Low temperature polycrystalline semiconductor device and method for manufacturing the same

By using NiCxOy and other materials as seed layers, the problems of polycrystalline silicon film quality and Ni pollution in LTPS TFT are solved, and the formation and large-area application of high-quality polycrystalline silicon films are achieved, reducing process costs and complexity.

CN111902930BActive Publication Date: 2024-11-26洪瑛
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980021419.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-10-29
Filing Date
2019-03-05
Publication Date
2024-11-26
Estimated Expiration
2039-03-05

AI Technical Summary

Technical Problem

In the prior art, when manufacturing low-temperature polysilicon thin film transistors (LTPS TFTs), it is difficult to form high-quality polysilicon thin films at low process costs, and the problems of grain uniformity and Ni element pollution in large-area displays have not been effectively solved.

Method used

Using materials such as NiCxOy, NiNxOy, NiCxNyOz as seed layers, the amorphous silicon layer is crystallized by heat treatment, combined with the catalytic reaction control layer and patterning process, a high-quality polycrystalline silicon film is formed, and the source is activated without using ion implantation. Pole and drain, reducing the lithography process stage.

Benefits of technology

A high-quality (111)-oriented LTPS film has a crystallinity of greater than or equal to 98%, reducing Ni pollution, expanding large-area applications, and reducing manufacturing costs and process complexity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN111902930B_ABST
    Figure CN111902930B_ABST
Patent Text Reader

Abstract

The present invention relates to a semiconductor device and a method for manufacturing the semiconductor device, the method comprising: a step of forming a buffer layer made of an insulating material on a substrate; a step of forming a seed layer made of at least one material selected from the group consisting of: NiCx-Oy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, NiCxNyOz:H, NixSiy and NixGey on the buffer layer; a step of forming a silicon layer of an amorphous silicon layer on the seed layer; and a step of crystallizing the amorphous silicon layer by heat treating the amorphous silicon layer to crystallize the amorphous silicon layer by catalysis of nickel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a poly MOS device and a method of manufacturing the same, and more particularly, to a CMOS using LTPS TFT. Background Art

[0002] Low temperature polycrystalline silicon thin film transistors (LTPS TFTs) with high mobility and high reliability are suitable as pixel switching devices for active-matrix organic light-emitting diode (AM-OLED) displays widely used in mobile devices such as smartphones.

[0003] Excimer Laser Annealing (ELA) is mainly used for crystallization of silicon to manufacture LTPS TFTs. Such LTPS TFTs have high mobility and high reliability, but may not maintain a certain level of crystal grain uniformity in a large-area display in which a large number of TFTs are arranged.

[0004] The MIC and MILC technologies that have been extensively studied in LTPS technology cause contamination of the Ni element and leakage current in the device, and are therefore not used in actual products. The ELA technology is accompanied by expensive equipment and high process costs, and the Metal Induced Crystallization (MIC) and Metal Induced Lateral Crystallization (MILC) methods using metal catalysts are cheap in terms of cost, but result in lower quality polysilicon thin films. Summary of the invention

[0005] Technical issues

[0006] Provided are a semiconductor device capable of forming a high-quality polysilicon thin film at a low process cost and a method for manufacturing the same.

[0007] Also provided is an LTPS semiconductor device which can have a large area by efficiently forming LTPS and a method for manufacturing the same.

[0008] Technical solutions to the problem

[0009] In a method of manufacturing an LTPS semiconductor device according to one aspect of the present disclosure, LTPS is formed by using a thin film made of at least one selected from the group consisting of NiCxOy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, NiCxNyOz:H, NixSiy, and NixGey as a seed.

[0010] According to one aspect of the present disclosure, a method for manufacturing a semiconductor device includes:

[0011] forming a buffer layer of insulating material on the substrate;

[0012] A seed layer forming operation of forming a seed layer of at least one selected from the group consisting of NiCxOy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, NiCxNyOz:H, NixSiy, and NixGey on the buffer layer;

[0013] A silicon layer forming operation of forming an amorphous silicon layer on the seed layer; and

[0014] A crystallization operation is performed in which the amorphous silicon layer is crystallized by a catalytic effect of Ni by heat-treating the amorphous silicon layer.

[0015] The method may further include forming a catalytic reaction controlling layer between the seed layer forming operation and the silicon layer forming operation.

[0016] The silicon layer forming operation may include:

[0017] forming an amorphous intrinsic silicon layer for forming a channel on the buffer layer;

[0018] forming an extrinsic silicon layer for forming a source / drain on the amorphous intrinsic silicon layer; and

[0019] A metal layer is formed on the extrinsic silicon layer.

[0020] The extrinsic silicon layer may be formed such that a first extrinsic silicon layer in contact with an amorphous silicon layer for forming a semiconductor channel has a lower doping concentration than a second extrinsic silicon layer.

[0021] The method may further include, after the crystallizing operation, a patterning operation of forming a source electrode and a drain electrode corresponding to the intrinsic silicon layer by patterning the metal layer and the extrinsic silicon layer.

[0022] The patterning operation may include:

[0023] exposing the first extrinsic silicon layer in a channel region between the source electrode and the drain electrode by patterning the metal layer and the second extrinsic silicon layer;

[0024] A spacer forming operation of forming an insulating spacer on the source electrode and an inner side of the second extrinsic silicon layer thereunder and on the drain electrode and an inner side of the second extrinsic silicon layer thereunder, wherein a lower end of the spacer covers the first extrinsic silicon layer with a preset width; and

[0025] A portion of the first extrinsic silicon layer not covered by the spacer is etched.

[0026] A P-type metal oxide semiconductor (PMOS) region and an N-type metal oxide semiconductor (NMOS) region may be divided on the extrinsic silicon layer, and

[0027] The silicon layer forming operation may include:

[0028] A p-type extrinsic silicon layer and a metal layer thereon are formed in the PMOS region, and an n-type extrinsic silicon layer and a metal layer thereon are formed in the NMOS region.

[0029] According to another aspect of the present disclosure, a semiconductor device may include:

[0030] Substrate

[0031] a buffer layer formed on the substrate;

[0032] a channel layer formed by an intrinsic polysilicon layer on the buffer layer;

[0033] polycrystalline source and drain formed of extrinsic silicon on both sides of the polycrystalline silicon layer;

[0034] A source electrode and a drain electrode, formed on the polycrystalline source electrode and the drain electrode;

[0035] a gate electrode corresponding to the channel layer; and

[0036] A NiSi2 contact layer is located between the source and the source electrode and between the drain and the drain electrode.

[0037] The extrinsic polycrystalline source and drain may include:

[0038] a first extrinsic silicon layer contacting both sides of the channel layer; and

[0039] A second extrinsic silicon layer is disposed on the first extrinsic silicon layer, wherein

[0040] The first extrinsic silicon layer may extend further toward the gate than the second extrinsic silicon layer to form a lightly doped drain (LDD).

[0041] A PMOS region and an NMOS region may be divided on the substrate, a p-type TFT including a source and a drain formed by a p-type extrinsic silicon layer may be formed in the PMOS region, and an n-type TFT including a source and a drain formed by an n-type extrinsic silicon layer may be formed in the NMOS region.

[0042] The beneficial effects of disclosure

[0043] According to example embodiments, a high-quality LTPS with a main orientation of (111) can be obtained, and the contamination of Ni can be negligibly reduced. When the crystallization of an a-Si film is induced by using an amorphous thin film seed layer made of at least one selected from the group consisting of NiCxOy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, NiCxNyOz:H, NiCxNyOz:H, NixSiy and NixGey, Ni is precipitated to the surface of the film and is therefore not retained in the TFT channel. The crystallinity of the LTPS is greater than or equal to 98%, the surface RMS is small, the particle uniformity is high, a large area can be expanded, the manufacturing cost is low and the productivity is high. In addition, compared with the existing method of manufacturing an LTPS semiconductor device, the method according to the example embodiment can reduce the photolithographic process by at least two stages. In addition, for the existing source-drain doping process, when the silicon channel is crystallized without ion implantation, the activation of the source and drain is performed simultaneously, and in particular, the activation of the source and drain can serve as a mass production process for a-Si TFTs, thereby enabling sharing of manufacturing facilities. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figures 1A to 1J Operations of a process for fabricating a semiconductor device according to the present disclosure are shown.

[0045] Figure 2A to Figure 2K Operations of a process for fabricating a CMOS device according to the present disclosure are shown. DETAILED DESCRIPTION

[0046] Hereinafter, example embodiments of the present disclosure will be described in detail with reference to the accompanying drawings. However, the embodiments of the present disclosure may be modified into various forms, and the scope of the present disclosure should not be understood to be limited to the embodiments described below. The embodiments of the present disclosure may be interpreted as providing to further thoroughly explain the spirit of the present disclosure to those skilled in the art. The same reference numerals in the figures indicate the same elements. The various elements and regions in the figures are schematically drawn. Therefore, the spirit of the present disclosure is not limited to the relative sizes or intervals drawn in the drawings.

[0047] Although the terms first, second, etc. may be used herein to describe various elements, these elements should not be limited to these terms. These terms are only used to distinguish one element from another element. For example, without departing from the scope of the present disclosure, a first element may be referred to as a second element, and conversely, a second element may be referred to as a first element.

[0048] The terms used herein are for the purpose of describing specific embodiments only and are not intended to limit example embodiments. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. It should be further understood that when used in this specification, the terms "comprises" and / or "have" specify the presence of stated features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.

[0049] Unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as commonly understood by one of ordinary skill in the art to which example embodiments belong. It should be further understood that terms, such as those defined in commonly used dictionaries, should be interpreted as having a meaning consistent with their meaning in the context of the relevant art and should not be interpreted in an idealized or overly formal sense unless explicitly so defined herein.

[0050] When a certain embodiment can be implemented in different ways, the specific processing order can be performed differently from the described order. For example, two processes described in succession can be performed substantially at the same time or can be performed in the reverse order of the described order.

[0051] Therefore, it is expected that the shapes shown in the figure will vary due to, for example, manufacturing techniques and / or tolerances. Therefore, the example embodiments should not be understood to be limited to the specific shapes of the zones shown herein, but may include, for example, shape deviations caused by manufacturing. As used herein, the term "and / or" includes any and all combinations of one or more of the associated listed items. The term "substrate" as used herein may mean the substrate itself or a stacked structure including a substrate and a predetermined layer or film formed on its surface. As used herein, "the surface of the substrate" may mean the exposed surface of the substrate itself, or the outer surface of a predetermined layer or film formed on the substrate. What is described as "above" or "on" may include not only those that are directly in contact with ..., but also those that are non-contacting above ....

[0052] Hereinafter, a method of manufacturing a MOS FET according to an example embodiment and a complementary metal-oxide semiconductor (CMOS) applying the MOS FET will be described in detail with reference to the accompanying drawings. In the following description, silicon is referred to as a channel material of a transistor, but according to another example embodiment, other semiconductor materials (e.g., germanium) other than silicon may be applied as an alternative material.

[0053] Figures 1A to 1J The main processes in the process of manufacturing a metal oxide silicon field effect transistor (MOS FET) according to the present disclosure are schematically illustrated.

[0054] like Figure 1A As shown in FIG. 1 , a buffer layer 11 is formed of an insulating material on a substrate 10. An electronic device structure formed in a previous process may exist below the buffer layer 11. The substrate 10 may be a glass substrate or a plastic substrate. The buffer layer 11 may be formed of an insulating material used to manufacture semiconductor devices, for example, may be formed of one of SiO2, SiNx, SiONx, or AlOx.

[0055] like Figure 1BAs shown in FIG. 1 , an amorphous seed layer 12 having a thickness of several nanometers is formed on the buffer layer 11. The seed layer 12 may be formed by atomic layer deposition (ALD), and the constituent material of the seed layer 12 is one of NiCxOy, NiNxOy, and NiCxNyOz, or one of NiCxOy:H, NiNxOy:H, and NiCxNyOz:H containing hydrogen (H). In addition to the above materials, the material of the seed layer 12 may be NixSiy or NixGey.

[0056] like Figure 1C As shown in , an intrinsic silicon layer 13 is formed by depositing intrinsic a-Si on a seed layer 12. Here, the thickness of the intrinsic silicon layer 13 can be adjusted within a range of about 50 nanometers to about 150 nanometers. As a selective element, a catalytic reaction control layer 12a can be formed between the seed layer 12 and the silicon layer 13 to suppress or control the violent reaction between the Ni catalyst material and silicon due to the direct contact between the seed layer 12 and the silicon layer 13. Before the silicon layer 13 is formed, a catalytic reaction control layer 12a with a thickness of several angstroms to several nanometers can be formed, and the Ni catalyst material can penetrate through the thickness. The maximum thickness of the catalytic reaction control layer 12a is limited to the thickness of the silicon layer 13 through which the Ni catalyst material can pass to reach it. The catalytic reaction control layer 12a can be formed of a common insulating material, such as SiO2, SiNx, SiONx or AlOx.

[0057] like Figure 1D As shown in FIG. 1 , a doped or non-intrinsic silicon layer 14 doped with a p-type dopant or an n-type dopant and a metal layer 15 are sequentially stacked on an intrinsic silicon layer 13. Among the dopants, the p-type dopant includes at least one selected from the group consisting of B, Al, Ga, and In, and the n-type dopant includes at least one selected from the group consisting of P, Sb, and As.

[0058] Here, the extrinsic silicon layer 14 may be formed as a single layer doped with a p-type dopant or an n-type dopant at a preset concentration, and according to the present embodiment, may include a first extrinsic silicon layer 14a and a second extrinsic silicon layer 14b having different doping concentrations. For example, the doping concentration of the first extrinsic silicon layer 14a in contact with the intrinsic silicon layer 13 is lower than the doping concentration of the second extrinsic silicon layer 14b thereon, and the first extrinsic silicon layer 14a and the second extrinsic silicon layer 14b are crystallized into polycrystalline silicon in a subsequent heat treatment process. The metal layer 15 may have a single layer or a multilayer structure. According to the present embodiment, the metal layer 15 may have a sandwich structure having a stacked structure of TiN / Al / TiN.

[0059] After the metal layer 15 is completed as described above, an a-Si island to be used as a channel of the TFT is formed by patterning the intrinsic silicon layer formed in the transistor region (particularly, formed on the entire surface of the substrate 10 ).

[0060] like Figure 1E As shown in FIG. 1 , Metal Induced Crystallization (MIC) is performed by heat treatment. According to this heat treatment, the a-Si of the amorphous silicon layer 13 on the seed layer 12 is crystallized, and thus, the silicon layer 13 formed of polycrystalline Si oriented in the (111) direction is obtained. In this process, Ni and Si of the seed layer 12 react with each other to produce NiSi2, which reaches the uppermost extrinsic silicon layer 14 after passing through the silicon layer 13 to form a contact layer 12' between the extrinsic silicon layer 14 and the metal layer 15, and nickel is precipitated to the outside of the extrinsic silicon layer 14 after the crystallization is completed. In addition, in the MIC process, the extrinsic silicon layer 13 is crystallized together, and the dopant of the extrinsic silicon layer 14 is activated to form a conductive region.

[0061] According to the example embodiments described above, source / drain doping by conventional ion implantation can be achieved by deposition of the non-intrinsic silicon layer 14 and the MIC process without a separate ion implantation process. At the current stage, the source and drain are not isolated yet, and the source S and drain D are obtained by a subsequent patterning process of the non-intrinsic silicon layer 14.

[0062] like Figure 1F As shown in FIG. 1 , the metal layer 15 and the second extrinsic silicon layer 14 b thereunder are patterned by using a photolithography method, thereby forming a source S and a drain D and a source electrode 15 a and a drain electrode 15 b corresponding thereto on both sides of the silicon semiconductor channel region C. According to this patterning, a portion of the first extrinsic silicon layer 14 a covering the intrinsic silicon layer 13 is exposed on the surface of the silicon semiconductor channel region C.

[0063] Here, the extension region of the first extrinsic silicon layer 14 a not covered by the second extrinsic silicon layer 14 b corresponds to a lightly doped drain (LDD) having lower conductivity than the second extrinsic silicon layer 14 b .

[0064] like Figure 1GAs shown in FIG. 1 , a spacer 16 for covering the upper portion of the first extrinsic silicon layer 14a is formed on opposite sides of a source electrode 15a and a drain electrode 15b, which are formed above both sides of the intrinsic silicon layer 13 at a predetermined height. The spacer 16 is formed not only on the side of the source electrode 15a and the drain electrode 15b, but also on the side of the second extrinsic silicon layer 14b under the source electrode 15a and the drain electrode 15b, and the lower end of the second extrinsic silicon layer 14b covers the surface of the first extrinsic silicon layer 14a. The spacer 16 may be formed of an insulating material (e.g., SiO2 or SiNx), and the spacer 16 covering the LDD region may be obtained by an entire surface deposition of SiO2 or SiNx and an etch back process.

[0065] like Figure 1H As shown in FIG. 1 , a portion of the extrinsic silicon layer between the source electrode 15a and the drain electrode 15b that is not covered by the spacer 16 is removed. Through this etching back process, the extension portion 14a′ of the first extrinsic silicon layer 14a corresponding to the LDD region is located under the spacer 16.

[0066] like Fig. 1I As shown in FIG. 1 , a gate insulating layer 17 is formed on the entire surface of the source electrode 15 a and the drain electrode 15 b and the intrinsic silicon layer 13 exposed therebetween, and a gate electrode 18 is formed in a channel region between the source electrode 15 a and the drain electrode 15 b.

[0067] Here, the gate insulating layer 17 may be formed of one of SiNx, SiO2, AlOx, or HfOx. The gate electrode 18 may be obtained by depositing and patterning the entire surface of MoW.

[0068] like Figure 1J As shown in the figure, an interlayer dielectric layer 19 having a contact hole 19a is formed on the gate electrode 18, and an electrode pad Ps, an electrode pad Pg and an electrode pad Pd which are electrically connected to the source electrode 15a, the drain electrode 15b and the gate electrode 18 respectively through the contact hole 19a are formed on the ILD layer 19.

[0069] In the above-described processes, only main parts have been described to help understand the example embodiments without describing a method of manufacturing a complete MOS.

[0070] In the following, reference will be made to Figure 2A to Figure 2K An embodiment of a method of manufacturing a CMOS for a display is described.

[0071] like Figure 2AAs shown in FIG. 1 , a buffer layer 21 and an amorphous seed layer 22 are sequentially formed on a substrate 20, defining (dividing) a PMOS region and an NMOS region in the substrate 20. The buffer layer 21 may be formed of one of SiO2, SiNx, SiONx, or AlOx.

[0072] The seed layer 22 is formed to a thickness of several nanometers. The seed layer 22 may be formed using thermal ALD, plasma enhanced thermal atomic layer deposition (PE-ALD), plasma enhanced chemical vapor deposition (PECVD), or the like. The constituent material of the seed layer 22 is at least one selected from the group consisting of NiCxOy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, NiCxNyOz:H, NixSiy, and NixGey. The material of the seed layer 22 material may include the crystallization of silicon at a lower temperature than the existing NiOx, thereby obtaining high-quality polycrystalline silicon.

[0073] like Figure 2B As shown in FIG. 2 , an intrinsic silicon layer 23 to be used as a channel of a transistor is formed of amorphous silicon on a seed layer 22. Here, the thickness of the intrinsic silicon layer 23 is about 50 nanometers to about 150 nanometers. A catalytic reaction control layer 22a as described above may be selectively formed. In other words, the catalytic reaction control layer 22a is a selective element and may be formed before the intrinsic silicon layer 23 is formed. The catalytic reaction control layer 22a may be formed of a common insulating material, such as SiOx, SiONx, or AlOx.

[0074] like Figure 2C As shown in FIG. 2 , a p-type extrinsic silicon layer 24 including a p-type dopant and a first metal layer 25 are sequentially formed on the intrinsic silicon layer 23. Here, the p-type extrinsic silicon layer 24 may be formed of a plurality of layers having different doping concentrations.

[0075] In the present embodiment, the p-type extrinsic silicon layer 24 includes a first extrinsic silicon layer 24a and a second extrinsic silicon layer 24b thereon. The doping concentration of the second extrinsic silicon layer 24b is relatively higher than the doping concentration of the first extrinsic silicon layer 24a. The first metal layer 25 may have a multilayer structure in which layers of the same or different types are stacked. According to the present embodiment, the first metal layer 25 may have a sandwich structure having a stacking structure of TiN / Al / TiN.

[0076] like Figure 2DAs shown in FIG. 1 , the p-type extrinsic silicon layer 24 is patterned from the first metal layer 25. Here, only the PMOS region is retained, and the p-type extrinsic silicon layer 24 is removed by etching from the first metal layer 25 in the remaining region. To this end, for a detailed example, the PMOS region to be protected is covered by a mask layer such as a photoresist, and then etched to remove the p-type extrinsic silicon layer 24 and the first metal layer 25 outside the PMOS region, including the NMOS region.

[0077] After the selective etching as described above, cleaning is performed, and then a stack structure including an n-type extrinsic silicon layer 26 in the NMOS region and a second metal layer 27 thereon is formed on the intrinsic silicon layer 23 in the NMOS region.

[0078] like Figure 2E As shown in FIG. 1 , an n-type extrinsic silicon layer 26 and a second metal layer 27 are formed in the NMOS region except the PMOS region. This process includes a process of depositing extrinsic silicon material and metal on the entire surface, and a process of removing the n-type extrinsic silicon and the metal thereon in a portion not including the NMOS region.

[0079] like Figure 2F As shown in the figure, the stacked structure for manufacturing p-type TFT and n-type TFT in the PMOS region and NMOS region obtained by the process described above is patterned, so that silicon islands 23a and silicon islands 23b that will serve as channels of p-type TFT and n-type TFT are formed from the amorphous non-intrinsic silicon layer 23.

[0080] like Figure 2G As shown in FIG. 1 , MIC is performed by heat treatment to form polycrystalline islands 23a' and 23b' from silicon islands 23a and 23b, which are (111) oriented. In this process, not only intrinsic silicon is crystallized, but also extrinsic silicon is crystallized. According to this crystallization, Ni and Si of the catalyst layer present under the intrinsic silicon layer 23 contact each other to form NiSi2, and NiSi2 rises to the top of the silicon layer and contacts the first metal layer 25 and the second metal layer 27 to act as a contact layer between silicon and metal.

[0081] In this embodiment, the heat treatment may be performed in a common furnace, and may also be performed in a furnace to which an electromagnetic field is applied.

[0082] like Figure 2H As shown in FIG. 1 , the first metal layer 25 and the second metal layer 27 are patterned to form source electrodes 25a and 27a and drain electrodes 25b and 27b in the PMOS region and the NMOS region, and the first extrinsic silicon layer 24a and the first extrinsic silicon layer 26a are exposed under the channel region C therebetween.

[0083] Over both sides of the intrinsic silicon layer 23, spacers 29 covering the first extrinsic silicon layer 24a and the first extrinsic silicon layer 26a are formed on opposite sides of the source electrodes 25a and 27a and the drain electrodes 25b and 27b formed at a preset height in the source region S and the drain region D. The spacers 29 are formed not only on the side surfaces of the source electrodes 25a and 27a and the drain electrodes 25b and 27b, but also on the side surfaces of the second extrinsic silicon layer 24b and the second extrinsic silicon layer 26b under the source electrodes 25a and 27a and the drain electrodes 25b and 27b, and the lower ends thereof cover the surfaces of the first extrinsic silicon layer 24a and the first extrinsic silicon layer 26a providing the LDD region by a preset width. The spacer 29 may be formed of an insulating material such as SiO 2 (or SiN x ) and the spacer 29 covering the LDD region may be obtained by an entire surface deposition of SiO 2 (or SiN x ) and an etch back process.

[0084] like Fig.2I As shown in FIG. 1 , the first extrinsic silicon layer 24a and the first extrinsic silicon layer 26a not covered by the spacer 29 are removed to expose the surfaces of the polysilicon islands 23a' and 23b' thereunder. Here, the surfaces of the polysilicon islands 23a' and 23b' are exposed by a self-aligned etching method using the source electrodes 25a and 27a, the drain electrodes 25b and 27b, and the spacer 29 as masks.

[0085] like Figure 2J As shown in FIG. 1 , a gate insulating layer 30 is formed on the PMOS region and the NMOS region, and each of the gate electrodes 31 a and 31 b is formed in a channel region of each of the PMOS region and the NMOS region.

[0086] Here, the gate insulating layer 30 may be formed of one of SiNx, SiO2, AlOx, or HfOx. The gate electrodes 31a and 31b may be obtained by depositing and patterning the entire surface of MoW.

[0087] like Figure 2K As shown in FIG. 1 , an ILD layer 32 having contact holes 32a connected to source electrodes 25a and 27a, drain electrodes 25b and 27b, and gate electrodes 31a and 31b is formed. Here, metal pads 33s, 33g, 33d, 34s, 34g, and 34d are formed to complete a CMOS having a PMOS TFT and an NMOS TFT. Thereafter, a process of forming additional elements of a device to which these CMOS are applied may be performed.

[0088] In the above process, each of the intrinsic amorphous silicon layer and the extrinsic silicon layer including an n-type dopant or a p-type dopant may be deposited in an independent cluster chamber.

[0089] The materials of the source / drain electrodes and the gate electrode as described above are associated with the control of the threshold voltage Vth of the device, and therefore need to be appropriately combined. In addition, the LDD of the first extrinsic silicon layer is associated with the control of the drain current and the control of the threshold voltage Vth, and therefore, whether LDD will be formed can be determined by the control of the drain current and the threshold voltage Vth. For example, LDD may not be formed in PMOS.

[0090] As described above, the method of manufacturing an LTPS TFT and a CMOS using the LTPS TFT according to the present disclosure is crystallized by basically using an amorphous Ni-based oxide as a catalyst. As a seed layer formed of a Ni-based oxide, one of NiCxOy, NiNxOy, and NiCxNyOz other than NiOx may be applied, or one of NiCxOy:H, NiNxOy:H, and NiCxNyOz:H containing hydrogen (H) may be applied. In addition, the seed layer may be formed of NixSiy or NixGey.

[0091] Through this process, a (111)-oriented LTPS TFT on a glass substrate or a plastic substrate can be obtained, and a CMOS can also be formed by using the LTPS TFT.

[0092] In addition, when a polysilicon channel is formed, an intrinsic silicon layer for the silicon channel and intrinsic silicon for the source and drain, i.e. silicon containing n-type dopants or p-type dopants, are formed. Therefore, in the MIC process, crystallization of intrinsic silicon and crystallization and activation of extrinsic silicon for the source and drain are simultaneously achieved without the existing separate ion implantation process.

[0093] In addition, the extrinsic silicon forming the source and drain is formed in multiple layers. Here, the dopant concentration of the first intrinsic silicon layer contacting the silicon channel may be lower than the dopant concentration of the second extrinsic silicon layer thereon, and the first extrinsic silicon layer may extend closer to the center of the channel than the second extrinsic silicon layer, thereby implementing an LDD with low conductivity.

[0094] The method of manufacturing a semiconductor device according to an example embodiment has been described with reference to the embodiment illustrated in the drawings to help understand the present disclosure, but this is only an example. Those skilled in the art should understand that various modifications and other equivalent embodiments from the examples are possible. Therefore, the technical scope of the present disclosure should be defined by the appended claims.

Claims

1. A method for manufacturing a semiconductor device, the method comprising: forming a buffer layer of insulating material on the substrate; A seed layer forming operation of forming a seed layer of at least one selected from the group consisting of NiCxOy, NiNxOy, NiCxNyOz, NiCxOy:H, NiNxOy:H, and NiCxNyOz:H on the buffer layer; forming an amorphous intrinsic silicon layer for forming a channel on the buffer layer; forming an amorphous non-intrinsic silicon layer for forming a source electrode and / or a drain electrode on the amorphous intrinsic silicon layer; forming a metal layer on the amorphous extrinsic silicon layer; as well as A crystallization operation of crystallizing the amorphous intrinsic silicon layer and the amorphous extrinsic silicon layer by a catalytic effect of nickel by heat treating the amorphous intrinsic silicon layer and the amorphous extrinsic silicon layer, The amorphous extrinsic silicon layer includes a first extrinsic silicon layer in contact with the amorphous intrinsic silicon layer and a second extrinsic silicon layer on the first extrinsic silicon layer.

2. The method for manufacturing a semiconductor device according to claim 1, further comprising: A catalytic reaction controlling layer is formed after the seed layer forming operation and before the amorphous intrinsic silicon layer is formed on the buffer layer.

3. The method for manufacturing a semiconductor device according to claim 1, further comprising: After the crystallization operation, a patterning operation is performed to form a source electrode and a drain electrode corresponding to the amorphous intrinsic silicon layer by patterning the metal layer and the amorphous extrinsic silicon layer.

4. The method for manufacturing a semiconductor device according to claim 3, wherein the patterning operation comprises: exposing the first extrinsic silicon layer in a channel region between the source electrode and the drain electrode by patterning the metal layer and the second extrinsic silicon layer; A spacer forming operation of forming an insulating spacer on the source electrode and an inner side of the second extrinsic silicon layer thereunder and on the drain electrode and an inner side of the second extrinsic silicon layer thereunder, wherein a lower end of the spacer covers the first extrinsic silicon layer with a preset width; and A portion of the first extrinsic silicon layer not covered by the spacer is etched.

5. The method for manufacturing a semiconductor device according to claim 1, wherein Arranging a P-type metal oxide semiconductor region and an N-type metal oxide semiconductor region in the amorphous extrinsic silicon layer, and the method further comprises: A p-type extrinsic silicon layer and a metal layer thereon are formed in the P-type metal oxide semiconductor region, and an n-type extrinsic silicon layer and a metal layer thereon are formed in the N-type metal oxide semiconductor region.

6. The method for manufacturing a semiconductor device according to claim 3, wherein Arranging a P-type metal oxide semiconductor region and an N-type metal oxide semiconductor region in the amorphous extrinsic silicon layer, and the method further comprises: A p-type extrinsic silicon layer and a metal layer thereon are formed in the P-type metal oxide semiconductor region, and an n-type extrinsic silicon layer and a metal layer thereon are formed in the N-type metal oxide semiconductor region.

7. The method for manufacturing a semiconductor device according to claim 4, wherein Arranging a P-type metal oxide semiconductor region and an N-type metal oxide semiconductor region on the amorphous extrinsic silicon layer, and the method further comprises: A p-type extrinsic silicon layer and a metal layer thereon are formed in the P-type metal oxide semiconductor region, and an n-type extrinsic silicon layer and a metal layer thereon are formed in the N-type metal oxide semiconductor region.

8. A semiconductor device manufactured by the method according to claim 1 to claim 7, the semiconductor device comprising: substrate; a buffer layer formed on the substrate; a channel layer formed by an intrinsic polysilicon layer on the buffer layer; an extrinsic polycrystalline source and drain formed of extrinsic silicon on both sides of the polycrystalline silicon layer; A source electrode and a drain electrode, formed on the polycrystalline source electrode and the drain electrode; a gate electrode corresponding to the channel layer; as well as A NiSi2 contact layer is located between the source and the source electrode and between the drain and the drain electrode.

9. The semiconductor device of claim 8, wherein the extrinsic polycrystalline source and drain comprise: A first extrinsic silicon layer, contacting two sides of the channel layer; as well as A second extrinsic silicon layer is disposed on the first extrinsic silicon layer, wherein The first extrinsic silicon layer extends further toward the gate electrode than the second extrinsic silicon layer to form a lightly doped drain.

10. The semiconductor device according to claim 8, wherein A P-type metal oxide semiconductor region and an N-type metal oxide semiconductor region are divided on the substrate, and A p-type thin film transistor including a source and a drain formed of a p-type extrinsic silicon layer is formed in the p-type metal oxide semiconductor region, and an n-type thin film transistor including a source and a drain formed of an n-type extrinsic silicon layer is formed in the n-type metal oxide semiconductor region.

11. The semiconductor device according to claim 9, wherein A P-type metal oxide semiconductor region and an N-type metal oxide semiconductor region are divided on the substrate, and A p-type thin film transistor including a source and a drain formed of a p-type extrinsic silicon layer is formed in the p-type metal oxide semiconductor region, and an n-type thin film transistor including a source and a drain formed of an n-type extrinsic silicon layer is formed in the n-type metal oxide semiconductor region.