Silver electrolyte for depositing a dispersion silver layer and contacting a surface having a dispersion silver layer
By using electrolytes of silver potassium cyanide and grain refining agent, uniform dispersion and high conductivity of the silver layer are achieved, the problems of uneven solid composition and high friction coefficient are solved, and the durability and wear resistance of the contacts are improved. simplifies the process.
Patent Information
- Application Number
- CN201980044369.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-07-05
- Filing Date
- 2019-06-26
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2039-06-26
AI Technical Summary
The solid components of existing silver electrolytes are unevenly dispersed during the deposition process, resulting in uneven surface properties, increasing cost and process complexity, and high friction coefficient leads to large interfacing force and severe wear, affecting the durability of the contact parts.
Using silver potassium cyanide-based electrolyte, combined with 0.2 to 10g/L grain refining agent and 1 to 150g/L solid components, uniformly disperse the solid components, reduce the use of additives, improve conductivity and wear resistance, suitable for for low and high current density deposition.
The uniform dispersion of solid components is achieved, the durability and conductivity of the silver layer are improved, the friction coefficient and interpolation force are reduced, the service life of the contact parts is extended, and process control is simplified.
Smart Images

Figure BDA0002873421050000171 
Figure BDA0002873421050000181
Abstract
Description
Technical Field
[0001] The invention relates to a silver electrolyte for depositing a silver layer on a substrate, a method for depositing a dispersion silver layer on a substrate and a contact surface, wherein an electrochemically deposited dispersion silver layer is arranged on the substrate. The invention also relates to the use of the contact surface for electrical contacting in a plug connection and the use of the silver electrolyte for coating a substrate by means of rack plating and / or barrel plating. Background Art
[0002] Silver is a very versatile material. Due to its ductility and softness, it can be processed in a variety of ways. Silver has the best thermal and electrical conductivity of all metals. This makes silver an interesting material for the electrical and electronics industry, especially for coating surfaces, especially contact surfaces. As interfaces for transmitting high currents, plugs and plug contacts are used, which have the lowest possible contact resistance, so silver coatings are often used in contact elements that are installed in such plug connectors and provide electrical contact in the plugged state.
[0003] Silver electrolytes are used for silver coating of substrates and for producing contact surfaces. In this context, various silver-containing solutions and dispersions are referred to as silver electrolytes, which are used for electrochemically, in particular electroplating, silvering surfaces. Silver electrolyte solutions may contain various further additives, such as grain refiners, dispersants, brighteners or solid components.
[0004] For use in the electrical and electronic sector, especially in plugs and plug contacts, electrical conductivity, contact resistance and friction coefficient are particularly important. In particular, the requirements for silver layers, especially electroplated silver layers, are to be considered to be increasing, especially with regard to increasing electron mobility.
[0005] If two silver-coated surfaces are moved back and forth over each other, high forces are required for this purpose, since plugging forces and pulling forces act. This is disadvantageous for contact with silver surfaces, since silver surfaces have a relatively high coefficient of friction, which leads to high plugging forces and pulling forces, especially in the case of plugging contact. Due to the high coefficient of friction, the silver surfaces wear, which severely limits the number of possible plugging cycles. In addition, there is the problem that silver surfaces tend to cold weld. However, the contact resistance of the system of two silver-coated surfaces is advantageous.
[0006] DE 10346206 A1 describes a contact surface for electrical contact. Finely dispersed graphite particles are deposited in the illustrated silver layer (which is produced by means of an electroplating method). By incorporating graphite into the silver layer, a reduction in friction is achieved, thereby achieving lower plugging forces, improved corrosion protection and a longer contact life due to increased wear protection. At the same time, good electrical contact is ensured.
[0007] DE 10 2008 030 988 B4 describes an electrochemical coating of a component, wherein the layer has a metallic structure and carbon nanotubes are introduced into the layer together with a dry lubricant. The introduction of the carbon nanotubes increases the electrical and thermal conductivity of the layer, and by mixing with a further dry lubricant the layer can be optimized for different purposes in terms of its wear behavior.
[0008] DE 2543082 A1 discloses a silver electrolyte for producing a silver coating, which also contains graphite, a gloss additive and a wetting agent. The graphite must be kept in suspension during deposition by pumping the bath containing the electrolyte in circulation.
[0009] The prior art describes silver electrolytes which additionally contain glossing agents or other substances which improve deposition, such as xanthates, urethanes or door putty oils. The electrolyte solutions also appear to require mechanical intervention to keep the solid components in suspension. Electrolytes containing various solid components are also described in the prior art in order to obtain properties of the deposition surface which are lost due to expensive additive systems.
[0010] A disadvantage of known silver electrolytes for depositing silver on surfaces is that they do not disperse the substances to be dispersed sufficiently uniformly in the electrolyte, which leads on the one hand to an uneven distribution of the solid components in the deposited layer and on the other hand to partial complete non-deposition. Likewise, some electrolytes are not suitable for uniformly dispersing the various types of solid components, so that pumping circulation or stirring is required during deposition, which has a negative impact on the uniformity of the surface obtained. In order to overcome these disadvantages, expensive additive systems are usually used, which can have an adverse effect on the deposited surface and, moreover, lead to increased costs.
[0011] The known electrolytes are not able to disperse further particles, in particular dry lubricants, sufficiently well to obtain a surface into which other substances, such as additives, are simultaneously introduced which negatively influence the resulting dispersion layer. This results in, among other things, inhomogeneities of the known surfaces.
[0012] Furthermore, it is disadvantageous that, up to now, it has usually been necessary to use a combination of solid components, such as carbon nanotubes and dry lubricants, in order to achieve suitable surface properties and to compensate for the shortcomings of the additive system. This also results in additional substances that negatively affect the homogeneity and further increase the costs. In addition, additives that are intended to improve deposition make process control and process monitoring even more expensive and complex.
[0013] A further disadvantage of the known electrolytes is that a high deposition temperature must be selected in order to ensure adequate deposition. Summary of the invention
[0014] The object of the present invention is therefore to provide a silver electrolyte which allows good dispersion of the solid components and at the same time allows the elimination of expensive additive systems for achieving uniform deposition. Another object of the present invention is to provide surfaces, in particular contact surfaces, which have increased wear resistance and good electrical conductivity. The object of the present invention is also to provide a deposition method for producing coated surfaces, in particular contact surfaces, with improved durability.
[0015] Durability here means a reduction in the required plugging force with increasing possible plugging cycles, a reduction in cold welding (ie welding of the soft silver layer due to microvibrations) and the maintenance of the most favorable possible contact resistance over the longest possible period of time.
[0016] The object of the invention is achieved by a silver electrolyte according to claim 1. Preferred embodiments of the silver electrolyte according to the invention are given in the dependent claims, which can be selectively combined with one another.
[0017] The invention also provides a method for depositing a dispersion silver layer on a substrate according to claim 8. Preferred embodiments of the method according to the invention are given in the dependent claims, which can optionally be combined with one another.
[0018] The invention also comprises a contact surface according to the following claim 12. Preferred embodiments of the contact surface according to the invention are given in the dependent claims, which can optionally be combined with one another.
[0019] The invention further relates to the use of the contact surface of the invention for electrical contacting in plug connections and to the use of the dispersion silver electrolyte of the invention for coating substrates by means of rack application and / or roll application.
[0020] The silver electrolyte for depositing a silver layer on a substrate comprises, according to the invention,
[0021] a) Potassium silver cyanide,
[0022] b) potassium cyanide with a content of at least 10 g / L,
[0023] c) at least one grain refiner having a content of 0.2 to 10 g / L;
[0024] d) at least one dispersant having a content of 1 to 10 g / L;
[0025] e) at least one solid component having a content of 1 to 150 g / L,
[0026] The particles of the solid component have an average particle size (d 50 ).
[0027] Surprisingly, it has been found that, by means of a silver electrolyte in the composition shown, various solid components can be uniformly dispersed to obtain a surface with a dispersion silver layer, which has improved durability and good electrical conductivity. The electrolyte of the invention is characterized in that extremely different dispersion silver layers can be produced with it. These layers are characterized by their good contact resistance with improved friction values or increased hardness, depending on the type and amount of the solid components introduced. The durability based on wear or friction of these layers exceeds that of a simple silver layer. In addition, the electrolyte of the invention is particularly well suited for uses in which solid components are used as the substance to be dispersed. In addition, a silver layer with good electrical conductivity is obtained by the electrolyte of the invention, so that the addition of further substances such as carbon nanotubes can be omitted. In addition, the electrolyte of the invention can be used both at low current densities and at high current densities. Therefore, the electrolyte can be used for various purposes and can be used, for example, for roller plating and rack plating. The electrolyte is suitable for many types of electrochemical deposition.
[0028] In the electrolyte according to the invention, the solid components are dispersed homogeneously. The particularly homogeneous dispersion ensures a homogeneous incorporation of the solid components into the deposited silver layer. In addition, the use of the electrolyte according to the invention reduces the concomitant incorporation of additives that usually negatively affect homogeneity.
[0029] Furthermore, the electrolyte is suitable for use with different solid components, so that the surface properties can be adapted to different applications. A further advantage of the electrolyte according to the invention is that the layer thickness can be varied and adapted to the respective application.
[0030] "Substituted" in the sense of the present invention means that a hydrogen atom on a hydrocarbon is replaced by another atom or group of atoms.
[0031] In the sense of the present invention, “solid components” are components which are not present in solution but are present as solids in the electrolyte and are also referred to in conjunction with the dispersion silver layer of the present invention as finely divided solid components.
[0032] In the sense of the present invention, the average particle size (d 50 ) means that 50% of the solid particles have a diameter smaller than the given value. 90 The value means that 90% of the particles of the solid component have a diameter smaller than the given value.
[0033] In the context of the present invention, "grain refinement" is the process of changing the grain size of the silver deposit to a smaller grain size.
[0034] “Dry lubricants” in the sense of the present invention are substances which improve the sliding properties of a surface.
[0035] In the sense of the present invention, a “hard material” is a substance which is characterized by its particularly high hardness.
[0036] The silver electrolyte is a solution, preferably an aqueous solution. The electrolyte may also contain additional solvents.
[0037] Unless otherwise stated, all content data in g / L are below based on the total volume of the electrolyte.
[0038] In an advantageous embodiment, the content of potassium silver cyanide in the electrolyte is at least 10 g / L, preferably at least 25 g / L, more preferably at least 40 g / L, and even more preferably at least 50 g / L.
[0039] The silver content in the electrolyte is advantageously at least 15 g / L, preferably at least 20 g / L, more preferably at least 25 g / L, and still more preferably at least 27 g / L.
[0040] Preferably, the silver content in the electrolyte is between 1 and 100 g / L, preferably between 5 and 50 g / L, and even more preferably between 10 and 30 g / L.
[0041] Preferably, the content of potassium silver cyanide in the electrolyte is at most 150 g / L, preferably at most 125 g / L, more preferably at most 100 g / L, and still more preferably at most 75 g / L.
[0042] The content of potassium cyanide is preferably at least 20 g / L, preferably at least 50 g / L, more preferably at least 80 g / L, still more preferably at least 100 g / L, further still more preferably at least 120 g / L and most preferably at least 140 g / L.
[0043] In an advantageous embodiment, the at least one grain refiner is selected from naphthalenesulfonic acid, naphthalenesulfonic acid derivatives or mixtures thereof.
[0044] The content of grain refiner is advantageously between 0.2 and 8 g / L, preferably between 0.3 and 6 g / L, more preferably between 0.4 and 5 g / L and still more preferably between 0.5 and 3 g / L.
[0045] The dispersant preferably contains C1-C 25 Alkyl sulfates containing an alkyl group, and preferably containing a C1-C 20 Preferably, the dispersant comprises an alkyl sulfate having a C1-C 20 alkyl sulfates, and more preferably, having C1-C 20 Sodium alkyl sulfate of an alkyl group. The alkyl group may be linear and / or branched.
[0046] Preferably, the at least one dispersant is present in an amount between 0.2 and 9 g / L, preferably between 0.3 and 8 g / L, more preferably between 0.4 and 7 g / L and more preferably between 0.5 and 6 g / L.
[0047] Preferably, the content of at least one solid component is between 5 and 125 g / L, preferably between 10 and 100 g / L, more preferably between 15 and 90 g / L, and still more preferably between 20 and 80 g / L.
[0048] Preferably, the content of at least one solid component is at least 5 g / L, preferably at least 10 g / L, more preferably at least 15 g / L, still more preferably at least 20 g / L, further still more preferably at least 30 g / L, and most preferably at least 40 g / L.
[0049] In an advantageous embodiment, the particles of the at least one solid component have an average particle size (d ) of 50 nm to 75 μm, preferably 100 nm to 50 μm, more preferably 500 nm to 35 μm, and more preferably 1 μm to 20 μm. 50 The diameter of the solid component and thus the average particle size (d 50 ) is determined by means of laser diffraction.
[0050] Suitable solid components are all types of organic or inorganic particles.
[0051] Preferably, the at least one solid component is a dry lubricant, a hard material or a mixture thereof, preferably a dry lubricant.
[0052] In an advantageous embodiment, at least one solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers and carbon modifications. In the sense of the present invention, carbon modifications are also understood to mean, in addition to diamond, hexagonal carbon, fullerenes and graphite, graphene, carbon nanotubes, carbon black, activated carbon, graphite fluoride, graphite oxide, Al2O3-coated graphite, non-graphitic forms of carbon and other forms.
[0053] According to a preferred embodiment, the at least one solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, graphite, graphite fluoride, graphite oxide, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, diamond, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably from MoS2, WS2, graphite, graphite oxide, hexagonal boron nitride or a mixture thereof, more preferably from graphite, graphite oxide, MoS2, WS2 or a mixture thereof, and even more preferably from graphite.
[0054] Al2O3-coated solid particles are produced by coating solid particles with the aid of controlled hydrolysis of Al(NO3)3·9H2O according to Huang & Xiong (2008) (Huang, Z.; Xiong, D. (2008): Coating of MoS2 with Al2O3 by pulse electrodeposition for Ni-MoS2 / Al2O3 composite coatings. Surfaces & Coatings & Technology 202 (2008) 3208-3214).
[0055] According to an advantageous embodiment, at least one solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers. Preferably, the at least one solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably consisting of MoS2, WS2, hexagonal boron nitride or a mixture thereof, more preferably consisting of MoS2, WS2 or a mixture thereof.
[0056] According to another advantageous embodiment, the at least one solid component is selected from carbon modifications. Preferably, the at least one solid component is selected from graphite, graphite fluoride, graphite oxide, diamond, Al2O3-coated graphite or a mixture thereof, preferably graphite, graphite fluoride, graphite oxide, Al2O3-coated graphite or a mixture thereof, more preferably graphite, graphite oxide or a mixture thereof, and even more preferably graphite.
[0057] Preferably, the electrolyte further comprises at least one additional solid component. The at least one additional solid component may be selected from the above-mentioned solid components.
[0058] Advantageously, the electrolyte may additionally contain a glossing agent. For this purpose, amounts of 1 to 1000 mg / L, preferably less than 50 mg / L, are generally used. Examples of glossing agents are phenylpropionic acid, phenylpropionic acid amide, triaminotriphenylmethane, 1-(p-aminophenyl)-3-methylpyrazole, stearamidopropyldimethyl-(β-hydroxyethyl)dihydrogenammonium phosphate, 1,5-diphenylcarbazide and chlorohydrate.
[0059] The silver electrolyte of the present invention may optionally contain further additives, such as stabilizers, dispersants and / or grain refiners, to further improve the properties of the electrolyte and to improve the properties of the deposited dispersion silver layer.
[0060] The above-mentioned embodiments may also be combined.
[0061] A further subject of the invention is a method for depositing a dispersion silver layer on a substrate, which according to the invention comprises the following steps:
[0062] a) providing the silver electrolyte of the present invention,
[0063] b) introducing a substrate into the silver electrolyte, and
[0064] c) performing deposition.
[0065] The method of the present invention comprises depositing a dispersion silver layer on a substrate of the silver electrolyte according to the present invention according to any of the above embodiments. The above description of the electrolyte according to the present invention also applies to the present method accordingly.
[0066] In the method according to the invention, all substrates commonly used for depositing silver layers and dispersion silver layers can be used. In the method according to the invention, the substrate preferably comprises a metal or a metal alloy. The dispersion silver layer is then deposited on the metal or metal alloy. The metal or metal alloy can, for example, contain copper and / or iron or consist of them. Likewise, further intermediate layers consisting of other metals, for example nickel or silver, can be present. These layers have various functions, for example increasing the adhesion of the dispersion silver layer on the substrate, corrosion protection, diffusion resistance, or improving other physical properties.
[0067] Electroplating or currentless methods can be used as deposition methods. Examples of electroplating methods are barrel plating, rack plating or strip plating.
[0068] The substrate is preferably cleaned, preferably degreased, before coating. Various pretreatment steps may be performed on the substrate. Here, a copper layer, a nickel layer and / or an additional silver layer may be deposited.
[0069] Preferably, the substrate is pre-silvered before step a). Preferably, the substrate is nickel-plated before pre-silvering.
[0070] According to an advantageous embodiment, the temperature when depositing in step c) is 1°C to 50°C, preferably 5°C to 40°C, more preferably 5°C to 35°C, still more preferably 10°C to 30°C, further still more preferably 15°C to 25°C, still more preferably 17°C to 22°C, and most preferably 20°C.
[0071] In an advantageous embodiment, the current density in step c) is 0.03 A / dm 2 Up to 1.2A / dm 2 , preferably 0.05A / dm 2 Up to 1.0A / dm 2 , more preferably 0.075A / dm 2 Up to 1.0A / dm 2 , more preferably 0.1A / dm 2 Up to 0.95A / dm 2 And more preferably 0.15A / dm 2 Up to 0.90A / dm 2 .
[0072] According to an advantageous embodiment, the method is barrel plating and / or rack plating.
[0073] The duration of the deposition can be selected depending on the desired layer thickness to be obtained and the application, barrel and / or rack plating. Due to the lower current density of barrel and rack plating compared to other methods, the deposition time is longer. In principle, the duration of the deposition is not limited.
[0074] Preferably, the duration of the deposition in step c) is at least 5 minutes, preferably at least 7 minutes, more preferably at least 9 minutes and still more preferably at least 11 minutes.
[0075] Preferably, the duration of the deposition in step c) is from 5 minutes to 100 minutes, preferably from 7 minutes to 75 minutes and more preferably from 10 minutes to 50 minutes.
[0076] Preferably, step a) is performed before step b), and more preferably, step b) is performed after step c).
[0077] Another subject matter of the invention relates to a contact surface in which an electrochemically deposited dispersion silver layer is arranged on a substrate according to the invention, and
[0078] The dispersion silver layer contains particles of at least one finely divided solid component having an average particle size (d 50 ).
[0079] The above descriptions of the electrolyte according to the invention and the method according to the invention also apply accordingly to the contact surface. Thus, the finely dispersed solid component can be selected from the above-mentioned solid components. As a substrate for the contact surface according to the invention, all the above-mentioned substrates can be used.
[0080] When a dry lubricant is used as the solid component, the contact surface according to the invention allows only one of the contact partners to be provided with a dispersion silver surface. The other contact partner can consist of a conventional metal surface without solid components, in particular dry lubricant components. This makes it possible to reduce costs. However, it is also possible to provide both contact partners with a dispersion silver surface.
[0081] The contact surface according to the invention is characterized by its advantageous wear resistance. In particular, the resistance to wear due to micro-movements, so-called micro-motions, during the plugging process is significantly improved. Such micro-movements occur, for example, in plugs of automobiles due to vibrations during operation of the automobile. Wear due to micro-movements can also occur due to temperature fluctuations.
[0082] Preferably, the contact surface further comprises at least one further solid component. Preferably, the at least one further solid component is a dry lubricant or a hard material. Preferably, the at least one further solid component is selected from the solid components described above for the electrolyte according to the invention, which are also correspondingly suitable for the contact surface.
[0083] In an advantageous embodiment, the particles of the at least one finely divided solid component have an average particle size (d ) of 50 nm to 75 μm, preferably 100 nm to 50 μm, more preferably 500 nm to 35 μm, and even more preferably 1 μm to 20 μm. 50 ). The same applies to the particles of the further solid components.
[0084] The content of at least one finely divided solid component in the dispersion silver layer can be varied by changing the deposition conditions. In this way, the properties of the surface with respect to contact resistance and wear resistance can be adjusted.
[0085] According to an advantageous embodiment of the contact surface, the dispersion silver layer comprises at least one finely divided solid component in an amount of at least 3.0 wt.-%, preferably at least 3.1 wt.-%, more preferably at least 3.2 wt.-%, even more preferably at least 3.3 wt.-% and further even more preferably at least 3.5 wt.-%, based on the total weight of the dispersion silver layer.
[0086] Preferably, the dispersion silver layer comprises at least one finely divided solid component in an amount ranging from 3.0 wt. % to 30.0 wt. %, preferably from 3.1 wt. % to 25 wt. %, more preferably from 3.1 wt. % to 20 wt. %, still more preferably from 3.1 wt. % to 15 wt. %, still further more preferably from 3.2 wt. % to 10 wt. %, and still more preferably from 3.5 wt. % to 10 wt. %, based on the total weight of the dispersion silver layer.
[0087] Preferably, the at least one finely divided solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers and carbon modifications.
[0088] According to an advantageous embodiment of the contact surface, the at least one finely dispersed solid component is selected from silicates, sulfides, carbides, nitrides, oxides, selenides, tellurides, organic and inorganic polymers. Preferably, the at least one finely dispersed solid component is selected from MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium-selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof, preferably consists of MoS2, WS2, hexagonal boron nitride or mixtures thereof, more preferably consists of MoS2, WS2 or mixtures thereof.
[0089] According to another advantageous embodiment of the contact surface, the at least one finely divided solid component is selected from carbon modifications. Preferably, the at least one finely divided solid component is selected from graphite, fluorinated graphite, graphite oxide, diamond, Al2O3-coated graphite or mixtures thereof, preferably graphite, fluorinated graphite, graphite oxide, Al2O3-coated graphite or mixtures thereof, more preferably graphite, graphite oxide or mixtures thereof, and even more preferably graphite.
[0090] According to a preferred embodiment, the at least one finely dispersed solid component is selected from MoS2, WS2, SnS2, graphite, graphite oxide, graphite fluoride, hexagonal boron nitride, silver niobium-selenide, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or a mixture thereof, preferably consisting of MoS2, WS2, graphite and hexagonal boron nitride or a mixture thereof.
[0091] In another advantageous embodiment of the contact surface, the at least one finely divided solid component is selected from graphite, MoS2, WS2 or mixtures thereof, preferably consists of graphite, and the dispersion silver layer contains the at least one finely divided solid component in an amount of at least 3.0 wt.-%, preferably at least 3.1 wt.-%, more preferably at least 3.2 wt.-%, and even more preferably at least 3.3 wt.-% and even more preferably at least 3.5 wt.-%, based on the total weight of the dispersion silver layer.
[0092] In another advantageous embodiment of the contact surface, the dispersion silver layer has a coefficient of friction μ at 0.3 N after 100 cycles of less than 1.4, preferably less than 1.2, more preferably less than 1.0, still more preferably less than 0.8, still further more preferably less than 0.6 and still more preferably 0.4.
[0093] According to another advantageous embodiment of the contact surface, the contact resistance at 1.0 N after 100 cycles is less than 1.0 mΩ, preferably less than 0.8 mΩ, more preferably less than 0.75 mΩ, even more preferably less than 0.7 mΩ, even more preferably less than 0.65 mΩ.
[0094] In another advantageous embodiment of the contact surface, the dispersion silver layer has a coefficient of friction μ at 1.0 N after 100 cycles of less than 1.0, preferably less than 0.8, more preferably less than 0.6, even more preferably less than 0.5 and even more preferably less than 0.45.
[0095] The layer thickness of the deposited dispersion silver layer is preferably between 0.5 μm and 200 μm, preferably between 1 μm and 100 μm, particularly preferably between 1.1 μm and 25 μm.
[0096] Advantageously, the contact surface is a micro-rough surface. The microstructure has a favorable effect on the tribological and electrical properties.
[0097] Preferably, the contact surface has a micro-roughness as described below by the average roughness value Ra of at least 0.05 μm, preferably at least 0.1 μm, more preferably at least 0.2 μm and still more preferably at least 0.3 μm.
[0098] Preferably, the touch surface has a micro-roughness as described below by the average roughness value Ra in the range of 0.05 μm to 5 μm, preferably 0.1 μm to 4 μm, more preferably 0.2 μm to 3 μm and still more preferably at least 0.3 μm to 2.5 μm.
[0099] In an advantageous embodiment, the contact surface has a fretting life at 1.0 N according to Song of greater than 7500 cycles, preferably greater than 10000 cycles, more preferably greater than 15000 cycles, even more preferably greater than 20000 cycles, and even more preferably greater than 25000 cycles.
[0100] The above-mentioned contact surface can be produced by means of the method according to the invention described above. Therefore, the present invention also includes a contact surface obtainable by the method according to the invention, wherein an electrochemically deposited dispersion silver layer is arranged on a substrate, and wherein the dispersion silver layer comprises at least one having an average particle size (d 50 ) of finely dispersed solid components.
[0101] The above statements about the electrolyte according to the invention, the method according to the invention and the contact surface according to the invention also apply accordingly to the contact surface obtainable by means of the method according to the invention. Thus, the finely divided solid component can be selected from the solid components mentioned above. As substrates for the contact surface according to the invention, all the aforementioned substrates can be used.
[0102] A further subject matter of the invention relates to the use of the contact surface according to the invention for electrical contacting in a plug connection.
[0103] A further subject matter of the present invention relates to the use of the dispersion silver electrolyte according to the invention for coating substrates by means of rack application and / or roll application.
[0104] Further advantages of the invention are apparent from the following description of preferred exemplary embodiments, which, however, are not to be understood as limiting in any way. All embodiments of the invention can be combined with one another within the scope of the invention. DETAILED DESCRIPTION
[0105] Material
[0106] For the tests, brass sheets from Metaq GmbH (material: CuZn39Pb3) with dimensions of 75 mm x 17 mm x 1 mm were used. The bronze balls used from KUGELPOMPEL HIS-Solutions GmbH (material: CuSn6) had a diameter of 3 mm.
[0107] KCN was purchased from Bücherl and K[Ag(CN)2] from Umicore.
[0108] From Dr.Ing.Max & Co. KG, ELFIT 73, a lustrous silver electrolyte based on KCN / silver potassium cyanide, SLOTOSIL BS 1591, a silver electrolyte based on KCN / silver potassium cyanide, SLOTOSIL BS 1592, a lustrous additive, and ALTIX, a lustrous silver electrolyte based on KCN / silver potassium cyanide, for depositing hard silver layers. Also from Dr. Ing. Max & Co. KG purchased CURUM 11, gloss additive, CURUM 12, wetting agent and antioxidant concentrate AG 111.
[0109] SLOTOSIL SG 1911 and SLOTOSIL SG 1912 are Dr.Ing.Max Additives for KCN / silver potassium cyanide based silver electrolytes for dispersion deposition from SLOTOSIL SG 1911. SLOTOSIL SG 1912 contains alkyl sulfates as dispersion stabilizer additives.
[0110] The graphite used was obtained from Kropfmühl AG. The individual graphite powders had a 50 =3μm (graphite UF1) to d 50 =11.5 μm (graphite EDM-L 98) and also vary in conductivity.
[0111] The sulfide particles used (MoS2, WS2) came from TriboteccgmbH and had a 50 =11μm and d 90 =23μm(MoS2 MOSXF) or d 50 =3μm and d 90 = Average particle size of 6 μm (WS2 WS2).
[0112] Measurement method
[0113] Wear test
[0114] The coated bronze ball is rubbed on the coated brass sheet on the wear test bench. A gravity of 0.3N or 1.0N is applied to the ball. It is rubbed on the coated brass sheet at a distance of 3mm with a selected force at a frequency of 1Hz. This is repeated for 100 cycles. During the test, the friction force is measured using a dynamometer U9C (HBM) and converted into a unitless friction coefficient μ using the normal force. In addition, after each cycle, the contact resistance at the contact between the coated brass sheet and the ball is measured. The measurement of the contact resistance is carried out by a digital multimeter 2750 / E (Keithley) using a four-conductor method.
[0115] Determine the micro-motion life according to Song
[0116] The same test equipment as for the conventional wear test was used for this test. The friction stroke was 50 μm long, the frequency and the normal force were kept at 1 Hz as described in the wear test, and the normal force was 0.3 N to 1.0 N. As a comparison standard, the life I according to Song was used, which is defined as R initial +5mΩ and based on the usual test standards ((Song, J.; Wang, L.; Koch, C. (2013): Correlation of friction and wear properties and life of surface protection layers of electrical contacts. In: Song, J. (Hrsg.): Elektrische und optische Verbindungstechnik 2013. Tagungsband derg MM-Fachtagung. 4. Symposium Connectors). The structure of the test equipment is described according to Song et al. The target amount is 50,000 cycles.
[0117] Measuring micro-roughness (average roughness value Ra)
[0118] The micro-roughness (as average roughness value Ra) was measured by means of an optical measuring method using a confocal microscope μsurfexplorer (manufacturer: nanofocus).
[0119] Determine the solid content
[0120] The solid content (in % by weight) was determined by X-ray diffraction. For this purpose, the X-ray diffraction pattern of the deposited thin layer was recorded using a D8 Advannes Davinci Desigh X-ray diffractometer (Bruker) with a Lynxeye solid detector using Cu Kα radiation. The solid content was determined by Rietfield refinement using the program DIFFRAC plus TOPAS Version 4.2 (Bruker) was used to analyze the corresponding diffraction patterns.
[0121] Determine the diameter of the solid component (d 50 , d 90 )
[0122] The particle diameter and average particle size of the solid components were determined by laser diffraction using the Sympatec Helos instrument. 50 and d 90 value.
[0123] Coating brass sheets and bronze balls
[0124] plating
[0125] The sample bodies were coated with a dispersion silver layer and a pure silver layer to obtain the contact surface. Brass sheets and bronze balls were coated for wear, contact resistance and fretting life tests. The sample bodies were first copper plated and then the parts were covered with a pure silver layer (comparative example, VB) or a dispersion silver layer (inventive example, EB).
[0126] Rinse thoroughly with water between steps.
[0127] Electroplating of brass sheets and bronze balls includes the following steps:
[0128] Steps 1 and 2: Degreasing of the substrate according to known methods; first alkaline degreasing step, at 60°C with ultrasound assistance for 1 minute. Second alkaline electrolytic degreasing step, at room temperature (25°C) for a treatment time of 2 to 3 minutes.
[0129] Step 3: Etch the copper using a sulfuric acid-based, non-complexing agent copper activation bath. The activation was performed at room temperature (25°C) for 0.5 minutes.
[0130] Step 4: Treat with a glossy copper bath to deposit a glossy surface. The glossy copper bath is a cyanide electrolyte. The electrolyte consists of 10 g / L KOH, 115 g / L KCN, 64 g / L CuCN, and 1.5 ml / l of glossy additive CUPRUM 11; 2.5 ml / l of base additive CUPRUM 12 operated at 60°C. The electrolyte has a 2 A / dm 2 For the Trommel variant, the current is 1.25 A / dm 2 .
[0131] Step 5: Pre-silver plating is carried out in a pre-silver plating bath with a cyanide electrolyte with a low silver content (120 g / L KCN, 3.7 g / L K[Ag(CN)2]). The pre-silver plating is carried out at room temperature (25°C). 2A / dm 2 as the cathode current density.
[0132] Step 6: Depositing a pure silver layer (comparative example, VB) or a dispersion silver layer (inventive example, EB).
[0133] The brass sheet is hung on a rack for coating. At the rack plating only the holding portion for the brass sheet is conductive.
[0134] Bronze balls were coated as a barrel plating material. The balls were placed in a sieve basket with a mesh size of 0.8 mm via silver-plated steel balls as a filling material and fixed to the electroplating equipment. The electroplating equipment with a pump was used to deposit the dispersion layer.
[0135] The electrolytes used can be found in Table 1.
[0136] Pure silver layer (VB1, VB2, VB3)
[0137] The brass sheet is moved at a stroke of 0.7 m / min. 2 The deposition was carried out for 22 minutes at a current density of 0.1 A / sheet. The ball was moved in the drum at 12 Upm and the silver layer was deposited at 0.25 A / dm 2 The current density was 1.85 A for 70 balls with about 300 g of filler material and the deposition time was 25 min.
[0138] Coating by dispersion silver layer (EB 1 to EB 6)
[0139] The brass sheet was moved at a stroke of 0.7 m / min, and the dispersion device (ULTRA-TURRAX T25, IKA-WerkegmbH & Co, KG) was set to 5000 Upm for the deposition of Examples EB1 to EB4 and 10000 Upm for the deposition of Examples EB5 to EB6. 2 The deposition was carried out at a current density of 0.23 A / sheet for 22 minutes for EB1 to EB4, and for 20 minutes for EB5 and EB6.
[0140] The ball is moved in the drum at 2 Upm and the silver layer is moved at 0.50 A / dm 2 The current density was deposited for 13 minutes (4.1 A for 70 balls with about 300 g of filling material).
[0141] Step 7: Antioxidant post-treatment; Antioxidant protector 160 mL / L of antioxidant concentrate AG 111 was used at 50°C and pH 5.3. The coated sample body was immersed in the antioxidant protector for 2 minutes. Then rinsed with deionized water and dried.
[0142] Table 1 lists the compositions of the pure silver bath and the dispersion silver bath.
[0143] Table 1: Composition of pure silver bath and dispersion silver bath
[0144]
[0145] The results of the wear and fretting tests are shown in Table 2. In addition, the contact resistance of the surface after 100 cycles is shown. The micro-roughness of the surface was likewise determined in the form of the average roughness value Ra. The graphite content of the graphite-containing dispersion silver layer was also measured.
[0146] Table 2: Measurement values
[0147]
[0148] nb: Unsure
[0149] The dispersion silver layers EB1 to EB4 with graphite or the dispersion silver layers EB5 and EB6 with disulfide are a great improvement. In the wear test at 0.3N and 100 cycles, these layers maintain a friction coefficient below 0.4, while the pure silver layers according to examples VB1 to VB3 have at least a significantly higher friction coefficient. The electrical contact resistance of the dispersion silver layers remains below 1.0 mΩ, while the contact resistance in the pure silver layers is higher, even above 2.5 mΩ in VB2.
[0150] Wear tests at 1.0 N and 100 cycles show that the dispersion silver layers with graphite and disulfide have very low friction coefficients even after 100 cycles. The conductivity of these dispersion silver layers is even slightly higher than that of pure silver layers.
[0151] The fretting test at 1.0 N showed that the graphite silver layers according to Examples 1, 3, 4 and 6 (EB1, EB3, EB4 and EB6) according to the present invention were superior to the pure silver layers of Comparative Examples 1 to 3 (VB1 to VB3).
[0152] It can be seen that the dispersion silver layers of Examples EB1 to EB6 according to the invention have completely good properties, especially a combination of low friction coefficient, low contact resistance and high fretting resistance. No comparative example shows a combination of advantageous properties.
[0153] Furthermore, it has been shown that contact surfaces having a content of graphite or metal sulfide particles, ie a solids content of more than 3.0% by weight, based on the total weight of the dispersion silver layer, show very good results.
Claims
1. A silver electrolyte for depositing a silver layer on a substrate, comprising a) potassium silver cyanide with a content of at least 50 g / L, b) potassium cyanide with a content of at least 100 g / L, c) at least one grain refiner having a content of 0.2 to 10 g / L; d) at least one dispersant having a content of 1 to 10 g / L; e) at least one solid component having a content of 1 to 150 g / L, The particles of the solid component have an average particle size of 1 μm to 20 μm. 50 ; The grain refiner is SLOTOSIL SG 1911; Wherein the at least one dispersant comprises a sodium alkyl sulfate having an unsubstituted or selectively substituted C1-C20 alkyl group.
2. The silver electrolyte according to claim 1, wherein at least one solid component is selected from a. graphite, graphite fluoride, graphite oxide, diamond, Al2O3 coated graphite or mixtures thereof; or b. MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3 coated MoS2 and Al2O3 coated WS2 or mixtures thereof; or c. MoS2, WS2, SnS2, NbS2, TaS2, graphite, graphite fluoride, graphite oxide, hexagonal boron nitride, silver niobium selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, diamond, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or their mixtures.
3. A method for depositing a dispersion silver layer on a substrate, comprising the following steps, a) providing the silver electrolyte according to claim 1 or 2, b) introducing a substrate into the silver electrolyte, and c) performing deposition.
4. The method according to claim 3, wherein the temperature in step c) is 15°C to 25°C, and / or wherein the current density in step c) is 0.05 A / dm 2 Up to 1.0A / dm 2 .
5. The method according to claim 3 or 4, wherein the method is barrel plating and / or rack plating.
6. A contact surface obtained according to the method according to any one of claims 3 to 5, wherein an electrochemically deposited dispersion silver layer is arranged on the substrate, The dispersion silver layer comprises particles of at least one finely divided solid component having an average particle size d of 1 μm to 20 μm. 50 ; wherein the dispersion silver layer comprises the at least one finely divided solid component in an amount ranging from 3.1 wt % to 15 wt %, based on the total weight of the dispersion silver layer; wherein the dispersion silver layer has a friction coefficient μ of less than 1.4 after 100 cycles at 0.3 N; The contact resistance is less than 1.0 mΩ after 100 cycles at 1.0 N. and The dispersion silver layer has a friction coefficient μ of less than 1.0 at 1.0 N after 100 cycles.
7. The contact surface according to claim 6, wherein at least one finely divided solid component is selected from a. MoS2, WS2, SnS2, NbS2, TaS2, hexagonal boron nitride, silver niobium-selenide, TiN, Si3N4, TiB2, WC, TaC, B4C, Al2O3, ZrO2, cubic BN, MoSe2, WSe2, TaSe2, NbSe2, SiC, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof; or b. graphite, graphite fluoride, graphite oxide, diamond, Al2O3 coated graphite or mixtures thereof; or c. MoS2, WS2, SnS2, graphite, graphite oxide, graphite fluoride, hexagonal boron nitride, silver niobium-selenide, SiC, Al2O3-coated graphite, Al2O3-coated MoS2 and Al2O3-coated WS2 or mixtures thereof.
8. The contact surface according to claim 6, wherein the at least one finely divided solid component is selected from graphite, MoS2, WS2 or mixtures thereof.
9. Use of a contact surface according to any one of claims 6 to 8 for electrical contacting in a plug connection.
10. Use of the dispersion silver electrolyte according to claim 1 or 2 for coating substrates by means of rack application and / or roll application.
Citation Information
Patent Citations
Component with a layer in which CNTs (carbon nanotubes) are embedded and methods for its production
DE102008030988B4
Contact surface e.g. for motor vehicle electrical contacts in engine bay, has silver layer with finely dispersed graphite particles
DE10346206A1
Cyanide silver electrolyte and process for the galvanic deposition of silver-graphite dispersion coatings and its application
DE2543082A1
Electrodeposition of silver with fluoropolymer nanoparticles
CN105229204A
Functional coating of pure silver layer / pure-graphite composite layer and preparation method of functional coating
CN105297095A