Positive electrode active material for non-aqueous electrolyte secondary battery and method for producing the same, method for evaluating positive electrode active material for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
By adding niobium to the lithium nickel-manganese composite oxide and adjusting its distribution, the gelation problem of the positive electrode active substance of the non-aqueous electrolyte secondary battery is solved, high battery characteristics and low cost manufacturing are achieved, and suitable for industrial-scale production.
Patent Information
- Application Number
- CN201980011787.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-02-06
- Filing Date
- 2019-01-25
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2039-01-25
AI Technical Summary
The positive electrode active substance of the existing non-aqueous electrolyte secondary battery has gelation problems during the manufacturing process, resulting in deterioration of operability and a decrease in yield. The niobium has poor effect in inhibiting gelation and is difficult to produce in industrial scale. Low cost manufacturing.
By adding a specific amount of niobium to the lithium nickel-manganese composite oxide, a secondary particle structure with multiple aggregation is formed. At least part of the niobium is dissolved in the interior of the primary particles, and the amount of lithium dissolved at 0.02% is adjusted by neutralization titration method. Within the range of ~0.10%, combined with specific sintering processes and evaluation methods, ensure uniform distribution of niobium to inhibit gelation.
Effectively inhibit the gelation of the positive electrode paste, improve battery characteristics, improve yield, and realize low-cost manufacturing in industrial scale production, simplify the evaluation and selection of positive electrode active substances, and obtain a secondary battery with high battery capacity.
Smart Images

Figure CN111699577B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a positive electrode active material for a non-aqueous electrolyte secondary battery and a method for producing the same, a method for evaluating the positive electrode active material for a non-aqueous electrolyte secondary battery, and a non-aqueous electrolyte secondary battery. Background Art
[0002] In recent years, with the popularization of portable electronic devices such as mobile phones and notebook computers, there is a strong demand for the development of small and lightweight secondary batteries with high battery capacity and durability. In addition, there is a strong demand for high-output secondary batteries for batteries used in electric vehicles such as power tools and hybrid vehicles.
[0003] As secondary batteries that meet such requirements, there are non-aqueous electrolyte secondary batteries such as lithium ion secondary batteries. Non-aqueous electrolyte secondary batteries are composed of a negative electrode, a positive electrode, and an electrolyte, and materials that can insert and remove lithium are used as active materials for the negative electrode and the positive electrode. Furthermore, non-aqueous electrolyte secondary batteries require higher thermal stability in addition to high battery capacity and durability.
[0004] Extensive research and development is being conducted on non-aqueous electrolyte secondary batteries. Among them, non-aqueous electrolyte secondary batteries using layered or spinel lithium metal composite oxides as positive electrode materials are being promoted for practical use as batteries with high energy density because they can achieve high voltages of 4V.
[0005] As positive electrode active materials for non-aqueous electrolyte secondary batteries, lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel that is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5 O2) and other lithium metal composite oxides.
[0006] Among the above positive electrode active materials, lithium nickel cobalt manganese composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 Lithium nickel cobalt manganese composite oxide is a layered compound similar to lithium cobalt composite oxide, lithium nickel composite oxide, etc., and contains nickel, cobalt and manganese in a composition ratio of 1:1:1 at the transition metal site.
[0007] On the other hand, in order to obtain a positive electrode having high performance (high cycle characteristics, high capacity, high output) as a non-aqueous electrolyte secondary battery, a technique of adding niobium to the above-mentioned lithium metal composite oxide has been proposed.
[0008] For example, Patent Document 1 proposes a general formula: Li a Ni 1-x-y-z Co x M y Nb z O b A non-aqueous secondary battery positive electrode active material formed by a composition consisting of at least one compound consisting of lithium, nickel, cobalt, element M, niobium and oxygen (wherein M is one or more elements selected from the group consisting of Mn, Fe and Al, 1≦a≦1.1, 0.1≦x≦0.3, 0≦y≦0.1, 0.01≦z≦0.05, 2≦b≦2.2). According to Patent Document 1, the Li-Nb-O system compound present near or inside the particle surface has high thermal stability, so that a positive electrode active material with high thermal stability and large discharge capacity can be obtained.
[0009] In addition, Patent Document 2 proposes a method of 1+x Ni a Mn b Co c O 2+d A positive electrode active material used in which niobium is added to a lithium-containing transition metal composite oxide having a layered structure represented by (x+a+b+c=1, 0.7≦a+b, 0<x≦0.1, 0≦c / (a+b)<0.35, 0.7≦a / b≦2.0, -0.1≦d≦0.1) so that the amount of niobium is 0.05 mass % or more and 2.00 mass % or less. According to Patent Document 5, by using such a positive electrode active material, the output characteristics under various temperature conditions can be improved.
[0010] In addition, Patent Document 3 proposes a positive electrode active material for a non-aqueous electrolyte secondary battery, which is formed of a lithium transition metal composite oxide composed of particles of a polycrystalline structure, obtained by a manufacturing method having a mixing step of mixing a lithium mixture obtained by mixing a nickel-containing hydroxide, a lithium compound and a niobium compound having an average particle size of 0.1 to 10 μm and a calcining step of calcining the lithium mixture at 700 to 840° C. in an oxidizing atmosphere, and has a porous structure and a specific surface area of 0.9 to 3.0 m 2 / g, and the content of alkali metals other than lithium is 20 mass ppm or less. The positive electrode active material achieves high thermal stability, high charge and discharge capacity, and excellent cycle characteristics.
[0011] In addition, the positive electrode of the non-aqueous electrolyte secondary battery is formed by, for example, mixing a positive electrode active material, a binder such as polyvinylidene fluoride (PVDF), and a solvent such as N-methyl-2-pyrrolidone (NMP) to form a positive electrode paste, and applying it to a collector such as aluminum foil. At this time, when lithium is freed from the positive electrode active material in the positive electrode paste, it reacts with the moisture contained in the binder and the like to generate lithium hydroxide. Sometimes the lithium hydroxide generated in this way reacts with the binder, which can cause gelation of the positive electrode paste. The gelation of the positive electrode paste can lead to deterioration of operability and a decrease in yield. This tendency is more significant when the lithium in the positive electrode active material is in excess compared to the stoichiometric ratio and the proportion of nickel is high.
[0012] Various methods have been tried to inhibit the gelation of the positive electrode paste. For example, Patent Document 4 proposes a positive electrode composition for a non-aqueous electrolyte secondary battery containing a positive electrode active material formed of a lithium transition metal composite oxide and an additive particle formed of an acidic oxide particle. In the positive electrode composition, lithium hydroxide generated by reacting with the water contained in the binder will preferentially react with the acidic oxide, inhibiting the reaction of the generated lithium hydroxide with the binder and inhibiting the gelation of the positive electrode mixture paste. In addition, the acidic oxide also acts as a conductive material in the positive electrode, which helps to reduce the overall resistance of the positive electrode and improve the output characteristics of the battery.
[0013] In addition, in Patent Document 5, as a method for manufacturing a lithium-ion secondary battery, a method for manufacturing a lithium-ion secondary battery is proposed, which includes the following steps: preparing a lithium transition metal oxide containing LiOH as a positive electrode active material; determining the molar amount P of LiOH contained in each 1 g of the positive electrode active material; preparing 0.05 moles or more of tungsten oxide calculated as tungsten atoms per 1 mole of LiOH relative to the molar amount P of LiOH; and kneading the positive electrode active material and tungsten oxide together with a conductive material and a binder in an organic solvent to prepare a positive electrode paste.
[0014] Prior art literature
[0015] Patent Literature
[0016] Patent Document 1: Japanese Patent Application Publication No. 2002-151071
[0017] Patent Document 2: Japanese Patent Application Publication No. 2011-070789
[0018] Patent Document 3: Japanese Patent Application Publication No. 2015-122298
[0019] Patent Document 4: Japanese Patent Application Publication No. 2012-028313
[0020] Patent Document 5: Japanese Patent Application Publication No. 2013-084395 Summary of the invention
[0021] Problems to be solved by the invention
[0022] Although the positive electrode active materials described in the above-mentioned Patent Documents 1 to 3 all attempt to improve battery characteristics, there is still a demand for further improvement of battery characteristics. In addition, Patent Document 1 records that niobium exists as a Li-Nb-O compound near the particle surface, and Patent Document 2 records that niobium is contained at least on the surface or inside of lithium containing transition metals, but in order to stabilize and improve battery characteristics, it is hoped that niobium can be more evenly distributed in the positive electrode active material.
[0023] In addition, although the positive electrode active materials of Patent Documents 4 and 5 are described as being able to suppress the viscosity increase of the positive electrode paste, there is no description of the effect of suppressing the gelation of the positive electrode paste in the positive electrode active material containing niobium. It should be noted that Patent Documents 1 to 3 also do not describe any effect of niobium on suppressing the gelation of the positive electrode paste.
[0024] In view of the above situation, the present invention aims to provide a positive electrode active material having high battery characteristics and suppressing the gelation of the positive electrode paste during the preparation of the positive electrode. In addition, the present invention aims to provide a method for easily and at low cost producing such a positive electrode active material in industrial-scale production. Furthermore, the present invention provides an evaluation method for a positive electrode active material that can easily select a positive electrode active material, wherein the positive electrode active material is a positive electrode active material containing niobium, can suppress the gelation of the positive electrode paste and can stably obtain a secondary battery with a high battery capacity.
[0025] Solution to the problem
[0026] In order to solve the above-mentioned problems, the present inventors conducted intensive studies and found that by adding a specific amount of niobium to a lithium nickel manganese composite oxide containing a specific amount of manganese, it is possible to simultaneously reduce the amount of leached lithium in the resulting positive electrode active material, increase the battery capacity, and inhibit the gelation of the positive electrode paste, thereby completing the present invention.
[0027] In a first aspect of the present invention, there is provided a positive electrode active material for a non-aqueous electrolyte secondary battery, which is a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium nickel manganese composite oxide formed of secondary particles formed by agglomeration of a plurality of primary particles, wherein the positive electrode active material is represented by the general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+αIt represents that M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.2, 0.33<(1-abc), 0≦α≦0.4; at least a portion of niobium is solid-dissolved in the interior of the primary particles, and the amount of lithium dissolved in water when the above-mentioned positive electrode active material is immersed in water determined by neutralization titration is 0.02 mass% to 0.10 mass% relative to the total positive electrode active material.
[0028] In addition, it is preferred that the maximum niobium concentration is 1 to 3 times the average niobium concentration inside the primary particle. In addition, the positive electrode active material contains a compound containing lithium and niobium, and the compound containing lithium and niobium is preferably present on the surface of the primary particle. In addition, the grain size (crystallite diameter) obtained by the Scherrer formula from the peak of the (003) surface in the X-ray diffraction pattern is preferably 110 nm to 200 nm. In addition, the volume average particle size MV is preferably 5 μm to 20 μm.
[0029] In a second aspect of the present invention, there is provided a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, which is a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium nickel manganese composite oxide formed of secondary particles formed by agglomeration of a plurality of primary particles, comprising the steps of mixing at least one of nickel manganese composite hydroxide particles and nickel manganese composite oxide particles with a niobium compound and a lithium compound; and calcining the lithium niobium mixture obtained by the mixing; the nickel manganese composite hydroxide particles and the nickel manganese composite oxide particles contain nickel, manganese and an arbitrary element M, and the atomic ratio of each metal is expressed as Ni:Mn:M=(1-ab ): a: b, wherein 0.05≦a≦0.6, 0≦b≦0.6, 0.33<(1-ab), M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta; the lithium-niobium mixture contains 0.03 atomic % to 3 atomic % of niobium relative to all metal elements other than lithium, and the above-mentioned positive electrode active material is adjusted so that at least a part of niobium is solid dissolved in the interior of the primary particles, and the amount of lithium dissolved in water when the positive electrode active material is immersed in water, determined by neutralization titration, is 0.02 mass % to 0.10 mass % relative to the total positive electrode active material.
[0030] In addition, the method for manufacturing the positive electrode active material preferably calcines the lithium-niobium mixture in an oxidizing atmosphere at 850°C to 1000°C. In addition, it is preferred that at least a portion of the niobium of the lithium nickel-manganese composite oxide is solid-dissolved in the primary particles, and the maximum niobium concentration inside the primary particles is 1 to 3 times or more. In addition, calcination is preferably performed in a manner such that the grain size of the positive electrode active material obtained by the Scherrer formula from the peak of the (003) plane in the X-ray diffraction pattern is 110 nm to 200 nm or less. In addition, it is preferred that the nickel-manganese composite hydroxide particles are obtained by crystallizing in a reaction aqueous solution containing a nickel-containing salt, a manganese-containing salt, and a salt containing any element M, by controlling the pH and ammonium ion concentration of the reaction aqueous solution within a prescribed range, and the nickel-manganese composite oxide particles are obtained by heat treating the nickel-manganese composite hydroxide particles obtained by the above-mentioned crystallization. In addition, the niobium compound is preferably niobic acid or niobium oxide, and the average particle size is 0.01 μm to 10 μm or less. In addition, the lithium compound is preferably lithium carbonate. Furthermore, the nickel-manganese composite oxide particles are preferably obtained by heat-treating nickel-manganese composite hydroxide particles at a temperature of 105° C. to 700° C. both inclusive.
[0031] In a third aspect of the present invention, there is provided a method for evaluating a positive electrode active material for a non-aqueous electrolyte secondary battery, which is a general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+α An evaluation method for a positive electrode active material for a non-aqueous electrolyte secondary battery formed of a lithium nickel manganese composite oxide represented by the present invention, wherein M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.2, 0.33<(1-abc), 0≦α≦0.4; a step of determining the amount of lithium dissolved in water when immersed in water obtained by neutralization titration; and a step of selecting a positive electrode active material whose amount of lithium dissolved in water is 0.02 mass % or more and 0.10 mass % or less relative to the total positive electrode active material.
[0032] In a fourth aspect of the present invention, there is provided a nonaqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode contains the positive electrode active material for the nonaqueous electrolyte secondary battery.
[0033] Effects of the Invention
[0034] The positive electrode active material of the present invention can suppress the gelation of the positive electrode paste when the positive electrode is made, and the secondary battery has high battery characteristics. In addition, the positive electrode active material of the present invention can improve the yield rate because it is easy to handle when the positive electrode is made. In addition, the method for manufacturing the positive electrode active material of the present invention can easily and at low cost manufacture such a positive electrode active material in industrial-scale production. Furthermore, the evaluation method of the positive electrode active material of the present invention can simply select a positive electrode active material, which is a positive electrode active material containing niobium, and can suppress the gelation when the positive electrode paste is made and obtain a secondary battery with a high battery capacity.
[0035] Furthermore, the method for evaluating a positive electrode active material for a non-aqueous electrolyte secondary battery can easily select a positive electrode active material that suppresses gelation of a positive electrode paste and has a high battery capacity. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] [ Figure 1 ] Figure 1 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0037] [ Figure 2 ] Figure 2 This is a diagram showing an example of a method for producing a positive electrode active material according to this embodiment.
[0038] [ Figure 3 ] Figure 3 This is a diagram showing an example of a method for evaluating the positive electrode active material according to the present embodiment.
[0039] [ Figure 4 ] Figure 4 This is a schematic diagram of a button-type battery used in battery evaluation.
[0040] [ Figure 5 ] Figure 5 It is a graph showing the results of XRD measurement of Examples and Comparative Examples. DETAILED DESCRIPTION
[0041] Hereinafter, the present embodiment of the present invention will be described with reference to the accompanying drawings. It should be noted that, in order to facilitate understanding of each configuration, a portion is emphasized or a portion is simplified in the accompanying drawings, which may be different from the actual structure, shape, size, etc.
[0042] 1. Positive electrode active material for non-aqueous electrolyte secondary batteries
[0043] The positive electrode active material for a non-aqueous electrolyte secondary battery according to the present embodiment (hereinafter also referred to as "positive electrode active material") is composed of particles of a polycrystalline structure, and contains a lithium nickel manganese composite oxide (hereinafter also referred to as "lithium metal composite oxide") formed of secondary particles formed by agglomeration of a plurality of primary particles. In addition, in the positive electrode active material, at least a portion of niobium is solid-dissolved in the interior of the primary particles, and the amount of lithium dissolved in water when the positive electrode active material is immersed in water (hereinafter also referred to as "dissolved lithium amount") obtained by neutralization titration is 0.02 mass % or more and 0.10 mass % or less relative to the total positive electrode active material.
[0044] The positive electrode active material according to this embodiment contains specific amounts of manganese and niobium and has an eluted lithium amount within the above range, thereby achieving both suppression of gelation of the positive electrode paste and excellent battery characteristics (high charge and discharge capacity, excellent output characteristics, thermal stability, etc.) of the positive electrode of the secondary battery.
[0045] [Composition of positive electrode active material]
[0046] The positive electrode active material is represented by the general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+α Indicates that M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.20, 0.33<(1-abc), 0≦α≦0.4.
[0047] (Mn)
[0048] In the above general formula (1), the range of a representing the content of Mn is 0.05≦a≦0.6, preferably 0.10≦a≦0.55, more preferably 0.10<a≦0.50, and further preferably 0.12≦a≦0.45. When the value of a is in the above range, excellent output characteristics and high energy density can be obtained, and thus the thermal stability also becomes a material with high thermal stability. On the other hand, when the value of a is less than 0.05, the improvement effect of thermal stability cannot be obtained, and when the value of a exceeds 0.6, the output characteristics and energy density decrease. In addition, in the positive electrode active material of the present embodiment, by containing Mn in the above range together with Nb described later, a secondary battery with reduced positive electrode resistance and very high output characteristics can be obtained.
[0049] (Element M)
[0050] In the above general formula (1), M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta. The range of the content b of M is 0≦b≦0.6. When the value of b exceeds 0, thermal stability, storage characteristics and battery characteristics can be improved. For example, when M includes Co, the battery capacity and output characteristics are more excellent. When M is Co, preferably 0.05≦b≦0.5, more preferably 0.1≦b≦0.4.
[0051] (Nb)
[0052] In the above general formula (1), the range of c representing the content of Nb is 0.0003≦c≦0.03. When the value of c is in the above range, a high battery capacity can be obtained when used for the positive electrode of a secondary battery. In addition, by containing Nb in the above range and by making the amount of dissolved lithium of the positive electrode active material in a specific range described later, the distribution of niobium present inside and / or on the surface of the primary particles can be made more uniform, and it is possible to take into account both the inhibition of gelation of the positive electrode paste and high battery characteristics. In addition, when lithium carbonate is used as a raw material for lithium, the amount of dissolved lithium of the positive electrode active material can be reduced, and the residual carbon can be reduced. On the other hand, when the value of c is less than 0.0003, the effect of reducing the amount of dissolved lithium and residual carbon cannot be obtained. In addition, when the value of c exceeds 0.03, there is a situation where segregation of niobium compounds is easily caused, reducing output characteristics and battery capacity.
[0053] Furthermore, from the viewpoint of making the distribution of niobium more uniform and obtaining a positive electrode active material having high battery characteristics, the range of c is preferably 0.0005≦c≦0.025, and more preferably 0.001≦c≦0.02.
[0054] It should be noted that, for example, in the above general formula (1), when the value of c exceeds 0.005, by using the method for producing the positive electrode active material described later, niobium is not only dissolved in the interior of the primary particles, but also forms lithium niobium compounds on the surface of the primary particles. However, even when the same amount of niobium is contained, by changing the conditions during production, there may be a situation where the lithium niobium compound is excessively formed on the surface of the primary particles, or the lithium niobium compound is formed unevenly. In this case, the expected battery characteristics and the effect of inhibiting the gelation of the positive electrode paste cannot be obtained. Here, by controlling the amount of dissolved lithium of the positive electrode active material within a suitable range, the lithium niobium compound can be formed on the surface of the primary particles in a more suitable amount and distribution. Therefore, when the range of c representing the niobium content is particularly 0.005<c<0.02, by controlling the amount of dissolved lithium of the positive electrode active material within a specific range, a secondary battery with better battery characteristics can be easily and stably obtained.
[0055] (Ni)
[0056] In the above general formula (1), the range of (1-abc) representing the Ni content is 0.33<(1-abc). Generally, the higher the Ni content, the higher the battery capacity (initial charge and discharge capacity) of the resulting secondary battery can be, but there is a tendency for the positive electrode paste to gel when the positive electrode is made. In the positive electrode active material of this embodiment, for example, when the nickel content in the above general formula is 0.5≦(1-abc) and 0.55≦(1-abc), by containing niobium in a specific range and controlling the amount of dissolved lithium in a specific range, the gelation of the positive electrode paste can be suppressed and the battery characteristics can be improved.
[0057] (Li)
[0058] In the above general formula (1), the range of d representing the content of Li is 0.95≦d≦1.2. Generally, the higher the content of Li, the more likely the positive electrode paste is to gel when the positive electrode is produced. In the positive electrode active material of the present embodiment, for example, when the content of Li is 1.0<d≦1.2 in the above general formula (1), by containing niobium in a specific range and controlling the amount of dissolved lithium in a specific range, the battery characteristics can be improved and the gelation of the positive electrode paste can be suppressed.
[0059] [Amount of dissolved lithium]
[0060] The present inventors have discovered that, in a positive electrode active material containing niobium in a specific amount, by adjusting the amount of eluted lithium in the positive electrode active material to a specific range, the distribution of niobium present inside and / or on the surface of the primary particles can be made more uniform, the gelation of the positive electrode paste can be suppressed, and the battery characteristics can be improved, thereby completing the present invention, although the detailed reason is not yet clear.
[0061] The amount of dissolved lithium of the positive electrode active material of the present embodiment is 0.02 mass % to 0.10 mass % relative to the total positive electrode active material, preferably 0.04 mass % to 0.08 mass %. When the amount of dissolved lithium is within the above range, the gelation of the positive electrode paste can be greatly suppressed and a secondary battery with excellent battery characteristics can be obtained. In addition, when the amount of dissolved lithium exceeds 0.10 mass %, the remaining lithium in the positive electrode active material becomes a lot, and it is difficult to suppress the gelation of the paste. On the other hand, when the amount of dissolved lithium is less than 0.02 mass %, the battery characteristics sometimes deteriorate.
[0062] In addition, for example, in the above general formula (1), when d representing the content of lithium exceeds 1 and the range of the content of nickel is 0.5≦(1-abc), the amount of dissolved lithium can also be 0.05 mass% or more and 0.10 mass% or less. In addition, for example, when d representing the content of lithium exceeds 1 and the range of (1-abc) is 0.55≦(1-abc), the amount of dissolved lithium can be 0.06 mass% or more and 0.10 mass% or less. When the content of nickel and the amount of dissolved lithium are within the above range, the gelation of the positive electrode paste can be greatly suppressed and a secondary battery with excellent battery characteristics can be obtained.
[0063] It should be noted that the amount of dissolved lithium is calculated as follows: 5 g of positive electrode active material is weighed, put into 100 ml of pure water at 25°C, immersed, stirred for 30 minutes and then filtered, the filtrate is neutralized and titrated with HCl aqueous solution, and the amount of lithium dissolved in pure water is calculated (mass % relative to the total mass of the positive electrode active material).
[0064] As described later, by containing manganese and niobium in a specific range in the manufacturing process of the positive electrode active material, adjusting the dissolved oxygen concentration in the reaction solution, the temperature of the reaction solution, etc. in the crystallization process (step S10), adjusting the sintering temperature in the sintering process (step S30), and adding a pre-sintering process (step S25), the amount of dissolved lithium in the positive electrode active material can be controlled to the above-mentioned range.
[0065] It should be noted that the dissolved lithium is considered to be residual lithium such as lithium existing in the crystals of the positive electrode active material and the like, which is derived from the residue of the lithium compound used as a raw material (unreacted lithium compound) or the like.
[0066] [Existing form of niobium]
[0067] The positive electrode active material involved in the present embodiment contains niobium and at least a part of the niobium is solid-dissolved in the primary particles. When niobium is contained in the positive electrode active material, the amount of lithium dissolved in the positive electrode active material can be reduced. The detailed reason is not clear, but the following phenomenon is inferred. That is, niobium (usually 5-valent) is an element with a higher valence than the nickel contained in the positive electrode active material. When the positive electrode active material is manufactured, the high-valence element is present in the sintering process (step S30). When the precursor particles (nickel composite hydroxide particles, nickel composite oxide particles, etc.) are sintered with lithium compounds, the need to increase the valence of nickel is reduced compared to the case of niobium without additives. Along with this, it is believed that the reaction of lithium compounds is easy to proceed, the residual amount of unreacted lithium compounds is reduced, and the amount of dissolved lithium is also reduced.
[0068] In particular, when lithium carbonate is used as a lithium compound, it has a tendency to remain as an unreacted lithium compound after the firing process due to its higher melting point than lithium hydroxide. However, it is believed that in the positive electrode active material involved in the present embodiment, by containing niobium, the reaction of lithium carbonate during firing is promoted, and the residual amount of unreacted lithium carbonate is eventually reduced, and while reducing the amount of dissolved lithium, the content of residual carbon as an impurity is also reduced.
[0069] In addition, when at least a portion of niobium is solid-dissolved in the primary particles, the effects of improving the thermal stability and reducing the positive electrode resistance when the positive electrode active material is used in a secondary battery can be obtained. It should be noted that niobium solid-dissolved in the primary particles means that niobium is detected by, for example, ICP emission spectrometry and niobium is detected in the primary particles by surface analysis of the primary particle cross section using EDX in a scanning transmission electron microscope (S-TEM), and niobium is preferably detected throughout the primary particles as described later.
[0070] [Niobium concentration in primary particles]
[0071] In the positive electrode active material of this embodiment, the maximum niobium concentration inside the primary particles (maximum niobium concentration / average niobium concentration) is preferably 1 to 3 times the average niobium concentration inside the primary particles. When the maximum niobium concentration / average niobium concentration exceeds the above range, the variation of the niobium concentration in the primary particles increases, and the battery characteristics of the positive electrode active material as a whole are reduced.
[0072] The variation of the niobium concentration in the primary particles can be confirmed by line analysis of the composition of the primary particle cross section by EDX measurement using a scanning transmission electron microscope (S-TEM). The maximum niobium concentration relative to the average niobium concentration in the primary particles (maximum niobium concentration / average niobium concentration) can be obtained by, for example, selecting any 20 or more primary particles from a plurality of secondary particles and performing line analysis of the composition in the cross section of each primary particle by EDX measurement using S-TEM. The direction of the line analysis is preferably carried out in the direction of the maximum length of the cross section of the primary particle, but in cases where the influence of the niobium compound described later is excluded, it can also be carried out in a direction that can be analyzed over a length of more than 50% of the maximum length. Based on the measured values of the niobium concentration of each primary particle obtained by line analysis, the maximum niobium concentration and the average niobium concentration in the primary particles are obtained, and the ratio of the maximum niobium concentration of each primary particle is calculated (maximum niobium concentration / average niobium concentration). Furthermore, by averaging the values of the ratio of the maximum niobium concentrations calculated from each primary particle, the maximum niobium concentration in the primary particle can be obtained. It should be noted that since the change in niobium concentration is a value within the primary particle, when the niobium compound on the surface of the primary particle is confirmed by a previous surface analysis, the change in niobium concentration is measured by line analysis using EDX at a position where the measured value of the niobium concentration near the surface of the primary particle is not affected by the presence of the niobium compound.
[0073] In order to obtain a higher effect, it is preferred to suppress the presence of a portion with an extremely low niobium concentration in the primary particles, and the minimum niobium concentration in the primary particles is preferably 50% or more relative to the average niobium concentration in the primary particles. Similarly to the above, the minimum niobium concentration can be obtained by selecting any 20 or more primary particles from a plurality of secondary particles and performing line analysis on the composition in the cross section of each primary particle by EDX measurement of S-TEM, and can be obtained by number averaging the [(minimum niobium concentration / average niobium concentration)×100](%) values calculated from a plurality of primary particles.
[0074] [Lithium niobium compounds]
[0075] The positive electrode active material according to the present embodiment preferably has niobium dissolved in the primary particles as described above, and a compound containing lithium and niobium (hereinafter also referred to as a "lithium niobium compound") present on the surface of the primary particles.
[0076] It is believed that the lithium ion conductivity of the lithium niobium compound is high and has the effect of promoting the movement of lithium ions. The lithium niobium compound formed on the surface of the primary particle can form a Li conduction path at the interface between the electrolyte and the primary particle. Therefore, it is believed that the output characteristics are improved by reducing the positive electrode resistance of the obtained secondary battery.
[0077] The lithium niobium compound is not particularly limited, but is preferably at least one selected from LiNbO 3 , LiNb 3 O 8 , and Li 3 NbO 4 , and more preferably Li 3 NbO 4 .
[0078] It should be noted that the lithium niobium compound does not necessarily cover the entire surface of the primary particles of the lithium metal composite oxide, and the positive electrode resistance can be reduced as long as it exists on at least a portion of the surface of the primary particles. Furthermore, it is preferred that the lithium niobium compound is fixed to the surface of the primary particles of the lithium metal composite oxide.
[0079] It should be noted that the surface of the primary particle in this specification refers to the surface of the primary particle exposed outside the secondary particle and the surface of the primary particle near the surface of the secondary particle that is connected to the outside of the secondary particle and can be impregnated with the electrolyte and the surface of the primary particle exposed in the internal gap. Furthermore, the particle boundary between the primary particles is included as long as the bonding of the primary particles is incomplete and the electrolyte becomes permeable.
[0080] The lithium niobium compound present on the surface of the primary particles can be formed by the reaction of the niobium compound used as the niobium raw material and the lithium compound used as the lithium raw material in the calcination step (step S30) described later. The reaction to form the lithium niobium compound is also presumably helpful in reducing the amount of eluted lithium. In addition, as described above, when lithium carbonate is used as the lithium compound, the content of residual carbon can be further reduced.
[0081] The lithium niobium compound may exist in a coexistence state of crystal and amorphous, or in an amorphous state. On the other hand, when the lithium niobium compound exists in a crystalline state, its presence can be confirmed by X-ray diffraction (XRD) measurement as its amount increases.
[0082] It should be noted that, regardless of the form in which the lithium niobium compound exists, it needs to react with the lithium compound during its formation process. Therefore, compared with the positive electrode active material without niobium addition, it is speculated that the reaction during sintering can be relatively promoted, and the effect of reducing the amount of eluted lithium in the positive electrode active material is obtained by being present at least in a part of the primary particle surface. In addition, when lithium carbonate is used as the lithium compound, the effect of reducing residual carbon is also obtained.
[0083] In addition, the presence of the lithium niobium compound can be indirectly evaluated by measuring the amount of eluted lithium in the positive electrode active material. For example, when the amount of eluted lithium is reduced by 0.03% by mass or more, preferably by 0.05% by mass or more, compared to the positive electrode active material produced under the same conditions except that niobium is not added, the formation of the lithium niobium compound can be inferred.
[0084] [Grain size of (003) plane]
[0085] The grain size of the (003) surface of the positive electrode active material is preferably between 110 nm and 200 nm, more preferably between 120 nm and 190 nm, and further preferably between 130 nm and 180 nm. In addition, when the grain size of the (003) surface is within the above range, it is easy to adjust the amount of dissolved lithium of the positive electrode active material to the above range. It should be noted that the grain size of the (003) surface can be set to the above range by adjusting the firing temperature in the firing process (step S30). It should be noted that the grain size of the (003) surface is the grain size obtained by the Scherrer formula from the peak of the (003) surface in the X-ray diffraction pattern.
[0086] (Volume average particle size MV)
[0087] The volume average particle size MV of the positive electrode active material is preferably 3 μm to 20 μm, more preferably 5 μm to 20 μm, and further preferably 5 μm to 15 μm. When the volume average particle size MV is in the above range, when the positive electrode active material is used for the positive electrode of the secondary battery, high output characteristics, battery capacity and high filling property of the positive electrode can be taken into account. If the average particle size of the positive electrode active material is less than 3 μm, high filling property of the positive electrode cannot be obtained. If the average particle size exceeds 20 μm, high output characteristics and high battery capacity cannot be obtained. It should be noted that the volume average particle size MV can be obtained, for example, based on the volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0088] 2. Method for producing positive electrode active material for non-aqueous electrolyte secondary battery
[0089] Figure 1-2 1 is a diagram showing an example of a method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to the present embodiment (hereinafter also referred to as a "method for producing a positive electrode active material"). Figure 1 As shown, the method for manufacturing a positive electrode active material includes mixing at least one of nickel manganese composite hydroxide particles (hereinafter, also referred to as "nickel composite hydroxide particles") and nickel manganese composite oxide particles (hereinafter, also referred to as "nickel composite oxide particles") (hereinafter, both are also collectively referred to as "precursor particles") with a niobium compound and a lithium compound (step S20); and calcining the lithium-niobium mixture obtained by mixing (step S30). The above-mentioned positive electrode active material can be easily manufactured by the method for manufacturing a positive electrode active material involved in this embodiment.
[0090] The method for producing a positive electrode active material according to the present embodiment adjusts the amount of lithium dissolved in water when the obtained positive electrode active material is immersed in water (hereinafter also referred to as "dissolved lithium amount") to a specific amount as described later, thereby obtaining a positive electrode active material in which niobium is uniformly distributed inside the primary particles and / or on the surface of the primary particles. Furthermore, in the method for producing a positive electrode active material according to the present embodiment, from the viewpoint of more uniform distribution of elements other than niobium inside the primary particles, as described below, Figure 2 As shown, it is preferably produced by crystallizing precursor particles (step S10).
[0091] The positive electrode active material obtained by the manufacturing method according to the present embodiment contains a lithium nickel manganese composite oxide (hereinafter also referred to as "lithium metal composite oxide") formed by secondary particles formed by agglomeration of a plurality of primary particles, and at least a portion of niobium is solid-dissolved in the interior of the primary particles of the lithium metal composite oxide. The positive electrode active material is, for example, of the general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+α , wherein M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.2, 0.33<(1-abc), 0≦α≦0.4. Figure 1-2 , an example of each process used in the manufacturing method of this embodiment is described. It should be noted that the following description is only an example of the manufacturing method and does not limit the manufacturing method.
[0092] [Crystallization Step (Step S10)]
[0093] First, in a reaction aqueous solution containing a nickel-containing salt (nickel salt), a manganese-containing salt (manganese salt) and a salt containing an arbitrary element M (element M salt), the pH and ammonium ion concentration of the reaction aqueous solution are controlled within a prescribed range to perform crystallization (step S10), thereby obtaining nickel-manganese composite hydroxide particles.
[0094] The nickel composite hydroxide particles obtained by the crystallization process (step S10) are mainly composed of secondary particles formed by the aggregation of multiple primary particles. By uniformly containing manganese inside the primary particles, manganese is also uniformly distributed in the primary particles of the lithium metal composite oxide (positive electrode active material) finally obtained, and the secondary battery using the positive electrode active material can obtain the effects of high thermal stability and reduced conductivity. In addition, by containing manganese in the primary particles of the nickel composite hydroxide particles, the firing temperature in the firing process (step S30) described later can be increased, so that niobium is uniformly dissolved in the primary particles of the lithium metal composite oxide (positive electrode active material).
[0095] It should be noted that when using raw materials other than precursor particles (nickel composite hydroxide particles and / or nickel composite oxide particles) as the precursor of the positive electrode active material, for example, when a mixture obtained by mixing a nickel-containing compound (nickel compound) such as nickel hydroxide with a manganese-containing compound (manganese compound), or particles obtained by coating a manganese compound on a nickel compound, and a lithium compound are mixed and sintered, the distribution of manganese in the obtained positive electrode active material sometimes becomes uneven, and the above-mentioned effect cannot be fully obtained.
[0096] (Composition of Nickel Composite Hydroxide Particles)
[0097] The nickel composite hydroxide particles contain nickel, manganese and an arbitrary element M, and the atomic ratio (2) of each element is represented by Ni:Mn:M=(1-ab):a:b, wherein 0.05≦a≦0.6, 0≦b≦0.6, 0.33<(1-ab), and M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta.
[0098] Nickel composite hydroxide particles can be, for example, represented by the general formula (2): Ni 1-a-b Mn a M b (OH) 2+β To represent, wherein M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, 0.33<1-ab, 0≦β≦0.4.
[0099] It should be noted that the nickel composite hydroxide particles can also be manufactured by a method other than the crystallization process (step S10) as long as they have the element ratio of the above general formula (2) (also referred to as "element ratio (2)"). However, from the perspective of making the distribution of the metal elements contained in the positive electrode active material more uniform and facilitating the control of the amount of dissolved lithium within the desired range, it is preferably obtained by the crystallization process (step S10).
[0100] The crystallization process (step S10) is not particularly limited as long as it is a method for obtaining the nickel composite hydroxide particles represented by the above-mentioned element ratio (2), and the following method can be used appropriately. First, an alkaline aqueous solution is added to a mixed aqueous solution containing a nickel salt, a manganese salt and a salt of any element M to form a reaction aqueous solution. Then, the reaction aqueous solution is stirred at a certain speed, and the nickel composite hydroxide particles are coprecipitated in the reaction aqueous solution and crystallized by controlling the pH and temperature of the reaction aqueous solution within a certain range. Below, each material used in the crystallization process and suitable crystallization conditions are described.
[0101] (Mixed aqueous solution)
[0102] The mixed aqueous solution uses, for example, a sulfate solution, a nitrate solution, a chloride solution, etc. The composition of the metal elements contained in the mixed aqueous solution is almost the same as the composition of the metal elements contained in the obtained nickel composite hydroxide particles. Therefore, the composition of the metal elements in the mixed aqueous solution can be modulated to be the same as the composition of the metal elements of the target nickel composite hydroxide.
[0103] (Alkaline aqueous solution)
[0104] As the aqueous alkali solution, for example, sodium hydroxide, potassium hydroxide or the like is used.
[0105] (Complementing agent)
[0106] A ligand may be added to the mixed aqueous solution together with the alkaline aqueous solution. The ligand is not particularly limited, as long as it can combine with nickel ions or other metal ions in the aqueous solution to form a coordination compound, and for example, an ammonium ion donor may be cited. The ammonium ion donor is not particularly limited, and for example, ammonia, ammonium sulfate, ammonium chloride, ammonium carbonate, ammonium fluoride, etc. may be used.
[0107] (Temperature and pH of the reaction aqueous solution)
[0108] It should be noted that the above-mentioned ammonium ion donor and other ligands may not be used in the crystallization step (step S10). That is, the ammonium ion concentration may not be controlled within a specified range in the crystallization step. When a ligand is not used, the temperature of the reaction aqueous solution is preferably in the range of more than 60°C and less than 80°C, and the pH of the reaction aqueous solution at the above temperature is preferably 10 or more and less than pH 12 (25°C reference).
[0109] When the pH of the reaction tank (reaction aqueous solution) exceeds 12 for crystallization, the nickel composite hydroxide particles will become fine particles, the filterability will also deteriorate, and sometimes spherical particles cannot be obtained. On the other hand, when the pH is less than 10, the generation rate of the nickel composite hydroxide particles will be significantly slowed down, Ni will remain in the filtrate, the amount of Ni precipitation will deviate from the target composition, and sometimes nickel composite hydroxide particles of the target ratio cannot be obtained.
[0110] In addition, when the temperature of the reaction aqueous solution exceeds 60°C, the solubility of Ni can be avoided from increasing, and the amount of Ni precipitation deviates from the target composition and the phenomenon of being unable to coprecipitate cannot be avoided. On the other hand, when the temperature of the reaction aqueous solution exceeds 80°C, the evaporation of water is large, so the slurry concentration becomes high, the solubility of Ni decreases, and in addition, crystals such as sodium sulfate are generated in the filtrate, the impurity concentration is increased, etc., and the charge and discharge capacity of the positive electrode active material may decrease.
[0111] On the other hand, when an ammonium ion donor such as ammonia is used as a complexing agent, the solubility of Ni increases, so the pH of the reaction aqueous solution is preferably 10 to 13, and the temperature of the reaction aqueous solution is preferably 30° C. to 60° C.
[0112] It should be noted that the above-mentioned pH and temperature are preferably constant values from the viewpoint that the composition of the obtained nickel composite hydroxide particles becomes uniform. For example, the pH fluctuation range is preferably within ±0.4, more preferably within ±0.3. When the pH fluctuation range is large, the crystallization reaction will be unstable, and sometimes nickel composite hydroxide particles with uniform composition cannot be obtained.
[0113] (Ammonium ion concentration)
[0114] The ammonium ion concentration in the reaction aqueous solution preferably remains as a fixed value in the scope of more than 3g / L and less than 25g / L. When the ammonium ion concentration is less than 3g / L, the solubility of the metal ion can not be maintained as certain, therefore, the primary particle of the plate-like hydroxide of neat shape and particle diameter can not be formed, and it is easy to generate the core of gelatinous, so that the particle size distribution is easy to broaden. On the other hand, when the ammonium ion concentration exceeds 25g / L, the solubility of the metal ion becomes too large, and the amount of metal ions remaining in the reaction aqueous solution increases, and becomes easy to cause the deviation of composition etc.
[0115] In addition, when the ammonium ion concentration changes, the solubility of the metal ions changes, and nickel composite hydroxide particles with a uniform composition cannot be formed, so it is preferably maintained at a constant value. For example, the ammonium ion concentration is preferably maintained at a desired concentration with an upper and lower limit of about 5 g / L.
[0116] (Dissolved oxygen concentration)
[0117] The dissolved oxygen concentration in the reaction aqueous solution is preferably adjusted to a range of 0.2 mg / L or more and 8.0 mg / L or less. By controlling the dissolved oxygen concentration within the above range, suitable nickel composite hydroxide particles can be obtained as a precursor of the positive electrode active material. It should be noted that in the crystallization step (step S10), from the viewpoint that the composition of the obtained nickel composite hydroxide particles becomes uniform, the dissolved oxygen concentration is preferably controlled within a certain range. The variation range of the dissolved oxygen concentration is preferably within ±0.2 mg / L, more preferably within ±0.1 mg / L.
[0118] It should be noted that the dissolved oxygen concentration can be measured by methods such as the Winkler method (chemical analysis method), the diaphragm permeation method (electrochemical method), and the fluorescence determination method. It should be noted that the dissolved oxygen concentration in the reaction aqueous solution can be adjusted by, for example, introducing gases such as inert gases (e.g., N2 gas, Ar gas, etc.) into the reaction tank and controlling the flow rate and composition of these gases. It should be noted that these gases can also flow through the space in the reaction tank, or can be blown into the reaction aqueous solution. In addition, it is preferred that the reaction aqueous solution is stirred with a proper amount of power within the range described later by using a stirring device such as a stirring blade, so that the overall dissolved oxygen concentration of the reaction aqueous solution is more uniform.
[0119] (Filtration and washing of crystallized product)
[0120] Then, after reaching a stable state, the crystallized product (precipitate) is collected, filtered, and washed with water to obtain nickel composite hydroxide particles. Alternatively, a mixed aqueous solution and an alkaline aqueous solution and an aqueous solution containing an ammonium ion donor according to the situation can be continuously supplied, overflowed from the reaction tank, and the precipitate is collected, filtered, and washed with water to obtain nickel-manganese composite hydroxide particles.
[0121] (Addition of element M)
[0122] When the nickel composite hydroxide particles contain element M (at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta), as a method of blending element M, from the viewpoint of improving the productivity of the crystallization process, a method of co-precipitating nickel manganese composite hydroxide particles (containing element M) by adding an aqueous solution containing element M to the above-mentioned mixed aqueous solution containing nickel and manganese is preferred.
[0123] As an aqueous solution containing element M, for example, an aqueous solution containing cobalt sulfate, sodium tungstate, tungsten oxide, molybdenum oxide, molybdenum sulfide, vanadium pentoxide, magnesium sulfate, magnesium chloride, calcium chloride, aluminum sulfate, sodium aluminate, titanium sulfate, ammonium peroxytitanate, potassium titanium oxalate, zirconium hydroxide, zirconium sulfate, chromium chloride, sodium tantalate, tantalic acid, etc. can be used.
[0124] The element M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, and can be added arbitrarily to improve thermal stability, storage characteristics, battery characteristics, etc.
[0125] Furthermore, in order to optimize the crystallization conditions and to easily control the composition ratio, a coating step of coating the element M may be provided after adding an aqueous alkali solution to a mixed aqueous solution containing at least nickel and manganese to cause crystallization.
[0126] The coating method is not particularly limited and a known method can be used. For example, 1) a method of coating the element M on a nickel composite hydroxide by adding an aqueous alkali solution to a mixed aqueous solution containing nickel and manganese (which does not contain the element M) to cause it to crystallize, or 2) a method of preparing a mixed aqueous solution containing nickel, manganese and a portion of the element M, coprecipitating nickel composite hydroxide particles (containing the element M), and then coating the coprecipitate with the element M to adjust the M content.
[0127] Hereinafter, an example of a coating method for element M is described. First, the composite hydroxide particles obtained by crystallization are dispersed in pure water to form a slurry. Next, a solution containing M that meets the target coating amount is mixed in the slurry, and an acid is dropped to reach a specified pH and adjusted. As an acid, for example, sulfuric acid, hydrochloric acid, nitric acid, etc. are used. Next, after the slurry is mixed for a specified time, the slurry is filtered and the residue is dried, and composite hydroxide particles coated with element M can be obtained. It should be noted that, as other coating methods, a spray drying method in which a solution containing a compound containing M is sprayed onto the composite hydroxide particles and then dried, a method in which a solution containing a compound containing M is impregnated into the composite hydroxide particles, etc. can be cited.
[0128] It should be noted that the crystallization process (step S10) can use a batch crystallization method or a continuous crystallization method. For example, in the batch crystallization method, after the reaction aqueous solution in the reaction tank reaches a stable normal state, the precipitate is collected, filtered, and washed with water to obtain nickel composite hydroxide particles. In addition, in the continuous crystallization method, a mixed aqueous solution and an alkaline aqueous solution and an aqueous solution containing an ammonium ion donor according to the situation are continuously supplied, and the precipitate is collected from the overflow of the reaction tank, filtered, and washed with water to obtain composite hydroxide particles.
[0129] [Heat treatment process (step S11)]
[0130] It should be noted that the manufacturing method of this embodiment may further include a step of heat treating the nickel composite hydroxide particles (step S11) before the mixing step (step S20) described later (see Figure 2). By heat treatment, at least a portion of the water contained in the nickel composite hydroxide particles is removed. By removing at least a portion of the water remaining in the nickel composite hydroxide particles, it is possible to prevent the deviation of Li / Me of the positive electrode active material obtained through the calcination step (step S30). In addition, by heat treating the nickel composite hydroxide particles, nickel composite oxide particles having the same atomic ratio as the above-mentioned element ratio (2) of the metal elements can also be obtained.
[0131] The heat treatment only needs to be heated to a temperature at which the residual moisture in the nickel composite hydroxide particles can be removed. For example, the temperature of the heat treatment is preferably above 105°C and below 700°C. When the nickel composite hydroxide particles are heated to above 105°C, at least a portion of the residual moisture can be removed. It should be noted that when the temperature of the heat treatment is lower than 105°C, a long time is required to remove the residual moisture, and therefore it is not suitable for industry. On the other hand, when the temperature of the heat treatment exceeds 700°C, the particles converted into composite oxide particles sometimes sinter and agglomerate. For example, when most of the nickel composite hydroxide particles are converted into nickel composite oxide particles, the temperature of the heat treatment is preferably above 350°C and below 700°C.
[0132] The atmosphere for heat treatment is not particularly limited, for example, from the viewpoint of easy operation, it is preferably carried out in air flow. In addition, the time of heat treatment is not particularly limited, for example, it can be more than 1 hour. When the time of heat treatment is less than 1 hour, there will be a situation where residual moisture in the composite hydroxide particles cannot be fully removed. In addition, the time of heat treatment is preferably more than 5 hours and less than 15 hours. In addition, the equipment used in the heat treatment is not particularly limited, as long as the composite hydroxide particles can be heated in air flow, for example, an air drier, an electric furnace that does not produce gas, etc. can be suitably used.
[0133] In the heat treatment, for example, the nickel composite hydroxide particles obtained in the crystallization step (step S10) may be heat treated (calcined) to obtain a nickel composite hydroxide having the general formula (3): Ni 1-a-b Mn a M b O 1+β Nickel composite oxide particles represented by the present invention, wherein M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, and 0≦β≦0.4.
[0134] [Mixing process (step S20)]
[0135] Next, at least one of the nickel-manganese composite hydroxide particles and the nickel-manganese composite oxide particles (precursor particles) is mixed with a niobium compound and a lithium compound (step S20). For example, after the heat treatment step (step S11), the obtained precursor particles, niobium compound, and lithium compound are mixed (step S20) to obtain a lithium-niobium mixture.
[0136] The precursor particles contain manganese in the primary particles, so that the lithium-niobium mixture can be sintered at a relatively high temperature. Moreover, by sintering at a high temperature, manganese and niobium can be evenly distributed (solid-dissolved) in the plurality of primary particles of the obtained positive electrode active material. The positive electrode active material containing (solid-dissolved) manganese and niobium in the plurality of primary particles has high thermal stability and reduced conductivity.
[0137] In the mixing process (step S20), as precursor particles, nickel composite hydroxide particles can be used alone, nickel composite oxide particles can be used alone, or nickel composite hydroxide particles and nickel composite oxide particles can be used simultaneously. In addition, as nickel composite oxide particles, nickel composite oxide particles represented by the above general formula (3) can also be used. It should be noted that the nickel-manganese composite oxide particles represented by the above general formula (3) can also be obtained by methods other than heat treatment. In addition, in the mixing process (step S20), one or more selected from the nickel composite hydroxide particles represented by the above general formula (2) and the nickel composite oxide particles represented by the above general formula (3) can also be mixed with the niobium compound and the lithium compound.
[0138] As the niobium compound, a known compound containing niobium can be used, for example, niobic acid, niobium oxide, niobium nitrate, niobium pentachloride, niobium nitrate, etc. can be used. Among these, niobic acid, niobium oxide, or a mixture thereof is preferred from the viewpoint of being easy to obtain and avoiding the mixing of impurities into the lithium metal composite oxide. It should be noted that when impurities are mixed into the lithium metal composite oxide, the thermal stability, battery capacity, and cycle characteristics of the obtained secondary battery will be reduced.
[0139] The niobium compound is preferably mixed in the form of particles (solid phase). When niobium is added in the solid phase, the particle size of the niobium compound changes the reactivity in the subsequent sintering process (step S30), so the particle size of the niobium compound used becomes one of the important factors. The average particle size of the niobium compound is preferably 0.01 μm to 10 μm, more preferably 0.05 μm to 3.0 μm, and further preferably 0.08 μm to 1.0 μm. When the average particle size is less than 0.01 μm, there is a problem that the handling of the powder becomes very difficult, and there is a problem that the niobium compound scatters in the mixing process (step S20) and the sintering process (step S30), resulting in a problem that the desired composition cannot be added to the active material. On the other hand, when the average particle size is greater than 10 μm, Nb is unevenly distributed in the sintered lithium metal composite oxide, and thermal stability cannot be ensured. It should be noted that the average particle size is a volume average particle size MV, which can be obtained based on, for example, a volume integral value measured by a laser diffraction scattering particle size distribution meter.
[0140] The niobium compound can be pulverized in advance using various pulverizers such as a ball mill, a planetary ball mill, a jet mill / nano jet mill, a bead mill, a pin mill, etc. to achieve the above-mentioned particle size range. In addition, the niobium compound can also be classified by a dry classifier or a sieve as needed. For example, the niobium compound can be sieved to obtain particles close to 0.01 μm.
[0141] The lithium compound is not particularly limited, and known compounds containing lithium can be used, for example, lithium carbonate, lithium hydroxide, lithium nitrate or a mixture thereof, etc. Among these, lithium carbonate, lithium hydroxide or a mixture thereof is preferred from the viewpoint of reducing the influence of residual impurities and melting at the firing temperature.
[0142] The mixing method of the precursor particles with the lithium compound and the niobium compound is not particularly limited, as long as the precursor particles, the lithium compound and the niobium compound are fully mixed to the extent that the skeleton of the precursor particles is not destroyed. As a mixing method, for example, a general mixer can be used for mixing, for example, a shaking mixer, a Lediger mixer, a Julia mixer, a V-type mixer, etc. can be used for mixing. It should be noted that the lithium-niobium mixture is preferably fully mixed before the sintering process (step S30) described later. When the mixing is insufficient, the ratio (Li / Me) of Li to the metal element Me other than Li between the particles of the positive electrode active material fluctuates, and there is a situation where problems such as insufficient battery characteristics are obtained.
[0143] The lithium compound is mixed so that the Li / Me in the lithium-niobium mixture is 0.95 or more and 1.2 or less. That is, the mixing is performed so that the Li / Me in the lithium-niobium mixture is the same as the Li / Me in the positive electrode active material to be obtained. This is because the molar ratio of Li / Me and each metal element does not change before and after the sintering process (step S30), so the Li / Me of the lithium-niobium mixture in the mixing process (step S20) becomes the Li / Me of the positive electrode active material. In addition, the niobium compound is mixed so that the niobium content in the lithium-niobium mixture is 0.03 atomic % or more and 3 atomic % or less relative to the total of the metal elements (Ni, Mn, element M, Nb) other than Li in the lithium-niobium mixture.
[0144] It should be noted that the mixing step (step S20) may include, for example, a crystallization step (step S10) of obtaining precursor particles by crystallization, a niobium coating step of mixing the obtained precursor particles with water, adding a niobium salt solution and an acid to the obtained slurry to obtain precursor particles coated with a niobium compound, and a step of mixing the precursor particles coated with a niobium compound with a lithium compound to obtain a lithium-niobium mixture. It should be noted that the niobium compound may be added in a solid phase or through the above-mentioned niobium coating step, and solid phase addition is preferred in industry from the viewpoint of productivity.
[0145] [Pre-firing process (step S25)]
[0146] When lithium hydroxide or lithium carbonate is used as a lithium compound, before the sintering process (step S30) described later, the lithium-niobium mixture is preferably kept at a temperature lower than the sintering temperature and between 350°C and 800°C, preferably between 450°C and 780°C, for pre-sintering. The time for maintaining the above-mentioned pre-sintering temperature is, for example, between 1 hour and 10 hours, preferably between 3 hours and 6 hours. During the pre-sintering, the diffusion of lithium into the nickel composite hydroxide particles is fully carried out, and a more uniform lithium metal composite oxide can be obtained. For example, when lithium carbonate is used as a lithium compound, it is preferably pre-sintered at a temperature between 400°C and 700°C for between 1 hour and 10 hours.
[0147] [Firing process (step S30)]
[0148] Next, the obtained lithium-niobium mixture is calcined (step S30). Through calcination, the lithium in the lithium compound diffuses into the precursor particles, thereby forming a lithium metal composite oxide (positive electrode active material) formed by particles with a polycrystalline structure. The lithium compound melts at the temperature during calcination and penetrates into the nickel composite hydroxide particles to form a lithium metal composite oxide. At this time, the niobium compound penetrates into the secondary particles of the precursor particles together with the molten lithium compound. In addition, if there are grain boundaries inside the primary particles, they will also penetrate. Thereby, the diffusion of niobium inside the primary particles is promoted, and at least a portion of niobium is solid-dissolved in the primary particles in the obtained lithium metal composite oxide. In addition, a portion of the niobium compound is also formed on the surface of the primary particles as a lithium niobium compound.
[0149] (Firing temperature)
[0150] The calcination temperature of the lithium-niobium mixture is preferably 850° C. to 1000° C., more preferably 900° C. to 950° C. When the calcination temperature is within the above range, melting of the lithium compound occurs, while the penetration and diffusion of the niobium compound are promoted. In addition, by increasing the temperature, the diffusion of niobium is promoted, and the crystallinity of the lithium metal composite oxide is improved, which can improve the output characteristics and energy density.
[0151] On the other hand, when the calcination temperature is less than 850°C, the diffusion of lithium and niobium in the nickel composite hydroxide particles may not be sufficient, unreacted lithium compounds and niobium compounds may remain, the crystal structure of the lithium metal composite oxide may not be fully complete, and the battery characteristics may be reduced. On the other hand, when the calcination temperature exceeds 1000°C, the particles of the lithium metal composite oxide may be sintered violently, and abnormal grain growth may occur. When abnormal grain growth occurs, the particles after calcination may become coarse and the particle shape may not be maintained, the specific surface area of the positive electrode active material may decrease, the positive electrode resistance of the secondary battery may increase, and the battery capacity may decrease.
[0152] (Firing time)
[0153] The calcination time is not particularly limited as long as the sintering reaction between the precursor particles and the lithium compound proceeds sufficiently, and is, for example, 1 hour or longer, preferably 3 hours or longer and 24 hours or shorter. If the calcination time is less than 1 hour, the formation of the lithium metal composite oxide may not proceed sufficiently.
[0154] (Firing atmosphere)
[0155] The atmosphere during firing is an oxidizing atmosphere. Here, an oxidizing atmosphere refers to an atmosphere in which the oxygen concentration is 3% by volume or more and 100% by volume or less. When the oxygen concentration of the firing atmosphere is less than 3% by volume, the obtained positive electrode active material cannot be fully oxidized, and the crystallinity of the lithium metal composite oxide may become insufficient. In addition, firing is preferably carried out in the atmosphere or in an oxygen flow, and is preferably carried out in an oxygen flow from the viewpoint of improving battery characteristics.
[0156] (Firing furnace)
[0157] The furnace (firing furnace) used for the sintering is not particularly limited, as long as the lithium-niobium mixture can be fired in an atmosphere to oxygen flow. The sintering furnace is preferably an electric furnace that does not generate gas. In addition, the sintering furnace can be a batch type furnace or a continuous type furnace.
[0158] The lithium metal composite oxide obtained after calcination can be used as a positive electrode active material. In addition, although the lithium metal composite oxide obtained after calcination suppresses sintering between particles, it sometimes forms coarse particles through weak sintering and agglomeration. In this case, the above sintering and agglomeration can be eliminated by crushing, and the particle size distribution can be adjusted to use it as a positive electrode active material.
[0159] [Amount of dissolved lithium]
[0160] The positive electrode active material (lithium metal composite oxide) obtained after the calcination step (step S30) is adjusted so that the amount of lithium dissolved in water when the positive electrode active material is immersed in water (dissolved lithium amount) obtained by neutralization titration is 0.02 mass % or more and 0.10 mass % or less relative to the total positive electrode active material. When the dissolved lithium amount is within the above range, niobium can be uniformly distributed inside and / or on the surface of the primary particles of the positive electrode active material, inhibiting the gelation of the positive electrode paste and further improving the battery characteristics of the secondary battery.
[0161] In addition, from the viewpoint of further improving battery characteristics, the lower limit of the amount of dissolved lithium in the positive electrode active material is preferably 0.03% by mass or more, and more preferably 0.04% by mass or more. When the lower limit of the amount of dissolved lithium is too small, lithium niobium compounds may be excessively or unevenly formed on the surface of the primary particles of the lithium metal composite oxide, thereby reducing the battery capacity.
[0162] In addition, as described above, the amount of dissolved lithium is a value that varies according to the composition and manufacturing method of the positive electrode active material. The amount of dissolved lithium of the positive electrode active material involved in this embodiment is preferably adjusted so that, for example, the amount of dissolved lithium of the positive electrode active material manufactured under the same manufacturing conditions other than the unmixed niobium compound is lower by 0.03% by mass or more, and more preferably adjusted to be lower by 0.04% by mass or more. When the amount of dissolved lithium is reduced to the above range, it can be considered that niobium is uniformly distributed inside and / or on the surface of the primary particles of the positive electrode active material.
[0163] It should be noted that the amount of dissolved lithium can be calculated by the following method: weigh 5 g of the positive electrode active material, put it into 100 ml of pure water at 25°C, immerse it, stir it for 30 minutes and then filter it, use HCl aqueous solution to neutralize and titrate the filtrate, and calculate the amount of lithium dissolved in the pure water (mass % relative to the total mass of the positive electrode active material).
[0164] The amount of dissolved lithium can be controlled within the above range by the following method, namely, in the manufacturing process of the positive electrode active material, manganese and niobium are contained within a specific range and in the crystallization process (step S10), the dissolved oxygen concentration in the reaction solution, the temperature of the reaction solution, etc. are adjusted, in the sintering process (step S30), the sintering temperature, etc. are adjusted, and a pre-sintering process is added before the sintering process (step S30).
[0165] 3. Evaluation method of positive electrode active materials for non-aqueous electrolyte secondary batteries
[0166] The evaluation method of the positive electrode active material for the non-aqueous electrolyte secondary battery according to the present embodiment (hereinafter also referred to as "the evaluation method of the positive electrode active material") is as follows: Figure 3 As shown, it includes determining the amount of lithium dissolved in water when immersed in water (hereinafter also referred to as "dissolved lithium amount") obtained by neutralization titration (step S40); and selecting a positive electrode active material having a dissolved lithium amount of 0.02% by mass or more and 0.10% by mass or less relative to the total positive electrode active material (step S50). Through the evaluation method of this embodiment, it is possible to simply select a positive electrode active material that can suppress gelation during the preparation of the positive electrode paste and obtain a secondary battery with a high battery capacity. It should be noted that step S50 can also be included in the above-mentioned method for manufacturing the positive electrode active material.
[0167] In addition, the positive electrode active material used in the evaluation method of this embodiment is represented by the general formula (1): Li d Ni 1-a-b- c Mn a M b Nb c O 2+α The lithium nickel manganese composite oxide represented by is formed, wherein M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.2, 0.33<(1-abc), 0≦α≦0.4. It should be noted that the preferred range and preferred characteristics of each element constituting the above general formula (1) are the same as those of the above positive electrode active material.
[0168] [Step of measuring the amount of eluted lithium (step S40)]
[0169] First, the amount of lithium dissolved in water when the positive electrode active material as the evaluation object is immersed in water (dissolved lithium amount) is determined by neutralization titration. The dissolved lithium amount can be obtained by the following method: weigh 5g of the positive electrode active material, put it into 100ml of pure water at 25°C, immerse it, stir it for 30 minutes, filter it, and use HCl aqueous solution to neutralize and titrate the filtrate to calculate the amount of lithium dissolved in pure water (mass % relative to the total mass of the positive electrode active material).
[0170] In the positive electrode active material represented by the general formula (1), when niobium is uniformly present inside and / or on the surface of the primary particles, the amount of eluted lithium in the obtained positive electrode active material can be reduced. Therefore, by measuring the amount of eluted lithium, the existing form of niobium can be indirectly evaluated.
[0171] [Positive Electrode Active Material Selection Step (Step S50)]
[0172] Next, a positive electrode active material having a lithium amount dissolved in water (dissolved lithium amount) of 0.02 mass % or more and 0.10 mass % or less relative to the total positive electrode active material is selected. By selecting a positive electrode active material having a lithium amount dissolved in the above range, the gelation of the positive electrode paste can be suppressed and a positive electrode active material with high battery characteristics can be easily obtained with high productivity.
[0173] In addition, as described above, the amount of dissolved lithium is a value that varies according to the composition and manufacturing method of the positive electrode active material. It is preferred to select the following positive electrode active material, that is, the amount of dissolved lithium of the positive electrode active material involved in the present embodiment is, for example, 0.03% by mass or more lower than the amount of dissolved lithium of the positive electrode active material manufactured under the same manufacturing conditions other than the unmixed niobium compound, and more preferably 0.04% by mass or more lower. When selecting a positive electrode active material with a dissolved lithium amount in the above range, it can be considered that niobium is uniformly distributed inside and / or on the surface of the primary particles of the positive electrode active material, and a positive electrode active material with high battery characteristics can be easily obtained with high productivity.
[0174] 4. Non-aqueous electrolyte secondary battery
[0175] The non-aqueous electrolyte secondary battery (hereinafter also referred to as "secondary battery") of this embodiment uses the above-mentioned positive electrode active material in the positive electrode. Below, for an example of the secondary battery of this embodiment, each component is described separately. The secondary battery of this embodiment includes a positive electrode, a negative electrode and a non-aqueous electrolyte, and is composed of the same components as a general lithium-ion secondary battery. It should be noted that the embodiments described below are only examples, and the non-aqueous electrolyte secondary battery is represented by the following embodiments, which can be implemented in various modified and improved ways based on the knowledge of those skilled in the art. In addition, the secondary battery is not particularly limited in its use.
[0176] (positive electrode)
[0177] The positive electrode of the secondary battery is made using the above-mentioned positive electrode active material. An example of a method for making a positive electrode is described below. First, the above-mentioned positive electrode active material (powdered), a conductive material and a binder are mixed, and then activated carbon, a target solvent for viscosity adjustment, etc. are added as needed, and the mixture is kneaded to make a positive electrode mixture paste (also called "positive electrode paste").
[0178] The mixing ratio of each material in the positive electrode mixture becomes a factor that determines the performance of the lithium secondary battery, and can be adjusted according to the purpose. The mixing ratio of the materials can be the same as that of the positive electrode of a known lithium secondary battery, for example, when the total mass of the solid content of the positive electrode mixture excluding the solvent is 100 mass%, it can contain 60 to 95 mass% of the positive electrode active material, 1 to 20 mass% of the conductive material and 1 to 20 mass% of the binder.
[0179] The obtained positive electrode mixture paste is applied to the surface of a collector such as aluminum foil, dried, and the solvent is dispersed to produce a sheet-like positive electrode. As required, the electrode density can also be increased by pressurization such as roller pressing. The sheet-like positive electrode thus obtained can be cut into appropriate sizes according to the target battery, etc., and used for the production of the battery. Among them, the production method of the positive electrode is not limited to the above-mentioned examples, and other methods can be used.
[0180] As the conductive material, for example, graphite (natural graphite, artificial graphite, expanded graphite, etc.), carbon black materials such as acetylene black and Ketjen black, etc. can be used.
[0181] As a binder, which plays a role of binding the active material particles, for example, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), fluorine rubber, ethylene propylene diene rubber, styrene butadiene, cellulose resin, polyacrylic acid, etc. can be used.
[0182] As required, the positive electrode active material, the conductive material and the activated carbon are dispersed, and the solvent in which the binder is dissolved is added to the positive electrode mixture. As the solvent, specifically, an organic solvent such as N-methyl-2-pyrrolidone can be used. In addition, in order to increase the double layer capacity, activated carbon can be added to the positive electrode mixture.
[0183] (negative electrode)
[0184] The negative electrode can use metallic lithium, lithium alloy, etc. In addition, the negative electrode can also be formed by mixing a binder with a negative electrode active material that can absorb and release lithium ions, adding an appropriate solvent to form a paste-like negative electrode mixture, applying the negative electrode mixture to the surface of a metal foil collector such as copper, drying, and compressing to increase the electrode density as needed.
[0185] As the negative electrode active material, for example, a sintered body of an organic compound such as natural graphite, artificial graphite, and phenolic resin, and a powder of a carbon material such as coke can be used. In this case, as the negative electrode binder, a fluorine-containing resin such as PVDF can be used in the same manner as the positive electrode, and as a solvent for dispersing these active materials and the binder, an organic solvent such as N-methyl-2-pyrrolidone can be used.
[0186] (Diaphragm)
[0187] A separator is disposed between the positive electrode and the negative electrode. The separator is a material that separates the positive electrode and the negative electrode and holds an electrolyte. A known separator can be used, for example, a film made of polyethylene, polypropylene, or the like, and a film having micropores can be used.
[0188] (Non-aqueous electrolyte)
[0189] Non-aqueous electrolyte, for example, has non-aqueous electrolyte, solid electrolyte etc. Non-aqueous electrolyte is formed by dissolving lithium salt as supporting salt in organic solvent. As organic solvent, cyclic carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate and trifluoropropylene carbonate can be used alone, in addition, chain carbonates such as diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate and dipropyl carbonate, and then, ether compounds such as tetrahydrofuran, 2-methyltetrahydrofuran and dimethoxyethane, sulfur compounds such as ethylmethyl sulfone, butane sultone, phosphorus compounds such as triethyl phosphate and trioctyl phosphate, etc., selected from one, or mixed two or more use.
[0190] As supporting salts, LiPF6, LiBF4, LiClO4, LiAsF6, LiN(CF3SO2)2, and complex salts thereof can be used. Furthermore, the non-aqueous electrolyte may further contain a radical scavenger, a surfactant, a flame retardant, and the like.
[0191] (Shape and structure of secondary battery)
[0192] As described above, the nonaqueous electrolyte secondary battery of the present invention, which is composed of the positive electrode, negative electrode, separator and nonaqueous electrolyte, can be in various shapes such as cylindrical and stacked. Even if any shape is adopted, the positive electrode and the negative electrode are stacked through the separator to form an electrode body, the obtained electrode body is impregnated with the nonaqueous electrolyte, and the positive electrode collector and the positive terminal connected to the outside and the negative electrode collector and the negative terminal connected to the outside are connected using a collector lead, etc., and are sealed in a battery box to complete the nonaqueous electrolyte secondary battery.
[0193] (Characteristics of Secondary Batteries)
[0194] The secondary battery involved in this embodiment can take into account high battery capacity and durability as well as high thermal stability caused by suppressing oxygen release during overcharging. In addition, the positive electrode active material used in the secondary battery involved in this embodiment can be obtained by the above-mentioned industrial manufacturing method. Therefore, the secondary battery involved in this embodiment can be suitable for power supplies for small portable electronic machines (notebook personal computers, mobile phone terminals, etc.) that usually require high capacity, power supplies for electric vehicles, power supplies for hybrid vehicles, etc.
[0195] Example
[0196] Hereinafter, the present invention will be described in more detail by way of the embodiments and comparative examples of the present invention, but the present invention is not limited to these embodiments. It should be noted that the analysis methods of the metals contained in the positive electrode active material in the embodiments and comparative examples and the various evaluation methods of the positive electrode active material are as follows.
[0197] (1) Composition analysis
[0198] The compositions of the obtained nickel-manganese composite hydroxide and the positive electrode active material were measured by ICP emission spectrometry.
[0199] (2) Average particle size MV
[0200] The average particle size (volume average particle size MV) was measured using a laser diffraction scattering particle size distribution analyzer (Microtrac HRA, manufactured by Nikkiso Co., Ltd.).
[0201] (3) Grain size and detection of lithium niobium compounds
[0202] The crystal structure of the obtained positive electrode active material and the qualitative evaluation of the lithium niobium compound were performed using an XRD diffractometer (manufactured by PANalytical, X'PertPRO). In addition, the grain size of the (003) plane was analyzed based on the XRD measurement results of the peak of the (003) plane existing near 2θ=18° and calculated using the Scherrer formula.
[0203] (4) Niobium concentration
[0204] The positive electrode active material is processed into a primary particle cross-sectional analysis that can be performed by S-TEM. Select any 30 primary particles from the multiple secondary particles contained in the positive electrode active material, and perform line analysis on the cross-sectional composition of each primary particle by EDX of S-TEM. At this time, the direction of line analysis is selected in a direction that does not affect the measured value of the niobium concentration near the surface of the primary particle due to the presence of niobium compounds on the surface of the primary particle when the surface analysis is performed in advance, and can be analyzed in a direction of more than 50% of the maximum length of the primary particle. Based on the measured value of the niobium concentration obtained by line analysis, the maximum niobium concentration and the average niobium concentration in the primary particle are obtained, and the ratio of the maximum niobium concentration of each primary particle is calculated respectively. Furthermore, the ratio of the maximum niobium concentration of the positive electrode active material is obtained by averaging the ratio of the maximum niobium concentration calculated from each primary particle.
[0205] (5) Amount of lithium dissolved
[0206] The amount of dissolved lithium is calculated as follows: 5 g of the crushed positive electrode active material is weighed, put into 100 ml of pure water at 25°C, immersed, stirred for 30 minutes and then filtered, and the filtrate is neutralized and titrated with HCl aqueous solution to calculate the amount of lithium dissolved in pure water (mass % relative to the total mass of the positive electrode active material).
[0207] (6) Initial charge capacity and initial discharge capacity
[0208] For the initial charge capacity and initial discharge capacity, make Figure 4 The button-type battery CBA (2032 button battery) shown in the figure was placed for about 24 hours. After the open circuit voltage (OCV) stabilized, the positive electrode was charged with a current density of 0.1 mA / cm 2 The initial charge capacity was taken as the cut-off voltage of 4.3 V, and after standing for 1 hour, the capacity when the cut-off voltage was discharged to 3.0 V was taken as the initial discharge capacity. The discharge capacity was measured using a multi-channel voltage / current generator (R6741A, manufactured by Advantest Corporation).
[0209] The button-type battery CBA was prepared by the following method. First, 52.5 mg of the obtained positive electrode active material, 15 mg of acetylene black and 7.5 mg of polyvinylidene fluoride resin (PTFE) were mixed and compressed at a pressure of 100 MPa to form a 11 mm diameter and 100 μm thickness battery. Figure 4The positive electrode (evaluation electrode) PE shown. After the prepared positive electrode PE was dried in a vacuum dryer at 120°C for 12 hours, the positive electrode PE was used to make a button-type battery CBA in an Ar atmosphere glove box with a dew point managed to -80°C. The negative electrode NE used lithium (Li) metal with a diameter of 17 mm and a thickness of 1 mm, and the electrolyte used an equal mixture of 1M ethylene carbonate (EC) and diethyl carbonate (DEC) with LiClO4 as the supporting electrolyte (manufactured by Toyama Pharmaceutical Industry Co., Ltd.). The separator SE used a polyethylene porous membrane with a film thickness of 25 μm. In addition, the button-type battery CBA has a gasket GA and a corrugated sheet WW, and is assembled into a button-type battery using a positive electrode can PC and a negative electrode can NC.
[0210] (7) Evaluation of the stability of positive electrode paste
[0211] 25.0 g of positive electrode active material, 1.5 g of carbon powder of conductive material, 2.9 g of polyvinylidene fluoride (PVDF) and N-methyl-2-pyrrolidone (NMP) were mixed with a planetary motion mixer to obtain a positive electrode composite paste. The amount of N-methyl-2-pyrrolidone (NMP) added was adjusted so that the viscosity obtained by the viscosity measurement method of the vibration viscometer specified in JIS Z8803: 2011 was 1.5 to 2.5 Pa·s. The obtained paste was stored for 76 hours, and the occurrence of gelation was visually evaluated. When no gelation occurred, it was recorded as "○", and when gelation occurred, it was recorded as "×".
[0212] [Example 1]
[0213] (Crystallization process)
[0214] A prescribed amount of pure water is added to a reaction tank (60 L), and the temperature in the tank is set to 70°C while stirring. At this time, N2 gas is flowed into the reaction tank so that the dissolved oxygen concentration in the reaction tank liquid is a certain value in the range of 0.2 mg / L to 0.8 mg / L. Furthermore, N2 gas is also supplied to the reaction tank during the crystallization process, and adjustment is performed so that the dissolved oxygen concentration in the reaction tank liquid is maintained at a certain value in the range of 0.2 mg / L to 0.8 mg / L throughout the crystallization process. A 2.0 M mixed aqueous solution of nickel sulfate, cobalt sulfate, and manganese sulfate and a 25 mass% sodium hydroxide solution as an alkaline solution are continuously added to the reaction tank simultaneously so that the molar ratio of nickel:cobalt:manganese in the reaction tank is 55:25:20.
[0215] It should be noted that before the 2.0M mixed aqueous solution of nickel sulfate, cobalt sulfate and manganese sulfate and the 25 mass % sodium hydroxide solution are added to the reaction tank, N2 gas is flowed in so that the dissolved oxygen concentration of each solution (the mixed aqueous solution, the sodium hydroxide solution) is adjusted to a certain value in the range of 0.2 mg / L or more and 0.8 mg / L or less. In the crystallization process, N2 gas is also supplied to adjust so that the dissolved oxygen concentration of each solution is maintained at a certain value in the range of 0.2 mg / L or more and 0.8 mg / L or less. In addition, it is adjusted so that the sodium hydroxide solution is heated to 70°C before the addition is started and maintained at 70°C during the addition to the reaction tank.
[0216] The flow rate is controlled so that the residence time of the mixed aqueous solution is 8 hours. In addition, the pH is controlled to be 10.8 to 11.1 (the pH fluctuation range is within 0.3) so that the dissolved nickel concentration in the reaction tank is 350 mg / L. After the reaction tank is stabilized, the slurry containing the nickel-cobalt-manganese composite hydroxide is recovered from the overflow port and filtered to obtain a cake of the nickel-cobalt-manganese composite hydroxide (crystallization process). 140 g of the nickel-cobalt-manganese composite hydroxide in the Denver filter that has been filtered is passed through 1 L of pure water to wash impurities (washing process).
[0217] The filtered powder was placed in a dryer and maintained at 400°C for 5 hours in an air flow of air (oxygen: 21 volume %) for heat treatment to obtain nickel-cobalt-manganese composite hydroxide particles / nickel-cobalt-manganese composite oxide particles (hereinafter also referred to as "precursor particles") represented by a molar ratio of nickel:cobalt:manganese (atomic ratio of 55:25:20).
[0218] (Mixing process)
[0219] The obtained precursor particles, lithium carbonate, and niobic acid (Nb2O5·nH2O) with an average particle size of 1.0 μm were weighed so that the molar ratio of nickel:cobalt:manganese:niobium was 54.6:24.7:19.7:1.0 and the atomic ratio (Li / Me) of lithium to the total metal of nickel, cobalt, manganese, and niobium was 1.03, and then, they were fully mixed using a shaking stirrer device (TURBULA Type T2C manufactured by WAB) to obtain a lithium-niobium mixture.
[0220] (Firing process)
[0221] The obtained lithium-niobium mixture was placed in a sintering furnace and kept at a furnace temperature of 700°C for 3 hours in an air flow of air (oxygen: 21 volume %) for pre-sintering. Then, the furnace temperature was raised to 900°C and kept for 10 hours for sintering. The sintered product was cooled and crushed to obtain lithium-nickel-cobalt-manganese-niobium composite oxide particles (positive electrode active material).
[0222] The volume average particle size MV of the obtained positive electrode active material is shown in Table 1. The results of XRD measurement confirmed that Figure 5 The peak of lithium niobium compound (Li-Nb compound) shown in Figure 1 was also confirmed. In addition, based on the results of STEM-EDX analysis, it was confirmed that niobium was dissolved in the crystal structure and that the maximum niobium concentration inside the primary particles was 1 to 3 times the average niobium concentration inside the primary particles. Furthermore, the grain size of the (003) plane calculated using the Scherrer formula based on the XRD measurement results was 125.5 nm.
[0223] (Evaluation of electrochemical characteristics)
[0224] The battery characteristics (initial charge and discharge capacity) of the secondary battery using the obtained positive electrode active material were evaluated according to the above method.
[0225] [Example 2]
[0226] In the same manner as the crystallization process of Example 1, precursor particles represented by a molar ratio (atomic ratio) of nickel:cobalt:manganese of 60:20:20 are obtained. The obtained precursor particles, lithium carbonate, and niobium acid (Nb2O5·nH2O) with an average particle size of 1.0 μm are weighed so that the molar ratio of nickel:cobalt:manganese:niobium is 59.6:19.7:19.7:1.0 and Li / Me is 1.03, and then, a shaking stirrer device (TURBULA Type T2C manufactured by WAB) is used to fully mix to obtain a lithium-niobium mixture. After the sintering process, the positive electrode active material is obtained and evaluated in the same manner as in Example 1. The XRD measurement results confirm that it belongs to the heterogeneous phase. Figure 5 The peak of the lithium niobium compound shown in FIG. 1 was also confirmed based on the results of EM-EDX analysis. In addition, it was confirmed that niobium was dissolved in the crystal structure and that the maximum niobium concentration inside the primary particles was 1 to 3 times the average niobium concentration inside the primary particles. Other evaluation results are shown in Table 1.
[0227] [Comparative Example 1]
[0228] The positive electrode active material was obtained and evaluated in the same manner as in Example 1 except that the obtained precursor particles and lithium carbonate were weighed and mixed so that the molar ratio of nickel:cobalt:manganese was 55.0:25.0:20.0 and Li / Me was 1.03. The evaluation results are shown in Table 1.
[0229] [Comparative Example 2]
[0230] The obtained precursor particles and lithium carbonate were weighed and mixed so that the molar ratio of nickel:cobalt:manganese was 60.0:20.0:20.0 and Li / Me was 1.03. The positive electrode active material was obtained and evaluated in the same manner as in Example 2. The evaluation results are shown in Table 1. In addition, the XRD pattern obtained by the crystal structure evaluation is shown in Figure 1 .
[0231] [Comparative Example 3]
[0232] The obtained precursor particles, lithium carbonate, and niobic acid (Nb2O5·nH2O) having an average particle size of 1.0 μm were weighed and mixed so that the molar ratio of nickel:cobalt:manganese:niobium was 59.6:19.7:19.7:1.0 and Li / Me was 1.03, and the mixture was calcined by holding the mixture at 820°C for 10 hours in an air flow. The positive electrode active material was obtained and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0233] [Comparative Example 4]
[0234] The obtained precursor particles and lithium carbonate were weighed and mixed so that the molar ratio of nickel:cobalt:manganese was 80.0:10.0:10.0 and Li / Me was 1.03, and the mixture was calcined by holding the mixture at 820°C for 10 hours in a gas flow. The positive electrode active material was obtained and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0235] [Comparative Example 5]
[0236] In addition to weighing the obtained precursor particles, lithium carbonate, niobate (Nb2O5· n H2O) was mixed so that the molar ratio of nickel:cobalt:manganese:niobium was 79.6:9.7:9.7:1.0 and Li / Me was 1.03, and the mixture was calcined at 820°C for 10 hours in a gas flow. The positive electrode active material was obtained and evaluated in the same manner as in Example 1. The evaluation results are shown in Table 1.
[0237] Table 1
[0238]
[0239] (Evaluation results)
[0240] As shown in Table 1, the positive electrode active materials of Examples 1 and 2 eluted less Li than the positive electrode active materials of Comparative Examples 1 and 2 produced under the same conditions except that Nb was not added, indicating that gelation of the positive electrode paste was suppressed during positive electrode production.
[0241] also, Figure 5 : is a diagram showing the XRD patterns of the embodiments and comparative examples. Figure 5 As shown, in the positive electrode active materials of Examples 1 and 2, peaks belonging to lithium niobium compounds as heterogeneous phases were confirmed ( Figure 1 (▼ in the figure indicates a peak corresponding to a different phase). On the other hand, in the positive electrode active material of Comparative Example 1, no peak belonging to the lithium niobium compound was confirmed.
[0242] In the positive electrode active material of the example, it is presumed that the formation of the lithium niobium compound reduces the amount of residual lithium such as unreacted lithium carbonate after calcination, thereby reducing the amount of eluted Li. Therefore, the formation of the lithium niobium compound has the effect of inhibiting gelation.
[0243] Furthermore, the positive electrode active material of Example 2 in which the Ni content in the general formula (1) is 0.55 or more suppresses gelation of the positive electrode paste and exhibits a higher charge and discharge capacity than the positive electrode active material of Comparative Example 2 having the same composition except that it does not contain Nb.
[0244] In addition, the positive electrode active material of Comparative Example 3 was manufactured under the same conditions as Example 2 except for the sintering temperature. However, since the sintering conditions (sintering temperature: less than 850° C.) were not suitable, the reaction between niobic acid and excess lithium could not proceed well and the amount of dissolved Li could not be reduced.
[0245] In addition, the positive electrode active materials of Comparative Examples 4 and 5 were manufactured under the same conditions except that Nb was not added in Comparative Example 4 and Nb was added in Comparative Example 5. However, due to inappropriate sintering conditions (sintering temperature: less than 850°C), the amount of eluted Li was not reduced regardless of whether Nb was added.
[0246] Possibility of industrial application
[0247] In this embodiment, a positive electrode active material for a non-aqueous electrolyte secondary battery having high capacity, durability and thermal stability can be obtained by an industrial manufacturing method. The non-aqueous electrolyte secondary battery is suitable for use as a power source for small portable electronic devices (notebook computers, mobile phone terminals, etc.) that generally require high capacity and high life.
[0248] In addition, the secondary battery of this embodiment is excellent in safety, capacity and durability compared with the existing battery using lithium cobalt oxide or lithium nickel oxide as the positive electrode active material. Therefore, since it can be miniaturized and has a long life, it is suitable for use as a power source for electric vehicles with limited mounting space.
[0249] Furthermore, the positive electrode active material of this embodiment and the secondary battery using the same can be used not only as a power source for electric vehicles driven purely by electrical energy, but can also be used in conjunction with internal combustion engines such as gasoline and diesel engines as a power source for so-called hybrid vehicles or a stationary storage battery.
[0250] It should be noted that the technical scope of the present invention is not limited to the forms described in the above embodiments, etc. One or more of the elements described in the above embodiments, etc. may be omitted. In addition, the elements described in the above embodiments, etc. may be combined as appropriate.
[0251] Explanation of symbols
[0252] CBA…Button battery
[0253] PE…Positive electrode (evaluation electrode)
[0254] NE…Negative electrode
[0255] SE…Diaphragm
[0256] GA...washer
[0257] WW...Corrugated Sheet
[0258] PC…Positive electrode tank
[0259] NC…Cathode tank
Claims
1. A positive electrode active material for a non-aqueous electrolyte secondary battery, comprising a lithium nickel manganese composite oxide formed of secondary particles formed by agglomeration of a plurality of primary particles, The positive electrode active material is represented by the general formula (1): Li d Ni 1-a-b-c Mn a M b Nb c O 2+α express, in, M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, 0.05≦a≦0.6, 0≦b≦0.6, 0.0003≦c≦0.03, 0.95≦d≦1.2, 0.33<(1-abc), 0≦α≦0.4, At least a portion of niobium is dissolved in the primary particles. The amount of lithium dissolved in water after immersing the positive electrode active material in 100 ml of water at 25° C. and stirring for 30 minutes, as determined by a neutralization titration method, is 0.02 mass % or more and 0.10 mass % or less based on the total amount of the positive electrode active material.
2. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1, in, The maximum niobium concentration in the interior of the primary particles is not less than 1 time and not more than 3 times the average niobium concentration in the interior of the primary particles.
3. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or claim 2, in, The positive electrode active material contains a compound containing lithium and niobium, The compound containing lithium and niobium exists on the surface of the primary particles.
4. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or claim 2, in, The crystallite size determined by the Scherrer equation based on the peak of the (003) plane in the X-ray diffraction pattern is 110 nm to 200 nm.
5. The positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 1 or claim 2, in, The volume average particle size MV is 5 μm or more and 20 μm or less.
6. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery, comprising: a step of mixing at least one of nickel-manganese composite hydroxide particles and nickel-manganese composite oxide particles with a niobium compound and a lithium compound, and The step of calcining the lithium-niobium mixture obtained by the mixing; The nickel-manganese composite hydroxide particles and the nickel-manganese composite oxide particles contain nickel, manganese and an arbitrary element M, and the atomic ratio of each metal is represented by Ni:Mn:M=(1-ab):a:b. in, 0.05≦a≦0.6, 0≦b≦0.6, 0.33<(1-ab), M is at least one element selected from Co, W, Mo, V, Mg, Ca, Al, Ti, Cr, Zr and Ta, The lithium-niobium mixture contains 0.03 atomic % to 3 atomic % of niobium relative to all metal elements other than lithium. The positive electrode active material is adjusted so that at least a portion of the niobium is solid-dissolved in the interior of the primary particles, and the amount of lithium dissolved in the water after immersing the positive electrode active material in 100 ml of water at 25° C. and stirring for 30 minutes, as determined by a neutralization titration method, is greater than or equal to 0.02 mass % and less than or equal to 0.10 mass % relative to the total positive electrode active material.
7. The method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6, in, The lithium-niobium mixture is sintered in an oxidizing atmosphere at a temperature of 850° C. to 1000° C.
8. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The maximum niobium concentration is 1 to 3 times the average niobium concentration in the interior of the primary particles.
9. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The calcination is performed so that the crystallite size of the positive electrode active material determined by the Scherrer equation based on the peak of the (003) plane in the X-ray diffraction pattern is 110 nm to 200 nm.
10. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The nickel-manganese composite hydroxide particles are obtained by controlling the pH and ammonium ion concentration of the reaction aqueous solution containing a nickel-containing salt, a manganese-containing salt and a salt containing an arbitrary element M within a predetermined range to perform crystallization, The nickel-manganese composite oxide particles are obtained by heat treating the nickel-manganese composite hydroxide particles obtained by the crystallization.
11. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The niobium compound is niobic acid or niobium oxide, and has an average particle size of 0.01 μm or more and 10 μm or less.
12. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The lithium compound is lithium carbonate.
13. A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to claim 6 or claim 7, in, The nickel-manganese composite oxide particles are obtained by heat-treating the nickel-manganese composite hydroxide particles at a temperature of 105° C. to 700° C. 14 . A nonaqueous electrolyte secondary battery comprising a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode contains the positive electrode active material for a nonaqueous electrolyte secondary battery according to claim 1 .