Graphene transistors containing functional N-heterocyclic carbene compounds, methods for preparing the same, and biosensors containing the same
By forming an N-heterocyclic carbene compound connection layer on the graphene channel layer and combining with biological probe units, the problems of reduced conductivity of graphene transistors and complexity of conventional modification methods are solved, and high sensitivity and selectivity of biological products are achieved Sensors simplify the process flow and maintain the excellent performance of graphene.
Patent Information
- Application Number
- CN201880069999.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-03-08
- Filing Date
- 2018-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2038-10-29
AI Technical Summary
The conductivity of existing graphene transistors decreases during surface modification, and conventional methods require additional chemical reaction steps, resulting in increased manufacturing costs and poor stability, making it difficult to improve the biosensor without changing the inherent excellent conductivity of graphene. Selectivity and sensitivity.
Using N-heterocyclic carbene compounds as the connecting layer, covalent bonds are formed on the surface of the graphene channel layer by chemical vapor deposition, and combined with biological probe units to achieve rapid and simple surface modification and doping, and enhance the graphene channel. Conductivity of the channel layer and performance of the biosensor.
It is achieved to improve the conductivity of the graphene channel layer and the sensitivity and selectivity of the biosensor without increasing the manufacturing cost, and to maintain the inherent excellent performance of graphene, simplify the process flow.
Smart Images

Figure CN111837239B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a graphene transistor and a method for manufacturing the same, and a biosensor using the graphene transistor. The graphene transistor includes a connection layer of an N-heterocyclic carbene compound having a functionalized terminal region. Background Art
[0002] Graphene is one of the carbon allotropes including carbon atoms, and has carbon atoms sp 2 Hybrid two-dimensional planar layered structure.
[0003] Compared with existing carbon materials, graphene has a very large surface area, chemical stability and shows excellent mechanical stability and thermal conductivity (about 5,000W / m·K). In addition, graphene has excellent transparency, which is due to its low absorption of visible light, etc., so that its transmittance of light with a wavelength of 550nm reaches 97%. And because its electrical-electronic properties remain intact, it has excellent flexibility and has strong elasticity even when physically stretched by 20%.
[0004] In addition, graphene is known to have very high electrical conductivity (intrinsic electron mobility is 20,000 cm 2 / V·s), because it behaves electrically like a semi-metal and the charges in graphene also act as zero effective mass particles.
[0005] Since its discovery by Novoselov and Game in 2004, graphene has become one of the most promising materials due to its excellent optical, physical and chemical properties. In recent years, graphene has been discussed for its applicability in touch panels, organic light-emitting devices, supercapacitors, hydrogen generation / storage devices, photovoltaic cells, photocatalysts, biosensors, etc.
[0006] In particular, graphene has become the focus of attention as carbon atoms of two-dimensional graphene having a hexagonal structure are used in transistors as reported to have field-effect properties when graphene is mechanically exfoliated and may replace conventional semiconductor materials such as silicon.
[0007] For example, when graphene is fabricated into a nanoribbon having a channel width of 10 nm or less, a band gap is formed due to a size effect, and thus, graphene can be used to fabricate a graphene transistor that exhibits excellent operating characteristics even at room temperature.
[0008] This graphene transistor has the property of increasing conductivity linearly according to the gate voltage. In particular, the graphene transistor shows very high charge mobility due to ballistic electron transfer, where the effective mass of electrons is 0, which gives the graphene transistor an excellent advantage.
[0009] However, despite having excellent physical properties as described above, the applicable technology is actually greatly limited due to reduced uniformity and dispersion due to the action of van der Waals forces between graphene layers, or reduced structural stability.
[0010] In recent years, various methods have been attempted to solve the above-mentioned problems. In particular, research on modifying the surface of graphene using functional groups has been actively conducted.
[0011] In particular, it is desirable to modify the surface of graphene because the modified graphene surface may affect the stability of the transistor against ions in solution or the selectivity and sensitivity of a biosensor including the transistor.
[0012] For this purpose, covalent functionalization methods are used in related technologies to covalently bond organic matter to hydrophilic functional groups on the surface and ends of graphene, such as forming oxygen functional groups such as epoxy groups, hydroxyl groups, carbonyl groups, and carboxylic acid groups thereon; non-covalent functionalization methods using non-covalent bonds (such as π-π bonds, hydrogen bonds, or charge interactions), etc.
[0013] For example, specific functions are imparted to graphene by chemically modifying the surface of graphene by covalently bonding graphene with functional monomers or polymers, or by physically modifying the surface of graphene with non-covalent bonds and then reducing it with a reducing agent such as hydrazine (N2H2) or sodium borohydride (NaBH4).
[0014] However, when the functional groups form covalent bonds on the surface of graphene, the sp 2 Key converted to sp 3 bonds, resulting in a decrease in the conductivity of graphene.
[0015] Moreover, since such covalent bonds are generally formed on the surface or end of most graphene, the surface of the graphene is partially modified. Therefore, the partially modified graphene has certain limitations in improving the performance of transistors, etc. In particular, it has a limit on the amount of attachment of biological probes, which makes it impossible to express the selectivity and sensitivity of a biosensor including such a graphene transistor to a desired degree.
[0016] Meanwhile, the advantage of non-covalent bonds is that the method of forming non-covalent bonds is relatively simple and the defects that can occur on the graphene surface are minimized to ensure the excellent physical properties of graphene, but the problem is that it shows poor stability when subjected to physical or chemical treatments.
[0017] In addition, since the conventional surface modification method as described above includes a multi-step process, namely, including modifying the surface of graphene and reducing graphene, the method requires additional chemical reaction steps, such as using or removing a reducing agent. This is a factor that reduces the performance of graphene transistors. In addition, conventional surface modification methods have many technical defects, such as low reproducibility, high temperature processing, incompatibility with mass production, etc.
[0018] In addition, biosensors using conventional graphene transistors have the following problems: they are manufactured through a two-step process including doping graphene and coupling a bioprobe to the graphene to improve the performance of the biosensor, thereby increasing the manufacturing cost.
[0019] Therefore, there is a great need for the following technology: it is possible to exhibit the excellent conductivity inherent in graphene and improve the selectivity and sensitivity of biosensors including graphene, and simultaneously perform the following steps: quickly modify, dope the surface of graphene and bind biological probes without any additional chemical reaction steps.
[0020] Prior art literature
[0021] Patent Document 1: Korean Patent Publication No. 2015-0120003 (October 27, 2015)
[0022] Patent Document 2: Korean Patent Publication No. 2013-0027199 (March 15, 2013) Summary of the invention
[0023] Technical issues
[0024] Therefore, the object of the present invention is to provide a transistor which can facilitate the modification of the surface of the graphene channel layer and the attachment of the biological probe to the graphene channel layer without any additional chemical reaction steps, and can more sensitively change the conductivity of the graphene channel layer through the specific binding of the material to be detected bound to the biological probe.
[0025] Technical solutions
[0026] In order to solve the above problems, according to one aspect of the present invention, a graphene transistor is provided, which includes a substrate, a graphene channel layer arranged on the substrate, a pair of metals arranged on the graphene channel layer and spaced apart from each other, and a connecting layer including an N-heterocyclic carbene compound arranged on the graphene channel layer.
[0027] According to another aspect of the present invention, a method for manufacturing a graphene transistor is provided, the method comprising growing graphene on a substrate by chemical vapor deposition using a hydrocarbon gas as a carbon source to form a graphene channel layer, forming a pair of metals on the graphene channel layer, and forming a connecting layer on the surface of the graphene channel layer exposed to the outside using a surface treatment agent including an N-heterocyclic carbene compound.
[0028] According to yet another aspect of the present invention, a biosensor is provided, comprising the graphene transistor as described above.
[0029] Beneficial Effects
[0030] The graphene transistor of the present invention can use an N-heterocyclic carbene compound as a connecting layer to easily connect the probe unit to the graphene channel layer, and has excellent stability to external environmental changes due to the presence of a chemical bond between the graphene channel layer and the probe unit. Therefore, the graphene transistor of the present invention has an advantage that it can sensitively detect electrochemical changes as changes in the conductivity of the graphene channel layer based on the bond between the probe unit and the target material.
[0031] Moreover, according to the method for manufacturing a graphene transistor of the present invention, a graphene channel layer and a connecting layer can be bonded to the graphene while modifying the surface of the graphene quickly and simply without performing any additional chemical reaction steps, thereby enhancing the convenience of manufacturing and saving manufacturing costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The following drawings attached to this specification are provided to illustrate the preferred embodiments of the present invention and are used to help further understand the technical scope of the present invention together with the above content of the present invention. Therefore, it should be understood that the present invention should not be interpreted as being limited to the details described in these drawings.
[0033] Figure 1 is a diagram showing a graphene transistor in which a bioprobe unit is attached to a connection layer.
[0034] Figure 2 Yes b) Figure 3 ), c) is an image of the micropatterned graphene electrode, d) is a microscope image of the micropatterned graphene electrode, and e) is a graph showing the Raman analysis results in areas A and B of d).
[0035] Figure 3 and Figure 4 is a flow chart illustrating a process for fabricating micropatterned graphene electrodes.
[0036] Figure 5is a schematic diagram of graphene showing that a carbene group of an N-heterocyclic carbene compound is covalently bonded to a graphene channel layer.
[0037] FIG. 6 shows the molecular formula and NMR data of N-heterocyclic carbene compounds having terminal regions functionalized with a) an azide group and b) a phthalimide group, respectively.
[0038] Figure 7 is a reaction diagram showing the steps of the process of synthesizing an N-heterocyclic carbene compound (NHC1).
[0039] Figure 8 is a reaction diagram showing the steps of the process of synthesizing N-heterocyclic carbene compounds (NHC2).
[0040] Fig. 9 is a reaction diagram showing the steps of the process of synthesizing N-heterocyclic carbene compounds (NHC3).
[0041] Fig.10 is a reaction diagram showing the steps of the process of synthesizing N-heterocyclic carbene compounds (NHC4).
[0042] Fig.11 is a reaction diagram showing the steps of the process for synthesizing an N-heterocyclic carbene compound (NHC5).
[0043] Fig.12 It is the nuclear magnetic resonance (NMR) spectrum of N-heterocyclic carbene compound (NHC5).
[0044] Fig.13 is a diagram showing the real-time response of a biosensor including a graphene transistor to H1N1 HA antigen.
[0045] Fig.14 is a diagram showing the real-time response of a biosensor including a graphene transistor to dopamine.
[0046] Fig.15 is a schematic diagram showing the formation of graphene on a copper substrate using a chemical vapor deposition (CVD) method.
[0047] Fig.16 It is a diagram showing conditions of the process for forming graphene shown in FIG. 6 .
[0048] Fig.17 is a graph showing transmittance according to the formation of graphene shown in FIG. 6 .
[0049] Fig.18 Shown is a process for treating the surface of a graphene transistor with an N-heterocyclic carbene compound.
[0050] FIG. 19 shows a) to c) a density functional theory (DFT) model of a graphene transistor, d) a graph of current-voltage characteristics, and e) a graph of transition curve characteristics.
[0051] Fig. 20 are graphs showing a) Raman data and b) current-voltage characteristics of a graphene transistor.
[0052] Fig.21 is a diagram showing the real-time response of a biosensor including a graphene transistor to geosmin.
[0053] Fig. 22 is a diagram showing the real-time response of a biosensor including a graphene transistor to Escherichia coli (E. coli). DETAILED DESCRIPTION
[0054] Hereinafter, the present invention will be described in detail.
[0055] 1. Graphene transistor
[0056] One aspect of the present invention provides a graphene transistor.
[0057] like Figure 1 As shown, the graphene transistor of the present invention includes a substrate, a graphene channel layer, a pair of metals and a connection layer.
[0058] The substrate is configured to be used as a support configured to support the composition of the graphene transistor according to the present invention. In this case, an insulating inorganic substrate such as a Si substrate, a glass substrate, a GaN substrate, a silicon dioxide substrate, a metal substrate such as Ni, Cu, W, a plastic substrate, etc. can be used as the substrate. When an insulating substrate is used, a SiO2 substrate is preferably used because the SiO2 substrate has excellent affinity for the graphene channel layer.
[0059] Moreover, the substrate can be selected from various materials on which graphene can be deposited. For example, the substrate can be formed of materials such as silicon germanium, silicon carbide (SiC), etc., and can include an epitaxial layer, a silicon-on-insulator layer, a semiconductor-on-insulator layer, etc.
[0060] The graphene channel layer constituting the graphene transistor of the present invention may include graphene. In this case, since a high current flows even in the off state when no voltage is applied to the gate, the on / off ratio of the operating current may be very low, which makes it possible to manufacture a high-performance transistor.
[0061] The graphene channel layer may include a single layer or a bi-layer graphene. However, when a bi-layer graphene is used, the sensitivity of the biosensor may be reduced due to the reduction in surface resistance. Figure 2 As shown, the graphene channel layer more preferably includes a single layer of graphene.
[0062] A pair of metals may be a source electrode and a drain electrode, which are formed on the graphene channel layer to be spaced apart from each other so as to apply a voltage to the graphene channel layer.
[0063] Such a source electrode and a drain electrode may be electrically connected through the graphene channel layer, and may include a material having conductivity. For example, the source electrode and the drain electrode may be formed of a metal, a metal alloy, a conductive metal oxide, a conductive metal nitride, and the like.
[0064] For example, the source electrode and the drain electrode may each independently include one selected from the group consisting of Cu, Co, Bi, Be, Ag, Al, Au, Hf, Cr, In, Mn, Mo, Mg, Ni, Nb, Pb, Pd, Pt, Re, Rh, Sb, Ta, Te, Ti, W, V, Zr, and Zn, and a combination thereof, but the present invention is not limited thereto. In this case, Pt is preferred in terms of contact characteristics of graphene and ease of etching.
[0065] The connection layer is configured to bond the biological probe unit to the graphene channel layer of the graphene transistor according to the present invention. Figure 3 and Figure 4 As shown, the connection layer may be disposed on the graphene channel layer exposed between a pair of metals spaced apart from each other.
[0066] The connecting layer may include an N-heterocyclic carbene compound.
[0067] Specifically, the N-heterocyclic carbene compound may be represented by Formula 1 below.
[0068] Formula 1
[0069]
[0070] wherein A may be an azide group or a phthalimide group; and
[0071] R1 may be an alkylene group or an alkoxyalkylene group having 1 to 10 carbon atoms and containing 1 to 5 repeating units. In this case, R1 is preferably an alkylene group or an alkoxyalkylene group having 1 to 8 carbon atoms and containing 1 to 4 repeating units, and in terms of the sensitivity of the conductivity of the graphene channel layer, more preferably an alkoxyalkylene group having 2 to 5 carbon atoms and containing 1 to 4 repeating units.
[0072] In addition, R2 and R3 can be identical or different from each other, and can be selected from any one of alkyl, cycloalkyl, alkenyl, alkynyl, aryl, alkylene group, alkenyl group, alkyne group, alkoxy group, arylalkyl and benzyl each having 1 to 20 carbon atoms. In this case, R2 and R3 are each independently preferably selected from any one of alkyl, cycloalkyl, alkenyl and benzyl each having 3 to 16 carbon atoms, and more preferably, with respect to the binding affinity of the graphene channel layer to the probe unit, each selected from cycloalkyl or benzyl each having 6 to 10 carbon atoms.
[0073] For N-heterocyclic carbene compounds, such as Figure 5 As shown, the carbene groups can be bonded to the graphene of the graphene channel layer via covalent bonds.
[0074] In this way, because the graphene channel layer forms a covalent bond with the carbene group of the N-heterocyclic carbene compound by self-bonding, the N-heterocyclic carbene compound has the effect of forming a band gap without any additional doping process and reducing the noise caused by non-specific external charges. In addition, the N-heterocyclic carbene compound has the effect of simplifying the process and saving costs because it does not require additional chemical treatment (such as adding a cross-linking agent) and the like.
[0075] In addition, the N-heterocyclic carbene compound may have a terminal region functionalized with an azide group or a phthalimide group (part A of Formula 1). Thus, the connecting layer can be combined with the bioprobe unit without any additional chemical reaction steps.
[0076] The N-heterocyclic carbene compound preferably comprises at least one selected from the group consisting of 6-4-(-azidobutyloxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylene, 6-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylene, 6-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylene, The invention further comprises a 6-(4-(1,3-diisoindol-2-yl)butoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene and a 6-(4-azidobutoxy-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene, more preferably a 6-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene or a 6-(4-azidobutoxy-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene.
[0077] The linker layer formed by the N-heterocyclic carbene compound as described above may form the linker layer in the form of a single layer.
[0078] When the connecting layer is formed in the form of a monolayer of an N-heterocyclic carbene compound, it not only has excellent intrinsic properties of graphene such as charge mobility, transmittance, and flexibility, but also has the effect of blocking noise signals generated by the entry of nonspecific external charges.
[0079] In addition, the connection layer may have a thickness of 0.1 nm to 1 nm. When the thickness of the connection layer is less than 0.1 nm, resistance may increase. On the other hand, when the thickness of the connection layer is greater than 1 nm, transmittance may decrease.
[0080] 2. Method for manufacturing graphene transistors
[0081] Another aspect of the present invention provides a method for manufacturing a graphene transistor.
[0082] Reference Figure 3 and Figure 4 The method for manufacturing a graphene transistor according to the present invention comprises: growing graphene on a substrate by chemical vapor deposition using hydrocarbon gas as a carbon source to form a graphene channel layer, forming a pair of metals on the graphene channel layer, and using a surface treatment agent containing an N-heterocyclic carbene compound to form a connection layer on the surface of the graphene channel layer exposed to the outside.
[0083] Such a graphene channel layer can be formed, for example, using a chemical vapor deposition method. In this case, when a chemical vapor deposition method is used, a single layer to a multilayer graphene showing excellent crystallinity can be obtained in a large area.
[0084] Chemical vapor deposition is a method of growing graphene by adsorbing a carbon precursor in the form of a gas or vapor with high kinetic energy onto a substrate surface, decomposing or reacting the carbon precursor to separate carbon atoms, and forming interatomic bonds between the corresponding carbon atoms.
[0085] According to the present invention, the chemical vapor deposition method may include at least one selected from the group consisting of plasma enhanced chemical vapor deposition (PECVD), atmospheric pressure chemical vapor deposition (APCVD) and low pressure chemical vapor deposition (LPCVD). In this case, the chemical vapor deposition method is preferably LPCVD because it can be deposited by minimizing defects in a large area.
[0086] According to a specific method for chemical vapor deposition, a graphene channel layer can be formed, for example, by depositing a metal catalyst (e.g., nickel, copper, aluminum, iron, etc.) on a wafer including silicon oxide. The layer is formed using a sputtering device and an electron beam evaporator to form a metal catalyst layer, the wafer is placed in a reactor together with a carbon source (e.g., CH4, C2H2, etc.), the wafer and the carbon source are heated so that carbon atoms can be absorbed into the metal catalyst layer, the wafer is cooled to separate the carbon atoms from the metal catalyst layer and crystallize the carbon atoms, and finally the metal catalyst layer is removed from the wafer.
[0087] However, the method of forming the graphene channel layer is not limited to the chemical vapor deposition method. For example, various methods may be used to form the graphene channel layer.
[0088] For example, the graphene channel layer can be formed by a physical exfoliation method in which graphene is prepared by exfoliating a layer from a graphite crystal composed of several layers using mechanical force, a chemical exfoliation method utilizing redox characteristics, or an epitaxial synthesis method in which a carbon source such as SiC is included or adsorbed in the crystal under high temperature conditions of 1,500°C.
[0089] A pair of metals may be a source electrode and a drain electrode, which may be formed using methods known in the art, such as thermal deposition, electron beam deposition, PECVD, LPCVD, physical vapor deposition (PVD), sputtering, ALD, and the like.
[0090] Forming a connection layer on the surface of the graphene channel layer exposed to the outside may include immersing the substrate in an N-heterocyclic carbene compound solution at room temperature for a predetermined period of time in the presence of argon gas, thereby forming the connection layer on the surface of the substrate on which the graphene channel layer is formed.
[0091] For the graphene channel layer and the connecting layer, the surface of the graphene channel layer can be modified by reacting for 5 to 300 seconds without any additional chemical reaction steps. Considering the convenience of improving manufacturing and saving manufacturing costs, the reaction is preferably carried out for 20 to 60 seconds. Its advantage is that it is simpler and faster than the methods known in the prior art.
[0092] The N-heterocyclic carbene compound constituting the connecting layer can be used, for example, Figures 7 to 11 According to the present invention, an N-heterocyclic carbene compound can be synthesized using an imidazolium salt as a source.
[0093] That is, in the present invention, in terms of the reactivity of the surface modification of the graphene channel layer, an imidazolium salt is used as a source to prepare a graphene transistor from an N-heterocyclic carbene compound having a cyclic structure.
[0094] When a carbene compound without a ring structure is used, the reaction conditions for modifying the surface of the graphene channel layer are very strict, and since it is impossible to modify the entire surface of the graphene channel, the effect of external charges may not be completely prevented. In addition, since the electrons provided by the carbene compound without a ring structure tend to be persistently accumulated in the graphene channel layer, thereby reducing the stability of the graphene channel layer itself, the electrons may be separated from the graphene channel layer again when the carbene compound is used in an amount higher than a predetermined amount.
[0095] 3. Biosensors
[0096] Yet another aspect of the present invention provides a biosensor comprising the graphene transistor as described above.
[0097] According to the biosensor of the present invention, it utilizes that the semiconductor characteristics of the current flowing through the graphene channel layer between the source electrode and the drain electrode change in response to the electric field.
[0098] Specifically, when the probe included in the bioprobe unit formed on the surface of the graphene channel layer reacts with the target, the electric field around the probe changes. As a result, the value of the current flowing through the graphene channel region between the source electrode and the drain electrode also changes. In this case, the target can be detected by measuring the current change.
[0099] When the graphene transistor as described above is used in a biosensor, the biosensor shows excellent sensitivity, specificity, speed and portability. In particular, when graphene is used in the channel layer, the biosensor shows excellent sensitivity and real-time detection performance due to the high charge carrier mobility and conductivity characteristics of graphene.
[0100] In addition, when the connection layer as described above is formed on the graphene channel layer in the transistor so that the biological probe unit combined with the connection layer exists in the channel region of the transistor, the sensitivity of the biosensor can be further improved, and the doping process and the attachment of the biological probe can be carried out simultaneously, thereby simplifying the process.
[0101] The fabrication method for such a biosensor may include doping a graphene channel layer, and bonding a bioprobe unit to a connection layer.
[0102] That is, in the case of a graphene transistor included in a biosensor, a band gap is formed by modifying the surface of a graphene channel layer with an N-heterocyclic carbene compound. Therefore, a separate doping process for forming a band gap is not required, but a doping process for adjusting the band gap energy is required in terms of operating efficiency and reliability.
[0103] In this case, the doping process may include at least one selected from the group consisting of substitutional doping, chemical doping, and surface charge transfer doping.
[0104] Among them, substitution doping is a method of replacing carbon atoms with boron or nitrogen. More specifically, substitution doping is a method of flowing a gas containing boron (i.e., HBO3, H2B6) and a gas containing nitrogen (i.e., NH3) together with methane to synthesize graphene substituted with boron and nitrogen, or when synthesizing graphene using chemical vapor deposition, heat treating the gas, or applying plasma to the gas at a high temperature while flowing the gas.
[0105] In particular, when the gas is flowed while being heat-treated at a high temperature, the graphene oxide can be reduced and substituted at the same time. Therefore, the method has the advantage that the doping degree can be adjusted by reducing the intensity of the plasma and the amount of the gas.
[0106] Chemical doping is a method of changing the work function of graphene using chemical substances. In this case, graphene can become p-type or n-type depending on the chemical substances used. In particular, gold chloride is preferably used.
[0107] The advantage of such chemical doping is that the doping level can be easily adjusted without changing the mechanical and chemical properties of the target material.
[0108] Meanwhile, when there is a material rich in or lacking electrons on the surface of graphene, the electronic state of graphene can be changed by making electrons leave graphene or transferring electrons to graphene. Surface charge transfer doping is a method using this method.
[0109] That is, when the structure of graphene is formed by coating or by depositing molecules capable of inducing charge transfer, charge transfer occurs spontaneously due to the difference in electronegativity from the carbon constituting the graphene. This is a method of doping graphene.
[0110] The adsorption material causing the surface charge transfer may include, for example, tetrafluorotetracyanoquinodimethane (F4-TCNQ) and fluoropolymer (CYTOP).
[0111] In addition, the combination of the biological probe unit and the connecting layer can be carried out by the following process: modifying the surface of the graphene channel layer with an N-heterocyclic carbene compound to form a connecting layer, and allowing the functional groups of the N-heterocyclic carbene compound constituting the connecting layer (such as an azide group or a phthalimide group) to react with the biological probe unit (such as an aptamer, an antibody, etc.) in the following state, that is, the functional groups of the N-heterocyclic carbene compound are exposed to the upper surface of the connecting layer.
[0112] Meanwhile, the doping of the graphene channel layer and the bonding of the bioprobe unit to the connecting layer can be performed simultaneously.
[0113] In the prior art, a graphene channel layer is first doped, and then an additional chemical treatment is performed to modify the surface of the graphene channel layer, and a bioprobe unit is attached to the graphene channel layer to fabricate a biosensor.
[0114] In contrast, according to the present invention, the bioprobe unit is directly bonded to the N-heterocyclic carbene compound. Therefore, since the graphene channel layer can be doped and the bioprobe unit can be attached at the same time, the process is simplified and the present invention shows the effect of improving economic feasibility.
[0115] Meanwhile, the bio-probe unit may include a probe material including one or more selected from the group consisting of an aptamer, a DNA, an antigen, an antibody, and a peptide.
[0116] Here, the aptamer refers to a peptide molecule synthesized from RNA, DNA, synthetic nucleotides, etc., and can be synthesized with a specific base sequence so that the aptamer can selectively bind to a target substance.
[0117] As an example, Fig.13 and 14 As shown, the biosensor according to the present invention can detect antigens or antibodies of H1N1 HA or dopamine using a probe material.
[0118] Hereinafter, the present invention will be described in further detail with reference to preferred embodiments of the present invention.
[0119] However, it should be understood that these embodiments disclosed herein are intended to illustrate the present invention in detail, but are not intended to limit the scope of the present invention.
[0120] [Manufacturing Example] Synthesis of N-heterocyclic carbene compounds having functionalized terminal regions
[0121] [Manufacturing Example 1] Synthesis of 6-(4-azidobutoxy-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene radical (hereinafter referred to as "NHC1")
[0122] Step 1: Synthesis of 4-(4-bromobutoxy)-2-nitroaniline
[0123] K2CO3 (1.8 g, 13.0 mmol) was added to a solution of anhydrous acetonitrile (65 mL) including 4-amino-3-nitrophenol (2.0 g, 13.0 mmol) and 1,4-dibromobutane (3.64 g, 16.9 mmol). The reaction mixture was stirred at 80 ° C for 12 hours in the presence of argon. After the reaction mixture was cooled to room temperature, the inorganic precipitate was filtered and washed with acetonitrile (50 mL). Thereafter, the solvent was evaporated and the resulting crude product was purified by silica gel column chromatography using a n-hexane: ethyl acetate gradient mixture.
[0124] In this case, the yield was 2.5 g (67%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 10 H 13 ESI-MS (m / z) of BrN2O3: 288.01, calculated value: 288.01.
[0125] Step 2: Synthesis of 5-(4-bromobutoxy)-1H-benzo[d]imidazole
[0126] Formic acid (45 mL) was added to isopropanol (60 mL) containing 4-(4-bromobutoxy)-2-nitroaniline (2.5 g, 8.65 mmol), iron powder (4.8 g, 86.5 mmol) and ammonium chloride (4.6 g, 86.5 mmol). The reaction mixture was stirred at 90 ° C for 16 hours in the presence of argon, cooled to room temperature, and then filtered through a sintered glass filter. The resulting solid was washed with isopropanol (3×50 mL). The filtered liquid was dried by evaporation and neutralized to a pH of 7 by adding a saturated sodium bicarbonate solution. Thereafter, the suspension was extracted with dichloromethane (3×100 mL). The organic layer was dried over sodium sulfate, and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane: methanol gradient mixture.
[0127] In this case, the yield was 1.86 g (80%), and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 10 H 13 ESI-MS (m / z) of BrN2O: 269.14, calculated value: 269.14.
[0128] Step 3: Synthesis of 5-(4-azidobutyloxy)-1H-benzo[d]imidazole
[0129] 5-(4-Bromobutoxy)-1H-benzo[d]imidazole (1.86 g, 6.91 mmol) and sodium azide (NaN3, 0.49 g, 7.6 mmol) were stirred in N,N-dimethylformamide (DMF) (35 mL) at 80 °C for 8 hours in the presence of argon. The reaction mixture was added to water (200 mL) and extracted with ethyl acetate (2×150 mL). The combined organic layers were dried over sodium sulfate and the solvent was evaporated. Thereafter, the crude product was purified by silica gel column chromatography using a dichloromethane: methanol gradient mixture.
[0130] In this case, the yield was 1.4 g (88%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 10 H 13 ESI-MS (m / z) of N5O: 231.25, calculated value: 231.26.
[0131] Step 4: Synthesis of 5-(4-azidobutyloxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide
[0132] 2-Iodopropane (15.1 mL, 151 mmol) was added to a suspension of 5-(4-azidobutyloxy)-1H-benzo[d]imidazole (1.4 g, 6.05 mmol) and cesium carbonate (CsCO, 1.97 g, 6.05 mmol) in acetonitrile (60 mL). The reaction mixture was stirred at 90 ° C for 24 hours in the presence of argon. Thereafter, excess 2-iodopropane and solvent were evaporated under vacuum. The crude product was purified by silica column chromatography using a dichloromethane: methanol gradient mixture.
[0133] In this case, the yield was 1.8 g (67%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 17 H 26 ESI-MS (m / z) of N5OI: 361.20, calculated value: 361.21.
[0134] Step 5: Synthesis of NHC1
[0135] 5-(4-azidobutyloxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide (80 mg, 0.18 mmol) was dissolved in anhydrous tetrahydrofuran (THF) (3.6 mL) and stirred in a glove box to obtain a carbene precursor (pre-carbene). As a blank solution, a 1 M THF solution of potassium hexamethyldisilazide (KHMDS) (0.18 mL, 0.18 mmol) was added dropwise to the mixture at room temperature and then stirred for 15 minutes. It can be observed that a white precipitate (KI) is formed immediately. The resulting mixture is filtered through a 0.2 μm polytetrafluoroethylene (PTFE) syringe filter and diluted with a carbene concentration of 0.05 M to prepare NHC1.
[0136] [Manufacturing Example 2] Synthesis of 6-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene free radical (hereinafter referred to as "NHC2")
[0137] Step 1: Synthesis of 4-(2-(2-(2-bromoethoxy)ethoxy)ethoxy)ethoxy)-2-nitroaniline
[0138] K2CO3 (1.8 g, 13.0 mmol) was added to a solution of anhydrous acetonitrile (65 mL) including 4-amino-3-nitrophenol (2.0 g, 13.0 mmol) and 1-bromo-2-(2-(2-(2-bromoethoxy)ethoxy)ethoxy)ethane (6.24 g, 19.5 mmol). The reaction mixture was stirred at 80 ° C for 12 hours in the presence of argon. After the reaction mixture was cooled to room temperature, the inorganic precipitate was filtered and washed with acetonitrile (80 mL). Thereafter, the solvent was evaporated and the crude product was purified by silica gel column chromatography using a n-hexane:ethyl acetate gradient mixture to obtain the product.
[0139] In this case, the yield was 3.8 g (75%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 14 H 21 ESI-MS (m / z) of BrN2O4: 393.06, calculated value: 393.07.
[0140] Step 2: Synthesis of 5-(2-(2-(2-(2-bromoethoxy)ethoxy)ethoxy)ethoxy)-1H-benzo[d]imidazole
[0141] Formic acid (48 mL) was added to isopropanol (70 mL) containing 4-(2-(2-(2-bromoethoxy)ethoxy)ethoxy)ethoxy-2-nitroaniline (3.8 g, 9.66 mmol), iron powder (5.40 g, 96.6 mmol) and ammonium chloride (5.16 g, 96.6 mmol). The reaction mixture was stirred at 90° C. for 20 hours under argon, cooled to room temperature and then filtered through a sintered glass. The obtained solid was washed with isopropanol (3×50 mL). The filtered liquid was dried by evaporation and neutralized to pH 7 by adding a saturated sodium bicarbonate solution. The suspension was then extracted with dichloromethane (3×100 ml). The organic layer was dried over sodium sulfate and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane:methanol gradient mixture.
[0142] In this case, the yield was 2.8 g (75%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 15 H 31 ESI-MS (m / z) of BrN2O4: 372.06, calculated value: 372.07.
[0143] Step 3: Synthesis of 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1H-benzo[d]imidazole
[0144] 5-(2-(2-(2-(2-(bromoethoxy)ethoxy)ethoxy)ethoxy)ethoxy-1H-benzo[d]imidazole (2.8 g, 7.5 mmol) was stirred with sodium azide (NaN3, 0.536 g, 8.25 mmol) in N,N-dimethylformamide (40 mL) at 80°C under argon for 8 hours. The reaction mixture was added to water (200 mL) and extracted with ethyl acetate (2×150 mL). The organic layer was dried over sodium sulfate and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane:methanol gradient mixture.
[0145] In this case, the yield was 2.0 g (80%), and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 15 H 21 ESI-MS (m / z) of N5O4: 335.15, calculated value: 335.16.
[0146] Step 4: Synthesis of 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide
[0147] 2-Iodopropane (14 mL, 141 mmol) was added to a suspension of 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)ethoxy)-1H-benzo[d]imidazole (1.9 g, 5.66 mmol) and cesium carbonate (1.84 g, 5.66 mmol) in acetonitrile (60 mL). The reaction mixture was stirred at 90 °C for 24 hours in the presence of argon. Thereafter, excess 2-iodopropane and solvent were evaporated under vacuum. The crude product was purified by silica column chromatography using a dichloromethane:methanol gradient mixture.
[0148] In this case, the yield was 2.1 g (70%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 21 H 34 ESI-MS (m / z) of N5O4: 420.26, calculated value: 420.26.
[0149] Step 5: Synthesis of NHC2
[0150] 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide (80 mg, 0.15 mmol) was dissolved in anhydrous THF (3 mL) and stirred in a glove box to obtain the carbene precursor. As a blank solution, 1 M KHMDS (0.15 mL, 0.18 mmol) in THF was added dropwise to the mixture at room temperature and then stirred for 15 minutes. Immediate formation of a white precipitate (KI) was observed. The resulting mixture was filtered through a 0.2 μm PTFE syringe filter and diluted with carbene at a concentration of 0.05 M to prepare NHC2.
[0151] [Manufacturing Example 3] Synthesis of 6-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene radical (hereinafter referred to as "NHC3")
[0152] Step 1: Synthesis of 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazol-3-ium bromide
[0153] Benzyl bromide (11 mL, 82 mmol) was added to a suspension of 5-(2-(2-(2-(2-(azidoethoxy)ethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazole (1.2 g, 3.58 mmol) and cesium carbonate (1.17 g, 3.58 mmol) in acetonitrile (36 mL). The reaction mixture was stirred at 90 °C for 24 hours in the presence of argon. Thereafter, the excess benzyl bromide was evaporated under vacuum. The crude product was purified by silica column chromatography using a dichloromethane:methanol gradient mixture.
[0154] In this case, the yield was 1.7 g (80%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 29 H 34 ESI-MS (m / z) of N5O4: 516.26, calculated value: 516.26.
[0155] Step 2: Synthesis of NHC3
[0156] 5-(2-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazol-3-ium bromide (90 mg, 0.15 mmol) was dissolved in anhydrous THF (3 mL) and stirred in a glove box to obtain the carbene precursor. As a blank solution, 1 M KHMDS (0.15 mL, 0.15 mmol) in THF was added dropwise to the mixture at room temperature and then stirred for 15 minutes. Immediate formation of a white precipitate (KBr) was observed. The resulting mixture was filtered through a 0.2 μm PTFE syringe filter and diluted with carbene at a concentration of 0.05 M to prepare NHC3.
[0157] [Manufacturing Example 4] Synthesis of 6-(4-(1,3-diisoindol-2-yl)butoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene radical (hereinafter referred to as "NHC4")
[0158] Step 1: Synthesis of 2-(4-(4-amino-3-nitrophenoxy)butoxy)isoindoline-1,3-dione
[0159] K2CO3 (1.8 g, 13.0 mmol) was added to a solution of anhydrous acetonitrile (65 mL) including 4-amino-3-nitrophenol (2.0 g, 13.0 mmol) and N-(4-bromobutyl)phthalimide (4.03 g, 14.3 mmol). The reaction mixture was stirred at 80 ° C for 12 hours in the presence of argon. After the reaction mixture was cooled to room temperature, the inorganic precipitate was filtered and washed with acetonitrile (50 mL). Afterwards, the solvent was evaporated and the crude product was purified by silica gel column chromatography using a hexane: ethyl acetate gradient mixture.
[0160] In this case, the yield was 3.65 g (79%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 18 H 17 ESI-MS (m / z) of N3O5: 355.11, calculated value: 355.12.
[0161] Step 2: Synthesis of 2-(4-((1H-benzo[d]imidazol-5-yl)oxy)butyl)isoindoline)-1,3-dione
[0162] Formic acid (45 mL) was added to isopropanol (60 mL) containing 2-(4-(4-amino-3-nitrophenoxy)butoxy)isoindoline-1,3-dione (3.0 g, 8.44 mmol), iron powder (4.71 g, 84.4 mmol) and ammonium chloride (4.51 g, 84.4 mmol). The reaction mixture was stirred at 90 °C for 16 hours in the presence of argon, cooled to room temperature, and then filtered through a sintered glass filter. The obtained solid was washed with isopropanol (3×60 mL). The filtered liquid was dried by evaporation and neutralized to pH 7 by adding a saturated sodium bicarbonate solution. The suspension was then extracted with dichloromethane (3×100 mL). The organic layer was dried over sodium sulfate, and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane:methanol gradient mixture.
[0163] In this case, the yield was 2.1 g (75%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 11 H 13 ESI-MS (m / z) of BrN2O: 335.13, calculated value: 335.13.
[0164] Step 3: Synthesis of 5-(4-(1,3-dihydroisoindolin-2-yl)butoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide
[0165] 2-Iodopropane (15 mL, 149 mmol) was added to a suspension of 2-(4-((1H-benzo[d]imidazol-5-yl)oxy)butyl)isoindoline-1,3-dione (2.0 g, 5.96 mmol) and cesium carbonate (Cs2CO3, 1.94 g, 5.96 mmol) in acetonitrile (60 mL). The reaction mixture was stirred at 90 °C for 24 hours in the presence of argon. Thereafter, excess 2-iodopropane and solvent were evaporated under vacuum. The crude product was purified by silica column chromatography using a dichloromethane: methanol gradient mixture.
[0166] In this case, the yield was 2.1 g (65%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 17 H 26 ESI-MS (m / z) of N5OI: 420.23, calculated value: 420.23.
[0167] Step 4: Synthesis of NHC4
[0168] 5-(4-(1,3-dioxoisoindolin-2-yl)butoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-3-ium iodide (99 mg, 0.18 mmol) was dissolved in anhydrous THF (3.6 mL) and stirred in a glove box to obtain the carbene precursor. As a blank solution, 1 M KHMDS (0.18 mL, 0.18 mmol) in THF was added dropwise to the mixture at room temperature and then stirred for 15 minutes. It was observed that a white precipitate (KI) was formed immediately. The resulting mixture was filtered through a 0.2 μm PTFE syringe filter and diluted with carbene at a concentration of 0.05 M to make NHC4.
[0169] [Manufacturing Example 5] Synthesis of 6-(4-azidobutyloxy-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene radical (hereinafter referred to as "NHC5")
[0170] Step 1: Synthesis of 4-(4-bromobutoxy)-2-nitroaniline
[0171] K2CO3 (1.8 g, 13.0 mmol) was added to a solution of anhydrous acetonitrile (65 mL) including 4-amino-3-nitrophenol (2.0 g, 13.0 mmol) and 1,4-dibromobutane (3.64 g, 16.9 mmol). The reaction mixture was stirred at 80 ° C for 12 hours in the presence of argon. After the reaction mixture was cooled to room temperature, the inorganic precipitate was filtered and washed with acetonitrile (50 mL). Thereafter, the solvent was evaporated and the crude product was purified by silica gel column chromatography using a n-hexane: ethyl acetate gradient mixture.
[0172] In this case, the yield was 2.5 g (67%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 10 H 13 ESI-MS (m / z) of BrN2O3: 288.01, calculated value: 288.01.
[0173] Step 2: Synthesis of 5-(4-bromobutoxy)-1H-benzo[d]imidazole
[0174] Formic acid (45 mL) was added to isopropanol (60 mL) containing 4-(4-bromobutoxy)-2-nitroaniline (2.5 g, 8.65 mmol), iron powder (4.8 g, 86.5 mmol) and ammonium chloride (4.6 g, 86.5 mmol). The reaction mixture was stirred at 90 ° C for 16 hours in the presence of argon, cooled to room temperature, and then filtered through a sintered glass filter. The resulting solid was washed with isopropanol (3×50 mL). The filtered liquid was dried by evaporation and neutralized to a pH of 7 by adding a saturated sodium bicarbonate solution. The suspension was then extracted with dichloromethane (3×100 mL). The organic layer was dried over sodium sulfate, and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane: methanol gradient mixture.
[0175] In this case, the yield was 1.86 g (80%), and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC 11 H 13 ESI-MS (m / z) of BrN2O: 269.14, calculated value: 269.14.
[0176] Step 3: Synthesis of 5-(4-azidobutyloxy)-1H-benzo[d]imidazole
[0177] 5-(4-Bromobutoxy)-1H-benzo[d]imidazole (1.86 g, 6.91 mmol) was stirred with N,N-dimethylformamide (35 mL) sodium azide (NaN3, 0.49 g, 7.6 mmol) at 80 °C for 8 hours in the presence of argon. The reaction mixture was added to water (200 mL) and extracted with ethyl acetate (2×150 mL). The combined organic layers were dried over sodium sulfate and the solvent was evaporated. The crude product was then purified by silica gel column chromatography using a dichloromethane: methanol gradient mixture.
[0178] In this case, the yield was 1.4 g (88%) and the NMR results were as follows: 1 H NMR (600 MHz, CDDl3): δC11 H 13 ESI-MS (m / z) of N5O: 231.25, calculated value: 231.26.
[0179] Step 4: Synthesis of 5-(4-azidobutyloxy)-1,3-dibenzyl-1H-benzo[d]imidazol-3-ium bromide
[0180] Benzyl bromide (20 mL, 20 mmol) was added to a suspension of 5-(4-azidobutyloxy)-1H-benzo[d]imidazole (1.4 g, 6.05 mmol) and cesium carbonate (Cs2CO3, 1.97 g, 6.05 mmol) in acetonitrile (60 mL). The reaction mixture was stirred at 90 ° C for 24 hours in the presence of argon. Thereafter, excess benzyl bromide and solvent were evaporated under vacuum. The crude product was purified by silica column chromatography using a dichloromethane: methanol gradient mixture.
[0181] Step 5: Synthesis of NHC5
[0182] 5-(4-azidobutyloxy)-1,3-dibenzyl-1H-benzo[d]imidazol-3-ium bromide (80 mg, 0.18 mmol) was dissolved in anhydrous THF (3.6 mL) and stirred in a glove box to obtain the carbene precursor. As a blank solution, a THF solution of 1 M KHMDS (0.18 mL, 0.18 mmol) was added dropwise to the mixture at room temperature and stirred for 15 minutes. It was observed that a white precipitate (KI) was formed immediately. The resulting mixture was filtered through a 0.2 μm PTFE syringe filter and diluted with a carbene concentration of 0.05 M to obtain NHC5.
[0183] The molecular formula of the thus prepared NHC5 was determined by nuclear magnetic resonance spectroscopy (NMR). Fig.12 .
[0184] [Example] Fabrication of graphene transistor
[0185] [Example 1] Fabrication of a graphene transistor using NHC1 as a connection layer
[0186] [1-1] Forming a graphene channel layer on a substrate
[0187] like Figures 15 to 17As shown, a copper foil is placed in a chamber and heated to 1,000°C. Then, the heated copper foil is kept for 30 minutes (pre-annealing for 20 minutes and stabilization for 10 minutes) under H2 surrounding at a pressure of 90mTorr and a flow rate of 8sccm, and CH4 is added at a total pressure of 560mTorr and a flow rate of 20sccm for 40 minutes. After that, the copper foil is cooled to 200°C at a rate of 35°C / min, and the furnace is cooled to room temperature to form a single-layer graphene layer on the copper foil.
[0188] Next, a graphene layer on a copper foil was formed by spin coating with a polymethyl methacrylate solution (PMMA) (MicroChem Corp, 950PMMA A4, 4% anisole solution) at a speed of 6,000 rpm / min, and then the graphene layer coated with PMMA was separated from the copper foil with an etchant. The graphene layer separated from the copper foil as described above was immersed in deionized water for 10 minutes to remove residual etchant ions remaining in the graphene layer.
[0189] The thus washed graphene layer was transferred to a polyethylene naphthalate (PEN) film as a substrate, and a PMMA solution was dropped on the graphene layer to remove the PMMA covering the graphene layer. As a result, a graphene channel layer was formed on the substrate. In this case, the transmittance of the graphene channel layer was maintained at 97.8%.
[0190] [1-2] Formation of micropatterned electrodes
[0191] The graphene channel layer formed on the substrate in Example [1-1] was spin-coated with a positive photoresist (AZ5214, Clariant Corp.), and then subjected to ultraviolet exposure, baking, and development processes to form a pattern on the graphene channel layer.
[0192] An oxygen plasma treatment reactive ion etching (RIE) method is used to form patterned electrodes (width (W) / length (L) = 1, L = channel length 100 μm) at both ends of the patterned aligned graphene channel layer, and image inversion, thermal deposition and lift-off processes are performed to manufacture a graphene transistor having micro-patterned electrodes (W / L = 5, L = channel length 100 μm) formed on the graphene channel layer.
[0193] [1-3] used a dip coating method to combine NHC1 with the graphene channel layer.
[0194] Anhydrous THF (5 mL) containing 0.25 mmol of iodinated or brominated benzo [d] imidazole-3-ium was stirred at room temperature in the presence of argon. At the same time, THF (0.25 mmol) including 1M HMDS as a blank solution was added dropwise to the benzo [d] imidazole-3-ium solution and then stirred for 15 minutes to prepare a mixed solution. In this case, it can be observed that a solid precipitate (KI or KBr) was immediately formed. Afterwards, the mixed solution was filtered through a 0.25 μm PTFE syringe filter and diluted with the carbene compound of manufacturing example 1 at a concentration of 0.05 mM to prepare a carbene solution including NHC1. After the filtration was completed, the graphene transistor prepared in Example [1-2] was soaked in the carbene solution at room temperature in the presence of argon for 20 minutes, washed with THF, deionized water (DI) and IPA, and then dried under vacuum to manufacture the graphene transistor of Example 1, wherein the carbene compound of NHC1 was attached to the graphene channel layer.
[0195] [Example 2] Fabrication of a graphene transistor using NHC2 as a connection layer
[0196] A graphene transistor was manufactured in the same manner as in Example 1, except that the N-heterocyclic carbene compound (NHC2) of Manufacturing Example 2 was used.
[0197] [Example 3] Fabrication of a graphene transistor using NHC3 as a connection layer
[0198] A graphene transistor was manufactured in the same manner as in Example 1, except that the N-heterocyclic carbene compound (NHC3) of Manufacturing Example 3 was used.
[0199] [Example 4] Fabrication of a graphene transistor using NHC4 as a connection layer
[0200] A graphene transistor was manufactured in the same manner as in Example 1, except that the N-heterocyclic carbene compound (NHC4) of Manufacturing Example 4 was used, and NHC4 was bonded to the graphene channel layer using the following chemical vapor deposition method.
[0201] The combination of NHC 4 and graphene channel layer is described more specifically as follows using chemical vapor deposition. The anhydrous THF (5mL) containing 0.15 to 0.25mmol of iodinated or brominated benzo [d] imidazole-3-ium is stirred at room temperature in the presence of argon. Meanwhile, as a blank solution, THF (0.15 to 0.25mmol) including 1M KHMDS (0.15 to 0.25mmol) is added dropwise to benzo [d] imidazole-3-ium solution, and then stirred for 15 minutes to prepare a mixed solution. In this case, it can be observed that a solid precipitate (KI or KBr) is formed immediately. Afterwards, the mixed solution is filtered by a PTFE syringe filter of 0.2 μm, and diluted with a concentration of 0.05M with the carbene compound of manufacturing example 4, to prepare the carbene solution including NHC4. After the filtration is completed, the THF solvent is removed from the mixed solution at 50 to 60° C., and the graphene transistor prepared in Example [1-2] is decompressed at 120 to 150° C. at a pressure of 500 mTorr for 15 to 30 minutes to vapor-deposit the carbene compound of NHC4 on the graphene channel layer. Then, the graphene transistor is washed with THF and IPA, and then dried under vacuum to manufacture the graphene transistor of Example 4, in which the carbene compound of NHC4 is attached to the graphene channel layer.
[0202] [Example 5] Fabrication of a graphene transistor using NHC5 as a connection layer
[0203] A graphene transistor was manufactured in the same manner as in Example 1, except that the N-heterocyclic carbene compound (NHC5) of Manufacturing Example 5 was used.
[0204] [Comparative Example 1]
[0205] A graphene transistor was produced in the same manner as in Example 1 except that the N-heterocyclic carbene compound was not used.
[0206] [Comparative Example 2]
[0207] The graphene transistors manufactured in Examples [1-1] and [1-2] were immersed in 30 mL of a methanol solution containing 0.0015% by weight of 1,5-diaminonaphthalene (1,5-diaminonapthalene, DAN) to react with DAN. Thereafter, the residual reactants were removed using distilled water, and the moisture was removed using nitrogen gas, so that the naphthalene rings of DAN formed a π-π interaction with the graphene channel layer. Then, the amino groups (-NH2) of DAN were exposed to the outside to manufacture a DAN π-π interacted graphene transistor (DAN π-πinteracted GT), in which the surface of the graphene channel layer was modified by the amino groups of DAN.
[0208] [Experimental Example 1]
[0209] In order to determine the difference in binding compatibility between the graphene channel layer and the N-heterocyclic carbene compound, the following were prepared: attachment of the biological probe unit (H1N1 HA antibody) to the N-heterocyclic carbene compound, doping of the graphene channel layer, graphene transistor of Example 1 (represented as "alkyl-NHC-covalent GT" in Figure 19d), Example 2, Example 3 (represented as "benzyl-NHC-covalent GT" in Figure 19d), Comparative Example 1 (bare GT) and Comparative Example 2 (DANπ-π interacting GT). Thereafter, 2 μL of H1N1 HA antibody at a concentration of 5 ng / mL was added to the graphene channel layer, and then a biosensor was fabricated in which the H1N1 HA antibody was connected to the connection layer via an EDC-NHS reaction. Modeling was performed according to density functional theory (DFT), and the current-voltage characteristics and transition curve characteristics of the biosensor were measured. The results are shown in Figure 19.
[0210] As shown in a) to c) of Figure 19, it is confirmed that the N-heterocyclic carbene compounds of NHC1 to NHC3 have high band gap energies (equivalent to strong electron density) of 0.51eV, 0.443eV and 0.521eV respectively relative to the graphene channel layer. Therefore, it can be seen that the carbene compound according to the present invention shows excellent binding affinity to the graphene channel layer. As shown in d) of Figure 19, the resistance of the graphene transistor (bare GT) of Comparative Example 1 is the lowest. From these facts, it can be seen that Examples 1 and 3 and the graphene channel layer of Comparative Example 1 are able to bond with carbene compounds. In addition, it is confirmed that the graphene transistors of Example 1 (alkyl-NHC-covalent) and Example 3 (benzyl-NHC-covalent) show increased resistance compared to Comparative Example 2 (π-π interacting GT). Therefore, it can be seen that the H1N1 HA antibody is successfully attached to each of the graphene transistors of Examples 1 and 3.
[0211] Meanwhile, as shown in FIG. 19 e , the graphene channel layer is doped with the N-heterocyclic carbene compound (NHC3)n, because when the H1N1 HA antigen is added, the transition curve shifts to the left by about 0.1 V.
[0212] [Experimental Example 2]
[0213] In order to examine the changes in the graphene channel layer caused by the N-heterocyclic carbene compound and the n-doping of the N-heterocyclic carbene compound, Example 1 (alkyl-NHC-covalent GT), Example 3 (benzyl-NHC-covalent GT), Comparative Example 1 (bare GT) and Comparative Example 2 (π-π interacting GT) were prepared and subjected to Raman spectroscopy analysis. Thereafter, the current-voltage characteristics of the graphene transistor were measured. The results are shown in Fig. 20In this case, pristine graphene refers to graphene in which the graphene channel layer is not functionalized with an N-heterocyclic carbene compound.
[0214] like Fig. 20 As shown in a), the graphene transistor functionalized with azide groups (NHC_N3_graphene, Example 1) or phthalimide groups (NHC_Nph_graphene, Example 3) was -1 ), indicating that the graphene channel layer consists of a single layer.
[0215] In contrast, it can be seen that the graphene transistor of Comparative Example 1, in which the graphene is not functionalized with the N-heterocyclic carbene compound, has a high conductivity at 2,600 (cm -1 ), indicating that the graphene channel layer is composed of multiple layers.
[0216] like Fig. 20 As shown in b), the n-doping increases in the order of the graphene transistors of Comparative Example 1, Comparative Example 2, Example 1, and Example 3. Therefore, it can be seen that the drain current (I ds ) constant gate voltage (V g ) increased negatively, indicating that the attachment amount of N-heterocyclic carbene compounds also increased.
[0217] [Experimental Example 3]
[0218] In order to examine the sensitivity of the biosensor, the graphene transistor of Example 3 (benzyl-NHC covalent GT) was manufactured, in which a carbene compound was formed. After that, 2 μL of H1N1 HA antibody and 2 μL of dopamine antibody (at a concentration of 5 ng / mL) were added to the graphene channel layer, respectively, and then a biosensor was manufactured in which the H1N1 HA antibody and the dopamine antibody were connected to the connection layer by an EDC-NHS reaction. Then, a detection test was performed, using a phosphate buffered saline (PBS) solution to treat the biosensor with H1N1 HA antigens (at a concentration of 0.1 nM to 100 nM) or 100 nM dopamine corresponding to the respective antigens. The results are shown in Fig.13 and 14 .
[0219] like Fig.13 and Fig.14 It was confirmed that the biosensor of the present invention can detect H1N1 HA antigen and dopamine at a concentration of 1 nM and 100 nM, respectively.
[0220] In addition, a graphene transistor of Example 4 in which a carbene compound was formed was manufactured. Thereafter, 2 μL of a geosmin-specific aptamer (5'-CTCTCGGGACGACCCGTTTGTTCCTCGGCTTTTTAAGAGGTCTGGTTGATGTCGTCCC-3', Bioneer Corporation) was added to the graphene channel layer, and then a biosensor was manufactured in which the geosmin-specific aptamer was connected to the biosensor through an EDC-NHS reaction. Then, a detection test was performed by treating the biosensor with a 1 to 100 fg / mL geosmin PBS solution. As a result, it was confirmed that geosmin could be detected at a concentration of 1 fg / mL using the biosensor of the present invention, as shown in FIG. Fig.21 shown.
[0221] In addition, a graphene transistor of Example 5 in which a carbene compound was formed was manufactured. Thereafter, 2 μL of antimicrobial peptide (AMP) (Magainin 1, Lugen Sci Inc.) (concentration of 5 ng / mL) was added to the graphene channel layer, and then a biosensor was manufactured in which AMP was attached to the biosensor by an EDC-NHS reaction. Then, the biosensor was treated with a PBS solution of 10 to 100 CFU / mL of Escherichia coli to perform a detection test. As a result, it was confirmed that the biosensor of the present invention was able to detect Escherichia coli up to 10 CFU / mL, as shown in FIG. Fig. 22 shown.
Claims
1. A graphene transistor, comprising: substrate; A graphene channel layer is disposed on the substrate; a pair of metals, arranged at both ends of the graphene channel layer in a manner of being spaced apart from each other; as well as a connecting layer, disposed on the graphene channel layer, and comprising an N-heterocyclic carbene compound, The N-heterocyclic carbene compound has a chemical structure represented by the following formula 1: [Formula 1] wherein A is an azide group or a phthalimide group, R1 is an alkylene or alkoxyalkylene group having 1 to 10 carbon atoms and containing 1 to 5 repeating units, and R2 and R3 are each independently any one selected from an alkyl group, a cycloalkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkylene group, an alkenylene group, an alkynylene group, an alkoxy group and an aralkyl group.
2. The graphene transistor according to claim 1, wherein: The connecting layer is formed by a covalent bond between a carbene group of the N-heterocyclic carbene compound and the graphene channel layer, and a terminal region of the N-heterocyclic carbene compound is functionalized with an azide group or a phthalimide group, thereby exposing the N-heterocyclic carbene compound.
3. The graphene transistor according to claim 1, wherein: The N-heterocyclic carbene compound includes at least one selected from the group consisting of: 6-4-(azidobutyloxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene free radical, 6-(2-(2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene free radical, 6-(2-(2-( 2-(2-azidoethoxy)ethoxy)ethoxy)ethoxy)-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene free radical, 6-(4-(1,3-diisoindol-2-yl)butoxy)-1,3-diisopropyl-1H-benzo[d]imidazol-2-ylidene free radical and 6-(4-azidobutoxy-1,3-dibenzyl-1H-benzo[d]imidazol-2-ylidene free radical.
4. The graphene transistor according to claim 1, wherein: The N-heterocyclic carbene compound is formed on the graphene channel layer exposed between the pair of metals.
5. The graphene transistor according to claim 1, wherein: The N-heterocyclic carbene compound forms a self-adhesive monolayer.
6. The graphene transistor according to claim 1, wherein: The thickness of the connecting layer is 0.1 nm to 1 nm.
7. The graphene transistor according to claim 1, wherein: The graphene channel layer includes a single layer or a double layer of graphene.
8. A method for manufacturing a graphene transistor, comprising: Using hydrocarbon gas as a carbon source, graphene is grown on a substrate by chemical vapor deposition to form a graphene channel layer; forming a pair of metals on the graphene channel layer by a thermal deposition process; and Using a surface treatment agent containing an N-heterocyclic carbene compound, forming a connection layer on the surface of the graphene channel layer exposed to the outside, The N-heterocyclic carbene compound has a chemical structure represented by the following formula 1: [Formula 1] wherein A is an azide group or a phthalimide group, R1 is an alkylene or alkoxyalkylene group having 1 to 10 carbon atoms and containing 1 to 5 repeating units, and R2 and R3 are each independently any one selected from an alkyl group, a cycloalkyl group, an alkenyl group, an alkynyl group, an aryl group, an alkylene group, an alkenylene group, an alkynylene group, an alkoxy group and an aralkyl group.
9. The manufacturing method according to claim 8, wherein: The N-heterocyclic carbene compound is synthesized using an imidazolium salt as a raw material.
10. A biosensor comprising the graphene transistor according to any one of claims 1 to 7.
11. The biosensor according to claim 10, wherein: The biosensor includes a bioprobe unit bonded to an azide group or a phthalimide group of a connection layer exposed to the graphene transistor, and The biological probe unit includes a probe material, and the probe material includes at least one selected from DNA, RNA, antigen, antibody and peptide.
12. The biosensor according to claim 11, wherein The antigen and the antibody are H1N1 HA antigen and H1N1 HA antibody, respectively.
Citation Information
Patent Citations
Graphene complex composition and transparent conductive film using thereof
KR1020100090552A
Layered structure of graphene, process for preparing the same, and transparent electrode and transistor comprising the structure
KR1020130006869A
Electronics comprising carbon thin film and electrochemical device comprising carbon thin film
KR1020130007528A
Method for manufacturing graphene thin film and graphene thin film manufactured by the same
KR1020150129108A
Production of chemically functionalized nano graphene materials
US20110017587A1