Semiconductor memory device and method of manufacturing the same
By adopting a dielectric layer with a multi-layer oxide structure in a semiconductor memory device, using multiple regions and annealing processes of zirconium, aluminum and oxides, the problem of insufficient leakage current and thermal stability under high integration is solved, and the problem of insufficient leakage current and thermal stability is achieved. Higher reliability and breakdown voltage characteristics.
Patent Information
- Application Number
- CN202010141333.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-14
- Filing Date
- 2020-03-04
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-03-04
AI Technical Summary
It is difficult for the existing semiconductor memory devices to effectively reduce leakage current under high integration, and the thermal stability and breakdown voltage characteristics of the dielectric layer are insufficient, which affects the reliability of the device.
Using a multi-layer oxide structure dielectric layer, a dielectric layer including zirconium, aluminum and oxide is formed through a deposition and annealing process, optimizes the dielectric constant and thermal stability, and controls the metal element through annealing process. Diffusion to form a dielectric layer with high dielectric constant and excellent breakdown voltage characteristics.
The leakage current is significantly reduced, the reliability and thermal stability of the semiconductor memory device are improved, and the breakdown voltage characteristics of the dielectric layer are improved.
Smart Images

Figure CN112086456B_ABST
Abstract
Description
[0001] This application claims the priority benefit of Korean Patent Application No. 10-2019-0070993 filed on June 14, 2019 in the Korean Intellectual Property Office, the disclosure of which is incorporated herein by reference in its entirety. Technical Field
[0002] The inventive concept relates to a semiconductor memory device and a method of manufacturing the semiconductor memory device. Background Art
[0003] Semiconductor devices are beneficial in the electronics industry due to their small size, versatility and / or low manufacturing cost. However, with the significant development of the electronics industry, semiconductor devices are being highly integrated. The line width of the pattern of the semiconductor device is being reduced for its high integration. New exposure techniques and / or expensive exposure techniques can be used for fine patterns to manufacture highly integrated semiconductor devices. Therefore, various studies have been conducted recently on new integration techniques. Summary of the invention
[0004] Some example embodiments of the inventive concepts provide a semiconductor memory device having improved reliability.
[0005] Some example embodiments of the inventive concepts provide a method of manufacturing a semiconductor memory device capable of reducing leakage current.
[0006] According to some example embodiments of the inventive concept, a semiconductor memory device may include a capacitor. The capacitor may include a first electrode, a second electrode, and a dielectric layer located between the first electrode and the second electrode. The dielectric layer may include a zirconium oxide aluminum layer, the zirconium oxide aluminum layer including: a first zirconium region adjacent to the first electrode; a first aluminum region separated from both the first electrode and the second electrode; a second aluminum region adjacent to the second electrode; and a second zirconium region located between the first aluminum region and the second aluminum region. Each of the first zirconium region and the second zirconium region may include zirconium and oxygen, and may not include aluminum. Each of the first aluminum region and the second aluminum region may include aluminum and oxygen, and may not include zirconium. The first aluminum region and the first zirconium region may be separated from each other by a first distance, and the first aluminum region and the second zirconium region may be separated from each other by a second distance, and the second distance may be shorter than the first distance.
[0007] According to some example embodiments of the inventive concept, a semiconductor memory device may include a capacitor. The capacitor may include a first electrode, a second electrode, and a dielectric layer between the first electrode and the second electrode. The dielectric layer may include a hafnium oxide layer adjacent to the first electrode and a zirconium oxide aluminum layer adjacent to the second electrode. The zirconium oxide aluminum layer may include a first surface contacting the hafnium oxide layer and a second surface contacting the second electrode, and an aluminum concentration in the zirconium oxide aluminum layer may be highest at the second surface and lowest at the first surface.
[0008] According to some example embodiments of the inventive concept, a semiconductor memory device may include a capacitor. The capacitor may include a first electrode, a second electrode, and a dielectric layer located between the first electrode and the second electrode. The dielectric layer may include a first dielectric layer, the first dielectric layer includes an A metal, a B metal, and oxygen, and the concentration of the B metal in the first dielectric layer may be the lowest adjacent to the first electrode and the highest adjacent to the second electrode.
[0009] According to some example embodiments of the inventive concept, a method for manufacturing a semiconductor memory device may include the following steps: depositing a first zirconium oxide layer on a substrate; depositing a first aluminum oxide layer on the first zirconium oxide layer; depositing a second zirconium oxide layer on the first aluminum oxide layer; and performing a first annealing process, wherein the first annealing process causes aluminum atoms in the first aluminum oxide layer to diffuse into the first zirconium oxide layer and the second zirconium oxide layer, thereby forming an initial dielectric layer including a first diffusion region and a second diffusion region. The method also includes the following steps: depositing a third zirconium oxide layer on the initial dielectric layer; and depositing a second aluminum oxide layer on the third zirconium oxide layer.
[0010] According to some example embodiments of the inventive concept, a method for manufacturing a semiconductor memory device may include the following steps: depositing a first A metal oxide layer including an A metal element on a substrate; depositing a first B metal oxide layer including a B metal element on the first A metal oxide layer; depositing a second A metal oxide layer including an A metal element on the first B metal oxide layer; and performing a first annealing process, wherein the first annealing process causes the B metal element in the first B metal oxide layer to diffuse into the first A metal oxide layer and the second A metal oxide layer, thereby forming an initial dielectric layer including a first diffusion region and a second diffusion region. The method may also include the following steps: depositing a third A metal oxide layer including an A metal element on the initial dielectric layer; and depositing a second B metal oxide layer including a B metal element on the third A metal oxide layer.
[0011] According to some example embodiments of the inventive concept, a method for manufacturing a semiconductor memory device may include the following steps: depositing a first A metal oxide layer on a substrate; depositing a first B metal oxide layer including a B metal element on the first A metal oxide layer; and performing a first annealing process, the first annealing process causing the B metal element in the first B metal oxide layer to diffuse into the first A metal oxide layer, thereby forming an initial dielectric layer that may include a first diffusion region. The method may also include the following steps: depositing a second A metal oxide layer on the initial dielectric layer; depositing a second B metal oxide layer including a B metal element on the second A metal oxide layer; and performing a second annealing process, the second annealing process causing the B metal element in the second B metal oxide layer to diffuse into the second A metal oxide layer, thereby forming a dielectric layer that may include a second diffusion region.
[0012] According to some example embodiments of the inventive concept, a method of manufacturing a semiconductor memory device including a capacitor may include the following steps: forming a first electrode; and forming a dielectric layer and a second electrode on the first electrode. The dielectric layer may be located between the first electrode and the second electrode, and may include: a first A metal oxide region including an A metal element; a second A metal oxide region including an A metal element on the first A metal oxide region; a first B metal oxide region including a B metal element between the first A metal oxide region and the second A metal oxide region; and a second B metal oxide region including a B metal element between the second A metal oxide region and the second electrode. Each of the first A metal oxide region and the second A metal oxide region may not include a B metal element. Each of the first B metal oxide region and the second B metal oxide region may not include an A metal element. The first A metal oxide region and the first B metal oxide region may be separated from each other by a first distance, and the first B metal oxide region and the second A metal oxide region may be separated from each other by a second distance, and the second distance may be shorter than the first distance. BRIEF DESCRIPTION OF THE DRAWINGS
[0013] Figure 1 Cross-sectional views showing semiconductor memory devices according to some example embodiments of the inventive concepts are illustrated.
[0014] Figure 2A is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts.
[0015] Figure 2B is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts.
[0016] FIG. 3A to FIG. 3C The present invention is a schematic diagram showing the manufacturing process of some exemplary embodiments of the present invention. Figure 1 A cross-sectional view of a method for manufacturing a semiconductor memory device.
[0017] Figure 4 is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts.
[0018] FIG. 5A to FIG. 5D Cross-sectional views showing methods of fabricating a semiconductor memory device according to some example embodiments of the inventive concepts are illustrated.
[0019] Figure 6 Plan views showing semiconductor memory devices according to some example embodiments of the inventive concepts are illustrated.
[0020] Figure 7 Shown along Figure 6 A cross-sectional view taken along line AA' and line BB'.
[0021] FIG. 8A to FIG. 8Q FIG. 1 shows a method of manufacturing a device having a plurality of components according to some example embodiments of the present invention. Figure 7 A cross-sectional view of a semiconductor memory device of the method. DETAILED DESCRIPTION
[0022] Now, some exemplary embodiments of the present inventive concept will be described in detail with reference to the accompanying drawings to help clearly explain the present inventive concept.
[0023] Figure 1 Cross-sectional views showing semiconductor memory devices according to some example embodiments of the inventive concepts are illustrated.
[0024] Reference Figure 1 , the semiconductor memory device 100 according to the present embodiment may include a first electrode 50 disposed on a substrate 1. The second electrode 60 may be disposed on the first electrode 50. The dielectric layer 40 may be disposed between the first electrode 50 and the second electrode 60. The capacitor may be composed of the first electrode 50, the second electrode 60, and the dielectric layer 40. The substrate 1 may be a single crystal silicon substrate or a silicon on insulator (SOI) substrate. Although not shown, an interlayer dielectric layer, a transistor, a contact plug, a connecting line, etc. may be disposed between the substrate 1 and the first electrode 50. For example, the first electrode 50 and the second electrode 60 may independently include one or more of a polysilicon layer doped with impurities, a silicon germanium layer doped with impurities, a metal nitride layer such as a titanium nitride layer, and a metal layer such as a tungsten layer, a copper layer, and an aluminum layer. The first electrode 50 may be referred to as a bottom electrode. The second electrode 60 may be referred to as a top electrode.
[0025] The dielectric layer 40 may include a first dielectric layer 10 and a second dielectric layer 30. The first dielectric layer 10 may be disposed between the second dielectric layer 30 and the first electrode 50. In some embodiments, the second dielectric layer 30 may include a material having a thermal stability better than that of the first dielectric layer 10. The second dielectric layer 30 may have a first surface 30a in contact with the first dielectric layer 10 and a second surface 30b in contact with the second electrode 60. The second dielectric layer 30 may preferably include an A metal, a B metal, and oxygen. The oxide layer of the A metal may have a dielectric constant greater than that of the oxide layer of the B metal. The oxide layer of the A metal may have a grain size greater than that of the oxide layer of the B metal. The A metal may preferably be, for example, hafnium (Hf) or zirconium (Zr). The B metal may preferably be, for example, niobium (Nb) or aluminum (Al). The second dielectric layer 30 may preferably be, for example, a zirconium oxide aluminum layer, a hafnium oxide aluminum layer, a zirconium oxide niobium layer, or a hafnium oxide niobium layer.
[0026] The first dielectric layer 10 may include, for example, a material whose dielectric constant is greater than that of the second dielectric layer 30. The first dielectric layer 10 may preferably be, for example, a hafnium oxide layer. In this case, the first dielectric layer 10 may have a tetragonal crystal structure and a dielectric constant of about to about The first dielectric layer 10 may be used to supplement the overall dielectric constant of the dielectric layer 40. When the second dielectric layer 30 is sufficient to provide the dielectric layer 40 with the desired dielectric constant and thermal stability, the first dielectric layer 10 may be omitted.
[0027] When a case is given in which the A metal is zirconium, the B metal is aluminum, and the first dielectric layer 10 is formed of a hafnium oxide layer, the case may be an example in which the first dielectric layer 10 does not include (e.g., may not include, may not contain) the A metal and the B metal, but includes a C metal (e.g., hafnium) different from the A metal and the B metal. On the contrary, when the A metal is hafnium, the first dielectric layer 10 may be omitted or the first dielectric layer 10 may include the A metal.
[0028] The concentration of the B metal included in the second dielectric layer 30 may be the highest at or near the second surface 30 b and the lowest at or near the first surface 30 a. The concentration of the A metal included in the second dielectric layer 30 may be the highest at or near the first surface 30 a and the lowest at or near the second surface 30 b. In some embodiments, the concentration of the A metal in the second dielectric layer 30 and the concentration of the B metal in the second dielectric layer 30 may be as follows: Figure 1 The changes in the second dielectric layer 30 are shown in FIG.
[0029] The second dielectric layer 30 may be divided into a plurality of regions based on the concentration gradient of atoms of the A metal and the B metal. For example, the second dielectric layer 30 may include: a first A metal region 12, adjacent to the first electrode 50 (e.g., closest to the first electrode 50); a first B metal region 16, separated from both the first electrode 50 and the second electrode 60; a second B metal region 24, adjacent to the second electrode 60 (e.g., closest to the second electrode 60); and a second A metal region 20, located between the first B metal region 16 and the second B metal region 24. The first A metal region 12 and the second A metal region 20 may include A metal and oxygen, but not B metal. When the A metal is zirconium, the first A metal region 12 and the second A metal region 20 may be referred to as the first zirconium region and the second zirconium region, respectively. When the A metal is hafnium, the first A metal region 12 and the second A metal region 20 may be referred to as the first hafnium region and the second hafnium region, respectively. The first B metal region 16 and the second B metal region 24 may include B metal and oxygen, but not A metal. When the B metal is aluminum, the first B metal region 16 and the second B metal region 24 may be referred to as a first aluminum region and a second aluminum region, respectively. When the B metal is niobium, the first B metal region 16 and the second B metal region 24 may be referred to as a first niobium region and a second niobium region, respectively. In some embodiments, the first A metal region 12 and the second A metal region 20 may include an A metal and oxygen, but may not include or may not contain a B metal. In some embodiments, the first B metal region 16 and the second B metal region 24 may include a B metal and oxygen, but may not include or may not contain an A metal.
[0030] The first distance D1 between the first B metal region 16 and the first A metal region 12 may be greater than the second distance D2 between the first B metal region 16 and the second A metal region 20. The first diffusion region 14 may be disposed between the first B metal region 16 and the first A metal region 12. The second diffusion region 18 may be disposed between the first B metal region 16 and the second A metal region 20. The third diffusion region 22 may be disposed between the second A metal region 20 and the second B metal region 24. Each of the first diffusion region 14, the second diffusion region 18, and the third diffusion region 22 may include an A metal, a B metal, and oxygen. The first diffusion region 14 may be wider than the second diffusion region 18. For example, the first diffusion region 14 may have a vertical width (corresponding to the first distance D1) greater than the vertical width (corresponding to the second distance D2) of the second diffusion region 18. When the A metal is zirconium and the B metal is aluminum, the first diffusion region 14, the second diffusion region 18, and the third diffusion region 22 may be referred to as a first zirconium aluminum region, a second zirconium aluminum region, and a third zirconium aluminum region, respectively. When the A metal is hafnium and the B metal is niobium, the first diffusion region 14, the second diffusion region 18, and the third diffusion region 22 may be referred to as a first hafnium niobium region, a second hafnium niobium region, and a third hafnium niobium region, respectively. The third diffusion region 22 may be wider than the second diffusion region 18. In some embodiments, the third diffusion region 22 may be as Figure 1 , has a vertical width greater than that of the second diffusion region 18. The vertical direction may refer to a direction along which the first A metal region 12, the first diffusion region 14, and the first B metal region 16 are stacked, and the first A metal region 12 and the first B metal region 16 are separated from each other in the vertical direction. The concentration of the A metal or the B metal in a single region (e.g., the first A metal region 12, the first B metal region 16, the second A metal region 20, the second B metal region 24, or one of the first diffusion region 14, the second diffusion region 18, and the third diffusion region 22) may be an average concentration of the A metal or the B metal in the region.
[0031] The second dielectric layer 30 may be in a crystalline state. The second surface 30b may have a surface roughness smaller than that of the zirconium oxide layer. The second surface 30b may preferably have a root mean square roughness (Rq) in the range of about 1nm to about 4.7nm. The surface roughness of the second dielectric layer 30 may be relatively small to reduce leakage current and improve breakdown voltage characteristics. Because the dielectric layer 40 includes the first dielectric layer 10 and the second dielectric layer 30, the dielectric layer 40 may have a high dielectric constant, excellent thermal stability, reduced leakage current and improved breakdown voltage characteristics. Therefore, the reliability of the semiconductor memory device 100 may be increased.
[0032] The following describes the production Figure 1 A method for a semiconductor memory device. Figure 2A is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts. FIG. 3A to FIG. 3C The present invention is a schematic diagram showing the manufacturing process of some exemplary embodiments of the present invention. Figure 1 A cross-sectional view of a method for manufacturing a semiconductor memory device.
[0033] Reference Figure 2A and Figure 3A , a substrate 1 may be prepared first. A first electrode 50 may be formed on the substrate 1. The first electrode 50 may be formed of a conductive material. A first dielectric layer 10 may be formed on the first electrode 50. The first dielectric layer 10 may be formed of a hafnium oxide layer by performing a deposition process such as atomic layer deposition (ALD) or chemical vapor deposition (CVD).
[0034] A deposition process such as ALD or CVD may be performed to deposit a first A metal oxide layer 12a on the first dielectric layer 10 (first step, S11). The first A metal oxide layer 12a may be formed to have a first thickness T1. The first A metal oxide layer 12a may be deposited in an amorphous state. For example, the first A metal oxide layer 12a may preferably be a zirconium oxide layer or a hafnium oxide layer.
[0035] A deposition process such as ALD or CVD may be performed to deposit a first B metal oxide layer 16a on the first A metal oxide layer 12a (second step, S21). The first B metal oxide layer 16a may be formed to have a second thickness T2. The second thickness T2 may be less than the first thickness T1. The first B metal oxide layer 16a may be deposited in an amorphous state. For example, the first B metal oxide layer 16a may preferably be an aluminum oxide layer or a niobium oxide layer. When the first A metal oxide layer 12a is a zirconium oxide layer and the first B metal oxide layer 16a is an aluminum oxide layer, because the grain size of the zirconium oxide layer is larger than the grain size of the aluminum oxide layer after crystallization, the grains of the aluminum oxide layer may be used to fill the gaps between the grains of the zirconium oxide layer, which may result in a reduction in surface roughness. Therefore, leakage current may be reduced. It will be understood that "element A fills element B" (or similar language) as used herein means that element A is in element B, but does not necessarily mean that element A completely fills element B.
[0036] A deposition process such as ALD or CVD may be performed to deposit a second A metal oxide layer 20a on the first B metal oxide layer 16a (third step, S31). The second A metal oxide layer 20a may be formed to have a third thickness T3. The third thickness T3 may be less than the first thickness T1 and greater than the second thickness T2. The third thickness T3 may preferably be half the first thickness T1. The second A metal oxide layer 20a may be deposited in an amorphous state. The second A metal oxide layer 20a may preferably be a zirconium oxide layer or a hafnium oxide layer.
[0037] Reference Figure 2A and Figure 3B , an annealing process (fourth step, S41) may be performed. One or more of nitrogen, argon and oxygen may be supplied to perform the annealing process. In this case, nitrogen or argon may be used to prevent or reduce oxidation of the first electrode 50. In the annealing process, oxygen may play a role in preventing or reducing the loss of combined oxygen of the oxide layers 12a, 20a and 16a to the atmosphere. The annealing process may be performed at a temperature of 350°C to 500°C. The annealing process may cause the B metal included in the first B metal oxide layer 16a to diffuse into the first A metal oxide layer 12a and the second A metal oxide layer 20a to form the first diffusion region 14 and the second diffusion region 18. Because the first A metal oxide layer 12a is thicker than the second A metal oxide layer 20a, the first diffusion region 14 may be formed to have a vertical width (corresponding to the first distance D1) greater than the vertical width (corresponding to the second distance D2) of the second diffusion region 18. The first diffusion region 14 and the second diffusion region 18 may include an A metal, a B metal and oxygen.
[0038] A fuzzy boundary may be established between the first B metal oxide layer 16a and each of the first A metal oxide layer 12a and the second A metal oxide layer 20a. Therefore, the first A metal region 12 may be formed between the first diffusion region 14 and the first dielectric layer 10, the first B metal region 16 may be formed between the first diffusion region 14 and the second diffusion region 18, and the second A metal region 20 may be formed on the second diffusion region 18. Therefore, the second initial dielectric layer 25 may be formed. The annealing process may make the second initial dielectric layer 25 crystalline. The time and temperature of the annealing process may be controlled so that a concentration gradient of the A metal and the B metal exists in the second initial dielectric layer 25.
[0039] Reference Figure 2A and Figure 3C, a deposition process such as ALD or CVD may be performed to deposit a third A metal oxide layer 22a on the second initial dielectric layer 25 (fifth step, S51). The third A metal oxide layer 22a may be deposited in an amorphous state. The third A metal oxide layer 22a may be formed to have a fourth thickness T4. The fourth thickness T4 may be less than the first thickness T1. For example, the first thickness T1 may be the same as the sum of the third thickness T3 and the fourth thickness T4. The fourth thickness T4 may preferably be half of the first thickness T1. For example, the third A metal oxide layer 22a may preferably be a zirconium oxide layer or a hafnium oxide layer. Because the third A metal oxide layer 22a is formed to have a fourth thickness T4 which is relatively smaller than the first thickness T1 under the condition that the second initial dielectric layer 25 becomes crystalline, the third A metal oxide layer 22a may have a relatively small grain size. Therefore, the second dielectric layer (see Figure 1 30) of the second surface (see Figure 1 30b) to provide reduced surface roughness.
[0040] The third A metal oxide layer 22a may contact the second A metal region 20 of the second preliminary dielectric layer 25. Since the second A metal region 20 does not include the B metal, the second A metal region 20 may have a material and structure substantially the same as those of the third A metal oxide layer 22a. Therefore, after the third A metal oxide layer 22a is deposited, a clear boundary may not be provided between the third A metal oxide layer 22a and the second A metal region 20.
[0041] A deposition process such as ALD or CVD may be performed to deposit a second B metal oxide layer 24a on the third A metal oxide layer 22a (sixth step, S61). For example, the second B metal oxide layer 24a may preferably be an aluminum oxide layer or a niobium oxide layer. The second B metal oxide layer 24a may be deposited in an amorphous state. The second B metal oxide layer 24a may be formed to have a fifth thickness T5. The fifth thickness T5 may be less than the first thickness T1, the third thickness T3, and the fourth thickness T4. The fifth thickness T5 may be the same as or greater than the second thickness T2.
[0042] Then, refer to Figure 1 and Figure 3C, a second electrode 60 may be formed on the second B metal oxide layer 24a. The second electrode 60 may be formed of a conductive material. The process temperature required for the deposition process for forming the second electrode 60 may allow the B metal included in the second B metal oxide layer 24a to diffuse into the third A metal oxide layer 22a to form the third diffusion region 22. The process temperature of the deposition process may allow the third A metal oxide layer 22a and the second B metal oxide layer 24a to become crystalline. In addition, a portion of the second B metal oxide layer 24a may become the second B metal region 24. Therefore, the second dielectric layer 30 may be finally formed.
[0043] The method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concept may include an annealing process (fourth step, S41) performed between the deposition step (third step, S31) for the second A metal oxide layer 20a and the deposition step (fifth step, S51) for the third A metal oxide layer 22a, so that the surface roughness of the second surface 30b of the second dielectric layer 30 can be reduced compared to the case where the annealing process is not performed. Therefore, the leakage current of the dielectric layer 40 can be reduced.
[0044] Although not shown, an additional annealing process for forming the third diffusion region 22 may be performed between the deposition step (sixth step, S61) for the second B metal oxide layer 24a and the formation step for the second electrode 60. An additional annealing process may also be performed between the deposition step (second step, S21) for the first B metal oxide layer 16a and the deposition step (third step, S31) for the second A metal oxide layer 20a. The first step S11 to the sixth step S61 may constitute a single cycle, and the single cycle may be repeatedly performed several times. In summary, the second dielectric layer 30 may be formed to have a desired thickness.
[0045] Figure 2B is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts. Figure 2B An example is shown in which the A metal is zirconium and the B metal is aluminum.
[0046] Reference Figure 2B and Figure 3A, a first electrode 50 and a first dielectric layer 10 may be formed on a substrate 1. A first zirconium oxide layer 12a in an amorphous state may be deposited on the first dielectric layer 10 to have a first thickness T1 (S10). A first aluminum oxide layer 16a in an amorphous state may be deposited on the first zirconium oxide layer 12a to have a second thickness T2 (S20). A second zirconium oxide layer 20a in an amorphous state may be deposited on the first aluminum oxide layer 16a to have a third thickness T3 (S30). The relationship between the first thickness T1, the second thickness T2, and the third thickness T3 may be the same as discussed above.
[0047] Reference Figure 2B and Figure 3B , an annealing process (S40) may be performed. Therefore, aluminum atoms contained in the first aluminum oxide layer 16a may diffuse into the first zirconium oxide layer 12a and the second zirconium oxide layer 20a to form the first diffusion region 14 and the second diffusion region 18. In addition, the first zirconium region 12 and the second zirconium region 20 and the first aluminum region 16 may be formed. Therefore, the second initial dielectric layer 25 may be formed, and the second initial dielectric layer 25 may have a crystalline state.
[0048] Reference Figure 2B and Figure 3C , a third zirconium oxide layer 22a in an amorphous state may be formed to have a fourth thickness T4 on the second initial dielectric layer 25 (S50). A second aluminum oxide layer 24a may be formed to have a fifth thickness T5 on the third zirconium oxide layer 22a. Figure 1 As shown in FIG. 1 , a second electrode 60 may be formed on the second aluminum oxide layer 24 a. Detailed process steps and structural changes may be referred to in Figure 2A The process steps and structural changes discussed are the same or similar.
[0049] Figure 4 is a flowchart illustrating a method of manufacturing a semiconductor memory device according to some example embodiments of the inventive concepts. FIG. 5A to FIG. 5D Cross-sectional views showing methods of fabricating a semiconductor memory device according to some example embodiments of the inventive concepts are illustrated.
[0050] Reference Figure 4 and Figure 5A, a first electrode 50 may be formed on the substrate 1. A first A metal oxide layer 12a may be deposited on the first electrode 50 to have a first thickness T1 (first step, S12). For example, the first A metal oxide layer 12a may be a zirconium oxide layer or a hafnium oxide layer. The first A metal oxide layer 12a may be deposited in an amorphous state. A first B metal oxide layer 16a may be deposited on the first A metal oxide layer 12a to have a second thickness T2 (second step, S22). The second thickness T2 may be less than the first thickness T1. The first B metal oxide layer 16a may be deposited in an amorphous state. For example, the first B metal oxide layer 16a may be an aluminum oxide layer or a niobium oxide layer. Although not shown in Figure 5A However, before forming the first A metal oxide layer 12a, a first electrode 50 may be formed. Figure 3A The first dielectric layer 10 is formed.
[0051] Reference Figure 4 and Figure 5B , a first annealing process (third step, S32) may be performed. Thus, the B metal contained in the first B metal oxide layer 16a may diffuse into the first A metal oxide layer 12a to form the first diffusion region 14. In addition, a portion of the first A metal oxide layer 12a may become the first A metal region 12, and a portion of the first B metal oxide layer 16a may become the first B metal region 16. Thus, an initial dielectric layer 26 may be formed. One or more of oxygen, nitrogen, and argon may be supplied to perform the first annealing process at a temperature of 350° C. to 500° C. The temperature and time of the first annealing process may be controlled to generate a concentration gradient of the B metal in the initial dielectric layer 26.
[0052] Reference Figure 4 and Figure 5C , the second A metal oxide layer 20a may be deposited on the initial dielectric layer 26 to have a sixth thickness T6 (fourth step, S42). The sixth thickness T6 may be greater than the second thickness T2. The sixth thickness T6 may be substantially the same as the first thickness T1. The sixth thickness T6 may be Figure 3A The third thickness T3 and Figure 3C The sum of the fourth thickness T4 of the second A metal oxide layer 20a. For example, the second A metal oxide layer 20a may preferably be a zirconium oxide layer or a hafnium oxide layer. The second A metal oxide layer 20a may be deposited in an amorphous state. The second B metal oxide layer 24a may be deposited on the second A metal oxide layer 20a to have a fifth thickness T5 (fifth step, S52). The fifth thickness T5 may be less than the sixth thickness T6. The second B metal oxide layer 24a may be deposited in an amorphous state. For example, the second B metal oxide layer 24a may be an aluminum oxide layer or a niobium oxide layer.
[0053] Reference Figure 4 and Figure 5D , a second annealing process (sixth step, S62) may be performed. Therefore, the B metal contained in the second B metal oxide layer 24a may diffuse into the second A metal oxide layer 20a to form the third diffusion region 22. In addition, the B metal contained in the first B metal region 16 may diffuse into the second A metal oxide layer 20a to form the second diffusion region 18. A portion of the second A metal oxide layer 20a may become the second A metal region 20, and a portion of the second B metal oxide layer 24a may become the second B metal region 24. Therefore, a dielectric layer 31 may be formed. One or more of oxygen, nitrogen and argon may be supplied to perform the second annealing process at a temperature of 350°C to 500°C. The temperature and time of the second annealing process may be controlled to generate a concentration gradient of the B metal in the dielectric layer 31. In the dielectric layer 31, the second diffusion region 18 may have a vertical width that is smaller than the vertical width of the first diffusion region 14 and the vertical width of the third diffusion region 22. Subsequently, a second electrode may be formed on the dielectric layer 31. Figure 5D In the equation, the concentration gradient of metal A and the concentration gradient of metal B can be expressed as Figure 1 In some embodiments, the concentration curve shown in Figure 5D As shown in , the second diffusion region 18 may have a thickness less than that of the first diffusion region 14 and that of the third diffusion region 22 .
[0054] Figure 4 The first step S12 to the sixth step S62 may constitute a single cycle, and in some embodiments, the single cycle may be repeatedly performed several times.
[0055] In some embodiments, Figure 2A , Figure 2B and Figure 4 The semiconductor memory device manufacturing method shown in FIG. 1 can be applied to a capacitor dielectric layer or to a gate dielectric layer of a gate pattern. For example, Figure 1 The dielectric layer 40 or Figure 5D The dielectric layer 31 may be a gate dielectric layer. In this case, the first electrode 50 may be omitted, and the second electrode 60 may correspond to a gate electrode.
[0056] Detailed examples of semiconductor memory devices including a dielectric layer according to some example embodiments of the inventive concepts will be described below. Figure 6 Plan views showing semiconductor memory devices according to some example embodiments of the inventive concepts are illustrated. Figure 7 Shown along Figure 6 A cross-sectional view taken along line AA' and line BB'.
[0057] Reference Figure 6 and Figure 7, a device isolation pattern 302 defining an active portion ACT may be provided on a substrate 301. Each of the active portions ACT may have an isolated shape. The active portions ACT may each have a strip shape elongated along a first direction X1 in a plan view. When viewed in a plan view, the active portion ACT may correspond to a portion of the substrate 301 surrounded by the device isolation pattern 302. The substrate 301 may include a semiconductor material. The active portions ACT may be arranged parallel to each other in the first direction X1, so that one of the active portions ACT may have an end portion adjacent to a central portion of an adjacent one of the active portions ACT.
[0058] The word line WL may cross the active portion ACT. The word line WL may be disposed in a groove formed in the device isolation pattern 302 and the active portion ACT. The word line WL may be parallel to a second direction X2 intersecting the first direction X1. The word line WL may be formed of a conductive material. A gate dielectric layer 307 may be disposed between each of the word lines WL and the inner surface of each groove. Although not shown, the groove may have its bottom surface relatively deeper in the device isolation pattern 302 and relatively shallower in the active portion ACT. The gate dielectric layer 307 may include one or more of thermal oxide, silicon nitride, silicon oxynitride, and a high-k dielectric. Each of the word lines WL may have a curved bottom surface.
[0059] The first doped region 312a may be disposed in the active portion ACT between a pair of word lines WL, and a pair of second doped regions 312b may be disposed in opposite edge portions of the active portion ACT. The first doped region 312a and the second doped region 312b may be doped with, for example, N-type impurities. The first doped region 312a may correspond to a common drain region, and the second doped region 312b may correspond to a source region. The transistor may be composed of each of the word lines WL and its adjacent first doped region 312a and second doped region 312b. Because the word lines WL are disposed in the groove, each of the word lines WL may have a channel region located therebelow, and the length of the channel region increases within a limited plane region. Therefore, short channel effects, etc. may be reduced and may be minimized.
[0060] The word line WL may have a top surface lower than the top surface of the active portion ACT. A word line cover pattern 310 may be provided on each of the word lines WL. The word line cover pattern 310 may have a line shape extending in the longitudinal direction of the word line WL, and may cover the entire top surface of the word line WL. The groove may have an inner space not occupied by the word line WL, and the word line cover pattern 310 may fill the unoccupied inner space of the groove. The word line cover pattern 310 may be formed of, for example, a silicon nitride layer. It will be understood that "element A covers element B" (or similar language) as used herein means that element A extends on element B, but does not necessarily mean that element A completely covers element B.
[0061] The interlayer dielectric pattern 305 may be disposed on the substrate 301. The interlayer dielectric pattern 305 may be formed of a single layer or multiple layers including one or more selected from a silicon oxide layer, a silicon nitride layer, and a silicon oxynitride layer. The interlayer dielectric pattern 305 may be formed to have an island shape spaced apart from each other in a plan view. The interlayer dielectric pattern 305 may be formed to simultaneously cover ends of two adjacent active portions ACT.
[0062] The top of the substrate 301, the top of the device isolation pattern 302, and the top of the word line capping pattern 310 may be partially recessed to form a first recessed region R1. Figure 6 The first recessed region R1 may have a mesh shape when viewed in a plan view as shown in FIG. The first recessed region R1 may have a sidewall aligned with the interlayer dielectric pattern 305 .
[0063] The bit line BL may be disposed on the interlayer dielectric pattern 305. The bit line BL may cross through the word line capping pattern 310 and the word line WL. Figure 6 As shown in , the bit line BL may be parallel to a third direction X3 intersecting the first direction X1 and the second direction X2. Each of the bit lines BL may include a bit line polysilicon pattern 330, a bit line ohmic pattern 331, and a bit line metal-containing pattern 332 stacked sequentially. The bit line polysilicon pattern 330 may include, for example, polysilicon doped with impurities or polysilicon not doped with impurities. The bit line ohmic pattern 331 may include, for example, a metal silicide layer. The bit line metal-containing pattern 332 may include, for example, one or more of a metal (e.g., tungsten, titanium, or tantalum) and a conductive metal nitride (e.g., titanium nitride, tantalum nitride, or tungsten nitride). A bit line capping pattern 337 may be disposed on each of the bit lines BL. The bit line capping pattern 337 is formed of a dielectric material such as a silicon nitride layer.
[0064] The bit line contact DC may be disposed in the first recessed region R1 intersecting the bit line BL. The bit line contact DC may include, for example, polysilicon doped with impurities or polysilicon not doped with impurities. Figure 6When viewed in a cross-sectional view taken along line BB' of FIG. 1 , the bit line contact DC may have a sidewall in contact with a sidewall of the interlayer dielectric pattern 305. Figure 6 When viewed in the plan view shown in FIG. 3 , the bit line contact DC may have a concave side surface in contact with the interlayer dielectric pattern 305. The bit line contact DC may electrically connect the first doped region 312a to the bit line BL.
[0065] The first recessed region R1 may have an empty space not occupied by the bit line contact DC, and the lower buried dielectric pattern 341 may occupy the empty space of the first recessed region R1. For example, the lower buried dielectric pattern 341 is formed of a single layer or multiple layers including one or more selected from a silicon oxide layer, a silicon nitride layer, and a silicon oxynitride layer.
[0066] When viewed in a plan view, the storage node contact BC may be disposed between a pair of adjacent bit lines BL. The storage node contacts BC may be spaced apart from each other. The storage node contacts BC may include, for example, polysilicon doped with impurities or polysilicon not doped with impurities. In some embodiments, each of the storage node contacts BC may have a configuration such as Figure 7 Between the bit lines BL, a dielectric pattern (not shown) may be disposed between the storage node contacts BC.
[0067] The bit line spacer SP may be placed between the bit line BL and the storage node contact BC. The bit line spacer SP may include a first sub-spacer 321 and a second sub-spacer 325 separated from each other across a gap region GP. The gap region GP may be an air gap. The first sub-spacer 321 may cover the sidewalls of the bit line BL and the sidewalls of the bit line cover pattern 337. The second sub-spacer 325 may be adjacent to the storage node contact BC. The first sub-spacer 321 and the second sub-spacer 325 may include the same material. For example, the first sub-spacer 321 and the second sub-spacer 325 may include a silicon nitride layer. In some embodiments, the gap region GP may be an empty space or a space in which a gas (e.g., air, nitrogen, argon, oxygen) is included.
[0068] The second sub-spacer 325 may have a bottom surface lower than the bottom surface of the first sub-spacer 321. The second sub-spacer 325 may have a top whose height (or level) is lower than the top of the first sub-spacer 321. Such a configuration can increase the formation margin for the landing pad LP to be discussed below. Therefore, the disconnection between the landing pad LP and the storage node contact BC can be reduced or prevented. The first sub-spacer 321 may extend to cover the sidewalls of the bit line contact DC, and may also cover the sidewalls and bottom surface of the first recessed region R1. For example, the first sub-spacer 321 may be placed between the bit line contact DC and the lower buried dielectric pattern 341, between the word line cover pattern 310 and the lower buried dielectric pattern 341, between the substrate 301 and the lower buried dielectric pattern 341, and between the device isolation pattern 302 and the lower buried dielectric pattern 341.
[0069] The storage node ohmic layer 309 may be disposed on the storage node contact BC. The storage node ohmic layer 309 may include, for example, a metal silicide. The storage node ohmic layer 309, the first sub-spacer 321, the second sub-spacer 325, and the bit line cover pattern 337 may be conformally covered by the diffusion stop pattern 311a. The diffusion stop pattern 311a may include, for example, a metal nitride, such as a titanium nitride layer or a tantalum nitride layer. The bonding pad LP may be disposed on the diffusion stop pattern 311a. The bonding pad LP may be formed of a material containing a metal such as tungsten. The bonding pad LP may have an upper portion covering the top surface of the bit line cover pattern 337, and have a width greater than the width of the storage node contact BC. The center of the bonding pad LP may deviate from the center of the storage node contact BC in the second direction X2. A portion of the bit line BL may be vertically overlapped with the bonding pad LP. The upper sidewall of the bit line cover pattern 337 may be vertically overlapped with the bonding pad LP and may be covered by the third sub-spacer 327. The second recessed region R2 may be formed on the other upper sidewall of the bit line capping pattern 337. It will be understood that "element A vertically overlaps element B" (or similar language) as used herein means that there is at least one vertical line intersecting both element A and element B. In some embodiments, the diffusion stop pattern 311a may be formed as shown in FIG. Figure 7 , having a uniform thickness along the surface of the storage node ohmic layer 309 , the surfaces of the first and second sub-spacers 321 and 325 , and the surface of the bit line capping pattern 337 .
[0070] The first covering pattern 358a may cover and connect the upper sidewalls of adjacent bonding pads LP. The first covering pattern 358a may have a uniform thickness regardless of the position. The first covering pattern 358a may define a third recessed region R3 between the bonding pads LP. The third recessed region R3 may be filled with a second covering pattern 360a. The first covering pattern 358a and the second covering pattern 360a may independently include a silicon nitride layer, a silicon oxide layer, a silicon oxynitride layer, or a porous layer. The first covering pattern 358a may have a porosity greater than that of the second covering pattern 360a. The first covering pattern 358a and the second covering pattern 360a may have a top surface coplanar with the top surface of the bonding pad LP.
[0071] The gap region GP between the first subspacer 321 and the second subspacer 325 may extend into the space between the bonding pads LP. The gap region GP may expose the bottom surface of the first capping pattern 358a. The gap region GP may extend toward the diffusion stop pattern 311a. For example, the diffusion stop pattern 311a may have a sidewall recessed between the bonding pad LP and the bit line capping pattern 337. The gap region GP may partially expose the top surface of the bit line capping pattern 337 and the bottom surface of the bonding pad LP.
[0072] The bottom electrode BE may be disposed on the corresponding bonding pad LP. For example, the bottom electrode BE may include a polysilicon layer doped with impurities, a metal nitride layer such as a titanium nitride layer, and one or more of a metal layer such as a tungsten layer, an aluminum layer, and a copper layer. The bottom electrode BE may have a circular columnar shape, a hollow cylindrical shape, or a cup shape. The upper side walls of adjacent bottom electrodes BE may be connected to each other by a support pattern 374a. The support pattern 374a may include a dielectric material such as a silicon nitride layer, a silicon oxide layer, and a silicon oxynitride layer. The support pattern 374a may include a support hole 374h. The support hole 374h may expose the side walls of adjacent bottom electrodes BE.
[0073] Between the bottom electrodes BE, an etch stop layer 370 may cover the top surfaces of the first capping pattern 358a and the second capping pattern 360a. The etch stop layer 370 may include a dielectric material such as a silicon nitride layer, a silicon oxide layer, and a silicon oxynitride layer. The dielectric layer DL may cover the surface of the bottom electrode BE and the surface of the support pattern 374a. The dielectric layer DL may be connected to the reference electrode BE. Figure 1 The dielectric layer 40 discussed or referred to Figure 5D The dielectric layer 31 discussed above is the same. The dielectric layer DL may be covered by the top electrode UE. For example, the top electrode UE may include a polysilicon layer doped with impurities, a silicon germanium layer doped with impurities, a metal nitride layer such as a titanium nitride layer, and a metal layer such as a tungsten layer, an aluminum layer, and a copper layer. One or more of the layers. The capacitor CAP may be composed of a bottom electrode BE, a dielectric layer DL, and a top electrode UE.
[0074] The semiconductor memory device according to some example embodiments of the present invention can be constructed so that the gap region GP can extend into the space between the bonding pads LP without being interrupted by the upper portion of the first sub-spacer 321 and the upper portion of the second sub-spacer 325, and thus can be fully disposed between the first sub-spacer 321 and the second sub-spacer 325. Because air (gas or vacuum) has a lower dielectric constant than that of silicon oxide, the gap region GP can reduce the parasitic capacitance between the bit line BL and the storage node contact BC. In addition, the parasitic capacitance between the bonding pads LP can be reduced. In addition, the semiconductor memory device according to some example embodiments of the present invention can be constructed to include a dielectric layer DL, and thus can have reduced leakage current, a high dielectric constant, and excellent thermal stability. Therefore, the reliability of the semiconductor memory device can be improved.
[0075] FIG. 8A to FIG. 8Q FIG. 1 shows a method of manufacturing a device having a plurality of components according to some example embodiments of the present invention. Figure 7 A cross-sectional view of a semiconductor memory device of the method.
[0076] Reference Fig. 8A , a device isolation pattern 302 may be formed on the substrate 301 to define an active portion ACT. A device isolation trench may be formed on the substrate 301, and the device isolation pattern 302 may fill the device isolation trench. The active portion ACT and the device isolation pattern 302 may be patterned to form a groove. In this step, the etching conditions for the substrate 301 and the device isolation pattern 302 may be appropriately controlled so that the device isolation pattern 302 may be easier to etch than the substrate 301. Therefore, the groove may have an uneven bottom surface.
[0077] A word line WL may be formed in the corresponding groove. A pair of word lines WL may cross each of the active portions ACT. Figure 6 and Fig. 8A As shown in , the pair of word lines WL may divide each of the active portions ACT into a first source / drain region SDR1 and a pair of second source / drain regions SDR2. The first source / drain region SDR1 may be defined between the pair of word lines WL, and a pair of second source / drain regions SDR2 may be defined on opposite edges of each of the active portions ACT.
[0078] Before forming the word line WL, a gate dielectric layer 307 may be formed on the inner surface of the groove. The gate dielectric layer 307 may be formed by a thermal oxidation process, a chemical vapor deposition process, and / or an atomic layer deposition process. A gate conductive layer may be formed to fill the groove and then etched back to form the word line WL. The word line WL may have a recessed top surface that is lower than the top surface of the active portion ACT. A dielectric layer such as a silicon nitride layer may be formed on the substrate 301 to fill the groove, and then the dielectric layer may be etched to form a word line capping pattern 310 on the corresponding word line WL. The term "and / or" as used herein includes any and all combinations of one or more of the related listed items.
[0079] Reference Figure 8B , the word line capping pattern 310 and the device isolation pattern 302 may be used as masks to dope impurities into the active portion ACT, and the active portion ACT may form a first doping region 312a and a second doping region 312b. Fig. 8A 301. A first doped region 312a and a second doped region 312b are formed in the first source / drain region SDR1 and the second source / drain region SDR2 shown in FIG. 301. A dielectric layer and a first polysilicon layer may be sequentially formed on the entire top surface of the substrate 301. The first polysilicon layer may be patterned to form a polysilicon mask pattern 330a. The polysilicon mask pattern 330a may be used as an etching mask to etch the dielectric layer, the device isolation pattern 302, the substrate 301, and the word line capping pattern 310 to simultaneously form a first recessed region R1 and an interlayer dielectric pattern 305. The interlayer dielectric pattern 305 may be formed to have a plurality of island shapes separated from each other. The interlayer dielectric pattern 305 may be formed to cover both ends of two adjacent active portions ACT. The first recessed region R1 may be formed to have a mesh shape in a plan view. The first recessed region R1 may expose the first doped region 312a. It will be understood that "formed simultaneously" means formed at almost (but not necessarily exactly) the same time in the same manufacturing step.
[0080] Reference Figure 8C, a second polysilicon layer 329 may be formed on the entire surface of the substrate 301 so that the first recessed region R1 may be filled with the second polysilicon layer 329. The second polysilicon layer 329 may be subjected to a planarization etching process to remove the second polysilicon layer 329 on the polysilicon mask pattern 330a and expose the top surface of the polysilicon mask pattern 330a. A bit line ohmic layer 331a, a bit line metal-containing layer 332a, and a bit line capping layer 337a may be sequentially formed on the polysilicon mask pattern 330a and the second polysilicon layer 329. The bit line ohmic layer 331a may be formed of, for example, a metal silicide such as cobalt silicide. The bit line ohmic layer 331a may be formed by depositing a metal layer on the polysilicon mask pattern 330a and the second polysilicon layer 329, performing an annealing process to form metal silicide by reacting the metal layer with polysilicon of the polysilicon mask pattern 330a and the second polysilicon layer 329, and then removing the unreacted metal layer.
[0081] A first mask pattern 339 may be formed on the bit line capping layer 337a and may define a planar shape of the bit line BL to be discussed below. The first mask pattern 339 may be formed on the bit line capping layer 337a. Figure 6 The first direction X1 and the second direction X2 shown in FIG. 1 extend in a third direction X3 intersecting with each other.
[0082] Reference Fig.8D , the first mask pattern 339 may be used as an etching mask to perform an etching process in which the bit line capping layer 337a, the bit line metal containing layer 332a, the bit line ohmic layer 331a, the polysilicon mask pattern 330a, and the second polysilicon layer 329 are sequentially etched to form a bit line capping pattern 337, a bit line contact DC, and a bit line BL including a bit line polysilicon pattern 330, a bit line ohmic pattern 331, and a bit line metal containing pattern 332. The etching process may partially expose the top surface of the interlayer dielectric pattern 305, and may also partially expose the inner sidewall and bottom surface of the first recessed region R1. The first mask pattern 339 may then be removed.
[0083] Reference Fig. 8E, a first sub-spacer layer may be conformally formed on the entire surface of the substrate 301. The first sub-spacer layer may conformally cover the bottom surface and the inner sidewall of the first recessed region R1. The first sub-spacer layer may be, for example, a silicon nitride layer. A dielectric layer such as a silicon nitride layer may be formed on the entire surface of the substrate 301 to fill the first recessed region R1, and then the dielectric layer may be anisotropically etched to leave a lower buried dielectric pattern 341 in the first recessed region R1. When the anisotropic etching process is performed, the first sub-spacer layer may also be etched to form a first sub-spacer 321. The anisotropic etching process may also expose the top surface of the interlayer dielectric pattern 305. A sacrificial spacer layer may be conformally formed on the entire surface of the substrate 301, and then the sacrificial spacer layer may be anisotropically etched to form a sacrificial spacer 323 covering the sidewall of the first sub-spacer 321. The sacrificial spacer 323 may include a material having an etching selectivity relative to the first sub-spacer 321. The sacrificial spacer 323 may be formed of, for example, a silicon oxide layer. A second sub-spacer 325 may be formed to cover the sidewall of the sacrificial spacer 323. The second sub-spacer 325 may be formed of, for example, a silicon nitride layer. After forming the second sub-spacer 325, the top surface of the interlayer dielectric pattern 305 may be exposed.
[0084] Reference Fig. 8E and Figure 8F , a polysilicon layer may be formed on the entire surface of the substrate 301 to fill the space between the bit lines BL, and then the polysilicon layer may be etched to form the initial storage node contact 350, and the upper sidewall of the first subspacer 321, the upper sidewall of the sacrificial spacer 323, and the upper sidewall of the second subspacer 325 may be exposed. The upper portion of the sacrificial spacer 323 and the upper portion of the second subspacer 325 may be removed so that the sacrificial spacer 323 and the second subspacer 325 have a top portion whose height (or level) is similar to the height (or level) of the top surface of the initial storage node contact 350. Therefore, the upper sidewall of the first subspacer 321 may be exposed. This process may provide a large process margin for forming the bonding pad LP to be discussed below. When the upper portion of the sacrificial spacer 323 and the upper portion of the second subspacer 325 are removed, the upper portion of the first subspacer 321 may also be partially removed, so that the first subspacer 321 may have a reduced width at its upper portion.
[0085] Reference Figure 8F and Figure 8G, a third sub-spacer layer may be conformally formed on the entire surface of the substrate 301, and then the third sub-spacer layer may be anisotropically etched to form a third sub-spacer 327 covering the exposed upper sidewall of the first sub-spacer 321. The third sub-spacer 327 may have a lower portion covering the exposed top end of the sacrificial spacer 323. The initial storage node contact 350 may be etched to expose the upper sidewall of the second sub-spacer 325, and a storage node contact BC may be formed at the same time. The third sub-spacer 327 may supplement the damaged upper portion of the first sub-spacer 321, and may cover the sacrificial spacer 323, thereby being used to reduce or prevent the bit line BL from being corroded by the etchant used to etch the storage node contact BC and the cleaning liquid used in the subsequent cleaning process. Therefore, the bit line BL may be protected from damage.
[0086] A storage node ohmic layer 309 may be formed on the top surface of the storage node contact BC. A diffusion stop layer 311 may be conformally formed on the entire surface of the substrate 301. A bonding pad layer 352 may be formed on the entire surface of the substrate 301, and the bonding pad layer 352 may fill the space between the bit line cover patterns 337. The bonding pad layer 352 may include, for example, tungsten. A second mask pattern 340 may be formed on the bonding pad layer 352. The second mask pattern 340 may be formed of, for example, an amorphous carbon layer (ACL). The second mask pattern 340 may define the position of the bonding pad LP discussed below. The second mask pattern 340 may be formed to vertically overlap with the storage node contact BC.
[0087] Reference Figure 8H The second mask pattern 340 may be used as an etching mask to perform an anisotropic etching process in which the bonding pad layer 352 is partially removed to form a bonding pad LP and an opening 354 exposing the diffusion stop layer 311 is simultaneously formed.
[0088] Reference Figure 8I , an isotropic etching process may be performed in which the diffusion stop layer 311 exposed to the opening 354 is removed to form diffusion stop patterns 311a spaced apart from each other and simultaneously expose portions of top surfaces of the third sub-spacer 327 and the bit line capping pattern 337. Depending on the extent of the isotropic etching process, the diffusion stop pattern 311a may be overetched to partially expose the bottom surface of the bonding pad LP.
[0089] Reference Figure 8I and Figure 8JAn anisotropic etching process may be performed to remove the portion of the bit line capping pattern 337 exposed to the opening 354 and may also remove the third sub-spacer 327, thus exposing the sacrificial spacer 323. In this case, a second recess region R2 may be formed on the bit line capping pattern 337.
[0090] Reference Figure 8J and Figure 8K , the second mask pattern 340 may be removed. An isotropic etching process may be performed in which the sacrificial spacer 323 is removed to form a gap region GP between the first sub-spacer 321 and the second sub-spacer 325. A thermal decomposition layer 356 may be formed to fill the opening 354 and the second recessed region R2. The thermal decomposition layer 356 may also be formed on the bonding pad LP. The thermal decomposition layer 356 may be formed to be close to the upper portion of the gap region GP.
[0091] Reference Figure 8L , a first annealing process may be performed in which an upper portion of the thermal decomposition layer 356 is thermally decomposed and removed to expose an upper sidewall and a top surface of the bonding pad LP, and thermal decomposition patterns 356a spaced apart from each other are formed simultaneously. A first capping layer 358 may be conformally formed on the thermal decomposition patterns 356a and the bonding pad LP.
[0092] Reference Figure 8L and Figure 8M , a second annealing process may be performed, in which the thermal decomposition pattern 356a may be all thermally decomposed, and the thermal decomposition pattern 356a may be degassed by the first capping layer 358, which results in the removal of the thermal decomposition pattern 356a. Then the gap region GP may expand between the bonding pads LP. The gap region GP may extend into the space between the first sub-spacer 321 and the second sub-spacer 325. A second capping layer 360 may be formed on the first capping layer 358.
[0093] Reference Figure 8M and Figure 8N , an etch back and / or chemical mechanical polishing (CMP) process may be performed to remove the first capping layer 358 and the second capping layer 360 on the bonding pad LP and expose the bonding pad LP. An etch stop layer 370 may be formed on the bonding pad LP, the first capping pattern 358a and the second capping pattern 360a. A first mold layer 372, a support layer 374 and a second mold layer 376 may be formed on the etch stop layer 370. The etch stop layer 370 and the support layer 374 may be formed of, for example, a silicon nitride layer. The first mold layer 372 and the second mold layer 376 may be formed of a material having an etching selectivity relative to the support layer 374. For example, the first mold layer 372 and the second mold layer 376 may be formed of a silicon oxide layer.
[0094] Reference Figure 8N and Fig.8O , the second mold layer 376, the support layer 374, the first mold layer 372, and the etch stop layer 370 may be sequentially patterned to form a bottom electrode hole BEH exposing the bonding pad LP. A conductive layer may be formed to fill the bottom electrode hole BEH, and then an etch back or CMP process may be performed to remove the conductive layer on the second mold layer 376 and form a bottom electrode BE in the bottom electrode hole BEH. A third mask pattern 378 may be formed on the second mold layer 376. The third mask pattern 378 may have a shape defining a support hole (see Figure 6 The opening 378h may expose a portion of the top surface of the adjacent bottom electrode BE and may also expose the second mold layer 376 between the adjacent bottom electrodes BE.
[0095] Reference Fig.8O and Figure 8P The third mask pattern 378 may be used as an etching mask to perform an anisotropic etching process in which the second mold layer 376 exposed to the opening 378h and the support layer 374 below the second mold layer 376 are removed to form a support pattern 374a and expose the first mold layer 372.
[0096] Reference Figure 8P and Figure 8Q , the third mask pattern 378 may be removed to expose the second mold layer 376. An isotropic etching process may be performed in which the first and second mold layers 372 and 376 are removed to expose the surfaces of the bottom electrodes BE and the support patterns 374a.
[0097] Then, if Figure 7 As shown in FIG. , a dielectric layer DL may be formed to conformally cover the substrate. Figures 1 to 5D The surface of the bottom electrode BE and the surface of the support pattern 374a are discussed. A top electrode UE may be formed on the dielectric layer DL.
[0098] According to some example embodiments of the inventive concept, a method of manufacturing a semiconductor memory device can reduce surface roughness of a dielectric layer and can reduce leakage current. In addition, the method of manufacturing a semiconductor memory device can easily form a gap region using a thermal decomposition layer.
[0099] According to the semiconductor memory device and the manufacturing method thereof according to the inventive concept, the surface roughness of the dielectric layer can be improved to reduce leakage current. Therefore, the reliability of the semiconductor memory device can be improved.
[0100] The subject matter disclosed above is considered to be illustrative, not restrictive, and the appended claims are intended to cover all such modifications, enhancements, and other embodiments that fall within the scope of the inventive concept. Therefore, to the maximum extent allowed by law, the scope will be determined by the broadest permissible interpretation of the claims and their equivalents, and should not be restricted or limited by the foregoing detailed description.
Claims
1. A semiconductor memory device, comprising a capacitor, in, The capacitor includes a first electrode, a second electrode, and a dielectric layer between the first electrode and the second electrode, and Wherein, the dielectric layer comprises a zirconium oxide aluminum layer, and the zirconium oxide aluminum layer comprises: a first zirconium region adjacent to the first electrode; a first aluminum region separated from both the first electrode and the second electrode; a second aluminum region adjacent to the second electrode; and The second zirconium region is located between the first aluminum region and the second aluminum region, wherein each of the first zirconium region and the second zirconium region includes zirconium and oxygen and does not contain aluminum, wherein each of the first aluminum region and the second aluminum region includes aluminum and oxygen and does not contain zirconium, and The first aluminum region and the first zirconium region are separated from each other by a first distance, and the first aluminum region and the second zirconium region are separated from each other by a second distance that is shorter than the first distance.
2. The semiconductor memory device according to claim 1, in, The zirconia aluminum layer includes a first surface facing the first electrode and a second surface facing the second electrode, and The aluminum concentration in the zirconium oxide aluminum layer is highest at the second surface and lowest at the first surface.
3. The semiconductor memory device according to claim 1, in, The aluminum concentration in the second aluminum region is greater than the aluminum concentration in the first aluminum region.
4. The semiconductor memory device according to claim 1, wherein the semiconductor memory device further comprises: include: a first diffusion region located between the first zirconium region and the first aluminum region; as well as A second diffusion region is located between the first aluminum region and the second zirconium region, wherein each of the first diffusion region and the second diffusion region includes zirconium, aluminum, and oxygen, wherein the first electrode and the second electrode are spaced apart from each other in a first direction, and The first diffusion region has a first thickness in the first direction, the second diffusion region has a second thickness in the first direction, and the first thickness is greater than the second thickness.
5. A method for manufacturing a semiconductor memory device, the method The following steps are involved: depositing a first zirconium oxide layer on a substrate; depositing a first aluminum oxide layer on the first zirconium oxide layer; depositing a second zirconium oxide layer on the first aluminum oxide layer; Performing a first annealing process, wherein the first annealing process causes aluminum atoms in the first aluminum oxide layer to diffuse into the first zirconium oxide layer and the second zirconium oxide layer, thereby forming an initial dielectric layer including a first diffusion region and a second diffusion region; depositing a third zirconium oxide layer on the initial dielectric layer; as well as depositing a second aluminum oxide layer on the third zirconium oxide layer, in, depositing a first zirconium oxide layer to have a first thickness; depositing a second zirconium oxide layer to have a second thickness; depositing a third zirconium oxide layer to have a third thickness; and The first thickness is greater than the second thickness and the third thickness. 6 . The method according to claim 5 , further comprising performing a second annealing process after depositing the second aluminum oxide layer, the second annealing process causing aluminum atoms in the second aluminum oxide layer to diffuse into the third zirconium oxide layer, thereby forming a third diffusion region. 7 . The method of claim 5 , further comprising performing a second annealing process before depositing the second zirconium oxide layer.
8. The method according to claim 5, in, The first thickness is equal to the sum of the second thickness and the third thickness. 9 . The method of claim 5 , further comprising depositing a hafnium oxide layer on the substrate before depositing the first zirconium oxide layer on the substrate.
10. A method for manufacturing a semiconductor memory device, the method The following steps are involved: depositing a first A metal oxide layer including an A metal element on a substrate; depositing a first B metal oxide layer including a B metal element on the first A metal oxide layer; depositing a second A metal oxide layer including an A metal element on the first B metal oxide layer; Performing a first annealing process, wherein the first annealing process causes the B metal element in the first B metal oxide layer to diffuse into the first A metal oxide layer and the second A metal oxide layer, thereby forming an initial dielectric layer including a first diffusion region and a second diffusion region; depositing a third A metal oxide layer including an A metal element on the initial dielectric layer; as well as depositing a second B metal oxide layer including a B metal element on the third A metal oxide layer, in, depositing a first A metal oxide layer to have a first thickness; depositing a second A metal oxide layer to have a second thickness; depositing a third A metal oxide layer to have a third thickness; and The first thickness is greater than the second thickness and the third thickness. 11 . The method according to claim 10 , further comprising performing a second annealing process after depositing the second B metal oxide layer, the second annealing process causing the B metal element in the second B metal oxide layer to diffuse into the third A metal oxide layer, thereby forming a third diffusion region. 12 . The method according to claim 10 , further comprising performing a second annealing process before depositing the second A metal oxide layer.
13. The method according to claim 10, in, The first thickness is equal to the sum of the second thickness and the third thickness.
14. The method of claim 10, further comprising depositing a C metal oxide layer on the substrate before depositing the first A metal oxide layer on the substrate, in, The C metal oxide layer does not contain the A metal element and the B metal element.
15. A method for manufacturing a semiconductor memory device, the method The following steps are involved: depositing a first A metal oxide layer on a substrate; depositing a first B metal oxide layer including a B metal element on the first A metal oxide layer; Performing a first annealing process, wherein the first annealing process causes the B metal element in the first B metal oxide layer to diffuse into the first A metal oxide layer, thereby forming an initial dielectric layer including a first diffusion region; depositing a second A metal oxide layer on the initial dielectric layer; depositing a second B metal oxide layer including a B metal element on the second A metal oxide layer; as well as performing a second annealing process, wherein the second annealing process causes the B metal element in the first B metal oxide layer to diffuse into the second A metal oxide layer to form a second diffusion region and causes the B metal element in the second B metal oxide layer to diffuse into the second A metal oxide layer to form a third diffusion region, thereby forming a dielectric layer including the second diffusion region and the third diffusion region, The first diffusion region has a first thickness in the first direction, the second diffusion region has a second thickness in the first direction, and the first thickness is greater than the second thickness.
16. A method of manufacturing a semiconductor memory device, the semiconductor memory device comprising a capacitor, the method The following steps are involved: forming a first electrode; as well as forming a dielectric layer and a second electrode on the first electrode, The dielectric layer is located between the first electrode and the second electrode and includes: A first A metal oxide region, comprising an A metal element; a second A metal oxide region including an A metal element on the first A metal oxide region; a first B metal oxide region including a B metal element between the first A metal oxide region and the second A metal oxide region; and A second B metal oxide region includes a B metal element between the second A metal oxide region and the second electrode, wherein each of the first A metal oxide region and the second A metal oxide region does not contain a B metal element, wherein each of the first B metal oxide region and the second B metal oxide region does not contain an A metal element, and The first A metal oxide region and the first B metal oxide region are separated from each other by a first distance, and the first B metal oxide region and the second A metal oxide region are separated from each other by a second distance shorter than the first distance.
17. The method according to claim 16, in, The first B metal oxide region has a first B metal element concentration, and the second B metal oxide region has a second B metal element concentration greater than the first B metal element concentration.
18. The method according to claim 16, in, The dielectric layer also includes: A first diffusion region is located between the first A metal oxide region and the first B metal oxide region; and The second diffusion region is located between the first B metal oxide region and the second A metal oxide region, Each of the first diffusion region and the second diffusion region includes an A metal element, a B metal element, and oxygen.
19. The method according to claim 18, in, The first electrode and the second electrode are spaced apart from each other in a first direction, and The first diffusion region has a first thickness in the first direction, the second diffusion region has a second thickness in the first direction, and the first thickness is greater than the second thickness.
20. The method according to claim 18, in, Forming the dielectric layer includes the following steps: sequentially depositing a first A metal oxide layer containing an A metal element, a first B metal oxide layer containing a B metal element, and a second A metal oxide layer containing an A metal element, wherein the first B metal oxide layer contacts both the first A metal oxide layer and the second A metal oxide layer; and then An annealing process is performed, which causes the B metal element of the first B metal oxide layer to diffuse into the first A metal oxide layer and the second A metal oxide layer, thereby forming a first diffusion region and a second diffusion region.
21. The method according to claim 18, in, The dielectric layer further includes a third diffusion region, the third diffusion region is located between the second A metal oxide region and the second B metal oxide region, and includes an A metal element, a B metal element, and oxygen.
22. The method according to claim 21, in, Forming the dielectric layer includes the following steps: The initial dielectric layer is formed by the following operations: sequentially depositing a first A metal oxide layer containing an A metal element, a first B metal oxide layer containing a B metal element, and a second A metal oxide layer containing an A metal element, wherein the first B metal oxide layer contacts both the first A metal oxide layer and the second A metal oxide layer; and then performing a first annealing process, wherein the first annealing process causes the B metal element of the first B metal oxide layer to diffuse into the first A metal oxide layer and the second A metal oxide layer, thereby forming a first diffusion region and a second diffusion region; sequentially depositing a third A metal oxide layer including an A metal element and a second B metal oxide layer including a B metal element on the initial dielectric layer; and The third A metal oxide layer and the second B metal oxide layer are converted into a third diffusion region and a second B metal oxide region, respectively.
23. The method according to claim 21, in, Forming the dielectric layer includes the following steps: sequentially depositing a first A metal oxide layer containing an A metal element and a first B metal oxide layer containing a B metal element; After sequentially depositing a first A metal oxide layer and a first B metal oxide layer, performing a first annealing process, the first annealing process causing a B metal element of the first B metal oxide layer to diffuse into the first A metal oxide layer, thereby forming a first diffusion region; sequentially depositing a second A metal oxide layer including an A metal element and a second B metal oxide layer including a B metal element on the first B metal oxide region; and then A second annealing process is performed, which causes the B metal element of the first B metal oxide region to diffuse into the second A metal oxide layer to form a second diffusion region, and causes the B metal element of the second B metal oxide layer to diffuse into the second A metal oxide layer to form a third diffusion region.
Citation Information
Patent Citations
Copper cooling plate with multilayer protrusions containing wear-resistant material for blast furnace
KR1020190070993A
Flash memory device with stacked dielectric structure including zirconium oxide and method for fabricating the same
CN101064349A
Dielectric layer for semiconductor device and method of manufacturing the same
CN1655362A
Method for fabricating capacitor in semiconductor device
CN1976008A
Fabricating method for capacitor with compositedielectric
KR1020050062132A