Semiconductor devices

By using a 2-level field plate structure composed of a semi-insulating film and a silicon oxide film in the semiconductor device, the problem of insufficient moisture resistance of the power module in a high-humidity environment is solved, the voltage resistance and moisture resistance are significantly improved, and the service life of the equipment is extended. .

CN112713124BActive Publication Date: 2024-10-25MITSUBISHI ELECTRIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011123282.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-10-25
Filing Date
2020-10-20
Publication Date
2024-10-25
Estimated Expiration
2040-10-20

AI Technical Summary

Technical Problem

In a high-humidity environment, the moisture resistance of power modules is insufficient, and moisture intrusion leads to device corrosion and reduced reliability. The aluminum electrodes in the terminal area of ​​the existing technology are easily affected by moisture, and the moisture resistance is insufficiently improved.

Method used

Design a semiconductor device that adopts a structure in which a main current flows in the thickness direction of a semiconductor substrate. An active area and a terminal area are provided. A semi-insulating film is used to cover the terminal area. A silicon oxide film functions as a field plate and is passed through a polysilicon film and a terminal area. The semi-insulating film forms a 2-stage field plate structure to improve voltage and moisture resistance.

Benefits of technology

The moisture resistance and voltage resistance of the semiconductor device are significantly improved, and the service life in a high-humidity environment is extended. The moisture resistance is better than the existing structure, the voltage resistance is increased by more than 1.2 times, the width of the terminal area is reduced, and the electric field distribution is more uniform.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112713124B_ABST
    Figure CN112713124B_ABST
Patent Text Reader

Abstract

A semiconductor device with improved moisture resistance is provided. A main current flows in the thickness direction of a semiconductor substrate, the semiconductor substrate has an active region through which the main current flows and a terminal region surrounding the active region outside the active region, and the semiconductor device has: a first main electrode provided on the active region; a second main electrode provided on the semiconductor substrate opposite to the first main electrode; an impurity region provided on the upper layer of the semiconductor substrate located at the outermost periphery of the terminal region; a first insulating film provided at the outer edge of the terminal region from above the inner edge of the impurity region to a portion of the upper portion of the semiconductor substrate; a second insulating film provided from above the inner edge of the terminal region to the edge of the active region; a first semi-insulating film covering from a portion of the impurity region not covered by the first insulating film to at least a portion of the upper portion of the first insulating film; and a second semi-insulating film covering from above the first semi-insulating film to a portion of the upper portion of the first main electrode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a semiconductor device, and more particularly to a semiconductor device having a bipolar transistor having an insulated gate. Background Art

[0002] The power module includes a power device, an insulating substrate, a resin case, a packaging material, etc. The power device is assembled into the power module and used in various applications. The power module is sometimes used in a harsh environment, such as a high humidity environment, and the long-term reliability of the power module is required.

[0003] For example, in a high humidity environment, moisture intrudes from the gap of the resin shell, and gradually intrudes into the packaging material from the surface and end face of the packaging material. After a period of time, it reaches the surface of the power device. "The influence of humidity on the high voltage blocking reliability of power IGBT modules and means of protection" (C, Papadopoulos, et al. Microelectronics Reliability, 88-90 (2018), 470-475.) discloses that moisture or mobile ions of moisture decomposed by the high electric field on the end surface of the power device corrode the aluminum film, causing physical damage or electrical damage to the device.

[0004] In addition, Fig. 1(c) of non-patent document 1 discloses a technology that applies SCC (Surface-Charge-Control) to a structure having an LNFLR (Linearly Narrowed Field Limiting Ring) as a terminal structure of a terminal region provided at the periphery of an active region, thereby improving the reliability of a power device, wherein a unit cell of a transistor is formed in the active region. In addition, Fig. 1(c) of non-patent document 1 is referred to as a conventional structure below.

[0005] Non-patent literature 1: S. Honda, et al, "High voltage device edge termination forwide temperature range plus humidity with surface charge control (SCC) technology", ISPSD2016, pp.291-294, 2016

[0006] In the case of the LNFLR using the SCC disclosed in non-patent document 1, the terminal region is covered with a semi-insulating film instead of an insulating film, a silicon oxide film covers a high-concentration N-type impurity region provided on the upper portion of the silicon substrate at the outermost periphery of the terminal region and the silicon substrate in the vicinity thereof, an aluminum electrode connected to the N-type impurity region climbs onto the silicon oxide film, and the aluminum electrode and the silicon oxide film are covered with a semi-insulating film.

[0007] The semi-insulating film functions as a carrier path. Carriers generated when the power device is electrically biased flow over the semi-insulating film and are discharged without being accumulated in the terminal region, thereby improving the reliability of the power device.

[0008] However, since the aluminum electrode in the terminal region is close to the inner surface of the resin case, it is easily affected by moisture that penetrates from the gap in the resin case, and there is room for improvement in moisture resistance. Summary of the invention

[0009] The present invention has been made to solve the above-mentioned problems, and an object of the present invention is to provide a semiconductor device having improved moisture resistance.

[0010] The semiconductor device according to the present invention is a semiconductor device in which a main current flows in the thickness direction of a semiconductor substrate, wherein the semiconductor substrate has: an active region in which the main current flows; and a terminal region which surrounds the active region on the outside compared with the active region, and the semiconductor device has: a first main electrode which is arranged on the active region; a second main electrode which is arranged on the opposite side of the semiconductor substrate to the first main electrode; an impurity region which is arranged on the upper layer of the semiconductor substrate located at the outermost periphery of the terminal region; a first insulating film which is arranged on the outer edge of the terminal region from above the inner edge of the impurity region to a part of the upper part of the semiconductor substrate; a second insulating film which is arranged from above the inner edge of the terminal region to the edge of the active region; a first semi-insulating film which covers from the part of the impurity region not covered by the first insulating film to at least a part of the upper part of the first insulating film; and a second semi-insulating film which covers from above the first semi-insulating film to a part of the upper part of the first main electrode.

[0011] Effects of the Invention

[0012] According to the semiconductor device according to the present invention, it is possible to obtain a semiconductor device having improved moisture resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a plan view schematically showing the upper surface structure of the semiconductor device according to the first embodiment of the present invention.

[0014] Figure 2 It is a cross-sectional view showing the structure of a semiconductor device according to Embodiment 1 of the present invention.

[0015] Figure 3 It is a cross-sectional view showing the structure of a semiconductor device according to a second embodiment of the present invention.

[0016] Figure 4 It is a cross-sectional view showing the structure of a semiconductor device according to a third embodiment of the present invention.

[0017] Figure 5 This is a diagram showing an equivalent circuit used in a moisture resistance test.

[0018] Figure 6 It is a graph showing the experimental results of the moisture resistance test.

[0019] Figure 7 This is a diagram showing the comparison results of the surface electric field distribution of the semiconductor devices in the first and second embodiments according to the present invention.

[0020] Figure 8 It is a diagram showing the depth distribution of the silicon nitride film.

[0021] Fig. 9 It is a cross-sectional view showing the structure of a semiconductor device according to a modification of the first embodiment of the present invention.

[0022] Fig.10 It is a cross-sectional view showing the structure of a semiconductor device according to a modification of the first embodiment of the present invention.

[0023] Fig.11 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0024] Fig.12 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0025] Fig.13 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0026] Fig.14 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0027] Fig.15 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0028] Fig.16 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0029] Fig.17 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0030] Fig.18 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0031] Fig.19 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0032] Fig. 20 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0033] Fig.21 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0034] Fig. 22 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0035] Fig.23 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0036] Fig.24 It is a cross-sectional view for explaining a method for manufacturing a semi-insulating film.

[0037] Description of the label

[0038] 3 semiconductor substrate, 4 impurity region, 5, 51 silicon oxide film, 6, 7 semi-insulating film, 8 polysilicon film, 9 trench, 15 emitter electrode, 23 collector electrode (electrode). DETAILED DESCRIPTION

[0039] <Foreword>

[0040] In the following description, "unit region" refers to the region forming the minimum unit structure of the transistor, i.e., the unit cell, and is also the "active region" through which the main current flows when the semiconductor device is in the on state. In addition, in the following, "outside" is the direction toward the periphery of the semiconductor device, and "inside" is the direction opposite to "outside". In addition, in the following, regarding the conductivity type of the impurity, the N type is usually defined as the "first conductivity type", and the P type, which is the conductivity type opposite to the N type, is defined as the "second conductivity type", but it can also be defined in the opposite sense.

[0041] In addition, the accompanying drawings are schematically shown, and the size and position of the images shown in different drawings may not be accurately recorded and may be appropriately changed. In addition, in the following description, the same structural elements are marked with the same reference numerals for illustration, and their names and functions are also the same. Therefore, their detailed description is sometimes omitted. In addition, in this specification, in the case of "above ~" and "covering ~", it does not prevent the presence of inclusions between the structural elements. For example, in the case of "B arranged on A" or "A covering B", it can be indicated that other structural elements C are arranged between A and B, or it can be indicated that other structural elements C are not arranged between A and B. In addition, in the following description, sometimes "upper", "lower", "side", "bottom", "table" or "back" are used to indicate specific positions and directions, but these terms are used for convenience in order to facilitate the understanding of the contents of the implementation method, and have nothing to do with the direction during actual implementation.

[0042] <Implementation Method 1>

[0043] Figure 1 FIG. 1 is a top view schematically showing the upper surface structure of an IGBT (Insulated Gate Bipolar Transistor) 100 according to the first embodiment of the present invention. Figure 1 As shown, the IGBT 100 is provided on a semiconductor substrate having a quadrangular shape in a plan view, and is roughly divided into a cell region CR (active region) in the center and a termination region TR in the periphery thereof.

[0044] Figure 2 yes Figure 1 The sagittal section at line AA is shown in Figure 1. Figure 2 As shown, the IGBT 100 has an impurity layer 11 which is selectively provided at 1×10 12 ~1×10 13 / cm 3 The concentration (N - ) The upper layer of the semiconductor substrate 3 containing N-type impurities is 1×10 15 ~1×10 16 / cm 3 The concentration (N) of the N-type impurity is 1×10 16 ~1×10 18 / cm 3The semiconductor substrate 3 has a P-type impurity concentration (P); and a trench gate electrode 16, which is provided in a manner that it is in contact with the side of the well layer 12 and the impurity layer 11 from the outermost surface of the semiconductor substrate 3 and reaches into the semiconductor substrate 3. In addition, it has: a gate insulating film 161, which is provided on the side of the trench gate electrode 16; an emitter region 13, which is selectively provided in the upper layer of the well layer 12, and is partially in contact with the gate insulating film 161, with a 1×10 15 ~1×10 16 / cm 3 The concentration (N) contains N-type impurities; the contact region 14 is selectively provided in the upper layer of the well layer 12, with a concentration of 1×10 18 ~1×10 19 / cm 3 The concentration (P ++ ) contains P-type impurities; and a dummy trench gate electrode 160, which is arranged on the outside of the trench gate electrode 16.

[0045] The dummy trench gate electrode 160 has a gate insulating film 161 on the side surface similarly to the trench gate electrode 16 , but is given an emitter potential similarly to the contact region 14 .

[0046] The inner dummy trench gate electrode 160 of the two dummy trench gate electrodes 160 is directly connected to the emitter electrode 15 (first main electrode), but the outer dummy trench gate electrode 160 is connected to the emitter electrode 15 via a contact hole (not shown) provided in the extending direction of the trench.

[0047] Furthermore, the trench gate electrode 16 is covered with an interlayer insulating film 162 , and the emitter electrode 15 covers the interlayer insulating film 162 .

[0048] The dummy trench gate electrode 160 is provided for the purpose of maintaining the withstand voltage of the IGBT 100 and preventing oscillation, but is not an essential structure, and a structure without the dummy trench gate electrode 160 may be provided.

[0049] In addition, a guard ring 17 is provided on the upper layer of the semiconductor substrate 3 from the outer edge of the cell region CR to the inner edge of the termination region TR. 17 ~1×10 18 / cm 3 The concentration (P + ) contains P-type impurities.

[0050] The guard ring 17 is provided for the purpose of maintaining the withstand voltage of the IGBT, and suppresses the electric field concentration from occurring at the bottom of the trench gate electrode 16 at the outermost periphery of the cell region CR.

[0051] The contact region 14 is also selectively provided on the upper layer portion of the guard ring 17 . The contact region 14 is connected to the emitter electrode 15 , and an emitter potential is applied to the guard ring 17 .

[0052] In addition, a 1×10 15 ~1×10 16 / cm 3 The concentration (P - ) A reduced surface field layer (RESURF: Reduced Surface Field) 18 containing P-type impurities. The reduced surface field layer 18 is provided for the purpose of maintaining a withstand voltage, and reduces the electric field at the outer edge of the guard ring 17 .

[0053] In addition, on the outside of the surface electric field reduction layer 18, a plurality of surface electric field reduction layers 181 whose length in the horizontal direction is shorter than the surface electric field reduction layer 18 are arranged in a manner that the configuration interval increases as it moves toward the outside. The P-type impurity concentration of the surface electric field reduction layer 181 is substantially the same as the P-type impurity concentration of the surface electric field reduction layer 18. The surface electric field reduction layer 181 is also provided for the purpose of maintaining a withstand voltage, and the voltage is shared by the PN junction of each surface electric field reduction layer and the semiconductor substrate 3, thereby maintaining a withstand voltage. In addition, the surface electric field reduction layers 18 and 181 are sometimes also referred to as JTE (Junction Termination Extension) layers.

[0054] In addition, a high concentration (N ++ ) An impurity region 4 containing an N-type impurity. The impurity region 4 is provided as a channel stopper, and by providing the impurity region 4, a depletion layer is prevented from reaching an end of the chip, thereby preventing a decrease in the withstand voltage holding capability.

[0055] In addition, a 1×10 15 ~1×10 16 / cm 3 A buffer layer 2 containing N-type impurities at a concentration (N) of 1×10 16 ~1×10 18 / cm 3 The collector layer 1 contains a P-type impurity at a concentration (P) of 1.3 Å, and the collector electrode 23 (second main electrode) is connected to the collector layer 1 .

[0056] A silicon oxide film 51 (second insulating film) is provided on the edge portion from the guard ring 17 to the inner side of the surface electric field reduction layer 18. A gate wiring 22 is provided on the silicon oxide film 51. The gate wiring 22 is provided along the cell region CR in the same manner as the guard ring 17, and the gate wiring 22 is connected to a gate wiring electrode 221 provided on the silicon oxide film 51. The gate wiring electrode 221 is an aluminum electrode and is electrically connected to the outside via a wire not shown. In addition, the silicon oxide films 5 and 51 can be composed of, for example, a silicon oxide film based on thermal oxidation (thermal oxide film), or a TEOS (tetraethylorthosilicate) oxide film (BPTEOS film) containing boron (B) and phosphorus (P), or a multilayer film of a thermal oxide film and a BPTEOS film.

[0057] A silicon oxide film 5 (first insulating film) is provided on semiconductor substrate 3 from above the inner edge of impurity region 4 to the vicinity of impurity region 4. Silicon oxide film 5 functions as a field plate to prevent extension of a depletion layer on the surface of semiconductor substrate 3.

[0058] Moreover, a semi-insulating film 6 (first semi-insulating film) is provided in such a manner as to cover the impurity region 4 from above the outer end edge portion of the silicon oxide film 5, and a semi-insulating film 7 (second semi-insulating film) is provided in such a manner as to cover the entire region of the terminal region TR including above the semi-insulating film 6 and the end edge portion of the cell region CR.

[0059] By adopting such a structure, the withstand voltage and moisture resistance of the IGBT 100 are improved. The evaluation of moisture resistance will be described later.

[0060] <Implementation Method 2>

[0061] Figure 3 is a cross-sectional view of an IGBT 200 according to a second embodiment of the present invention, Figure 2 The sectional view corresponding to the sagittal sectional view of the IGBT 100 shown in FIG. Figure 3 For use with Figure 2 The same components of the IGBT 100 described above are denoted by the same reference numerals, and redundant description will be omitted.

[0062] like Figure 3As shown in FIG. 1 , in the IGBT 200, the outer edge of the silicon oxide film 5 provided on the semiconductor substrate 3 from the inner edge of the impurity region 4 to the impurity region 4 is formed to have a step, and the conductive polysilicon film 8 is provided to fill the step. By providing the polysilicon film 8, the upper surface of the silicon oxide film 5 and the upper surface of the polysilicon film 8 are substantially at the same height, and form a flat surface. The semi-insulating film 6 is provided to cover the impurity region 4 from above the flat surface, and the semi-insulating film 7 is provided to cover the entire region of the termination region TR including the semi-insulating film 6 and the edge of the cell region CR.

[0063] By adopting such a structure, the withstand voltage and moisture resistance of the IGBT 200 are improved. The evaluation of moisture resistance will be described later.

[0064] <Implementation Method 3>

[0065] Figure 4 is a cross-sectional view of an IGBT 300 according to a third embodiment of the present invention, Figure 2 The sectional view corresponding to the sagittal sectional view of the IGBT 100 shown in FIG. Figure 4 For use with Figure 2 The same components of the IGBT 100 described above are denoted by the same reference numerals, and redundant description will be omitted.

[0066] like Figure 4 As shown in FIG. 1 , in the IGBT 300, the outer edge of the silicon oxide film 5 provided on the semiconductor substrate 3 from the inner edge of the impurity region 4 to the vicinity of the impurity region 4 is formed to have a step, and is formed so as to cover the inner surface of the trench 9 penetrating the impurity region 4 and reaching the semiconductor substrate 3. Then, the polysilicon film 8 is provided so as to fill the step of the silicon oxide film 5 and fill the trench 9 whose inner surface is covered by the silicon oxide film 5. By providing the polysilicon film 8, the upper surface of the silicon oxide film 5 and the upper surface of the polysilicon film 8 are substantially the same height, and become a flat surface. The semi-insulating film 6 is provided so as to cover the upper surface of the impurity region 4 from above the flat surface, and the semi-insulating film 7 is provided so as to cover the entire region of the termination region TR including the upper surface of the semi-insulating film 6 and the edge of the cell region CR.

[0067] By adopting such a structure, the withstand voltage and moisture resistance of the IGBT 300 are improved. The evaluation of moisture resistance will be described later.

[0068] <Pressure resistance and moisture resistance>

[0069] Next, the withstand voltage and moisture resistance of the IGBT 100 will be described. Figure 5 : represents an equivalent circuit used for a moisture resistance test on the IGBT 100. Figure 5 As shown in FIG. 1 , during the humidity resistance test, the gate electrode G and the emitter electrode E of the IGBT 100 are short-circuited and connected to the ground (0 V), thereby lowering the gate-emitter voltage V GE Set to 0 V and set the IGBT 100 to a normally-off state. In addition, a collector voltage V is applied to the collector electrode C from a DC power supply. CC Moreover, in Figure 6 2 shows the experimental results of a moisture resistance test performed at a temperature of 150° C. and a relative humidity of 85% with the power supply voltage being 85% of the rated voltage.

[0070] exist Figure 6 In FIG. 1 , a comparison result of the withstand voltage (static withstand voltage), moisture resistance, and terminal region width of the IGBTs 100 to 300 of the first to third embodiments described above and the conventional structure is shown in a bar graph. Figure 6 , the results of normalizing the moisture resistance, withstand voltage, and terminal region width of Embodiments 1 to 3 based on the moisture resistance, withstand voltage, and terminal region width of the conventional structure are shown.

[0071] The moisture resistance was evaluated at a temperature of 150°C and a relative humidity of 85% in the following manner: Figure 5 As shown, the gate electrode G and the emitter electrode E are short-circuited, and the power supply voltage is set to 85% of the rated voltage. For example, in the case of a device with a rated voltage of 6.5 kV class, a power supply voltage of 5525 V is applied.

[0072] That is, the power supply voltage is continuously applied until the device changes in characteristics, is damaged, or reaches a predetermined time. For example, a sample that is evaluated as having no change in characteristics, appearance degradation, or damage even after 1000 hours under the above conditions has twice the moisture resistance of a sample that is damaged after 500 hours, and is excellent in moisture resistance. In this way, the quality of moisture resistance is evaluated by the length of time that a constant performance is maintained.

[0073] The withstand voltage is evaluated by a normal dynamic withstand voltage test of a semiconductor device, and the terminal region width is evaluated by comparing the width of the terminal region of each of the IGBTs 100 to 300 of the first to third embodiments with the width of the terminal region of a conventional structure.

[0074] like Figure 6As shown, the test results of moisture resistance in any of the first to third embodiments are better than those in the conventional structure, and in all the embodiments, no damage occurred even when the test took 1.5 times longer than that in the conventional structure. This is considered to be because, in the conventional structure, an aluminum electrode is provided in the terminal region, while in the IGBTs 100 to 300 of the first to third embodiments, the semi-insulating film 6 is provided instead of the aluminum electrode, thereby eliminating corrosion of the aluminum electrode by moisture and improving moisture resistance.

[0075] In addition, the breakdown voltage of Embodiment 2 is improved by about 1.2 times compared with Embodiment 1. This is because the polysilicon film 8 is provided at the outer edge portion of the silicon oxide film 5 in the termination region, and the polysilicon film 8 functions as a field plate.

[0076] That is, Figure 3 As shown, with respect to IGBT 200, since the thickness t2 (second thickness) of the silicon oxide film 5 between the polysilicon film 8 and the surface of the semiconductor substrate 3 is thinner than the thickness t1 (first thickness) of the silicon oxide film 5 between the semi-insulating film 6 and the surface of the semiconductor substrate 3, the polysilicon film 8 and the semi-insulating film 6 form a two-level field plate structure.

[0077] The field plate structure here refers to a multilayer structure of a conductive film, an insulating film, and a semiconductor layer, and the two-level field plate structure refers to a structure in which two conductive films each form a field plate with respect to the semiconductor layer via an insulating film.

[0078] The IGBT 200 has a semi-insulating film 6 and a two-layer film consisting of a polysilicon film 8 and a semi-insulating film 6 on the silicon oxide film 5 with a thickness t1 and the silicon oxide film 5 with a thickness t2, respectively, and can be said to have a two-level field plate structure relative to the semiconductor substrate 3.

[0079] In the case of the IGBT 200, in the withstand voltage mode, N is generated at the interface between the semiconductor substrate 3 and the silicon oxide film 5 directly below the silicon oxide film 5 of the field plate structure. - The electron accumulation layer becomes a pseudo high concentration N - layer, blocking N - The drift layer is an extension of the depletion layer on the surface of the semiconductor substrate 3 , and an electric field concentration occurs just below the edge of the field plate.

[0080] However, in the two-stage field plate structure, by appropriately setting the length of each field plate and the thickness of the insulating film (silicon oxide film 5) below it, the electric field concentration directly below the field plate can be dispersed. By suppressing the local electric field concentration, the withstand voltage can be improved. The more the number of field plates, the finer the electric field concentration can be dispersed and the higher the withstand voltage.

[0081] Thus, the IGBT 200 of the second embodiment having the two-stage field plate structure has a higher withstand voltage than the IGBT 100 of the first embodiment having the one-stage field plate structure. Figure 6 As shown, the IGBT 300 of the third embodiment also has a two-stage field plate structure, and therefore has a higher withstand voltage than the IGBT 100 .

[0082] Furthermore, the terminal region width of the IGBT 300 of the third embodiment is narrower than that of the first and second embodiments. Figure 4 As shown, in the IGBT 300, a trench 9 penetrating the impurity region 4 and reaching the semiconductor substrate 3 is provided on the outer peripheral side of the terminal region, and a polysilicon film 8 is buried in the trench 9 via a silicon oxide film 5, so the length of the field plate, here, the creepage distance of the polysilicon film 8 becomes longer. Therefore, the withstand voltage is constant and the width of the terminal region can be reduced. In addition, by adopting this structure, the withstand voltage can be increased even if the width of the terminal region is the same as in other embodiments.

[0083] Figure 7 The IGBTs 100 and 200 in the first and second embodiments are shown in FIG. Figure 2 and Figure 3 The comparison results of the surface electric field distribution in the BB line area are shown. Figure 7 In the graph, the vertical axis (Y axis) is the electric field strength (MV / cm), and the horizontal axis (X axis) is the distance normalized so that the terminal area width is constant.

[0084] exist Figure 7 In the figure, the surface electric field distribution in Embodiment 1 is represented by a solid line, and the surface electric field distribution in Embodiment 2 is represented by a dotted line. The peak portion of the surface electric field distribution in Embodiment 1 is the electric field intensity at the end of the semi-insulating film 6, and the peak portion of the surface electric field distribution in Embodiment 2 is the electric field intensity at the end of the polysilicon film 8.

[0085] Voltage is the integral of the electric field and the distance. Figure 7 In FIG. 1 , the area of ​​the region defined by the electric field distribution and the X-axis represents the withstand voltage. Figure 7 The diagram shows the local electric field distribution of the portion where the field plate structure is provided, indicating that the IGBT 200 of the second embodiment has a larger electric field distribution area and a higher withstand voltage than the IGBT 100 of the first embodiment.

[0086] <Material of Semi-Insulating Film>

[0087] Next, the materials of the semi-insulating film 6 and the semi-insulating film 7 are described. In order to use the semi-insulating film 6 as a field plate, it is formed of a resistive material. As an example, the semi-insulating film 6 is set to be a resistive thin film composed of silicon nitride having a composition with excess Si compared to Si3N4. Thus, the semi-insulating film 6 can be used as a field plate, suppressing the local electric field concentration in the terminal region and improving the withstand voltage.

[0088] If the ratio of Si to N (Si:N) is too small, it is difficult to cause hopping conduction of the semi-insulating film 6, and it does not function as a conductive field plate. In order to function as a field plate, there is no upper limit for Si:N, but due to the limitations of the film forming temperature and the process of chemical reaction during film forming, there is an upper limit for Si:N, which is generally Si:N≤1:2.5.

[0089] Figure 8 An example of the depth profile of a semi-insulating film is shown. Figure 8 In the figure, the horizontal axis represents the depth (nm) and the vertical axis represents the atomic density ratio (%). Figure 8 It is the depth distribution of the silicon nitride film formed on silicon, and the Si:N is about 2:1.

[0090] Since the semi-insulating film 6 is semi-insulating, it is more susceptible to the influence of external charges and mobile ions in the packaging material of the power module than metal materials such as aluminum electrodes. In order to block the influence of external charges, the semi-insulating film 6 is covered with the semi-insulating film 7. The semi-insulating film 7 is in contact with the emitter electrode 15 on the cell region side, and can suppress the influence of external charges by utilizing the hopping conduction characteristics of the semi-insulating film.

[0091] That is, the semi-insulating film 6 is in a floating state and is easily affected by external charges, but the semi-insulating film 7 is in contact with the emitter electrode 15 (ground) on the cell region side and has the same potential as the high voltage side via the semi-insulating film 6 on the terminal region side. Therefore, the internal potential distribution of the semi-insulating film 7 is approximately fixed and is not easily affected by external charges. In addition, the resistivity of the semi-insulating films 6 and 7 at 20V and 25°C is 10 13 ~10 16 Ωcm.

[0092] Hopping conduction refers to a conduction mechanism caused by the excitation of carriers within the band gap of a material. If hopping conduction exists, the local charge temporarily induced by external influences will not remain fixed at the same position, but will gradually move to the ground or high potential side and disappear. If the charge remains fixed at the same position, the electric field distribution inside the semiconductor substrate will be affected by dielectric phenomena, causing the withstand voltage to decrease. However, since the semi-insulating film has hopping conduction characteristics, the decrease in withstand voltage can be suppressed.

[0093] If the semi-insulating film 6 and the semi-insulating film 7 have electrical resistance, the same effect can be obtained regardless of whether they are made of the same material or different materials. Even in the case of the same composition, a step is formed at the outer peripheral end of the semi-insulating film 6 relative to the semi-insulating film 7, so that the semi-insulating film 6 and the semi-insulating film 7 can be distinguished when observed in cross section. In addition, since the film thickness of the portion that becomes the two-layer structure of the semi-insulating film 6 and the semi-insulating film 7 is thicker than the film thickness of the portion that only has the semi-insulating film 7, the semi-insulating film 6 and the semi-insulating film 7 can be distinguished when observed in cross section.

[0094] <Modification>

[0095] At once Figure 1 In the IGBT 100 of the first embodiment shown in the figure, the semi-insulating film 6 is provided so as to cover the impurity region 4 from the outer edge portion of the silicon oxide film 5 in the termination region TR. Fig. 9 As in the IGBT 100A shown in the figure, the silicon oxide film 5 is provided so as to cover the entire upper part of the terminal region. The effect produced by adopting this structure is the same as that of the IGBT 100.

[0096] In addition, Figure 1 In the IGBT 100 of the first embodiment shown in the figure, the semi-insulating film 6 is provided so as to cover the impurity region 4 from the outer edge portion of the silicon oxide film 5 in the termination region TR. Fig.10 As in the IGBT 100B shown in FIG. 1 , the semi-insulating film 6 covers the entire upper portion of the silicon oxide film 5 in the terminal region, and covers the silicon oxide film 51 provided from above the guard ring 17 to the inner edge portion of the resurf layer 18, and the edge portion of the cell region CR. The effect produced by adopting this structure is the same as that of the IGBT 100. In this case, the semi-insulating film 7 is electrically connected to the emitter electrode 15 via the semi-insulating film 6.

[0097] In this way, the structure in which the semi-insulating film 6 is provided so as to cover the upper edge portion of the cell region CR from above the silicon oxide film 51 provided from above the guard ring 17 to the upper edge portion on the inner side of the resurf layer 18 can also be applied to the IGBTs 200 and 300 of the second and third embodiments. The effect produced by adopting this structure is the same as that of the IGBTs 200 and 300.

[0098] In the three embodiments 1 to 3, the moisture blocking effect is enhanced by further covering the semi-insulating film 7 with another semi-insulating film, an insulating film, a polyimide resin, or the like.

[0099] In addition, the silicon oxide film 5 may be provided continuously over the entire terminal region or may be provided intermittently. Even when these structures are adopted, the same effects as those of the IGBTs 100 to 300 of the first to third embodiments are achieved.

[0100] <Method for Forming Semi-Insulating Film>

[0101] Next, use Figures 11 to 19 The method for manufacturing the semi-insulating film 6 and the semi-insulating film 7 will be described. Figures 11 to 19 2 shows a cross section centered on the outer peripheral portion of the termination region TR, and illustration of impurity regions and impurity layers other than the impurity region 4 is omitted.

[0102] First, in Fig.11 In the process shown, after the silicon oxide film 5 is formed on the semiconductor substrate 3, a resist mask RM1 for patterning the silicon oxide film 5 is formed by photolithography (photolithography).

[0103] Next, in Fig.12 In the process shown, after the silicon oxide film 5 is patterned by etching using the resist mask RM1, the resist mask RM1 is removed.

[0104] Next, in Fig.13 In the step shown, N-type impurities are ion-implanted into the semiconductor substrate 3 using the silicon oxide film 5 provided with the opening OP1 for forming the impurity region 4 as an implantation mask to form the impurity region 4 .

[0105] Next, in Fig.14 In the process shown, a resist mask RM2 for further patterning the silicon oxide film 5 is formed by photolithography.

[0106] Next, in Fig.15 In the process shown, after the silicon oxide film 5 is patterned by etching using the resist mask RM2, the resist mask RM2 is removed. In this process, the silicon oxide film 51 from above the guard ring 17 to the inner edge of the resurf layer 18 is patterned.

[0107] Next, in Fig.16 In the illustrated process, a semi-insulating film 6 of silicon nitride is formed by, for example, CVD (Chemical Vapor Deposition) so as to cover the silicon oxide film 5 and the semiconductor substrate 3 .

[0108] Next, in Fig.17In the process shown, a resist mask RM3 for patterning the semi-insulating film 6 is formed by photolithography on the semi-insulating film 6. The resist mask RM3 formed here has a pattern such that the semi-insulating film 6 remains from above the outer edge of the silicon oxide film 5 to above the impurity region 4.

[0109] Next, in Fig.18 In the process shown, after the semi-insulating film 6 is patterned by etching using the resist mask RM3, the resist mask RM3 is removed.

[0110] Next, in Fig.19 In the process shown, a semi-insulating film 7 of silicon nitride is formed by, for example, CVD to cover the semi-insulating film 6, the silicon oxide film 5, the semiconductor substrate 3, and the silicon oxide film 51, thereby forming the semi-insulating film 6 and the semi-insulating film 7.

[0111] In addition, when using Fig.15 and Fig.18 In the etching process described above, plasma etching using a reactive gas, wet etching using a chemical solution, or a combination of these two methods can be used.

[0112] In addition, if you use Fig.11 , Fig.14 and Fig.17 As described above, in order to form the semi-insulating film 6 and the semi-insulating film 7, three photolithography processes must be performed. However, depending on the type of reactive gas or chemical solution, when selective etching of the semi-insulating film 6 and the silicon oxide film 5 is possible, the use of the photolithography process can be omitted by using the semi-insulating film 6 as an etching mask for the silicon oxide film 5. Fig.17 The photolithography process described above can form the semi-insulating film 6 and the semi-insulating film 7 by performing the photolithography process twice.

[0113] Next, use Figure 20 to Figure 24 , a manufacturing method for forming the semi-insulating film 6 and the semi-insulating film 7 by two photolithography steps is described.

[0114] First, after using Figure 11 to Figure 13 In the process described above, an impurity region 4 is formed in a semiconductor substrate 3. Then, Fig. 20 In the illustrated process, the semi-insulating film 6 of silicon nitride is formed by, for example, CVD so as to cover the silicon oxide film 5 and the semiconductor substrate 3 .

[0115] Next, in Fig.21In the process shown, a resist mask RM2 for patterning the semi-insulating film 6 is formed by photolithography on the semi-insulating film 6. The resist mask RM2 formed here has a pattern such that the semi-insulating film 6 remains on the upper part of the silicon oxide film 5 in the terminal region and on the impurity region 4, and the semi-insulating film 6 remains on the silicon oxide film 51 on the inner edge portion from the guard ring 17 (not shown) to the surface electric field reduction layer 18 (not shown) and on the edge portion of the cell region CR.

[0116] Next, in Fig. 22 In the process shown, after the semi-insulating film 6 is patterned by etching using the resist mask RM2, the resist mask RM2 is removed.

[0117] Next, in Fig.23 In the process shown, the silicon oxide film 5 is patterned by etching using the patterned semi-insulating film 6 as a mask. As a result, the silicon oxide film 5 remains from the terminal region and the guard ring 17 (not shown) to the inner edge of the reduced surface electric field layer 18 (not shown). In addition, the silicon oxide film 5 remaining from the guard ring 17 to the inner edge of the reduced surface electric field layer 18 becomes a silicon oxide film 51.

[0118] Then, in Fig.24 In the illustrated process, the semi-insulating film 7 of silicon nitride is formed by, for example, CVD so as to cover the semi-insulating film 6 and the semiconductor substrate 3 , thereby forming the semi-insulating film 6 and the semi-insulating film 7 .

[0119] When such a manufacturing method is applied, Fig.10 The IGBT 100B shown has the following structure: the semi-insulating film 6 covers the impurity region 4 from the upper part of the silicon oxide film 5 in the terminal region, and covers the silicon oxide film 51 provided from the guard ring 17 to the inner edge of the resurf layer 18 and the edge of the cell region CR.

[0120] <Application to other semiconductor devices>

[0121] In the above-described embodiments 1 to 3 and the modified examples, IGBT is used as an example. However, as long as it is a semiconductor device with a terminal region, such as a MOS (Metal Oxide Semiconductor) transistor or various diodes, the static withstand voltage can be maintained and the moisture resistance can be improved by applying the structure of the above-mentioned terminal region.

[0122] Furthermore, in the first to third embodiments and the modified examples, the trench gate type IGBT is described as an example, but the structure of the terminal region described above can also be applied to a planar gate type IGBT or a MOS transistor.

[0123] In addition, the present invention can freely combine the various embodiments, or appropriately modify or omit the various embodiments within the scope of the invention.

Claims

1. A semiconductor device in which a main current flows in a thickness direction of a semiconductor substrate, in, The semiconductor substrate has: an active region through which the main current flows; and a termination region which surrounds the active region on the outside compared to the active region, The semiconductor device has: a first main electrode disposed on the active area; a second main electrode disposed on the semiconductor substrate on the opposite side to the first main electrode; an impurity region provided in an upper layer portion of the semiconductor substrate located at the outermost periphery of the termination region; A first insulating film is provided at the outer edge of the termination region from above the inner edge of the impurity region to a portion of the upper portion of the semiconductor substrate; a second insulating film provided from above the inner edge portion of the termination region to above the edge portion of the active region; a first semi-insulating film covering from a portion of the impurity region not covered by the first insulating film to at least a portion of an upper portion of the first insulating film; as well as a second semi-insulating film covering a portion of the first main electrode from above the first semi-insulating film, The second semi insulating film covers the first semi insulating film in a region corresponding to a portion of the impurity region not covered by the first insulating film.

2. The semiconductor device according to claim 1, in, The first semi-insulating film covers from a portion of the impurity region not covered by the first insulating film to an outer edge portion of the first insulating film.

3. The semiconductor device according to claim 1, in, The first insulating film has a step at the outer edge portion. The semiconductor device further includes a polysilicon film provided on the first insulating film so as to fill the step. The first semi-insulating film covers the portion of the impurity region not covered by the first insulating film to the polysilicon film and the first insulating film. A first thickness of the first insulating film between the second semi-insulating film and the semiconductor substrate is thicker than a second thickness of the first insulating film between the polysilicon film and the semiconductor substrate.

4. The semiconductor device according to claim 1, in, The first insulating film has a step at an outer edge portion, and the first insulating film covers an inner surface of a trench that penetrates the impurity region and reaches the semiconductor substrate. The semiconductor device further includes a polysilicon film provided on the first insulating film so as to fill the step and to fill the trench. The first semi-insulating film covers the portion of the impurity region not covered by the first insulating film to the polysilicon film and the first insulating film. A first thickness of the first insulating film between the second semi-insulating film and the semiconductor substrate is thicker than a second thickness of the first insulating film between the polysilicon film and the semiconductor substrate.

5. The semiconductor device according to claim 1, in, The first semi-insulating film covers from a portion of the impurity region not covered by the first insulating film to an entire upper portion of the first insulating film.

6. The semiconductor device according to any one of claims 2 to 5, in, The first semi-insulating film is further provided so as to cover from above the second insulating film to above the edge portion of the active region.

7. The semiconductor device according to claim 1, in, The first semi-insulating film is composed of 3 N 4 The resistive thin film is composed of silicon nitride having a composition in excess of Si.