Graphene precursor identification method, identification device and recording medium
By determining the zero point of the diffraction angle and calculating the integral intensity ratio, accurately distinguishing the hexagonal crystal system and rhombic crystal system in the graphite raw materials, the problem of difficulty in distinguishing graphene precursors is solved, and low-cost generation and efficient production of graphene are achieved.
Patent Information
- Application Number
- CN201980031804.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-05-14
- Filing Date
- 2019-02-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-02-26
AI Technical Summary
The prior art is difficult to accurately determine the ratio of the hexagonal crystalline graphite layer and the rhombic crystalline graphite layer through powder X-ray diffraction patterns, which leads to difficulty in identifying graphene precursors and affects the low-cost generation of graphene.
By determining the zero point of the diffraction angle, the peak positions of the hexagonal and rhombic crystalline graphite layers are calculated, the integral intensity is calculated, and whether the graphite raw material is a graphene precursor is determined according to the specific integral intensity ratio. This method is used to achieve graphene Accurately judge and generate.
Reliable peak separation of graphite raw materials is achieved, and the ratio of hexagonal crystal system and rhombic crystal system in graphite raw materials is accurately measured, ensuring low-cost generation and efficient production of graphene.
Smart Images

Figure CN112105918B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method, a device and a program for distinguishing a graphene precursor of a graphite raw material mixed with hexagonal graphite layers and rhombohedral graphite layers. Background Art
[0002] Graphene is a new type of carbon material discovered by Dr. Geim and Dr. Novosolv of Manchester University in the UK in 2004. According to them, it has been found that graphene has a strength of more than 100 times that of steel, and has 10 to 100 times the thermal conductivity and electrical properties of metals. Furthermore, due to the extremely small planar crystal structure, it has a complete barrier property that prevents all substances such as gas and liquid from passing through, and has properties that are far superior to those of conventional substances.
[0003] Due to this great discovery, the Nobel Prize in Physics was awarded to the two of them in 2010, just six years after the discovery, breaking the tradition of the Nobel Prize. Since then, research on next-generation semiconductors, communication components, electronic devices, batteries, etc. based on graphene has been booming, and even in Europe and the United States, it is claimed that the 21st century will become the "era of graphene valley", imitating the Silicon Valley in California, USA, which developed with the high performance of silicone semiconductors in the second half of the 20th century.
[0004] Graphene is an extremely thin nano-carbon material with a thickness of only one atom. Since carbon atoms have a special crystal structure in which a two-dimensional plane is formed by bonding in a honeycomb shape, the electron mobility of graphene is extremely high, and graphene also shows excellent physical properties in terms of optical properties, thermal properties, mechanical properties, etc. Therefore, as a next-generation material, the research and development of graphene is being actively promoted. There are several methods for synthesizing graphene, but among them, there is a method for obtaining graphene from graphite (black lead), which is also a material for pencils. Graphite is a substance in which two-dimensional graphene is bonded to each other into a multi-layer three-dimensional structure, so graphene can be obtained by peeling it off (see patent document 1).
[0005] The benefit of the exfoliation method of exfoliating graphene from graphite is that it can greatly reduce production costs. Compared with CVD (chemical vapor deposition), which is the main method for producing graphene other than the exfoliation method, the high production efficiency of the exfoliation method is obvious. CVD is a method in which a substrate such as copper is placed in a vacuum container and a gas containing carbon, which is the material of graphene, is flowed therein. It is possible to form a large-area, high-quality graphene film on the substrate, but because a vacuum environment is used, the cost is relatively high, and in order to produce 1m 2Depending on the quality, tens to hundreds of tons of graphene will be consumed. On the other hand, in the peeling method, graphene weighing about 1 kg can be obtained at the same cost of tens to hundreds of tons. This is because graphene is extremely thin and light, and its surface area per unit weight is 2500m 2 / g is a huge value, so if the weight is 1kg, the area of the film formed on the substrate is equivalent to 2.5 million m 2 That is, if the weight is used as the basis for comparison, the cost difference between CVD and exfoliation is about 2.5 million times.
[0006] On the one hand, the crystal structure of graphite can be known by investigating the diffraction phenomenon caused by scattering or interference of X-rays when irradiating a sample with X-rays (X-ray diffraction). As long as the peak separation of the obtained profile is performed by the powder X-ray diffraction method, the existence ratio of each crystal structure can be determined based on the integrated intensity ratio of each peak (see non-patent document 1).
[0007] Prior Art Literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application No. 2016-038692
[0010] Non-patent literature
[0011] Non-patent document 1: RA Young, "The Rietveld Method", International Union of Crystallography Oxford University Press 1995, p. 255-275 Summary of the invention
[0012] Problems to be solved by the invention
[0013] It is expected that graphene produced by CVD will be produced in small quantities for high value-added applications in the future. However, if such applications are excluded, it is reliable to produce graphene in large quantities for industrial use in various applications by exfoliation.
[0014] In this case, it is important to determine the existence ratio of each crystal structure based on the integrated intensity of two peaks near the diffraction angle 2θ of 42 to 46° in the profile obtained by powder X-ray diffraction method from the graphite raw material, and evaluate the suitability as a graphene precursor.
[0015] Figure 7 (a) and (b) are diagrams showing the profiles of powder X-ray diffraction patterns in which peaks can be identified and in which peaks cannot be identified. Figure 7 As shown in (a) of FIG. 1 , when the peaks can be clearly identified from the appearance of the profile, peak separation can be sufficiently performed by peak profile fitting.
[0016] However, in the powder X-ray diffraction pattern for graphite raw materials derived from, for example, natural graphite, Figure 7 As shown in (b), the contoured appearance shows a gentle mountain over the entire angle range, and the peaks cannot be distinguished from the appearance. In such a case, peak separation cannot be performed even if peak contour fitting is simply applied.
[0017] The present invention has been made in view of such circumstances, and an object of the present invention is to provide a method, an apparatus and a program for identifying a graphene precursor that can reliably perform peak separation by peak profile fitting using a powder X-ray diffraction pattern of a graphite raw material.
[0018] Means for solving problems
[0019] (1) In order to achieve the above-mentioned purpose, the method for distinguishing a graphene precursor of the present invention is a method for distinguishing a graphene precursor of a graphite raw material that is a mixture of hexagonal graphite layers and rhombohedral graphite layers, and is characterized by comprising: a step of determining the zero point of the diffraction angle based on the powder X-ray diffraction data of the graphite raw material; a step of calculating the peak position specific to the hexagonal graphite layer and the rhombohedral graphite layer based on the determined zero point, assuming that the surface spacing of the graphene sheet forming the graphite raw material and the crystal structure within the graphene sheet are the same in any graphite layer mixed into the graphite raw material; a step of calculating the integrated intensity at the calculated peak position; and a step of distinguishing whether the graphite raw material is a graphene precursor based on the calculated integrated intensity.
[0020] Thus, peak separation can be reliably performed using the powder X-ray diffraction pattern of the graphite raw material. As a result, the ratio of the hexagonal graphite layer and the rhombohedral graphite layer in the graphite raw material can be accurately measured, and whether the graphite raw material is a graphene precursor can be accurately and precisely determined. Thus, the exfoliation method can be applied to generate graphene at a low cost.
[0021] (2) In addition, the method for identifying a graphene precursor of the present invention is characterized in that, in the step of determining the zero point of the diffraction angle, the peak position of the diffraction line having the graphene sheet as a lattice plane is used under the assumption that the interplanar spacing of the graphene sheet forming the graphite raw material is the same in any structure mixed into the graphite raw material, thereby determining the zero point of the diffraction angle based on the peak position.
[0022] (3) In addition, the method for identifying a graphene precursor of the present invention is characterized in that, in the step of determining the zero point of the diffraction angle, the peak position of the diffraction line having the plurality of graphene sheets as lattice planes is used, thereby eliminating errors and accurately determining the zero point of the diffraction angle.
[0023] (4) In addition, the method for identifying a graphene precursor of the present invention is characterized in that, in the step of identifying, it is determined whether the ratio of the calculated integrated intensity value of the 101 diffraction line of the hexagonal graphite layer at the peak position to the integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer is greater than a given value. Thus, the graphite raw material to which the graphene exfoliation method can be applied can be identified using the integrated intensity value that is easy to compare.
[0024] (5) In addition, the method for distinguishing a graphene precursor of the present invention is characterized in that, when the calculated integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer is set to P3 and the integrated intensity value of the 101 diffraction line of the hexagonal graphite layer is set to P4, it is determined whether P3 / (P3+P4) is greater than 0.31. Thus, the graphite raw material to which the graphene exfoliation method can be applied can be clearly distinguished using specific numerical values.
[0025] (6) In addition, the discrimination device of the present invention is a discrimination device for graphene precursors of a graphite raw material in which hexagonal graphite layers and rhombohedral graphite layers are mixed, and is characterized by comprising: a zero point determination unit, which determines the zero point of the diffraction angle for the powder X-ray diffraction data of the graphite raw material; a peak position calculation unit, which calculates the peak position specific to the hexagonal graphite layer and the rhombohedral graphite layer based on the determined zero point, assuming that the plane spacing of the graphene sheet forming the graphite raw material and the crystal structure in the graphene sheet are the same in any graphite layer mixed as the graphite raw material; an integrated intensity calculation unit, which calculates the integrated intensity at the calculated peak position; and an output unit, which can discriminately output whether the graphite raw material is a graphene precursor based on the calculated integrated intensity. Thus, it is possible to reliably perform peak separation using the powder X-ray diffraction pattern for the graphite raw material and discriminate whether it is a graphene precursor.
[0026] (7) In addition, the discrimination program of the present invention is a discrimination program for graphene precursors of a graphite raw material mixed with hexagonal graphite layers and rhombohedral graphite layers, characterized by causing a computer to perform the following processing: a process of determining the zero point of the diffraction angle for the powder X-ray diffraction data of the graphite raw material; a process of calculating the peak position specific to the hexagonal graphite layer and the rhombohedral graphite layer based on the determined zero point, assuming that the interplanar spacing of the graphene sheet forming the graphite raw material and the crystal structure in the graphene sheet are the same in any graphite layer mixed with the graphite raw material; a process of calculating the integrated intensity at the calculated peak position; and a process of discriminatingly outputting whether the graphite raw material is a graphene precursor based on the calculated integrated intensity. Thus, peak separation can be reliably performed using the powder X-ray diffraction pattern of the graphite raw material, and discrimination can be performed as to whether it is a graphene precursor.
[0027] Effects of the Invention
[0028] According to the present invention, peak separation can be reliably performed by peak profile fitting using a powder X-ray diffraction pattern of a graphite raw material. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 (a) and (b) are diagrams showing the crystal structures of a hexagonal graphite layer and a rhombohedral graphite layer of graphite, respectively.
[0030] Figure 2 This is a schematic diagram showing the structure of the graphene precursor identification system of the present invention.
[0031] Figure 3 This is a block diagram showing the functional structure of the graphene precursor identification device of the present invention.
[0032] Figure 4 : is a flowchart showing the method for identifying a graphene precursor of the present invention.
[0033] Figure 5 (a) and (b) are graphs schematically showing the profiles of the powder X-ray diffraction patterns of the graphite raw material at 2θ of 0 to 90° and 40 to 45°, respectively.
[0034] Figure 6 It is a figure which shows the table which shows the experimental result of each sample.
[0035] Figure 7 (a) and (b) are diagrams showing the profiles of powder X-ray diffraction patterns in which a peak can be discerned and in which a peak cannot be discerned, respectively. DETAILED DESCRIPTION
[0036] Next, refer to the attached Figure 1 In order to facilitate understanding of the description, the same components are denoted by the same reference numerals in each drawing, and repeated descriptions are omitted.
[0037] [Graphene Precursor]
[0038] The hexagonal graphite layer contained in a large amount of natural graphite is very stable, so graphene is peeled off by giving energy that exceeds the van der Waals force between the graphene layers. Moreover, the energy required for peeling is inversely proportional to the cube of the thickness. Therefore, in a thick state where the layers are countless and overlapped, the energy is very weak, so graphene is peeled off by weak physical forces such as ultrasound, but when peeling from a somewhat thin graphite, it becomes necessary to have a very large amount of energy.
[0039] The exfoliation method for generating graphene by exfoliating graphite can be further improved by using a suitable "graphene precursor". Graphene precursor is graphite with a certain crystalline structure. If it is subjected to a conventional exfoliation process (ultrasonic, supercritical, high-pressure jet, collision, grinding, oxidation-reduction, microwave (in ionic liquid), kneading, etc.), the production efficiency can be increased by 2.5 million times compared to the production of graphene by CVD method, according to theoretical values.
[0040] Compared with general graphite, graphene precursor has lower crystallinity and is easy to peel off, so even without the concentration process required in the previous peeling method, high-concentration graphene can be generated in large quantities. Through this technology, mass production of graphene can be carried out (annual production of 100 tons to 10,000 tons of super-scale), and sufficient material supply can be carried out in the fields of secondary batteries, capacitors, resin-rubber composite materials, and composite materials for building materials that require relatively cheap nano blanks (20 to 100 tons per 1kg). It is believed that the development of materials for the use of graphene will become more prosperous in the future. If the above method becomes a standard, the discrimination of graphene precursors will become more important for enterprises and organizations that supply graphene precursors as their raw materials.
[0041] [Principle of the discrimination method]
[0042] Such a graphene precursor is composed of a rhombohedral graphite layer 3RH containing a certain ratio or more relative to the hexagonal graphite layer 2H. In addition, the so-called hexagonal system can be any crystal structure that has a roughly hexagonal crystal, and can be an absolute hexagonal crystal, a hexagonal crystal with a portion of the crystal structure destroyed, or a hexagonal crystal that is deformed in whole or in part. The same is true for the rhombohedral system.
[0043] Figure 1(a) and (b) are diagrams showing the crystal structures of the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH of graphite, respectively. It is known that natural graphite is divided into three types of crystal structures, namely, hexagonal graphite layer, rhombohedral graphite layer, and disordered graphite layer, according to the overlapping pattern of the layers. Figure 1 As shown in (a), the hexagonal graphite layer 2H is a crystal structure in which layers are stacked in the order of ABABAB..., as shown in FIG. Figure 1 As shown in (b), the rhombohedral graphite layer 3RH has a crystal structure in which layers are stacked in the order of ABCABCABC... However, the rhombohedral graphite layer 3RH is actually classified as a rhombohedral crystal, but is regarded as Figure 1 As shown in (b), hexagonal crystals are pseudo-formed and are represented using axes of the hexagonal system (that is, hereinafter, in any crystal system, the a-axis, b-axis, and c-axis of the hexagonal system are used to represent).
[0044] Regarding natural graphite, rhombohedral graphite layers are almost non-existent in the excavation stage, but the ratio increases due to pulverization in the refining stage, and the rhombohedral graphite layers exist in about 14% of the natural graphite-based carbon blank. The ratio of rhombohedral graphite layers can be increased by treating natural graphite with physical force and heat, and the ratio can be further increased by using radio wave force.
[0045] The crystal structure of graphite can be known by a method (X-ray diffraction) that investigates diffraction phenomena caused by scattering and interference of X-rays when the sample is irradiated with X-rays. Therefore, it is possible to compare the integrated intensity of the unique peaks in each crystal structure measured by X-ray diffraction, and to determine whether the sample is a graphene precursor based on whether the ratio of rhombohedral crystal graphite layers is above a given value. For example, the following mathematical formula (1) can be used for determination.
[0046] 31%≤Rate(3RH)=P3 / (P3+P4)···(1)
[0047] P3: Integrated intensity value of rhombohedral graphite layer (101) (2θ = 43 degrees level)
[0048] P4: Integrated intensity value of hexagonal graphite layer (101) (2θ = 44d degree level)
[0049] The integrated intensity of the peak of the powder X-ray diffraction pattern can be calculated by assigning initial values (position, width, height, etc.) to the peak and setting constraints during refinement so that the parameters do not diverge, and performing profile fitting. At this time, since the convergence position of the parameters changes according to the setting of the initial values, it is necessary to use appropriate initial values in the calculation of the correct integrated intensity.
[0050] Therefore, in the present invention, the assumption is used that "the graphite raw material contains two types of homogeneous crystals, namely hexagonal graphite layers 2H and rhombohedral graphite layers 3RH, but both are obtained under a closed synthesis environment (generation environment), so the surface spacing between graphene sheets and the structure of the graphene sheets are the same in any structure."
[0051] Therefore, the following relations (1) and (2) hold true for the lattice constants in the two crystal structures.
[0052] (1) The lengths of the a and b axes of 2H are equal to those of the a and b axes of 3RH.
[0053] (2) The length of the c-axis of 2H is 2 / 3 times the length of the c-axis of 3RH.
[0054] The initial value of the peak position is determined so as to satisfy these two relationships. Since the peak position is finally accurate, it is okay to use a value slightly deviated from the correct value as the initial value. In addition, the length of the c-axis can also be calculated and solved based on the peak position of the 002 plane appearing at about 26°.
[0055] [Structure of the discrimination system of graphene precursor]
[0056] Next, a system capable of distinguishing a graphene precursor based on the above-mentioned assumption will be described. Figure 2 2 is a schematic diagram showing the structure of the graphene precursor discrimination system 10. Figure 2 As shown, the graphene precursor identification system 10 includes an X-ray diffraction device 100 and an identification device 200. The X-ray diffraction device 100 and the identification device 200 are connected so as to be able to send and receive information. The connection includes information transmission via a storage medium regardless of wired or wireless.
[0057] (X-ray diffraction device)
[0058] The X-ray diffraction device 100 is a device for measuring a powder X-ray diffraction pattern by irradiating a powder sample S with X-rays of a certain wavelength such as CuKα1 rays. The X-ray diffraction device 100 includes a goniometer 110, which includes an X-ray source arm 120, a detector arm 130, and a sample support table 150. The X-ray source arm 120 supports an X-ray source 121, and the detector arm 130 supports an X-ray detector 131.
[0059] The sample support table 150 provided at the center of the goniometer 110 detachably supports the sample holder 155. A powder sample S is filled in a recess formed in the sample holder 155.
[0060] The X-ray source arm 120 and the detector arm 130 are each independently rotatable around the same rotation axis, which is set to pass through the surface of the sample S supported by the goniometer 110 .
[0061] An X-ray generator 122 and a divergence slit 125 are fixed to the X-ray source arm 120. Other optical elements, such as a solar slit for parallelizing X-rays and a monochromator for extracting characteristic X-rays from X-rays containing various wavelengths, can also be arranged on the X-ray source arm 120 as needed.
[0062] A filament that generates thermal electrons when energized and a target that is disposed opposite to the filament are provided inside the X-ray generator 122. In the target, a region where the thermal electrons collide becomes the X-ray source 121.
[0063] The detector arm 130 is provided with a scattering slit 135, a light receiving slit 137 and an X-ray detector 131. The scattering slit 135 prevents scattered X-rays from entering the X-ray detector 131. The light receiving slit 137 prevents X-rays other than concentrated X-rays from entering the X-ray detector 131. The X-ray detector 1311 is, for example, composed of a 0-dimensional X-ray detector, which outputs a signal corresponding to the amount of received X-rays, and the intensity detection circuit calculates the X-ray intensity based on the output signal. As the X-ray detector, a 1-dimensional X-ray detector or a 2-dimensional X-ray detector can also be used. In addition, the X-ray diffraction device 100 can be an X-ray diffraction device as long as it has a focusing optical system and can measure a powder X-ray diffraction pattern, and a structure different from the above, such as setting the X-ray detector 131 on the Rowland Circle, can also be adopted.
[0064] (Graphene precursor identification device)
[0065] The graphene precursor identification device 200 has a processor 200p and a memory 200m in hardware structure, and can be configured by a PC, for example. The identification device 200 can calculate the integrated intensity of the peaks of each crystal structure for the graphite raw material mixed with the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH based on the powder X-ray diffraction pattern obtained by the processor 200p executing the program stored in the memory 200m. As a result, the user can determine whether it is a graphene precursor.
[0066] The determination device 200 receives input from the user and outputs the processing result to the user. The input from the user can be performed via an operation device such as a keyboard, a mouse, or a touch screen, and can be displayed via an output device such as a display.
[0067] Figure 32 is a block diagram showing the functional structure of the graphene precursor identification device 200. Figure 3 As shown, the identification device 200 includes a data management unit 210 , an input unit 220 , a zero point determination unit 230 , an integrated intensity calculation unit 260 , a fitting execution unit 240 , a determination unit 270 , and an output unit 280 .
[0068] The data management unit 210 stores and manages the powder X-ray diffraction data received from the X-ray diffraction device 100 for the sample. The input unit 220 receives input from an operating device such as a keyboard, a mouse, or a touch screen operated by a user. For example, when the user specifies a sample via an operating device, the input unit 220 receives the specification, and the data management unit 210 sets the powder X-ray diffraction data of the specified sample as a processing object. In addition, the powder X-ray diffraction data refers to data obtained by the powder X-ray diffraction method, and the powder X-ray diffraction pattern or profile refers to a pattern or profile captured by using the obtained data as a diffraction pattern or profile. Although the capturing method is different, the object data is essentially the same.
[0069] The zero point determination unit 230 determines the zero point of the diffraction angle for the powder X-ray diffraction data of the graphite raw material. Preferably, under the assumption that the c-axis length of the hexagonal graphite layer 2H of the graphite raw material is 2 / 3 of the c-axis length of the rhombohedral graphite layer 3RH, the zero point of the diffraction angle is determined according to the peak position of the diffraction line caused by the common lattice plane in the c-axis direction in the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH. Thus, the zero point of the diffraction angle can be determined according to the peak position. It is preferred to use the peak position of the diffraction line caused by the lattice planes in multiple c-axis directions to determine the zero point of the diffraction angle. For example, when using two peak positions, it is only necessary to solve the simultaneous equations. In addition, when using more than three peak positions, regression analysis such as the least squares method can be used. Thus, it is possible to eliminate errors and correctly determine the zero point of the diffraction angle. In addition, the zero point can also be determined using a single peak position, and in this case, since a high-order peak is used, the influence of errors can be suppressed to a small extent.
[0070] The integral intensity calculation unit 260 calculates the peak position specific to the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH according to the determined zero point, under the assumption that the length of the a-axis and the b-axis of the hexagonal graphite layer 2H of the graphite raw material is consistent with the length of the a-axis and the b-axis of the rhombohedral graphite layer 3RH, and the c-axis length of the hexagonal graphite layer 2H is 2 / 3 of the c-axis length of the rhombohedral graphite layer 3RH. Thus, it is possible to reliably perform peak separation using the powder X-ray diffraction pattern for the graphite raw material. As a result, it is possible to correctly measure the ratio of the rhombohedral graphite layer 3RH to the hexagonal graphite layer 2H in the graphite raw material, so that it is possible to correctly and accurately distinguish whether the graphite raw material is a graphene precursor. In this way, the graphene exfoliation method can be applied to generate graphene at low cost.
[0071] Then, the integrated intensity calculation unit 260 calculates the integrated intensity at the calculated peak position based on the result obtained by the fitting execution unit 240. The fitting execution unit 240 fits the function representing the peak for the X-ray diffraction peak based on the assigned initial value. For example, in the scenario of determining the peak position of the main peak, it is possible to perform a fitting based on the full pattern decomposition for a relatively wide angle range based on the information of the crystal system and lattice constant. In addition, in the scenario of calculating the integrated intensity, it is possible to perform a fitting using a Lorentz function.
[0072] The determination unit 270 determines whether the graphite raw material is a graphene precursor based on the calculated integrated intensity. In the step of determination, it is preferred to determine whether the ratio of the integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer 3RH at the calculated peak position to the integrated intensity value of the 101 diffraction line of the hexagonal graphite layer 2H is greater than a given value. Thus, the graphite raw material to which the graphene exfoliation method can be applied can be determined using an integrated intensity value that is easy to compare.
[0073] Specifically, when the calculated integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer 3RH is set to P3, and the integrated intensity value of the 101 diffraction line of the hexagonal graphite layer 2H is set to P4, it is preferably determined whether P3 / (P3+P4) is greater than 0.31. Thus, the graphite raw material to which the graphene exfoliation method can be applied can be clearly determined using specific numerical values.
[0074] Based on the calculated integrated intensity, the output unit 280 can output whether the graphite raw material is a graphene precursor in a discriminative manner. For example, the output unit 280 can display the integrated intensity value P3 of the 101 diffraction line of the rhombohedral graphite layer 3RH and the integrated intensity value P4 of the 101 diffraction line of the hexagonal graphite layer 2H on the display in a comparative manner. In addition, the output unit 280 can also display the ratio P3 / (P3+P4) of the above-mentioned integrated intensity values. In this case, the display is set to the discriminating material and the user himself discriminates whether the sample is a graphene precursor. On the other hand, the output unit 280 can also display the result of discriminating whether the sample is a graphene precursor by the judging unit 270. In this case, the burden of discriminating for the user disappears.
[0075] [Method for identifying graphene precursors]
[0076] By using the determination system 10 configured as described above, it is possible to determine whether the graphite raw material is a graphene precursor. Figure 4 This is a flowchart showing a method for identifying a graphene precursor. The method will be described from the stage of preparing powder X-ray diffraction data to facilitate understanding.
[0077] First, prepare graphite raw materials. The graphite raw materials used as graphene precursors can be generated by implementing a process based on electric wave force and a process based on physical force in a vacuum or air. That is, in a vacuum or air, natural graphite materials are treated with electric wave forces such as microwaves, millimeter waves, plasma, electromagnetic induction heating (IH), magnetic fields, and physical forces such as ball grinding, jet grinding, centrifugal force, and supercritical forces, thereby obtaining a graphite carbon blank containing more rhombohedral graphite layers 3RH. It is preferred that the effects brought by electric wave force and physical force are simultaneously exerted, but it is also possible to cause electric wave force and physical force to exert their effects alternately at given intervals.
[0078] The powder X-ray diffraction pattern of the graphite raw material prepared in this way is measured (step S1). At this time, it is preferable to measure until 2θ becomes 90° or more. Figure 5 (a) and (b) are graphs schematically showing the profiles of the powder X-ray diffraction patterns of the graphite raw material at 2θ of 0 to 90° and 40 to 45°, respectively. Figure 5 (b) is to Figure 5 The enlarged curve in the dashed line of (a) is shown in Figure 2. Figure 5 Although the peaks cannot be identified in (a) and (b), schematic curve graphs are used to facilitate understanding.
[0079] Based on the obtained powder X-ray diffraction pattern, the peak positions of the 002, 004, and 006 diffraction lines of graphite are calculated by full pattern decomposition (step S2). Full pattern decomposition is a method of performing profile fitting over a wide angle range based on information on the crystal system and lattice constants.
[0080] In this way, the length of the c-axis of the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH of graphite is determined (step S3), thereby determining the zero point of 2θ. Then, the initial value of the length of the a-axis of the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH of graphite is set to the same value (step S4). Based on the initial values of the hexagonal graphite layer 2H and the rhombohedral graphite layer 3RH of graphite, the initial values of the four peak positions with 2θ of 42 to 46° are calculated (step S5). At this time, from the perspective of processing efficiency, it is preferred to cut out the data with 2θ of 40 to 50°. In addition, the initial values of the shape parameters of the four peaks are set (step S6).
[0081] Contour fitting is performed in the optimal order so that each parameter does not diverge, thereby refining each parameter (step S7). The integrated intensity ratio Rate(3RH)=P3 / (P3+P4) of the 101 peaks of the rhombohedral graphite layer 3RH and the hexagonal graphite layer 2H of the graphite obtained in this way is calculated (step S8). Then, the value of the ratio Rate(3RH) of the two peaks obtained is displayed (step S9). In addition, although it is possible to select the peak representing the rhombohedral graphite layer 3RH and the peak representing the hexagonal graphite layer 2H, it is preferred to use P3 and P4. Preferably, if the powder X-ray diffraction data of the graphite raw material is determined, the value of Rate(3RH)=P3 / (P3+P4) is automatically displayed.
[0082] In addition, in step S7, the contour fitting of the four peaks is performed by the following steps. That is, the scale factor is refined, and the half widths of P2 and P3 are refined. At this time, the half widths of P4 and P5 are preferably set to the same value as P3. Then, the peak positions of P2 to P5 are refined. In addition, the series of actions of the above-mentioned steps S2 to S9 can be performed by executing the program.
[0083] [Example]
[0084] The data of the sample were measured using the above-mentioned method for identifying the graphene precursor, and the value of Rate (3RH) was determined. Figure 6 Graph 1 is a diagram showing a table showing the experimental results of each sample. For each sample, samples provided by Graphene Platform Corporation were used, and data from the provider are shown as reference values.
[0085] In the profile fitting when solving Rate(3RH), based on several literature values (theoretical values of bonding distances), more than 100 measured data, and assuming that 2H Thus, the initial value of the peak position is determined. Then, the value where only the half width of P2 is narrower than the other peaks is adopted as the initial value. This is because it is judged that there are many cases where only P2 is visible in the measured data, and it has a narrower half width than the other three peaks. Finally, since the half width of P2 is refined independently, it is sufficient as long as it is narrower than P3 to P5, and there is no need to set the initial value more finely than necessary.
[0086] In the case of identifying graphene precursors, it is believed that various materials of various crystallite sizes are mixed according to the properties of graphite samples. In such cases, it is believed that the Lorentz function can give correct fitting results. Therefore, the Lorentz function is used as the profile function.
[0087] In this way, the value of Rate(3RH) can be automatically calculated with high accuracy from measurement to analysis based on the powder X-ray diffraction pattern in which the four peaks to be separated cannot be identified at all. Figure 6 As shown, a measured value of Rate (3RH) approximately close to the reference value is obtained. In the above-mentioned embodiment, the Lorentz function is used, but profile fitting can also be performed using the FP (Fundamental Parameter) method.
[0088] Explanation of symbols
[0089] 10: Discrimination system
[0090] 100: X-ray diffraction device
[0091] 110: Goniometer
[0092] 120: X-ray source arm
[0093] 121: X-ray source
[0094] 122: X-ray generating device
[0095] 125: Diverging Slits
[0096] 130: Detector arm
[0097] 131: X-ray detector
[0098] 135: Scattering Slit
[0099] 137: Light receiving slit
[0100] 150: Sample support table
[0101] 155: Sample holder
[0102] 200: Identification device
[0103] 200m: Memory
[0104] 200p: Processor
[0105] 210: Data Management Department
[0106] 220: Input
[0107] 230: Zero point determination department
[0108] 240: Fitting execution unit
[0109] 260: Integrated intensity calculation unit
[0110] 270: Judgment Department
[0111] 280: Output
[0112] S: sample.
Claims
1. A method for identifying a graphene precursor is a method for identifying a graphene precursor of a graphite raw material mixed with hexagonal graphite layers and rhombohedral graphite layers, characterized in that: include: The step of determining the zero point of the diffraction angle according to the peak position of the diffraction line based on one or more lattice planes in the c-axis direction for the powder X-ray diffraction data of the graphite raw material; A step of calculating the peak positions specific to the hexagonal graphite layer and the rhombohedral graphite layer based on the determined zero point, assuming that the interplanar spacing of the graphene sheet forming the graphite raw material and the crystal structure in the graphene sheet are the same in any graphite layer mixed as the graphite raw material, the lengths of the a-axis and the b-axis of the hexagonal graphite layer are equal to the lengths of the a-axis and the b-axis of the rhombohedral graphite layer, and the c-axis length of the hexagonal graphite layer of the graphite raw material is 2 / 3 of the c-axis length of the rhombohedral graphite layer; Based on the profile fitting, a step of calculating the integrated intensity at the peak position with the calculated peak position as an initial value and refined by the profile fitting; and Based on the calculated integrated intensity, when it is determined that the graphite raw material contains a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer, the graphite raw material is judged to be a graphene precursor; when it is determined that the graphite raw material does not contain a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer, the graphite raw material is judged to be not a graphene precursor.
2. The method for identifying a graphene precursor according to claim 1, characterized in that: In the step of determining the zero point of the diffraction angle, the peak position of the diffraction line having the graphene sheet as a lattice plane is used under the assumption that the interplanar spacing of the graphene sheets forming the graphite raw material is the same in any structure mixed into the graphite raw material.
3. The method for identifying a graphene precursor according to claim 2, characterized in that: In the step of determining the zero point of the diffraction angle, the peak positions of diffraction lines having the plurality of graphene sheets as lattice planes are used.
4. The method for identifying a graphene precursor according to any one of claims 1 to 3, characterized in that: In the step of determining, it is determined whether the ratio of the calculated integrated intensity value of the 101 diffraction line of the hexagonal graphite layer at the peak position to the integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer is greater than a given value, When the ratio relative to the integrated intensity value is determined to be greater than a given value, the graphite raw material is determined to be a graphene precursor, and when the ratio relative to the integrated intensity value is determined to be less than a given value, the graphite raw material is determined to be not a graphene precursor.
5. The method for identifying a graphene precursor according to claim 4, characterized in that: When the calculated integrated intensity value of the 101 diffraction line of the rhombohedral graphite layer is set to P3, and the calculated integrated intensity value of the 101 diffraction line of the hexagonal graphite layer is set to P4, it is determined whether P3 / (P3+P4) is greater than 0.31, When the P3 / (P3+P4) is greater than or equal to 0.31, the graphite raw material is determined to be a graphene precursor, and when the P3 / (P3+P4) is less than 0.31, the graphite raw material is determined not to be a graphene precursor.
6. A discriminating device for a graphene precursor of a graphite raw material mixed with hexagonal graphite layers and rhombohedral graphite layers, characterized in that: have: A zero point determination unit determines the zero point of the diffraction angle based on the peak position of the diffraction line based on one or more lattice planes in the c-axis direction for the powder X-ray diffraction data of the graphite raw material; A peak position calculation unit, which calculates peak positions specific to the hexagonal graphite layer and the rhombohedral graphite layer based on the determined zero point, assuming that the plane spacing of the graphene sheet forming the graphite raw material and the crystal structure in the graphene sheet are the same in any graphite layer mixed as the graphite raw material, the lengths of the a-axis and the b-axis of the hexagonal graphite layer are equal to the lengths of the a-axis and the b-axis of the rhombohedral graphite layer, and the c-axis length of the hexagonal graphite layer of the graphite raw material is 2 / 3 of the c-axis length of the rhombohedral graphite layer; an integrated intensity calculation unit that calculates, based on profile fitting, an integrated intensity at a peak position that takes the calculated peak position as an initial value and is refined by the profile fitting; and The output unit, based on the calculated integrated intensity, can output that the graphite raw material is a graphene precursor when it is determined that the graphite raw material contains a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer, and can output that the graphite raw material is not a graphene precursor when it is determined that the graphite raw material does not contain a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer.
7. A recording medium, which is a non-transitory computer-readable recording medium of a discrimination program for a graphene precursor of a graphite raw material in which hexagonal graphite layers and rhombohedral graphite layers are mixed, characterized in that: The program causes the computer to execute the following processing: For the powder X-ray diffraction data of the graphite raw material, the processing of determining the zero point of the diffraction angle according to the peak position of the diffraction line based on one or more lattice planes in the c-axis direction; Under the assumption that the inter-plane spacing of the graphene sheet forming the graphite raw material and the crystal structure in the graphene sheet are the same in any graphite layer mixed as the graphite raw material, the lengths of the a-axis and the b-axis of the hexagonal graphite layer are equal to the lengths of the a-axis and the b-axis of the rhombohedral graphite layer, and the c-axis length of the hexagonal graphite layer of the graphite raw material is 2 / 3 of the c-axis length of the rhombohedral graphite layer, the processing of calculating the peak positions specific to the hexagonal graphite layer and the rhombohedral graphite layer according to the determined zero point; Based on the profile fitting, a process of calculating the integrated intensity at the peak position which takes the calculated peak position as an initial value and is refined by the profile fitting; and Based on the calculated integrated intensity, when it is determined that the graphite raw material contains a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer, it can be outputted that the graphite raw material is a graphene precursor. When it is determined that the graphite raw material does not contain a rhombohedral graphite layer at a certain ratio or more relative to the hexagonal graphite layer, it can be outputted that the graphite raw material is not a graphene precursor.