Sealing sheet

By designing a sealing sheet with a heat-resistant layer with a high glass transition temperature and a soft layer with a low glass transition temperature, the problem of warping of the seal during peeling and cooling at high temperatures is solved, achieving excellent heat resistance. and stability.

CN111718560BActive Publication Date: 2024-10-08NITTO DENKO CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010194878.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-19
Filing Date
2020-03-19
Publication Date
2024-10-08
Estimated Expiration
2040-03-19

AI Technical Summary

Technical Problem

The existing sealing body is easily peeled off when repeatedly heated to high temperatures, and is prone to warping during the cooling process, making it difficult to effectively suppress it.

Method used

A sealing sheet is designed, which contains a two-layer structure: one layer has a glass transition temperature Tg1 of 150°C or more and has excellent heat resistance, and the other layer has a glass transition temperature Tg2 of 80°C or lower. By adjusting the inorganic filler The proportion and composition control the difference in linear expansion coefficient and suppress warpage.

Benefits of technology

The sealing body has excellent heat resistance at high temperatures and is not easy to peel off, and effectively suppresses warpage during the cooling process to ensure the stability and sealing effect of the sealing layer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111718560B_ABST
    Figure CN111718560B_ABST
Patent Text Reader

Abstract

The present invention provides a sealing sheet. The sealing sheet (1) seals an electronic component (21). The sealing sheet (1) has, in order toward one side in the thickness direction: a first layer (2) in contact with the electronic component (21) when the electronic component (21) is sealed, and a second layer (3) exposed to the outside. The first layer (2) and the second layer (3) are each thermosetting. The glass transition temperature Tg1 of the first layer (2) after curing is above 150°C. The glass transition temperature Tg2 of the second layer (3) after curing is below 80°C.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a sealing sheet, and more particularly to a sealing sheet for sealing electronic components. Background Art

[0002] Conventionally, it is known to seal electronic components with a sealing sheet.

[0003] As such a sealing sheet, for example, a resin sheet including an outermost layer and an innermost layer each containing a thermosetting component has been proposed (for example, refer to Patent Document 1 listed below).

[0004] The resin sheet described in Patent Document 1 is placed on an electronic component, and then hot-pressed to embed the electronic component. Next, the resin sheet is thermally cured to form a sealed body (cured sheet).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2018-103584 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, the sealing body (cured sheet) described in Patent Document 1 may be separated from the electronic component when repeatedly heated to high temperatures.

[0010] Furthermore, the resin sheet is required to suppress the warping of the sealed body when cooling the high-temperature sealed body after curing.

[0011] The present invention provides a sealing sheet which has excellent heat resistance after sealing an electronic component and can suppress warping.

[0012] Solutions for solving problems

[0013] The present invention (1) comprises a sealing sheet for sealing an electronic component, wherein the sealing sheet comprises, in order toward one side in the thickness direction: a first layer in contact with the electronic component when the electronic component is sealed, and a second layer exposed to the outside, wherein the first layer and the second layer are each thermosetting, and the glass transition temperature Tg1 of the first layer after curing is above 150°C, and the glass transition temperature Tg2 of the second layer after curing is below 80°C.

[0014] The present invention (2) comprises the sealing sheet according to (1), wherein the first layer contains more than 70% by mass of an inorganic filler, and the second layer contains 70% by mass or less of an inorganic filler.

[0015] The present invention (3) comprises the sealing sheet according to (2), wherein the difference between the ratio of the inorganic filler in the first layer and the ratio of the inorganic filler in the second layer is 50% by mass or less.

[0016] Effects of the Invention

[0017] The sealing sheet of the present invention has excellent heat resistance because the glass transition temperature Tg1 of the cured first layer is as high as 150° C. or more after sealing an electronic component and curing.

[0018] In addition, the glass transition temperature Tg1 of the cured first layer is higher than the above-mentioned glass transition temperature Tg2 of the cured second layer. Therefore, in the process of cooling the cured sealing sheet to room temperature by heating at a high temperature higher than the glass transition temperature Tg1 of the first layer, when the temperature of the cured sealing sheet reaches the glass transition temperature Tg1 of the cured first layer, the cured first layer becomes glass-like, while the cured second layer is still rubber-like. The above-mentioned cooling process is further performed, and when the temperature of the cured sealing sheet reaches the glass transition temperature Tg2 of the cured second layer, the cured second layer becomes glass-like. Then, the above-mentioned process is further performed, and the cured first and second layers, both of which are glass-like, reach room temperature.

[0019] Furthermore, in the temperature range from the glass transition temperature Tg2 of the cured second layer to room temperature, the cured first and second layers are both hard (in the same state), but if there is a difference in linear expansion coefficients, the cured sealing sheet is prone to warping due to the difference.

[0020] However, in the sealing sheet of the present invention, the glass transition temperature Tg2 of the second layer after curing is as low as 80° C. or less. Therefore, the temperature range from the glass transition temperature Tg2 of the second layer after curing to room temperature is narrow. Therefore, even if there is a difference in the linear expansion coefficients of the first layer and the second layer after curing, the above-mentioned warping can be suppressed. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 middle, Figure 1 A~ Figure 1 B shows a diagram for explaining one embodiment of the sealing sheet of the present invention and its production, Figure 1 A shows a cross-sectional view of the sealing sheet, Figure 1 B shows a diagram of preparing the first layer and the second layer respectively.

[0022] Figure 2 middle, Figure 2 A~ Figure 2 B is used for illustration purposes Figure 1 A is a diagram showing a method of sealing an electronic component with a sealing sheet, Figure 2 A shows the steps of preparing the electronic components and the sealing sheet, respectively. Figure 2 B shows a step of sealing the electronic component with a sealing sheet.

[0023] Description of Reference Numerals

[0024] 1 Sealing sheet

[0025] 2 Layer 1

[0026] 3 Layer 2

[0027] 21 Electronic components DETAILED DESCRIPTION

[0028] Reference Figure 1 A~ Figure 2 B One embodiment of the sealing sheet of the present invention is described.

[0029] Figure 1 The sealing sheet 1 shown in A is used for Figure 2 The electronic component 21 shown in A is sealed to produce Figure 2 The electronic component sealing sheet 1 is not the electronic component sealing package 30 (see FIG. Figure 2 B), and also not the sealing layer 20 after the electronic component 21 is sealed (refer to Figure 2 B). The sealing sheet 1 is a precursor (before complete curing) sheet for forming a sealing layer 20 as a component of an electronic component sealed package 30, does not include the electronic component 21, and is specifically a device that is distributed as a component itself and can be used industrially.

[0030] like Figure 1 As shown in A, the sealing sheet 1 has a substantially plate shape (film shape) extending in a plane direction perpendicular to the thickness direction. The sealing sheet 1 has one surface and the other surface spaced apart in the thickness direction.

[0031] The sealing sheet 1 includes, for example, a first layer 2 and a second layer 3 in this order toward one side in the thickness direction. Specifically, the sealing sheet 1 includes the first layer 2 and the second layer 3 disposed on one surface in the thickness direction of the first layer 2. The sealing sheet 1 preferably includes only the first layer 2 and the second layer 3.

[0032] The first layer 2 forms the other surface in the thickness direction of the sealing sheet 1. The first layer 2 has a substantially plate shape extending in the plane direction. The first layer 2 has one surface and the other surface spaced apart in the thickness direction.

[0033] It should be noted that the first layer 2 is described later and is also used when the sealing sheet 1 is used to seal the electronic element 21 (see Figure 2 A~ Figure 2 B) a contact layer that contacts one surface 23 and a peripheral side surface 25 (described later) of the electronic component 21 in the thickness direction, and one surface 26 of the substrate 22 surrounding the electronic component 21 in the thickness direction.

[0034] In addition, the first layer 2 is a heat-resistant improving layer, which is in close contact (contact) with the electronic component 21 when the sealing sheet 1 seals the electronic component 21, and is also in close contact (contact) with the substrate 22 on which the electronic component 21 is mounted, and even if the sealing layer 20 is repeatedly heated, the sealing layer 20 is prevented from peeling off from the electronic component 21 and / or the substrate 22, and is prevented from being damaged (cracked).

[0035] In addition, the first layer 2 is configured so as to be deformed according to the shape of the electronic element 21 when the sealing sheet 1 seals the electronic element 21 .

[0036] The first layer 2 has thermosetting properties.

[0037] The material of the first layer 2 is not particularly limited as long as the glass transition temperature Tg1 (described later) of the first layer 2 after curing is within a desired range. Examples of the material of the first layer 2 include a first sealing composition containing a thermosetting component.

[0038] The thermosetting component is a component that is temporarily softened by heating when the electronic element 21 is sealed, is melted and flows, and is cured by further heating.

[0039] In addition, the thermosetting component is, for example, in the first layer 2 at the B stage, not the C stage (i.e., a state before complete curing). It should be noted that the B stage is a state between the A stage where the thermosetting component is liquid and the C stage where it is completely cured, and is a state where curing is slightly advanced and the compression modulus is smaller than that of the C stage.

[0040] The thermosetting component includes, for example, a main agent, a curing agent, and a curing accelerator.

[0041] As the main agent, for example, epoxy resin, phenolic resin, melamine resin, vinyl ester resin, cyanoester resin, maleimide resin, silicone resin, etc. can be listed. As the main agent, from the viewpoint of heat resistance, etc., epoxy resin can be preferably listed. When the main agent is epoxy resin, the thermosetting component constitutes the epoxy thermosetting component together with the curing agent (epoxy curing agent) and curing accelerator (epoxy curing accelerator) described later.

[0042] Examples of the epoxy resin include bifunctional epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, modified bisphenol A epoxy resin, modified bisphenol F epoxy resin, and biphenyl epoxy resin, and polyfunctional epoxy resins having three or more functions such as phenol novolac epoxy resin, cresol novolac epoxy resin, trihydroxyphenylmethane epoxy resin, tetrahydroxyphenylethane epoxy resin, and dicyclopentadiene epoxy resin. These epoxy resins may be used alone or in combination of two or more.

[0043] Preferably, a combination of a bifunctional epoxy resin and a multifunctional epoxy resin is used, and more preferably, a combination of a bisphenol A type epoxy resin and a trishydroxyphenylmethane type epoxy resin is used.

[0044] The epoxy resin may be in a liquid, solid, or semisolid state at 25° C. A combination of a liquid and a solid state at 25° C. is preferred, and a single use of a semisolid at 25° C. is also preferred.

[0045] The proportion of the main agent (preferably epoxy resin) in the first sealing composition is, for example, 1% by mass or more, preferably 2.5% by mass or more, more preferably 4% by mass or more, and, for example, 30% by mass or less, preferably 10% by mass or less, more preferably 5% by mass or less. In addition, the proportion of the main agent (preferably epoxy resin) in the thermosetting component is, for example, 30% by mass or more, preferably 40% by mass or more, and, for example, 90% by mass or less, preferably 75% by mass or less.

[0046] The curing agent is a component (preferably an epoxy resin curing agent) that cures the above-mentioned main agent by heating. As the curing agent, for example, phenolic resins such as biphenylphenol novolac type and triphenylmethane type can be listed. Preferably, a phenolic resin of triphenylmethane type can be listed. The mixing number of the curing agent is, for example, 30 parts by mass or more, preferably 40 parts by mass or more, and for example, 150 parts by mass or less, preferably 120 parts by mass or less relative to 100 parts by mass of the main agent.

[0047] The curing accelerator is a catalyst (thermosetting catalyst) (preferably an epoxy resin curing accelerator) that promotes the curing of the main agent by heating, and examples thereof include organic phosphorus compounds, imidazole compounds such as 2-phenyl-4-methyl-5-hydroxymethylimidazole (2P4MHZ), etc. Preferred examples include imidazole compounds. The amount of the curing accelerator mixed is, for example, 0.05 parts by mass or more relative to 100 parts by mass of the main agent, and, for example, 5 parts by mass or less.

[0048] In addition, the first sealing composition preferably further contains an inorganic filler.

[0049] The inorganic filler is an inorganic particle that improves the deformation inhibition of the first sealing layer 6 (described later) after curing. As the material of the inorganic filler, for example, inorganic compounds such as quartz glass, talc, silica, alumina, aluminum nitride, silicon nitride, and boron nitride can be listed. These can be used alone or in combination of two or more. Preferably, silica can be listed.

[0050] The shape of the inorganic filler is not particularly limited, and examples thereof include a substantially spherical shape, a substantially plate shape, a substantially needle shape, and an irregular shape. Preferably, a substantially spherical shape is used.

[0051] The average value of the maximum length of the inorganic filler (average particle size in the case of a substantially spherical shape) is, for example, 50 μm or less, preferably 20 μm or less, more preferably 10 μm or less, and for example, 0.1 μm or more, preferably 0.5 μm or more.

[0052] Furthermore, the inorganic filler may include a first filler and a second filler having an average value of the maximum length smaller than an average value of the maximum length of the first filler.

[0053] The average value of the maximum length of the first filler (the average particle size in the case of a substantially spherical shape) is, for example, 1 μm or more, preferably 3 μm or more, and, for example, 50 μm or less, preferably 30 μm or less.

[0054] The average value of the maximum length of the second filler (average particle size in the case of a substantially spherical shape) is, for example, less than 1 μm, or preferably 0.8 μm or less, and, for example, 0.01 μm or more, or preferably 0.1 μm or more.

[0055] The materials of the first filler and the second filler may be the same or different.

[0056] Furthermore, the surface of the inorganic filler (first filler and / or second filler) may be partially or entirely surface-treated with a silane coupling agent or the like.

[0057] The proportion of the inorganic filler in the first sealing composition (first layer 2) is, for example, 60% by mass or more, preferably 70% by mass or more, more preferably more than 70% by mass, further preferably more than 75% by mass, particularly preferably more than 80% by mass, most preferably more than 80% by mass, and more preferably more than 82.5% by mass. In addition, the proportion of the inorganic filler in the first sealing composition is, for example, 95% by mass or less, preferably 90% by mass or less.

[0058] When the ratio of the inorganic filler in the first layer 2 exceeds the above lower limit, an increase in the first linear expansion coefficient α1 of the first layer 2 is suppressed, thereby effectively suppressing warping of the sealing layer 20 and improving the heat resistance of the sealing layer 20 .

[0059] When the ratio of the inorganic filler in the first layer 2 is lower than the upper limit, the handling property of the sealing sheet 1 can be excellent. In particular, when the ratio of the inorganic filler in the first layer 2 exceeds 90 mass %, the first layer 2 is too hard and thus becomes brittle, and sometimes the package shape cannot be maintained during process flow (handling).

[0060] In addition, when the inorganic filler includes the first filler and the second filler, the content of the first filler in the inorganic filler is, for example, more than 50% by mass, preferably more than 60% by mass, and for example, less than 90% by mass, preferably less than 75% by mass. The content of the second filler in the inorganic filler is the remainder described above.

[0061] Furthermore, the first sealing composition may contain additives such as a thermoplastic resin, an organic filler, a silane coupling agent, and a pigment.

[0062] Thermoplastic resin is a component that improves the flexibility of the first layer 2 when the electronic element 21 is sealed. As the thermoplastic resin, for example, natural rubber, butyl rubber, isoprene rubber, chloroprene rubber, ethylene-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ethylene-acrylate copolymer, polybutadiene resin, polycarbonate resin, thermoplastic polyimide resin, polyamide resin (6-nylon, 6,6-nylon, etc.), phenoxy resin, acrylic resin, saturated polyester resin (PET, etc.), polyamide-imide resin, fluororesin, styrene-isobutylene-styrene block copolymer, etc. As the thermoplastic resin, from the viewpoint of improving the dispersibility with the main agent (preferably epoxy resin), acrylic resin can be preferably listed.

[0063] Examples of the acrylic resin include carboxyl-containing (meth)acrylate copolymers (preferably carboxyl-containing acrylate copolymers) obtained by polymerizing monomer components including a (meth)acrylate alkyl ester having a linear or branched alkyl group and other monomers (copolymerizable monomers).

[0064] Examples of the alkyl group include alkyl groups having 1 to 6 carbon atoms, such as methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, tert-butyl group, isobutyl group, pentyl group, and hexyl group.

[0065] Examples of other monomers include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid.

[0066] The weight average molecular weight of the thermoplastic resin is, for example, 100,000 or more, preferably 500,000 or more, and, for example, 1,000,000 or less, preferably 800,000 or less.

[0067] The ratio (solid content ratio) of the thermoplastic resin in the first sealing composition is, for example, 0.1 mass % or more, preferably 0.5 mass % or more, and, for example, 5 mass % or less, preferably 1 mass % or less. The thermoplastic resin may be prepared by diluting with a solvent (such as methyl ethyl ketone).

[0068] There are no particular limitations on the organic filler, and for example, polymer particles can be cited. As the polymer constituting the polymer particles, for example, silicone polymers (silicone rubber), acrylic polymers, epoxy polymers, styrene polymers, etc. can be cited. Preferably, silicone polymers can be cited. The shape of the polymer particles is not particularly limited, and for example, a roughly spherical shape, a roughly plate shape, a roughly needle shape, an irregular shape, etc. can be cited. Preferably, a roughly spherical shape can be cited. The average value of the maximum length of the polymer particles (the average particle size in the case of a roughly spherical shape) is, for example, greater than 0.5 μm, and, for example, less than 20 μm.

[0069] It should be noted that the polymer particles may contain functional groups such as epoxy groups, carboxyl groups, and hydroxyl groups (preferably epoxy groups) on their surfaces.

[0070] The content ratio of the organic filler in the first sealing composition is, for example, 1 mass % or more, preferably 2 mass % or more, and, for example, 8 mass % or less, preferably 5 mass % or less.

[0071] As the silane coupling agent, for example, epoxy-containing silane coupling agents can be cited. As the epoxy-containing silane coupling agent, for example, glycidoxyalkyldialkyldialkoxysilanes such as 3-glycidoxypropylmethyldimethoxysilane and 3-glycidoxypropylmethyldiethoxysilane, for example, glycidoxyalkyltrialkoxysilanes such as 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane can be cited. Preferably, glycidoxyalkyltrialkoxysilane can be cited. The content ratio of the silane coupling agent in the first sealing composition is, for example, 0.2% by mass or more, preferably 1% by mass or more, and, for example, 5% by mass or less, preferably 2.5% by mass or less.

[0072] As the pigment, for example, black pigments such as carbon black can be cited. The average particle size of the pigment is, for example, 0.001 μm or more, for example, 1 μm or less. The proportion of the pigment in the first sealing composition is, for example, 0.1 mass % or more, preferably 0.25 mass % or more, and, for example, 2 mass % or less, preferably 0.75 mass % or less.

[0073] The thickness of the first layer 2 is the distance between one surface and the other surface of the first layer 2, and is, for example, 10 μm or more, preferably 20 μm or more, more preferably 50 μm or more, and, for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less.

[0074] As described above, the first layer 2 has thermosetting properties and can be cured (completely cured, brought to a C-stage) by heating.

[0075] Next, the physical properties of the first layer 2 after curing will be described.

[0076] The glass transition temperature Tg1 of the first layer 2 after curing is 150° C. or higher, preferably 155° C. or higher, more preferably 160° C. or higher, further preferably 165° C. or higher, particularly preferably 170° C. or higher, and most preferably 175° C. or higher. In addition, the glass transition temperature Tg1 of the first layer 2 after curing is, for example, 230° C. or lower, preferably 210° C. or lower, and more preferably 190° C. or lower.

[0077] The glass transition temperature Tg1 of the first layer 2 after curing is calculated as the peak value of tanδ(E” / E') obtained by dynamic viscoelasticity measurement in a tensile mode at a frequency of 1 Hz, a heating rate of 10°C / min, a temperature range of 0 to 260°C. It should be noted that the glass transition temperature Tg2 of the second layer 3 after curing described later is also measured by the same method as described above.

[0078] When the glass transition temperature Tg1 of the first layer 2 after curing is lower than the above lower limit, the heat resistance of the sealing layer 20 including the first layer 2 (first sealing layer 6) after curing decreases.

[0079] The tensile storage modulus E'1 of the cured first layer 2 at 260°C is, for example, 0.05 GPa or more, preferably 0.1 GPa or more, more preferably 0.2 GPa or more, further preferably 0.5 GPa or more, particularly preferably 0.75 GPa or more, and is, for example, 10 GPa or less, preferably 5 GPa or less.

[0080] The tensile storage modulus E'1 of the first layer 2 after curing is obtained together with the measurement of the glass transition temperature Tg1 described above. The tensile storage modulus E'2 of the second layer 3 after curing is also measured by the same method as described above.

[0081] When the tensile storage modulus E′1 of the cured first layer 2 at 260° C. is not less than the above lower limit, warping of the cured sealing sheet 1 (sealing layer 20 ) can be suppressed, and the cured first layer 2 has excellent heat resistance.

[0082] When the tensile storage modulus E′1 of the first layer 2 after curing at 260° C. is not more than the upper limit described above, warping of the sealing sheet 1 (sealing layer 20 ) after curing can be suppressed, and excellent sealing reliability can be achieved.

[0083] The first linear expansion coefficient α1 of the first layer 2 after curing is, for example, 50 ppm or less, preferably 25 ppm or less, more preferably 20 ppm or less, further preferably 10 ppm or less, particularly preferably 7 ppm or less, and, for example, 0 ppm or more, and further, 1 ppm or more. The first linear expansion coefficient α1 is a linear expansion coefficient at a glass transition temperature Tg1 or less.

[0084] When the first linear expansion coefficient α1 of the first layer 2 after curing is not more than the above upper limit, the warpage suppression property of the first layer 2 after curing can be improved, and the heat resistance of the first layer 2 after curing is excellent.

[0085] like Figure 1 As shown in A, the second layer 3 forms one surface in the thickness direction of the sealing sheet 1. The second layer 3 has a substantially plate shape extending in the plane direction. The second layer 3 has one surface and the other surface spaced apart in the thickness direction.

[0086] The second layer 3 is disposed on the entire surface of one surface of the first layer 2. The other surface of the second layer 3 is in contact with one surface of the first layer 2. One surface of the second layer 3 is exposed on one side in the thickness direction.

[0087] Layer 2 3 Figure 2 A~ Figure 2 The non-contact layer indicated by B is, for example, not in contact with the electronic element 21 when the sealing sheet 1 seals the electronic element 21 , and specifically, covers the electronic element 21 via the first layer 2 .

[0088] In addition, the second layer 3 supports and softly constrains (suppresses excessive flow) the first layer 2 that is deformed in accordance with the electronic element 21 when the sealing sheet 1 seals the electronic element 21. Specifically, when the second layer 3 seals the electronic element 21, the other surface of the second layer 3 is deformed in accordance with the deformation of the first layer 2. On the other hand, one surface of the second layer 3 maintains its flat (planar) shape.

[0089] Moreover, the second layer 3 is a warping suppression layer (deformation suppression layer) that suppresses the following situations: when the sealing sheet 1 seals the electronic component 21 and / or when the sealing sheet 1 is cured by subsequent heating, the temperature becomes high, and then when the cured sealing sheet 1 is cooled, the cured sealing sheet 1 (i.e., the sealing layer 20) warps (deformation caused by cooling).

[0090] The second layer 3 has thermosetting properties.

[0091] The material of the second layer 3 is not particularly limited as long as the glass transition temperature Tg2 (described later) of the second layer 3 after curing is within a desired range. Examples of the material of the second layer 3 include a second sealing composition containing a thermosetting component.

[0092] The second sealing composition includes, for example, components contained in the first sealing composition. The type and blending ratio of each component are appropriately selected from the above range.

[0093] Among them, as the epoxy resin (main agent of the thermosetting component) contained in the second sealing composition, preferably a modified bisphenol A type epoxy resin can be cited. The proportion of the main agent (preferably the epoxy resin) in the first sealing composition is, for example, 5% by mass or more, preferably 15% by mass or more, more preferably 17.5% by mass or more, and further preferably 20% by mass or more, and is, for example, 50% by mass or less, preferably 35% by mass or less.

[0094] Moreover, as a phenol resin (curing agent of a thermosetting component) contained in a 2nd sealing composition, a biphenyl phenol novolac type phenol resin is preferably mentioned.

[0095] In addition, it is preferred that the second sealing composition does not contain an organic filler.

[0096] In addition, it is preferred that the inorganic filler does not contain the second filler and contains only the first filler.

[0097] In addition, the proportion of the inorganic filler (preferably the first filler) in the second sealing composition (second layer 3) is, for example, 80 mass % or less, preferably 70 mass % or less, more preferably less than 70 mass %, further preferably 65 mass % or less, and, for example, 25 mass % or more, preferably 50 mass % or more.

[0098] When the proportion of the inorganic filler in the second layer 3 is lower than the above upper limit, the warping caused by the excessive increase of the tensile storage modulus E'2 described later can be suppressed. When the proportion of the inorganic filler in the second layer 3 is higher than the above lower limit, the cured second layer 3 can suppress excessive flow in the cured first layer 2. In particular, when the proportion of the inorganic filler in the second layer 3 is 50% by mass or more, the excessive flow of the first layer 2 during sealing can be suppressed, and the deviation of the thickness can be suppressed.

[0099] In addition, the proportion of the inorganic filler in the second sealing composition is preferably lower than the proportion of the inorganic filler in the first sealing composition. In this case, the heat resistance is improved by the cured first layer 2, and since the cured second layer 3 is soft, the force constraining the first layer 2 becomes weak, and the warping of the cured sealing sheet 1 can be suppressed.

[0100] It is preferred that the ratio of the inorganic filler in the first sealing composition exceeds 70% by mass, and the ratio of the inorganic filler in the second sealing composition is 70% by mass or less.

[0101] More preferably, the ratio of the inorganic filler in the first sealing composition exceeds 70% by mass, and the ratio of the inorganic filler in the second sealing composition is 65% by mass or less.

[0102] In addition, the ratio of the ratio of the inorganic filler in the first sealing composition to the ratio of the inorganic filler in the second sealing composition (ratio of the inorganic filler in the first sealing composition / ratio of the inorganic filler in the second sealing composition) is, for example, more than 1, preferably 1.25 or more, and is, for example, 5 or less, preferably 2 or less, and more preferably 1.75 or less. When the ratio is above the lower limit, the cured second layer 3 is soft, so the force constraining the first layer 2 becomes weak, and warping can be more reliably suppressed. When the ratio is below the upper limit, the difference in viscosity between the first layer 2 and the second layer 3 can be minimized, so that the thickness deviation can be suppressed.

[0103] The difference between the ratio of the inorganic filler in the first layer and the ratio of the inorganic filler in the second layer (specifically, the value obtained by subtracting the ratio of the inorganic filler in the second layer from the ratio of the inorganic filler in the first layer) is, for example, 60% by mass or less, preferably 50% by mass or less, and more preferably 30% by mass or less. When the above difference is below the above upper limit, the difference in viscosity between the first layer 2 and the second layer 3 can be reduced as much as possible, and therefore, the deviation in thickness can be suppressed.

[0104] On the other hand, the above-mentioned difference is, for example, 1 mass % or more, preferably more than 5 mass %, more preferably 10 mass % or more, and further preferably 20 mass % or more.

[0105] In particular, when the difference is 20 mass % or more, the inorganic filler in the first layer 2 is large, so that the heat resistance can be maintained and warping due to an excessive increase in the tensile storage modulus E'2 can be suppressed.

[0106] As described above, the second layer 3 has thermosetting properties and can therefore be cured (completely cured, brought to a C-stage) by heating.

[0107] Next, the physical properties of the second layer 3 after curing will be described.

[0108] The glass transition temperature Tg2 of the cured second layer 3 is lower than the above-mentioned glass transition temperature Tg1 of the cured first layer 2, specifically, 80° C. or less. The glass transition temperature Tg2 of the cured second layer 3 is preferably 75° C. or less, more preferably 70° C. or less, further preferably 65° C. or less, particularly preferably 60° C. or less, and most preferably 55° C. or less.

[0109] The glass transition temperature Tg2 of the second layer 3 after curing is 40° C. or higher, for example, and preferably 45° C. or higher.

[0110] When the glass transition temperature Tg2 of the second layer 3 after being cured is higher than the upper limit described above, the warping of the sealing layer 20 including the second layer 3 after being cured cannot be sufficiently suppressed.

[0111] In addition, the glass transition temperature Tg2 of the cured second layer 3 is 80° C. or less, so the temperature range from the glass transition temperature Tg2 of the cured second layer to room temperature is narrow. Therefore, even if the linear expansion coefficients of the cured first layer 2 and the second layer 3 are different, warping can be suppressed.

[0112] When the glass transition temperature Tg2 of the second layer 3 after being cured is higher than the above lower limit, the shape retention of the second layer 3 after being cured can be ensured.

[0113] In particular, when the glass transition temperature Tg2 of the cured second layer 3 is 40° C. or less, the resin such as the thermosetting component contained in the second sealing composition is too soft, so the cured second layer 3 cannot be cut. Furthermore, it becomes difficult to pick up the cured second layer 3.

[0114] In addition, the temperature (temperature difference) (Tg1-Tg2) obtained by subtracting the glass transition temperature Tg2 of the second layer 3 after curing from the glass transition temperature Tg1 of the first layer 2 after curing is, for example, 70° C. or more, preferably 90° C. or more, more preferably 100° C. or more, further preferably 110° C. or more, particularly preferably 120° C. or more, and, for example, 150° C. or less, preferably 140° C. or less. When the temperature difference is within the above range, both heat resistance and warpage suppression are excellent.

[0115] The tensile storage modulus E'2 of the cured second layer 3 at 260° C. is, for example, 1 GPa or less, preferably 0.3 GPa or less, more preferably 0.1 GPa or less, further preferably 0.05 GPa or less, and, for example, 0.001 GPa or more, preferably 0.005 GPa or more.

[0116] When the tensile storage modulus E′2 of the second layer 3 at 260° C. is less than the upper limit described above, the warping of the sealing sheet 1 (sealing layer 20 ) after curing can be more effectively suppressed.

[0117] The ratio (E'1 / E'2) of the tensile storage modulus E'1 of the first layer 2 at 260°C after curing to the tensile storage modulus E'2 of the second layer 3 at 260°C after curing is, for example, 1.5 or more, preferably 10 or more, more preferably 30 or more, further preferably 60 or more, particularly preferably 100 or more, and, for example, 200 or less.

[0118] When the ratio of the tensile storage modulus E'2 is equal to or greater than the lower limit, the second layer 3 after curing is soft, so the force restraining the first layer 2 is weakened, and warping can be more reliably suppressed.

[0119] The first linear expansion coefficient α1 of the cured second layer 3 is, for example, 25 ppm or more, preferably 45 ppm or more, more preferably 55 ppm or more, and further preferably 75 ppm or more, and is, for example, 200 ppm or less, and preferably 100 ppm or less. The first linear expansion coefficient α1 is a linear expansion coefficient at a temperature below the glass transition temperature Tg2.

[0120] The first linear expansion coefficient α1 of the second layer 3 after curing is, for example, larger than the first linear expansion coefficient α1 of the first layer 2 after curing. Specifically, the difference is, for example, greater than 10 ppm, preferably greater than 20 ppm, more preferably greater than 30 ppm, and further preferably greater than 40 ppm. In addition, for example, it is less than 200 ppm, preferably less than 100 ppm.

[0121] The thickness of the second layer 3 is the distance between one surface and the other surface of the second layer 3, and is, for example, 10 μm or more, preferably 20 μm or more, more preferably 50 μm or more, and, for example, 300 μm or less, preferably 200 μm or less, more preferably 100 μm or less.

[0122] The thickness of the sealing sheet 1 is the distance between the other surface of the first layer 2 and one surface of the second layer 3, and is the total thickness of the first layer 2 and the second layer 3, and is, for example, 50 μm or more, preferably 100 μm or more, and, for example, 2000 μm or less, preferably 500 μm or less.

[0123] To produce the sealing sheet 1, for example, Figure 1 As shown in B, first, the first layer 2 and the second layer 3 are formed respectively, and then, as Figure 1 As shown in A, the first layer 2 and the second layer 3 are bonded together.

[0124] First, a first sealing composition is prepared to form the first layer 2. Specifically, the above-mentioned components are mixed and blended to prepare an A-stage first sealing composition. Preferably, the above-mentioned components (and a solvent as required) are blended and mixed to prepare a varnish.

[0125] Then, a varnish is applied to the surface of the first release sheet 4 indicated by the virtual line and dried by heating to obtain the B-stage first layer 2. The first layer 2 may be formed directly from the first sealing composition by kneading and extrusion without preparing a varnish.

[0126] In order to form the second layer 3, a second sealing composition is prepared. Specifically, the above-mentioned components are mixed and mixed to prepare the second sealing composition of the A stage. Preferably, the above-mentioned components (and the solvent as required) are compounded and mixed to prepare a varnish. Then, the varnish is applied to the surface of the second peeling sheet 5 shown by the virtual line, and it is dried by heating to obtain the second layer 3 of the B stage. It should be noted that the second layer 3 can also be formed directly from the second sealing composition by mixing and extruding without preparing the varnish.

[0127] It should be noted that one of the first layer 2 and the second layer 3 may be directly formed (arranged) on the other.

[0128] From the viewpoint that both the first layer 2 and the second layer 3 have thermosetting properties, the sealing sheet 1 is preferably in the B-stage.

[0129] Next, refer to Figure 2 A~ Figure 2 B will describe a method for manufacturing the electronic component sealed package 30 by sealing the electronic component 21 with the sealing sheet 1.

[0130] This method is Figure 2 As shown in A of FIG. 1 , first, the sealing sheet 1 and the electronic component 21 are prepared separately.

[0131] The sealing sheet 1 is prepared according to the above-mentioned production method.

[0132] The electronic component 21 is prepared in a state of being mounted on the substrate 22, for example. The electronic component 21 and the substrate 22 constitute a component mounting substrate 29. That is, the component mounting substrate 29 includes the electronic component 21 and the substrate 22.

[0133] The electronic component 21 has a generally flat plate shape extending in the surface direction. Specifically, the electronic component 21 integrally comprises: a surface 23 and another surface 24 opposite to each other in the thickness direction, and a peripheral side surface 25 connecting their peripheries. It should be noted that an electrode (not shown) is provided on the other surface 24 of the electronic component 21. The electronic component 21 is not particularly limited, and various electronic components can be listed, for example, hollow electronic components, semiconductor components, etc. The thickness of the electronic component 21 is, for example, more than 50 μm, and, for example, less than 500 μm.

[0134] The substrate 22 has a substantially flat plate shape extending in the plane direction. The substrate 22 has one surface 26 in the thickness direction opposite to the electronic element 21. A terminal (not shown) electrically connected to an electrode (not shown) of the electronic element 21 is provided on one surface 26 of the substrate 22. As the material of the substrate 22, ceramics such as alumina, polymers such as polyimide, etc. can be listed, and ceramics are preferably listed from the viewpoint of heat resistance.

[0135] Then, if Figure 2 As shown in FIG. 8A , the sealing sheet 1 is arranged on the element mounting substrate 29 so that the first layer 2 faces the electronic element 21 .

[0136] Then, if Figure 2 The arrow of A and Figure 2 As shown in B, the sealing sheet 1 is directed toward the other side in the thickness direction and hot pressed using, for example, a flat plate press (not shown). At this time, the sealing sheet 1 is plastically deformed in accordance with the outer shape of the electronic component 21 .

[0137] Thereby, the sheet 1 for sealing is temporarily softened, and the electronic component 21 is embedded. In other words, the electronic component 21 is embedded in the sheet 1 for sealing.

[0138] The first layer 2 is deformed in accordance with the outer shape of the electronic element 21. In addition, the first layer 2 is in contact with one surface 26 of the substrate 22 that does not overlap with the electronic element 21 when projected in the thickness direction.

[0139] On the other hand, the other surface of the second layer 3 is deformed in accordance with the deformation of the first layer 2 , while one surface maintains a flat shape.

[0140] Next, the sealing sheet 1 in the B-stage is thermally cured by heating (transformed to the C-stage, completely cured) to form the sealing layer 20 .

[0141] The heating conditions are, for example, conditions under which the thermosetting components contained in the first layer 2 and the second layer 3 can be completely cured (C-staged), and specifically, the temperature is, for example, 150° C. or higher, preferably 170° C. or higher, and, for example, 200° C. or lower, preferably 180° C. or lower. The heating time is, for example, 0.5 hours or higher, preferably 1 hour or higher, and, for example, 4 hours or lower.

[0142] The sealing layer 20 cured by heating includes the first sealing layer 6 in which the first layer 2 is cured, and the second sealing layer 7 in which the second layer 3 is cured. It is preferred that the sealing layer 20 includes only the first sealing layer 6 and the second sealing layer 7.

[0143] The first sealing layer 6 corresponds to the first layer 2 after curing, and has the same physical properties as the first layer 2 after curing.

[0144] The second sealing layer 7 corresponds to the cured second layer 3 and has the same physical properties as those of the cured second layer 3 .

[0145] After heating, the high-temperature sealing layer 20 is usually cooled to room temperature (about 10 to 30° C.) by cooling or the like.

[0146] In this way, the electronic component sealed package 30 including the component mounting substrate 29 and the sealing layer 20 is manufactured. The electronic component sealed package 30 preferably includes only the component mounting substrate 29 and the sealing layer 20 .

[0147] Moreover, for the sealing sheet 1, after the electronic element 21 is sealed and cured, the cured first layer 2 (first sealing layer 6) has a glass transition temperature Tg1 as high as 150° C. or more, so it has excellent heat resistance. That is, even when the electronic element sealing package 30 is repeatedly heated to a high temperature (for example, a high temperature of 150° C. or more), the sealing layer 20 has excellent heat resistance that can continuously seal the electronic element 21.

[0148] In addition, the glass transition temperature Tg1 of the cured first layer 2 (first sealing layer 6) is higher than the above-mentioned glass transition temperature Tg2 of the cured second layer 3 (second sealing layer 7). Therefore, in the process of cooling the cured sealing sheet 1 to room temperature by heating at a high temperature (for example, a high temperature of 150°C or more) above the glass transition temperature Tg1 of the first layer 2, when the temperature of the cured sealing sheet 1 becomes the glass transition temperature Tg1 of the cured first layer 2, the cured first layer 2 becomes glass-like, while the cured second layer 3 is still rubber-like. The above-mentioned cooling process is further performed, and when the temperature of the cured sealing sheet 1 becomes the glass transition temperature Tg2 of the cured second layer 3, the cured second layer 3 becomes glass-like. That is, in the above-mentioned cooling process of the cured sealing sheet 1, the state changes from rubber-like to glass-like in the order of the cured first layer 2 and the cured second layer 3.

[0149] Then, the above process further proceeds, and the first layer 2 and the second layer 3 which have both become glassy (that is, in the same state) and have been solidified reach room temperature.

[0150] In the temperature range from the glass transition temperature Tg2 of the cured second layer 3 to room temperature, the cured first layer 2 and the second layer 3 are both hard. However, when there is a difference in the first linear expansion coefficient α1, the cured sealing sheet 1 is prone to warping due to the difference and because the cured first layer 2 and the second layer 3 are in contact with each other.

[0151] Furthermore, when the glass transition temperature Tg2 of the cured second layer 3 exceeds 80°C (high), the temperature range from the glass transition temperature Tg2 of the cured second layer 3 to room temperature (the temperature difference between the two) becomes wider, that is, although the state between the cured first layer 2 and the second layer 3 is common, the temperature range in which warping caused by the difference in the first linear expansion coefficient α1 is likely to occur becomes wider. Therefore, the above-mentioned warping cannot be fully suppressed.

[0152] However, in this embodiment, the glass transition temperature Tg2 of the cured second layer 3 is as low as 80° C. or less, so the temperature range in which warping easily occurs is narrow. Therefore, even if the first linear expansion coefficients α1 of the cured first layer 2 and the second layer 3 are different, the above-mentioned warping can be suppressed.

[0153] It should be noted that in the above-mentioned embodiment, the component mounting substrate 29 includes a single electronic component 21, but although not shown, it may include, for example, a plurality of electronic components 21. This can also achieve the same effects as in the first embodiment.

[0154] Example

[0155] Preparation example, embodiment and comparative example are shown below, and the present invention is described in more detail.It should be noted that the present invention is not subject to any limitation of preparation example, embodiment and comparative example.In addition, the specific numerical values ​​such as the blending ratio (containing ratio), physical property value, parameter used in the following description can be replaced by the upper limit (defined as the numerical value of "below", "not enough") or the lower limit (defined as the numerical value of "above", "exceeding") of the blending ratio (containing ratio), physical property value, parameter etc. recorded in the above-mentioned "specific embodiments", corresponding to them.

[0156] The components used in the preparation examples are shown below.

[0157] Acrylic resin HME-2006M manufactured by Negami Industries, Ltd., carboxyl group-containing acrylic acid ester copolymer, weight average molecular weight: 600,000, methyl ethyl ketone solution with a solid content concentration of 20% by mass

[0158] Epoxy resin A EPICLON EXA-4850-150 manufactured by DIC Corporation, modified bisphenol A type epoxy resin, liquid at 25°C

[0159] Epoxy resin B jER828 manufactured by DIC Corporation, bisphenol A type epoxy resin, liquid at 25°C

[0160] Epoxy resin C: EPPN501-HY manufactured by Nippon Kayaku Co., Ltd., trishydroxyphenylmethane type epoxy resin, solid at 25°C

[0161] Phenolic resin A: MEH-7851SS manufactured by Meiwa Chemicals Co., Ltd., biphenylphenol novolac type phenolic resin

[0162] Phenolic resin B TPM-100 manufactured by Gunei Chemical Industry Co., Ltd., triphenylmethane type phenolic resin

[0163] Curing accelerator 2-phenyl-4-methyl-5-hydroxymethylimidazole (2P4MHZ)

[0164] Organic filler EP-2601 manufactured by Dow Corning Toray Co., Ltd., spherical silicone polymer particles having an epoxy group and an average particle size of 2 μm

[0165] First filler: FB-5SDC manufactured by Denka Co., Ltd., spherical silica powder (inorganic filler), average particle size 5 μm)

[0166] Second filler: An inorganic filler obtained by surface-treating 100 parts by mass of SC220G-SMJ (average particle size: 0.5 μm) manufactured by ADMATECHS CO., LTD. with 1 part by mass of 3-methacryloxypropyltrimethoxysilane (product name: KBM-503 manufactured by Shin-Etsu Chemical Co., Ltd.).

[0167] Silane coupling agent KBM-403 manufactured by Shin-Etsu Chemical Co., Ltd., 3-glycidoxypropyltrimethoxysilane

[0168] Carbon black Mitsubishi Chemical Corporation #20, black pigment

[0169] Preparation Examples 1 to 5

[0170] (Preparation of the second layer)

[0171] According to the compounding recipe described in Table 1, a second sealing composition was prepared, and then a second layer 3 having a thickness of 75 μm in a B-stage state was prepared from the second sealing composition.

[0172] Preparation Examples 6 to 9

[0173] (Preparation of Layer 1)

[0174] According to the compounding recipe described in Table 1, a first sealing composition was prepared, and then a first layer 2 having a thickness of 75 μm in a B-stage state was prepared from the first sealing composition.

[0175] Evaluation of physical properties after curing of Preparation Examples 1 to 9

[0176] The second layer 3 of each of Preparation Examples 1 to 5 was heated at 150° C. for 1 hour to be cured (C-staged). Then, the following physical properties of the cured second layer 3 were evaluated.

[0177] In addition, the first layer 2 of each of Preparation Examples 6 to 9 was evaluated for the following physical properties in the same manner as the second layer 3 after curing (C-stage).

[0178] Table 1 shows the results.

[0179] <Tensile storage modulus E' and glass transition temperature Tg>

[0180] After only the first layer 2 after curing was processed into an outer shape of 0.1 cm in length and 5 cm in width, the dynamic viscoelasticity was measured using the following measuring apparatus and measuring conditions.

[0181] Measuring device: Solid viscoelasticity measuring device (model: RSA-G2, manufactured by TA Instruments)

[0182] Mode: Stretch

[0183] Scanning temperature: 0~260℃

[0184] Frequency: 1Hz

[0185] Heating rate: 10℃ / min

[0186] The tensile storage modulus E'1 of the cured first layer 2 at 260° C. was obtained. A curve of tan δ (=E" / E'1) was obtained from the tensile storage modulus E' and the tensile loss modulus E", and the glass transition temperature Tg1 was obtained as the peak value of tan δ.

[0187] The tensile storage modulus E'2 and the glass transition temperature Tg2 of the second layer 3 after curing at 260° C. were also determined in the same manner as described above.

[0188] <1st Linear Expansion Coefficient>

[0189] The cured first layer 2 was processed into an outer shape of 15 mm in length and 4.5 mm in width, and then placed in a tensile jig in a thermomechanical measuring apparatus (manufactured by Rigaku Corporation: Model TMA8310), and the first linear expansion coefficient α1 was calculated.

[0190] The measurement conditions are as follows.

[0191] Temperature range: above 25°C and below glass transition temperature Tg

[0192] Tensile load: 2g

[0193] Heating rate: 5℃ / min

[0194] The first linear expansion coefficient α1 of the second layer 3 after solidification is also determined in the same manner as described above.

[0195] Example 1 to Comparative Example 2

[0196] (Manufacture of Sealing Sheet)

[0197] The first layer 2 and the second layer 3 described in Table 1 are bonded together. Figure 1 A shows a sealing sheet 1 including a first layer 2 and a second layer 3. Tables 2 and 3 also show the physical properties of the first layer 2 and the second layer 3 in the sealing sheet 1.

[0198] (evaluate)

[0199] The following items were evaluated. The results are shown in Tables 2 and 3.

[0200] (Warp)

[0201] The outer shape of the sealing sheet 1 of each of Example 1 to Comparative Example 2 was processed into a rectangular shape of 87 mm in length and 87 mm in width.

[0202] Then, the sealing sheet 1 was hot-pressed at the center of the surface of an alumina plate (100 mm in length, 100 mm in width, 0.2 mm in thickness, first linear expansion coefficient α1: 8 ppm) under the following attaching conditions to prepare a sample.

[0203] <Attachment Conditions>

[0204] Temperature: 95℃

[0205] Pressurization time: 60 seconds

[0206] Pressure: 300kPa

[0207] Then, the sample was heated at 170°C for 2 hours to thermally cure (C-stage) the sealing sheet 1. Then, the sample was allowed to cool to 25°C.

[0208] Then, the warpage amount of the sealing sheet 1 (the warpage amount after curing) was measured at 25° C. Specifically, in the sample, the height of the four corners of the sealing sheet 1 after curing from the surface of the alumina plate was measured. Then, the average value of the heights (measured values) of the four corners was obtained as the warpage (warpage amount).

[0209] The warpage was evaluated according to the following criteria.

[0210] ○: Warping is less than 1 mm.

[0211] △: The warpage is 1 mm or more and less than 1.5 mm.

[0212] ×: The warpage is 1.5 mm or more.

[0213] (Thermal cycle test)

[0214] The outer shape of each sealing sheet 1 of Example 1 to Comparative Example 2 was processed into a circular shape having a diameter of 3 mm.

[0215] Then, the sealing sheet 1 was placed at the center of the surface of an alumina plate (100 mm in length, 100 mm in width, and 0.2 mm in thickness), and hot pressing was performed under the following attaching conditions to prepare a sample.

[0216] <Attachment Conditions>

[0217] Temperature: 95℃

[0218] Pressurization time: 60 seconds

[0219] Pressure: 300kPa

[0220] Then, the sample was heated at 150°C for 1 hour to thermally cure (C-stage) the sealing sheet 1. Then, the sample was allowed to cool to 25°C.

[0221] Then, the samples were subjected to a heat cycle test (temperature -50°C to 125°C, 1 cycle for 1 hour, 1000 cycles), and the heat resistance was evaluated according to the following criteria.

[0222] ◯: After the heat cycle test, neither the cracking of the sealing sheet 1 nor the peeling of the sealing sheet 1 from the alumina plate occurred.

[0223] Δ: After the heat cycle test, cracks in the sealing sheet 1 or peeling of the sealing sheet 1 from the alumina plate occurred.

[0224] ×: After the heat cycle test, both the cracking of the sealing sheet 1 and the peeling of the sealing sheet 1 from the alumina plate occurred.

[0225] (Deviation in thickness of sealing sheet after curing)

[0226] The thickness in the plane direction of the sealing sheet (sealing layer 20 ) after curing in Examples 1 and 4 to 6 was measured, and the variation was evaluated according to the following criteria.

[0227] ○: The variation in thickness is less than 5 μm.

[0228] △: The variation in thickness is 5 μm or more and less than 10 μm.

[0229] ×: The variation in thickness is 10 μm or more.

[0230] [Table 1]

[0231]

[0232] [Table 2]

[0233]

[0234] [Table 3]

[0235]

[0236] It should be noted that the above invention is provided as an exemplary embodiment of the present invention, but it is merely an illustration and is not to be construed as limiting. Modifications of the present invention that are obvious to those skilled in the art are included in the claims.

Claims

1. A sealing sheet, characterized in that: It is a sealing sheet used to seal electronic components. The sealing sheet includes, in order toward one side in the thickness direction: a first layer in contact with the electronic component when the electronic component is sealed, and a second layer exposed to the outside. The first layer and the second layer are each thermosetting. The first layer and the second layer each contain an inorganic filler, The difference between the ratio of the inorganic filler in the first layer and the ratio of the inorganic filler in the second layer is 60% by mass or less, The glass transition temperature Tg1 of the first layer after curing is 150° C. or higher. The glass transition temperature Tg2 of the second layer after curing is 80° C. or less.

2. The sealing sheet according to claim 1, wherein The first layer contains more than 70% by mass of an inorganic filler, The second layer contains 70 mass % or less of an inorganic filler.

3. The sealing sheet according to claim 2, wherein: The difference between the ratio of the inorganic filler in the first layer and the ratio of the inorganic filler in the second layer is 50 mass % or less.