Round rod shaped glass and method for producing the same
By thermal elongation on multiple rollers and using a mold release agent, round rod molding glass with a diameter of less than 3.5 mm was successfully manufactured, which solved the problem of difficult molding of small round rods in the prior art, and reduced the optical glass lens Manufacturing cost and waste quantity.
Patent Information
- Application Number
- CN202011078756.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-10
- Filing Date
- 2020-10-10
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2040-10-10
AI Technical Summary
The prior art is difficult to manufacture round rod molded glass with a diameter of less than 6 mm, resulting in high manufacturing cost of optical lenses and large amount of glass waste, and the amount of cutting glass cannot be effectively reduced.
By thermally elongating on a plurality of rollers with concave and convex surfaces, a round rod molded glass with a cross-sectional diameter of 3.5 mm or less is formed, without grinding, and a mold release agent is used during the manufacturing process to reduce adhesion between the glass and the rollers. , realize the forming of small-diameter round rods.
It is achieved to reduce the cost and waste of glass in optical glass lens manufacturing, reduce the amount of glass cutting, and improve the production efficiency.
Smart Images

Figure CN112645570B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a round rod shaped glass having a very small diameter and a method for manufacturing the same. Background Art
[0002] Optical glass is usually obtained as a strip material or an elongated plate material called an E-bar, which is formed into a glass product having a predetermined shape. Specifically, first, a glass piece with a relatively simple shape is produced with the same glass volume as the target object, and then the glass piece is precisely formed. Optical glass is expected to be able to mass-produce products of the same shape from the perspective of industrial convenience, so in the production of the glass piece, it is also expected to be able to mass-produce products of the same shape.
[0003] As an example of a method for manufacturing the glass flakes, the following method can be cited: prepare a slender rectangular parallelepiped glass with one side sufficiently longer than the other sides, shape the rectangular parallelepiped glass into a cylindrical round rod-shaped glass, and then cut it in a direction perpendicular to the height of the cylinder to obtain a sheet-shaped (here, a disc-shaped or cylindrical) glass flake. The sheet-shaped glass flakes are preferably used as materials for optical lenses due to the similarity of their shapes.
[0004] As a method for manufacturing the above-mentioned sheet-shaped glass pieces, for example, there can be cited the method of Patent Document 1. Patent Document 1 discloses "a method for manufacturing a lens, characterized in that a glass block heated to a temperature above the softening temperature and below the flow temperature is loaded between three or more rollers that are parallel to each other and rotate in the same direction, and a glass round rod having a predetermined diameter is gradually formed by gradually clamping the interval between the rotating rollers, and then the glass round rod is cut, molded, and ground to form a lens having a predetermined radius of curvature."
[0005] In addition, Patent Document 2 discloses "a method for manufacturing a glass round rod, wherein a glass blank is introduced by moving it on a guide slope (chute), wherein the glass blank is heated until at least 10 10 The glass blank is formed into a round rod with a circular cross section by rotating the glass blank in a direction opposite to the rotation direction of the rollers, and the glass blank on the guide slope (bevel groove) is moved by the glass blank rolling down on the guide slope (bevel groove). ".
[0006] Patent document 3 discloses "a method for manufacturing small-divided glass blanks for lenses, characterized in that when manufacturing a plurality of small-divided glass blanks for lenses from a glass round rod, the glass round rod is inserted between two rollers rotating in the same direction, the interval between the two rollers is narrowed, the glass round rod heated to a temperature above the softening temperature is pressed from both sides, a plurality of flange-shaped blades are arranged at equal intervals along the axial direction on at least one of the two rollers, a plurality of circumferential grooves are simultaneously formed on the glass round rod, and then the glass round rod is cut at each groove to form small-divided glass blanks of equal weight suitable for lenses."
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: (Japanese) Patent Publication No. 54-117514
[0010] Patent Document 2: (Japanese) Patent Publication No. 2000-16822
[0011] Patent Document 3: (Japanese) Patent Publication No. 2002-114532 Summary of the invention
[0012] Problems to be solved by the invention
[0013] As can be seen from patent documents 1 to 3, the development of a manufacturing method for round rod glass (hereinafter also referred to as round rod formed glass) as a material for sheet glass pieces is being widely promoted. On the other hand, as a glass product, the demand for miniaturized glass products is high, and in the field of optical lenses, the diameter of lenses is also required to be reduced. If the diameter of the cross section of the round rod formed glass as a material for an optical lens can be made to be close to the diameter of the optical lens as a final product, the time and amount of cutting the glass on the side of the round rod formed glass can be reduced, so the glass manufacturing cost can be suppressed, and the amount of waste glass scraps (sludge) discharged along with the cutting of the glass can be suppressed, which is also advantageous in terms of the environment.
[0014] Regarding the diameter of the round-rod-molded glass after round-rod molding, there is no description in Patent Document 1. In addition, in Patent Document 2, paragraph
[0061] discloses a round-rod-molded glass with a diameter of 6 mm, but does not disclose a round-rod-molded glass with a smaller diameter. Furthermore, in Patent Document 3, paragraph
[0029] discloses a round-rod-molded glass with a diameter of 7 mm, but does not disclose a round-rod-molded glass with a smaller diameter.
[0015] Solutions to Solve Problems
[0016] The present inventors focused on the above-mentioned problems and developed a method for obtaining a round glass rod having a diameter of 3.5 mm or less from a round rod forming apparatus by adopting a characteristic production method without grinding or polishing the side surfaces.
[0017] That is, the present invention includes the following contents.
[0018] [1] A round rod shaped glass having a cross-sectional diameter of 3.5 mm or less, a side surface surface roughness Ra of 1.5 or less, and an aspect ratio (major axis / cross-sectional radius) of 35 or more.
[0019] [2] The round rod shaped glass according to [1], wherein at least one end portion has a curvature radius R of 1500 μm or less.
[0020] [3] The round rod shaped glass according to [1] or [2], which is not subjected to grinding treatment.
[0021] [4] The round rod shaped glass according to any one of [1] to [2], which contains a component derived from a release agent.
[0022] [5] The round rod formed glass as described in any one of [1] to [3], wherein the ratio of the content of the release agent on at least one end surface of the round rod formed glass to the content of the release agent in the center portion (inside the glass) of a cross section perpendicular to the length direction of the round rod formed glass is 0.5 or less.
[0023] [6] The round rod shaped glass according to [4] or [5], wherein the release agent is boron nitride.
[0024] [7] An optical glass material obtained by cutting and grinding the round rod-shaped glass described in [1] to [6].
[0025] [8] A method for producing round-rod shaped glass, comprising the step of thermally stretching prism glass or round-rod glass using a plurality of rollers having projections and depressions on the surface to form a round-rod shaped glass having a cross-sectional diameter of 3.5 mm or less.
[0026] [9] The manufacturing method according to [8], wherein the diameter of the roller is 20 mm or less.
[0027]
[10] The manufacturing method according to [8] or [9], wherein the difference between the maximum height and the minimum height of the projections and recesses is greater than or equal to 0.1 mm and less than or equal to 1.0 mm.
[0028] Effects of the Invention
[0029] Since the round rod molded glass of the present invention has a small cross-sectional diameter of less than 3.5 mm, if it is used as a material, the amount of cut glass can be suppressed when manufacturing small glass products (especially optical glass lenses), the glass manufacturing cost can be suppressed, and the amount of glass waste can be reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 (a) to (d) are schematic diagrams of the forming process of round rod-shaped glass.
[0031] Figure 2 It is a figure which shows the surface processing state of the roller used in Example.
[0032] Figure 3 is a side view of round rod-shaped glass ( Figure 3 (a)), and a side view of the end of a glass having a side surface cold-worked (glass having a side surface cut) ( Figure 3 (b)).
[0033] Description of Reference Numerals
[0034] 11 Prismatic glass
[0035] 12 Round rod shaped glass
[0036] 2(21, 22, 23) Rollers
[0037] 201 Roller
[0038] 202 Glass contact part DETAILED DESCRIPTION
[0039] In this specification, "%" used to indicate glass components means "mass %" unless otherwise specified. In addition, in this specification, the upper and lower limits of "to" used to determine the numerical range are included in the range. For example, when the content of a glass constituent component is expressed as "10 to 20%", it means 10% or more and 20% or less by mass.
[0040] In addition, the content (content ratio) of the glass components can be quantified by known methods, such as inductively coupled plasma atomic emission spectroscopy (ICP-AES), inductively coupled plasma mass spectrometry (ICP-MS), etc. In the present invention, the content of a glass component of 0% means that the component is essentially not contained, and the component is allowed to be contained at an unavoidable impurity level.
[0041] [Method for producing round rod-shaped glass]
[0042] (Round rod forming device)
[0043] The method for producing round rod shaped glass of the present invention comprises the step of heat-stretching prism glass or round rod glass by a plurality of rollers having concavoconvex surfaces to form round rod shaped glass having a cross-sectional diameter of 3.5 mm or less. Figure 1 Provide detailed explanation.
[0044] like Figure 1 As shown in FIG. 1 , the method for manufacturing round rod shaped glass is performed by a round rod forming device having a plurality of, preferably three, rollers. The details are described by taking the case of using three rollers as an example. First, softened prism glass 11 ( 11.1 ) is supplied to two rollers 21 and 22 that are in contact with or close to each other by rolling on a supply member 3. Figure 1 (a) and (b)). Next, the movable roller 23 is arranged to contact the prism glass 11, and the three rollers are rotated in the same direction ( Figure 1 (c)). When the rollers 21, 22, and 23 are rotated, the prism glass 11 is also rotated, and the prism glass 11 is stretched in the longitudinal direction (long axis direction) while gradually deforming from a prism to a cylindrical shape. The rotation of the rollers 21, 22, and 23 is continued until the prism glass 11 is stretched to a desired diameter (less than 3.5 mm) ( Figure 1 (d)), and then removed from the rollers 21, 22, 23 to obtain a round rod shaped glass 12.
[0045] The plurality of rollers used in round rod forming glass may be in contact with each other or may be separated. The upper limit of the gap between the rollers is preferably 1.5 mm or less, more preferably 1.0 mm or less, further preferably 0.8 mm or less, and further preferably 0.5 mm or less. When manufacturing round rod forming glass with a small cross-sectional diameter, the gap is preferably small. The parallelism between the rollers is preferably less than 0.1, more preferably less than 0.05.
[0046] The roller 2 is composed of a roller shaft 201 and a glass contact portion 202 disposed outside the roller shaft. The side surface of the prism glass 11 or the round rod-shaped glass 12 contacts the glass contact portion 202. Specific examples of the roller 2 include: Figure 2 (a), (b), (c). The surface of the glass contact portion 202 may be processed to form projections and depressions (for example, knurling). Figure 2 (a) is knurling and embossing processing, Figure 2 (b) is knurling twill processing. In addition, the glass contact portion 202 can also be coated without knurling. For example, Figure 2 The roller shown in (c) is a roller having a coating having projections and depressions (for example, applied by Gripping Venus Japan Coating Center Co., Ltd.) applied on the glass contact portion 202. It should be noted that even a roller having a Gripping Venus coating can have an effect of suppressing slippage, but the reproducibility is sometimes inferior to that of a roller having a processed roller shape.
[0047] When the cross-sectional diameter of the round rod-shaped glass is set to 3.5 mm or less, the glass is softened further than when a round rod-shaped glass with a larger diameter is manufactured, so the temperature of the roller is set higher. Therefore, the glass is easy to slip relative to the roller. However, since the glass contact portion 202 has unevenness on the surface, the gripping force on the glass can be increased, and the slip phenomenon can be suppressed.
[0048] It should be noted that knurling or coating to give the roller surface an irregularity of 1 μm or more and 1.0 mm or less can be expected to improve gripping force. However, from the viewpoint of maintaining the shape of the irregularities when the roller is used repeatedly, it is preferable to have irregularities by knurling.
[0049] The difference in the concavoconvexity (maximum height - minimum height) formed by knurling is preferably 0.1 mm or more and 1.0 mm or less. The lower limit of the difference in the concavoconvexity is preferably 0.3 mm, more preferably 0.5 mm, and further preferably 0.6 mm. The upper limit of the difference in the concavoconvexity is preferably 0.9 mm, more preferably 0.8 mm, and further preferably 0.7 mm.
[0050] In order to obtain round rod-shaped glass with a small diameter, it is necessary to reduce the cross-sectional diameter of the roller (the glass contact portion of the roller). The cross-sectional diameter of the roller is preferably less than 20.0 mm for multiple rollers used, more preferably less than 18.0 mm, and further preferably less than 16.0 mm. In order to reduce the cross-sectional diameter of round rod-shaped glass, it is necessary to reduce the cross-sectional diameter of the roller, but if the cross-sectional diameter is too small, sufficient rigidity to withstand glass deformation cannot be obtained. Therefore, the cross-sectional diameter of the roller is preferably greater than 5.0 mm, more preferably greater than 7.0 mm, and further preferably greater than 9.0 mm.
[0051] In the method for producing round rod-shaped glass, first, glass of a material having a predetermined shape is put into a softening furnace to soften the glass.
[0052] It should be noted that, as a standard for the temperature of the softening furnace, the actual temperature of the furnace environment of the softening furnace (sometimes referred to as "the furnace temperature of the softening furnace" in this specification) is preferably the softening point of the glass (T 10 7.65) and less than the flow temperature. This is because, if the temperature in the softening furnace is lower than the softening point of the glass, the deformation of the glass is insufficient and is not preferred. On the other hand, if the temperature in the softening furnace is higher than the flow temperature, it causes the glass to fuse with the roller surface and is not preferred. By adjusting the temperature in the softening furnace of the glass to the above range, the glass can be sufficiently elongated in the subsequent process, and round rod-shaped glass of less than 3.5 mm can be obtained. The temperature in the softening furnace is preferably above the softening point + 50°C, more preferably above the softening point + 80°C, and further preferably above the softening point + 90°C. On the other hand, the upper limit of the temperature in the softening furnace for softening the glass is preferably above the softening point + 250°C, more preferably above the softening point + 200°C, and further preferably above the softening point + 180°C.
[0053] It should be noted that in the actual softening process, it is important to soften the glass within a certain period of time. At this time, the heat Q = (Tf-Ts) × t generated by the product of the furnace temperature Tf, the temperature Ts of the glass arranged in the furnace, and the holding time t is set to a certain value so that the temperature Ts of the glass reaches the softening point within a limited time. Based on this idea, the furnace temperature Tf and the holding time t are determined. Therefore, in the present invention, the furnace temperature Tf and the holding time t are not limited to the specific temperature and time of the embodiment.
[0054] Next, the glass softened in the softening furnace is moved to a round rod forming machine, and the rollers are rotated to form a round rod. There is no particular restriction on the roller temperature for round rod forming, but if the roller temperature is too high, it becomes difficult to control the adhesion of the glass due to thermal degradation of the rollers, and therefore the roller temperature is preferably 800°C or less. The upper limit of the softening point of the glass is preferably 750°C or less, more preferably 700°C or less, further preferably 650°C or less, further preferably 600°C or less, and particularly preferably 550°C or less. There is no particular restriction on the preferred lower limit of the softening point, and as a standard, a softening point of 400°C or more is sufficient.
[0055] (Release Agent)
[0056] Before the prism glass (or round rod glass) of the material is formed by the round rod forming device, a release agent may be applied to the surface of the prism glass. By applying the release agent, the round rod formed glass 12 can be easily removed from the round rod forming device. In addition, the release agent may be applied not only to the prism glass (or round rod glass) but also to the roller.
[0057] The release agent is attached to the surface of the glass and is used to easily remove the round rod-shaped glass from a roller or the like. Therefore, the release agent has a tendency to spread thinner toward both ends of the round rod-shaped glass due to elongation. Therefore, regarding the content of the release agent contained in the round rod-shaped glass of the present invention, the ratio of the content of the release agent at at least one end of the round rod-shaped glass when the content of the release agent at the center (inside the glass) in the cross section perpendicular to the longitudinal direction is 1 may be 0.5 or less. Sometimes, it may be 0.4 or less, or 0.2 or less.
[0058] Since the round-rod shaped glass 12 is shaped by the above-described method, components derived from the mold release agent may be contained near the surface of the obtained round-rod shaped glass 12 .
[0059] It should be noted that as a mold release agent, a mold release agent containing boron nitride (BN) is preferably used. Molybdenum disulfide can also be used, but since molybdenum disulfide has lower heat resistance than boron nitride, boron nitride is preferred.
[0060] [Round rod molded glass]
[0061] The round rod shaped glass of the present invention has a cross-sectional diameter of 3.5 mm or less, a surface roughness Ra of the side surface of 1.5 or less, and an aspect ratio (major axis / cross-sectional radius) of 35 or more. This will be described in detail below.
[0062] (shape)
[0063] The round-rod shaped glass of the present invention is a long and thin round rod having a cylindrical shape. Since the round-rod shaped glass is formed by heat stretching as described above, the end portion thereof forms a curved surface protruding in the longitudinal direction.
[0064] The cross-sectional diameter of the round rod molded glass is 3.5 mm or less. If it is 3.5 mm or less, the amount of glass waste can be reduced when molding into the final product, and the glass manufacturing cost can be reduced. The cross-sectional diameter is preferably 3.0 mm or less, and more preferably 2.8 mm or less.
[0065] The length of the major axis of the round rod molded glass depends on the shape of the glass used as the material, and is not particularly limited, but may be, for example, 30 mm or more.
[0066] (Surface roughness Ra, Rz of side surface)
[0067] The surface of the side surface of the round rod molded glass of the present invention, except for the end, is formed by the stretching method of the roller 2. Therefore, compared with the cut side surface, the values of Ra and Rz are small, and it is not easy to have cracks or notches caused by impact during transportation or handling. The Ra of the side surface of the round rod molded glass is preferably 1.5 μm or less, more preferably 1.4 μm or less, and further preferably 1.3 μm or less. In addition, the Rz of the side surface of the round rod molded glass is preferably 10.0 μm or less, more preferably 9.0 μm or less, and further preferably 8.0 μm or less. It should be noted that the Ra and Rz recorded in this specification are values obtained using a surface roughness and profile shape measuring machine (model: SURFCOM 2900SD3 (manufactured by Tokyo Seimitsu Co., Ltd.)).
[0068] (Aspect Ratio)
[0069] The round rod shaped glass of the present invention is further elongated than before, so that the diameter of the cross section is 3.5 mm or less. Therefore, when using materials of the same shape, a round rod shaped glass with a large aspect ratio can be obtained compared with the conventional method. The aspect ratio (length of the major axis / cross section radius) of the round rod shaped glass of the present invention is preferably 35 or more, more preferably 38 or more, and even more preferably 40 or more.
[0070] (Curvature radius R of the end)
[0071] The round rod shaped glass of the present invention is obtained by stretching from a prism glass (or round rod glass according to the case) of a size that is easy to handle to obtain a round rod shaped glass with a cross-sectional diameter of 3.5 mm or less. Therefore, the radius of curvature R of the end is smaller than that of a cold-processed product (grinding or polishing the side surface), and has the advantage that cracks or notches caused by impact on the end during transportation or handling are not easily generated. The preferred radius of curvature R of at least one end of the round rod shaped glass is 1500 μm or less, more preferably 1300 μm or less, further preferably 1200 μm or less, further preferably 1100 μm or less, and further preferably 1000 μm or less. The radius of curvature R described in this specification is a value obtained using a surface roughness profile measuring machine (model: SURFCOM2900SD3 (manufactured by Tokyo Seimitsu Co., Ltd.)).
[0072] (Surface angle α)
[0073] At least one end of the round rod shaped glass of the present invention has a smaller surface angle α than when the side surface is ground or polished. Here, the surface angle α refers to the angle formed by the side surface portion of the cylinder at the end of the round rod and the tangent line (contact surface). When the side surface is ground, if the outer periphery of the cylindrical shaped glass is ground, the side surface portion is ground while leaving the upper side of the circular end, so the angle formed by the side surface portion of the cylinder and the tangent line (contact surface) of the end of the round rod becomes larger.
[0074] The radius of curvature R is shown together with the face angle α. Figure 3 . Figure 3 (a) is an enlarged view of the end of the round rod-shaped glass of the present invention, Figure 3 (b) is an enlarged view of the end of the round glass rod when the side is ground and polished. Figure 3 (a) and (b) can also be understood that the surface angle α of the round rod glass that has been ground and polished on the side is larger, and the round rod glass has the advantage that it is difficult to produce cracks or gaps when it contacts other parts or the round rod glass during transportation or processing.
[0075] The surface angle α of at least one end of the round rod molded glass of the present invention is preferably 27° or less, more preferably 25° or less, further preferably 23° or less, and further preferably 21° or less. The surface angle α described in this specification is a value obtained using a surface roughness profile measuring machine (model: SURFCOM2900SD3 (manufactured by Tokyo Seimitsu Co., Ltd.)).
[0076] (Materials for round rod-shaped glass (prismatic glass, round rod glass))
[0077] As the material of the round rod forming glass, a rectangular parallelepiped prismatic glass or a cylindrical round rod glass is used. By placing these glasses in a round rod forming device and stretching the glass, round rod forming glass can be obtained. The shape of the prismatic glass or round rod glass as the material of the round rod forming glass is not particularly limited as long as it can be placed in a round rod forming device and formed. If it is a prismatic glass, in order to prevent the cross section of the obtained round rod forming glass from becoming an ellipse, the cross section is preferably a square. Prismatic glass can be directly cut out from the flowing glass from the glass melting furnace after solidifying into a plate shape, so it is easy to obtain.
[0078] (Shape change rate)
[0079] As described above, the manufacturing method of the present invention greatly stretches the material to obtain a round rod-shaped glass, so the shape change rate is large. For example, the change rate C between the long axis of the prism glass as the material and the long axis of the round rod-shaped glass is L It depends on the shape of the prism glass selected as the material, but is preferably 2.7 or more, more preferably 2.9 or more.
[0080] In addition, the change rate C of the aspect ratio of the prism glass and the round rod molded glass A It is preferably 4.0 or more, more preferably 5.0 or more, and further preferably 5.5 or more.
[0081] It should be noted that, as for the cross-sectional radius used in the calculation of the aspect ratio, in the case of prism glass, half the length of any side of the cross section is used as the cross-sectional radius.
[0082] The type of glass that can be used is not particularly limited. As mentioned above, the temperature for softening the glass (the temperature in the softening furnace) is determined according to the type of glass, so the softening point (T 10 7.65 ) requires prior confirmation.
[0083] (Knoop hardness)
[0084] It should be noted that in the present invention, since cracks are less likely to occur than in a round bar after grinding, the Knoop hardness of the glass used in the material of the shape of the present invention is preferably 600 or less. It is more preferably 550 or less, further preferably 500 or less, further preferably 450 or less, further preferably 400 or less, and particularly preferably 350 or less. There is no specific lower limit for the Knoop hardness, but as a standard, a Knoop hardness of 100 or more is sufficient.
[0085] As a glass material with low Knoop hardness, there can be cited glasses whose main component of the glass skeleton is not SiO2, that is, glasses whose cation % ratio of SiO2 / (B2O3+P2O5) is 1 or less, preferably 0.5 or less, more preferably 0.2 or less, and more preferably 0.1 or less. In addition, there can be cited glasses whose cation % ratio of (SiO2+B2O3) / P2O5) is 1 or less, preferably 0.5 or less, more preferably 0.2 or less, and further preferably 0.1 or less, and whose anion % ratio of F / O is 0.01 or more, more preferably 0.10 or more, and further preferably 0.20 or more.
[0086] (Wear)
[0087] As another point of view, from the perspective of reducing production costs by being able to form a round rod without grinding, the lower the wear degree and the longer the grinding time of the glass, the greater the advantage of using this method to make an approximate shape. Therefore, it is preferred to use glass with a wear degree of 125 or less. The more preferred upper limit of the wear degree is 100 or less, more preferably 90 or less, further preferably 80 or less, further preferably 70 or less, and particularly preferably 60 or less. The preferred lower limit of the wear degree is not particularly limited, and as a standard, a wear degree of 10 or more can be considered. As a glass with high wear degree, for example, a glass with a total content of Re2O3 (Re is a rare earth element containing La, Gd, Yb, Lu and Y) in the glass of more than 30% and a ratio of Re2O3 / (SiO2+B2O3+P2O5) of more than 20% can be exemplified.
[0088] As a glass with a low softening point, a glass with a large value of (10×Li+Na+K+Zn+Bi+F-Si / 2-(La+Gd+Y+Yb) / 4) can be exemplified. Specifically, if the initial value is below -10, thermal degradation of the component becomes significant. On the other hand, if the initial value is above 0, there is a tendency for the softening point of the glass to be below 700°C, and the obtained glass can also be provided for precision pressing, so the utilization value of the present invention is high. The value is more preferably above 10, further preferably above 20, and further preferably above 30. Even more preferably above 40.
[0089] [Example]
[0090] Example
[0091] Hereinafter, the present invention will be further described by way of examples. It should be noted that the present invention is not limited to the examples.
[0092] [Production of round rod-shaped glass]
[0093] First, glass raw materials (content ratio is mass %) are mixed, melted at 1300-1450°C depending on the glass state, cast into a mold, and annealed at a temperature of 50°C-100°C plus the Tg temperature of each glass to obtain a plate-shaped optical glass. The composition (mass % of elements) of each glass is shown in Table 6, and the glass properties are shown in Table 7.
[0094] Next, the plate-shaped glass was cut and the like, and material glass (prism glass or cylindrical glass) having the shape shown in Table 2 was obtained.
[0095] In addition, for Examples 1 to 6, round rod forming glass was produced at the roller temperature shown in Table 1 using a round rod forming device A equipped with a roller of 9 mm in diameter (the characteristics of the obtained round rod forming glass are shown in Table 2). The material glass used was glass softened in advance in a softening furnace (temperature and residence time are shown in Table 1). For Comparative Example 1, round rod forming glass was produced in the same manner using a conventional round rod forming device B equipped with a roller of 30 mm in diameter. The shape change rate, surface roughness, and end shape of the obtained round rod forming glass are shown in Table 3.
[0096] In addition, for Examples 7 to 9, the round rod forming device A was also used to obtain round rod shaped glasses shown in Table 4. In addition, for Examples 2 to 6, the round rod forming device B was used to obtain round rod shaped glasses with a diameter of 7.5 mm as shown in Table 4. It should be noted that for Comparative Examples 3 to 6, the side surfaces of the obtained 7.5 mm diameter were cut to obtain round rod shaped glasses cut to a predetermined cross-sectional diameter. The obtained cut round rod shaped glasses did not satisfy the present invention in terms of aspect ratio, surface roughness, and end shape.
[0097] [Table 1]
[0098]
[0099] [Table 2]
[0100]
[0101] [Table 3]
[0102]
[0103] [Table 4]
[0104]
[0105] [Table 5]
[0106]
[0107] [Table 6]
[0108]
[0109] [Table 7]
[0110]
[0111] The improved round rod forming device (round rod forming device A) provides round rod formed glass of the present invention having a diameter of 3.5 mm or less. The surface roughness Ra of the side surface of the round rod formed glass is 1.5 or less, and the aspect ratio (major axis / cross-sectional radius) is 35 or more. Glass having such characteristics could not be produced by conventional round rod formed glass, but can be produced for the first time according to the present invention.
[0112] Industrial Applicability
[0113] The present invention is useful in the technical field of optical glass. In particular, the round rod-shaped glass of the present invention has a small cross-section diameter, so when molding a glass lens, the amount of glass scraps can be reduced.
Claims
1. A method for manufacturing round rod shaped glass, characterized in that: The process comprises the steps of heat-stretching prism glass or round rod glass by using a plurality of rollers to form round rod shaped glass. The roller has a roller shaft and a glass contact portion arranged outside the roller shaft, and the surface of the glass contact portion has irregularities. By rotating a plurality of rollers in the same direction, the prism glass or round rod glass is rotated and deformed into a cylindrical shape while being stretched in the longitudinal direction. The cross-sectional diameter of the round rod shaped glass formed is 3.5 mm or less, At least one end of the round-rod shaped glass is formed of a curved surface protruding in the length direction.
2. The manufacturing method according to claim 1, characterized in that The diameter of the roller is 20 mm or less.
3. The manufacturing method according to claim 1 or 2, characterized in that: The difference between the maximum height and the minimum height of the concavoconvexities is 0.1 mm or more and 1.0 mm or less.
4. The manufacturing method according to claim 1 or 2, characterized in that: At least one end portion of the round-rod shaped glass has a curvature radius R of 1500 μm or less.
5. The manufacturing method according to claim 1 or 2, characterized in that: No grinding process was performed.
6. The manufacturing method according to claim 1 or 2, characterized in that: The round rod molded glass contains a component derived from a release agent.
7. The manufacturing method according to claim 1 or 2, characterized in that: The ratio of the content of the release agent on at least one end surface of the round rod-shaped glass to the content of the release agent in the center of the cross section perpendicular to the longitudinal direction of the round rod-shaped glass, that is, inside the glass, is 0.5 or less.
8. The manufacturing method according to claim 6, characterized in that: The release agent is boron nitride.
9. A round rod shaped glass, characterized in that: It is formed by the manufacturing method according to any one of claims 1 to 8, The surface roughness Ra of the side surface is 1.5 μm or less, and the aspect ratio, that is, the major axis / cross-sectional radius, is 35 or more.