength range (tolerance range) of 895 to 915 nm. The nominal wavelength of the 16 lasers, i.e., the actual operating wavelength, is 903 nm.
[0377] The basic features of this sensor include:
[0378] Vertical detection angle -15° to +15°, spacing 2° between scanning planes; horizontal detection angle 360°. The software includes a multi-beam function with 16 beams to minimize shadowing effects. The horizontal resolution of the laser system is 0.1° to 0.4°, depending on the rotation speed. The rotation speed for vertical detection is adjustable between 5 and 20 Hz. At a data rate of 2 Mbytes / second, 300,000 points / second are detected. The achieved measurement accuracy is here approximately + / -3 cm, which corresponds to 1σ. The detectable measuring distance is between 1 mm and 100 meters. The energy requirement of the sensor system is 8 Watts of electrical power, which corresponds to 0.7 A at 12 V. The overall dimensions of the sensor are: diameter 100 mm and height 65 mm.
[0379] Measurement method
[0380] To reduce the scattered light signal, the sensor head of the LiDAR sensor was shielded on the side away from the measurement path. Only lasers 1, 3, 5, 7, 8, 10, 12 and 14 were used. In addition, the field of view (FOV) of the sensor in the sensor interface was limited to 20° (350°-10°). The reflective surface was a smooth white surface coated with a colorant containing TiO2. The distance between the wall and the LiDAR sensor was 2.5m.
[0381] The sample was tested with a sample holder parallel to the LiDAR sensor, with the back of the sample about 15 mm in front of the LiDAR sensor, so that both the output signal and the returning input signal had to pass through the wall thickness of the test plate. Analysis was performed using the "VeloView" software from Velodyne, the manufacturer of the LiDAR sensor. The average value of the measured intensity of the sample was determined. This sample average was divided by the average value of the reference measurement (air) to determine the relative intensity.
[0382] The measured intensity of the re-recorded laser signal is 0% to 100%. The lower the attenuation (weakening) of the signal, that is, the higher the intensity of the measured signal, the more suitable the cover is for LiDAR auxiliary sensor applications in the automotive field. The transmittance of each plate to IR radiation in the range of 800nm to 1600nm is determined according to DIN ISO 13468-2:2006. The light transmittance in the VIS region of the spectrum (380 to 780nm, transmittance Ty) is determined according to DIN ISO13468-2:2006 (D65, 10°, layer thickness of the sample plate: 4mm). The transmittance measurement is performed using a Lambda 950 spectrophotometer from Perkin Elmer with a photometer ball.
[0383] Wear test:
[0384] The wear test was carried out using the car wash test format according to DIN ISO 15082:2017-06.
[0385] Ten double cleanings were performed with a stirred suspension of quartz powder in water (1.5 g of quartz powder per liter of water).
[0386] MVR:
[0387] The melt volume flow rate (MVR) was determined using a Zwick 4106 instrument from Zwick Roell in accordance with ISO 1133:2012-03 (at a test temperature of 300° C., a mass of 1.2 kg). In addition, the MVR was measured after a preheating time of 5, 20 and 30 minutes. This is a measure of the melt stability under elevated thermal stress.
[0388] result
[0389] Table 1: Measurement results of light transmittance Ty (D65, 10°) (VIS) of substrate layer and LiDAR sensor suitability
[0390]
[0391] It is clear from Table 1 that only certain substrate materials are suitable. Even very thin layer thicknesses of unsuitable materials, such as polypropylene, attenuate the sensor signal so severely that intensities are no longer measurable in the measurement configuration. It is also surprising that different substrates such as polyamide (Example 16) and ABS (Example 17) show no permeability to the LiDAR sensor in this measurement configuration. All these thermoplastics are transparent or at least translucent in the infrared range at the relevant layer thicknesses. Surprisingly, completely amorphous polymers such as polyethersulfone and polyester also show high attenuation to the LiDAR sensor.
[0392] Even modified polycarbonates, such as siloxane-containing polycarbonates, are not suitable for combination with LiDAR sensors.
[0393] It is also completely surprising that combinations of colorants soluble in a polycarbonate matrix also lead in some cases to high attenuation of the LiDAR signal (Examples 2 and 3). In contrast, the inventive combination of colorants in a thermoplastic matrix based on bisphenol A polycarbonate can be combined with LiDAR sensors in a suitable manner.
[0394] In addition, the melt volume flow rate of several compositions was measured at 300°C and 320°C under a load of 1.2 kg at certain time intervals according to ISO 1133-1:2011 (Table 2). It can be seen that the substrate materials 2 and 3 of the comparative examples are significantly more unstable than the substrate material 11 of the invention.
[0395] Table 2: MVR of substrate materials 2, 3 and 11
[0396]
[0397] Table 3: Measurement results of LiDAR sensor suitability of protective layers
[0398]
[0399] The results were analyzed by calculation.
[0400] Table 4: Transmission of multilayer bodies in the IR range
[0401]
[0402] * corresponds essentially to the thickness of the substrate layer.
[0403] For the tests of multilayer bodies, substrate materials were selected which showed high permeability to the LiDAR signal in the tests. Different multilayer bodies were tested and investigated, the combinations of which showed high permeability. It can be seen that the particle size of the particles used, in particular in order to achieve good scratch resistance, influences the attenuation of the LiDAR signal. High scratch resistance is important for reducing the effects of weathering. It can be seen that only certain particle sizes in combination with suitable substrate materials are suitable for LiDAR sensors.
[0404] Table 5: Attenuation of LiDAR signal before wear test
[0405]
[0406] Table 6: Attenuation of LiDAR signal after wear test
[0407]
[0408] The multilayer body according to the invention still had a minimum signal of 65% after the abrasion test.
[0409] Table 7: Transmission of multilayer bodies in the IR range
[0410]
[0411] *The values in brackets indicate the results before the car wash line test.
[0412] It was found completely surprisingly that organic paint systems, especially those without nanoparticles, showed greater attenuation for LiDAR sensors after a car wash test according to DIN ISO 15082:2017-06.
Claims
1. A sensor system comprising a) a LiDAR sensor that emits laser light having a wavelength of 800 to 1600 nm, and b) a covering body partially or completely surrounding the LiDAR sensor, the covering body being used to be penetrated by the laser, the covering body comprising a multi-layer body, the multi-layer body in turn comprising i) a substrate layer comprising a thermoplastic composition based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10min), measured according to ISO 1133-1:2012-03 at 300°C and 1.2kg load, wherein the composition has a light transmittance in the range of 380 to 780 nm of less than 25.0%, measured according to DIN ISO 13468-2:2006 at D65 and 10° at a layer thickness of 4 mm, and wherein the substrate layer has a transmittance of at least 40% at its respective thickness for IR radiation in the range from 800 nm to 1600 nm, determined in accordance with DIN ISO 13468-2:2006, The thermoplastic composition of the substrate layer comprises the following components: i) at least 70% by weight of aromatic polycarbonate, ii) at least one green and / or blue colorant, and iii) at least one red and / or violet colorant, iv) optionally other colorants, wherein the sum of the colorants ii) to iv) is at least 0.05% by weight, and The at least one colorant of group ii) is a colorant selected from the following: colorants of formula (1), (2a-c), (3), (4a), (4b), (5), (6), (7) and / or (8) in Rc and Rd independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 3 independently for each R, wherein the radicals R5 to R20 independently of one another represent hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl, fluorine, chlorine, bromine, sulfone, CN, and M is aluminum, nickel, cobalt, iron, zinc, copper or manganese, in R1 and R2 independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 4, and at least one colorant of group iii) is a colorant selected from the group consisting of: colorants of formula (9), (10), (11), (12), (13), (14a), (14b) and / or (15), wherein R is selected from H and p-methylanilino, in Ra and Rb independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 3 independently for each R, and The colorant of group iv) is selected from the yellow and orange colorants of formula (16), (17), (18), (19) and / or (20) and wherein the composition comprises no further colorants than the colorants of groups ii) to iv), v) optionally one or more additives selected from heat stabilizers, mold release agents, UV absorbers, flame retardants, antistatic agents and / or flow improvers, vi) 0 to less than 5.0 wt. % of other thermoplastic polymers, and vii) 0 to less than 0.005 wt. % carbon black, and The thickness of the substrate layer is 1.0 to 6.0 mm. and ii) optionally a primer layer based on polymethyl methacrylate and comprising at least one UV absorber, iii) a polysiloxane-based topcoat layer comprising a combination of an organically modified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Other particles ≥0.50μm, The topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged.
2. The sensor system according to claim 1, wherein the topcoat layer comprises at least one UV absorber selected from the group consisting of benzophenones, resorcinols, 2-(2-hydroxyphenyl)benzotriazoles, hydroxyphenyl-s-triazines, 2-cyanoacrylates and / or oxalanilides. 3 . The sensor system according to claim 1 , wherein the organomodified silane is at least one methyltrialkoxysilane, at least one dimethyldialkoxysilane or a mixture thereof.
4. A sensor system according to claim 1 or 2, wherein the multilayer body comprises one or more primer layers with a thickness of 0.3 μm to 8 μm, each of which contains at least one UV absorber selected from benzophenones, resorcinols, 2-(2-hydroxyphenyl)benzotriazoles, hydroxyphenyl-s-triazines, 2-cyanoacrylates, oxalic acid anilides and / or hindered amines (HALS). 5 . The sensor system according to claim 1 , wherein the covering comprises no further layers besides the substrate layer i, one or more topcoat layers iii and optionally one or more primer layers ii. 6 . The sensor system according to claim 1 , wherein only air or elements which do not impair the functionality of the LiDAR sensor are present between the LiDAR sensor and the covering. 7 . The sensor system according to claim 1 , wherein the topcoat layer contains no further particles besides the silicon dioxide particles.
8. The sensor system according to claim 1 or 2, wherein the D of the silica particles measured by scanning transmission electron microscopy is 90 Less than 50nm. 9 . The sensor system according to claim 1 , wherein the multilayer body comprises a topcoat layer iii) and optionally a primer layer ii) on both sides of the substrate layer.
10. The sensor system according to claim 1 or 2, wherein the covering body is a front panel, a rear panel, a bumper, a radiator grille, a roof, a roof module or a vehicle side part.
11. The sensor system according to claim 1 or 2, wherein the sum of colorants ii) to iv) in the thermoplastic composition of the substrate layer is at least 0.10% by weight, And wherein the thermoplastic composition does not contain other thermoplastics. 12 . The sensor system according to claim 1 , wherein the composition of the substrate layer comprises no further components besides components i-iii) and optionally one or more of components iv) to vii).
13. Vehicle comprising a sensor system according to one of claims 1 to 12.
14. Use of a polysiloxane-based topcoat as a coating layer for a LiDAR sensor cover, the cover being intended to be penetrated by the laser of the LiDAR sensor, the topcoat comprising a combination of an organically modified silane and a silica sol, wherein the topcoat comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 ≥0.50μm other particles, the covering body comprises a multilayer body, the multilayer body in turn comprises i) a substrate layer comprising a thermoplastic composition based on an aromatic polycarbonate having a melt volume flow rate MVR of 8 to 20 cm 3 / (10min), measured according to ISO 1133-1:2012-03 at 300°C and 1.2kg load, wherein the composition has a light transmittance in the range of 380 to 780 nm of less than 25.0%, measured according to DIN ISO 13468-2:2006 at D65 and 10° at a layer thickness of 4 mm, and wherein the substrate layer has a transmittance of at least 40% at its respective thickness for IR radiation in the range from 800 nm to 1600 nm, determined in accordance with DIN ISO 13468-2:2006, The thermoplastic composition of the substrate layer comprises the following components: i) at least 70% by weight of aromatic polycarbonate, ii) at least one green and / or blue colorant, and iii) at least one red and / or violet colorant, iv) optionally other colorants, wherein the sum of the colorants ii) to iv) is at least 0.05% by weight, and The at least one colorant of group ii) is a colorant selected from the following: colorants of formula (1), (2a-c), (3), (4a), (4b), (5), (6), (7) and / or (8) in Rc and Rd independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 3 independently for each R, wherein the radicals R5 to R20 independently of one another represent hydrogen, methyl, ethyl, propyl, isopropyl, butyl, isobutyl, tert-butyl, pentyl, neopentyl, hexyl, 1,1,2-trimethylpropyl, fluorine, chlorine, bromine, sulfone, CN, and M is aluminum, nickel, cobalt, iron, zinc, copper or manganese, in R1 and R2 independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 4, and at least one colorant of group iii) is a colorant selected from the group consisting of: colorants of formula (9), (10), (11), (12), (13), (14a), (14b) and / or (15), wherein R is selected from H and p-methylanilino, in Ra and Rb independently represent a linear or branched alkyl group or a halogen group, n represents a natural number from 0 to 3 independently for each R, and The colorant of group iv) is selected from the yellow and orange colorants of formula (16), (17), (18), (19) and / or (20) and wherein the composition comprises no further colorants than the colorants of groups ii) to iv), v) optionally one or more additives selected from heat stabilizers, mold release agents, UV absorbers, flame retardants, antistatic agents and / or flow improvers, vi) 0 to less than 5.0 wt. % of other thermoplastic polymers, and vii) 0 to less than 0.005 wt. % carbon black, and The thickness of the substrate layer is 1.0 to 6.0 mm. and ii) optionally a primer layer based on polymethyl methacrylate and comprising at least one UV absorber, iii) a polysiloxane-based topcoat layer comprising a combination of an organically modified silane and a silica sol, wherein the topcoat layer comprises a D 90 Silica particles smaller than 0.50 μm and do not contain D 90 Other particles ≥0.50μm, The topcoat layer is on the side of the substrate layer opposite to the side of the substrate layer on which the LiDAR sensor is arranged.