Terminal protection tape and method for manufacturing semiconductor device with electromagnetic wave shielding film
By using a viscoelastic layer on a terminal protection tape that meets specific conditions in semiconductor devices, the problem of short circuits in the circuit when forming electromagnetic wave shielding films for external terminal electrodes is solved, achieving effective burial of terminal electrodes and simplification of processes.
Patent Information
- Application Number
- CN201980052146.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2018-08-08
- Filing Date
- 2019-08-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2039-08-08
AI Technical Summary
In the prior art, when forming electromagnetic wave shielding films, the external terminal electrodes of semiconductor devices are prone to short circuits due to differences in height or shape, and the shielding part setting process is complicated.
A terminal protection tape is used, which has a viscoelastic layer with a tanδ value of 0.2 or higher at 50°C and a thickness of 80 to 800 μm. It satisfies a specific ratio between energy storage modulus and terminal height and is used to form an electromagnetic wave shielding film on a semiconductor device. Through the moderate adhesion and flexibility of the viscoelastic layer, the terminal electrodes can be effectively buried.
Even for terminal electrodes that are prone to floating, such as solder balls, effective burial can be achieved to prevent short circuits, simplify the process, and avoid complex shielding setups.
Smart Images

Figure CN112585742B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a terminal protection tape and a method for producing a semiconductor device with an electromagnetic wave shielding film using the terminal protection tape.
[0002] This application claims priority based on Japanese Patent Application No. 2018-149699 filed in Japan on August 8, 2018, and uses the contents thereof herein. Background Art
[0003] Conventionally, when mounting a multi-pin LSI package for an MPU or gate array on a printed wiring board, a semiconductor device having a plurality of electronic components has been used in which a protruding electrode (hereinafter referred to as a "terminal" in this specification) made of eutectic solder, high-temperature solder, gold, etc. is formed on its connection pad. In addition, a mounting method is adopted in which these terminals are brought into contact with corresponding terminal portions on a chip mounting substrate to perform melting / diffusion bonding.
[0004] With the popularization of personal computers, the Internet has also become common. Now, smartphones and tablet terminals can also be connected to the Internet. The use of wireless communication technology to transmit digital images, music, photos, text information, etc. through the Internet is increasing. In turn, IoT (Internet of Things) is also becoming popular, which will bring innovative changes to the packaging technology of semiconductor devices such as sensors, RFID (Radio frequency identifier), MEMS (Micro Electro Mechanical Systems), and wireless components used in various application fields such as home appliances and automobiles to make them more intelligent.
[0005] As electronic devices continue to evolve, the requirements for semiconductor devices are increasing year by year. In particular, heat dissipation and noise suppression are two important points in order to meet the needs of high performance, miniaturization, high integration, low power consumption, and low cost.
[0006] In response to such heat dissipation and noise suppression measures, a method of forming a shielding layer by covering the electronic component module with a conductive material is adopted, as disclosed in Patent Document 1. In Patent Document 1, a conductive resin applied to the top and side surfaces of a singulated electronic component module is heated and cured to form a shielding layer.
[0007] As a method of forming a shield layer by covering a semiconductor device with terminals with a conductive material, methods such as sputtering, ion plating, and spraying are also known.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2011-151372 Summary of the invention
[0011] Technical Problems to be Solved by the Invention
[0012] In the method for manufacturing an electronic component disclosed in Patent Document 1, a conductive resin is applied to an external terminal electrode provided on the back side of an assembly substrate in a state where the external terminal electrode is buried in an adhesive sheet. Since a shielding portion is provided at a predetermined position of the adhesive sheet, a short circuit between the external terminal electrode and the electromagnetic wave shielding film can be prevented.
[0013] However, depending on the height or shape of the external terminal electrode, the external terminal electrode may not be fully buried in the adhesive sheet, resulting in a short circuit between the external terminal electrode and the electromagnetic wave shielding film. In addition, the process of providing a shielding portion at a predetermined position of the adhesive sheet is complicated.
[0014] Therefore, the object of the present invention is to provide a terminal protection tape and a method for manufacturing a semiconductor device with an electromagnetic wave shielding film using the terminal protection tape. The terminal protection tape is a terminal protection tape used in the process of forming an electromagnetic wave shielding film on a semiconductor device with terminals, and can bury terminal electrodes that have bumps and are prone to floating, such as solder balls.
[0015] Technical means to solve technical problems
[0016] That is, the present invention provides the following terminal protection tape and a method for producing a semiconductor device with an electromagnetic wave shielding film using the terminal protection tape.
[0017] [1] A terminal protection tape used in a process of forming an electromagnetic wave shielding film on a semiconductor device with terminals,
[0018] It has a viscoelastic layer.
[0019] In a dynamic viscoelasticity measurement of the viscoelastic layer, a tan δ value at 50° C. is 0.2 or more, and a thickness of the viscoelastic layer is 80 to 800 μm.
[0020] [2] The terminal protection tape according to [1], wherein the storage modulus G'(50°C) (MPa) of the viscoelastic layer at 50°C, the height h0 (μm) of the terminal, and the thickness d1 (μm) of the viscoelastic layer satisfy the following equations (1) and (2).
[0021] 0.01MPa≤G'(50℃)≤15MPa···(1)
[0022] 1.2≤d1 / h0≤5.0···(2)
[0023] [3] The terminal protection tape according to [1] or [2], wherein the storage modulus G'(25°C) (MPa) of the viscoelastic layer at 25°C satisfies the following formula (3).
[0024] 0.05MPa≤G'(25℃)≤20MPa···(3)
[0025] [4] The terminal-protecting tape according to any one of [1] to [3], wherein the viscoelastic layer includes a embedding layer and an adhesive layer.
[0026] [5] The terminal protection tape according to [4], comprising the adhesive layer, the embedding layer, and a substrate in this order.
[0027] [6] The terminal protection tape according to [5], which is a double-sided tape having the adhesive layer, the embedding layer, the substrate, and a second adhesive layer in this order.
[0028] [7] A method for manufacturing a semiconductor device with an electromagnetic wave shielding film, comprising:
[0029] A step of embedding the terminals of the semiconductor device with terminals in the viscoelastic layer of the terminal protection tape described in any one of [1] to [6]; and
[0030] The step of forming an electromagnetic wave shielding film on an exposed surface of the semiconductor device with terminals which is not embedded in the viscoelastic layer of the terminal protection tape.
[0031] [8] A method for manufacturing a semiconductor device with an electromagnetic wave shielding film, comprising:
[0032] A step of embedding the terminals of the semiconductor device assembly with terminals in the viscoelastic layer of the terminal protection tape according to any one of [1] to [6];
[0033] The step of cutting the semiconductor device assembly with terminals to form semiconductor devices with terminals in which the terminals are buried in the viscoelastic layer of the terminal protection tape; and
[0034] The step of forming an electromagnetic wave shielding film on an exposed surface of the semiconductor device with terminals which is not embedded in the viscoelastic layer of the terminal protection tape.
[0035] Effects of the Invention
[0036] According to the present invention, a terminal protection tape and a method for manufacturing a semiconductor device with an electromagnetic wave shielding film using the terminal protection tape can be provided. The terminal protection tape is a terminal protection tape used in the process of forming an electromagnetic wave shielding film on a semiconductor device with terminals, and can bury terminal electrodes that are prone to floating, such as solder balls. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 This is a cross-sectional view schematically showing one embodiment of the terminal protection tape of the present invention.
[0038] Figure 2 This is a cross-sectional view schematically showing another embodiment of the terminal protection tape of the present invention.
[0039] Figure 3 This is a cross-sectional view schematically showing another embodiment of the terminal protection tape of the present invention.
[0040] Figure 4 This is a cross-sectional view schematically showing another embodiment of the terminal protection tape of the present invention.
[0041] Figure 5 This is a cross-sectional view schematically showing one embodiment of a method for manufacturing a semiconductor device with an electromagnetic wave shielding film according to the present invention.
[0042] Figure 6 This is a cross-sectional view schematically showing another embodiment of the method for manufacturing a semiconductor device with an electromagnetic wave shielding film according to the present invention.
[0043] Figure 7 It is a cross-sectional view schematically showing an example of a method for manufacturing a semiconductor device with an electromagnetic wave shielding film according to a comparative example. DETAILED DESCRIPTION
[0044] Figure 1 The cross-sectional view schematically shows an embodiment of the terminal protection tape of the present invention. In addition, in order to facilitate understanding of the features of the present invention, for convenience, important parts of the figures used in the following description are sometimes enlarged and displayed, and the dimensional ratios of the various components are not necessarily the same as the actual ones.
[0045] Figure 1 The terminal protection tape 1 shown is a terminal protection tape 1 used in the process of forming an electromagnetic wave shielding film on a semiconductor device with terminals, and has a viscoelastic layer 12 composed of a embedding layer 13 and an adhesive layer 14. In the dynamic viscoelasticity measurement of the viscoelastic layer 12, the tanδ value at 50°C is 0.2 or more, and the thickness of the viscoelastic layer 12 is 80 to 800 μm.
[0046] like Figure 1 As shown, the terminal protection tape of this embodiment may include a release film 21 on the outermost layer of the viscoelastic layer 12 on the embedding layer 13 side, or may include a release film 20 on the outermost layer of the viscoelastic layer 12 on the adhesive layer 14 side.
[0047] The terminal protection tape of this embodiment is not limited to Figure 1 The terminal protection tape shown in the figure can be used for the terminal protection tape without damaging the effect of the present invention. Figure 1 Some of the configurations of the terminal protection tapes shown are changed, deleted, or added.
[0048] Figure 1 The terminal protection tape 1 shown can be used in the following process: the two release films 20 and 21 are peeled off, placed on a support, and the semiconductor device with terminals is pressed from above with the terminal side facing downward, the terminals are buried in the viscoelastic layer 12, and an electromagnetic wave shielding film is further formed thereon. In the dynamic viscoelasticity measurement of the viscoelastic layer 12, since the tanδ value at 50°C is 0.2 or more and the thickness of the viscoelastic layer 12 is 80 to 800 μm, when the terminals of the semiconductor device with terminals are buried in the viscoelastic layer 12, even terminal electrodes with bumps and easy to float, such as solder balls, can be buried, and the terminal forming surface of the semiconductor device with terminals as the target can be made to be closely attached to the viscoelastic layer 12. As a result, the terminal electrode and the electromagnetic wave shielding film can be prevented from short-circuiting, and there is no need to set a shielding part with a complicated process.
[0049] like Figure 2 As shown in the terminal protection tape 2 , the terminal protection tape of this embodiment may have a structure having an adhesive layer 14 , a embedding layer 13 and a substrate 11 in sequence, and may also have a release film 20 on the outermost layer on the adhesive layer 14 side of the viscoelastic layer 12 .
[0050] Figure 2 The terminal protection tape 2 shown can be used in the following process: the release film 20 is peeled off, the semiconductor device with terminals is pressed onto the viscoelastic layer 12 on the substrate 11 as a support body with the terminal side facing downward, the terminals are buried in the viscoelastic layer 12, and an electromagnetic wave shielding film is further formed thereon. In the dynamic viscoelasticity measurement of the viscoelastic layer 12, since the tanδ value at 50°C is 0.2 or more and the thickness of the viscoelastic layer 12 is 80 to 800 μm, when the terminals of the semiconductor device with terminals are buried in the viscoelastic layer 12, even terminal electrodes with unevenness and easy to float, such as solder balls, can be buried, and the terminal forming surface of the semiconductor device with terminals as the target can be made to be closely attached to the viscoelastic layer 12. As a result, the terminal electrode and the electromagnetic wave shielding film can be prevented from short-circuiting, and there is no need to set a shielding part with a complicated process.
[0051] like Figure 3 As shown in the terminal protection tape 3, the terminal protection tape of this embodiment can be a structure having an adhesive layer 14, a burying layer 13 and a substrate 11 in sequence, and can also have a release film 20 on the outermost layer on the adhesive layer 14 side of the viscoelastic layer 12, and can also have a second adhesive layer 15 (i.e., a bonding adhesive layer) for attaching to a support body on the side of the substrate 11 opposite to the viscoelastic layer 12, and can also be a double-sided tape having a release film 22 on the outermost layer on the second adhesive layer 15 side.
[0052] Figure 3 The terminal protection tape 3 shown can be used in the following process: peeling off the peeling film 22, such as Figure 4 The semiconductor device with terminals is fixed to the support 30 as shown, and the release film 20 is further peeled off, and the semiconductor device with terminals is pressed to the viscoelastic layer 12 with the terminal side facing downward, and the terminals are buried in the viscoelastic layer 12, and an electromagnetic wave shielding film is further formed thereon. In the dynamic viscoelasticity measurement of the viscoelastic layer 12, since the tanδ value at 50°C is 0.2 or more and the thickness of the viscoelastic layer 12 is 80 to 800μm, when the terminals of the semiconductor device with terminals are buried in the viscoelastic layer 12, even terminal electrodes that are prone to floating, such as solder balls, can be buried, and the terminal forming surface of the semiconductor device with terminals as the target can be made to be closely attached to the viscoelastic layer 12. As a result, a circuit short circuit between the terminal electrode and the electromagnetic wave shielding film can be prevented, and there is no need to set a shielding part with a complicated process.
[0053] Next, each layer constituting the terminal protection tape according to the present embodiment will be described.
[0054] ◎Viscoelastic layer
[0055] In the terminal protection tape of the present embodiment, the viscoelastic layer can be used to protect the terminal forming surface (in other words, the circuit surface) of a semiconductor device with terminals and the terminals arranged on the terminal forming surface. In the dynamic viscoelasticity measurement of the viscoelastic layer, the tanδ value at 50°C is greater than 0.2, and the thickness of the viscoelastic layer is 80 to 800 μm.
[0056] In the dynamic viscoelasticity measurement of the viscoelastic layer, by making the tanδ value at 50°C to be 0.2 or more and the thickness of the viscoelastic layer to be 80 to 800 μm, even for terminal electrodes of various shapes and sizes such as solder balls that are prone to floating, they can be buried using the appropriate viscosity of the viscoelastic layer. In addition, it is preferred that the viscoelastic layer has a buried layer and an adhesive layer. By making the viscoelastic layer have a buried layer and an adhesive layer, it is easy to achieve the above-mentioned appropriate dynamic viscoelasticity, and appropriate adhesion can be given to the terminal forming surface and the terminal.
[0057] In the present specification, "tan δ of the viscoelastic layer at 50°C" can be obtained by dividing the loss modulus G" (50°C) of the viscoelastic layer at 50°C by the storage modulus G' (50°C). In addition, "tan δ of the viscoelastic layer at 25°C" described later can be obtained by dividing the loss modulus G" (25°C) of the viscoelastic layer at 25°C by the storage modulus G' (25°C).
[0058] In the present specification, the "loss modulus G" and "storage modulus G'" of the viscoelastic layer can be obtained by measuring the viscoelastic layer from room temperature to 100°C using a shear viscosity measuring device under the measuring conditions of a frequency of 1 Hz and a heating rate of 10°C / min.
[0059] Therefore, in the dynamic viscoelasticity measurement of the viscoelastic layer, the tanδ value at 50°C must be 0.2 or more, preferably 0.3 or more, and more preferably 0.5 or more. By making the tanδ value at 50°C above the lower limit, the followability of the terminal electrode and the fluidity of the viscoelastic layer can be ensured, so the embedding property (hereinafter also referred to as the embedding property) of the terminal electrode can be improved. The tanδ value at 50°C can be set to 3.5 or less, 3.0 or less, or 2.5 or less.
[0060] The upper limit value and the lower limit value of tan δ at 50° C. may be arbitrarily combined.
[0061] For example, tan δ at 50° C. is preferably 0.2 to 3.5, more preferably 0.3 to 3.0, and even more preferably 0.5 to 2.5.
[0062] The thickness of the viscoelastic layer must be 80 to 800 μm, preferably 100 to 790 μm, and more preferably 130 to 780 μm.
[0063] By making the thickness of the viscoelastic layer greater than the lower limit, even terminal electrodes that are prone to floating, such as solder balls, can be buried. In addition, by making the thickness of the buried layer less than the upper limit, the terminal protection tape can be prevented from becoming too thick.
[0064] Here, “the thickness of the viscoelastic layer” refers to the thickness of the entire viscoelastic layer, and the thickness of the viscoelastic layer composed of a plurality of embedding layers and adhesive layers refers to the total thickness of the embedding layers and adhesive layers.
[0065] In the present specification, the “thickness of a layer” may be a value represented by an average value of thicknesses measured at five randomly selected locations, and is measured using a constant pressure thickness measuring device in accordance with JIS K77130.
[0066] It is preferred that the storage modulus G′(50° C.) (MPa) of the viscoelastic layer at 50° C. satisfies the following formula (1).
[0067] 0.01MPa≤G'(50℃)≤15MPa···(1)
[0068] By satisfying the formula (1), even terminal electrodes of various shapes and sizes such as solder balls that are prone to floating can be buried more easily.
[0069] G'(50°C) is preferably 0.01 to 15 MPa, more preferably 0.02 to 12.5 MPa, and even more preferably 0.03 to 10 MPa.
[0070] It is preferred that the thickness d1 (μm) of the viscoelastic layer and the height h0 (μm) of the terminal satisfy the following formula (2).
[0071] 1.2≤d1 / h0≤5.0···(2)
[0072] By satisfying the formula (2), even terminal electrodes of various shapes and sizes such as solder balls that are prone to floating can be buried more easily.
[0073] d1 / h0 is preferably 1.2 to 5.0, more preferably 1.3 to 5.0, and further preferably 1.4 to 5.0.
[0074] In the terminal protection tape of the present embodiment, the storage modulus G′(25° C.) (MPa) of the viscoelastic layer at 25° C. preferably satisfies the following formula (3).
[0075] 0.05MPa≤G'(25℃)≤20MPa···(3)
[0076] By satisfying the formula (3), the shape of the terminal protection tape can be easily maintained at room temperature, and the embedding layer can be easily suppressed from penetrating to the end portion.
[0077] G' (25°C) is preferably 0.05 to 20 MPa, more preferably 0.06 to 15 MPa, and further preferably 0.07 to 10 MPa.
[0078] In the dynamic viscoelasticity measurement of the viscoelastic layer, the tan δ value at 25° C. may be 0.10 to 1.4, preferably 0.20 to 1.0, and more preferably 0.30 to 0.8.
[0079] When the terminal-forming surface of the semiconductor device with terminals is brought into close contact with the viscoelastic layer 12 , it is preferable to bring the terminal-forming surface of the semiconductor device with terminals into close contact directly with the adhesive layer 14 of the viscoelastic layer 12 .
[0080] At this time, in order to prevent adhesive residue on the terminal forming surface and the terminals, the adhesive layer 14 is preferably set to be harder than the embedding layer 13 .
[0081] 0Buried layer
[0082] In the terminal protection tape of the present embodiment, the embedding layer refers to a layer in the viscoelastic layer that embeds and protects the terminals of the semiconductor device with terminals.
[0083] The embedding layer is in sheet or film form, and its constituent material is not particularly limited as long as the above-mentioned conditions are satisfied. In this specification, "sheet or film form" means a thin film with small thickness variation within a plane and flexibility.
[0084] For example, when the purpose is to suppress deformation of the viscoelastic layer caused by the viscoelastic layer covering the terminal forming surface of a semiconductor device with terminals to be protected reflecting the shape of the terminals existing on the semiconductor surface, preferred constituent materials of the buried layer, from the perspective of further improving the adhesion of the buried layer, include urethane (meth) acrylate resins, acrylic resins, and the like.
[0085] The embedding layer may be a single layer or a plurality of layers of two or more. When the embedding layer is a plurality of layers, the plurality of layers may be the same as or different from each other, and the combination of the plurality of layers is not particularly limited.
[0086] In addition, in this specification, not limited to the case of buried layers, "multiple layers may be the same as or different from each other" means "all the layers may be the same, all the layers may be different, or only some of the layers may be the same", and "multiple layers are different from each other" means "at least one of the constituent materials and thicknesses of each layer is different from each other".
[0087] The thickness of the buried layer can be appropriately adjusted according to the height of the terminal on the terminal forming surface of the semiconductor device with the terminal to be protected within the range of 80 to 800 μm of the thickness of the viscoelastic layer, but from the point of view of being able to easily absorb the influence of the terminal with a higher height, it is preferably 50 to 600 μm, more preferably 70 to 550 μm, and particularly preferably 80 to 500 μm. By making the thickness of the buried layer above the lower limit, a viscoelastic layer with higher terminal protection performance can be formed. In addition, by making the thickness of the buried layer below the upper limit, productivity and winding suitability in a roll shape are improved.
[0088] Here, “the thickness of the buried layer” refers to the thickness of the entire buried layer. For example, the thickness of a buried layer composed of a plurality of layers refers to the total thickness of all the layers constituting the buried layer.
[0089] The embedding layer preferably has a soft property suitable for embedding the terminals, and is preferably softer than the adhesive layer.
[0090] (Composition for forming buried layer)
[0091] The embedding layer can be formed using a embedding layer forming composition containing its constituent materials.
[0092] For example, a buried layer forming composition is applied to the surface on which the buried layer is to be formed, dried as required, and cured by irradiation with energy rays, thereby forming a buried layer at a target location. In addition, a buried layer forming composition is applied to a release film, dried as required, and cured by irradiation with energy rays, thereby forming a buried layer of a target thickness, and the buried layer can be transferred to a target location. A more specific method for forming the buried layer will be described in detail later together with the method for forming other layers. The content ratio of the components that do not vaporize at room temperature in the buried layer forming composition is generally the same as the content ratio of the components of the buried layer. Here, "normal temperature" refers to a temperature that is not particularly cooled or heated, that is, a normal temperature, for example, a temperature of 15 to 30°C.
[0093] The embedding layer forming composition can be applied using a known method, for example, methods using various coaters such as an air knife coater, a blade coater, a rod coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a knife coater, a screen coater, a Meyer rod coater, and a kiss coater.
[0094] The drying conditions of the embedding layer forming composition are not particularly limited. When the embedding layer forming composition contains a solvent described below, it is preferably dried by heating. In this case, the drying is preferably performed at 70 to 130° C. for 10 seconds to 5 minutes, for example.
[0095] When the embedding layer forming composition has energy ray curability, it is preferably cured by irradiation with energy rays.
[0096] Examples of the embedding layer forming composition include a embedding layer forming composition (I) containing an acrylic resin.
[0097] {Burying layer forming composition (I)}
[0098] The embedding layer forming composition (I) contains an acrylic resin.
[0099] As the composition (I) for forming a buried layer, a composition containing an adhesive resin (I-1a) which is an acrylic resin in the first adhesive composition (I-1) described later and an energy-ray-curable compound, or a composition containing an energy-ray-curable adhesive resin (1-2a) in which an unsaturated group is introduced into the side chain of the adhesive resin (I-1a) which is an acrylic resin in the first adhesive composition (I-2) can be used as the composition (I) for forming a buried layer.
[0100] The adhesive resin (I-1a) and the energy-ray curable compound used in the embedding layer forming composition (I) are the same as those described for the adhesive resin (I-1a) and the energy-ray curable compound used in the first adhesive composition (I-1) described later.
[0101] The adhesive resin (I-2a) used in the embedding layer forming composition (I) is the same as the adhesive resin (I-2a) used in the first adhesive composition (I-2) described later.
[0102] The embedding layer forming composition (I) preferably further contains a crosslinking agent. The crosslinking agent used in the embedding layer forming composition (I) is the same as the crosslinking agent used in the first adhesive composition (I-1) and the first adhesive composition (I-2) described below.
[0103] The embedding layer forming composition (I) may further contain a photopolymerization initiator and other additives. The photopolymerization initiator and other additives used in the embedding layer forming composition (I) are the same as those described in the first adhesive composition (I-1) and the first adhesive composition (I-2) described later.
[0104] The embedding layer forming composition (I) may contain a solvent. The solvent used in the embedding layer forming composition (I) is the same as the solvent used in the first adhesive composition (I-1) and the first adhesive composition (I-2) described below.
[0105] By adjusting either or both of the molecular weight of the adhesive resin (I-1a) and the molecular weight of the energy-ray curable compound in the embedding layer forming composition (I), the embedding layer can be designed to have a flexible property suitable for embedding the terminal.
[0106] Furthermore, by adjusting the content of the crosslinking agent in the embedding layer forming composition (I), the embedding layer can be designed to have a soft property suitable for embedding a terminal.
[0107] <<Method for preparing composition for forming buried layer>>
[0108] The embedding layer forming composition such as the embedding layer forming composition (I) can be obtained by blending the respective components constituting the composition.
[0109] The order of adding the components when blending them is not particularly limited, and two or more components may be added simultaneously.
[0110] When a solvent is used, the solvent may be mixed with any blending components other than the solvent to dilute the blending components in advance and then used, or the solvent may be mixed with the blending components without diluting the blending components in advance and then used.
[0111] The method for mixing the components during blending is not particularly limited, and may be appropriately selected from the following known methods: a method of mixing by rotating a stirring bar or a stirring blade, a method of mixing using a mixer, a method of mixing by applying ultrasonic waves, and the like.
[0112] The temperature and time for adding and mixing the components are not particularly limited as long as the components do not deteriorate, and may be appropriately adjusted. However, the temperature is preferably 15 to 30°C.
[0113] [Composition of buried layer]
[0114] The composition of the embedding layer in the present embodiment is a composition obtained by removing the solvent from the above-mentioned embedding layer forming composition (I).
[0115] When the embedding layer forming composition (I) is a composition containing an adhesive resin (I-1a) as an acrylic resin in the first adhesive composition (I-1) described later and an energy-ray curable compound, the content ratio of the adhesive resin (I-1a) as an acrylic resin in the embedding layer (1) relative to the total mass of the embedding layer (1) is preferably 50 to 99% by mass, more preferably 55 to 95% by mass, and further preferably 60 to 90% by mass. As another aspect of the present invention, the content ratio of the adhesive resin (I-1a) as an acrylic resin relative to the total mass of the embedding layer (1) can be 45 to 90% by mass, or 50 to 85% by mass. In addition, the content ratio of the energy-ray curable compound relative to the total mass of the embedding layer (1) is preferably 0.5 to 50% by mass, and further preferably 5 to 45% by mass. When the embedding layer (1) contains a crosslinking agent, the content of the crosslinking agent relative to the total mass of the embedding layer (1) is preferably 0.1 to 10 mass %, more preferably 0.2 to 9 mass %, and even more preferably 0.3 to 8 mass %.
[0116] When the embedding layer forming composition (I) is a composition containing an energy-ray-curable adhesive resin (1-2a) having an unsaturated group introduced into the side chain of an adhesive resin (I-1a) as an acrylic resin, the content ratio of the energy-ray-curable adhesive resin (1-2a) having an unsaturated group introduced into the side chain in the embedding layer (2) is preferably 10 to 70% by mass, more preferably 15 to 65% by mass, and further preferably 20 to 60% by mass relative to the total mass of the embedding layer. When the embedding layer (2) contains a crosslinking agent, the content ratio of the crosslinking agent relative to the total mass of the embedding layer (2) is preferably 0.1 to 10% by mass, more preferably 0.2 to 9% by mass, and further preferably 0.3 to 8% by mass. The embedding layer (2) of the present embodiment may further contain the adhesive resin (I-1a) as the acrylic resin. At this time, the content ratio of the adhesive resin (I-1a) as an acrylic resin relative to the total mass of the embedding layer (2) is preferably 45 to 95 mass%, more preferably 50 to 90 mass%, and further preferably 55 to 85 mass%. In addition, as another aspect of the present invention, the content ratio of the adhesive resin (I-1a) as an acrylic resin relative to the total mass of the embedding layer (2) can be 25 to 80 mass%, can also be 30 to 75 mass%, and can also be 35 to 70 mass%. In addition, when the embedding layer (2) of this embodiment further contains the adhesive resin (I-1a) as an acrylic resin, the content of the adhesive resin (1-1a) is preferably 100 to 200 mass parts, more preferably 110 to 180 mass parts, and further preferably 120 to 170 mass parts relative to 100 mass parts of the adhesive resin (1-2a).
[0117] The composition of the adhesive resin (I-1a) as an acrylic resin contained in the embedding layer (1), the energy-ray-curable compound, and the energy-ray-curable adhesive resin (1-2a) with an unsaturated group introduced into the side chain of the adhesive resin (I-1a) contained in the embedding layer (2) can be the same as the description of the adhesive resin (I-1a) as an acrylic resin, the energy-ray-curable compound, and the energy-ray-curable adhesive resin (1-2a) with an unsaturated group introduced into the side chain of the adhesive resin (I-1a) used in the first adhesive composition (I-1) described later.
[0118] In this embodiment, the embedding layer (2) comprising an adhesive resin (1-2a), an adhesive resin (1-1a), and a cross-linking agent is preferred. At this time, the adhesive resin (1-1a) is preferably an acrylic polymer having a structural unit from an alkyl (meth)acrylate and a unit from a carboxyl-containing monomer. In addition, the adhesive resin (1-2a) is preferably an acrylic polymer obtained by reacting an unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group with an acrylic polymer having a structural unit from an alkyl (meth)acrylate and a unit from a hydroxyl-containing monomer. The cross-linking agent can use the compounds exemplified in the first adhesive composition (I-1) described later, and toluene diisocyanate is particularly preferred.
[0119] The content ratio of the structural unit derived from the (meth) alkyl ester to the total mass of the adhesive resin (1-1a) is preferably 75 to 99 mass%, more preferably 80 to 98 mass%, and further preferably 85 to 97 mass%. As another aspect of the present invention, the content ratio of the structural unit derived from the (meth) alkyl ester to the total mass of the adhesive resin (1-1a) may be 70 to 95 mass%, or 80 to 95 mass%. The content ratio of the structural unit of the carboxyl group-containing monomer to the total mass of the adhesive resin (1-1a) is preferably 1.0 to 30 mass%, more preferably 2.0 to 25 mass%, and further preferably 3.0 to 20 mass%. As another aspect of the present invention, the content ratio of the structural unit of the carboxyl group-containing monomer to the total mass of the adhesive resin (1-1a) may be 3.0 to 20 mass%, or 5.0 to 15 mass%. The number of carbon atoms of the alkyl group of the (meth) alkyl ester in the adhesive resin (1-1a) is preferably 4 to 12, and more preferably 4 to 8. In addition, in the adhesive resin (1-1a), alkyl acrylate is preferred. Among them, the alkyl (meth)acrylate is particularly preferably n-butyl acrylate. In addition, as the carboxyl group-containing monomer in the adhesive resin (1-1a), ethylenically unsaturated monocarboxylic acids, ethylenically unsaturated dicarboxylic acids, anhydrides of ethylenically unsaturated dicarboxylic acids, etc. can be listed, among which ethylenically unsaturated monocarboxylic acids are preferred, (meth)acrylic acid is more preferred, and acrylic acid is particularly preferred.
[0120] The weight average molecular weight of the adhesive resin (1-1a) according to the present embodiment is preferably 100,000 to 800,000, more preferably 150,000 to 700,000, and even more preferably 200,000 to 600,000.
[0121] In addition, in this specification, unless otherwise specified, "weight average molecular weight" means a polystyrene conversion value measured by gel permeation chromatography (GPC) method.
[0122] The content ratio of the structural unit derived from the (meth)acrylic acid alkyl ester relative to the total mass of the adhesive resin (1-2a) is preferably 1.0 to 95% by mass, more preferably 2.0 to 90% by mass, and further preferably 3.0 to 85% by mass. The content ratio of the unit derived from the hydroxyl-containing monomer relative to the total mass of the adhesive resin (1-2a) is preferably 1.0 to 50% by mass, more preferably 2.0 to 45% by mass, and further preferably 3.0 to 40% by mass. The number of carbon atoms of the alkyl group of the (meth)acrylic acid alkyl ester in the adhesive resin (1-2a) is preferably 1 to 12, and further preferably 1 to 4. The adhesive resin (1-2a) preferably has two or more structural units derived from the (meth)acrylic acid alkyl ester, more preferably has structural units derived from methyl (meth)acrylate and n-butyl (meth)acrylate, and further preferably has structural units derived from methyl methacrylate and n-butyl acrylate. As the hydroxyl-containing monomer in the adhesive resin (1-2a), the hydroxyl-containing monomer exemplified in the first adhesive composition (I-1) described later can be used, and 2-hydroxyethyl acrylate is particularly preferred. As the unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group, the compound exemplified in the first adhesive composition (I-2) described later can be used, and 2-methacryloyloxyethyl isocyanate is particularly preferred. When all hydroxyl groups from the hydroxyl-containing monomer are set to 100 mol, the amount of the unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group is preferably 10 to 150 mol, more preferably 20 to 140 mol, and further preferably 30 to 130 mol.
[0123] The weight average molecular weight of the adhesive resin (1-2a) of the present embodiment is preferably 10,000 to 500,000, more preferably 20,000 to 400,000, and even more preferably 30,000 to 300,000.
[0124] 〇Adhesive layer
[0125] Hereinafter, in order to distinguish it from the second adhesive layer for bonding to a support body described later, the adhesive layer constituting the viscoelastic layer may be referred to as a "first adhesive layer".
[0126] The first adhesive layer is in a sheet or film shape and contains an adhesive.
[0127] Examples of the adhesive include adhesive resins such as acrylic resins (adhesives formed from resins having a (meth)acryloyl group), urethane resins (adhesives formed from resins having urethane bonds), rubber resins (adhesives formed from resins having rubber structures), silicone resins (adhesives formed from resins having siloxane bonds), epoxy resins (adhesives formed from resins having epoxy groups), polyvinyl ethers, and polycarbonates, among which acrylic resins are preferred.
[0128] In addition, in the present invention, "adhesive resin" is a concept that includes both resins having adhesiveness and resins having adhesion. For example, it includes not only resins having adhesiveness itself, but also resins that exhibit adhesiveness by using other components such as additives, or resins that exhibit adhesiveness by the presence of triggers such as heat or water.
[0129] The first adhesive layer may be only one layer (single layer) or may be two or more layers. When it is a plurality of layers, the plurality of layers may be the same as or different from each other, and the combination of the plurality of layers is not particularly limited.
[0130] The thickness of the first adhesive layer is preferably 1 to 800 μm, more preferably 2 to 100 μm, and particularly preferably 8 to 20 μm.
[0131] Here, “the thickness of the first adhesive layer” refers to the thickness of the entire first adhesive layer. For example, the thickness of the first adhesive layer composed of a plurality of layers refers to the total thickness of all layers constituting the first adhesive layer.
[0132] The first adhesive layer may be formed using an energy-ray-curable adhesive or a non-energy-ray-curable adhesive. The first adhesive layer formed using an energy-ray-curable adhesive can easily adjust the physical properties before and after curing.
[0133] In the present invention, "energy rays" refer to rays having energy particles among electromagnetic waves or charged particle beams, and examples thereof include ultraviolet rays and electron beams.
[0134] The ultraviolet rays can be irradiated by using, for example, a high pressure mercury lamp, a fusion H lamp, or a xenon lamp as an ultraviolet source. The electron beam can be irradiated by using an electron beam generated by an electron beam accelerator or the like.
[0135] In the present invention, “energy ray-curable” means a property of being cured by irradiation with energy rays, and “non-energy ray-curable” means a property of not being cured even by irradiation with energy rays.
[0136] {{First adhesive composition}}
[0137] The first adhesive layer can be formed using a first adhesive composition containing an adhesive. For example, the first adhesive composition is applied to the surface of the object to be formed on the first adhesive layer and dried as required, thereby forming the first adhesive layer at the target site. In addition, the first adhesive composition is applied to a release film and dried as required, thereby forming a first adhesive layer of a target thickness, and the first adhesive layer can also be transferred to the target site. A more specific formation method of the first adhesive layer will be described in detail later together with the formation method of other layers. The content ratio of the components that do not vaporize at room temperature in the first adhesive composition is usually the same as the content ratio of the components of the first adhesive layer. In addition, in the present embodiment, "normal temperature" refers to a temperature that is not particularly cooled or heated, that is, a normal temperature, for example, a temperature of 15 to 25°C can be cited.
[0138] The first adhesive composition can be applied using a known method, for example, methods using various coaters such as an air knife coater, a blade coater, a rod coater, a gravure coater, a roll coater, a roll knife coater, a curtain coater, a die coater, a blade coater, a screen coater, a Meyer rod coater, and a kiss coater.
[0139] The drying conditions of the first adhesive composition are not particularly limited. When the first adhesive composition contains a solvent described below, it is preferably dried by heating. In this case, the drying is preferably performed at 70 to 130° C. for 10 seconds to 5 minutes, for example.
[0140] When the first adhesive layer is energy-ray-curable, the first adhesive composition containing an energy-ray-curable adhesive, that is, the energy-ray-curable first adhesive composition, can include, for example, a first adhesive composition (I-1) containing a non-energy-ray-curable adhesive resin (I-1a) (hereinafter, sometimes abbreviated as "adhesive resin (I-1a)") and an energy-ray-curable compound; a first adhesive composition (I-2) containing an energy-ray-curable adhesive resin (I-2a) (hereinafter, sometimes abbreviated as "adhesive resin (I-2a)") having an unsaturated group introduced into the side chain of the non-energy-ray-curable adhesive resin (I-1a); a first adhesive composition (I-3) containing the adhesive resin (I-2a) and an energy-ray-curable low molecular weight compound, etc.
[0141] {First Adhesive Composition (I-1)}
[0142] As described above, the first adhesive composition (I-1) contains the non-energy ray-curable adhesive resin (I-1a) and the energy ray-curable compound.
[0143] (Adhesive resin (I-1a))
[0144] The adhesive resin (I-1a) is preferably an acrylic resin.
[0145] Examples of the acrylic resin include acrylic polymers having at least a structural unit derived from an alkyl (meth)acrylate.
[0146] The acrylic resin may contain only one type of structural unit or two or more types of structural units. When there are two or more types of structural units, the combination and ratio of these structural units may be arbitrarily selected.
[0147] Examples of the alkyl (meth)acrylate include alkyl (meth)acrylates in which the alkyl group constituting the alkyl ester has 1 to 20 carbon atoms, and the alkyl group is preferably linear or branched.
[0148] More specifically, the alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, isononyl (meth)acrylate, and tert-butyl (meth)acrylate. ) decyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate (also known as lauryl (meth)acrylate), tridecyl (meth)acrylate, tetradecyl (meth)acrylate (also known as myristyl (meth)acrylate), pentadecyl (meth)acrylate, hexadecyl (meth)acrylate (also known as palmityl (meth)acrylate), heptadecyl (meth)acrylate, octadecyl (meth)acrylate (also known as stearyl (meth)acrylate), nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like.
[0149] From the viewpoint of improving the adhesive force of the first adhesive layer, the acrylic polymer preferably has a structural unit derived from an alkyl (meth)acrylate in which the alkyl group has 4 or more carbon atoms. Furthermore, from the viewpoint of further improving the adhesive force of the first adhesive layer, the alkyl group preferably has 4 to 12 carbon atoms, more preferably 4 to 8 carbon atoms. Furthermore, the alkyl (meth)acrylate in which the alkyl group has 4 or more carbon atoms is preferably an alkyl acrylate.
[0150] It is preferred that the acrylic polymer further has a structural unit derived from a functional group-containing monomer in addition to the structural unit derived from the (meth)acrylic acid alkyl ester.
[0151] Examples of the functional group-containing monomer include monomers that can react with a crosslinking agent described below to generate a crosslinking starting point, or can react with an unsaturated group in an unsaturated group-containing compound to introduce an unsaturated group into a side chain of an acrylic polymer.
[0152] Examples of the functional group in the functional group-containing monomer include a hydroxyl group, a carboxyl group, an amino group, and an epoxy group.
[0153] That is, examples of the functional group-containing monomer include a hydroxyl group-containing monomer, a carboxyl group-containing monomer, an amino group-containing monomer, and an epoxy group-containing monomer.
[0154] Examples of the hydroxyl-containing monomer include hydroxyalkyl (meth)acrylates such as hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate; and non-(meth)acrylic unsaturated alcohols such as vinyl alcohol and allyl alcohol (i.e., unsaturated alcohols that do not have a (meth)acryloyl skeleton).
[0155] Examples of the carboxyl group-containing monomer include ethylenically unsaturated monocarboxylic acids (monocarboxylic acids having ethylenically unsaturated bonds) such as (meth)acrylic acid and crotonic acid; ethylenically unsaturated dicarboxylic acids (dicarboxylic acids having ethylenically unsaturated bonds) such as fumaric acid, itaconic acid, maleic acid, and citraconic acid; anhydrides of the ethylenically unsaturated dicarboxylic acids; (meth)acrylic acid carboxylalkyl esters such as 2-carboxyethyl methacrylate, and the like.
[0156] The functional group-containing monomer is preferably a hydroxyl group-containing monomer or a carboxyl group-containing monomer, and more preferably a hydroxyl group-containing monomer.
[0157] The functional group-containing monomer constituting the acrylic polymer may be one type or two or more types. When two or more types are used, the combination and ratio of the monomers may be arbitrarily selected.
[0158] In the acrylic polymer, the content of the structural unit derived from the functional group-containing monomer is preferably 1 to 35% by mass, more preferably 3 to 32% by mass, and particularly preferably 5 to 30% by mass, based on the total amount of the structural units.
[0159] The acrylic polymer may further have a structural unit derived from other monomers in addition to the structural unit derived from the (meth)acrylic acid alkyl ester and the structural unit derived from the functional group-containing monomer.
[0160] The other monomers are not particularly limited as long as they are copolymerizable with the (meth)acrylic acid alkyl ester and the like.
[0161] Examples of the other monomers include styrene, α-methylstyrene, vinyltoluene, vinyl formate, vinyl acetate, acrylonitrile, and acrylamide.
[0162] The other monomers constituting the acrylic polymer may be one type or two or more types. When two or more types are used, the combination and ratio of the other monomers may be arbitrarily selected.
[0163] The acrylic polymer can be used as the non-energy ray-curable adhesive resin (I-1a).
[0164] On the other hand, a product obtained by reacting an unsaturated group-containing compound having an energy-ray-polymerizable unsaturated group (energy-ray-polymerizable group) with a functional group in the acrylic polymer can be used as the energy-ray-curable adhesive resin (I-2a).
[0165] In the present invention, "energy ray polymerizability" means a property of polymerizing by irradiation with energy rays.
[0166] The adhesive resin (I-1a) contained in the first adhesive composition (I-1) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of these can be arbitrarily selected.
[0167] In the first adhesive composition (I-1), the content of the adhesive resin (I-1a) is preferably 5 to 99% by mass, more preferably 10 to 95% by mass, and particularly preferably 15 to 90% by mass, relative to the total mass of the first adhesive composition (I-1).
[0168] (Energy ray curable compound)
[0169] Examples of the energy-ray-curable compound contained in the first adhesive composition (I-1) include monomers or oligomers that have an energy-ray-polymerizable unsaturated group and are curable by irradiation with energy rays.
[0170] Examples of monomers in the energy-ray-curable compound include poly(meth)acrylates such as trimethylolpropane tri(meth)acrylate, pentaerythritol (meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, 1,4-butanediol di(meth)acrylate, and 1,6-hexanediol (meth)acrylate; urethane (meth)acrylate; polyester (meth)acrylate; polyether (meth)acrylate; epoxy (meth)acrylate, and the like.
[0171] Examples of the oligomer in the energy-ray curable compound include oligomers obtained by polymerizing the monomers exemplified above.
[0172] The energy beam curable compound is preferably a urethane (meth)acrylate or a urethane (meth)acrylate oligomer because the molecular weight is relatively large and the storage modulus of the first adhesive layer is less likely to decrease.
[0173] In this specification, the "oligomer" refers to a substance having a weight average molecular weight or a formula weight of 5,000 or less.
[0174] The energy-ray-curable compound contained in the first adhesive composition (I-1) may be one type or two or more types. When two or more types are used, the combination and ratio of these types may be arbitrarily selected.
[0175] In the first adhesive composition (I-1), the content of the energy ray-curable compound is preferably 1 to 95% by mass, more preferably 5 to 90% by mass, and particularly preferably 10 to 85% by mass, relative to the total mass of the first adhesive composition (I-1).
[0176] (Crosslinking agent)
[0177] When the acrylic polymer having a structural unit derived from a functional group-containing monomer in addition to a structural unit derived from an alkyl (meth)acrylate is used as the adhesive resin (I-1a), the first adhesive composition (I-1) preferably further contains a crosslinking agent.
[0178] The crosslinking agent crosslinks the adhesive resins (I-1a) by reacting with the functional groups, for example.
[0179] Examples of the crosslinking agent include isocyanate crosslinking agents (crosslinking agents having an isocyanate group) such as toluene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, and adducts of these diisocyanates; epoxy crosslinking agents (crosslinking agents having a glycidyl group) such as ethylene glycol glycidyl ether; aziridine crosslinking agents (crosslinking agents having an aziridine group) such as hexa[1-(2-methyl)-aziridinyl]triphosphatriazine; metal chelate crosslinking agents (crosslinking agents having a metal chelate structure) such as aluminum chelate; isocyanurate crosslinking agents (crosslinking agents having an isocyanuric acid skeleton), and the like.
[0180] From the viewpoints of increasing the cohesive force of the adhesive to increase the adhesive force of the first adhesive layer and from the viewpoint of easy availability, the crosslinking agent is preferably an isocyanate crosslinking agent.
[0181] The crosslinking agent contained in the first adhesive composition (I-1) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of the crosslinking agents may be arbitrarily selected.
[0182] In the first adhesive composition (I-1), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 1 to 10 parts by mass, based on 100 parts by mass of the adhesive resin (I-1a).
[0183] (Photopolymerization Initiator)
[0184] The first adhesive composition (I-1) may further contain a photopolymerization initiator. Even when the first adhesive composition (I-1) containing the photopolymerization initiator is irradiated with relatively low energy rays such as ultraviolet rays, the curing reaction proceeds sufficiently.
[0185] Examples of the photopolymerization initiator include benzoin compounds such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, benzoin benzoic acid, benzoin benzoic acid methyl ester, and benzoin dimethyl ketal; acetophenone compounds such as acetophenone, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, and 2,2-dimethoxy-1,2-diphenylethane-1-one; phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide Acylphosphine oxide compounds; sulfides such as benzyl phenyl sulfide and tetramethylthiuram monosulfide; α-keto alcohol compounds such as 1-hydroxycyclohexyl phenyl ketone; azo compounds such as azobisisobutyronitrile; titanocene compounds such as titanocene; thioxanthone compounds such as thioxanthone; peroxide compounds; diketone compounds such as diacetyl; benzil, dibenzil, benzophenone, 2,4-diethylthioxanthone, 1,2-diphenylmethane, 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]acetone, 2-chloroanthraquinone, etc.
[0186] Furthermore, as the photopolymerization initiator, for example, quinone compounds such as 1-chloroanthraquinone, photosensitizers such as amines, and the like can be used.
[0187] The photopolymerization initiator contained in the first adhesive composition (I-1) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of these can be arbitrarily selected.
[0188] In the first adhesive composition (I-1), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the energy ray-curable compound.
[0189] (Other additives)
[0190] The first adhesive composition (I-1) may further contain other additives that are not included in any of the above components within a range that does not impair the effects of the present invention.
[0191] Examples of the other additives include known additives such as antistatic agents, antioxidants, softeners (plasticizers), fillers (fillers), rust inhibitors, colorants (pigments, dyes), sensitizers, thickeners, reaction retarders, and crosslinking accelerators (catalysts).
[0192] In addition, the reaction retarder refers to an additive that suppresses, for example, an unintended crosslinking reaction in the first adhesive composition (I-1) during storage due to the action of a catalyst mixed in the first adhesive composition (I-1). As the reaction retarder, for example, a reaction retarder that forms a chelate complex by using a chelate for the catalyst can be listed, and more specifically, a reaction retarder having two or more carbonyl groups (-C(=O)-) in one molecule can be listed.
[0193] The other additives contained in the first adhesive composition (I-1) may be one type or two or more types. When there are two or more types, the combination and ratio of these additives may be arbitrarily selected.
[0194] In the first adhesive composition (I-1), the content of other additives is not particularly limited and may be appropriately selected according to the type of the additives.
[0195] (Solvent)
[0196] The first adhesive composition (I-1) may contain a solvent. When the first adhesive composition (I-1) contains a solvent, its coating suitability on the surface to be coated is improved.
[0197] The solvent is preferably an organic solvent. Examples of the organic solvent include ketones such as methyl ethyl ketone and acetone; esters (carboxylates) such as ethyl acetate; ethers such as tetrahydrofuran and dioxane; aliphatic hydrocarbons such as cyclohexane and n-hexane; aromatic hydrocarbons such as toluene and xylene; and alcohols such as 1-propanol and 2-propanol.
[0198] As the solvent, for example, the solvent used in preparing the adhesive resin (I-1a) can be directly used in the first adhesive composition (I-1) without removing it from the adhesive resin (I-1a), or a solvent of the same type or a different type from the solvent used in preparing the adhesive resin (I-1a) can be added when preparing the first adhesive composition (I-1).
[0199] The first adhesive composition (I-1) may contain only one type of solvent or two or more types of solvent. When the number of solvents is two or more, the combination and ratio of the solvents may be arbitrarily selected.
[0200] In the first adhesive composition (I-1), the content of the solvent is not particularly limited and may be appropriately adjusted.
[0201] [First Adhesive Composition (I-2)]
[0202] As described above, the first adhesive composition (I-2) contains the energy-ray-curable adhesive resin (I-2a) in which an unsaturated group is introduced into the side chain of the non-energy-ray-curable adhesive resin (I-1a).
[0203] (Adhesive resin (I-2a))
[0204] The adhesive resin (I-2a) can be obtained, for example, by reacting an unsaturated group-containing compound having an energy ray-polymerizable unsaturated group with a functional group in the adhesive resin (I-1a).
[0205] The unsaturated group-containing compound is a compound having, in addition to the energy-ray-polymerizable unsaturated group, a group capable of bonding to the adhesive resin (I-1a) by reacting with a functional group in the adhesive resin (I-1a).
[0206] Examples of the energy beam polymerizable unsaturated group include a (meth)acryloyl group, a vinyl group (also referred to as an ethylidene group), an allyl group (also referred to as a 2-propenyl group), and the like, and a (meth)acryloyl group is preferred.
[0207] Examples of the group that can be bonded to the functional group in the adhesive resin (I-1a) include an isocyanate group and a glycidyl group that can be bonded to a hydroxyl group or an amino group, and a hydroxyl group and an amino group that can be bonded to a carboxyl group or an epoxy group.
[0208] Examples of the unsaturated group-containing compound include (meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, and glycidyl (meth)acrylate. (Meth)acryloyloxyethyl isocyanate is preferred, and 2-methacryloyloxyethyl isocyanate is particularly preferred.
[0209] The isocyanate compound can bond to the hydroxyl group in the adhesive resin (I-1a). When all the hydroxyl groups in the adhesive resin (I-1a) are set to 100 mol, the usage amount of the isocyanate compound is preferably 10 to 150 mol, more preferably 20 to 140 mol, and further preferably 30 to 130 mol.
[0210] The adhesive resin (I-2a) contained in the first adhesive composition (I-2) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of these can be arbitrarily selected.
[0211] In the first adhesive composition (I-2), the content of the adhesive resin (I-2a) is preferably 5 to 99% by mass, more preferably 10 to 95% by mass, and particularly preferably 10 to 90% by mass, relative to the total mass of the first adhesive composition (I-2).
[0212] (Crosslinking agent)
[0213] For example, when the same acrylic polymer as the acrylic polymer having a structural unit derived from a functional group-containing monomer in the adhesive resin (I-1a) is used as the adhesive resin (I-2a), the first adhesive composition (I-2) may further contain a crosslinking agent.
[0214] Examples of the cross-linking agent in the first adhesive composition (I-2) include the same cross-linking agents as those in the first adhesive composition (I-1).
[0215] The cross-linking agent contained in the first adhesive composition (I-2) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of the cross-linking agents may be arbitrarily selected.
[0216] In the first adhesive composition (I-2), the content of the crosslinking agent is preferably 0.01 to 50 parts by mass, more preferably 0.1 to 20 parts by mass, and particularly preferably 1 to 10 parts by mass, based on 100 parts by mass of the adhesive resin (I-2a).
[0217] (Photopolymerization Initiator)
[0218] The first adhesive composition (I-2) may further contain a photopolymerization initiator. Even when the first adhesive composition (I-2) containing the photopolymerization initiator is irradiated with relatively low energy rays such as ultraviolet rays, the curing reaction proceeds sufficiently.
[0219] Examples of the photopolymerization initiator in the first adhesive composition (I-2) include the same photopolymerization initiators as those in the first adhesive composition (I-1).
[0220] The photopolymerization initiator contained in the first adhesive composition (I-2) may be only one kind or two or more kinds. When two or more kinds are used, the combination and ratio of these can be arbitrarily selected.
[0221] In the first adhesive composition (I-2), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, based on 100 parts by mass of the adhesive resin (I-2a).
[0222] (Other additives)
[0223] The first adhesive composition (I-2) may further contain other additives that are not included in any of the above components within a range that does not impair the effects of the present invention.
[0224] Examples of the other additives in the first adhesive composition (I-2) include the same other additives as those in the first adhesive composition (I-1).
[0225] The other additives contained in the first adhesive composition (I-2) may be one type or two or more types. When there are two or more types, the combination and ratio of these additives may be arbitrarily selected.
[0226] In the first adhesive composition (I-2), the content of other additives is not particularly limited and may be appropriately selected according to the type.
[0227] (Solvent)
[0228] The first adhesive composition (I-2) may contain a solvent for the same purpose as in the case of the first adhesive composition (I-1).
[0229] Examples of the solvent in the first adhesive composition (I-2) include the same solvents as those in the first adhesive composition (I-1).
[0230] The first adhesive composition (I-2) may contain only one type of solvent or two or more types of solvent. When there are two or more types of solvent, the combination and ratio of the solvents may be arbitrarily selected.
[0231] In the first adhesive composition (I-2), the content of the solvent is not particularly limited and may be appropriately adjusted.
[0232] {First Adhesive Composition (I-3)}
[0233] As described above, the first adhesive composition (I-3) contains the adhesive resin (I-2a) and an energy-ray-curable low-molecular compound.
[0234] In the first adhesive composition (I-3), the content of the adhesive resin (I-2a) is preferably 5 to 99% by mass, more preferably 10 to 95% by mass, and particularly preferably 15 to 90% by mass, relative to the total mass of the first adhesive composition (I-3).
[0235] (Energy ray curable low molecular weight compound)
[0236] The energy-ray-curable low molecular weight compound contained in the first adhesive composition (I-3) includes monomers or oligomers having an energy-ray-polymerizable unsaturated group and curable by irradiation with energy rays, and the same energy-ray-curable compounds as the energy-ray-curable compounds contained in the first adhesive composition (I-1) can be listed.
[0237] The energy ray-curable low molecular weight compound contained in the first adhesive composition (I-3) may be one type or two or more types. When two or more types are used, the combination and ratio of these types may be arbitrarily selected.
[0238] In the first adhesive composition (I-3), the content of the energy-ray-curable low molecular weight compound is preferably 0.01 to 300 parts by mass, more preferably 0.03 to 200 parts by mass, and particularly preferably 0.05 to 100 parts by mass, relative to 100 parts by mass of the adhesive resin (I-2a).
[0239] (Photopolymerization Initiator)
[0240] The first adhesive composition (I-3) may further contain a photopolymerization initiator. Even when the first adhesive composition (I-3) containing the photopolymerization initiator is irradiated with relatively low energy rays such as ultraviolet rays, the curing reaction proceeds sufficiently.
[0241] Examples of the photopolymerization initiator in the first adhesive composition (I-3) include the same photopolymerization initiators as those in the first adhesive composition (I-1).
[0242] The photopolymerization initiator contained in the first adhesive composition (I-3) may be one kind or two or more kinds. When two or more kinds are used, the combination and ratio of these can be arbitrarily selected.
[0243] In the first adhesive composition (I-3), the content of the photopolymerization initiator is preferably 0.01 to 20 parts by mass, more preferably 0.03 to 10 parts by mass, and particularly preferably 0.05 to 5 parts by mass, relative to 100 parts by mass of the total content of the adhesive resin (I-2a) and the energy-ray-curable low molecular weight compound.
[0244] (Other additives)
[0245] The first adhesive composition (I-3) may further contain other additives that are not included in any of the above components within a range that does not impair the effects of the present invention.
[0246] Examples of the other additives include the same additives as those in the first adhesive composition (I-1).
[0247] The other additives contained in the first adhesive composition (I-3) may be one type or two or more types. When two or more types are used, the combination and ratio of these additives may be arbitrarily selected.
[0248] In the first adhesive composition (I-3), the content of other additives is not particularly limited and may be appropriately selected according to the type.
[0249] (Solvent)
[0250] The first adhesive composition (I-3) may contain a solvent for the same purpose as in the case of the first adhesive composition (I-1).
[0251] Examples of the solvent in the first adhesive composition (I-3) include the same solvents as those in the first adhesive composition (I-1).
[0252] The first adhesive composition (I-3) may contain only one type of solvent or two or more types of solvent. When the number of solvents is two or more, the combination and ratio of the solvents may be arbitrarily selected.
[0253] In the first adhesive composition (I-3), the content of the solvent is not particularly limited and may be appropriately adjusted.
[0254] {First adhesive composition other than first adhesive compositions (I-1) to (I-3)}
[0255] So far, the first adhesive composition (I-1), the first adhesive composition (I-2) and the first adhesive composition (I-3) have been mainly described, but the components described as their contained components can also be used in all first adhesive compositions other than these three first adhesive compositions (in this embodiment, referred to as "first adhesive compositions other than the first adhesive compositions (I-1) to (I-3)").
[0256] As the first adhesive composition other than the first adhesive compositions (I-1) to (I-3), in addition to energy-ray-curable first adhesive compositions, non-energy-ray-curable first adhesive compositions can be mentioned.
[0257] As the non-energy ray-curable first adhesive composition, for example, there can be listed compositions containing adhesive resins such as acrylic resins (resins having a (meth)acryloyl group), carbamate resins (resins having a carbamate bond), rubber resins (resins having a rubber structure), silicone resins (resins having a siloxane bond), epoxy resins (resins having an epoxy group), polyethylene ether, or polycarbonate. The non-energy ray-curable first adhesive composition containing an acrylic resin is preferred.
[0258] The first adhesive composition other than the first adhesive compositions (I-1) to (I-3) preferably contains one or more crosslinking agents, and the content thereof can be set similarly to the case of the first adhesive composition (I-1) and the like.
[0259] <Method for preparing first adhesive composition>
[0260] The first adhesive composition (I-1) to (I-3) and the like can be obtained by blending the components constituting the first adhesive composition, that is, by blending the adhesive and components other than the adhesive as required.
[0261] The order of adding the components when blending them is not particularly limited, and two or more components may be added simultaneously.
[0262] When a solvent is used, the solvent may be mixed with any blending components other than the solvent to dilute the blending components in advance and then used, or the solvent may be mixed with the blending components without diluting the blending components in advance and then used.
[0263] The method for mixing the components during blending is not particularly limited, and may be appropriately selected from the following known methods: a method of mixing by rotating a stirring bar or a stirring blade, a method of mixing using a mixer, a method of mixing by applying ultrasonic waves, and the like.
[0264] The temperature and time for adding and mixing the components are not particularly limited as long as the components do not deteriorate, and may be appropriately adjusted. However, the temperature is preferably 15 to 30°C.
[0265] {Composition of the first adhesive layer}
[0266] The composition of the first adhesive layer in the present embodiment is a composition obtained by removing the solvent from the first adhesive layer composition.
[0267] When the first adhesive layer composition is the first adhesive composition (I-1), the adhesive resin (I-1a) in the first adhesive layer (I-1) is preferably 50 to 99% by mass, more preferably 55 to 95% by mass, and further preferably 60 to 90% by mass. In addition, as another aspect of the present invention, the adhesive resin (I-1a) can be 25 to 80% by mass, 30 to 75% by mass, or 35 to 70% by mass relative to the total mass of the first adhesive layer (I-1). In addition, the energy ray curable compound is preferably 1 to 50% by mass, more preferably 2 to 48% by mass, and further preferably 5 to 45% by mass relative to the total mass of the first adhesive layer (I-1). When the first adhesive layer (I-1) contains a crosslinking agent, the content of the crosslinking agent relative to the total mass of the first adhesive layer (I-1) is preferably 0.1 to 10 mass %, more preferably 0.2 to 9 mass %, and even more preferably 0.3 to 8 mass %.
[0268] When the first adhesive layer composition is the first adhesive composition (I-2), the content ratio of the adhesive resin (I-2a) in the first adhesive layer (I-2) relative to the total mass of the first adhesive layer (I-2) is preferably 50 to 99% by mass, more preferably 60 to 98% by mass, and further preferably 70 to 97% by mass. When the first adhesive layer (I-2) contains a crosslinking agent, the content ratio of the crosslinking agent relative to the total mass of the first adhesive layer (I-2) is preferably 0.1 to 10% by mass, more preferably 0.2 to 9% by mass, and further preferably 0.3 to 8% by mass.
[0269] When the first adhesive layer composition is the first adhesive composition (I-3), the content ratio of the adhesive resin (I-2a) in the first adhesive layer (I-3) relative to the total mass of the first adhesive layer (I-3) is preferably 50 to 99% by mass, more preferably 55 to 95% by mass, and further preferably 60 to 90% by mass. In addition, the content ratio of the energy ray curable low molecular weight compound relative to the total mass of the first adhesive layer (I-3) is preferably 1 to 50% by mass, more preferably 2 to 48% by mass, and further preferably 5 to 45% by mass. When the first adhesive layer (I-3) contains a crosslinking agent, the content ratio of the crosslinking agent relative to the total mass of the first adhesive layer (I-3) is preferably 0.1 to 10% by mass, more preferably 0.2 to 9% by mass, and further preferably 0.3 to 8% by mass.
[0270] In this embodiment, the first adhesive layer (I-2) is preferably composed of an adhesive resin (1-2a) and a crosslinking agent. In this case, the adhesive resin (1-2a) is preferably an acrylic polymer obtained by reacting an unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group with an acrylic polymer having a structural unit derived from an alkyl (meth)acrylate and a unit derived from a hydroxyl-containing monomer. The crosslinking agent can use the compounds exemplified in the first adhesive composition (I-1), and toluene diisocyanate is particularly preferably used.
[0271] The content ratio of the structural unit derived from the (meth)acrylic acid alkyl ester to the total mass of the adhesive resin (1-2a) is preferably 50 to 99 mass%, more preferably 60 to 98 mass%, and further preferably 70 to 97 mass%. The content ratio of the unit derived from the hydroxyl-containing monomer to the total mass of the adhesive resin (1-2a) is preferably 0.5 to 15 mass%, more preferably 1.0 to 10 mass%, and further preferably 2.0 to 10 mass%. The number of carbon atoms of the alkyl group of the (meth)acrylic acid alkyl ester in the adhesive resin (1-2a) is preferably 1 to 12, and more preferably 1 to 4. The adhesive resin (1-2a) preferably has two or more structural units derived from the (meth)acrylic acid alkyl ester, more preferably has structural units derived from methyl (meth)acrylate and n-butyl (meth)acrylate, and further preferably has structural units derived from methyl methacrylate and n-butyl acrylate. As the hydroxyl-containing monomer in the adhesive resin (1-2a), the hydroxyl-containing monomer exemplified in the above-mentioned first adhesive composition (I-1) can be used, and 2-hydroxyethyl acrylate is particularly preferred. As the unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group, the compound exemplified in the first adhesive composition (I-2) can be used, and 2-methacryloyloxyethyl isocyanate is particularly preferred. When all hydroxyl groups from the hydroxyl-containing monomer are set to 100 mol, the amount of the unsaturated group-containing compound having an isocyanate group and an energy-ray-polymerizable unsaturated group is preferably 20 to 80 mol, more preferably 25 to 75 mol, and further preferably 30 to 70 mol.
[0272] ◎Base material
[0273] The substrate is in a sheet or film shape, and examples of its constituent material include various resins.
[0274] Examples of the resin include polyethylenes such as low-density polyethylene (also referred to as LDPE), linear low-density polyethylene (also referred to as LLDPE), and high-density polyethylene (also referred to as HDPE); polyolefins other than polyethylene such as polypropylene, polybutene, polybutadiene, polymethylpentene, and norbornene resins; ethylene-vinyl acetate copolymers (also referred to as EVA), ethylene-(meth)acrylic acid copolymers, ethylene-(meth)acrylate copolymers, and ethylene-norbornene copolymers (i.e., copolymers obtained using ethylene as a monomer); polyvinyl chloride, vinyl chloride copolymers, and the like. Vinyl chloride resin (i.e., resin obtained using vinyl chloride as a monomer); polystyrene; polycycloolefin; polyesters such as polyethylene terephthalate (also called PET), polyethylene naphthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene 2,6-naphthalate, and fully aromatic polyesters in which all structural units have aromatic cyclic groups; copolymers of two or more of the above polyesters; poly(meth)acrylate; polyurethane; polyurethane acrylate; polyimide; polyamide; polycarbonate; fluororesin; polyacetal; modified polyphenylene ether; polyphenylene sulfide; polysulfone; polyether ketone, etc.
[0275] In addition, the resin may include, for example, a polymer alloy such as a mixture of the polyester and other resins. Preferably, the amount of the resin other than polyester in the polymer alloy of the polyester and other resins is relatively small.
[0276] Examples of the resin include crosslinked resins obtained by crosslinking one or more of the resins listed above; and modified resins such as ionomers using one or more of the resins listed above.
[0277] In addition, in this specification, "(meth)acrylic acid" is a concept that includes both "acrylic acid" and "methacrylic acid". The same applies to terms similar to (meth)acrylic acid, for example, "(meth)acrylate" is a concept that includes both "acrylate" and "methacrylate", and "(meth)acryloyl" is a concept that includes both "acryloyl" and "methacryloyl".
[0278] The resin constituting the substrate may be one type or two or more types. When two or more types are used, the combination and ratio of the resins may be arbitrarily selected.
[0279] The substrate may be a single layer (single layer) or may be a plurality of layers of two or more. When the substrate is a plurality of layers, the plurality of layers may be the same as or different from each other, and the combination of the plurality of layers is not particularly limited.
[0280] The thickness of the substrate is preferably 5 to 1000 μm, more preferably 10 to 500 μm, further preferably 15 to 300 μm, and particularly preferably 20 to 150 μm.
[0281] Here, the “thickness of the substrate” refers to the thickness of the entire substrate. For example, the thickness of a substrate composed of a plurality of layers refers to the total thickness of all the layers constituting the substrate.
[0282] The substrate is preferably a substrate with high thickness accuracy, i.e., a substrate in which the thickness deviation is suppressed at any position. As materials that can be used to constitute such a substrate with high thickness accuracy, for example, polyethylene, polyolefins other than polyethylene, polyethylene terephthalate, ethylene-vinyl acetate copolymer (EVA) and the like can be listed among the above-mentioned constituent materials.
[0283] In addition to the above-mentioned main constituent materials such as the resin, the base material may contain various known additives such as a filler, a colorant, an antistatic agent, an antioxidant, an organic lubricant, a catalyst, and a softener (plasticizer).
[0284] The substrate may be transparent or opaque, may be colored according to the purpose, or may have other layers deposited thereon.
[0285] When the viscoelastic layer is energy ray-curable, it is preferred that the substrate transmits energy rays.
[0286] The substrate can be produced by a known method. For example, a substrate containing a resin can be produced by molding a resin composition containing the resin.
[0287] ◎Release film
[0288] The release film may be a release film known in the art.
[0289] Preferred examples of the release film include a release film in which at least one surface of a film made of a resin such as polyethylene terephthalate is subjected to a release treatment such as silicone treatment, and a release film in which at least one surface of the film is a release surface made of polyolefin.
[0290] The thickness of the release film is preferably the same as the thickness of the substrate.
[0291] ◎Second adhesive layer
[0292] The second adhesive layer (ie, the laminating adhesive layer) is an adhesive layer for laminating the terminal protective tape of the present embodiment to a support.
[0293] The second adhesive layer may be an adhesive layer known in the art, and may be appropriately selected from the adhesive layers described above with respect to the first adhesive layer in combination with the support.
[0294] The second adhesive composition for forming the second adhesive layer is the same as the first adhesive composition, and the preparation method of the second adhesive composition is also the same as the preparation method of the first adhesive composition.
[0295] ◇Manufacturing method of terminal protection tape
[0296] The terminal protection tape can be manufactured by sequentially laminating the above-mentioned layers so as to have corresponding positional relationships. The method of forming each layer is the same as described above.
[0297] For example, the above-mentioned buried layer forming composition is applied to the stripping treatment surface of the release film, and dried as needed, thereby laminating the buried layer. The above-mentioned first adhesive composition is applied to the stripping treatment surface of another release film, and dried as needed, thereby laminating the first adhesive layer. By laminating the buried layer on the release film with the first adhesive layer on another release film, a terminal protection tape formed by laminating the release film, the buried layer, the first adhesive layer and the release film in sequence is obtained. The release film can be removed when using the terminal protection tape.
[0298] In addition, the terminal protection tape in which the embedding layer and the first adhesive layer are sequentially laminated on the base material in the thickness direction thereof can be produced by the method described below.
[0299] For example, the stripping film on the buried layer side of the terminal protection tape formed by sequentially stacking the stripping film, the buried layer, the first adhesive layer and the stripping film is stripped off, and the stripping film is bonded to the substrate, thereby obtaining a terminal protection tape having the buried layer, the first adhesive layer and the stripping film sequentially stacked on the substrate. The stripping film can be removed when using the terminal protection tape.
[0300] In addition, for example, the buried layer is formed by extrusion molding with a composition on a substrate, thereby the buried layer is stacked on the substrate. The above-mentioned first adhesive composition is applied to the stripping treatment surface of the release film, and dried as required, thereby stacking the first adhesive layer. Then, the first adhesive layer on the release film is fitted with the buried layer on the substrate, thereby also obtaining a terminal protection tape stacked with a buried layer, the first adhesive layer and the release film on the substrate. The release film can be removed when using the terminal protection tape.
[0301] Furthermore, a terminal protection tape in the form of a double-sided tape in which the second adhesive layer, the base material, the embedding layer, and the first adhesive layer are sequentially laminated in the thickness direction thereof can be produced by the method described below.
[0302] For example, prepare the above-mentioned terminal protection tape in which a buried layer, a first adhesive layer and a stripping film are sequentially stacked on a substrate. The above-mentioned second adhesive composition is applied to the stripping treatment surface of another stripping film, and dried as required, thereby stacking the second adhesive layer. Then, the second adhesive layer on the stripping film is fitted with the substrate of the terminal protection tape, thereby obtaining a terminal protection tape in which a stripping film, a second adhesive layer, a substrate, a buried layer, a first adhesive layer and a stripping film are sequentially stacked. The stripping film can be removed when using the terminal protection tape.
[0303] In the above-mentioned manufacturing method, it is possible to appropriately add any one or both of the formation process and the stacking process of the other layers in such a way that the stacking position of the other layers of the terminal protection tape other than the above-mentioned layers is at an appropriate position, thereby manufacturing the terminal protection tape other than the above-mentioned layers.
[0304] ◇Method for manufacturing semiconductor device with electromagnetic wave shielding film
[0305] The terminal protection tape of the present embodiment can be used, for example, in the following method of manufacturing a semiconductor device with an electromagnetic wave shielding film.
[0306] Figure 5 The method for manufacturing a semiconductor device with an electromagnetic wave shielding film of this embodiment is schematically shown as follows: a terminal protection tape 3 having an adhesive layer 14, a burying layer 13 and a substrate 11 is sequentially formed. Figure 4 1 is a cross-sectional view of an embodiment of a method for manufacturing a semiconductor device with an electromagnetic wave shielding film, wherein the semiconductor device is fixed to a support body 30 as shown.
[0307] First, if Figure 5 (a) Figure 5 As shown in (b), the semiconductor device 65 with terminals is pressed onto the viscoelastic layer 12 of the terminal protection tape with the terminal 91 side, that is, the terminal forming surface 63 a of the circuit board 63 facing downward, so that the terminal 91 is buried in the viscoelastic layer 12 .
[0308] At this time, the viscoelastic layer 12 is brought into contact with the terminal 91 of the semiconductor device with a terminal 65, and the semiconductor device with a terminal 65 is pressed against the terminal protection tape. Thus, the outermost surface of the viscoelastic layer 12 on the adhesive layer 14 side is pressed against the surface of the terminal 91 and the terminal forming surface 63a of the circuit substrate 63 in sequence. At this time, the viscoelastic layer 12 is heated to soften the viscoelastic layer 12, and spreads between the terminals 91 in a manner covering the terminals 91, closely adheres to the terminal forming surface 63a, and at the same time covers the surface of the terminal 91, especially the surface of the portion near the terminal forming surface 63a, thereby burying the terminal 91.
[0309] As a method of press-bonding the semiconductor device 65 with terminals to the terminal protection tape, a known method of pressing various sheets to an object for attachment can be applied, and examples thereof include a method using a laminating roll or a vacuum laminator.
[0310] The pressure when the semiconductor device 65 with terminals is pressed against the terminal protection tape is not particularly limited, but is preferably 0.1 to 1.5 MPa, more preferably 0.3 to 1.3 MPa. The heating temperature is preferably 30 to 70° C., more preferably 35 to 65° C., and particularly preferably 40 to 60° C. In addition, the first adhesive layer 14 of the viscoelastic layer 12 is preferably attached to the terminal forming surface 63a.
[0311] The conductive resin 101 is applied to the exposed surface of the semiconductor device 65 with terminals ( Figure 5 (c)), and further heat-curing it, thereby forming an electromagnetic wave shielding film 10 ( Figure 5 (d)). As a method for forming the electromagnetic wave shielding film 10 by covering with a conductive material, a method such as sputtering, ion plating, spraying, etc. can also be used.
[0312] In the dynamic viscoelasticity measurement of the viscoelastic layer 12, the tanδ value at 50°C is 0.2 or more, and the thickness of the viscoelastic layer 12 is 80 to 800 μm. Therefore, when the terminal of the semiconductor device with the terminal is embedded in the viscoelastic layer 12, even the terminal electrode that is easy to float, such as the solder ball, can be embedded, and the terminal forming surface 63a of the circuit substrate 63 can be made to be closely attached to the viscoelastic layer 12. As a result, the terminal 91 as the terminal electrode can be prevented from short-circuiting with the electromagnetic wave shielding film 10, and there is no need to set a shielding part with a complicated process.
[0313] By picking up the semiconductor device 66 with the electromagnetic wave shielding film from the terminal protection tape 3 having the viscoelastic layer 12, the semiconductor device 65 with the terminal covered by the electromagnetic wave shielding film 10 can be taken out. Figure 5 (e)).
[0314] Figure 5 In the method for manufacturing a semiconductor device with an electromagnetic wave shielding film shown, the semiconductor device with terminals 65 to be shielded from electromagnetic waves may be a semiconductor device with terminals 65 manufactured individually or may be a semiconductor device with terminals 65 singulated by dicing.
[0315] Figure 5In the manufacturing method of a semiconductor device with an electromagnetic wave shielding film shown, although a method of using a terminal protection tape 3 to perform electromagnetic wave shielding on a semiconductor device 65 with terminals in which individual electronic components 61, 62 that have been singulated are sealed with a sealing resin 64 is shown, as described below, a terminal protection tape 2 can also be used to perform electromagnetic wave shielding on a semiconductor device 65 with terminals in a semiconductor device assembly 6 with terminals before singulation.
[0316] Figure 6 The method for manufacturing a semiconductor device with an electromagnetic wave shielding film of this embodiment is a cross-sectional view schematically showing another embodiment of a method for electromagnetic wave shielding of a semiconductor device 65 with terminals using a terminal protection tape 2 having an adhesive layer 14, a embedding layer 13 and a substrate 11 in sequence.
[0317] First, if Figure 6 (a) Figure 6 As shown in (b), the semiconductor device assembly 6 with terminals connected via the circuit substrate 63 is pressed onto the viscoelastic layer 12 of the terminal protection tape with the terminal 91 side, that is, the terminal forming surface 63a of the circuit substrate 63 facing downward, so as to be in contact with the Figure 5 (a) Figure 5 The terminal 91 is embedded in the viscoelastic layer 12 in the same manner as in (b).
[0318] At this time, while applying pressure to the semiconductor device assembly 6 with terminals from the upper side, Figure 5 (a) Figure 5 The terminal 91 is embedded in the viscoelastic layer 12 of the terminal protection tape in the same manner as in (b).
[0319] In addition, the viscoelastic layer 12 is heated while being laminated, so that the viscoelastic layer 12 can be softened and the viscoelastic layer 12 can be closely attached to the terminal forming surface 63a of the circuit substrate 63. The pressure when the semiconductor device assembly 6 with terminals is pressed against the terminal protection tape is not particularly limited, but is preferably 0.1 to 1.5 MPa, more preferably 0.3 to 1.3 MPa. The heating temperature is preferably 30 to 70°C, more preferably 35 to 65°C, and particularly preferably 40 to 60°C. In addition, the first adhesive layer 14 of the viscoelastic layer 12 is preferably laminated to the terminal forming surface 63a.
[0320] Next, the semiconductor device assembly 6 with terminals is cut to produce semiconductor devices 65 with terminals ( Figure 6 (c)). The terminal protection tape of the present embodiment used in the process of forming the electromagnetic wave shielding film is also used as a dicing tape for the semiconductor device assembly 6 with terminals. Figure 5In the method for manufacturing a semiconductor device with an electromagnetic wave shielding film shown in FIG. 1 , when the semiconductor device with terminals 65 to be shielded from electromagnetic waves is a semiconductor device with terminals 65 singulated by dicing, the semiconductor device with terminals on the dicing tape is picked up and reattached to the terminal protection tape ( Figure 5 (a)) is necessary. On the other hand, Figure 6 In the method for manufacturing a semiconductor device with an electromagnetic wave shielding film shown, the operation of re-attaching the semiconductor device with terminals 65 on the dicing tape to the terminal protection tape can be omitted.
[0321] The conductive resin 101 is applied to the exposed surface of the semiconductor device 65 with terminals ( Figure 6 (d)). At this time, when the separation of the conductive resin 101 at the boundary portion of each semiconductor device 65 with a terminal of the semiconductor device assembly 6 with a terminal is not sufficient, an expansion device or the like can be used to stretch the terminal protection tape. The individual semiconductor devices 65 with terminals can be singulated in a state where the respective sides of the singulated semiconductor devices 65 with terminals are coated with the conductive resin 101. Furthermore, the conductive resin 101 coated on the top surface and the side surface of the singulated semiconductor device 65 with terminals is heated and cured, thereby forming an electromagnetic wave shielding film 10 ( Figure 6 (e)). Alternatively, the conductive material may be directly sputtered onto the semiconductor device 65 with terminals ( Figure 6 (c)) to form an electromagnetic wave shielding film 10 ( Figure 6 (e)).
[0322] In the dynamic viscoelasticity measurement of the viscoelastic layer 12, the tanδ value at 50°C is 0.2 or more, and the thickness of the viscoelastic layer 12 is 80 to 800 μm. Therefore, when the terminal of the semiconductor device assembly 6 with a terminal is embedded in the viscoelastic layer 12, even the terminal electrodes that are prone to floating, such as solder balls, can be embedded, and the terminal forming surface 63a of the circuit substrate 63 can be made to adhere closely to the viscoelastic layer 12. As a result, the terminal 91 as the terminal electrode can be prevented from short-circuiting with the electromagnetic wave shielding film 10, and there is no need to provide a shielding portion with a complicated process.
[0323] By picking up the semiconductor device 66 with the electromagnetic wave shielding film from the terminal protection tape having the viscoelastic layer 12, the semiconductor device 65 with the terminal covered by the electromagnetic wave shielding film 10 can be taken out. Figure 6 (f)).
[0324] In the terminal protection tape of the present embodiment, the height h0 of the terminal 91 is preferably lower than the thickness d1 of the viscoelastic layer 12, preferably 1.2≤d1 / h0≤5.0. Specifically, the height h0 of the terminal 91 is preferably 50 to 300 μm, more preferably 60 to 270 μm, and particularly preferably 80 to 240 μm. By making the height of the terminal 91 above the lower limit, the function of the terminal 91 can be further improved. In addition, by making the height of the terminal 91 below the upper limit, the effect of suppressing the viscoelastic layer 12 from remaining on the upper part of the terminal 91 becomes higher.
[0325] In addition, in this specification, "the height of the terminal" refers to the height of the part of the terminal that is located at the highest position from the terminal forming surface. When the semiconductor device assembly 6 with terminals and the semiconductor device 65 with terminals have a plurality of terminals 91, the height h0 of the terminal 91 may be the average value of the terminals. The height of the terminal can be measured, for example, using a non-contact 3D optical interference type surface roughness meter (manufactured by Veeco Instruments Inc., trade name: Wyko NT1100).
[0326] The width of the terminal 91 is not particularly limited, but is preferably 170 to 350 μm, more preferably 200 to 320 μm, and particularly preferably 230 to 290 μm. By making the width of the terminal 91 greater than the lower limit, the function of the terminal 91 can be further improved. In addition, by making the height of the terminal 91 less than the upper limit, the effect of suppressing the viscoelastic layer 12 from remaining on the upper part of the terminal 91 becomes higher.
[0327] In addition, in this specification, the "width of the terminal" refers to the maximum value of a line segment obtained by connecting two different points on the terminal surface with a straight line when looking down at the terminal from a direction perpendicular to the terminal forming surface. When the terminal is spherical or hemispherical, the "width of the terminal" refers to the maximum diameter (terminal diameter) of the terminal when looking down at the terminal.
[0328] The distance between adjacent terminals 91 (i.e., the pitch between terminals) is not particularly limited, but is preferably 250 to 800 μm, more preferably 300 to 600 μm, and particularly preferably 350 to 500 μm. By making the distance greater than the lower limit, the burying property of the terminal 91 can be further improved. In addition, by making the distance less than the upper limit, the effect of suppressing the viscoelastic layer 12 from remaining on the upper part of the terminal 91 becomes higher.
[0329] In addition, in this specification, "the distance between adjacent terminals" refers to the minimum value of the distance between the surfaces of adjacent terminals.
[0330] Example
[0331] The present invention will be described in more detail below by way of specific examples, but the present invention is not limited to the following examples.
[0332] <Single body>
[0333] The formal names of the abbreviated monomers are shown below.
[0334] HEA: 2-Hydroxyethyl Acrylate
[0335] BA: n-butyl acrylate
[0336] MMA: Methyl Methacrylate
[0337] AAc: Acrylic acid
[0338] (Preparation of Composition A for Laminating Adhesive Layer Forming)
[0339] 33.6 parts by mass of an acrylic copolymer (weight average molecular weight (Mw) 400,000), 66.4 parts by mass of methyl ethyl ketone as a solvent, and 0.2 parts by mass of a polycyclic epoxy compound (manufactured by MITSUBISHI GASCHEMICAL COMPANY, INC., product name "TETRAD-C") as a cross-linking agent were added, and stirred for 30 minutes to prepare a composition A for forming a laminating adhesive layer, wherein the acrylic copolymer was formed of 90 parts by mass of BA and 10 parts by mass of AAc.
[0340] (Manufacturing of Laminating Adhesive Layer A)
[0341] The composition A for forming a laminating adhesive layer was applied onto the release-treated surface of a release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) obtained by silicone treatment on one side of a polyethylene terephthalate film, and heated and dried at 100°C for 1 minute to produce a laminating adhesive layer A with a thickness of 20 μm.
[0342] (Preparation of Adhesive Layer-Forming Composition B)
[0343] A solution of a resin (adhesive main component, solid content 35% by mass) was prepared by adding 2-methacryloyloxyethyl isocyanate (about 50 mol% relative to HEA) to an acrylic copolymer composed of 74 parts by mass of BA, 20 parts by mass of MMA and 6 parts by mass of HEA. 0.5 parts by mass of toluene diisocyanate (manufactured by TOYOCHEM CO., LTD., product name "BHS-8515", solid content concentration: 37.5%) as a crosslinking agent was added to 100 parts by mass of the adhesive main component, and stirred for 30 minutes to prepare an adhesive layer forming composition B.
[0344] (Manufacturing of Adhesive Layer B)
[0345] The adhesive layer forming composition B was applied onto the release-treated surface of a release film (“SP-PET381031” manufactured by Lintec Corporation, 38 μm thick) obtained by silicone treatment on one side of a polyethylene terephthalate film, and heated and dried at 100° C. for 1 minute to prepare an adhesive layer B having a thickness of 20 μm.
[0346] (Preparation of Burying Layer Forming Composition A)
[0347] 100 parts by mass of a solution (solid content: 33.6% by mass) of an acrylic copolymer (weight average molecular weight (Mw) 400,000) formed of 90 parts by mass of BA and 10 parts by mass of AAc, 50 parts by mass of a solution (solid content: 45% by mass) of a resin (weight average molecular weight (Mw) 100,000), and 2.5 parts by mass of toluene diisocyanate (manufactured by TOYOCHEM CO., LTD., product name: "BHS-8515", solid content concentration: 37.5%) as a cross-linking agent were added, and stirred for 30 minutes to prepare a buried layer forming composition A, wherein the resin was prepared by adding 2-methacryloyloxyethyl isocyanate to an acrylic copolymer formed of 62 parts by mass of BA, 10 parts by mass of MMA and 28 parts by mass of HEA so that the addition rate relative to 100 mol% of HEA was 80 mol%.
[0348] (Preparation of Burying Layer Forming Composition B)
[0349] 33.6 parts by mass of an acrylic copolymer (weight average molecular weight (Mw) 400,000) formed by 90 parts by mass of BA and 10 parts by mass of AAc, 66.4 parts by mass of methyl ethyl ketone as a solvent, and 0.2 parts by mass of a polycyclic epoxy compound (manufactured by MITSUBISHI GAS CHEMICAL COMPANY, INC., product name "TETRAD-C") as a cross-linking agent were added, and stirred for 30 minutes to prepare a buried layer forming composition B.
[0350] (Base material)
[0351] A polyethylene terephthalate (PET) film (product name “Cosmo Shine A4100”, thickness 50 μm, manufactured by TOYOBO Co., Ltd.) was used for the substrate 11 .
[0352] (Preparation of semiconductor device with terminals)
[0353] When evaluating the embedding properties of the terminal protection tapes of Examples and Comparative Examples, the following semiconductor devices with terminals were prepared.
[0354] ·Semiconductor device with terminal(1)
[0355] Semiconductor device size: 10mm×10mm
[0356] Terminal height: 200μm
[0357] Terminal diameter: 250μm
[0358] Terminal pitch: 400μm
[0359] Number of terminals: 10×10=100
[0360] ·Semiconductor device with terminal(2)
[0361] Semiconductor device size: 10mm×10mm
[0362] Terminal height: 100μm
[0363] Terminal diameter: 250μm
[0364] Terminal pitch: 400μm
[0365] Number of terminals: 10×10=100
[0366] <Evaluation of burial properties>
[0367] Will Figure 3 The release film 22 on the side of the adhesive layer 15 of the terminal protection tape 3 is peeled off and adhered to the SUS plate 30, thereby producing Figure 4 The sample for evaluation of embedding property of the shape of the test piece was peeled off the release film 20 on the adhesive layer 14 side, and the test piece was placed on a heating plate adjusted to 50° C. with the SUS plate 30 side facing downward. Figure 5 As shown in (a), the semiconductor device with terminals was pressed onto the viscoelastic layer 12 with a pressing pressure (load) of 1.1 MPa, a pressing time of 40 s, and a heating time of 50° C. with the terminal side of the semiconductor device with terminals facing downward. The embedding property evaluation was performed on 9 semiconductor devices with terminals.
[0368] Immediately after stamping, the embedding property was confirmed by observing from the side. If the lower surface of all semiconductor devices with terminals was adhered to the terminal protection tape and the terminals were covered by the terminal protection tape and could not be observed, it was evaluated as good embedding property just after stamping (A). If the lower surface of at least one semiconductor device with terminals floated from the terminal protection tape and the terminals could be observed between the terminal protection tape and the semiconductor device body, it was evaluated as poor embedding property just after stamping (B).
[0369] Then, after cooling to room temperature for 1 hour, the semiconductor device with terminals was observed from the side to confirm the embedding property. The case where the lower surface of all the semiconductor devices with terminals was adhered to the terminal protection tape and the terminals were covered by the terminal protection tape and could not be observed was evaluated as good embedding property after 1 hour of stamping (A). The case where the lower surface of at least one semiconductor device with terminals floated from the terminal protection tape and the terminals could be observed between the terminal protection tape and the semiconductor device body was evaluated as poor embedding property after 1 hour of stamping (B).
[0370] [Example 1]
[0371] <Manufacture of terminal protection tape>
[0372] The embedding layer forming composition A is coated on the release-treated surface of a release film ("SP-PET381031" manufactured by Lintec Corporation, with a thickness of 38 μm) obtained by subjecting one side of a polyethylene terephthalate film to a release treatment using silicone treatment, and after heating and drying at 100°C for 1 minute, the release-treated surface of a release film ("SP-PET382150" manufactured by Lintec Corporation, with a thickness of 38 μm) obtained by subjecting one side of a polyethylene terephthalate film to a release treatment using silicone treatment is laminated on the embedding layer forming composition A to produce a embedding layer with a thickness of 50 μm.
[0373] The surfaces of the embedding layers from which the laminated release films were peeled off were bonded together to produce an embedding layer having a thickness of 100 μm. In the same manner, embedding layers were bonded and stacked to produce an embedding layer A having a thickness of 300 μm.
[0374] The embedding layer A with a thickness of 300 μm was bonded to the adhesive layer B with a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Example 1 having the viscoelastic layer 12 having a thickness of 320 μm in the form shown.
[0375] <Measurement of shear storage modulus of viscoelastic layer>
[0376] By peeling off the two release films in the terminal protection tape 1 of Example 1, three layers of viscoelastic layer 12 with a thickness of 320 μm were stacked to form a viscoelastic layer with a thickness of 960 μm. A cylindrical evaluation sample with a diameter of 8 mm and a thickness of 960 μm was prepared from the viscoelastic layer, and the sample was set in a shear viscosity measuring device. At this time, the sample was placed in the setting position of the measuring device and the measuring fixture was pressed from the upper surface of the sample, thereby fixing and setting the sample in the setting position.
[0377] The shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') were measured from room temperature to 100°C under the measurement conditions of frequency: 1 Hz and heating rate: 10°C / min. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C were determined. The results are shown in Table 1.
[0378] <Evaluation of burial properties>
[0379] The release film on the buried layer A side of the terminal protection tape 1 of Example 1 was peeled off and attached to the easy-adhesion treated side of a polyethylene terephthalate (PET) film (product name "Cosmo Shine A4100", thickness 50 μm, manufactured by TOYOBO Co., Ltd.) as a substrate to produce a terminal protection tape 1 of Example 1. Figure 2 The terminal protection tape 2 of Example 1 having the viscoelastic layer 12 in the form of substrate 11 / embedding layer 13 / adhesive layer 14 is shown.
[0380] Furthermore, the laminating adhesive layer A is laminated on the side opposite to the embedding layer A of the substrate of the terminal protection tape 2 of Example 1 to produce Figure 3 The terminal-protecting tape 3 of Example 1 having the viscoelastic layer 12 in the form shown.
[0381] The release film on the side of the adhesive layer A of the terminal protection tape 3 of Example 1 was peeled off and adhered to a SUS plate to prepare a Figure 4 The sample for evaluation of embedding property in the form of was peeled off the release film on the adhesive layer B side, and the sample was placed on a heating plate adjusted to 50° C. with the SUS plate side facing downward. Figure 5 As shown in (a), the semiconductor device with terminals (1) with a terminal height of h0 = 200 μm was pressed onto the terminal protection tape 3 of Example 1 at a pressing pressure (load) of 1.1 MPa, a pressing time of 40 s, and a heating time of 50° C., with the terminal side of the semiconductor device with terminals (1) facing downward. The embedding property evaluation was performed on 9 semiconductor devices with terminals. The ratio (d1 / h0) of the thickness d1 (μm) of the viscoelastic layer 12 to the height h0 (μm) of the terminal was 1.6.
[0382] Immediately after stamping, the embedding property was checked by observing from the side, and the lower surface of all the semiconductor devices with terminals was adhered to the terminal protection tape, and the terminals were covered by the terminal protection tape and could not be observed (the embedding property immediately after stamping was good (A)). The results are shown in Table 1.
[0383] Then, the semiconductor device with terminals was cooled to room temperature for 1 hour and then observed from the side to check the embedding property. Figure 5 As shown in (b), the lower surfaces of all semiconductor devices with terminals were bonded to the terminal protection tape, and the terminals were covered by the terminal protection tape and could not be observed (the embedding property after pressing for 1 hour was good (A)). The results are shown in Table 1.
[0384] [Example 2]
[0385] <Manufacture of terminal protection tape>
[0386] A 470 μm-thick embedding layer A was produced on the release-treated surface of the release film in the same manner as in Example 1 except that the thickness of the embedding layer A was changed.
[0387] The embedding layer A with a thickness of 470 μm was laminated on the adhesive layer B with a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Example 2 having the viscoelastic layer 12 having a thickness of 490 μm is shown.
[0388] <Measurement of shear storage modulus of viscoelastic layer>
[0389] Next, by peeling off the two release films in the terminal protection tape 1 of Example 2, two viscoelastic layers 12 with a thickness of 490 μm are laminated, thereby forming a viscoelastic layer with a thickness of 980 μm. Then, in the same manner as in Example 1, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') of the viscoelastic layer 12 in the terminal protection tape 1 of Example 2 are measured. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C are calculated. The results are shown in Table 1.
[0390] <Evaluation of burial properties>
[0391] In the same manner as in Example 1, the terminal protection tape 1 of Example 2 was used to manufacture Figure 2 The terminal-protecting tape 2 of Example 2 has a viscoelastic layer 12 in the form shown.
[0392] Further, in the same manner as in Example 1, the terminal protection tape 2 of Example 2 was used to manufacture Figure 3The terminal-protecting tape 3 of Example 2 having the viscoelastic layer 12 in the form shown.
[0393] For the terminal protection tape 3 of Example 2, the semiconductor device (2) with terminals having a terminal height of h0 = 100 μm was used to confirm the embedding property ((d1 / h0) was 4.9) immediately after punching. The results were as follows: Figure 5 As shown in (b), the lower surface of all semiconductor devices with terminals is bonded to the terminal protection tape, and the terminals are covered by the terminal protection tape and cannot be observed (the embedding property is good immediately after stamping (A)). The results are shown in Table 1. In addition, the embedding property after stamping for 1 hour was confirmed, and the results were as follows Figure 5 As shown in (b), the lower surfaces of all semiconductor devices with terminals were bonded to the terminal protection tape, and the terminals were covered by the terminal protection tape and could not be observed (the embedding property after pressing for 1 hour was good (A)). The results are shown in Table 1.
[0394] [Example 3]
[0395] <Manufacture of terminal protection tape>
[0396] A embedding layer A having a thickness of 770 μm was produced on the release-treated surface of the release film in the same manner as in Example 1 except that the thickness of the embedding layer A was changed.
[0397] The embedding layer A with a thickness of 770 μm was laminated on the adhesive layer B with a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Example 3 having the viscoelastic layer 12 having a thickness of 790 μm is shown.
[0398] <Measurement of shear storage modulus of viscoelastic layer>
[0399] Next, the two release films in the terminal protection tape 1 of Example 3 are peeled off, and the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') of the viscoelastic layer 12 with a thickness of 790 μm in the terminal protection tape 1 of Example 3 are measured in the same manner as in Example 1. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C are calculated. The results are shown in Table 1.
[0400] <Evaluation of burial properties>
[0401] In the same manner as in Example 1, the terminal protection tape 1 of Example 3 was used to manufacture Figure 2 The terminal-protecting tape 2 of Example 3 having the viscoelastic layer 12 in the form shown.
[0402] Further, in the same manner as in Example 1, the terminal protection tape 2 of Example 3 was used to manufacture Figure 3 The terminal-protecting tape 3 of Example 3 having the viscoelastic layer 12 in the form shown.
[0403] For the terminal protection tape 3 of Example 3, the semiconductor device (1) with terminals having a terminal height of h0 = 200 μm was used to confirm the embedding property ((d1 / h0) was 4.0) immediately after punching. The results were as follows: Figure 5 As shown in (b), the lower surface of all semiconductor devices with terminals is bonded to the terminal protection tape, and the terminals are covered by the terminal protection tape and cannot be observed (the embedding property is good immediately after stamping (A)). In addition, the embedding property is confirmed 1 hour after stamping, and the result is as follows Figure 5 As shown in (b), the lower surfaces of all semiconductor devices with terminals were bonded to the terminal protection tape, and the terminals were covered by the terminal protection tape and could not be observed (the embedding property after pressing for 1 hour was good (A)). The results are shown in Table 1.
[0404] [Example 4]
[0405] <Manufacture of terminal protection tape>
[0406] A 120 μm-thick embedding layer A was produced on the release-treated surface of the release film in the same manner as in Example 1 except that the thickness of the embedding layer A was changed.
[0407] The embedding layer A with a thickness of 120 μm was laminated on the adhesive layer B with a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Example 4 having the viscoelastic layer 12 having a thickness of 140 μm is shown.
[0408] <Measurement of shear storage modulus of viscoelastic layer>
[0409] Next, by peeling off the two release films in the terminal protection tape 1 of Example 4, 7 viscoelastic layers 12 with a thickness of 140 μm were stacked, thereby forming a viscoelastic layer with a thickness of 980 μm. Then, in the same manner as in Example 1, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') of the viscoelastic layer 12 in the terminal protection tape 1 of Example 4 were measured. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C were calculated. The results are shown in Table 1.
[0410] <Evaluation of burial properties>
[0411] In the same manner as in Example 1, the terminal protection tape 1 of Example 4 was used to manufacture Figure 2 The terminal-protecting tape 2 of Example 4 has a viscoelastic layer 12 in the form shown.
[0412] Further, in the same manner as in Example 1, the terminal protection tape 2 of Example 4 was used to manufacture Figure 3 The terminal-protecting tape 3 of Example 4 having the viscoelastic layer 12 in the form shown.
[0413] For the terminal protection tape 3 of Example 4, the semiconductor device (2) with terminals having a terminal height of h0 = 100 μm was used to confirm the embedding property ((d1 / h0) was 1.4) immediately after punching. The results were as follows: Figure 5 As shown in (b), the lower surface of all semiconductor devices with terminals is bonded to the terminal protection tape, and the terminals are covered by the terminal protection tape and cannot be observed (the embedding property is good immediately after stamping (A)). In addition, the embedding property is confirmed 1 hour after stamping, and the result is as follows Figure 5 As shown in (b), the lower surfaces of all semiconductor devices with terminals were bonded to the terminal protection tape, and the terminals were covered by the terminal protection tape and could not be observed (the embedding property after pressing for 1 hour was good (A)). The results are shown in Table 1.
[0414] [Comparative Example 1]
[0415] <Terminal protection tape>
[0416] The adhesive layer B having a thickness of 20 μm was used as the terminal protection tape of Comparative Example 1.
[0417] <Measurement of shear storage modulus of viscoelastic layer>
[0418] Multiple adhesive layers B with a thickness of 20 μm were stacked to form a viscoelastic layer with a thickness of 1000 μm. A cylindrical evaluation sample with a diameter of 8 mm and a thickness of 1000 μm was prepared from the viscoelastic layer. The shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') were measured in the same manner as in Example 1 using the sample. The shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C were determined. The results are shown in Table 1.
[0419] <Evaluation of burial properties>
[0420] A 20 μm thick adhesive layer B was laminated on the easy-adhesion treated surface of the substrate A, and the laminating adhesive layer A was laminated on the side of the substrate A opposite to the adhesive layer B, thereby manufacturing a terminal protection tape of Comparative Example 1.
[0421] The release film on the adhesive layer A side of the terminal protection tape of Comparative Example 1 was peeled off and adhered to a SUS plate, and then the release film on the adhesive layer B side was peeled off and placed on a heating plate adjusted to 50° C. with the SUS plate side facing downward. Figure 7 As shown in (a), the semiconductor device with terminals (1) with a terminal height of h0 = 200 μm was pressed onto the terminal protection tape of Comparative Example 1 at a pressing pressure of 1.1 MPa, a pressing time of 40 s, and a heating time of 50° C., with the terminal side of the semiconductor device with terminals facing downward. The embedding property evaluation was performed on 9 semiconductor devices with terminals. The ratio (d1 / h0) of the thickness d1 (μm) of the viscoelastic layer to the height h0 (μm) of the terminal was 0.1.
[0422] Immediately after stamping, observe from the side to confirm the embedding property. The results are as follows Figure 7 As shown in (b), the lower surface of all semiconductor devices with terminals floated from the terminal protection tape, and the terminal was observed between the terminal protection tape and the semiconductor device body (bad embedding property immediately after punching (B)). The results are shown in Table 1.
[0423] Then, the semiconductor device with terminals was cooled to room temperature for 1 hour and then observed from the side to check the embedding property. Figure 7 As shown in (b), the lower surface of all semiconductor devices with terminals floated from the terminal protection tape, and the terminals were observed between the terminal protection tape and the semiconductor device body (poor embedding after 1 hour of pressing (B)).
[0424] [Comparative Example 2]
[0425] <Manufacture of terminal protection tape>
[0426] The embedding layer forming composition B obtained above was applied onto the release-treated surface of a release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) obtained by silicone treatment on one side of a polyethylene terephthalate film, and heated and dried at 120°C for 2 minutes to produce a embedding layer B with a thickness of 300 μm.
[0427] The embedding layer B having a thickness of 300 μm was laminated on the adhesive layer B having a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Comparative Example 2 having the viscoelastic layer 12 having a thickness of 320 μm in the form shown.
[0428] <Measurement of shear storage modulus of viscoelastic layer>
[0429] Next, by peeling off the two release films in the terminal protection tape 1 of Comparative Example 2, a plurality of viscoelastic layers 12 with a thickness of 320 μm were laminated to form a viscoelastic layer with a thickness of 960 μm. Then, in the same manner as in Example 1, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') of the viscoelastic layer 12 in the terminal protection tape 1 of Comparative Example 2 were measured. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C were calculated. The results are shown in Table 1.
[0430] <Evaluation of burial properties>
[0431] The release film on the buried layer B side of the terminal protection tape 1 of Comparative Example 2 was peeled off and laminated on the easy-adhesion treated side of the substrate A, and the laminating adhesive layer A was laminated on the side of the substrate A opposite to the buried layer B, thereby producing Figure 3 The terminal protection tape 3 of Comparative Example 2 of the embodiment shown.
[0432] The release film on the side of the adhesive layer A of the terminal protection tape 3 of Comparative Example 2 was peeled off and the tape was adhered to a SUS plate to prepare a Figure 4 The sample for evaluation of embedding property was prepared by peeling off the release film on the adhesive layer B side and placing it on a heating plate adjusted to 50°C with the SUS plate side facing downward. Next, the semiconductor device (1) with terminals, whose terminal height was h0 = 200 μm, was pressed onto the terminal protection tape 3 of Comparative Example 2 at a pressing pressure of 1.1 MPa, a pressing time of 40 s, and a heating time of 50°C, with the terminal side of the semiconductor device (1) with terminals facing downward. The embedding property evaluation was performed on 9 semiconductor devices with terminals. The ratio (d1 / h0) of the thickness d1 (μm) of the viscoelastic layer to the height h0 (μm) of the terminal was 1.6.
[0433] Immediately after stamping, the embedding property was checked by observing from the side. As a result, the lower surface of all semiconductor devices with terminals floated from the terminal protection tape, and the terminal was observed between the terminal protection tape and the semiconductor device body (bad embedding property immediately after stamping (B)). The results are shown in Table 1.
[0434] Then, after cooling to room temperature for 1 hour, the semiconductor devices with terminals were observed from the side to confirm the embedding property. As a result, the lower surface of all the semiconductor devices with terminals floated from the terminal protection tape, and the terminals were observed between the terminal protection tape and the semiconductor device body (bad embedding property (B) immediately after stamping). The results are shown in Table 1.
[0435] [Comparative Example 3]
[0436] <Manufacture of terminal protection tape>
[0437] The embedding layer forming composition B obtained above was applied onto the release-treated surface of a release film ("SP-PET381031" manufactured by Lintec Corporation, thickness 38 μm) obtained by silicone treatment on one side of a polyethylene terephthalate film, and heated and dried at 120°C for 2 minutes to produce a embedding layer B with a thickness of 150 μm.
[0438] The embedding layer B having a thickness of 150 μm was laminated on the adhesive layer B having a thickness of 20 μm to produce Figure 1 The terminal-protecting tape 1 of Comparative Example 3 having the viscoelastic layer 12 having a thickness of 170 μm in the form shown.
[0439] <Measurement of shear storage modulus of viscoelastic layer>
[0440] Next, by peeling off the two release films in the terminal protection tape 1 of Comparative Example 3, a plurality of viscoelastic layers 12 with a thickness of 170 μm were laminated to form a viscoelastic layer with a thickness of 1020 μm. Then, in the same manner as in Example 1, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') of the viscoelastic layer 12 in the terminal protection tape 1 of Comparative Example 3 were measured. Among them, the shear storage modulus G' and tanδ (loss modulus G" / storage modulus G') at 25°C and 50°C were calculated. The results are shown in Table 1.
[0441] <Evaluation of burial properties>
[0442] The release film on the buried layer B side of the terminal protection tape 1 of Comparative Example 3 was peeled off and laminated on the easy-adhesion treated surface side of the substrate A, and the laminating adhesive layer A was laminated on the side of the substrate A opposite to the buried layer to produce Figure 3 The terminal protection tape 3 of Comparative Example 3 of the embodiment shown.
[0443] The release film on the side of the adhesive layer A of the terminal protection tape 3 of Comparative Example 3 was peeled off and adhered to a SUS plate to prepare a Figure 4The sample for embedding property evaluation was prepared by peeling off the release film on the adhesive layer B side and placing it on a heating plate adjusted to 50°C with the SUS plate side facing downward. Next, the semiconductor device (1) with terminals, whose terminal height was h0 = 200 μm, was pressed onto the terminal protection tape 3 of Comparative Example 3 at a pressing pressure of 1.1 MPa, a pressing time of 40 s, and a heating time of 50°C, with the terminal side of the semiconductor device (1) with terminals facing downward. The embedding property evaluation was performed on 9 semiconductor devices with terminals. The ratio (d1 / h0) of the thickness d1 (μm) of the viscoelastic layer to the height h0 (μm) of the terminal was 0.9.
[0444] Immediately after stamping, the embedding property was checked by observing from the side. As a result, the lower surface of all semiconductor devices with terminals floated from the terminal protection tape, and the terminal was observed between the terminal protection tape and the semiconductor device body (bad embedding property immediately after stamping (B)). The results are shown in Table 1.
[0445] Then, after cooling to room temperature for 1 hour, the semiconductor devices with terminals were observed from the side to confirm the embedding property. As a result, the lower surface of all the semiconductor devices with terminals floated from the terminal protection tape, and the terminals were observed between the terminal protection tape and the semiconductor device body (bad embedding property (B) immediately after stamping). The results are shown in Table 1.
[0446]
[0447] According to the results shown in Table 1, when the terminal protection tape of the example of the present embodiment is used to shield the semiconductor device with the terminal from electromagnetic waves, the tanδ value at 50°C is 0.2 or more in the dynamic viscoelasticity measurement of the viscoelastic layer, and the thickness of the viscoelastic layer is 80 to 800 μm, so the bumps that are prone to floating can be buried in the viscoelastic layer 12, and the terminal forming surface of the semiconductor device can be closely attached to the viscoelastic layer. As a result, it is possible to prevent the bumps as the terminal electrodes from short-circuiting with the electromagnetic wave shielding film, and it is not necessary to set a shielding part with a complicated process.
[0448] Industrial Applicability
[0449] The terminal protection tape of this embodiment can be used to protect the terminals of a semiconductor device with terminals when electromagnetic wave shielding is performed on the semiconductor device with terminals. Using the terminal protection tape of this embodiment, electromagnetic wave shielding can be performed on a semiconductor device with terminals, and a semiconductor device with an electromagnetic wave shielding film can be manufactured.
[0450] Description of Reference Numerals
[0451] 1, 2, 3: terminal protection tape; 10: electromagnetic wave shielding film; 11: substrate; 12: viscoelastic layer; 13: burying layer; 14: adhesive layer; 15: second adhesive layer (bonding adhesive layer); 30: support body; 6: semiconductor device assembly with terminals; 60: semiconductor device assembly; 60a: terminal forming surface; 61, 62: electronic components; 63: circuit substrate; 63a: terminal forming surface; 64: sealing resin layer; 65: semiconductor device with terminals; 66: semiconductor device with electromagnetic wave shielding film; 91: terminal; 101: conductive resin; 20, 21, 22: peeling film.
Claims
1. A terminal protection tape used in a process of forming an electromagnetic wave shielding film on a semiconductor device with terminals, It has a viscoelastic layer. In the dynamic viscoelasticity measurement of the viscoelastic layer, the tan δ value at 50° C. is 0.5 or more and 2.5 or less, and the thickness of the viscoelastic layer is 80 to 800 μm. In the dynamic viscoelasticity measurement of the viscoelastic layer, the tan δ value at 25° C. is in the range of 0.30 to 0.8, the viscoelastic layer comprising a embedding layer and an adhesive layer, The material constituting the buried layer contains an acrylic resin. The adhesive layer contains an adhesive, and the adhesive is an acrylic resin. in, The storage modulus G'(50°C) of the viscoelastic layer at 50°C in MPa, the height h0 of the terminal in μm, and the thickness d1 of the viscoelastic layer in μm satisfy the following equations (1) and (2): 0.01MPa≤G'(50℃)≤15MPa···(1), 1.2≤d1 / h0≤5.0···(2), The storage modulus G'(25°C) of the viscoelastic layer at 25°C in units of MPa satisfies the following formula (3): 0.05MPa≤G'(25℃)≤20MPa···(3). 2 . The terminal protection tape according to claim 1 , comprising the adhesive layer, the embedding layer, and a substrate in this order. 3 . The terminal protection tape according to claim 2 , which is a double-sided tape comprising the adhesive layer, the embedding layer, the base material, and a second adhesive layer in this order.
4. A method for manufacturing a semiconductor device with an electromagnetic wave shielding film, comprising: A step of embedding the terminal of the semiconductor device with a terminal in the viscoelastic layer of the terminal protection tape according to any one of claims 1 to 3; and The step of forming an electromagnetic wave shielding film on an exposed surface of the semiconductor device with terminals which is not embedded in the viscoelastic layer of the terminal protection tape.
5. A method for manufacturing a semiconductor device with an electromagnetic wave shielding film, comprising: A step of embedding the terminals of a semiconductor device assembly with terminals in the viscoelastic layer of the terminal protection tape according to any one of claims 1 to 3; The step of cutting the semiconductor device assembly with terminals to form semiconductor devices with terminals in which the terminals are buried in the viscoelastic layer of the terminal protection tape; and The step of forming an electromagnetic wave shielding film on an exposed surface of the semiconductor device with terminals which is not embedded in the viscoelastic layer of the terminal protection tape.
Citation Information
Patent Citations
Method for manufacturing electronic component module, and electronic component module
JP2011151372A
Adhesive tape for surface protection of a semiconductor wafer and method of producing a semiconductor wafer
CN103525324A
Radiation-curing adhesive tape for dicing
CN104081500A
Electronic component module, and method for manufacturing the same
JP2014183181A
Semiconductor processing sheet
JP2017165880A