A three-dimensional vibration test sensor based on additive manufacturing technology and preparation method

The three-way vibration test sensor prepared through additive manufacturing technology solves the complexity of traditional sensor materials and processes, achieves high sensitivity and adaptability, is suitable for micro vibration detection in harsh environments, and ensures rapid and Low cost production.

CN111504443BActive Publication Date: 2024-11-01JILIN UNIVERSITY
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202010527260.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-11
Publication Date
2024-11-01
Estimated Expiration
2040-06-11

AI Technical Summary

Technical Problem

Traditional vibration sensors have shortcomings in material selection, production process complexity, insufficient structural stiffness and low sensitivity. It is difficult to effectively detect small vibrations in harsh environments, and it is difficult to meet the growing demand for sensitivity and stability.

Method used

Using a three-way vibration test sensor based on additive manufacturing technology, a new piezoelectric ceramic material and flexible packaging cover are prepared through 3D printing technology, combining lever structure and vibration-conducting liquid to realize the sensor manufacturing of customized structures and composite materials, which enhances the sensor Sensitivity and adaptability.

Benefits of technology

It realizes fast and low-cost sensor production, improves the sensitivity and structural performance consistency of micro vibration detection, is suitable for harsh environments, and improves information utilization and sensor interaction through wireless data transmission and visualization technology.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111504443B_ABST
    Figure CN111504443B_ABST
Patent Text Reader

Abstract

A three-dimensional vibration test sensor based on additive manufacturing technology and a preparation method thereof belong to the field of detection technology. The center hole of the cylinder in the vibration test assembly of the three-dimensional vibration test sensor based on additive manufacturing technology of the present invention is fixedly connected to the center rod of the base, and the lower end of the sensor housing is fixedly connected to the middle plate in the base; the data input end of the vibration signal acquisition card in the information management module is communicatively connected with the data transmission interface of each sensing component in the vibration test assembly, and the vibration-conducting liquid is used as the vibration conduction medium, and the piezoelectric layer and the packaging body are manufactured by additive manufacturing technology. The present invention can continuously conduct vibration waves, and the piezoelectric layer has high conductivity and sensitivity, which optimizes and improves the quality and quantity of the collected vibration signals, and the manufacturing process is simple and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of detection technology, and specifically relates to a three-dimensional vibration test sensor based on additive manufacturing technology and a preparation method thereof. Background Art

[0002] Vibration measurement sensor is an important branch of a wide variety of sensors. Its function is to quantitatively convert the vibration displacement, vibration velocity and vibration acceleration caused by vibration into electrical signals, record them and feedback them to the user. Due to the limitations of the development of materials science and electronic metrology technology, common vibration sensors now include fiber grating vibration sensors, piezoelectric vibration sensors and capacitive vibration sensors. Most of these sensors are made of traditional metal materials and semiconductor materials, and there are some obvious shortcomings, such as: complex manufacturing process, insufficient structure, high rigidity and hardness but insufficient flexibility, inability to effectively detect tiny vibrations, and difficulty in application in harsh environments. Therefore, the sensitivity, stability and other performance of the sensor cannot meet people's growing needs.

[0003] Traditional piezoelectric ceramic sensors mostly use single lead zirconate titanate as a pressure-sensitive element. With the development of new materials, some composite materials with excellent performance have gradually emerged. Piezoelectric ceramic composite materials incorporating metal ions have attracted the attention of a large number of Chinese and foreign researchers and have developed rapidly in the field of sensor preparation. Metallic conductive materials such as Al, Zn, At and Ag have been tried as sensors. The high-quality proportion of metal materials enables the sensor to obtain better conductivity and sensitivity. Flexible sensors prepared from polymers and flexible substrates are becoming more and more widely used.

[0004] There are some common shortcomings in the preparation methods of traditional sensors, such as the complicated preparation process and backward preparation technology. Especially for the preparation of sensors for flexible composite materials, it is difficult to achieve uniform molding of composite materials. Additive manufacturing technology is based on digital model files and uses adhesive materials such as powdered metals, plastics and composite materials to construct objects by printing layer by layer. The technology has the advantages of being fast and simple, with high molding accuracy, no by-products, and capable of manufacturing various structural products. It has important applications in mold manufacturing, industrial design, construction engineering, and the medical industry. Applying additive manufacturing technology to the manufacturing process of sensors has made the preparation of customized structure sensors and composite material sensors a reality. Summary of the invention

[0005] The purpose of the present invention is to provide a three-axis vibration test sensor and a preparation method based on additive manufacturing technology to overcome the shortcomings of traditional vibration test sensors.

[0006] The three-way vibration test sensor based on additive manufacturing technology of the present invention is composed of a base A, a vibration test component B, a sensor housing C and a data management module D, wherein the base A is composed of a chassis 1, a middle plate 2 and a center rod 3, and the chassis 1, the middle plate 2 and the center rod 3 are arranged in sequence from bottom to top and fixedly connected; the center hole 6 of the cylinder 13 in the vibration test component B is fixedly connected to the center rod 3 of the base A, and the lower end of the sensor housing C is fixedly connected to the upper surface of the middle plate 2 in the base A; the data input end of the vibration signal acquisition card 35 in the data management module D is communicatively connected to the data transmission interface 21 of the sensing component I4, the sensing component III8, the sensing component II10, the sensing component IV11, the sensing component V15 and the sensing component VI17 in the vibration test component B.

[0007] The vibration test assembly B is composed of a sensing assembly I4, a cantilever beam I5, a cantilever beam III7, a sensing assembly III8, a cantilever beam II9, a sensing assembly II10, a sensing assembly IV11, a cantilever beam IV12, a cylinder 13, a cantilever beam V14, a sensing assembly V15, a cantilever beam VI16 and a sensing assembly VI17, wherein the cylinder 13 is provided with a center hole 6; the inner end of the cantilever beam I5 is fixedly connected to the upper left end of the cylinder 13, and the sensing assembly I4 is fixedly connected to the upper near outer end of the cantilever beam I5; the inner end of the cantilever beam II9 is ​​fixedly connected to the upper right end of the cylinder 13, and the sensing assembly Component II10 is fixedly connected to the lower side of the outer end of cantilever beam II9; the inner end of cantilever beam III7 is fixedly connected to the lower end of the front side of the cylinder 13, and the sensing component III8 is fixedly connected to the upper side of the outer end of cantilever beam III7; the inner end of cantilever beam IV12 is fixedly connected to the lower right end of the cylinder 13, and the sensing component IV11 is fixedly connected to the upper side of the outer end of cantilever beam IV12; the inner end of cantilever beam V14 is fixedly connected to the lower rear end of the cylinder 13, and the sensing component V15 is fixedly connected to the upper side of the outer end of cantilever beam V14; the inner end of cantilever beam VI16 is fixedly connected to the lower left end of the cylinder 13, and the sensing component VI17 is fixedly connected to the upper side of the outer end of cantilever beam VI16.

[0008] The sensing components Ⅰ4, Ⅲ8, Ⅱ10, Ⅳ11, Ⅴ15 and Ⅵ17 have the same structure, and are all composed of a liquid tank 18, a vibration-guided liquid 20, a data transmission interface 21, a copper wire 22 and a piezoelectric piece 23. The top surface of the liquid tank 18 is provided with an infusion port 19; the vibration-guided liquid 20 is placed in the liquid tank 18, the piezoelectric piece 23 is embedded in the center of the bottom surface of the liquid tank 18, and the data transmission interface 21 is connected to the piezoelectric piece 23 via the copper wire 22.

[0009] The piezoelectric sheet 23 is composed of an interdigitated electrode I24, a conductive silver paste I25, a substrate 26, a piezoelectric layer 27, a packaging cover 28, an electrode layer 29, a conductive silver paste II30 and an interdigitated electrode II31. A hole I32 is provided on the left side of the packaging cover 28, and a hole II33 is provided on the right side of the packaging cover 28; the substrate 26, the piezoelectric layer 27 and the electrode layer 29 are arranged in sequence from bottom to top and fixedly connected, and the packaging cover 28 is fixedly connected to the substrate 26; the conductive silver paste II30 is fixedly connected to the left side of the electrode layer 29, the right end of the interdigitated electrode II31 is fixedly connected to the conductive silver paste II30 through the hole I32 of the packaging cover 28, the conductive silver paste I25 is fixedly connected to the right side of the electrode layer 29, and the left end of the interdigitated electrode I24 is fixedly connected to the conductive silver paste I25 through the hole II33 of the packaging cover 28.

[0010] The data management module D is composed of a power management unit 34, a vibration signal acquisition card 35, a vibration signal processing unit 36, a wireless transmission unit 37 and a signal display unit 38; the vibration signal processing unit 36 ​​is communicatively connected to the vibration signal acquisition card 35, the wireless transmission unit 37 is communicatively connected to the vibration signal processing unit 36 ​​and the signal display unit 38, and data transmission is performed by wireless communication; the signal display unit 38 is communicatively connected to the vibration signal acquisition card 35, and visually displays the detection data processed by the vibration signal acquisition card 35; the power management unit 34 is powered by a 3.7V lithium battery, and is connected to the vibration signal acquisition card 35, the vibration signal processing unit 36 ​​and the wireless transmission unit 37 using a MicroUSB interface.

[0011] The method for preparing the three-dimensional vibration test sensor based on additive manufacturing technology of the present invention includes a method for preparing the piezoelectric layer 27, a method for preparing the electrode layer 29 and a method for preparing the packaging cover 28:

[0012] 1.1 The method for preparing the piezoelectric layer 27 comprises the following steps:

[0013] The piezoelectric layer 27 material described in 1.1.1 is a new type of piezoelectric ceramic material compounded by 3D printing technology, wherein the mass ratio of lead zirconate titanate, graphite, zinc oxide and copper hydroxide is 100:20:10:10, and is printed by SLS 3D printing technology;

[0014] 1.1.2 At room temperature, lead zirconate titanate solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:1.5, ball-milled for 12 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form a suspension A;

[0015] 1.1.3 At room temperature, graphite solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:0.5, ball-milled for 8 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form suspension B;

[0016] 1.1.4 After mixing suspension A and suspension B, add 70% alcohol solution by mass, and disperse by ultrasonic to mix the solutions evenly to obtain a mixed solution with a certain mass fraction. Place the mixed solution in an 85℃ constant temperature oven and dry for 12 hours to obtain mixed solid powder particles, which are then passed through a 200 sieve;

[0017] 1.1.5 Grind zinc oxide and copper hydroxide solid particles at room temperature, use trisodium citrate dihydrate as dispersant and anhydrous ethanol as grinding aid, and then ball mill for 8 hours. Then, place the mixed solution in a 60℃ constant temperature oven and dry for 12 hours to obtain mixed solid powder particles, which are passed through a 200-sieve, wherein the mass ratio of lead zirconate titanate: zinc oxide: copper hydroxide: citric acid dihydrate is 100:10:15:5;

[0018] 1.1.6 Mix the powders obtained in step 3 and step 4, add 10% polyvinyl alcohol sol, use ionized water as solvent, stir and disperse with ultrasonic aid to obtain suspension C;

[0019] 1.1.7 Add 2g of silica sol to suspension C, shake evenly until the silica sol is completely dissolved in the suspension, then dry and remove the solvent to obtain a powdered piezoelectric mixed material to obtain a new type of piezoelectric ceramic material;

[0020] 1.1.8 Use SLS 3D printing technology to print the piezoelectric layer of the sensing component with a specific structure; smooth the surface of the processed piezoelectric layer, and then place the piezoelectric layer in a cleaning solution and an ethanol solution in turn for ultrasonic cleaning for 10 minutes each, remove the piezoelectric layer, dry it at low temperature, and cool it to room temperature;

[0021] 1.1.9 The piezoelectric layer is polarized by oil bath polarization. The polarization medium is dimethyl thermal conductive silicone oil. The polarization temperature is 50-80℃, the polarization voltage is 40-60KV / mm, and the duration is 1-2 hours. After the polarization is completed, the film is naturally cooled to room temperature under the condition of constant polarization voltage, and the surface of the piezoelectric layer is cleaned again with ethanol solution;

[0022] 1.2 The preparation method of the electrode layer 29 comprises the following steps:

[0023] 1.2.1 The electrode layer 29 is composed of conductive silver paste, interdigitated electrodes and lead-out copper wires 22;

[0024] 1.2.2 Scrub the piezoelectric layer 27 material in an ionic aqueous solution and dry it in alcohol vapor;

[0025] 1.2.3 Using silicon dioxide as a target material and applying magnetron sputtering technology, a silicon dioxide film is deposited on the piezoelectric layer 27 material;

[0026] 1.2.4 Indium tin oxide is selected as the main material of the interdigital electrode I 24 and the interdigital electrode II 31, and indium tin oxide is sputtered on silicon dioxide using magnetron sputtering technology;

[0027] 1.2.5 Ag is used as the main material of the conductive silver paste I 25 and the conductive silver paste II 30, and the conductive silver paste I 25 and the conductive silver paste II 30 are used to lead out the copper wire 22 at both ends of the interdigital electrode I 24 and the interdigital electrode II 31 respectively;

[0028] 1.2.6 Use anhydrous ethanol to clean the remaining conductive silver paste I25 and conductive silver paste II30;

[0029] 1.3 The method for preparing the packaging cover 28 comprises the following steps:

[0030] 1.3.1 The production process of the packaging cover 28 is as follows: E51 epoxy resin with an epoxy value of 0.38-0.42 is used as a substrate, graphene and styrene thermoplastic elastomer are used as fillers, the surface is covered with a polyethylene film with a thickness of 0.5 mm, phenolic amine is used as a curing agent, and acetone solution is used as a diluent, wherein the mass ratio of E51 epoxy resin, graphene, styrene thermoplastic elastomer and phenolic amine is 5:1:1:0.1;

[0031] 1.3.2 Mix E51 epoxy resin and phenolic amine in a mass ratio of 5:0.1, heat in a heating furnace at 70°C for 30 minutes, and take out;

[0032] 1.3.3 Rapidly add acetone to the mixture of E51 epoxy resin and phenolic amine, and stir rapidly, while slowly adding graphene and styrene thermoplastic elastomer filler. After the mixture is stirred evenly, place it in a vacuum dryer for vacuum treatment to obtain an encapsulation layer mixture;

[0033] 1.3.4 The encapsulation mixture is cut into pieces and mixed with a chlorinated polyethylene thermoplastic elastomer, and then extruded into a filament having isolated double percolation micro-nodes at a temperature of 180 degrees Celsius using a single screw extruder;

[0034] 1.3.5 Use fused deposition modeling 3D printing technology to print the packaging layer structure, clean it and cool it to room temperature, and then apply the polyethylene film on it by pressing.

[0035] The beneficial effects of the present invention are:

[0036] Compared with traditional molding technology, additive manufacturing technology enables the production process of the customized structure acceleration sensor to be realized and meet the requirements, and can ensure fast and low-cost production during large-scale production. The production time of each sensor is short, the use of raw materials is streamlined, and products produced in different batches can ensure consistent structural performance.

[0037] The metal ion filler used in the present invention makes the piezoelectric layer have higher conductivity and sensitivity, and is more sensitive to small effects. The raw materials used in the production are widely available. The sensor made of polymer encapsulation cover and flexible substrate has the advantages of light weight, softness, and easy processing. The environmentally friendly material will not cause adverse reactions in the human body when in contact with the human body. Compared with sensors made of traditional metal materials or semiconductor materials, the prepared flexible sensor has a wider range of applications, exhibits better working performance in harsh environments, and is easy to carry.

[0038] The three-dimensional acceleration sensor designed and customized by the present invention can structurally amplify the tiny vibration of the device under test into a larger vibration amplitude through the lever effect, and uses a vibration-conducting liquid as a vibration transmission medium, which can continuously transmit vibration waves, so that the sensor can continuously convert force signals into electrical signals for continuous output.

[0039] The vibration signal collection and processing method of the present invention can effectively improve the utilization rate of information, optimize and improve the quality and quantity of the collected vibration signals, and provide a mechanism for determining whether there is any sensor working abnormality and abnormal alarm working mechanism, and effectively display the signals collected by the sensor through computer visualization technology, with good interactivity. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Schematic diagram of the structure of a three-axis vibration test sensor based on additive manufacturing technology

[0041] Figure 2 Schematic diagram of the structure of base A and vibration test component B

[0042] Figure 3 The structural diagram of base A

[0043] Figure 4 Schematic diagram of the structure of vibration test component B

[0044] Figure 5 Schematic diagram of the structure of the sensing component

[0045] Figure 6 Schematic diagram of the structure of the piezoelectric sheet 23

[0046] Figure 7 is a cross-sectional view of the packaging cover 28

[0047] Figure 8 A top view of the piezoelectric layer 27 and the electrode layer 29

[0048] Fig. 9 Schematic diagram of the structure of the interdigitated electrode Ⅰ24

[0049] Fig.10 Schematic diagram of the structure of data management module D

[0050] Fig.11 The manufacturing flow chart of the piezoelectric layer 27 is as follows:

[0051] Fig.12 A flowchart of the production of the packaging cover 28

[0052] Among them: A. Base B. Vibration test component C. Sensor housing D. Data management module 1. Chassis 2. Middle plate 3. Center rod 4. Sensing component I 5. Cantilever beam I 6. Center hole 7. Cantilever beam III 8. Sensing component III 9. Cantilever beam II 10. Sensing component II 11. Sensing component IV 12. Cantilever beam IV 13. Cylinder 14. Cantilever beam V 15. Sensing component V 16. Cantilever beam VI 17. Sensing component VI 18. Liquid tank 19. Infusion port 20. Vibration-guiding liquid 21. Data transmission interface 22. Copper wire 23. Piezoelectric sheet 24. Interdigitated electrode I 25. Conductive silver paste I 26. Substrate 27. Piezoelectric layer 28. Package cover 29. Electrode layer 30. Conductive silver paste II 31. Interdigitated electrode II 32. Hole I 33. Hole II 34. Power management unit 35. Vibration signal acquisition card 36. Vibration signal processing unit 37. Wireless transmission unit 38. Signal display unit DETAILED DESCRIPTION

[0053] like Figures 1 to 3 As shown, the three-way vibration test sensor based on additive manufacturing technology of the present invention is composed of a base A, a vibration test component B, a sensor housing C and a data management module D, wherein the base A is composed of a chassis 1, a middle plate 2 and a center rod 3, and the chassis 1, the middle plate 2 and the center rod 3 are arranged in sequence from bottom to top and fixedly connected; the center hole 6 of the cylinder 13 in the vibration test component B is fixedly connected to the center rod 3 of the base A, and the lower end of the sensor housing C is fixedly connected to the upper surface of the middle plate 2 in the base A; the data input end of the vibration signal acquisition card 35 in the data management module D is communicatively connected to the data transmission interface 21 of the sensing component I4, the sensing component III8, the sensing component II10, the sensing component IV11, the sensing component V15 and the sensing component VI17 in the vibration test component B.

[0054] like Figure 4As shown, the vibration test assembly B is composed of a sensing assembly I4, a cantilever beam I5, a cantilever beam III7, a sensing assembly III8, a cantilever beam II9, a sensing assembly II10, a sensing assembly IV11, a cantilever beam IV12, a cylinder 13, a cantilever beam V14, a sensing assembly V15, a cantilever beam VI16 and a sensing assembly VI17, wherein the cylinder 13 is provided with a center hole 6; the inner end of the cantilever beam I5 is fixedly connected to the upper left end of the cylinder 13, and the sensing assembly I4 is fixedly connected to the upper near outer end of the cantilever beam I5; the inner end of the cantilever beam II9 is ​​fixedly connected to the upper right end of the cylinder 13, and the sensing assembly Component II10 is fixedly connected to the lower side of the outer end of cantilever beam II9; the inner end of cantilever beam III7 is fixedly connected to the lower end of the front side of the cylinder 13, and the sensing component III8 is fixedly connected to the upper side of the outer end of cantilever beam III7; the inner end of cantilever beam IV12 is fixedly connected to the lower end of the right side of the cylinder 13, and the sensing component IV11 is fixedly connected to the upper side of the outer end of cantilever beam IV12; the inner end of cantilever beam V14 is fixedly connected to the lower end of the rear side of the cylinder 13, and the sensing component V15 is fixedly connected to the upper side of the outer end of cantilever beam V14; the inner end of cantilever beam VI16 is fixedly connected to the lower end of the left side of the cylinder 13, and the sensing component VI17 is fixedly connected to the upper side of the outer end of cantilever beam VI16.

[0055] like Figure 5 As shown, the sensing components Ⅰ4, Ⅲ8, Ⅱ10, Ⅳ11, Ⅴ15 and Ⅵ17 have the same structure, and are all composed of a liquid tank 18, a vibration-guiding liquid 20, a data transmission interface 21, a copper wire 22 and a piezoelectric piece 23. The top surface of the liquid tank 18 is provided with an infusion port 19; the vibration-guiding liquid 20 is placed in the liquid tank 18, the piezoelectric piece 23 is embedded in the center of the bottom surface of the liquid tank 18, and the data transmission interface 21 is connected to the piezoelectric piece 23 via the copper wire 22.

[0056] like Figures 6 to 9 As shown, the piezoelectric sheet 23 is composed of an interdigitated electrode Ⅰ24, a conductive silver paste Ⅰ25, a substrate 26, a piezoelectric layer 27, a packaging cover 28, an electrode layer 29, a conductive silver paste Ⅱ30 and an interdigitated electrode Ⅱ31. A hole Ⅰ32 is provided on the left side of the packaging cover 28, and a hole Ⅱ33 is provided on the right side of the packaging cover 28; the substrate 26, the piezoelectric layer 27 and the electrode layer 29 are arranged in sequence from bottom to top and fixedly connected, and the packaging cover 28 is fixedly connected to the substrate 26; the conductive silver paste Ⅱ30 is fixedly connected to the left side of the electrode layer 29, the right end of the interdigitated electrode Ⅱ31 is fixedly connected to the conductive silver paste Ⅱ30 through the hole Ⅰ32 of the packaging cover 28, the conductive silver paste Ⅰ25 is fixedly connected to the right side of the electrode layer 29, and the left end of the interdigitated electrode Ⅰ24 is fixedly connected to the conductive silver paste Ⅰ25 through the hole Ⅱ33 of the packaging cover 28.

[0057] like Fig.10As shown, the data management module D is composed of a power management unit 34, a vibration signal acquisition card 35, a vibration signal processing unit 36, a wireless transmission unit 37 and a signal display unit 38; a periodic data sampling method is used in the acquisition process, and 10,000 data are fixedly sampled for signals from different sensing components to form data acquisition points. By adjusting the sampling frequency, the frequency is kept at 30 Hz-70 Hz and the sampling time is always an integer multiple of the signal period; the vibration signal processing unit 36 ​​is connected to the vibration signal acquisition card 35 for communication, centrally amplifies the vibration data collected by the acquisition card, performs data fitting and integration processing on the vibration data collected at each point, obtains a smooth vibration waveform, solves the vibration intensity values ​​in three directions within a certain frequency range, obtains the relationship curve between amplitude and time through FFT processing, obtains the amplitude, effective value and mean, compares the amplitude, effective value and mean with the preset threshold, and performs vibration warning if the amplitude, effective value and mean exceed the preset threshold;

[0058] The wireless transmission unit 37 is communicatively connected to the vibration signal processing unit 36 ​​and the signal display unit 38, and uses wireless communication to transmit data; the signal display unit 38 is communicatively connected to the vibration signal acquisition card 35, and visually displays the detection data of the vibration signal acquisition card 35; the power management unit 34 is powered by a 3.7V lithium battery, and is connected to the vibration signal acquisition card 35, the vibration signal processing unit 36 ​​and the wireless transmission unit 37 using a Micro USB interface.

[0059] like Fig.11 and Fig.12 As shown, the preparation method of the three-axis vibration test sensor based on additive manufacturing technology of the present invention includes a preparation method of the piezoelectric layer 27, a preparation method of the electrode layer 29 and a preparation method of the packaging cover 28:

[0060] 1.1 The method for preparing the piezoelectric layer 27 comprises the following steps:

[0061] The piezoelectric layer 27 material described in 1.1.1 is a new type of piezoelectric ceramic material compounded by 3D printing technology, wherein the mass ratio of lead zirconate titanate, graphite, zinc oxide and copper hydroxide is 100:20:10:10, and is printed by SLS 3D printing technology;

[0062] 1.1.2 At room temperature, lead zirconate titanate solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:1.5, ball-milled for 12 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form a suspension A;

[0063] 1.1.3 At room temperature, graphite solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:0.5, ball-milled for 8 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form suspension B;

[0064] 1.1.4 After mixing suspension A and suspension B, add 70% alcohol solution by mass, and disperse by ultrasonic to mix the solutions evenly to obtain a mixed solution with a certain mass fraction. Place the mixed solution in an 85℃ constant temperature oven and dry for 12 hours to obtain mixed solid powder particles, which are then passed through a 200 sieve;

[0065] 1.1.5 Grind zinc oxide and copper hydroxide solid particles at room temperature, use trisodium citrate dihydrate as dispersant and anhydrous ethanol as grinding aid, and then ball mill for 8 hours. Then, place the mixed solution in a 60℃ constant temperature oven and dry for 12 hours to obtain mixed solid powder particles, which are passed through a 200-sieve, wherein the mass ratio of lead zirconate titanate: zinc oxide: copper hydroxide: citric acid dihydrate is 100:10:15:5;

[0066] 1.1.6 Mix the powders obtained in step 3 and step 4, add 10% polyvinyl alcohol sol, use ionized water as solvent, stir and disperse with ultrasonic aid to obtain suspension C;

[0067] 1.1.7 Add 2g of silica sol to suspension C, shake evenly until the silica sol is completely dissolved in the suspension, then dry and remove the solvent to obtain a powdered piezoelectric mixed material to obtain a new type of piezoelectric ceramic material;

[0068] 1.1.8 Use SLS 3D printing technology to print the piezoelectric layer of the sensing component with a specific structure; smooth the surface of the processed piezoelectric layer, and then place the piezoelectric layer in a cleaning solution and an ethanol solution in turn for ultrasonic cleaning for 10 minutes each, remove the piezoelectric layer, dry it at low temperature, and cool it to room temperature;

[0069] 1.1.9 The piezoelectric layer is polarized by oil bath polarization. The polarization medium is dimethyl thermal conductive silicone oil. The polarization temperature is 50-80℃, the polarization voltage is 40-60KV / mm, and the duration is 1-2 hours. After the polarization is completed, the film is naturally cooled to room temperature under the condition of constant polarization voltage, and the surface of the piezoelectric layer is cleaned again with ethanol solution;

[0070] 1.2 The preparation method of the electrode layer 29 comprises the following steps:

[0071] 1.2.1 The electrode layer 29 is composed of conductive silver paste, interdigitated electrodes and lead-out copper wires 22;

[0072] 1.2.2 Scrub the piezoelectric layer 27 material in an ionic aqueous solution and dry it in alcohol vapor;

[0073] 1.2.3 Using silicon dioxide as a target material and applying magnetron sputtering technology, a silicon dioxide film is deposited on the piezoelectric layer 27 material;

[0074] 1.2.4 Indium tin oxide is selected as the main material of the interdigital electrode I 24 and the interdigital electrode II 31, and indium tin oxide is sputtered on silicon dioxide using magnetron sputtering technology;

[0075] 1.2.5 Ag is used as the main material of the conductive silver paste I 25 and the conductive silver paste II 30, and the conductive silver paste I 25 and the conductive silver paste II 30 are used to lead out the copper wire 22 at both ends of the interdigital electrode I 24 and the interdigital electrode II 31 respectively;

[0076] 1.2.6 Use anhydrous ethanol to clean the remaining conductive silver paste I25 and conductive silver paste II30;

[0077] 1.3 The method for preparing the packaging cover 28 comprises the following steps:

[0078] 1.3.1 The production process of the packaging cover 28 is as follows: E51 epoxy resin with an epoxy value of 0.38-0.42 is used as a substrate, graphene and styrene thermoplastic elastomer are used as fillers, the surface is covered with a polyethylene film with a thickness of 0.5 mm, phenolic amine is used as a curing agent, and acetone solution is used as a diluent, wherein the mass ratio of E51 epoxy resin, graphene, styrene thermoplastic elastomer and phenolic amine is 5:1:1:0.1;

[0079] 1.3.2 Mix E51 epoxy resin and phenolic amine in a mass ratio of 5:0.1, heat in a heating furnace at 70°C for 30 minutes, and take out;

[0080] 1.3.3 Rapidly add acetone to the mixture of E51 epoxy resin and phenolic amine, and stir rapidly, while slowly adding graphene and styrene thermoplastic elastomer filler. After the mixture is stirred evenly, place it in a vacuum dryer for vacuum treatment to obtain an encapsulation layer mixture;

[0081] 1.3.4 The encapsulation mixture is cut into pieces and mixed with a chlorinated polyethylene thermoplastic elastomer, and then extruded into a filament having isolated double percolation micro-nodes at a temperature of 180 degrees Celsius using a single screw extruder;

[0082] 1.3.5 Use fused deposition modeling 3D printing technology to print the packaging layer structure, clean it and cool it to room temperature, and then apply the polyethylene film on it by pressing.

Claims

1. A three-way vibration test sensor based on additive manufacturing technology, comprising a base (A), a vibration test assembly (B), a sensor housing (C) and a data management module (D), wherein the data management module (D) comprises a power management unit (34), a vibration signal acquisition card (35), a vibration signal processing unit (36), a wireless transmission unit (37) and a signal display unit (38), wherein the vibration signal processing unit (36) is communicatively connected to the vibration signal acquisition card (35); the wireless transmission unit (37) is communicatively connected to the vibration signal processing unit (36) and the signal display unit (38), and data transmission is performed by wireless communication; the signal display unit (38) is communicatively connected to the vibration signal acquisition card (35); the power management unit (34) is powered by a 3.7V lithium battery, and a Micro USB is used to transmit data. The interface is connected with the vibration signal acquisition card (35), the vibration signal processing unit (36) and the wireless transmission unit (37); the base (A) is composed of a chassis (1), a middle plate (2) and a center rod (3), and the chassis (1), the middle plate (2) and the center rod (3) are arranged in sequence from bottom to top and fixedly connected; the center hole (6) of the cylinder (13) in the vibration test component (B) is fixedly connected to the center rod (3) of the base (A), and the lower end of the sensor housing (C) is fixedly connected to the upper surface of the middle plate (2) in the base (A); the data input end of the vibration signal acquisition card (35) in the data management module (D) is communicatively connected with the data transmission interface (21) of the sensing component I (4), the sensing component III (8), the sensing component II (10), the sensing component IV (11), the sensing component V (15) and the sensing component VI (17) in the vibration test component (B); It is characterized in that The vibration test assembly (B) is composed of a sensing assembly I (4), a cantilever beam I (5), a cantilever beam III (7), a sensing assembly III (8), a cantilever beam II (9), a sensing assembly II (10), a sensing assembly IV (11), a cantilever beam IV (12), a cylinder (13), a cantilever beam V (14), a sensing assembly V (15), a cantilever beam VI (16) and a sensing assembly VI (17), wherein the cylinder (13) is provided with a center hole (6); the inner end of the cantilever beam I (5) is fixedly connected to the upper left end of the cylinder (13), and the sensing assembly I (4) is fixedly connected to the upper surface of the cantilever beam I (5) near the outer end; the inner end of the cantilever beam II (9) is fixedly connected to the upper right end of the cylinder (13) The sensing component II (10) is fixedly connected to the lower side of the cantilever beam II (9); the inner end of the cantilever beam III (7) is fixedly connected to the lower end of the front side of the cylinder (13), and the sensing component III (8) is fixedly connected to the upper side of the outer end of the cantilever beam III (7); the inner end of the cantilever beam IV (12) is fixedly connected to the lower right end of the cylinder (13), and the sensing component IV (11) is fixedly connected to the upper side of the outer end of the cantilever beam IV (12); the inner end of the cantilever beam V (14) is fixedly connected to the lower rear end of the cylinder (13), and the sensing component V (15) is fixedly connected to the upper side of the outer end of the cantilever beam V (14); the inner end of the cantilever beam VI (16) is fixedly connected to the lower left end of the cylinder (13), and the sensing component VI (17) is fixedly connected to the upper side of the outer end of the cantilever beam VI (16).

2. The three-axis vibration test sensor based on additive manufacturing technology according to claim 1, It is characterized in that The sensing components I (4), III (8), II (10), IV (11), V (15) and VI (17) have the same structure, and are all composed of a liquid tank (18), a vibration-guiding liquid (20), a data transmission interface (21), a copper wire (22) and a piezoelectric sheet (23). The top surface of the liquid tank (18) is provided with an infusion port (19); the vibration-guiding liquid (20) is placed in the liquid tank (18), the piezoelectric sheet (23) is embedded in the center of the bottom surface of the liquid tank (18), and the data transmission interface (21) is connected to the piezoelectric sheet (23) via the copper wire (22).

3. The three-axis vibration test sensor based on additive manufacturing technology according to claim 2, It is characterized in that The piezoelectric sheet (23) is composed of an interdigitated electrode I (24), a conductive silver paste I (25), a substrate (26), a piezoelectric layer (27), a packaging cover (28), an electrode layer (29), a conductive silver paste II (30) and an interdigitated electrode II (31). The packaging cover (28) is provided with a hole I (32) on the left side and a hole II (33) on the right side. The substrate (26), the piezoelectric layer (27) and the electrode layer (29) are arranged in an orderly manner from bottom to top. The packaging cover (28) is fixedly connected to the substrate (26); the conductive silver paste II (30) is fixedly connected to the left side of the electrode layer (29); the right end of the interdigitated electrode II (31) is fixedly connected to the conductive silver paste II (30) through the hole I (32) of the packaging cover (28); the conductive silver paste I (25) is fixedly connected to the right side of the electrode layer (29); the left end of the interdigitated electrode I (24) is fixedly connected to the conductive silver paste I (25) through the hole II (33) of the packaging cover (28).

4. A method for preparing a three-dimensional vibration test sensor based on additive manufacturing technology according to claim 1, characterized in that it includes a method for preparing a piezoelectric layer (27), a method for preparing an electrode layer (29) and a method for preparing a packaging cover (28): 4.1 The method for preparing the piezoelectric layer (27) comprises the following steps: The piezoelectric layer (27) material described in 4.1.1 is a piezoelectric ceramic material composited using 3D printing technology, wherein the mass ratio of lead zirconate titanate, graphite, zinc oxide and copper hydroxide is 100:20:10:10, and is printed using SLS 3D printing technology; 4.1.2 At room temperature, lead zirconate titanate solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:1.5, ball-milled for 12 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form suspension A; 4.1.3 At room temperature, graphite solid powder and sodium hexametaphosphate are mixed in a mass ratio of 100:0.5, ball-milled for 8 hours with anhydrous ethanol as a grinding aid, and then allowed to stand to form suspension B; 4.1.4 After mixing suspension A and suspension B, add 70% alcohol solution by mass, and disperse by ultrasonic to mix the solutions evenly to obtain a mixed solution of a certain mass fraction. Place the mixed solution in a constant temperature box at 85℃ and dry for 12 hours to obtain mixed solid powder particles, which are then passed through a 200 sieve; 4.1.5 Grind zinc oxide and copper hydroxide solid particles at room temperature, use trisodium citrate dihydrate as dispersant and anhydrous ethanol as grinding aid, and then ball mill for 8 hours. Then, place the mixed solution in a 60℃ constant temperature oven and dry for 12 hours to obtain mixed solid powder particles, which are passed through a 200 sieve, wherein the mass ratio of lead zirconate titanate: zinc oxide: copper hydroxide: citric acid dihydrate is 100:10:15:5; 4.1.6 Mix the powders obtained in step 4.1.3 and step 4.1.4, add 10% polyvinyl alcohol sol, use ionized water as solvent, stir and disperse with ultrasonic aid to obtain suspension C; 4.1.7 Add 2 g of silica sol to the suspension C, shake evenly until the silica sol is completely dissolved in the suspension, dry it, remove the solvent, and obtain a powdered piezoelectric mixed material to obtain a piezoelectric ceramic material; 4.1.8 Use SLS 3D printing technology to print the piezoelectric layer of the sensing component with a specific structure; smooth the surface of the processed piezoelectric layer, and then place the piezoelectric layer in a cleaning solution and an ethanol solution for ultrasonic cleaning for 10 minutes each, remove the piezoelectric layer, dry it at low temperature, and cool it to room temperature; 4.1.9 The piezoelectric layer is polarized by oil bath polarization. The polarization medium is dimethyl thermal conductive silicone oil. The polarization temperature is 50-80℃, the polarization voltage is 40-60KV / mm, and the duration is 1-2 hours. After the polarization is completed, the film is naturally cooled to room temperature under the condition of constant polarization voltage, and the surface of the piezoelectric layer is cleaned again with ethanol solution; 4.2 The preparation method of the electrode layer (29) comprises the following steps: 4.2.1 The electrode layer (29) is composed of conductive silver paste, interdigitated electrodes and lead-out copper wires (22); 4.2.2 Scrub the piezoelectric layer (27) material in an ionic aqueous solution and dry it in alcohol vapor; 4.2.3 Using silicon dioxide as a target material and applying magnetron sputtering technology, a silicon dioxide film is deposited on the piezoelectric layer (27) material; 4.2.4 Indium tin oxide is selected as the main material of the interdigitated electrode I (24) and the interdigitated electrode II (31), and indium tin oxide is sputtered on silicon dioxide using magnetron sputtering technology; 4.2.5 Ag is used as the main material of the conductive silver paste I (25) and the conductive silver paste II (30), and the conductive silver paste I (25) and the conductive silver paste II (30) are used to lead out the copper wires (22) at both ends of the interdigitated electrode I (24) and the interdigitated electrode II (31), respectively; 4.2.6 Clean the remaining conductive silver paste I (25) and conductive silver paste II (30) with anhydrous ethanol; 4.3 The method for preparing the packaging cover (28) comprises the following steps: 4.3.1 The production process of the packaging cover (28) is as follows: an E51 epoxy resin with an epoxy value of 0.38-0.42 is used as a substrate, graphene and styrene thermoplastic elastomer are used as fillers, the surface is covered with a polyethylene film with a thickness of 0.5 mm, phenolic amine is used as a curing agent, and an acetone solution is used as a diluent, wherein the mass ratio of E51 epoxy resin, graphene, styrene thermoplastic elastomer and phenolic amine is 5:1:1:0.1; 4.3.2 Mix E51 epoxy resin and phenolic amine in a mass ratio of 5:0.1, heat in a heating furnace at 70°C for 30 minutes, and take out; 4.3.3 Rapidly add acetone to the mixture of E51 epoxy resin and phenolic amine, and stir rapidly, while slowly adding graphene and styrene thermoplastic elastomer filler. After the mixture is stirred evenly, place it in a vacuum dryer for vacuum treatment to obtain an encapsulation layer mixture; 4.3.4 The encapsulation mixture is shredded and mixed with a chlorinated polyethylene thermoplastic elastomer, and then extruded into a filament having isolated double percolation micro-nodes at a temperature of 180 degrees Celsius using a single screw extruder; 4.3.5 Use fused deposition modeling 3D printing technology to print the packaging layer structure, clean it and cool it to room temperature, and then apply the polyethylene film on it by pressing.

Citation Information

Cited By

  • Piezoelectric sensor with resonating microstructures

    US12582332B2

  • Piezoelectric sensor with resonating microstructures

    US20220409095A1