Battery electrode and method for producing the same
By heat treatment of the boundary part of the electrode, Young's modulus is reduced, the problem of uneven volume density of the electrode material layer is solved, and the lithium ion precipitation state and electrode performance are improved.
Patent Information
- Application Number
- CN201980038721.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-06-11
- Filing Date
- 2019-06-05
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2039-06-05
AI Technical Summary
During the manufacturing process of battery electrodes, the volume density of the electrode material layer in the boundary portion of the single-sided coating area and the double-sided coating area is low, resulting in a different precipitation state of lithium than other regions, resulting in capacity deterioration and deterioration of cycle characteristics.
In the production method of electrodes, the current collector at the boundary portion of the double-sided coating area and the single-sided coating area is heat treated to reduce the Young's modulus, thereby increasing the contact range between the pressure roller and the boundary portion and reducing the contact range of the pressure roller and the boundary portion. Range of low volume density areas.
It effectively reduces the low volume density region of the electrode material layer, improves the uniformity of lithium ion precipitation, reduces the deterioration of capacity and cycling characteristics, and improves the overall performance of the electrode structure.
Smart Images

Figure CN112292770B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a battery electrode and a method for producing the same. Background Art
[0002] In recent years, the demand for batteries, especially rechargeable secondary batteries, has been increasing for electronic devices such as computers and smartphones. The battery has a structure in which electrodes (positive and negative electrodes) and an electrolyte are provided in a casing.
[0003] Here, the battery electrode can be manufactured by at least (i) coating an electrode material layer on the main surface of a collector (metal foil) to form an electrode precursor, and (ii) using a roller device to move the electrode precursor in one direction between a pair of rollers and pressurize the electrode precursor.
[0004] Regarding this press roller device, Patent Document 1 discloses using a piezoelectric drive element to adjust the distance between the rotation axes of a pair of press rollers. The pair of press rollers capable of adjusting the distance between the rotation axes can be used, for example, to press a precursor of an electrode having the following form.
[0005] Specifically, in a precursor of an electrode 100' having a single-sided coating region in which an electrode material layer 20' is coated on one main surface of a current collector 10', and a double-sided coating region in which electrode material layers 20' and 30' adjacent to the single-sided coating region are coated on both sides of the current collector 10', a pair of pressing rollers 40' capable of adjusting the distance between rotating axes can be used. In the precursor of the electrode 100', the total thickness of the current collector 10' in the double-sided coating region and the electrode material layers 20' and 30' supplied to both main surfaces of the current collector 10' is greater than the total thickness of the current collector 10' in the single-sided coating region and the electrode material layers 20' supplied to one main surface of the current collector 10' (refer to Figure 4A to Figure 4E ).
[0006] Therefore, in the precursor of the electrode 100' having the above-mentioned form, if a pair of pressing rollers 40' with adjustable distance between rotating axes are used, the distance between rotating axes can be adjusted according to the total thickness of the single-sided coating area and the total thickness of the double-sided coating area, thereby applying a specified pressure to each coating area.
[0007] Patent Document 1: Japanese Patent Application Publication No. 2015-089556 Summary of the invention
[0008] However, the inventors of the present application have found that the following technical problems may occur when pressurizing the electrode precursor 100 ′ including the single-sided coated region and the double-sided coated region adjacent to the single-sided coated region.
[0009] Specifically, when a pair of pressure rollers 40' are used to pressurize the single-sided coated area and the double-sided coated area, the pressurization state of the single-sided coated area located at the boundary portion 70' between the double-sided coated area and the single-sided coated area may be different from the pressurization state of the single-sided (or double-sided) coated area located at the portion other than the boundary portion 70'. This is because due to the presence of the electrode material layer 30' located at the end of the double-sided coated area, it is not easy for the pressure roller 40' to contact the collector 10' located at the single-sided coated area at the boundary portion 70' (refer to Figure 4A to Figure 4E ). Therefore, there is a concern that the collector 10' and the electrode material layer 20' located in the single-sided coated area of the boundary portion 70' cannot be properly pressurized by the pair of pressure rollers 40' facing each other. As a result, there is a concern that the volume density of the electrode material layer 20' located in the single-sided coated area of the boundary portion 70' is relatively low compared to the volume density of the electrode material layers 20' and 30' located in the portion other than the boundary portion 70'. That is, the electrode material layer 20' located in the single-sided coated area of the boundary portion 70' may become a low volume density area 23' (refer to Figure 1 upper part).
[0010] For example, when the battery is a lithium-ion secondary battery, the volume density of the electrode material layer is locally low in the low volume density region 23', and the lithium precipitation state caused by this is different from the lithium precipitation state in other regions. Alternatively, the presence of the low volume density region 23' may be the main cause of capacity degradation and cycle characteristics. In addition, when the electrode 100', which may include such a low volume density region 23', specifically the positive electrode and the negative electrode are laminated with each other through a separator to obtain an electrode structure, the presence of the low volume density region 23' may cause the characteristic deviation of the electrode structure.
[0011] Therefore, an object of the present invention is to provide an electrode and a method for manufacturing the same, which can reduce the range of the low volume density area of the electrode material layer in the single-sided coating area located at the boundary part between the single-sided coating area and the double-sided coating area when the electrode has a single-sided coating area and a double-sided coating area adjacent to the single-sided coating area.
[0012] In order to achieve the above object, in one embodiment of the present invention, an electrode is provided, which is a battery electrode, comprising:
[0013] A double-sided coating area, including a current collector and an electrode material layer coated on both sides of the current collector; and
[0014] The single-sided coating region is adjacent to the double-sided coating region and includes the current collector and the electrode material layer coated on one side of the current collector.
[0015] The Young's modulus of the current collector located at a boundary portion between the double-sided coated region and the single-sided coated region is relatively lower than the Young's modulus of the current collector located at a portion other than the boundary portion.
[0016] In order to achieve the above object, in one embodiment of the present invention, a manufacturing method is provided, which is a manufacturing method for a battery electrode, comprising the following steps:
[0017] (i) forming a precursor of the electrode having a double-sided coating region and a single-sided coating region, wherein the electrode material layer is coated on both sides of the current collector, the single-sided coating region and the double-sided coating region are adjacent to each other, and the electrode material layer is coated on one main surface of the current collector; and
[0018] (ii) a step of pressurizing the precursor of the electrode,
[0019] Before the precursor of the electrode is pressurized, the current collector located at a boundary portion between the double-sided coated region and the single-sided coated region is locally heat treated.
[0020] According to one embodiment of the present invention, when the battery electrode has a single-sided coating region and a double-sided coating region adjacent to the single-sided coating region, the range of the low volume density region of the electrode material layer in the single-sided coating region at the boundary portion between the single-sided coating region and the double-sided coating region can be appropriately reduced. In addition, the effects described in this specification are merely illustrative and not limiting, and may also have additional effects. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a schematic cross-sectional view comparing a conventional pressurized state of an electrode precursor and a pressurized state of an electrode precursor according to an embodiment of the present invention.
[0022] Figure 2 This is a schematic diagram showing a state in which a current collector located at a boundary portion is subjected to heat treatment using a high-frequency induction heating device.
[0023] Figure 3 This is a graph comparing Examples 1 and 2 with a comparative example (conventional example).
[0024] Figure 4A It is a schematic diagram showing the technical problem of the present application.
[0025] Figure 4B This is a schematic cross-sectional view showing a state in which pressure is applied to the single-sided coated region except for the boundary portion between the double-sided coated region and the single-sided coated region.
[0026] Figure 4C It means from Figure 4B A schematic cross-sectional view of a state in which a single-sided coated area other than a boundary portion between a double-sided coated area and a single-sided coated area is pressurized after a predetermined time has passed.
[0027] Figure 4D It means from Figure 4C A schematic cross-sectional view of a state in which a single-sided coating area located at a boundary between a double-sided coating area and a single-sided coating area is pressurized after a predetermined time has passed.
[0028] Figure 4E It means from Figure 4D A schematic cross-sectional view of the state in which the double-sided coating area is pressurized after a predetermined time has passed.
[0029] Figure 5 is a schematic cross-sectional view of a secondary battery.
[0030] Figure 6 is a schematic partial cross-sectional view of a wound electrode structure in a secondary battery.
[0031] Figure 7 This is a schematic exploded perspective view of a laminated film type square lithium ion secondary battery.
[0032] Fig. 8A is with Figure 7 The shown lithium ion secondary battery is a schematic exploded perspective view of a laminated film type lithium ion secondary battery of a different form.
[0033] Figure 8B The electrode structure in the laminated film type lithium ion secondary battery is Figure 7 and Fig. 8A Schematic cross-sectional view of arrow AA.
[0034] Fig. 9 This is a schematic exploded perspective view of an application example of a lithium-ion secondary battery (battery pack: single cell) having a laminate structure.
[0035] Fig. 10A This is a block diagram showing the structure of an application example (electric vehicle) of a lithium ion secondary battery including a laminate structure.
[0036] Fig. 10B This is a block diagram showing the structure of an application example (power storage system) of a lithium ion secondary battery including a laminate structure.
[0037] Fig. 10C This is a block diagram showing the structure of an application example (electric tool) of a lithium ion secondary battery including a laminate structure. DETAILED DESCRIPTION
[0038] Hereinafter, a battery electrode and a method for producing the same according to an embodiment of the present invention will be described with reference to the drawings.
[0039] (Method for producing battery electrode of the present invention)
[0040] First, a method for producing a battery electrode according to an embodiment of the present invention will be described (see Figure 1 lower side).
[0041] As described above, the inventors of the present application focus on the technical problem of reducing the volume density of the electrode material layer in the single-sided coated area located at the boundary portion between the single-sided coated area and the double-sided coated area when the electrode has a single-sided coated area and a double-sided coated area adjacent to the single-sided coated area. Specifically, the inventors of the present application focus on the technical problem that the direct factor for reducing the volume density of the electrode material layer is that "due to the presence of the electrode material layer located at the end of the double-sided coated area, it is not easy for the pressure roller to properly contact the collector in the single-sided coated area located at the boundary portion." As a result, in order to appropriately solve this technical problem, the inventors of the present application have developed a method for manufacturing a battery based on the following technical ideas.
[0042] The manufacturing method of the battery electrode of the present invention is based on the technical idea of "preparing the precursor of the electrode 100 to pressurize, locally heat-treating the current collector 10 located at the boundary portion 70 between the double-sided coating area and the single-sided coating area." According to the technical idea of the present invention, the timing of the local heat treatment of the current collector 10 located at the boundary portion 70 may be after the electrode material layer 20 is coated on the main surface of the current collector 10 (that is, after the precursor of the above-mentioned electrode 100 is formed), or it may be before the electrode material layer 20 is coated on the main surface of the current collector 10. In addition, in the latter form, before the electrode material layer 20 is coated on the main surface of the current collector 10, the current collector 10 may exist but the electrode material layer may not exist. Therefore, in the latter form, from the viewpoint of effective heat treatment, it is preferred to locally heat-treat the current collector 10 located at the boundary portion 70 on the basis of pre-knowing the location to be the boundary portion 70. In addition, the "boundary portion" referred to in this specification refers to the portion transitioning from the double-sided coating area to the single-sided coating area, or the portion transitioning from the single-sided coating area to the double-sided coating area. The "heat treatment" referred to in this specification refers to a treatment of providing thermal energy to the collector in a broad sense. The "heat treatment" referred to in this specification refers to a treatment used to improve ductility by providing thermal energy to the collector to eliminate deformation inside the collector and soften it. From this point of view, the "heat treatment" may also be referred to as "annealing treatment" or "annealing treatment". The "electrode precursor" referred to in this specification refers to a double-sided coating area having an electrode material layer coated on both sides of the collector, and a single-sided coating area having an electrode material layer adjacent to the double-sided coating area coated on one main surface of the collector.
[0043] According to this technical idea, the part of the collector 10 which is located at the boundary part 70 between the double-sided coating area and the single-sided coating area and is subjected to heat treatment can be softened due to the heat energy supplied to the part. Therefore, by implementing this heat treatment, the Young's modulus of the collector 10 located at the boundary part 70 can be reduced compared with the Young's modulus of the collector 10 located at the part other than the boundary part 70. In particular, since the electrode material layer 20 is on the upper side of the collector 10 located in the single-sided coating area of the boundary part 70, the deadweight of the electrode material layer 20 can work. Therefore, the collector 10 located in the single-sided coating area of the boundary part 70 subjected to heat treatment can be gently bent in the downward direction.
[0044] Thus, when the precursor of the electrode 100 is subsequently pressurized using a pair of press rollers 40, the range in which the press rollers 40 can contact the collector 10 located in the single-sided coated region of the boundary portion 70 can be increased compared to the conventional case where no heat treatment is performed. In addition, from the viewpoint of appropriately increasing the range in which the press rollers 40 can contact the collector 10 located in the single-sided coated region of the boundary portion 70, it is preferred that the Young's modulus of the collector 10 located in the boundary portion 70 be reduced by more than 50% of the Young's modulus of the collector located outside the boundary portion 70.
[0045] As a result, the range in which the current collector 10 and the electrode material layer 20 located in the single-sided coated region of the boundary portion 70 can be appropriately pressurized can be expanded by the pair of pressing rollers 40 facing each other. Therefore, the range of the low volume density region 23 of the electrode material layer 20 located in the single-sided coated region of the boundary portion 70 can be reduced. In other words, the range of the high volume density of the electrode material layer 20 located in the single-sided coated region of the boundary portion 70 can be increased.
[0046] Thus, the difference between the volume density of the electrode material layer in the coating area located at the boundary portion 70 and the volume density of the electrode material layer located outside the boundary portion can be reduced. Specifically, the ratio (A / B) of the volume density (A) of the electrode material layer located at the boundary portion relative to the volume density (B) of the electrode material layer located outside the boundary portion can be set to be greater than 0.9 and less than 1.0. Therefore, in the case where the electrode has a single-sided coating area and a double-sided coating area adjacent to the single-sided coating area, it is also possible to form an electrode material layer with a reduced range of the low volume density area 23 as a whole. As a result, the electrode can function appropriately as a component of the battery.
[0047] As described above, since the scope of the low volume density region of the electrode material layer can be reduced as a whole, when the battery is a lithium ion secondary battery, the precipitation state of lithium in the boundary portion can be appropriately suppressed and can be different from the precipitation state of lithium in other parts except the boundary portion. In addition, since the scope of the low volume density region can be reduced as a whole, the degradation of capacity and cycle characteristics can also be reduced. In addition, since the scope of the low volume density region of the constituent elements of the electrode, that is, the electrode material layer, can be reduced, when the electrodes (positive and negative electrodes) are laminated to each other across the separator to obtain the electrode structure, the characteristic deviation of the electrode structure can also be appropriately suppressed.
[0048] In one embodiment, the method for producing an electrode of the present invention preferably takes the following form.
[0049] In one embodiment, it is preferred that the current collector 10 and the electrode material layers 20 and 30 located at the boundary portion 70 be subjected to a non-contact heat treatment.
[0050] In the manufacturing method of the present invention, from the viewpoint that the shape of the current collector located at the boundary portion is easily deformed compared to the current collector located outside the boundary portion, the current collector located at the boundary portion is subjected to heat treatment. Here, the constituent elements of the electrode, namely the current collector and the electrode material layer, can affect the battery characteristics. Therefore, for example, if the heating device is directly contacted with the current collector and the electrode material layer in the single-sided coating area located at the boundary portion while heating, there is a concern that the current collector and the electrode material layer will break due to direct contact.
[0051] Therefore, it is preferred to perform non-contact heat treatment on the current collector and the electrode material layer located at the above-mentioned boundary portion rather than direct contact. As an example, it is preferred to use a high-frequency induction heating device 80 to implement non-contact heat treatment. The high-frequency induction heating device 80 refers to a device that, for example, if the heated body is placed in a coil-shaped component connected to an AC power source, uses an AC current to generate a high-density eddy current near the surface of the heated body, and uses the Joule heat to heat the surface of the heated body. If this device is used and the current collector 10 (and the electrode material layer) is placed in a coil-shaped component connected to an AC power source, it is possible to use an AC current to generate a high-density eddy current near the surface of the current collector 10 (and the electrode material layer), and use the Joule heat to heat the surface of the current collector (and the electrode material layer).
[0052] In addition, it is preferred that the high-frequency induction heating device 80 is driven when the collector 10 located at the boundary portion 70 is opposed to each other. The boundary portion 70 between the double-sided coating area and the single-sided coating area can be formed at a certain interval. Therefore, it is not necessary to use a high-frequency induction heating device to continuously heat the precursor of the electrode. Therefore, it is preferred that when the precursor of the electrode moves in one direction, the high-frequency induction heating device (especially the coil-shaped component) is located at a specified position closer to the front section than the pressure roller in order to heat the collector at the boundary portion, and when the coil-shaped component of the high-frequency induction heating device is opposed to the collector located at the boundary portion, the device is driven. Thus, the high-frequency induction heating device 80 can be used only when necessary, and the heating of the collector, etc. other than the boundary portion 70 can be appropriately avoided.
[0053] (Battery electrode of the present invention)
[0054] Hereinafter, a battery electrode according to an embodiment of the present invention will be described.
[0055] The battery electrode 100 of the present invention can be obtained by the manufacturing method of the present invention described above. In particular, the battery electrode of the present invention may have the following characteristics. Specifically, as described above, the local portion of the collector 10 located at the boundary portion 70 between the double-sided coating area and the single-sided coating area and subjected to heat treatment can be softened due to the heat energy supplied to the portion. Therefore, compared with the case where the heat treatment is not applied, the shape of the collector 10 located at the boundary portion 70 becomes an easily deformable state. In one embodiment, from the perspective of appropriately increasing the range in which the collector 10 located in the single-sided coating area of the boundary portion 70 can contact the pressure roller 40, the Young's modulus of the collector 10 located at the boundary portion 70 is reduced by more than 50% compared with the Young's modulus of the collector 10 located in the portion other than the boundary portion 70. Furthermore, the properties and shape of the temporarily deformed collector located at the boundary portion 70 do not return to the original state after the pressurization treatment. That is, this means that in the battery electrode of the present invention obtained after the pressurization treatment, the Young's modulus of the current collector 10 at the boundary portion 70 is relatively lower than the Young's modulus of the current collector 10 at a portion other than the boundary portion 70 .
[0056] As described above, in the present invention, by a pair of pressing rollers 40 facing each other, the range in which the current collector 10 and the electrode material layer 20 located in the single-sided coated area of the boundary portion 70 can be appropriately pressurized can be expanded. Therefore, in the electrode of the present invention obtained after pressurization, the range of the low volume density region 23 of the electrode material layer 20 located in the single-sided coated area of the boundary portion 70 can be reduced. In one embodiment, compared with the case where the boundary portion 70 is not subjected to heat treatment, the range of the low volume density region 23 of the electrode material layer located in the single-sided coated area of the boundary portion 70 can be reduced by more than half. Thus, the difference between the volume density of the electrode material layer 20 located in the coated area of the boundary portion 70 and the volume density of the electrode material layer 20 located in the portion other than the boundary portion 70 can be reduced. Specifically, the ratio (A / B) of the volume density (A) of the electrode material layer located in the boundary portion to the volume density (B) of the electrode material layer located in the portion other than the boundary portion can be set to 0.9 or more and 1.0 or less. Thus, even when the electrode includes a single-sided coated region and a double-sided coated region adjacent to the single-sided coated region, an electrode material layer with a reduced range of the low volume density region 23 can be formed in an overall favorable manner.
[0057] In addition, the structural elements in the case where the battery of the present invention is used as a lithium ion secondary battery will be specifically described below.
[0058] In a lithium-ion secondary battery, during charging, for example, lithium ions are released from the positive electrode material (positive electrode active material) and are absorbed in the negative electrode active material via the non-aqueous electrolyte. Also, during discharging, for example, lithium ions are released from the negative electrode active material and are absorbed in the positive electrode material (positive electrode active material) via the non-aqueous electrolyte.
[0059] The components constituting the lithium-ion secondary battery are stored in the electrode structure storage component (battery can). As the components constituting the lithium-ion secondary battery, a positive electrode, a negative electrode, an electrolyte and a separator can be cited. The positive electrode is composed of, for example, a positive electrode collector and a positive electrode material layer. The negative electrode is composed of, for example, a negative electrode collector and a negative electrode material layer. In addition, a positive electrode lead portion is installed on the positive electrode collector, and a negative electrode lead portion is installed on the negative electrode collector.
[0060] A positive electrode material layer containing a positive electrode active material is formed on the main surface of the positive electrode collector constituting the positive electrode. As materials constituting the positive electrode collector, conductive materials such as aluminum, nickel, and stainless steel can be exemplified. As the positive electrode active material, a positive electrode material that can absorb / release lithium is contained. The positive electrode material layer may also contain a positive electrode binder, a positive electrode conductive agent, and the like. As positive electrode materials, lithium-containing compounds can be cited. From the perspective of obtaining high energy density, lithium-containing composite oxides and lithium-containing phosphate compounds are preferably used. Lithium-containing composite oxides are oxides containing lithium and one or more elements (hereinafter referred to as "other elements". Lithium is not included here) as constituent elements, and have a layered rock salt type crystal structure or a spinel type crystal structure. In addition, a lithium-containing phosphate compound is a phosphate compound containing lithium and one or more elements (other elements) as constituent elements, and has an olivine type crystal structure.
[0061] A negative electrode material layer containing a negative electrode active material is formed on the main surface of the negative electrode current collector constituting the negative electrode. As materials constituting the negative electrode current collector, conductive materials such as copper, nickel, and stainless steel can be cited. As negative electrode active materials, a negative electrode material that can absorb / release lithium is contained. The negative electrode material layer may also contain a negative electrode binder, a negative electrode conductive agent, etc. The negative electrode binder and the negative electrode conductive agent may be the same as the positive electrode binder and the positive electrode conductive agent.
[0062] The electrode structure composed of a positive electrode, a separator and a negative electrode can be a state in which the positive electrode, the separator, the negative electrode and the separator are wound, or a state in which the positive electrode, the separator, the negative electrode and the separator are stacked. The electrode structure can be in the form of being stored in the electrode structure storage component in a wound state. Alternatively, the electrode structure can be in the form of being stored in the electrode structure storage component in a stacked state. In the above case, the external shape of the electrode structure storage component can be cylindrical or square (flat) in form. As the form of a lithium ion secondary battery, coin type, button type, disc type, flat plate type, square type, cylindrical type, laminated type (laminated film type) can be cited.
[0063] As materials constituting the electrode structure storage component (battery can) of the cylindrical secondary battery, iron (Fe), nickel (Ni), aluminum (Al), titanium (Ti), etc. or their alloys, stainless steel (SUS), etc. can be cited. In order to prevent electrochemical corrosion accompanying the charging and discharging of the secondary battery, it is preferred that the battery can be plated with nickel, etc., for example. The outer casing in the laminated (laminated film type) secondary battery is preferably in the form of a laminated structure having a plastic material layer (fusion layer), a metal layer and a plastic material layer (surface protection layer), that is, in the form of a laminated film. In the case of a laminated film type secondary battery, for example, after the outer casing is folded in a manner in which the fusion layers are opposite to each other across the electrode structure, the peripheral edge portions of the fusion layers are fused to each other. However, the outer casing can also be formed by bonding two laminated films together by an adhesive, etc. The fusion layer is composed of, for example, a film of an olefin resin such as polyethylene, polypropylene, modified polyethylene, modified polypropylene, or a polymer thereof. The metal layer is composed of, for example, aluminum foil, stainless steel foil, nickel foil, etc. The surface protection layer is composed of, for example, nylon, polyethylene terephthalate, etc. Among them, the outer covering member is preferably an aluminum laminated film in which a polyethylene film, an aluminum foil, and a nylon film are laminated in sequence. However, the outer covering member may also be a laminated film having other laminated structures, a polymer film such as polypropylene, or a metal film.
[0064] In the following, when the battery is composed of a lithium ion secondary battery, the positive electrode component, negative electrode component, positive electrode mixture layer, positive electrode active material, negative electrode mixture layer, negative electrode active material, binder, conductive agent, separator, and non-aqueous electrolyte that constitute the lithium ion secondary battery are described.
[0065] In the positive electrode component, a positive electrode mixture layer containing a positive electrode active material is formed on both sides of the positive electrode collector. That is, the positive electrode mixture layer contains a positive electrode material that can absorb / release lithium as a positive electrode active material. The positive electrode mixture layer may further contain a positive electrode binder, a positive electrode conductor, etc. As materials constituting the positive electrode collector, for example, copper (Cu), aluminum (Al), nickel (Ni), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), zinc (Zn), germanium (Ge), indium (In), gold (Au), platinum (Pt), silver (Ag), palladium (Pd), etc., or conductive materials such as alloys containing any of the above, stainless steel, etc. can be exemplified. As the form of the positive electrode collector or the negative electrode collector described later, a foil-like material can be exemplified.
[0066] Lithium-containing compounds can be cited as positive electrode materials. From the perspective of obtaining high energy density, lithium-containing composite oxides and lithium-containing phosphate compounds are preferably used. Lithium-containing composite oxides are oxides containing lithium and one or more elements (hereinafter referred to as "other elements". However, except for lithium) as constituent elements, and have a layered rock salt type crystal structure or a spinel type crystal structure. In addition, lithium-containing phosphate compounds are phosphate compounds containing lithium and one or more elements (other elements) as constituent elements, and have an olivine type crystal structure.
[0067] The preferred materials constituting the positive electrode material, namely, the lithium-containing composite oxide and the lithium-containing phosphate compound are described in detail below. In addition, other elements constituting the lithium-containing composite oxide and the lithium-containing phosphate compound are not particularly limited, but any one or two or more elements belonging to Groups 2 to 15 in the long-period periodic table can be cited. From the viewpoint of obtaining a high voltage, nickel is preferably used. <ni>,cobalt <co>,manganese ,iron <fe>.
[0068] Specific examples of the lithium-containing composite oxide having a layered rock salt type crystal structure include compounds represented by Formula (B), Formula (C), and Formula (D).
[0069] Li a Mn 1-b-c Ni b M 11 c O 2-d F e (B)
[0070] Here, M 11 It is made from cobalt <co>,magnesium <mg>,aluminum <al>,boron ,titanium <ti>,vanadium <v>,chromium <cr>,iron <fe>,copper <cu>, zinc <zn>,zirconium <zr>,molybdenum ,tin <sn>,calcium <ca>,strontium <sr>and tungsten <w>At least one element selected from the group consisting of a, b, c, d, and e satisfies the following values:
[0071] 0.8≤a≤1.2
[0072] 0<b<0.5
[0073] 0≤c≤0.5
[0074] b+c<1
[0075] -0.1≤d≤0.2
[0076] 0≤e≤0.1.
[0077] However, the composition differs depending on the charge and discharge state, and a is a value in the fully discharged state.
[0078] Li a Ni 1-b M 12 b O 2-c F d (C)
[0079] Here, M 12 It is made from cobalt <co>,manganese ,magnesium <mg>,aluminum <al>,boron ,titanium <ti>,vanadium <v>,chromium <cr>,iron <fe>,copper <cu>, zinc <zn>,molybdenum ,tin <sn>,calcium <ca>,strontium <sr>and tungsten <w>At least one element selected from the group consisting of a, b, c, d has values that satisfy:
[0080] 0.8≤a≤1.2
[0081] 0.005≤b≤0.5
[0082] -0.1≤c≤0.2
[0083] 0≤d≤0.1.
[0084] However, the composition differs depending on the charge and discharge state, and a is a value in the fully discharged state.
[0085] Li a Co 1-b M 13 b O 2-c F d (D)
[0086] Here, M 13 It is made of nickel <ni>,manganese ,magnesium <mg>,aluminum <al>,boron ,titanium <ti>,vanadium <v>,chromium <cr>,iron <fe>,copper <cu>, zinc <zn>,molybdenum ,tin <sn>,calcium <ca>,strontium <sr>and tungsten <w>At least one element selected from the group consisting of a, b, c, d has values that satisfy:
[0087] 0.8≤a≤1.2
[0088] 0≤b<0.5
[0089] -0.1≤c≤0.2
[0090] 0≤d≤0.1.
[0091] However, the composition differs depending on the charge and discharge state, and a is a value in the fully discharged state.
[0092] As lithium-containing composite oxides having a layered rock salt type crystal structure, specifically, LiNiO2, LiCoO2, LiCo 0.98 Al 0.01 Mg 0.01 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.8 Co 0.15 Al 0.05 O2、LiNi 0.33 Co 0.33 Mn 0.33 O2、Li 1.2 Mn 0.52 Co 0.175 Ni 0.1 O2、Li 1.15 (Mn 0.65 Ni 0.22 Co 0.13 ) 0.85 O2. In addition, as LiNiMnO-based materials, specifically, LiNi 0.5 Mn 1.50 O4.
[0093] For example, in getting Li 1.15 (Mn 0.65 Ni 0.22 Co 0.13 ) 0.85 In the case where O2 is used as the positive electrode active material, first, nickel sulfate (NiSO4), cobalt sulfate (CoSO4), and manganese sulfate (MnSO4) are mixed together. Then, water is dispersed in the mixture to prepare an aqueous solution. Next, sodium hydroxide (NaOH) is added to the aqueous solution while the aqueous solution is fully stirred, thereby obtaining a coprecipitate (manganese-nickel-cobalt composite coprecipitated hydroxide). Thereafter, the coprecipitate is washed with water and dried, and then lithium hydroxide monohydrate is added to the coprecipitate to obtain a precursor. Then, the precursor is calcined in the atmosphere (800°C×10 hours), thereby obtaining the above-mentioned positive electrode active material.
[0094] For example, in obtaining LiNi 0.5 Mn 1.50 In the case where O4 is used as the positive electrode active material, first, lithium carbonate (Li2CO3), manganese oxide (MnO2), and nickel oxide (NiO) are weighed, and the weighed materials are mixed using a ball mill. In this case, the mixing ratio (molar ratio) of the main elements is set to Ni:Mn=25:75. Next, the mixture is calcined in the atmosphere (800°C×10 hours) and then cooled. Next, the calcined products are mixed again using a ball mill, and then the calcined products are calcined again in the atmosphere (700°C×10 hours), thereby obtaining the above-mentioned positive electrode active material.
[0095] In addition, as a lithium-containing composite oxide having a spinel crystal structure, a compound represented by formula (E) can be exemplified.
[0096] Li a Mn 2-b M 14 b O c F d (E)
[0097] Here, M 14 It is made from cobalt <co>,nickel <ni>,magnesium <mg>,aluminum <al>,boron ,titanium <ti>,vanadium <v>,chromium <cr>,iron <fe>,copper <cu>, zinc <zn>,molybdenum ,tin <sn>,calcium <ca>,strontium <sr>and tungsten <w>At least one element selected from the group consisting of a, b, c, d has values that satisfy:
[0098] 0.9≤a≤1.1
[0099] 0≤b≤0.6
[0100] 3.7≤c≤4.1
[0101] 0≤d≤0.1.
[0102] However, the composition differs depending on the charge and discharge state, and a is a value in a completely discharged state. As a lithium-containing composite oxide having a spinel crystal structure, specifically, LiMn 2 O 4 can be exemplified.
[0103] Furthermore, as the lithium-containing phosphate compound having an olivine-type crystal structure, a compound represented by formula (F) can be exemplified.
[0104] Li a M 15 PO4 (F)
[0105] Here, M 15 It is made from cobalt <co>,manganese ,iron <fe>,nickel <ni>,magnesium <mg>,aluminum <al>,boron ,titanium <ti>,vanadium <v>,niobium <nb>,copper <cu>, zinc <zn>,molybdenum ,calcium <ca>,strontium <sr>, Tungsten <w>Zirconium <zr>At least one element selected from the group consisting of a, the value of a satisfies:
[0106] 0.9≤a≤1.1.
[0107] However, the composition varies depending on the charge and discharge state, and a is a value in a fully discharged state. As lithium-containing phosphate compounds having an olivine-type crystal structure, specifically, LiFePO4, LiMnPO4, LiFe 0.5 Mn 0.5 PO4、LiFe 0.3 Mn 0.7 PO4.
[0108] Alternatively, as the lithium-containing composite oxide, a compound represented by the formula (G) can be exemplified.
[0109] (Li2MnO3) x (LiMnO2) 1-x (G)
[0110] Here, the value of x satisfies:
[0111] 0≤x≤1.
[0112] However, the composition differs depending on the charge and discharge state, and x is a value in the fully discharged state.
[0113] The positive electrode may contain, in addition to the above, oxides such as titanium oxide, vanadium oxide, and manganese dioxide, disulfides such as titanium disulfide and molybdenum sulfide, chalcogenides such as niobium selenide, sulfur, and conductive polymers such as polyaniline and polythiophene.
[0114] In the negative electrode component, a negative electrode mixture layer is formed on both sides of the negative electrode collector. As the material constituting the negative electrode collector, for example, copper (Cu), aluminum (Al), nickel (Ni), magnesium (Mg), titanium (Ti), iron (Fe), cobalt (Co), zinc (Zn), germanium (Ge), indium (In), gold (Au), platinum (Pt), silver (Ag), palladium (Pd), etc., or conductive materials such as alloys containing any of them, stainless steel, etc. can be exemplified. From the viewpoint of improving the adhesion of the negative electrode mixture layer to the negative electrode collector based on the so-called anchoring effect, it is preferred to roughen the surface of the negative electrode collector. In this case, at least the surface of the region of the negative electrode collector where the negative electrode mixture layer should be formed is roughened. As a roughening method, for example, a method of forming fine particles by electrolytic treatment can be cited. Electrolytic treatment is a method of providing concave and convex surfaces on the surface of the negative electrode collector by forming fine particles on the surface of the negative electrode collector by electrolysis in an electrolytic cell. Alternatively, the negative electrode component may be a structure composed of lithium foil, lithium sheet, or lithium plate. The negative electrode mixture layer contains a negative electrode material that can absorb / release lithium as a negative electrode active material. The negative electrode mixture layer may also contain a negative electrode binder, a negative electrode conductive agent, etc. The negative electrode binder and the negative electrode conductive agent may be the same as the positive electrode binder and the positive electrode conductive agent.
[0115] As a material constituting the negative electrode active material, for example, a carbon material can be cited. Since the change in the crystal structure of the carbon material when absorbing / releasing lithium is very small, a high energy density can be stably obtained. In addition, since the carbon material functions as a negative electrode conductive agent, the conductivity of the negative electrode mixture is improved. As a carbon material, for example, graphitizable carbon (soft carbon), difficult graphitizable carbon (hard carbon), black lead (graphite) and highly crystalline carbon materials with developed crystal structures can be cited. However, the interplanar spacing of the (002) plane in the difficult graphitizable carbon is preferably 0.37nm or more, and the interplanar spacing of the (002) plane in the graphite is preferably 0.34nm or less. More specifically, as a carbon material, for example, pyrolytic carbon, pitch coke, needle coke, coke such as petroleum coke, black lead, glassy carbon fiber, organic polymer compound sintered body that can be obtained by calcining (carbonizing) phenolic resin, furan resin and other polymer compounds at an appropriate temperature, carbon fiber, activated carbon, carbon black, polymers such as polyacetylene, etc. can be cited. In addition, as the carbon material, other examples include low-crystalline carbon heat-treated at a temperature of about 1000° C. or lower, and amorphous carbon may also be used. The shape of the carbon material may be any of fibrous, spherical, granular, and scaly.
[0116] Alternatively, as materials constituting the negative electrode active material, for example, materials containing one or more of metal elements and semi-metal elements as constituent elements (hereinafter referred to as "metal-based materials") can be cited, thereby enabling high energy density to be obtained. The metal-based material may be any of a simple substance, an alloy, and a compound, or a material composed of two or more of the above, or a material having one or more of the above phases in at least one part. In addition to materials composed of two or more metal elements, alloys also include materials containing one or more metal elements and one or more semi-metal elements. In addition, alloys may also contain non-metallic elements. As the structure of the metal-based material, for example, a solid solution, a eutectic (eutectic mixture), an intermetallic compound, and coexistence of two or more of them can be cited.
[0117] As metal elements and semi-metal elements, for example, metal elements and semi-metal elements that can form alloys with lithium can be cited. Specifically, for example, magnesium (Mg), boron (B), aluminum (Al), gallium (Ga), indium (In), silicon (Si), germanium (Ge), tin (Sn), lead (Pb), antimony (Sb), bismuth (Bi), cadmium (Cd), silver (Ag), zinc (Zn), hafnium (Hf), zirconium (Zr), yttrium (Y), palladium (Pd), platinum (Pt) can be exemplified, but among them, silicon (Si) and tin (Sn) have excellent ability to absorb / release lithium, and from the viewpoint of significantly obtaining high energy density, silicon (Si) and tin (Sn) are preferred.
[0118] As materials containing silicon as a constituent element, simple substance of silicon, silicon alloys, and silicon compounds can be cited, and materials consisting of two or more of the above can also be materials having one or more of the above phases in at least one part. As materials containing tin as a constituent element, simple substance of tin, tin alloys, and tin compounds can be cited, and materials consisting of two or more of the above can also be materials having one or more of the above phases in at least one part. Simple substance is a simple substance in the usual sense, which can contain a small amount of impurities and does not necessarily mean that the purity is 100%.
[0119] Elements other than silicon that constitute silicon alloys or silicon compounds include tin (Sn), nickel (Ni), copper (Cu), iron (Fe), cobalt (Co), manganese (Mn), zinc (Zn), indium (In), silver (Ag), titanium (Ti), germanium (Ge), bismuth (Bi), antimony (Sb), and chromium (Cr); carbon (C) and oxygen (O) may also be mentioned.
[0120] As silicon alloys or silicon compounds, specifically, SiB4, SiB6, Mg2Si, Ni2Si, TiSi2, MoSi2, CoSi2, NiSi2, CaSi2, CrSi2, Cu5Si, FeSi2, MnSi2, NbSi2, TaSi2, VSi2, WSi2, ZnSi2, SiC, Si3N4, Si2N2O, SiO v (0<v≤2, preferably 0.2<v<1.4), LiSiO.
[0121] Examples of elements other than tin that constitute the tin alloy or tin compound include silicon (Si), nickel (Ni), copper (Cu), iron (Fe), cobalt (Co), manganese (Mn), zinc (Zn), indium (In), silver (Ag), titanium (Ti), germanium (Ge), bismuth (Bi), antimony (Sb), and chromium (Cr). Examples of carbon (C) and oxygen (O) include tin alloys or tin compounds. Specifically, SnO w (0<w≤2), SnSiO3, LiSnO, Mg2Sn. In particular, the material containing tin as a constituent element is preferably a material containing tin (first constituent element), a second constituent element and a third constituent element (hereinafter referred to as "Sn-containing material"). As the second constituent element, for example, cobalt (Co), iron (Fe), magnesium (Mg), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), nickel (Ni), copper (Cu), zinc (Zn), gallium (Ga), zirconium (Zr), niobium (Nb), molybdenum (Mo), silver (Ag), indium (In), cesium (Ce), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silicon (Si), and as the third constituent element, for example, boron (B), carbon (C), aluminum (Al), phosphorus (P) can be mentioned. If the Sn-containing material contains the second constituent element and the third constituent element, high battery capacity and excellent cycle characteristics can be obtained.
[0122] Among them, the Sn-containing material is preferably a material containing tin (Sn), cobalt (Co) and carbon (C) as constituent elements (referred to as "SnCoC-containing material"). In the SnCoC-containing material, for example, the carbon content is 9.9 mass % to 29.7 mass %, and the content ratio of tin and cobalt {Co / (Sn+Co)} is 20 mass % to 70 mass %. This is because a high energy density can be obtained. The SnCoC-containing material has a phase including tin, cobalt and carbon, and the phase is preferably a low crystalline or amorphous phase. Since the phase is a reaction phase capable of reacting with lithium, excellent properties are obtained by the presence of the reaction phase. When CuKα rays are used as specific X-rays and the scanning speed is set to 1 degree / minute, the half-peak width (diffraction angle 2θ) of the diffraction peak obtained by X-ray diffraction of the reaction phase is more than 1 degree. This is because lithium is more smoothly absorbed / released and the reactivity with the non-aqueous electrolyte is reduced. The SnCoC-containing material may have a phase including a single substance or a part of each constituent element in addition to the low crystalline or amorphous phase.
[0123] If the X-ray diffraction patterns before and after the electrochemical reaction with lithium are compared, it is possible to easily determine whether the diffraction peaks obtained by X-ray diffraction correspond to reaction phases capable of reacting with lithium. For example, if the position of the diffraction peaks before and after the electrochemical reaction with lithium changes, the corresponding reaction phases are capable of reacting with lithium. In this case, for example, the diffraction peaks of low crystallinity or amorphous reaction phases appear in the range of 2θ=20 degrees to 50 degrees. It can be considered that such reaction phases, for example, include the above-mentioned constituent elements, which are low crystallized or amorphized mainly due to the presence of carbon.
[0124] In the SnCoC-containing material, at least a portion of the carbon as a constituent element is preferably combined with a metal element or a semi-metal element. This is because the aggregation and crystallization of tin and the like are suppressed. Regarding the bonding state of the elements, for example, X-ray photoelectron spectroscopy (XPS) using Al-Kα rays or Mg-Kα rays as a soft X-ray source can be used for confirmation. In the case where at least a portion of the carbon is combined with a metal element or a semi-metal element, the peak of the synthetic wave on the 1s orbital (C1s) of carbon appears in a region below 284.5 eV. In addition, energy calibration is performed so that the peak of the 4f orbital (Au4f) of the gold atom is obtained at 84.0 eV. At this time, usually, surface contamination carbon exists on the surface of the material, so the peak of C1s of the surface contamination carbon is set to 284.8 eV, and the peak is set as the energy standard. In the XPS measurement, the waveform of the peak of C1s is obtained in the form of a peak including the peak of the surface contamination carbon and the peak of the carbon in the SnCoC-containing material. Therefore, for example, the two peaks may be separated from each other by performing analysis using commercially available software. In the waveform analysis, the position of the main peak existing on the lowest binding energy side is set as the energy standard (284.8 eV).
[0125] The SnCoC-containing material is not limited to the material (SnCoC) whose constituent elements are only tin, cobalt and carbon. For example, in addition to tin, cobalt and carbon, the SnCoC-containing material may also contain any one or two or more of silicon (Si), iron (Fe), nickel (Ni), chromium (Cr), indium (In), niobium (Nb), germanium (Ge), titanium (Ti), molybdenum (Mo), aluminum (Al), phosphorus (P), gallium (Ga), bismuth (Bi) and the like as constituent elements.
[0126] In addition to SnCoC-containing materials, materials containing tin, cobalt, iron and carbon as constituent elements (hereinafter referred to as "SnCoFeC-containing materials") are also preferred materials. The composition of SnCoFeC-containing materials is arbitrary. As an example, when the iron content is set to be small, the carbon content is 9.9 mass % to 29.7 mass %, the iron content is 0.3 mass % to 5.9 mass %, and the content ratio of tin and cobalt {Co / (Sn+Co)} is 30 mass % to 70 mass %. In addition, when the iron content is set to be large, the carbon content is 11.9 mass % to 29.7 mass %, the content ratio of tin, cobalt and iron {(Co+Fe) / (Sn+Co+Fe)} is 26.4 mass % to 48.5 mass %, and the content ratio of cobalt and iron {Co / (Co+Fe)} is 9.9 mass % to 79.5 mass %. This is because high energy density can be obtained within such a composition range. The physical properties (half peak width, etc.) of the SnCoFeC-containing material are the same as those of the above-mentioned SnCoC-containing material.
[0127] Alternatively, other than these, examples of the material constituting the negative electrode active material include metal oxides such as iron oxide, ruthenium oxide, and molybdenum oxide, and polymer compounds such as polyacetylene, polyaniline, and polypyrrole.
[0128] Among them, the material constituting the negative electrode active material preferably includes both carbon materials and metal-based materials for the following reasons. That is, metal-based materials, especially materials containing at least one of silicon and tin as constituent elements, have the advantage of high theoretical capacity, but are prone to severe expansion / contraction during charging and discharging. On the other hand, carbon materials have low theoretical capacity, but have the advantage of not being easy to expand / contract during charging and discharging. Thus, by using both carbon materials and metal-based materials, while obtaining a high theoretical capacity (in other words, battery capacity), expansion / contraction during charging and discharging is suppressed.
[0129] The positive electrode mixture layer and the negative electrode mixture layer can be formed based on a coating method, for example. That is, it can be formed based on a method of mixing a positive electrode active material or a negative electrode active material in a particle (powder) form with a positive electrode binder, a negative electrode binder, etc., and then dispersing the mixture in a solvent such as an organic solvent, and coating it on a positive electrode collector and a negative electrode collector (for example, a coating method using a coating device provided with the aforementioned mold and back roll). However, the coating method is not limited to this method, and further, it is not limited to the coating method. For example, a negative electrode component can be obtained by molding a negative electrode active material, and a positive electrode component can also be obtained by molding a positive electrode active material. Molding, for example, only requires the use of a press. Alternatively, it can be formed based on a gas phase method, a liquid phase method, a spraying method, or a calcination method (sintering method). The gas phase method is a PVD method (physical vapor deposition method) such as a vacuum vapor deposition method, a sputtering method, an ion plating method, and a laser ablation method, and various CVD methods (chemical vapor deposition methods) including a plasma CVD method. As liquid phase methods, electrolytic plating and electroless plating methods can be cited. Spraying is a method of spraying a positive electrode active material or a negative electrode active material in a molten state or a semi-molten state onto a positive electrode collector or a negative electrode collector. The calcination method is, for example, a method of applying a mixture dispersed in a solvent onto a negative electrode collector by a coating method, and then heat treating it at a temperature higher than the melting point of the negative electrode binder, etc. Atmosphere calcination methods can include reaction calcination and hot press calcination.
[0130] As positive electrode binders and negative electrode binders, specifically, styrene-butadiene rubbers such as styrene-butadiene rubber (SBR), fluorine rubbers, synthetic rubbers such as ethylene propylene diene; fluorine resins such as polyvinylidene fluoride (PVdF), polyvinyl fluoride, polyimide, polytetrafluoroethylene (PTFE), ethylene-tetrafluoroethylene copolymer (ETFE), copolymers and modified products of these fluorine resins; polyolefin resins such as polyethylene and polypropylene; acrylic resins such as polyacrylonitrile (PAN) and polyacrylate; polymer materials such as carboxymethyl cellulose (CMC), etc., and at least one selected from copolymers based on these resin materials can also be exemplified. As copolymers of polyvinylidene fluoride, more specifically, for example, polyvinylidene fluoride-hexafluoropropylene copolymers, polyvinylidene fluoride-tetrafluoroethylene copolymers, polyvinylidene fluoride-chlorotrifluoroethylene copolymers, polyvinylidene fluoride-hexafluoropropylene-tetrafluoroethylene copolymers can be listed. In addition, conductive polymers can also be used as positive electrode binders and negative electrode binders. As the conductive polymer, for example, substituted or unsubstituted polyaniline, polypyrrole, polythiophene, and (co)polymers composed of one or two selected from these can be used.
[0131] As the positive electrode conductive agent and the negative electrode conductive agent, for example, carbon materials such as graphite, carbon fiber, carbon black, carbon nanotubes, graphite, vapor growth carbon fiber (Vapor Growth Carbon Fiber: VGCF), acetylene black (AB), Ketjen black (KB) can be cited, and one or more of them can be mixed and used. As carbon nanotubes, for example, multi-walled carbon nanotubes (MWCNT) such as single-walled carbon nanotubes (SWCNT) and double-walled carbon nanotubes (DWCNT) can be cited. In addition, as long as it is a conductive material, a metal material or a conductive polymer material can also be used.
[0132] In order to prevent lithium from being accidentally deposited on the negative electrode component during charging, it is preferred that the chargeable capacity of the negative electrode material is greater than the discharge capacity of the positive electrode material. That is, the electrochemical equivalent of the negative electrode material capable of occluding and releasing lithium is greater than the electrochemical equivalent of the positive electrode material. In addition, the lithium deposited on the negative electrode component is lithium metal, for example, when the electrode reaction material is lithium.
[0133] The positive lead portion can be installed on the positive electrode collector based on spot welding or ultrasonic welding. It is desirable that the positive lead portion is a metal foil or a mesh, but as long as it is electrochemically and chemically stable and conductivity is obtained, the positive lead portion may not be a metal. As the material of the positive lead portion, for example, aluminum (Al) can be cited. Nickel (Ni) and the like. The negative lead portion can be installed on the negative electrode collector based on spot welding or ultrasonic welding. It is desirable that the negative lead portion is a metal foil or a mesh, but as long as it is electrochemically and chemically stable and conductivity is obtained, the negative lead portion may not be a metal. As the material of the negative lead portion, for example, copper (Cu), nickel (Ni) and the like can be cited. The positive lead portion and the negative lead portion can also be composed of a protrusion protruding from the positive collector and the negative collector as a part of the positive collector and the negative collector.
[0134] The diaphragm separates the positive electrode component from the negative electrode component and allows lithium ions to pass through while preventing current short circuit caused by contact between the positive electrode component and the negative electrode component. The diaphragm includes, for example, a porous membrane formed of a synthetic resin, such as a polyolefin resin (polypropylene resin, polyethylene resin), a polyimide resin, a polytetrafluoroethylene resin, a polyvinylidene fluoride resin, a polyphenylene sulfide resin, and an aromatic polyamide; a porous membrane such as ceramics; glass fibers (for example, including glass filters); non-woven fabrics formed of liquid crystal polyester fibers, aromatic polyamide fibers, and cellulose fibers, ceramic non-woven fabrics, etc., among which porous membranes of polypropylene and polyethylene are preferred. Alternatively, the diaphragm can also be composed of a laminated film laminated with two or more porous membranes, and can also be a diaphragm coated with an inorganic layer, or a diaphragm containing an inorganic substance. Among them, the porous membrane composed of a polyolefin resin has an excellent anti-short circuit effect, and can achieve an improved safety of the battery based on the circuit-breaking effect, so it is preferred. Polyethylene resin can obtain a circuit-breaking effect within a range of 100°C to 160°C, and has excellent electrochemical stability, so it is particularly preferred as a material constituting the diaphragm. In addition, chemically stable resins can use materials copolymerized or blended with polyethylene or polypropylene. Alternatively, the porous membrane may have a structure of three or more layers, for example, in which a polypropylene resin layer, a polyethylene resin layer, and a polypropylene resin layer are laminated in sequence. The thickness of the diaphragm is preferably 5 μm to 50 μm, more preferably 7 μm to 30 μm. If the diaphragm is too thick, the filling amount of the active material is reduced, the battery capacity is reduced, and the ionic conductivity is reduced, and the current characteristics are reduced. If the diaphragm is too thin on the contrary, the mechanical strength of the diaphragm is reduced.
[0135] In addition, the diaphragm may also have a structure in which a resin layer is provided on one or both sides of a porous film as a substrate. As a resin layer, a porous matrix resin layer carrying an inorganic substance can be cited. By adopting this structure, oxidation resistance can be obtained, thereby suppressing the degradation of the diaphragm. As a material constituting the matrix resin layer, for example, polyvinylidene fluoride (PVdF), hexafluoropropylene (HFP), polytetrafluoroethylene (PTFE) can be cited, and in addition, their copolymers can also be used. As an inorganic substance, a metal, a semiconductor or their oxides, nitrides can be cited. For example, aluminum (Al), titanium (Ti) etc. can be cited as a metal, and silicon (Si), boron (B) etc. can be cited as a semiconductor. In addition, the inorganic substance is actually preferably a substance without conductivity and a large heat capacity. If the heat capacity is large, it is useful as a heat sink when the current generates heat, and the thermal runaway of the battery can be more effectively suppressed. As such inorganic substances, oxides or nitrides such as aluminum oxide (Al2O3), boehmite (monohydrate of aluminum oxide), talc, boron nitride (BN), aluminum nitride (AlN), titanium dioxide (TiO2), and silicon oxide can be cited. As the particle size of the inorganic substance, 1nm to 10μm can be cited. If it is smaller than 1nm, it is difficult to obtain, and even if it can be obtained, it is not suitable in terms of cost. If it is larger than 10μm, the distance between the electrodes becomes larger, and the active material filling amount cannot be fully obtained in a limited space, and the battery capacity becomes lower. The inorganic substance can also be contained in a porous film as a substrate. The resin layer can be obtained, for example, by applying a slurry composed of a matrix resin, a solvent and an inorganic substance on a substrate (porous membrane), and passing through a poor solvent for the matrix resin and a good solvent bath for the solvent to separate the phases, and then drying it.
[0136] As the puncture strength of the diaphragm, 100gf to 1kgf can be cited, preferably 100gf to 480gf. If the puncture strength is low, there is a concern about short circuit, and if the puncture strength is high, there is a concern about decreased ion conductivity. As the air permeability of the diaphragm, 30 seconds / 100cc to 1000 seconds / 100cc can be cited, preferably 30 seconds / 100cc to 680 seconds / 100cc. If the air permeability is too low, there is a concern about short circuit, and if the air permeability is too high, there is a concern about decreased ion conductivity.
[0137] Examples of lithium salts that constitute a non-aqueous electrolyte suitable for use in a lithium ion secondary battery include LiPF6, LiClO4, LiBF4, LiAsF6, LiSbF6, LiTaF6, LiNbF6, LiSiF6, LiAlCl4, LiCF3SO3, LiCH3SO3, LiN(CF3SO2)2, LiC(CF3SO2)3, LiC4F9SO3, Li(FSO2)2N, Li(CF3SO2)2N, Li(C2F5SO2)2N, Li(CF3SO2)3C, LiBF3(C2F5), LiB(C2O4)2, LiB(C6F5)4, LiPF3(C2F5)3, 1 / 2Li2B 12 F 12 , Li2SiF6, LiCl, LiBr, LiI, lithium difluoro[oxalate-O,O']borate, lithium bis(oxalatoborate), but are not limited thereto.
[0138] In addition, as organic solvent, cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) can be used, preferably one side of ethylene carbonate and propylene carbonate, or further preferably both are mixed and used, thus, the improvement of cycle characteristics can be achieved. In addition, as solvent, from the viewpoint of obtaining high ion conductivity, chain carbonates such as above-mentioned cyclic carbonates, diethyl carbonate, dimethyl carbonate, ethyl methyl carbonate or methyl propyl carbonate can also be mixed and used. Alternatively, 2,4-difluoroanisole, vinylene carbonate can also be contained in the solvent. 2,4-difluoroanisole can improve discharge capacity, and in addition, vinylene carbonate can improve cycle characteristics. Thus, if they are mixed and used, discharge capacity and cycle characteristics can be improved, so it is preferred.
[0139] Alternatively, examples of the organic solvent include chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (PMC), ethyl propyl carbonate (PEC), and fluoroethylene carbonate (FEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyltetrahydrofuran (2-MeTHF), 1,3-dioxolane (DOL), and 4-methyl-1,3-dioxolane (4-MeDOL); chain ethers such as 1,2-dimethoxyethane (DME) and 1,2-diethoxyethane (DEE); cyclic esters such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain esters such as methyl acetate, ethyl acetate, propyl acetate, methyl formate, ethyl formate, propyl formate, methyl butyrate, methyl propionate, ethyl propionate, and propyl propionate. Alternatively, as an organic solvent, tetrahydropyran, 1,3 dioxane, 1,4 dioxane, N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMA), N-methylpyrrolidone (NMP), N-methyloxazolidinone (NMO), N,N'-dimethylimidazolidinone (DMI), dimethyl sulfoxide (DMSO), trimethyl phosphate (TMP), nitromethane (NM), nitroethane (NE), sulfolane (SL), methyl sulfolane, acetonitrile (AN), anisole, propionitrile, glutaronitrile (GLN), adiponitrile (ADN), methoxyacetonitrile (MAN), 3-methoxypropionitrile (MPN), diethyl ether, butylene carbonate, 3-methoxypropionitrile, N,N-dimethylformamide, dimethyl sulfoxide, trimethyl phosphate. Alternatively, an ionic liquid can also be used. As an ionic liquid, a known ionic liquid can be used, and it can be selected as needed.
[0140] The electrolyte layer can also be formed by a non-aqueous electrolyte and a retaining polymer compound. The non-aqueous electrolyte is retained by a retaining polymer compound, for example. The electrolyte layer in this manner is a gel electrolyte or a solid electrolyte, which obtains a high ion conductivity (for example, more than 1 mS / cm at room temperature) and prevents leakage of the non-aqueous electrolyte. The electrolyte can be a liquid electrolyte, or a gel electrolyte or a solid electrolyte. In the gel electrolyte, since a vacuum injection process of the electrolyte is not required and a continuous coating process can be used, it is excellent in productivity when manufacturing large-area lithium-ion batteries.
[0141] As the polymer compound for maintenance, specifically, polyacrylonitrile, polyvinylidene fluoride, polytetrafluoroethylene, polyhexafluoropropylene, polyethylene oxide, polypropylene oxide, polyphosphazene, polysiloxane, polyvinyl fluoride (PVF), polychlorotrifluoroethylene (PCTFE), perfluoroalkoxy fluororesin (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), ethylene-tetrafluoroethylene copolymer (ETFE), ethylene-chlorotrifluoroethylene copolymer (ECTFE), polyvinyl acetate, polyvinyl alcohol, polymethyl methacrylate, polyacrylic acid, polymethacrylic acid, styrene-butadiene rubber, nitrile-butadiene rubber, polystyrene, polycarbonate, polyethylene oxide, vinyl chloride can be illustrated.They can be used independently or in combination.In addition, the polymer compound for maintenance can also be a copolymer.As a copolymer, specifically, polyvinylidene fluoride-hexafluoropropylene copolymer etc. can be illustrated, but wherein, from the viewpoint of electrochemical stability, polyvinylidene fluoride is preferably used as a homopolymer, and polyvinylidene fluoride-hexafluoropropylene copolymer is preferably used as a copolymer. In addition, as a filler, a highly heat-resistant compound such as Al2O3, SiO2, TiO2, BN (boron nitride), etc. may be contained.
[0142] Hereinafter, a lithium ion secondary battery composed of a cylindrical lithium ion secondary battery will be described. Figure 5 A schematic cross-sectional view of a cylindrical lithium-ion secondary battery is shown. Figure 6 A schematic partial cross-sectional view of an electrode structure constituting a lithium-ion secondary battery along the longitudinal direction is shown. Here, Figure 6 This is a schematic partial cross-sectional view of a portion where the positive electrode lead portion and the negative electrode lead portion are not provided. In order to simplify the drawing, the electrode structure is shown flat, but in reality, the electrode structure is wound and therefore curved.
[0143] In the lithium ion secondary battery, an electrode structure 111 and a pair of insulating plates 102 and 103 are housed in a substantially hollow cylindrical electrode structure housing 101. The electrode structure 111 can be produced, for example, by laminating a positive electrode member 112 and a negative electrode member 114 with a separator 116 interposed therebetween to obtain an electrode structure, and then winding the electrode structure.
[0144] The electrode structure storage component (battery can) 101 has a hollow structure with one end closed and the other end open, and is made of iron (Fe), aluminum (Al), etc. The surface of the electrode structure storage component 101 may also be plated with nickel (Ni), etc. A pair of insulating plates 102 and 103 are arranged to sandwich the electrode structure 111 and extend perpendicularly to the winding circumference of the electrode structure 111. The battery cover 104, the safety valve mechanism 105 and the thermistor element (PTC element, Positive Temperature Coefficient element) 106 are riveted to the open end of the electrode structure storage component 101 via a gasket 107, thereby sealing the electrode structure storage component 101. The battery cover 104 is made of the same material as the electrode structure storage component 101, for example. The safety valve mechanism 105 and the thermistor element 106 are arranged on the inner side of the battery cover 104, and the safety valve mechanism 105 is electrically connected to the battery cover 104 via the thermistor element 106. In the safety valve mechanism 105, when the internal pressure exceeds a certain level due to an internal short circuit, heating from the outside, etc., the disc 105A turns over. As a result, the electrical connection between the battery cover 104 and the electrode structure 111 is cut off. In order to prevent abnormal heating caused by a large current, the resistance of the thermistor element 106 increases as the temperature rises. The gasket 107 is made of an insulating material, for example. Asphalt or the like may also be applied to the surface of the gasket 107.
[0145] A center pin 108 is inserted into the winding center of the electrode structure 111. However, the center pin 108 does not have to be inserted into the winding center. A positive lead portion 113 made of a conductive material such as aluminum is connected to the positive electrode component 112. Specifically, the positive lead portion 113 is mounted on the positive electrode collector 112A. A negative lead portion 115 made of a conductive material such as copper is connected to the negative electrode component 114. Specifically, the negative lead portion 115 is mounted on the negative electrode collector 114A. The negative lead portion 115 is welded to the electrode structure housing component 101 and is electrically connected to the electrode structure housing component 101. The positive lead portion 113 is welded to the safety valve mechanism 105 and is electrically connected to the battery cover 104. In addition, in Figure 5 In the example shown, the negative electrode lead portion 115 is provided at one location (the outermost peripheral portion of the wound electrode structure), but may be provided at two locations (the outermost peripheral portion and the innermost peripheral portion of the wound electrode structure).
[0146] The electrode structure 111 is formed by laminating a positive electrode member 112 having a positive electrode material layer 112B formed on a positive electrode current collector 112A and a negative electrode member 114 having a negative electrode mixture layer 114B formed on a negative electrode current collector 114A via a separator 116. The positive electrode mixture layer 112B is not formed in a region of the positive electrode current collector 112A to which the positive electrode lead portion 113 is attached, and the negative electrode mixture layer 114B is not formed in a region of the negative electrode current collector 114A to which the negative electrode lead portion 115 is attached.
[0147] The specifications of the lithium ion secondary battery are exemplified in the following table.
[0148]
[0149]
[0150] The positive electrode component 112 can be made based on the following method. That is, first, lithium carbonate (Li2CO3) and cobalt carbonate (CoCO3) are mixed, and then the mixture is fired in air (900°C × 5 hours) to obtain a lithium-containing composite oxide (LiCoO2). In this case, the mixing ratio is set to, for example, Li2CO3:CoO3=0.5:1 in terms of molar ratio. Furthermore, 91 parts by mass of the positive electrode active material (Li x CoO2), 3 parts by mass of a positive electrode binder (polyvinylidene fluoride) and 6 parts by mass of a positive electrode conductor (black lead, graphite) are mixed to obtain a positive electrode mixture. Furthermore, the positive electrode mixture is mixed with an organic solvent (N-methyl-2-pyrrolidone) to obtain a paste-like positive electrode mixture slurry. Next, a coating device is used to apply the positive electrode mixture slurry to both sides of a strip-shaped positive electrode collector 112A (equivalent to a substrate, composed of an aluminum foil with a thickness of 20 μm), and then the positive electrode mixture slurry is dried to form the laminated structure described in Examples 1 to 3 (positive electrode mixture layer 112B). Next, the first layer and the second layer (positive electrode mixture layer 112B) of the laminated structure are punched (pressurized, compressed) using the method described in Examples 1 to 3 and the roller press described in Examples 1 to 3.
[0151] When preparing the negative electrode component 114, first, 97 parts by mass of the negative electrode active material (graphite or a mixed material of graphite and silicon) and 3 parts by mass of the negative electrode binder (polyvinylidene fluoride) are mixed to obtain a negative electrode mixture. 50 is set to 20 μm. Alternatively, as a negative electrode binder, for example, a mixture of 1.5 parts by mass of an acrylic modified form of a styrene-butadiene copolymer and 1.5 parts by mass of carboxymethyl cellulose is used. Then, the negative electrode mixture is mixed with an organic solvent (N-methyl-2-pyrrolidone) to obtain a paste-like negative electrode mixture slurry. Then, the electrode mixture slurry is applied to both sides of a strip-shaped negative electrode collector 114A using a coating device, and then the negative electrode mixture slurry is dried to form a negative electrode material layer 114B. Furthermore, the negative electrode material layer 114B is punched (pressurized, compressed) using a roller press.
[0152] The separator 116 is composed of a microporous polyethylene film having a thickness of 20 μm. In addition, a non-aqueous electrolyte having a composition shown in the following table is impregnated into the electrode structure 111. In addition, the solvent of the non-aqueous electrolyte is a broad concept that includes not only liquid materials but also materials having ion conductivity that can dissociate electrolyte salts. Therefore, in the case of using a polymer compound having ion conductivity, the polymer compound is also included in the solvent.
[0153]
[0154] Alternatively, in the case of preparing a non-aqueous electrolyte, the first compound, the second compound, the third compound, and other materials are mixed and stirred. As the first compound, lithium bis(fluorosulfonyl)imide (LiFSI) or lithium bis(trifluoromethyl)sulfonyl)imide (LiTFSI) is used. In addition, as the second compound, acetonitrile (AN), propionitrile (PN) or butyronitrile (BN) as a non-oxygen-containing mononitrile compound or methoxyacetonitrile (MAN) as an oxygen-containing mononitrile compound are used. Further, as the third compound, vinylene carbonate (VC), vinyl ethylene carbonate (VEC or methylene ethylene carbonate (MEC) as an unsaturated cyclic carbonate are used, or as 4-fluoro-1,3-dioxolane-2-one (FEC) or carbonate bis(fluoromethyl) ester) (DFDMC) as a halogenated carbonate, or as succinonitrile (SN) as a polynitrile compound. Furthermore, as other materials, ethylene carbonate (EC) as a cyclic ester carbonate, dimethyl carbonate (DMC) as a chain carbonate, lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4) as electrolyte salts are used. However, the electrolyte solution is not limited to the above composition.
[0155] The lithium ion secondary battery can be manufactured, for example, according to the following process.
[0156] First, as described above, the positive electrode material layer 112B is formed on the positive electrode current collector 112A, and the negative electrode material layer 114B is formed on the negative electrode current collector 114A.
[0157] Thereafter, the positive electrode lead portion 113 is attached to the positive electrode collector 112A by welding or the like. Also, the negative electrode lead portion 115 is attached to the negative electrode collector 114A by welding or the like. Next, the positive electrode component 112 and the negative electrode component 114 are laminated and wound with a separator 116 made of a microporous polyethylene film having a thickness of 20 μm therebetween (more specifically, an electrode structure of the positive electrode component 112 / separator 116 / negative electrode component 114 / separator 116 is wound), to prepare the electrode structure 111, and then a protective tape (not shown) is attached to the outermost periphery. Thereafter, the center pin 108 is inserted into the center of the electrode structure 111. Next, the electrode structure 111 is housed inside the electrode structure housing component (battery can) 101 while being sandwiched between a pair of insulating plates 102 and 103. In this case, the front end of the positive electrode lead 113 is attached to the safety valve mechanism 105 by welding or the like, and the front end of the negative electrode lead 115 is attached to the electrode structure housing member 101. Thereafter, an organic electrolyte or a non-aqueous electrolyte is injected under reduced pressure to allow the organic electrolyte or the non-aqueous electrolyte to permeate the separator 116. Next, the battery cover 104, the safety valve mechanism 105, and the thermistor element 106 are riveted to the open end of the electrode structure housing member 101 via the gasket 107.
[0158] Hereinafter, a lithium ion secondary battery composed of a laminated lithium ion secondary battery will be described. The lithium ion secondary battery is composed of a flat-plate laminated film type lithium ion secondary battery in which a positive electrode member, a separator, and a negative electrode member are wound. Figure 7 and Fig. 8A A schematic exploded perspective view of a secondary battery is shown, Figure 8B Show Figure 7 and Fig. 8A The electrode structure shown is a schematic enlarged cross-sectional view along the arrow AA (a schematic enlarged cross-sectional view along the YZ plane). Figure 8B A schematic partial cross-sectional view (a schematic partial cross-sectional view along the XY plane) of a portion of the electrode structure shown in FIG. Figure 6 Same as shown.
[0159] In this secondary battery, an electrode structure 111 is housed inside an outer casing 120 made of a laminate film. The electrode structure 111 can be manufactured by laminating a positive electrode component 112 and a negative electrode component 114 with a separator 116 and an electrolyte layer 118 interposed therebetween, and then winding the laminated structure. A positive electrode lead 113 is attached to the positive electrode component 112, and a negative electrode lead 115 is attached to the negative electrode component 114. The outermost periphery of the electrode structure 111 is protected by a protective tape 119.
[0160] The positive lead 113 and the negative lead 115 protrude in the same direction from the inside of the outer casing 120 toward the outside. The positive lead 113 is formed of a conductive material such as aluminum. The negative lead 115 is formed of a conductive material such as copper, nickel, stainless steel, etc. These conductive materials are, for example, in the form of a thin plate or a mesh.
[0161] The outer casing 120 is capable of being Figure 7 A film folded in the direction of the arrow R shown, a concave portion (embossing) for accommodating the electrode structure 111 is provided in a part of the outer packaging part 120. The outer packaging part 120 is, for example, a laminated film formed by laminating a fusion layer, a metal layer and a surface protection layer in sequence. In the manufacturing process of the lithium-ion secondary battery, the outer packaging part 120 is folded in a manner that the fusion layers are opposite to each other across the electrode structure 111, and then the peripheral edge portions of the fusion layers are fused to each other. However, the outer packaging part 120 can also be formed by bonding two laminated films together with the aid of an adhesive or the like. The fusion layer is, for example, composed of a film of polyethylene, polypropylene, etc. The metal layer is, for example, composed of aluminum foil, etc. The surface protection layer is, for example, composed of nylon, polyethylene terephthalate, etc. Among them, the outer packaging part 120 is preferably an aluminum laminated film formed by laminating a polyethylene film, an aluminum foil, and a nylon film in sequence. However, the outer packaging part 120 can also be a laminated film having other laminated structures, a polymer film such as polypropylene, or a metal film. Specifically, it is composed of a moisture-resistant aluminum laminate film (total thickness: 100 μm) in which a nylon film (thickness: 30 μm), an aluminum foil (thickness: 40 μm), and an unstretched polypropylene film (thickness: 30 μm) are laminated in this order from the outside.
[0162] In order to prevent the entry of outside air, a sealing film 121 is inserted between the outer casing 120 and the positive electrode lead 113, and between the outer casing 120 and the negative electrode lead 115. The sealing film 121 is made of a material having adhesion to the positive electrode lead 113 and the negative electrode lead 115, for example, a polyolefin resin, more specifically, a polyolefin resin such as polyethylene, polypropylene, modified polyethylene, and modified polypropylene.
[0163] like Figure 8B As shown, the positive electrode member 112 has positive electrode mixture layers 112B on both sides of a positive electrode current collector 112A. In addition, the negative electrode member 114 has negative electrode mixture layers 114B on both sides of a negative electrode current collector 114A.
[0164] The electrolyte layer can also be a structure containing a non-aqueous electrolyte and a holding polymer compound, and the non-aqueous electrolyte is held by the holding polymer compound. This electrolyte layer is a gel electrolyte, which has a high ionic conductivity (for example, 1 mS / cm or more at room temperature) and prevents leakage of the non-aqueous electrolyte. The electrolyte layer may also have other materials such as additives.
[0165] In addition, in the electrolyte layer as a gel-like electrolyte, the solvent of the non-aqueous electrolyte is a broad concept that includes not only liquid materials but also materials with ion conductivity that can dissociate the electrolyte salt. Thus, in the case of using a polymer compound with ion conductivity, the polymer compound is also included in the solvent. It is also possible to directly use a non-aqueous electrolyte instead of a gel-like electrolyte layer. In this case, the non-aqueous electrolyte is impregnated in the electrode structure.
[0166] Specifically, in the case of forming an electrolyte layer, first, a non-aqueous electrolyte is prepared. Then, the non-aqueous electrolyte, a polymer compound for retention, and an organic solvent (dimethyl carbonate) are mixed to prepare a gel precursor solution. As a polymer compound for retention, a copolymer of hexafluoropropylene and vinylidene fluoride (copolymerization amount of hexafluoropropylene = 6.9 mass %) is used. Next, the precursor solution is applied to the positive electrode component and the negative electrode component, and then the precursor solution is dried to form a gel electrolyte layer.
[0167] A lithium ion secondary battery including a gel electrolyte layer can be produced, for example, based on the following three processes.
[0168] In the first process, first, the positive electrode mixture layer 112B is formed on both sides of the positive electrode collector 112A, and the negative electrode mixture layer 114B is formed on both sides of the negative electrode collector 114A. On the other hand, a non-aqueous electrolyte, a polymer compound for retention, and an organic solvent are mixed to prepare a gel precursor solution. Furthermore, the precursor solution is applied to the positive electrode component 112 and the negative electrode component 114, and then the precursor solution is dried to form a gel electrolyte layer. Thereafter, the positive electrode lead part 113 is installed on the positive electrode collector 112A, and the negative electrode lead part 115 is installed on the negative electrode collector 114A by welding or the like. Next, the positive electrode component 112 and the negative electrode component 114 are laminated and wound with a separator 116 composed of a microporous polypropylene film to prepare the electrode structure 111, and then a protective tape 119 is attached to the outermost periphery. After that, the outer casing 120 is folded so as to sandwich the electrode structure 111, and then the outer peripheral edges of the outer casing 120 are joined to each other by heat fusion or the like, so that the electrode structure 111 is sealed inside the outer casing 120. In addition, a sealing film (acid-modified propylene film) 121 is inserted between the positive electrode lead portion 113 and the negative electrode lead portion 115 and the outer casing 120 in advance.
[0169] Alternatively, in the second process, first, the positive electrode component 112 and the negative electrode component 114 are prepared. Then, the positive electrode lead 113 is attached to the positive electrode component 112, and the negative electrode lead 115 is attached to the negative electrode component 114. After that, the positive electrode component 112 and the negative electrode component 114 are laminated and wound with the separator 116 interposed therebetween to prepare a wound body as a precursor of the electrode structure 111, and then a protective tape 119 is attached to the outermost periphery of the wound body. Next, the outer casing 120 is folded so as to sandwich the wound body, and then the outer periphery of the outer casing 120 except for one side is joined by a heat fusion method or the like, and the wound body is stored in the bag-shaped outer casing 120. On the other hand, a non-aqueous electrolyte, a monomer as a raw material of a polymer compound, a polymerization initiator, and other materials such as a polymerization inhibitor added as needed are mixed to prepare an electrolyte composition. Then, the electrolyte composition is injected into the bag-shaped outer casing 120, and then the outer casing 120 is sealed by heat fusion method, etc. Then, the monomer is thermally polymerized to form a polymer compound, thereby forming a gel electrolyte layer.
[0170] Alternatively, in the third process, in addition to using a polymer compound to coat the double-sided separator 116, in the same manner as in the second process, a winding body is prepared and stored in the bag-shaped outer packaging member 120. The polymer compound coated on the separator 116 is, for example, a polymer (homopolymer, copolymer or multi-polymer) with vinylidene fluoride as a component. Specifically, it is polyvinylidene fluoride, a binary copolymer with vinylidene fluoride and hexafluoropropylene as components, a ternary copolymer with vinylidene fluoride, hexafluoropropylene and chlorotrifluoroethylene as components, etc. Polymers with vinylidene fluoride as a component and other one or more polymer compounds can also be used. Afterwards, a non-aqueous electrolyte is prepared to be injected into the interior of the outer packaging member 120, and then the opening of the outer packaging member 120 is sealed using a heat fusion method or the like. Next, while applying a load to the outer packaging member 120, it is heated to make the separator 116 fit closely with the positive electrode member 112 and the negative electrode member 114 with the help of a polymer compound. Thus, the polymer compound is impregnated with the non-aqueous electrolyte solution and the polymer compound is gelled to form an electrolyte layer.
[0171] In the third process, the expansion of the lithium ion secondary battery is suppressed compared to the first process. In addition, in the third process, since the solvent and the monomer as the raw material of the polymer compound are almost not left in the electrolyte layer compared to the second process, the formation process of the polymer compound is well controlled. Therefore, the positive electrode component 112, the negative electrode component 114 and the separator 116 are fully in close contact with the electrolyte layer.
[0172] Alternatively, the negative electrode active material (silicon) and the precursor of the negative electrode binder (polyamic acid) may be mixed to obtain a negative electrode mixture. In this case, the mixing ratio is set to silicon:polyamic acid=80:20 in terms of dry weight ratio. The average particle size of silicon is d 50 The thickness was set to 1 μm. As solvents for polyamic acid, N-methyl-2-pyrrolidone and N,N-dimethylacetamide were used. In addition, after compression molding, the negative electrode mixture slurry was heated in a vacuum atmosphere at 100°C for 12 hours. Thus, polyimide as a negative electrode binder was formed.
[0173] Hereinafter, application examples of the present invention will be described.
[0174] The battery having the above-mentioned electrode (specifically, a lithium-ion secondary battery) can be applied without particular limitation to a lithium-ion secondary battery used in machinery, equipment, instruments, devices, systems (a collection of multiple devices, etc.) that can be used as a power source for driving / action or a storage power source for power storage. The lithium-ion secondary battery used as a power source can be a main power source (a power source used preferentially) or an auxiliary power source (a power source used instead of the main power source or switched from the main power source). When the lithium-ion secondary battery is used as an auxiliary power source, the main power source is not limited to the lithium-ion secondary battery.
[0175] As the uses of lithium ion secondary batteries, specifically, there can be exemplified various electronic devices such as video cameras, camcorders, digital cameras, mobile phones, personal computers, televisions, various display devices, cordless phones, stereo headphones, music players, portable radios, electronic papers such as electronic books and electronic newspapers, portable information terminals including PDAs, electrical equipment (including portable electronic equipment), toys, portable household appliances such as electric shavers, lighting equipment such as room lights, medical electronic equipment such as pacemakers and hearing aids, storage devices such as memory cards, battery packs used as detachable power sources for personal computers, power tools such as electric drills and electric saws, power storage systems such as household battery systems that store electricity for emergency situations, home energy servers (home power storage devices), power supply systems, power storage units, backup power supplies, electric vehicles such as electric cars, electric motorcycles, electric bicycles, Segway (registered trademark), electric driving force conversion devices (specifically, for example, power motors) for electric vehicles, aircraft, and ships, but the uses are not limited to these.
[0176] Among them, the lithium ion secondary battery in the present invention is effectively applied to battery packs, electric vehicles, power storage systems, power supply systems, power tools, electronic equipment, electrical equipment, etc. Since excellent battery characteristics are required, performance improvement can be effectively achieved by using the lithium ion secondary battery in the present invention. The battery pack is a power source using a lithium ion secondary battery, which is a so-called assembled battery, etc. An electric vehicle is a vehicle that uses a lithium ion secondary battery as a driving power source to operate (drive), and can also be a car (hybrid vehicle, etc.) that also has a driving source other than a secondary battery. The power storage system (power supply system) is a system that uses a lithium ion secondary battery as a storage power source. For example, in a household power storage system (power supply system), since electricity is stored in a lithium ion secondary battery as a storage power source, household electrical products, etc. can be used using electricity. Power tools are tools that use lithium ion secondary batteries as a driving power source to move movable parts (such as drill bits, etc.). Electronic equipment and electrical equipment are devices that use lithium ion secondary batteries as working power sources (power supply sources) to perform various functions.
[0177] Hereinafter, several application examples of the lithium ion secondary battery will be described in detail. In addition, the configuration of each application example described below is merely an example, and the configuration can be changed as appropriate.
[0178] A battery pack is a simple battery pack (so-called soft package) using a lithium-ion secondary battery, for example, mounted on an electronic device represented by a smartphone. Or, for example, an assembled battery consisting of six lithium-ion secondary batteries connected in a manner of 2 parallel and 3 series. In addition, the connection form of the lithium-ion secondary battery can be series, parallel, or a hybrid of the two.
[0179] Fig. 9 A schematic stereogram showing a battery pack using a single cell is shown. The battery pack is a simple battery pack (so-called soft package) using a single lithium-ion secondary battery, and is mounted on electronic devices such as smartphones. The battery pack includes, for example, a power supply 131 composed of the lithium-ion secondary battery described in Example 5, and a circuit substrate 133 connected to the power supply 131. A positive lead portion 113 and a negative lead portion 115 are installed on the power supply 131.
[0180] A pair of adhesive tapes 135 are attached to both sides of the power supply 131. A protection circuit (PCM: Protection Circuit Module) is provided on the circuit substrate 133. The circuit substrate 133 is connected to the positive lead portion 113 via the tab 132A, and is connected to the negative lead portion 115 via the tab 132B. In addition, a lead 134 with a connector for external connection is connected to the circuit substrate 133. When the circuit substrate 133 is connected to the power supply 131, the circuit substrate 133 is protected from the top and bottom by the label 136 and the insulating sheet 137. By attaching the label 136, the circuit substrate 133 and the insulating sheet 137 are fixed. The circuit substrate 133 includes a control unit, a switch unit, a PTC, and a temperature detection unit (not shown). The power supply 131 can be connected to the outside via the positive terminal and the negative terminal (not shown), and the power supply 131 can be charged and discharged via the positive terminal and the negative terminal. The temperature detection unit can detect the temperature via the temperature detection terminal (so-called T terminal).
[0181] Next, Fig. 10A A block diagram showing the configuration of an electric vehicle, which is a hybrid vehicle, is shown. The electric vehicle, for example, includes a control unit 201, various sensors 202, a power source 203, an engine 211, a generator 212, inverters 213 and 214, a driving motor 215, a differential device 216, a transmission 217, and a clutch 218 inside a metal housing 200. In addition, the electric vehicle includes, for example, a front wheel drive shaft 221 connected to the differential device 216 and the transmission 217, a front wheel 222, a rear wheel drive shaft 223, and a rear wheel 224.
[0182] The electric vehicle can travel with either the engine 211 or the motor 215 as a driving source. The engine 211 is a main power source, such as a gasoline engine. When the engine 211 is used as a power source, the driving force (rotational force) of the engine 211 is transmitted to the front wheel 222 or the rear wheel 224 via, for example, the differential device 216, the transmission 217 and the clutch 218 as a driving unit. The rotational force of the engine 211 is also transmitted to the generator 212, and the generator 212 generates AC power by using the rotational force. The AC power is converted into DC power via the inverter 214 and stored in the power supply 203. On the other hand, when the motor 215 as a conversion unit is used as a power source, the power (DC power) supplied from the power supply 203 is converted into AC power via the inverter 213, and the AC power is used to drive the motor 215. The driving force (rotational force) converted from the electric power by the motor 215 is transmitted to the front wheels 222 or the rear wheels 224 via, for example, the differential device 216 , the transmission 217 , and the clutch 218 as a driving unit.
[0183] When the electric vehicle is decelerated by a brake mechanism (not shown), the resistance during deceleration can be transmitted as a rotational force to the motor 215, and the rotational force can be used to generate AC power in the motor 215. The AC power is converted into DC power by the inverter 213, and the DC regenerative power is stored in the power supply 203.
[0184] The control unit 201 controls the overall operation of the electric vehicle, and includes, for example, a CPU, etc. The power supply 203 includes one or more lithium-ion secondary batteries (not shown) described in Embodiment 4 and Embodiment 5. The power supply 203 can also be configured as follows: connected to an external power supply, and storing electricity by receiving power supply from the external power supply. Various sensors 202 are used, for example, to control the speed of the engine 211 and to control the opening of the throttle valve (throttle opening) not shown. Various sensors 202 include, for example, a speed sensor, an acceleration sensor, an engine speed sensor, etc.
[0185] Furthermore, although the electric vehicle is described as a hybrid vehicle, the electric vehicle may be a vehicle (electric vehicle) that operates only using the power source 203 and the motor 215 without using the engine 211 .
[0186] Next, Fig. 10B 2 is a block diagram showing the configuration of a power storage system (power supply system). The power storage system includes a control unit 231, a power supply 232, a smart meter 233, and a power hub 234 inside a house 230 such as a general residence or a commercial building.
[0187] The power source 232 can be connected to an electrical device (electronic device) 235 installed inside the house 230, and can be connected to an electric vehicle 237 parked outside the house 230. In addition, the power source 232 can be connected to a self-contained generator 236 installed in the house 230 via a power hub 234, and can be connected to an external centralized power system 238 via a smart meter 233 and a power hub 234. The electrical device (electronic device) 235 includes, for example, one or more household appliances. As household appliances, for example, refrigerators, air conditioners, televisions, water heaters, etc. can be cited. The self-contained generator 236 is composed of, for example, a solar generator, a wind turbine, etc. As the electric vehicle 237, for example, electric cars, hybrid cars, electric motorcycles, electric bicycles, Segway (registered trademark), etc. can be cited. Examples of the centralized power system 238 include commercial power supplies, power generation devices, power transmission networks, and smart grids (next-generation power transmission networks). In addition, for example, thermal power plants, nuclear power plants, hydroelectric power plants, wind power plants, etc. can also be cited. Examples of power generation devices of the centralized power system 238 include various solar cells, fuel cells, wind power generation devices, micro-hydroelectric power generation devices, geothermal power generation devices, etc., but are not limited to them.
[0188] The control unit 231 controls the overall operation of the power storage system (including the use state of the power supply 232), and includes, for example, a CPU. The power supply 232 includes one or more lithium-ion secondary batteries (not shown) described in Embodiments 4 and 5. The smart meter 233 is, for example, a network-compatible power meter installed in the house 230 on the power demand side, and can communicate with the power supply side. In addition, the smart meter 233 can supply efficient and stable energy by, for example, communicating with the outside and controlling the balance of demand / supply in the house 230.
[0189] In this power storage system, for example, power is stored in the power supply 232 from the centralized power system 238 as an external power supply via the smart meter 233 and the power concentrator 234, and power is stored in the power supply 232 from the self-contained generator 236 as an independent power supply via the power concentrator 234. Since the power stored in the power supply 232 is supplied to the electrical equipment (electronic equipment) 235 and the electric vehicle 237 according to the instruction of the control unit 231, the electrical equipment (electronic equipment) 235 can be operated, and the electric vehicle 237 can be charged. That is, the power storage system is a system that can store and supply power in the house 230 using the power supply 232.
[0190] The power stored in the power source 232 can be used arbitrarily. Therefore, for example, power can be stored in the power source 232 from the centralized power system 238 at night when the power rate is cheap, and the power stored in the power source 232 can be used during the day when the power rate is expensive.
[0191] The power storage system described above may be installed in one household (one family), or in multiple households (multiple families).
[0192] Next, Fig. 10C A block diagram showing the structure of an electric tool is shown. The electric tool is, for example, an electric drill, and includes a control unit 241 and a power source 242 inside a tool body 240 made of a plastic material or the like. A drill head 243 as a movable part is rotatably mounted on the tool body 240, for example. The control unit 241 controls the overall operation of the electric tool (including the use status of the power source 242), and includes, for example, a CPU or the like. The power source 242 includes one or more lithium-ion secondary batteries (not shown) described in Example 4 and Example 5. The control unit 241 supplies power from the power source 242 to the drill head 243 according to the operation of an action switch not shown in the figure.
[0193] The present invention has been described above based on the preferred embodiments, but the present invention is not limited to the above embodiments and can be variously modified. The composition, structure of the laminated structure, the composition, structure of the rolling device, and the method for manufacturing the laminated structure described in the embodiments are illustrative and can be appropriately changed. In the embodiments, an example of inserting the laminated structure into the pressing roller from the 1A end and the 2A end side of the laminated structure is described, but the laminated structure can also be inserted into the pressing roller from the 1B end and the 2B end side of the laminated structure. It is also possible to combine the positive electrode component or negative electrode component (electrode component) having a laminated structure described in Examples 1 to 3 with a positive electrode component or negative electrode component (electrode component) having a composition and structure other than the positive electrode component or negative electrode component described in Examples 1 to 3 to form an electrode structure. The electrode structure can also be in a stacked state other than a wound state.
[0194] The secondary battery of the present invention can be used as a notebook personal computer, a battery pack used as a detachable power source for a personal computer, etc., various display devices, portable information terminals including PDAs (Personal Digital Assistants, portable information terminals), mobile phones, smart phones, cordless phones, main units, subunits, image recording equipment (camcorders, camcorders), digital cameras, electronic books (e-books), electronic papers such as electronic newspapers, electronic dictionaries, music players, portable music players, radios, portable radios, headphones, stereo headphones, game consoles, wearable devices (for example, smart watches, wristbands, smart glasses, medical equipment, health products), navigation systems, memory cards, pacemakers, hearing aids, power tools, electric shavers, refrigerators, air conditioners, televisions, stereos, water heaters, microwave ovens, dishwashers, washing machines, dryers, lighting equipment including indoor lights, etc., various electrical equipment (including portable electronic devices), toys, medical equipment, robots, IoT equipment, IoT terminals, load regulators, signal machines, rail vehicles, golf carts, electric carts, electric vehicles (including hybrid electric vehicles), etc., as driving power sources or auxiliary power sources. In addition, it can be mounted on a storage power source for buildings or power generation equipment represented by a residence, or used to supply electricity to them. In an electric vehicle, the conversion device that converts electricity into driving force by supplying electricity is usually a motor. As a control device (control unit) that performs information processing related to vehicle control, it includes a control device that displays the remaining power of the secondary battery based on information related to the remaining power of the secondary battery. In addition, secondary batteries can also be used in storage devices in so-called smart grids. This type of storage device not only supplies electricity, but also can store electricity by receiving power supply from other power sources. As other power sources, for example, thermal power generation, nuclear power generation, hydroelectric power generation, solar cells, wind power generation, geothermal power generation, fuel cells (including biofuel cells), etc. can be used.
[0195] The electrode of the present invention can be used in a secondary battery in a battery pack having a secondary battery and a control unit (control unit) for controlling the secondary battery. In addition, the electrode of the present invention can be used in a secondary battery in an electronic device that receives power from a secondary battery.
[0196] The electrode of the present invention can be used for a secondary battery in an electric vehicle having a conversion device that receives power from a secondary battery and converts it into a driving force for a vehicle, and a control device (control unit) that processes information related to vehicle control based on information related to the secondary battery. In the electric vehicle, the conversion device usually receives power from the secondary battery to drive the motor and generate driving force. The drive of the motor can also utilize renewable energy. In addition, the control device processes information related to vehicle control based on the remaining battery level of the secondary battery. In the electric vehicle, for example, in addition to electric vehicles, electric motorcycles, electric bicycles, rail vehicles, etc., so-called hybrid vehicles are also included.
[0197] The secondary battery can also be used in a power storage device in a so-called smart grid. This power storage device not only supplies electricity, but also can store electricity by receiving power supply from other power sources. It can be a method of using the electrode of the present invention for a secondary battery in the power storage device. As other power sources, for example, thermal power generation, nuclear power generation, hydroelectric power generation, solar cells, wind power generation, geothermal power generation, fuel cells (including biofuel cells) and the like can be used.
[0198] The electrode of the present invention can be used in a secondary battery in a power storage system (or power supply system) configured to receive power from a secondary battery and / or supply power from a power source to a secondary battery. The power storage system can be any power system as long as it generally uses power, including a simple power device. The power storage system includes, for example, a smart grid, a home energy management system (HEMS), a vehicle, etc., and can also store electricity.
[0199] The electrode of the present invention can be used in a secondary battery in a power storage power source having a secondary battery and configured to be connected to an electronic device to be powered. Basically, it can be used in any power storage system, power supply system or power device regardless of the purpose of the power storage power source, for example, it can be used in a smart grid.
[0200] Example
[0201] Hereinafter, the method for producing a battery electrode of the present invention and the battery electrode obtained by the production method will be described.
[0202] (Comparative Example)
[0203] The method for manufacturing the battery electrode 100 ′ (conventional) is carried out through the following steps.
[0204] First, using a coating device, the electrode material is intermittently coated on one main surface of the metal foil serving as the collector 10' and the electrode material is intermittently coated on the other main surface. At this time, the intermittent area of the electrode material supplied to one main surface of the metal foil is supplied in a manner that is staggered with the intermittent area of the electrode material supplied to the other main surface of the metal foil. Through the above, a precursor of the electrode 100' is formed, which includes a double-sided coating area in which the electrode material layers 20' and 30' are coated on both sides of the collector 10', and a single-sided coating area in which the electrode material layer 20' adjacent to the double-sided coating area is coated on one side of the collector 10'.
[0205] Next, from the viewpoint of increasing the density of the electrode material layer contained in the precursor of the formed battery electrode 100', the precursor of the battery electrode 100' is continuously moved in one direction between a pair of opposing press rollers 40', and the press rollers 40' press the precursor (see Figure 1 Upper side and Figure 4A to Figure 4E ). After a predetermined period of time has passed, the battery electrode 100 ′ is cooled, thereby finally obtaining the battery electrode 100 ′.
[0206] When obtaining the battery electrode 100 ′, the setting values related to the following items are set as follows.
[0207] Radius of a pair of pressure rollers 40': 0.375m (0.25m~0.50m)
[0208] Thickness of current collector (metal foil) 10 ′: 6 μm (4 μm to 20 μm)
[0209] Thickness of electrode material layer 20': 90 μm (50 μm to 125 μm)
[0210] Thickness of electrode material layer 30': 90 μm
[0211] positive electrode
[0212] Area density 30mg / cm 2 ~50mg / cm 2
[0213] Bulk density 3.9g / cm 3 ~4.3g / cm 3
[0214] Linear pressure during stamping: 10kN / cm~40kN / cm
[0215] negative electrode
[0216] Area density 10mg / cm 2 ~30mg / cm 2
[0217] Bulk density 3.9g / cm 3 ~4.3g / cm 3
[0218] Linear pressure during stamping: 6kN / cm~30kN / cm
[0219] Here, after the collector 10' is punched into a dumbbell shape, a tensile test is carried out at room temperature (23°C) with a chuck spacing of 50mm and a tensile speed of 1mm / min using a universal tensile tester of Instron, and the Young's modulus is calculated based on the tangent of the rising portion of the obtained load-elongation curve. The Young's modulus of the collector 10' obtained as a constituent element of the battery electrode 100' is 74Gpa. In other words, the rigidity of the collector 10' is relatively high. Therefore, even if the electrode material layer 20' is on the upper side of the collector 10' in the single-sided coating area located at the boundary portion 70', the self-weight of the electrode material layer 20' acts, and the degree of bending of the collector 10' in the single-sided coating area that has been heat-treated and located at the boundary portion 70' in the downward direction is also small.
[0220] Therefore, when the precursor of the electrode 100' is pressurized using a pair of pressure rollers 40', the range in which the pressure rollers 40' can contact the collector 10' in the single-sided coated area of the boundary portion 70' is small. As a result, it is not easy to pressurize the collector and the electrode material layer in the single-sided coated area of the boundary portion by a pair of pressure rollers opposing each other. Therefore, the range of the low volume density region 23' of the electrode material layer 20' in the single-sided coated area of the boundary portion 70' is relatively large, about 0.8 mm. Specifically, in the low volume density region 23' (width: about 0.8 mm), the ratio (A / B) of the volume density (A) of the electrode material layer 20' located in the boundary portion 70' to the volume density (B) of the electrode material layer 20' located in the portion other than the boundary portion 70' is less than 0.9 (refer to Figure 3 ).
[0221] (Example 1)
[0222] The method for producing the battery electrode 100 is carried out through the following steps.
[0223] First, using a coating device, the electrode material is intermittently coated on one main surface of the metal foil serving as the collector 10 and the electrode material is intermittently coated on the other main surface. At this time, the intermittent region of the electrode material supplied to one main surface of the metal foil is supplied in a manner that is staggered with the intermittent region of the electrode material supplied to the other main surface of the metal foil. Through the above, a precursor of the electrode 100 is formed, which includes a double-sided coating region in which the electrode material layers 20 and 30 are coated on both sides of the collector 10, and a single-sided coating region in which the electrode material layer 20 adjacent to the double-sided coating region is coated on a single side of the collector 10.
[0224] In Example 1, unlike the above-mentioned comparative example, after the precursor of the electrode body 100 is formed, before the precursor is pressurized, a high-frequency induction heating device 80 is used to implement a heat treatment (heat treatment temperature: 200 degrees) of the collector 10 located at the boundary portion 70 of the double-sided coating area and the single-sided coating area. Through such a heat treatment, the part of the collector 10 located at the boundary portion 70 softens due to the heat energy supplied to the part. The Young's modulus of the softened part of the collector is 66Gpa. In other words, the rigidity of the collector 10 located at the boundary portion 70 is relatively low. Therefore, the electrode material layer 20 is on the upper side of the collector 10 located in the single-sided coating area of the boundary portion 70, and the self-weight of the electrode material layer 20 acts, so that the degree of bending of the collector 10 in the single-sided coating area of the boundary portion 70 that has been subjected to heat treatment to the downward direction is greater than that of the comparative example.
[0225] In this state, after the heat treatment of the current collector located at the boundary portion 70 is performed, from the viewpoint of increasing the density of the electrode material layer included in the precursor of the battery electrode 100, the precursor of the battery electrode 100 is continuously moved in one direction between a pair of opposing press rollers 40 while being pressurized by the press rollers 40 (see Figure 1 Lower side and Figure 2 ). After a predetermined period of time has passed, the battery electrode 100 is cooled to finally obtain the battery electrode 100 .
[0226] In addition, the setting values when obtaining the battery electrode 100 are the same as those described in the above-mentioned comparative example, and therefore, the description thereof will be omitted to avoid duplication of description.
[0227] As described above, the degree of bending of the collector 10 in the single-sided coating area of the boundary portion 70 to which the heat treatment is applied is greater than that of the comparative example. Therefore, after the precursor of the electrode 100 is pressed using a pair of pressing rollers 40, the range in which the collector 10 in the single-sided coating area of the boundary portion 70 and the pressing roller 40 can contact becomes larger than that of the comparative example. As a result, it becomes easier to pressurize the collector and the electrode material layer in the single-sided coating area of the boundary portion by a pair of pressing rollers opposed to each other than in the comparative example. Therefore, compared with the comparative example, the range of the low volume density region 23 of the electrode material layer 20 in the single-sided coating area of the boundary portion 70 is narrowed to about 0.5 mm. Specifically, in the low volume density region 23 (width: about 0.5 mm), the ratio (A / B) of the volume density (A) of the electrode material layer 20 located at the boundary portion 70 to the volume density (B) of the electrode material layer 20 located at the portion other than the boundary portion 70 is less than 0.9 (refer to Figure 3 ). As can be seen from the above, in Example 1, the range of the low volume density region is narrowed compared to the comparative example. Furthermore, in the current collector 10 as a constituent element of the finally obtained battery electrode 100, the Young's modulus of the current collector 10 located at the boundary portion 70 between the double-sided coating region and the single-sided coating region is reduced by about 10% compared to the Young's modulus of the current collector 10 located at the portion other than the boundary portion 70.
[0228] (Example 2)
[0229] The method for producing the battery electrode 100 is carried out through the following steps.
[0230] First, similarly to Example 1, a precursor of an electrode 100 is formed, which includes a double-sided coating region where electrode material layers 20 and 30 are coated on both sides of a current collector 10 , and a single-sided coating region where electrode material layer 20 adjacent to the double-sided coating region is coated on one side of the current collector 10 .
[0231] In Example 2, unlike Example 1, after the precursor of the electrode 100 is formed, before the precursor is pressed, a high-frequency induction heating device 80 is used to supply greater heat energy to implement a heat treatment (heat treatment temperature: >200 degrees) of the collector 10 located at the boundary portion 70 between the double-sided coating area and the single-sided coating area. Through such a heat treatment, compared with Example 1, the part of the collector 10 located at the boundary portion 70 is softened due to the heat energy supplied to the part. The Young's modulus of the softened part of the collector is 33Gpa. That is, compared with Example 1, the rigidity of the collector 10 located at the boundary portion 70 is lower. Therefore, the electrode material layer 20 is on the upper side of the collector 10 located in the single-sided coating area of the boundary portion 70, and the self-weight of the electrode material layer 20 acts, so that the degree of bending of the collector 10 in the single-sided coating area of the boundary portion 70 to which the heat treatment is applied is greater than that of Example 1.
[0232] Next, after the current collector at the boundary portion 70 is heat treated, the precursor of the electrode 100 is pressed by a pair of press rollers 40 (see Figure 1 Lower side and Figure 2 ). After a predetermined period of time has passed, the battery electrode 100 is cooled to finally obtain the battery electrode 100 .
[0233] In addition, the setting values when obtaining the battery electrode 100 are the same as those described in the above-mentioned comparative example, and therefore, the description thereof will be omitted to avoid duplication of description.
[0234] As described above, the degree of downward bending of the collector 10 in the single-sided coated area of the boundary portion 70 to which the heat treatment is applied becomes larger than that in Example 1. Therefore, after the precursor of the electrode 100 is pressurized using a pair of pressure rollers 40, the range in which the collector 10 in the single-sided coated area of the boundary portion 70 and the pressure roller 40 can contact becomes larger than that in Example 1. As a result, it becomes easier to pressurize the collector and the electrode material layer in the single-sided coated area of the boundary portion by a pair of pressure rollers opposed to each other than in Example 1. Therefore, compared with Example 1, the range of the low volume density region 23 of the electrode material layer 20 in the single-sided coated area of the boundary portion 70 becomes narrower, about 0.3 mm. Specifically, in the low volume density region 23 (width: about 0.3 mm), the ratio (A / B) of the volume density (A) of the electrode material layer 20 located at the boundary portion 70 to the volume density (B) of the electrode material layer 20 located at the portion other than the boundary portion 70 is less than 0.9 (refer to Figure 3 ). As can be seen from the above, in Example 2, the range of the low volume density region is narrower than that in Example 1. Furthermore, in the current collector 10 as a constituent element of the finally obtained battery electrode 100, the Young's modulus of the current collector 10 located at the boundary portion 70 between the double-sided coating region and the single-sided coating region is reduced by more than 50% compared with the Young's modulus of the current collector 10 located at a portion other than the boundary portion 70.
[0235] CROSS-REFERENCE TO RELATED APPLICATIONS
[0236] This application claims priority under the Paris Convention based on Japanese Patent Application No. 2018-111371 (filing date: June 11, 2018, invention title: "Battery electrode and method for producing the same"). All the contents disclosed in the application are incorporated herein by reference.
[0237] Description of Reference Numerals
[0238] 10…current collector (metal foil); 20…electrode material layer; 23…low volume density region; 30…electrode material layer; 40…a pair of press rollers; 101…electrode structure storage member (battery can); 102, 103…insulating plate; 104…battery cover; 105…safety valve mechanism; 105A…disc; 106…thermistor element (PTC element, Positive TemperatureCoefficient element); 107... washer; 108... center pin; 111... electrode structure; 112... positive electrode; 112A... positive electrode current collector; 112B... positive electrode material layer; 113... positive electrode lead; 114... negative electrode component; 114A... negative electrode current collector; 114B... negative electrode material layer; 115... negative electrode lead; 116... separator; 118... electrolyte layer; 119... protective tape; 120... exterior component; 121... sealing film; 131... power supply; 132A, 132B... pole ear; 133... circuit board; 134... lead with connector; 135... adhesive tape; 136... label; 137... insulating sheet; 200... shell body; 201…control unit; 202…various sensors; 203…power source; 211…engine; 212…generator; 213, 214…inverter; 215…motor; 216…differential device; 217…transmission; 218…clutch; 221…front wheel drive shaft; 222…front wheel; 223…rear wheel drive shaft; 224…rear wheel; 230…house; 231…control unit; 232…power source; 233…smart meter; 234…power hub; 235…electrical equipment (electronic equipment); 236…self-contained generator; 237…electric vehicle; 238…centralized power system; 240…tool body; 241…control unit; 242…power source; 243…drill head;< / zr> < / w> < / sr> < / ca> < / zn> < / cu> < / nb> < / v> < / ti> < / al> < / mg> < / ni> < / fe> < / co> < / w> < / sr> < / ca> < / sn> < / zn> < / cu> < / fe> < / cr> < / v> < / ti> < / al> < / mg> < / ni> < / co> < / w> < / sr> < / ca> < / sn> < / zn> < / cu> < / fe> < / cr> < / v> < / ti> < / al> < / mg> < / ni> < / w> < / sr> < / ca> < / sn> < / zn> < / cu> < / fe> < / cr> < / v> < / ti> < / al> < / mg> < / co> < / w> < / sr> < / ca> < / sn> < / zr> < / zn> < / cu> < / fe> < / cr> < / v> < / ti> < / al> < / mg> < / co> < / fe> < / co> < / ni>
Claims
1. A manufacturing method is a method for manufacturing a battery electrode, comprising the following steps: (i) forming a precursor of the electrode having a double-sided coating region and a single-sided coating region, wherein the electrode material layer is coated on both sides of the current collector, the single-sided coating region and the double-sided coating region are adjacent to each other, and the electrode material layer is coated on one main surface of the current collector; and (ii) a step of pressurizing the precursor of the electrode, Before the precursor of the electrode is pressurized, the current collector located at the boundary between the double-sided coating region and the single-sided coating region is locally heat-treated. By performing the heat treatment, the current collector located at the boundary portion is locally softened.
2. The manufacturing method according to claim 1, wherein: By performing the heat treatment, the bending region of the current collector located at the boundary portion is increased compared to a case where the heat treatment is not performed.
3. The manufacturing method according to claim 1 or 2, wherein: Pressing the precursor of the electrode is performed using a pair of press rollers positioned so as to sandwich the precursor, By performing the heat treatment, the size of the space region formed between the current collector located at the boundary portion and the pressing roller directly facing each other is relatively reduced compared to a case where the heat treatment is not performed.
4. The manufacturing method according to claim 1 or 2, wherein: By performing the heat treatment, the Young's modulus of the current collector located at the boundary portion is reduced compared to the Young's modulus of the current collector located at a portion other than the boundary portion.
5. The manufacturing method according to claim 4, wherein: The Young's modulus of the current collector located at the boundary portion is reduced by 50% or more of the Young's modulus of the current collector located at a portion other than the boundary portion.
6. The manufacturing method according to claim 1 or 2, wherein: The heat treatment is performed in a non-contact manner with the current collector and the electrode material layer located at the boundary portion.
7. The manufacturing method according to claim 6, wherein: The non-contact heat treatment is performed using a high-frequency induction heating device.
8. The manufacturing method according to claim 7, wherein: When the high-frequency induction heating device and the current collector located at the boundary portion are opposed to each other, the high-frequency induction heating device is driven.
9. The manufacturing method according to claim 1 or 2, wherein: After the precursor of the electrode is pressurized, a ratio A / B of a volume density A of the electrode material layer located at the boundary portion to a volume density B of the electrode material layer located at a portion other than the boundary portion is greater than or equal to 0.9 and less than or equal to 1.
0.
10. The manufacturing method according to claim 1 or 2, wherein: After the precursor of the electrode is pressurized, the size of the low volume density region of the electrode material layer located at the boundary portion is relatively reduced compared to a case where the heat treatment is not performed.