Toner for electrostatic charge image development, toner storage unit, image forming apparatus, and image forming method
By combining crystalline and non-crystalline polyester resins into the toner and controlling the spin-spin relaxation time using pulsed NMR analysis, the balance between the toner's low-temperature fixing and cleaning capabilities was solved, achieving optimized low-temperature fixing and cleaning effects.
Patent Information
- Application Number
- CN202011170208.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-29
- Filing Date
- 2020-10-27
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-10-27
AI Technical Summary
Existing toners struggle to balance low-temperature fixing and cleaning capabilities, resulting in poor cleaning performance of low-melting-point toners during low-temperature fixing, which affects the efficiency and quality of image forming equipment.
By combining crystalline and non-crystalline polyester resins in the toner and using the Hahn echo method of pulsed NMR analysis to control the spin-spin relaxation time, uniform dispersion and phase separation of the crystalline resin are achieved, optimizing the thermal behavior of the toner to achieve low stretching temperature, prevention of poor cleaning, and low-temperature fixing.
This technology enables efficient fixing at low temperatures while preventing toner adhesion and poor cleaning, thus improving the efficiency of image forming equipment and image quality.
Smart Images

Figure CN112748649B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a toner for developing an electrostatic charge image, a toner storage unit (stored unit), an image forming apparatus, and an image forming method. Background Art
[0002] In an image forming device such as an electrophotographic device or an electrostatic recording device, a toner is used to develop an electrostatic latent image formed on a photoreceptor to form a toner image, and the toner image is transferred to a recording medium such as paper and fixed by heating to form an image. When a full-color image is formed, four colors of toner (such as black, yellow, magenta and cyan) are usually used for development. At this time, after the toner images of the various colors are transferred and overlapped on the recording medium, they are fixed simultaneously by heating. In order to achieve the intention of low power consumption and shortened warm-up time, toners with low temperature fixability have been studied. However, toners with low melting points have poor cleaning ability. Therefore, there is a need to achieve them.
[0003] For example, in Japanese Unexamined Patent Application Publication No. 2014-224980, it has been attempted to achieve low-temperature fixability and heat-resistant storage stability by optimizing the balance between the amount of crystalline resin and the shell thickness.
[0004] For example, in Japanese Unexamined Patent Application Publication No. 2013-190552, it has been attempted to prevent cleaning failure by optimizing the toner shape and the kind of additives.
[0005] An object of the present disclosure is to provide a toner for electrostatic charge image development that can satisfy low stretching temperature, prevention of poor cleaning, low temperature fixability, and high maximum fixing temperature. Summary of the invention
[0006] According to one aspect of the present disclosure, a toner for electrostatic charge image development is provided. The toner has a spin-spin relaxation time of 0.30 milliseconds or more but 1.50 milliseconds or less at 90°C. The toner has a spin-spin relaxation time of 0.0185 milliseconds or more but 0.0300 milliseconds or less at 50°C. The spin-spin relaxation time of the toner at 90°C and the spin-spin relaxation time of the toner at 50°C are obtained by a Hahn echo method of pulsed NMR analysis.
[0007] According to the present disclosure, a toner for electrostatic charge image development that can satisfy low stretching temperature, prevention of cleaning failure, low temperature fixability, and high maximum fixing temperature can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1is a schematic diagram of a cross section of a toner;
[0009] Figure 2 is the CO2 phase diagram; and
[0010] Figure 3 The present invention is a diagram showing the overall configuration of an image forming apparatus according to one embodiment of the present disclosure. DETAILED DESCRIPTION
[0011] (toner for developing electrostatic charge images)
[0012] Regarding the toner for electrostatic charge image development of the present disclosure, the spin-spin relaxation time of the toner at 90° C. is 0.30 msec or more but 1.50 msec or less, and the spin-spin relaxation time of the toner at 50° C. is 0.0185 msec or more but 0.0300 msec or less. The spin-spin relaxation time of the toner at 90° C. and the spin-spin relaxation time of the toner at 50° C. are obtained by a Hahn echo method of pulsed NMR analysis.
[0013] The toner for electrostatic charge image development of the present disclosure preferably includes at least one selected from a non-crystalline polyester resin and a crystalline polyester resin, and further includes a releasing agent and a colorant as needed.
[0014] The present inventors have diligently studied to provide a toner for electrostatic charge image development that can satisfy the prevention of poor cleaning and low-temperature fixability. As a result, they have found that, in a combination in which a crystalline resin and a non-crystalline resin are compatible, in order to achieve sufficient phase separation of the crystalline resin and the non-crystalline resin in the toner and to uniformly disperse the crystalline resin in the form of fine domains, the following two points are important. Figure 1 A schematic diagram showing a cross section of a toner.
[0015] First, fine domains of the crystalline resin are uniformly dispersed in a matrix structure in which the crystalline resin and the non-crystalline resin are compatible in the toner or a resin composition constituting the toner.
[0016] Second, the toner resin is annealed to promote crystal growth of the crystalline resin encapsulated in the toner resin to form a phase separation structure of the crystalline resin and the non-crystalline resin.
[0017] Specifically, the present inventors have found that it is important that the toner production step includes the following steps.
[0018] (1) A step of uniformly dispersing a crystalline polyester resin in the form of fine domains by LCP.
[0019] (The details of LCP will be described below.)
[0020] (2) A step of forming a phase separation structure of the crystalline resin and the non-crystalline resin at a certain rate after uniformly blending the crystalline resin and the non-crystalline resin in a resin composition constituting the toner.
[0021] By performing these steps, sufficient phase separation of the crystalline resin and the non-crystalline resin and formation of uniformly dispersed fine domains can be achieved in the toner or the resin composition constituting the toner. As a result, the thermal behavior of the toner can be controlled. Therefore, a toner that can satisfy the prevention of poor cleaning and low-temperature fixability can be obtained.
[0022] As a result of diligent studies conducted by the present inventors, thermal behavior of a toner that can satisfy prevention of poor cleaning and low-temperature fixability can be confirmed from a spin-spin relaxation time obtained by a Hahn echo method of pulsed NMR analysis, and the present inventors have completed the present disclosure.
[0023] That is, the toner of the present disclosure has the following characteristics. The spin-spin relaxation time of the toner at 90° C. is 0.30 msec or more but 1.5 msec or less, and the spin-spin relaxation time of the toner at 50° C. is 0.0185 msec or more but 0.0300 msec or less. Here, the spin-spin relaxation time of the toner at 90° C. and the spin-spin relaxation time of the toner at 50° C. are obtained by the Hahn echo method of pulsed NMR analysis.
[0024] When the spin-spin relaxation time of the toner at 90°C is less than 0.30 milliseconds, low-temperature fixability decreases. When the spin-spin relaxation time of the toner at 90°C is greater than 1.5 milliseconds, the maximum fixing temperature becomes low. When the spin-spin relaxation time of the toner at 50°C is less than 0.0185 milliseconds, the minimum scraping temperature becomes high. When the spin-spin relaxation time of the toner at 50°C is greater than 0.0300 milliseconds, poor cleaning occurs.
[0025] In terms of low temperature fixability and higher maximum fixing temperature, the toner preferably has a spin-spin relaxation time at 90° C. of 1.0 msec or more but 1.5 msec or less.
[0026] In terms of the minimum scraping temperature, the spin-spin relaxation time of the toner at 50° C. is preferably 0.0200 msec or more but 0.0250 msec or less.
[0027] The spin-spin relaxation time (t2) in the present disclosure is a characteristic value reflecting the thermal behavior of the toner. The toner is measured by the Hahn echo method of pulsed NMR analysis, and the spin-spin relaxation time calculated from the decay curve obtained is regarded as t2. The spin-spin relaxation time (t2) presents the mobility of the molecules constituting the toner. Therefore, the hardness of the toner at a certain temperature can be evaluated. For example, when the molecules constituting the toner with a low melting point are heated, a long spin-spin relaxation time (t2) is exhibited due to the high mobility when melting. In the case of discussing fixability and preventing poor cleaning, the focus is on the temperature of the melting behavior obtained when the toner passes through the fixing device and is heated, and the behavior of the toner particles adhering to the photoreceptor, drum or cleaning component in the device. Moreover, the thermal environment to which the toner will be exposed varies depending on the respective situation. Therefore, in the present disclosure, the spin-spin relaxation time (t2) of the toner at 90° C. in which the former case is considered and the spin-spin relaxation time (t2) of the toner at 50° C. in which the latter case is considered are evaluated.
[0028] <Pulse NMR Analysis>
[0029] In the present disclosure, the pulsed NMR analysis of the toner is preferably performed by the following method. That is, using pulsed NMR: Minispec mq series (available from Bruker), a high-frequency magnetic field as a pulse is applied to the toner loaded in an NMR tube, and the magnetization vector is rotated. Then, the mobility of the molecules constituting the toner is evaluated from the time until the x and y components decay (= relaxation time).
[0030] [1. Sample]
[0031] The toner (40 mg) was weighed and loaded into an NMR tube having a diameter of 10 mm. Then, the toner was heated in a preheater with the temperature adjusted to 90°C for 15 minutes, and used for measurement. Note that even in a toner having the same temperature of 90°C, such a sample once heated to a temperature higher than 90°C and returned to 90°C by cooling has significantly different characteristics due to its drastic change in crystal state. Therefore, the temperature of the preheater must be adjusted to 90°C, and the heating of the sample needs to be started then.
[0032] [2. Measurement conditions]
[0033] Hahn echo method
[0034] First 90° pulse interval (Separation): 0.01 milliseconds
[0035] Final pulse interval: 20 ms
[0036] Number of data points used for fitting: 40 points
[0037] Cumulative number: 32 times
[0038] Temperature: 90℃
[0039] [3. Calculation method of spin-spin relaxation time (t2)]
[0040] The spin-spin relaxation time (t2) was calculated from the decay curve obtained by the Hahn echo method measured by pulsed NMR using the exponential approximation of ORIGIN 8.5 (available from Origin Lab). It is known that the spin-spin relaxation time is shorter as the molecular mobility is lower, and the spin-spin relaxation time is longer as the molecular mobility is higher.
[0041] <Crystalline Polyester Resin>
[0042] The toner for electrostatic charge image development preferably includes a crystalline polyester resin.
[0043] The melting point of the crystalline polyester resin preferably falls within the range of 50° C. or more but 100° C. or less, more preferably within the range of 55° C. or more but 90° C. or less, even more preferably within the range of 55° C. or more but 85° C. or less.
[0044] When the melting point is 50° C. or more, blocking is not caused in the stored toner, and the storability of the toner and the storability of the fixed image after fixing become good. When the melting point is 100° C. or less, sufficient low-temperature fixability can be obtained.
[0045] Note that the melting point of the crystalline polyester resin can be determined as the peak temperature of an endothermic peak obtained by differential scanning calorimetry (DSC).
[0046] The "crystalline polyester resin" in the present disclosure includes not only a polymer formed of 100% polyester structure but also a copolymer of a monomer constituting polyester and another monomer. However, the ratio of the other monomer in the copolymer is 50% by mass or less.
[0047] The crystalline polyester resin used in the toner of the present disclosure is synthesized from, for example, a polyvalent carboxylic acid component and a polyvalent alcohol component. The crystalline polyester resin may be a commercially available product or may be a synthesized product.
[0048] Examples of the polyvalent carboxylic acid component include divalent carboxylic acid components and trivalent or higher carboxylic acid components.
[0049] Examples of the divalent carboxylic acid component include: aliphatic dicarboxylic acids such as oxalic acid, succinic acid, glutaric acid, adipic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonane dicarboxylic acid, 1,10-decane dicarboxylic acid, 1,12-dodecane dicarboxylic acid, 1,14-tetradecane dicarboxylic acid and 1,18-octadecane dicarboxylic acid (stearic acid); and aromatic dicarboxylic acids such as dibasic acids (e.g. phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid and mesakonin acid). Moreover, examples of the divalent carboxylic acid component include anhydrides thereof and lower alkyl esters thereof.
[0050] Examples of the trivalent or higher carboxylic acid component include: 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid; and anhydrides thereof and lower alkyl esters thereof.
[0051] These may be used alone or in combination.
[0052] The acid component may contain a dicarboxylic acid component having a sulfonic acid group in addition to the polyvalent carboxylic acid component. The acid component may further contain a dicarboxylic acid component having a double bond.
[0053] Examples of the polyvalent alcohol component include divalent alcohol components and trivalent or higher alcohol components.
[0054] The divalent alcohol component is preferably an aliphatic diol, more preferably a straight-chain aliphatic diol having a carbon number of 2 or more but 20 or less in the main chain portion. When the straight-chain aliphatic diol is used, the crystallinity and melting point of the polyester resin are less reduced than in the case where a branched aliphatic diol is used. The carbon number in the main chain portion is more preferably 14 or less.
[0055] The amount of the aliphatic diol in the polyvalent alcohol component is preferably 80 mol% or more, more preferably 90 mol% or more. When the amount is 80 mol% or more, the crystallinity of the polyester resin is high and the melting temperature is high. Therefore, the toner anti-blocking property, image storage stability and low-temperature fixability are more excellent.
[0056] Examples of the aliphatic diol include ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1-9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol and 1,14-eicosadecanediol. Among them, ethylene glycol is preferred in terms of availability.
[0057] Examples of the trivalent or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, and pentaerythritol.
[0058] These may be used alone or in combination.
[0059] For the purpose of, for example, adjusting the acid value and the hydroxyl value as required, a polyvalent carboxylic acid or a polyvalent alcohol may be added at the final stage of the synthesis.
[0060] Examples of the polyvalent carboxylic acid include: aromatic carboxylic acids such as terephthalic acid, isophthalic acid, phthalic anhydride, trimellitic anhydride, pyromellitic acid, and naphthalene dicarboxylic acid; aliphatic carboxylic acids such as maleic anhydride, fumaric acid, succinic acid, alkenyl succinic anhydride, and adipic acid; and alicyclic carboxylic acids such as cyclohexane dicarboxylic acid.
[0061] Examples of the polyvalent alcohol include: aliphatic diols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butylene glycol, hexylene glycol, neopentyl glycol, and glycerol; alicyclic diols such as cyclohexanediol, cyclohexanedimethanol, and hydrogenated bisphenol A; and aromatic diols such as bisphenol A-ethylene oxide adduct and bisphenol A-propylene oxide adduct.
[0062] The crystalline polyester resin can be produced at a polymerization temperature of, for example, 180° C. or more but 230° C. or less. The reaction is promoted by reducing the pressure in the reaction system as needed, and removing water or alcohol generated at the time of condensation.
[0063] When the monomer is insoluble or incompatible at the reaction temperature, a solvent with a high boiling point may be added as a solubilizing agent to dissolve the monomer. The polycondensation reaction is promoted by removing the solubilizing agent. When a monomer with poor compatibility is present in the copolymerization reaction, the monomer with poor compatibility may be pre-condensed with the acid or alcohol to be polycondensed, and then the resultant may be polycondensed with the main component.
[0064] Examples of catalysts that can be used to produce the polyester resin include: alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; metal compounds such as zinc, manganese, antimony, titanium, tin, zirconium and germanium; phosphite compounds; phosphate compounds; and amine compounds.
[0065] Specific examples of the catalyst include compounds such as sodium acetate, sodium carbonate, lithium acetate, lithium carbonate, calcium acetate, calcium stearate, magnesium acetate, zinc acetate, zinc stearate, zinc naphthenate, zinc chloride, manganese acetate, manganese naphthenate, titanium tetraethoxide, titanium tetrapropoxide, titanium tetraisopropoxide, titanium tetrabutoxide, antimony trioxide, triphenylantimony, tributylantimony, tin formate, tin oxalate, tetraphenyltin, dibutyltin dichloride, dibutyltin oxide, diphenyltin oxide, zirconium tetrabutoxide, zirconium naphthenate, zirconyl carbonate, zirconyl acetate, zirconyl stearate, zirconyl octoate, germanium oxide, triphenyl phosphite, tris(2,4-di-tert-butylphenyl) phosphite, ethyltriphenylphosphonium bromide, triethylamine, and triphenylamine.
[0066] The acid value of the crystalline polyester resin (the amount of KOH in mg required to neutralize 1 g of the resin) is preferably in the range of 3.0 mg KOH / g or more but 30.0 mg KOH / g or less, more preferably in the range of 6.0 mg KOH / g or more but 25.0 mg KOH / g or less, even more preferably in the range of 8.0 mg KOH / g or more but 20.0 mg KOH / g or less.
[0067] The weight average molecular weight (Mw) of the crystalline polyester resin is preferably 6,000 or more but 35,000 or less. When the weight average molecular weight (Mw) is 6,000 or more, uneven fixing caused by the toner penetrating into its surface when the toner is fixed on a recording medium such as paper, and a reduction in the folding resistance strength of the fixed image can be prevented. When the weight average molecular weight (Mw) is 35,000 or less, the viscosity of the toner when melted is not too high. As a result, the temperature at which the viscosity reaches a level suitable for fixing is not high, thereby preventing the low-temperature fixability from deteriorating.
[0068] The main component (50% by mass or more) of the crystalline resin containing the crystalline polyester resin is preferably a crystalline polyester resin synthesized by using an aliphatic monomer (hereinafter may be referred to as "crystalline aliphatic polyester resin"). In this case, the composition ratio of the aliphatic monomer constituting the crystalline aliphatic polyester resin is preferably 60% by mole or more, more preferably 90% by mole or more. Suitable examples of the aliphatic monomer include the aliphatic diols and dicarboxylic acids listed above.
[0069] The amount of the crystalline polyester resin is preferably 1% by mass or more but 20% by mass or less, more preferably 10% by mass or more but 18% by mass or less, relative to the amount of the toner in terms of low temperature fixability and toner strength.
[0070] <Non-crystalline polyester resin>
[0071] In the present disclosure, the toner preferably contains a non-crystalline polyester resin as a binder resin of the toner. Examples of the non-crystalline polyester resin include modified polyester resins and unmodified polyester resins. The inclusion of a modified polyester resin is more preferred.
[0072] <<Modified polyester resin>>
[0073] As the modified polyester resin, a modified polyester resin obtained by introducing a urea bond into a polyester resin may be used.
[0074] Examples of the constituent components of the modified polyester resin include polyester prepolymers having an isocyanate group. Examples of the polyester prepolymer (A) having an isocyanate group include products obtained by reacting a polyester having an active hydrogen group, which is a polycondensate of a polyol (1) and a polycarboxylic acid (2), with a polyisocyanate (3). Examples of the active hydrogen group contained in the polyester include a hydroxyl group (alcoholic hydroxyl group and phenolic hydroxyl group), an amino group, a carboxyl group, and a mercapto group. Among them, an alcoholic hydroxyl group is preferred.
[0075] Examples of the polyol (1) include diol (1-1) and trivalent or higher polyol (1-2). (1-1) alone or a mixture of (1-1) and a small amount of (1-2) is preferred.
[0076] Examples of the diol (1-1) include alkylene glycols (e.g., ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylene glycol, and 1,6-hexanediol); alkylene ether glycols (e.g., diethylene glycol, triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, and polytetramethylene ether glycol); alicyclic glycols (e.g., 1,4-cyclohexanedimethanol and hydrogenated bisphenol A); bisphenols (e.g., bisphenol A, bisphenol F, and bisphenol S); alkylene oxide (e.g., ethylene oxide, propylene oxide, and butylene oxide) adducts of the above-listed alicyclic glycols; and alkylene oxide (e.g., ethylene oxide, propylene oxide, and butylene oxide) adducts of the above-listed bisphenols. Among them, alkylene glycols having 2 or more but 12 or less carbon atoms and alkylene oxide adducts of bisphenols are preferred. Alkylene oxide adducts of bisphenol, and combinations of alkylene oxide adducts of bisphenol and alkylene glycol having 2 or more but 12 or less carbon atoms are particularly preferred.
[0077] Examples of the trivalent or higher polyol (1-2) include trivalent or higher but octavalent or lower aliphatic polyvalent alcohols; octavalent or higher aliphatic polyvalent alcohols (e.g., glycerol, trimethylolethane, trimethylolpropane, pentaerythritol, and sorbitol); trivalent or higher phenols (e.g., trisphenol PA, phenol novolac, and cresol novolac); and alkylene oxide adducts of the above trivalent or higher polyphenols.
[0078] Examples of the polyvalent carboxylic acid (2) include dicarboxylic acid (2-1) and trivalent or higher polycarboxylic acid (2-2). (2-1) alone and a mixture of (2-1) with a small amount of (2-2) are preferred.
[0079] Examples of dicarboxylic acids (2-1) include alkylene dicarboxylic acids (e.g., succinic acid, adipic acid, and sebacic acid); alkenylene diacids (e.g., maleic acid and fumaric acid); and aromatic dicarboxylic acids (e.g., phthalic acid, isophthalic acid, terephthalic acid, and naphthalene dicarboxylic acid). Among them, alkenylene dicarboxylic acids having 4 or more but 20 or less carbon atoms and aromatic dicarboxylic acids having 8 or more but 20 or less carbon atoms are preferred.
[0080] Examples of trivalent or higher polycarboxylic acids (2-2) include aromatic polycarboxylic acids having 9 or more but 20 or less carbon atoms (e.g., trimellitic acid and pyromellitic acid). As the polycarboxylic acid (2), the above anhydrides or lower alkyl esters (e.g., methyl ester, ethyl ester, and isopropyl ester) can be used.
[0081] The ratio between the polyol (1) and the polycarboxylic acid (2) is typically 2 / 1 to 1 / 1, preferably 1.5 / 1 to 1 / 1, more preferably 1.3 / 1 to 1.02 / 1, in terms of the equivalent ratio [OH] / [COOH] of hydroxyl groups [OH] to carboxyl groups [COOH].
[0082] Examples of the polyisocyanate (3) include aliphatic polyisocyanates (e.g., tetramethylene diisocyanate, hexamethylene diisocyanate, and 2,6-diisocyanate methylhexanoate); alicyclic polyisocyanates (e.g., isophorone diisocyanate and cyclohexylmethane diisocyanate); aromatic diisocyanates (e.g., tolylene diisocyanate and diphenylmethane diisocyanate); aromatic aliphatic diisocyanates (e.g., α, α', α'-tetramethylxylylene diisocyanate); isocyanurates; polyisocyanates blocked by phenol derivatives, oximes, caprolactams, etc.; and combinations thereof.
[0083] The ratio of the polyisocyanate (3) as the equivalent ratio [NCO] / [OH] of the isocyanate group [NCO] to the hydroxyl group [OH] of the polyester having a hydroxyl group is typically 5 / 1 to 1 / 1, preferably 4 / 1 to 1.2 / 1, more preferably 2.5 / 1 to 1.5 / 1.
[0084] The amount of the polyisocyanate (3) constituting the component in the polyester prepolymer (A) having an isocyanate group at its terminal is typically 0.5% by mass or more but 40% by mass or less, preferably 1% by mass or more but 30% by mass or less, more preferably 2% by mass or more but 20% by mass or less.
[0085] With respect to one molecule of the polyester prepolymer (A) having an isocyanate group, the number of isocyanate groups contained is typically 1 or more, preferably 1.5 or more but 3 or less on average, more preferably 1.8 or more but 2.5 or less on average.
[0086] In the present disclosure, amines may be used as crosslinking agents and / or chain extenders when synthesizing modified polyester resins.
[0087] Examples of the amine (B) include diamines (B1), trivalent or higher polyamines (B2), amino alcohols (B3), aminothiols (B4), amino acids (B5), and products obtained by blocking the amino group of any value of B1 to B5 (B6).
[0088] Examples of the diamine (B1) include: aromatic diamines (e.g., phenylenediamine, diethyltoluenediamine, and 4,4'-diaminodiphenylmethane); alicyclic diamines (4,4'-diamino-3,3'-dimethyldicyclohexylmethane, diaminecyclohexane, and isophoronediamine); and aliphatic diamines (e.g., ethylenediamine, tetramethylenediamine, and hexamethylenediamine).
[0089] Examples of the trivalent or higher polyamine (B2) include diethylenetriamine and triethylenetetramine.
[0090] Examples of the amino alcohol (B3) include ethanolamine and hydroxyethylaniline.
[0091] Examples of the aminomercaptan (B4) include aminoethylmercaptan and aminopropylmercaptan.
[0092] Examples of the amino acid (B5) include aminopropionic acid and aminocaproic acid.
[0093] Examples of the product (B6) obtained by blocking the amino group of any of B1 to B5 include ketimine compounds and oxazoline compounds obtained from any of amines B1 to B5 and ketones (e.g., acetone, methyl ethyl ketone and methyl isobutyl ketone). Among these amines (B), B1 and a mixture of B1 and a small amount of B2 are preferred.
[0094] In crosslinking and / or elongation, a terminal blocking agent may be used as needed to adjust the molecular weight of the modified polyester resin obtained after the reaction is completed. Examples of the terminal blocking agent include monoamines (e.g., diethylamine, dibutylamine, butylamine, and laurylamine) and products obtained by blocking any of the monoamines (e.g., ketimine compounds).
[0095] The ratio of amine (B) is typically 1 / 2 to 2 / 1, preferably 1.5 / 1 to 1 / 1.5, and more preferably 1.2 / 1 to 1 / 1.2, and the ratio of amine (B) is the equivalent ratio [NCO] / [NHx] of the isocyanate group [NCO] in the polyester prepolymer (A) having an isocyanate group to the amino group [NHx] in the amine (B).
[0096] 《Unmodified polyester resin》
[0097] In the present disclosure, instead of adding only the modified polyester resin (A), it is preferred to add the unmodified polyester (C) (unmodified polyester resin) as a toner binder component together with (A). The combined use of the unmodified polyester (C) improves low-temperature fixability, as well as gloss and gloss uniformity when the toner is used in a full-color device. Examples of (C) include the same polycondensates of the polyols (1) and polycarboxylic acids (2) exemplified above as the polyester components of (A). Preferred examples thereof also include the same as (A). (C) is not only a non-modified polyester, but also a polyester modified with a chemical bond other than a urea bond. For example, (C) may be a polyester modified with a urethane bond. Preferably, (A) and (C) are at least partially compatible in terms of low-temperature fixability and thermal offset resistance. Therefore, it is preferred that the polyester components of (A) and (C) have similar compositions. When (A) is contained, the mass ratio between (A) and (C) is typically 5 / 95 to 75 / 25, preferably 10 / 90 to 25 / 75, even more preferably 12 / 88 to 25 / 75, and particularly preferably 12 / 88 to 22 / 78.
[0098] The peak molecular weight of (C) is typically 1,000 or more but 30,000 or less, preferably 1,500 or more but 10,000 or less, more preferably 2,000 or more but 8,000 or less. When the peak molecular weight thereof is 1,000 or more, the heat-resistant storage stability is not deteriorated. When the peak molecular weight thereof is 10,000 or less, the low-temperature fixability is not deteriorated.
[0099] The hydroxyl value of (C) is preferably 5 mg KOH / g or more, more preferably 10 mg KOH / g or more but 120 mg KOH / g or less, particularly preferably 20 mg KOH / g or more but 80 mg KOH / g or less. When the hydroxyl value is 5 or more, it is advantageous in terms of heat-resistant storage stability and low-temperature fixing property.
[0100] The acid value of (C) is typically 0.5 mg KOH / g or more but 40 mg KOH / g or less, preferably 5 mg KOH / g or more but 35 mg KOH / g or less. When the toner has the acid value, the toner tends to be negatively charged easily.
[0101] When the acid value and the hydroxyl value fall within the aforementioned ranges, respectively, the toner is less susceptible to influences from environments under high temperature and high humidity conditions and under low temperature and low humidity conditions, which does not cause image degradation.
[0102] <Release Agent>
[0103] As a mold release agent, common waxes can be used.
[0104] The wax may be any conventional wax, and examples thereof include polyolefin waxes (eg, polyethylene wax and polypropylene wax); long-chain hydrocarbons (eg, paraffin wax and SASOL wax); and carbonyl-containing waxes. Among them, paraffin wax is preferred.
[0105] Examples of the carbonyl-containing wax include polyalkanoic acid esters (e.g., carnauba wax, montan wax, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerol tribehenate, and 1,18-octadecanediol distearate); polyalkanoic acid esters (e.g., tristearyl trimellitate and distearyl maleate); polyalkanoic acid amides (e.g., ethylenediamine dibehenylamide); polyalkylamides (e.g., tristearyl trimellitate amide); and dialkyl ketones (e.g., distearyl ketone). Among them, polyalkanoic acid esters are preferred.
[0106] The melting point of the wax is generally 40° C. or more but 160° C. or less, preferably 50° C. or more but 120° C. or less, more preferably 60° C. or more but 90° C. or less.
[0107] The melt viscosity of the wax is preferably 5 cps or more but 1,000 cps or less, more preferably 10 cps or more but 100 cps or less, as a value measured at a temperature 20° C. higher than the melting point.
[0108] The amount of the wax in the toner is usually 0% by mass or more but 40% by mass or less, preferably 3% by mass or more but 30% by mass or less.
[0109] <Colorant>
[0110] The colorant is not particularly limited and any known dyes and pigments may be used.
[0111] Examples of dyes and pigments include, but are not limited to, carbon black, aniline black dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide, yellow ochre, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Vulcan fast yellow (5G, R), tartrate yellow lake, quinoline yellow lake, anthrasan yellow BGL, isoindolinone yellow, red iron oxide, red lead, lead cinnabar, cadmium red, cadmium mercury red, antimony cinnabar, permanent red 4R, para red, fischer red (fischer red), and tartrate yellow lake. red), p-chloro-o-nitroaniline red, lithoyl fast scarlet G, bright fast scarlet, bright magenta BS, permanent red (F2R, F4R, FRL, FRLL, F4RH), fast scarlet VD, Balkan fast ruby B, bright scarlet G, lithoyl red GX, permanent red F5R, bright magenta 6B, pigment scarlet 3B, jujube 5B, toluidine chestnut, permanent jujube F2K, Helio jujube BL, jujube 10B, BON chestnut light, BON chestnut medium, eosin lake, rhodamine lake B, rhodamine lake Y, alizarin lake, thioindigo red B, thioindigo purple, oil red, quinacridone Ketone red, pyrazolone red, polyazo red, chrome cinnabar, benzidine orange, cycloketone orange, oil orange, cobalt blue, azure blue, basic blue lake, malachite blue lake, Victoria blue lake, metal-free phthalocyanine blue, phthalocyanine blue, fast sky blue, indanthrene blue (RS, BC), indigo, ultramarine, Prussian blue, anthraquinone blue, fast violet B, methyl violet lake, cobalt violet, manganese violet, dioxane violet, anthraquinone violet, chrome green, zinc green, chromium oxide, chrome green, emerald green, pigment green B, naphthol green B, green gold, acid green lake, malachite green lake, phthalocyanine green, anthraquinone green, titanium oxide, zinc flower, zinc lithopone, and mixtures of the foregoing.
[0112] The amount of the colorant in the toner is generally 1% by mass or more but 15% by mass or less, preferably 3% by mass or more but 10% by mass or less.
[0113] Colorants can be used as masterbatches compounded with resins.
[0114] Examples of the binder resin kneaded with the masterbatch used in the method for producing the masterbatch include, in addition to the modified polyester resin and the unmodified polyester resin exemplified above, styrene polymers (e.g., polystyrene, poly(p-chlorostyrene) and polyvinyltoluene) and substituted products thereof; styrene-based copolymers such as styrene-p-chlorostyrene copolymers, styrene-propylene copolymers, styrene-vinyltoluene copolymers, styrene-vinylnaphthalene copolymers, styrene-methyl acrylate copolymers, styrene-ethyl acrylate copolymers, styrene-butyl acrylate copolymers, styrene-octyl acrylate copolymers, styrene-methyl methacrylate copolymers, styrene-ethyl methacrylate copolymers, styrene -butyl methacrylate copolymer, styrene-chloromethylacrylate α-methyl ester copolymer, styrene-acrylonitrile copolymer, styrene-methyl vinyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-acrylonitrile-indene copolymer, styrene-maleic acid copolymer, and styrene-malate copolymer; and polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resin, epoxy polyol resin, polyurethane, polyamide, polyvinyl butyral, polyacrylic resin, rosin, modified rosin, terpene resin, aliphatic or alicyclic hydrocarbon resin, aromatic petroleum resin, chlorinated paraffin, and paraffin. These can be used alone or in combination.
[0115] The masterbatch of the present disclosure can be obtained by mixing the masterbatch resin and the colorant via applying high shear force and then kneading them. At this time, in order to improve the interaction between the colorant and the resin, an organic solvent can be used. Such a method is preferably used because the colorant wet cake can be used directly and does not need to be dried: the water-containing aqueous paste of the colorant is mixed and kneaded with the resin and the organic solvent, and the colorant is transferred to the resin side to remove the water content and the organic solvent content (so-called flash method). In order to mix and knead, a high shear-dispersion device such as a three-roll mill is preferably used.
[0116] <Charge Control Agent>
[0117] The toner of the present disclosure may contain a charge control agent as needed.
[0118] The charge control agent may be a known charge control agent, and examples thereof include nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdate chelate pigments, rhodamine dyes, alkoxyamines, quaternary ammonium salts (including fluorine-modified quaternary ammonium salts), alkylamides, phosphorus, phosphorus compounds, tungsten, tungsten compounds, fluorine-based active agents, metal salts of salicylic acid, and metal salts of salicylic acid derivatives.
[0119] Specific examples of the charge control agent include nigrosine dye BONTRON 03, quaternary ammonium salt BONTRON P-51, metal-containing azo dye BONTRON S-34, hydroxynaphthoic acid-based metal complex E-82, salicylic acid-based metal complex E-84 and phenol-based condensate E-89 (available from Orient Chemical Industries Co., Ltd.); quaternary ammonium salt molybdenum complex TP-302 and TP-415 (available from Hodogaya Chemical Co., Ltd.); quaternary ammonium salt COPY CHARGE PSYVP2038, triphenylmethane derivative COPY BLUE PR, quaternary ammonium salt COPY CHARGE NEG VP2036 and COPY CHARGE NX VP434 (available from Hoechst GmbH); LRA-901 and boron complex LR-147 (available from Japan Carlit Co., Ltd.); copper phthalocyanine; perylene; quinacridone; azo pigments; and polymer compounds having a sulfonic acid group, a carboxyl group, a quaternary ammonium salt, etc. as functional groups.
[0120] The amount of the charge control agent is not generalized because it depends on the type of binder resin, the presence or absence of additives used as necessary, and the toner production method (including dispersion method). However, the amount of the charge control agent is preferably 0.1 parts by mass or more but 10 parts by mass or less, more preferably 0.2 parts by mass or more but 5 parts by mass or less, relative to 100 parts by mass of the non-crystalline polyester resin.
[0121] The charge control agent may be dissolved and dispersed after being melted and kneaded with the masterbatch and the resin. The charge control agent may be directly dissolved or dispersed in an organic solvent. Alternatively, the charge control agent may be fixed on the surface of the toner particles after the toner particles are manufactured.
[0122] <External additives>
[0123] As an external additive for assisting the fluidity, developability and chargeability of toner particles, oxide particles are preferred. However, other inorganic fine particles and hydrophobized inorganic fine particles may be used in combination therewith.
[0124] It is more preferred that at least one of the inorganic fine particles whose primary particles have an average particle size of 1 nm or more but 100 nm or less, and more preferably 5 nm or more but 70 nm or less, be added. It is more preferred that at least one of the inorganic fine particles whose primary particles have an average particle size of 20 nm or less, and at least one of the inorganic fine particles whose primary particles have an average particle size of 30 nm or more, be added. It is also preferred that the specific surface area measured by the BET method is 20 nm. 2 / g or greater but 500m 2 / g or less.
[0125] Examples of inorganic fine particles such as oxide fine particles include silicon dioxide, aluminum oxide, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, silica sand, clay, mica, wollastonite, diatomaceous earth, chromium oxide, cerium oxide, red iron oxide, antimony trioxide, magnesium oxide, zirconium oxide, barium sulfate, barium carbonate, calcium carbonate, silicon carbide and silicon nitride. Among them, silicon dioxide and titanium dioxide are particularly preferred.
[0126] In addition to the above, fatty acid metal salts (such as zinc stearate and aluminum stearate), fluoropolymers, and polymer fine particles obtained by soap-free emulsion polymerization, suspension polymerization and dispersion polymerization such as polystyrene, methacrylate copolymers, acrylate copolymers, resins based on polymer particles obtained by condensation polymerization (such as silicone, benzoguanamine and nylon) or thermosetting resins can also be used.
[0127] Particularly preferred examples of external additives include hydrophobized silica, titania, titanium oxide and alumina fine particles. Examples of silica fine particles include HDK H 2000, HDK H 2000 / 4, HDK H 2050EP, HVK21 and HDK H 1303 (available from Hoechst GmbH), and R972, R974, RX200, RY200, R202, R805 and R812 (available from Nippon Aerosil Co., Ltd.). Examples of titanium dioxide fine particles include P-25 (available from Nippon Aerosil Co., Ltd.), STT-30 and STT-65C-S (available from Titan Kogyo Ltd.), TAF-140 (available from Fuji Titanium Industry, Co., Ltd.), and MT-150W, MT-500B, MT-600B and MT-150A (available from Tayca Corp.). Specific examples of hydrophobized titanium oxide fine particles include: T-805 (available from Nippon Aerosil Co., Ltd.); STT-30A and STT-65S-S (available from Titan Kogyo, Ltd.); TAF-500T and TAF-1500T (available from Fuji Titanium Industry Co., Ltd.); MT-100S and MT-100T (available from Tayca Corp.); and IT-S (available from Ishihara Sangyo Kaisha Ltd.). Hydrophobized oxide fine particles, silica fine particles, titanium dioxide fine particles, and alumina fine particles can be obtained by treating hydrophilic fine particles with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, and octyltrimethoxysilane. Silicone oil-treated oxide fine particles obtained by treating the oxide fine particles with silicone oil while heating them as needed are also preferred.
[0128] Examples of silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methyl hydrogen silicone oil, alkyl-modified silicone oil, fluorine-modified silicone oil, polyether-modified silicone oil, alcohol-modified silicone oil, amino-modified silicone oil, epoxy-modified silicone oil, epoxy / polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, acryl, methacrylic-modified silicone oil, and α-methylstyrene-modified silicone oil.
[0129] For example, the amount of the external additive is 0.1% by mass or more but 5% by mass or less, preferably 0.3% by mass or more but 3% by mass or less, relative to the amount of the toner.
[0130] For example, the glass transition temperature (Tg) of the toner of the present disclosure is typically 40° C. or more but 70° C. or less, preferably 45° C. or more but 55° C. or less. When the glass transition temperature (Tg) is 40° C. or more, the heat-resistant storage stability of the toner becomes good. When the glass transition temperature (Tg) is 70° C. or less, the low-temperature fixability is more excellent.
[0131] For example, the disclosed toners including crosslinked and / or elongated polyester resins exhibit better storage properties than known polyester-based toners, even when the glass transition temperature is low.
[0132] As the storage modulus of the toner of the present disclosure, the modulus measured at a frequency of 20 Hz is 10,000 dyne / cm 2 The temperature (TG') is usually 100°C or more, preferably 110°C or more but 200°C or less.
[0133] As for the viscosity of the toner disclosed in the present invention, the temperature (Tη) measured at a frequency of 20 Hz at which the viscosity reaches 1,000 poise is generally 180°C or less, preferably 90°C or more but 160°C or less. In order to achieve excellent low-temperature fixability and heat offset resistance, TG' is preferably higher than Tη. That is, the difference between TG' and Tη (TG'-Tη) is preferably 0°C or more. The difference is more preferably 10°C or more, particularly preferably 20°C or more. The upper limit of the difference is not particularly limited. In order to achieve heat-resistant storage stability and excellent low-temperature fixability, the difference between Tη and Tg is preferably 0°C or more but 100°C or less. The difference is more preferably 10°C or more but 90°C or less, particularly preferably 20°C or more but 80°C or less.
[0134] <Method for controlling domain diameter of crystalline resin encapsulated in toner>
[0135] LCP is an abbreviation of liquid phase carbon dioxide process, and is a process of dispersing a resin by using critical CO 2 as a solvent. Figure 2 The CO2 phase diagram is presented. Becoming supercritical means a state where liquid and gas coexist when the temperature and pressure of the environment become equal to or greater than a certain degree (critical point). In the case of carbon dioxide, Figure 2The upper right part in corresponds to the supercritical state. Supercritical CO2 with such characteristics has the same diffusivity as gas and the same solubility as liquid. Therefore, supercritical CO2 makes many resins form small molecules, resulting in good solubility. When the supercritical CO2 diffused between the resin molecules is immediately decompressed, CO2 can immediately diffuse and disperse the resin into fragments. When the supercritical CO2 is decompressed, all CO2 as a solvent becomes gas. Therefore, CO2 can be collected and recovered immediately. This is the principle of LCP dispersion. In the LCP-CPES (crystalline polyester resin) dispersion process, ethyl acetate is used as a solvent. First, CPES (crystalline polyester resin) and ethyl acetate are premixed. At this time, CPES is completely dissolved in ethyl acetate at one time. Then, the CPES-dissolved liquid is added to high-pressure CO2 and pressure is applied thereto. Decompression immediately promotes dispersion. This operation disperses CPES in coarse fragments, and finally the coarse fragments are dispersed by a bead mill to complete it. In the CPES dispersion process by LCP, the median diameter of the CPES domain can be controlled by the ER (evaporation residue) of the CPES solution and the CO2 / CPES ratio. In addition, the domain diameter of the crystalline resin can be reduced by reducing the ER of the CPES solution or increasing the CO2 / CPES ratio.
[0136] <Annealing treatment>
[0137] Annealing treatment increases the crystallinity of crystalline resin. When crystalline material is annealed, its heat increases the molecular mobility of polymer chains to a certain extent. Therefore, the polymer chains are reoriented to a more stable structure; that is, a regular crystal structure, resulting in crystallization. Annealing treatment activates the molecular motion of crystalline polyester in toner as much as possible, and is performed within a limited temperature range relative to the melting point of crystalline polyester. When the treatment is performed at a temperature equal to or higher than the melting point of the crystalline material, the polymer chains obtain energy higher than the energy required for reorientation. Therefore, recrystallization does not occur. Annealing treatment can be performed at any stage as long as it is performed after the step of forming toner particles. Examples of other units for controlling the crystallinity of the resin include methods for adjusting the difference between the solubility parameter of the non-crystalline polyester resin and the solubility parameter of the crystalline polyester resin. When the difference (SP1-SP2) between the SP value (SP1) of the non-crystalline polyester resin and the SP value (SP2) of the crystalline resin is greater than 1.30, the non-crystalline polyester resin and the crystalline polyester resin are almost incompatible. Therefore, it is believed that the functions of the respective resins are separated to maintain storage properties.
[0138] <Method for Confirming Domains of Crystalline Resin Encapsulated in Toner by Transmission Electron Microscopy>
[0139] Confirmation of the domains of the crystalline resin encapsulated in the toner of the present disclosure is preferably evaluated by a method using TEM (transmission electron microscope) as described below.
[0140] A cross section of a toner observed by a transmission electron microscope (TEM) is prepared in the following manner. When the toner is dyed with ruthenium, the crystalline resin contained in the toner has a large contrast and is easily observed. When dyeing with ruthenium, the amount of ruthenium atoms varies with the strength of the dyeing. Therefore, the strongly dyed part has a large number of said atoms and does not transmit electron rays, and appears as a black image when observed. At the same time, the weakly dyed part easily transmits electron rays and appears as a white image when observed. More specifically, compared with other organic components constituting the toner, the crystalline polyester is dyed weakly. It is believed that this is because the penetration of the dyeing material in the crystalline polyester is weaker than the penetration of the dyeing material in the other organic components constituting the toner due to, for example, density differences. Ruthenium that has not penetrated into the interior of the crystalline polyester is easily retained at the interface between the crystalline polyester and the non-crystalline resin. When the crystal has a needle-like shape, the crystalline polyester is observed as a black image.
[0141] Hereinafter, a method for preparing a cross section of a toner dyed with ruthenium will be described. First, the toner is immersed in a 0.5% mass ruthenium tetroxide solution, and block dyeing (bkock staining) is performed for 30 minutes to 90 minutes. Next, the toner dyed with ruthenium is encapsulated in a resin obtained by mixing an epoxy resin as a main agent and an amine as a curing agent in a mass ratio of 1:1, and the resultant is allowed to stand for 24 hours. Then, an ultrasonic ultramicrotome (available from Leica, UC7) is used to cut the encapsulated product at a cutting rate of 0.6 mm / s with a radius length (e.g., 4.0 μm, in the case where the weight average particle size (D4) is 8.0 μm) from the outermost surface of the cylindrical resin of the toner, thereby exposing the cross section of the central part of the toner. Then, it is cut so that the film thickness is 250 nm to prepare a thin slice sample of the cross section of the toner. By cutting the encapsulated product in this way, a cross section of the central part of the toner can be obtained. The obtained flake sample was dyed for 1 to 5 minutes under RuO4 gas in an atmosphere of 500 Pa using a vacuum electron dyeing device (available from filgen, VSC4R1H). Then, a TEM image was prepared using a scanning transmission electron microscope (available from JEOL, JEM2100). The crystalline resin as unevenly distributed domains on the cross section and surface of the toner was observed using the obtained TEM image, and was presented as a black contrast using the image processing software "Image-J".
[0142] <Method for measuring domain diameter of crystalline polyester resin>
[0143] In the present disclosure, the domain diameter of the crystalline polyester resin means a numerical average of major diameters of the crystalline polyester resin domains determined based on the above TEM image.
[0144] Specifically, TEM images of cross sections of 100 toner particles were prepared by the aforementioned method. All major diameters of the crystalline polyester resin domains present in the cross sections of the 100 toner particles were calculated using the image processing software "Image-J". Then, the arithmetic mean thereof was calculated.
[0145] The obtained arithmetic mean value was regarded as the domain diameter of the crystalline polyester resin.
[0146] The domain diameter of the crystalline polyester resin is preferably 0.10 μm or more but 1.0 μm or less. A domain diameter of 0.10 μm or more is advantageous in terms of poor cleaning. A domain diameter of 1.0 μm or less is advantageous in terms of stretchability.
[0147] <Evaluation of the amount of crystalline resin on the surface by TEM image>
[0148] A small amount of crystalline resin present near the surface of the colorant is more effective because poor cleaning is prevented. Examples of units for preventing the crystalline resin from being exposed to the surface of the colorant and units for finely dispersing the crystalline resin in the toner include the addition of a dispersant that includes a styrene-acryl-based main chain as its structure and has an affinity with the crystalline resin in the toner. When the coverage of the crystalline polyester resin on the surface of the toner is less than 20%, the crystalline resin is not excessively exposed to the toner surface particles. Therefore, the adhesion of the toner particles increases, and prevention of poor cleaning can be highly achieved. As described above, the toner that meets the above-defined range can highly achieve prevention of poor cleaning. The coverage of the crystalline polyester resin on the surface of the toner can be determined by the above TEM image.
[0149] Specifically, TEM images of cross sections of 100 toner particles were prepared by the aforementioned method. Then, the area of all crystalline polyester domains unevenly distributed in the toner surface (from the outermost surface to a depth of 10 mm) of the 100 toner particles and the area of the toner surface of the 100 toner particles were measured using the image processing software "Image-J". The arithmetic mean was substituted into the following equation (1) to calculate the coverage (%).
[0150]
[0151] Here, "A" is the arithmetic mean of the toner surface area when the cross section is observed.
[0152] “B” is the arithmetic mean of the area of the crystalline polyester resin on the toner surface when the cross section is observed.
[0153] The coverage is preferably less than 10% because prevention of poor cleaning is more excellent.
[0154] The lower limit of the coverage ratio is not particularly limited and may be appropriately selected depending on the intended purpose. For example, the lower limit of the coverage ratio may be greater than 0%, may be 3% or more, or may be 5% or more.
[0155] (Two-component carrier)
[0156] When the toner for electrostatic charge image development of the present disclosure is used in a two-component developer, it may be mixed with a magnetic carrier. The ratio between the carrier and the toner in the developer is preferably 1 part by mass or more but 10 parts by mass or less of the toner relative to 100 parts by mass of the carrier.
[0157] Examples of magnetic carriers include those well known in the art, such as iron powder having a particle diameter of about 20 μm or more but 200 μm or less, ferrite powder having a particle diameter of about 20 μm or more but 200 μm or less, magnetite powder having a particle diameter of about 20 μm or more but 200 μm or less, and magnetic resin carriers having a particle diameter of about 20 μm or more but 200 μm or less. Examples of coating materials include: urea-formaldehyde resin, melamine resin; benzoguanamine resin; urea resin; polyamide resin; epoxy resin; acrylic resin; polymethyl methacrylate resin; polyacrylonitrile resin; polyvinyl acetate resin; polyvinyl alcohol resin; polyvinyl butyral resin; polystyrene-based resins, such as polystyrene resins and styrene-acryl copolymer resins; halogenated olefin resins, such as polyvinyl chloride; polyester-based resins, such as polyethylene terephthalate resins and polybutylene terephthalate resins; polycarbonate-based resins; polyethylene resins; polyvinyl fluoride resins; polyvinylidene fluoride resins; polytrifluoroethylene resins; polyhexafluoropropylene resins; copolymers of vinylidene fluoride and acryl monomers; copolymers of vinylidene fluoride and vinyl fluoride; fluorine trimers, such as trimers of tetrafluoroethylene, vinylidene fluoride and non-fluorinated monomers; and silicone resins. The coating resin may contain, for example, conductive powder as required. Examples of conductive powders include metal powders, carbon black, titanium oxide, tin oxide, and zinc oxide.
[0158] The conductive powder preferably has an average particle diameter of 1 μm or less. The toner for electrostatic charge image development of the present disclosure may be used as a single-component magnetic toner having no carrier or as a non-magnetic toner.
[0159] (Toner storage unit)
[0160] The toner storage unit of the present disclosure includes: a unit configured to store toner; and, the toner stored in the unit for electrostatic charge image development. Examples of embodiments of the toner storage unit include a toner storage container, a developing device, and a process cartridge.
[0161] The toner storage container includes: a container; and toner stored in the container for developing an electrostatic charge image.
[0162] The developing device is a device having a unit configured to store toner for developing an electrostatic charge image and to develop the toner.
[0163] The process cartridge is a process cartridge that integrates at least an electrostatic latent image carrier (also referred to as an image carrier) and a developing unit. The process cartridge is configured to store a toner for developing an electrostatic charge image and to be detachably mounted in an image forming apparatus. The process cartridge may further include at least one selected from a charging unit, an exposure unit, and a cleaning unit.
[0164] When the toner storage unit of the present disclosure is installed in an image forming apparatus to form an image, image formation utilizing characteristics of the toner for electrostatic charge image development including low stretching temperature, prevention of poor cleaning, low temperature fixability, and high maximum fixing temperature can be performed.
[0165] (Image Forming Apparatus and Image Forming Method)
[0166] The image forming apparatus of the present disclosure includes at least an electrostatic latent image bearing body, an electrostatic latent image forming unit, and a developing unit, and further includes other units as necessary.
[0167] The image forming method of the present disclosure includes at least an electrostatic latent image forming step and a developing step, and further includes other steps as necessary.
[0168] The image forming method can be suitably performed by an image forming device. The electrostatic latent image forming step can be suitably performed by an electrostatic latent image forming unit. The developing step can be suitably performed by a developing unit. Other steps can be suitably performed by other steps.
[0169] More preferably, the image forming device of the present disclosure includes: an electrostatic latent image carrier; an electrostatic latent image forming unit, which is configured to form an electrostatic latent image on the electrostatic latent image carrier; a developing unit, which includes a colorant and is configured to use the colorant to develop the electrostatic latent image formed on the electrostatic latent image carrier to form a colorant image; a transfer unit, which is configured to transfer the colorant image formed on the electrostatic latent image carrier to the surface of a recording medium; and a fixing unit, which is configured to fix the colorant image transferred to the surface of the recording medium.
[0170] More preferably, the image forming method of the present invention includes: an electrostatic latent image forming step of forming an electrostatic latent image on an electrostatic latent image carrier; a developing step of developing the electrostatic latent image formed on the electrostatic latent image carrier using a colorant to form a colorant image; a transferring step of transferring the colorant image formed on the electrostatic latent image carrier to the surface of a recording medium; and a fixing step of fixing the colorant image transferred to the surface of the recording medium.
[0171] In the developing unit and the developing step, a toner for electrostatic charge image development is used. The toner image can be formed by using a developer which preferably contains a toner for electrostatic charge image development and further contains other components such as a carrier as required.
[0172] In an image forming apparatus and an image forming method, by using the toner for electrostatic charge image development of the present disclosure, image formation utilizing the following characteristics of the toner for electrostatic charge image development including low stretching temperature, prevention of poor cleaning, low temperature fixability and high maximum fixing temperature can be performed.
[0173] <Electrostatic Latent Image Bearing Body>
[0174] The material, structure and size of the electrostatic latent image bearing body are not particularly limited and can be appropriately selected from those known in the art. Examples of the material include inorganic photoreceptors (e.g., amorphous silicon and selenium) and organic photoreceptors (e.g., polysilane and phthalopolymethine). Among them, amorphous silicon is preferred in terms of long life time.
[0175] <Electrostatic Latent Image Forming Unit and Electrostatic Latent Image Forming Step>
[0176] The electrostatic latent image forming unit is not particularly limited and may be appropriately selected depending on the intended purpose, as long as it is a unit configured to form an electrostatic latent image on the electrostatic latent image bearing body. Examples of the electrostatic latent image forming unit include a unit including at least a charging member configured to charge the surface of the electrostatic latent image bearing body and an exposure member configured to expose the surface of the electrostatic latent image bearing body in an imagewise manner.
[0177] The electrostatic latent image forming step is not particularly limited and can be appropriately selected depending on the intended purpose, as long as it is a step of forming an electrostatic latent image on the electrostatic latent image bearing member. For example, the electrostatic latent image forming step can be performed by using an electrostatic latent image forming unit, and can be performed by charging the surface of the electrostatic latent image bearing member and exposing the surface in an image-wise manner.
[0178] 《Charging Components and Charging》
[0179] The charging member is not particularly limited and may be appropriately selected depending on the intended purpose. Examples of the charging member include: a contact charger equipped with, for example, a conductive or semiconductive roller, a brush, a film, or a rubber blade known in the art; and a non-contact charger utilizing corona discharge, such as a corona discharger and a scorotron.
[0180] For example, charging can be performed by applying a voltage to the surface of the electrostatic latent image bearing member using a charging member.
[0181] 《Exposure Parts and Exposure》
[0182] The exposure means is not particularly limited and may be appropriately selected depending on the intended purpose, as long as it can expose the surface of the electrostatic latent image bearing body charged by the charging means in the shape of an image to be formed. Examples of the exposure means include various exposure means such as a copy optical exposure means, a rod lens array exposure means, a laser optical exposure means, and a liquid crystal shutter optical exposure means.
[0183] <Developing Unit and Developing Step>
[0184] The developing unit is not particularly limited and may be appropriately selected depending on the intended purpose, so long as it is a developing unit that includes toner and is configured to develop an electrostatic latent image formed on an electrostatic latent image bearing member to form a visible image.
[0185] The developing step is not particularly limited and may be appropriately selected depending on the intended purpose as long as it is a step of developing the electrostatic latent image formed on the electrostatic latent image bearing member using a toner to form a visible image. The developing step may be performed by, for example, a developing unit.
[0186] The developing unit may be a dry developing type developing unit or may be a wet developing type developing unit. Alternatively, the developing unit may be a monochrome developing unit or may be a multicolor developing unit. The developing unit preferably includes a developing device as follows: an agitator configured to rub and stir the toner to be charged; a magnetic field generating unit fixed inside the developing unit; and a rotatable developer carrier configured to carry the developer containing the toner on the surface.
[0187] <Other units and other steps>
[0188] Examples of other units include a transfer unit, a fixing unit, a cleaning unit, a neutralizing unit, a recycling unit, and a control unit.
[0189] Examples of the other steps include a transfer step, a fixing step, a cleaning step, a charge removal step, a recovery step, and a control step.
[0190] Hereinafter, image formation using the toner for electrostatic charge image development of the present disclosure will be described.
[0191] Figure 3 The present invention is a diagram showing the overall configuration of an image forming apparatus according to one embodiment of the present disclosure.
[0192] Figure 3 The image forming device 1 shown in the figure is a color image forming device configured to form a color image through the following tandem imaging components (hereinafter referred to as imaging components): it includes an image reading component 10, an image forming component 11, a paper supply component 12, a transfer component 13, a fixing component 14 and a paper discharge component 15.
[0193] The image reading part 10 is a part configured to read a document image and generate image information. The image reading part 10 includes a contact glass 101 and a reading sensor 102. In the image reading part 10, light is emitted to the document, the emitted light is received by a sensor such as a charge coupled device (CCD) or a contact image sensor (CIS), and an electric color separation signal of RGB colors as three primary colors of light is read.
[0194] The image forming part 11 includes five image forming units 110S, 110Y, 110M, 110C and 110K, which are configured to form and output toner images of four colors of yellow (Y), magenta (M), cyan (C) and black (K) and the toner (S) for electrostatic charge image development of the present disclosure.
[0195] The five image forming units 110S, 110Y, 110M, 110C, and 110K have the same configuration except that they use mutually different color toners of S toner, Y toner, M toner, C toner, and K toner as image forming materials. They are replaced at the end of their service life. The image forming units 110S, 110Y, 110M, 110C, and 110K are each detachably mounted in the apparatus main body 2 constituting a so-called process cartridge. The common configuration will be described by taking the image forming unit 110K configured to form a K toner image as an example.
[0196] The image forming unit 110K includes, for example, a charging device 111K (charging member), a photoreceptor 112K (electrostatic latent image carrier) as an image carrier for K color toner configured to carry a K color toner image on its surface, a developing device 114K (developing unit), a charge removing device 115K, and a photoreceptor cleaning device 116K (cleaning unit). Since these devices are supported on a common support and integrally and detachably mounted in the apparatus main body 2, they can be replaced at the same time.
[0197] The photoreceptor 112K is a drum-shaped photoreceptor having an outer diameter of 60 mm including an organic photosensitive layer formed on the surface of a substrate. The photoreceptor 112K is driven by a driving unit to rotate counterclockwise. When the charging device 111K applies a charging bias to a charging wire as a charging electrode of a charger (charging unit), discharge occurs between the charging wire and the circumferential surface of the photoreceptor 112K to uniformly charge the surface of the photoreceptor 112K. In the present embodiment, the surface of the photoreceptor 112K is charged to have a negative polarity that is the same as the charge polarity of the toner. The charging bias used is a charging bias generated by superimposing an AC voltage on a DC voltage. Instead of the charger, a charging roller arranged to be in contact with or adjacent to the photoreceptor 112K may be used.
[0198] The uniformly charged surface of the photoreceptor 112K is optically scanned by laser light emitted from an exposure device 113 (exposure means) to be described below to form a K electrostatic latent image. In the entire area of the uniformly charged surface of the photoreceptor 112K, the potential is attenuated in the portion irradiated with the laser to form an electrostatic latent image in which the potential in the portion irradiated with the laser is smaller than the potential in the remaining portion (that is, the background portion). The K electrostatic latent image is developed by a developing device 114K (to be described below) using K toner to form a K toner image. The K toner image is first transferred onto an intermediate transfer belt 131 (to be described below).
[0199] The developing device 114K includes a container for storing a two-component developer containing a K toner and a carrier, and is configured to carry the developer on the surface of the developing sleeve by the magnetic force of a magnetic roller in a developing sleeve provided in the container. The developing sleeve receives a developing bias having the same polarity as that of the toner and having a charging potential that is higher than the charging potential of the electrostatic latent image on the photoreceptor 112K but lower than the charging potential of the photoreceptor 112K. Between the developing sleeve and the electrostatic latent image on the photoreceptor 112K, a developing potential from the developing sleeve to the electrostatic latent image occurs. Between the developing sleeve and the background portion of the photoreceptor 112K, a non-developing potential that transfers the toner on the developing sleeve to the sleeve surface occurs. By the action of the developing potential and the non-developing potential, the K toner on the developing sleeve is allowed to selectively adhere to the electrostatic latent image on the photoreceptor 112K, and then developed to form a toner image of K color on the photoreceptor 112K.
[0200] The charge removing device 115K is configured to remove charges from the surface of the photoreceptor 112K after the toner image has been first transferred onto the intermediate transfer belt 131. The photoreceptor cleaning device 116K includes a cleaning blade and a cleaning brush, and is configured to remove, for example, residual toner remaining after transfer on the surface of the photoreceptor 112K that has undergone charge removal by the charge removing device 115K.
[0201] exist Figure 3 In the embodiment, for example, the image forming unit 110S includes a charging device 111S, a photoreceptor 112S as an image carrier for a special color toner configured to carry a special color toner image on its surface, a developing device 114S, a neutralizing device 115S, and a photoreceptor cleaning device 116S. The other image forming units 110C, 110M, and 110Y have the same configuration. That is, the image forming unit 110C, the image forming unit 110M, the image forming unit 110Y, and the image forming unit 110S form an S toner image, a Y toner image, an M toner image, and a C toner image on the photoreceptor 112S, the photoreceptor 112Y, the photoreceptor 112M, and the photoreceptor 112C, respectively, in the same manner as the image forming unit 110K.
[0202] An exposure device 113 as a latent image writing member or an exposure member is arranged above the image forming units 110S, 110Y, 110M, 110C, and 110K. The exposure device 113 optically scans the photosensitive bodies 112S, 112Y, 112M, 112C, and 112K by laser light emitted from a laser diode based on image information transmitted from the image reading member 10 or an external device such as a personal computer.
[0203] The exposure device 113 is configured to irradiate the photoreceptors 112S, 112Y, 112M, 112C, and 112K via a plurality of optical lenses and mirrors by laser light emitted from a light source, while the polygon mirror driven to rotate by a polygon motor polarizes the light in the main scanning direction. Instead of the laser light, LED light emitted from a plurality of LEDs may be used for optical writing and irradiation.
[0204] The paper supply unit 12 is configured to supply paper sheets as an example of paper to the transfer unit 13, and includes a paper storage unit 121, a paper pickup roller 122, a paper supply belt 123, and a registration roller 124. The paper pickup roller 122 is rotatably provided to transfer the paper stored in the paper storage unit 121 to the paper supply belt 123. The paper pickup roller 122 provided as above is configured to pick up the paper in the uppermost portion from the stored paper to place the paper on the paper supply belt 123. The paper supply belt 123 is configured to convey the paper picked up by the paper pickup roller 122 to the transfer unit 13. The registration roller 124 is configured to supply the paper when a portion of the intermediate transfer belt 131 on which the toner image is formed reaches the secondary transfer nip 139 as the transfer nip of the transfer unit 13.
[0205] The transfer member 13 is arranged below the image forming units 110S, 110Y, 110M, 110C, and 110K. The transfer member 13 includes a driving roller 132, a driven roller 133, an intermediate transfer belt 131, primary transfer rollers 134S, 134Y, 134M, 134C, and 134K, a secondary transfer roller 135, a secondary transfer reverse roller 136, a toner deposition amount sensor 137, and a belt cleaning device 138.
[0206] The intermediate transfer belt 131 serves as an endless intermediate transfer member and is supported in a tensioned manner by, for example, a driving roller 132, a driven roller 133, a secondary transfer reverse roller 136, and primary transfer rollers 134S, 134Y, 134M, 134C, and 134K arranged inside the loop of the intermediate transfer belt 131. Here, "arranged" means "arranged and disposed" or "arranged at a determined position", and "supported in a tensioned manner" means "supported under application of tension".
[0207] Driven by the drive unit Figure 3 The driving roller 132 that rotates clockwise allows the intermediate transfer belt 131 to move and run endlessly in the same direction. The intermediate transfer belt 131 moves in a state of contacting the photosensitive bodies 112S, 112Y, 112M, 112C, and 112K.
[0208] The thickness of the intermediate transfer belt 131 is 20 to 200 [μm], preferably about 60 [μm]. The volume resistivity is 1×10 6 Up to 1×10 12 [Ω·em], preferably about 1×10 9 A carbon-dispersed polyimide resin having a low carbon content of [Ω·em] (as measured at an applied voltage of 100 V using HIRESTA-UP MCP HT45 available from Mitsubishi Chemical Corporation) is desirable.
[0209] The toner deposition amount sensor 137 is arranged near the intermediate transfer belt 131 supported by the driving roller 132. The toner deposition amount sensor 137 serves as a toner amount detector configured to detect the amount of the toner image transferred to the intermediate transfer belt 131. The toner deposition amount sensor 137 includes a light reflection type photosensor. The toner deposition amount sensor 137 is configured to detect the amount of light reflected from the image of the toner (including the special color toner) adhered and formed on the intermediate transfer belt 131 to measure the toner deposition amount. In view of the function, for example, the toner deposition amount sensor 137 may be a toner concentration sensor conventionally used as a toner concentration detector configured to detect and measure the toner concentration. In this case, it is possible to avoid arranging a new toner amount detector, thereby resulting in cost reduction due to the reduction in the number of components. Instead of the position facing the intermediate transfer belt 131, the toner deposition amount sensor 137 may be arranged at a position for detecting the toner image on the photoreceptor 112.
[0210] The primary transfer rollers 134S, 134Y, 134M, 134C, and 134K are arranged to face the photosensitive bodies 112S, 112Y, 112M, 112C, and 112K, respectively, via the intermediate transfer belt 131. The primary transfer rollers 134S, 134Y, 134M, 134C, and 134K follow and rotate to move the intermediate transfer belt 131. With this configuration, a primary transfer nip is formed where the outer side surface of the intermediate transfer belt 131 abuts on the photosensitive bodies 112S, 112Y, 112M, 112C, and 112K (which means that the outer side surface of the intermediate transfer belt 131 is in contact with the photosensitive bodies 112S, 112Y, 112M, 112C, and 112K). A primary transfer bias is applied to each of the primary transfer rollers 134S, 134Y, 134M, 134C, and 134K by a primary transfer bias power supply. This forms a primary transfer bias between the S, Y, M, C, and K toner images on the photoreceptors 112S, 112Y, 112M, 112C, and 112K and the primary transfer rollers 134S, 134Y, 134M, 134C, and 134K. The toner images of the respective colors are sequentially transferred onto the intermediate transfer belt 131.
[0211] In response to the rotation of the photoreceptor 112S, the S toner image formed on the surface of the S photoreceptor 112S enters the S primary transfer nip. By the action of the transfer bias or the clamping pressure, the S toner image is transferred once from the photoreceptor 112S to the intermediate transfer belt 131. The intermediate transfer belt 131 to which the S toner image has been transferred once in this manner passes sequentially through the Y, M, C, and K primary transfer nips. The Y, M, C, and K toner images on the photoreceptors 112Y, 112M, 112C, and 112K are sequentially superimposed on the S toner image for primary transfer. Through the primary transfer by superimposing the toner images, the superimposed toner images (including the color toner images and the special toner (e.g., transparent toner) images) are formed on the intermediate transfer belt 131. That is, the toner images on the surfaces of the image carrier for the color toner and the image carrier for the special toner are superimposed and transferred onto the intermediate transfer belt 131 .
[0212] The primary transfer rollers 134S, 134Y, 134M, 134C, and 134K are each formed of an elastic roller including a metal core rod and a conductive sponge layer fixed on the surface of the core rod. The primary transfer rollers each have an outer diameter of 16 [mm] and a core rod diameter of 10 [mm]. The resistance value R of the sponge layer is calculated from the current I flowing when a voltage of 1,000 [V] is applied to the core rods of the primary transfer rollers 134S, 134Y, 134M, 134C, and 134K by pressing a grounded metal roller having an outer diameter of 30 [mm] with a force of 10 [N]. Specifically, the resistance value R of the sponge layer calculated based on Ohm's law (R=V / I) from the current I flowing when a voltage of 1,000 [V] is applied to the core rod is about 3×10 7 [Ω]. A primary transfer bias output from a primary transfer bias power supply under constant current control is applied to the primary transfer rollers 134S, 134Y, 134M, 134C, and 134K. For example, a transfer charger or a transfer brush may be used instead of the primary transfer rollers 134S, 134Y, 134M, 134C, and 134K.
[0213] The secondary transfer roller 135 is driven by a driving unit to rotate together with the intermediate transfer belt 131 and the paper sandwiched between the secondary transfer roller 135 and the secondary transfer reverse roller 136. The secondary transfer roller 135 contacts the outer surface of the intermediate transfer belt 131 to form a secondary transfer nip 139 as a transfer nip. The secondary transfer roller 135 also serves as a nip forming member and a transfer member for transferring the toner image on the intermediate transfer belt to the recording medium sandwiched at the secondary transfer nip. The secondary transfer reverse roller 136 serves as a nip forming member and a reverse member. The secondary transfer roller 135 is grounded, while the secondary transfer reverse roller 136 receives a secondary transfer bias applied by the secondary transfer bias power supply 130.
[0214] The secondary transfer bias power supply 130 includes a DC power supply and an AC power supply. The secondary transfer bias power supply 130 can output a secondary transfer bias obtained by superimposing an AC voltage on a DC voltage. The output terminal of the secondary transfer bias power supply 130 is coupled to the mandrel of the secondary transfer reverse roller 136. The mandrel potential of the secondary transfer reverse roller 136 is substantially the same as the output voltage from the secondary transfer bias power supply 130.
[0215] The application of the secondary transfer bias to the secondary transfer reverse roller 136 forms a secondary transfer bias between the secondary transfer reverse roller 136 and the secondary transfer roller 135 to electrostatically transfer the toner having the negative polarity from the secondary transfer reverse roller 136 side to the secondary transfer roller 135 side. This makes it possible to transfer the toner having the negative polarity on the intermediate transfer belt 131 from the secondary transfer reverse roller 136 side to the secondary transfer roller 135 side.
[0216] The secondary transfer bias power supply 130 uses a DC component having the same negative polarity as the toner, so that the time-averaged potential of the superimposed bias has the same negative polarity as the toner. Instead of grounding the secondary transfer roller 135 while applying the superimposed bias to the secondary transfer reverse roller 136, the core bar of the secondary transfer reverse roller 136 may be grounded while applying the superimposed bias to the secondary transfer roller 135. In this case, the DC voltage and the DC component are made different.
[0217] When using paper with high surface irregularities, such as embossed paper, a superimposed bias is applied to reciprocally move the toner from one side of the intermediate transfer belt 131 to the other side of the paper, but relatively move the toner, thereby transferring the toner to the paper. This makes it possible to improve the transferability to the concave portion of the paper, resulting in an increase in the transfer rate and an improvement in abnormal images such as blanks. At the same time, when using paper with low surface irregularities, such as ordinary transfer paper, a contrast pattern reflecting surface irregularities does not appear. Therefore, the application of the secondary transfer bias generated only by the DC component makes it possible to obtain sufficient transferability.
[0218] The secondary transfer reverse roller 136 includes a core rod formed of, for example, stainless steel or aluminum and a resistive layer stacked on the rod. The secondary transfer reverse roller 136 has the following properties. Specifically, its outer diameter is about 24 [mm]. The core rod diameter is about 16 [mm]. The resistive layer is formed of, for example, a material obtained by dispersing conductive particles such as carbon or metal complexes in polycarbonate, fluorine-based rubber, silicon-based rubber, rubber such as acrylonitrile-butadiene rubber (NBR) and ethylene-propylene-diene rubber (EPDM), NBR / epichlorohydrin rubber (ECO) copolymer, or semi-conductive rubber formed from polyurethane. Its volume resistivity is 10 6 [Ω] to 1012 [Ω], expected 10 7 [Ω] to 10 9 [Ω]. A foamed rubber having a rubber hardness (ASKER-C) of 20 to 50 degrees or a rubber having a rubber hardness of 30 to 60 degrees can be used. However, since the secondary transfer reverse roller 136 contacts the secondary transfer roller 135 via the intermediate transfer belt 131, it is desirable to be formed of a sponge that does not produce a non-contact portion even under a small contact pressure. Toner that has not been transferred to the paper remains on the intermediate transfer belt 131 that has passed through the secondary transfer nip after the secondary transfer. The toner is removed and cleaned from the surface of the intermediate transfer belt 131 by a belt cleaning device 138 including a cleaning blade that contacts the surface of the intermediate transfer belt 131.
[0219] The fixing member 14 is of a belt-fixing type, and includes an endless fixing belt 141 and a pressure roller 142 pressed against the fixing belt 141. The fixing belt 141 is supported around a fixing roller 143 and a heating roller 144, and at least one of the rollers is provided with a heat source / heating unit (e.g., a heater, a lamp, or an electromagnetic induction type heating device). The fixing belt 141 forms a fixing nip portion between the fixing belt 141 and the pressure roller 142, wherein the fixing belt 141 is pressed between the fixing roller 143 and the pressure roller 142.
[0220] The paper supplied to the fixing part 14 is clamped at the fixing nip having a surface such that the unfixed toner image is adhered to the fixing belt 141. Because the toner in the toner image is softened by the application of heat or pressure, the toner image is fixed, and then the paper is discharged to the outside of the apparatus. In the case where an image is formed on the other surface of the paper opposite to the surface on which the toner image has been transferred, the paper is conveyed to the paper reversing mechanism after the fixing of the toner image, and the paper is reversed by the paper reversing mechanism. The toner image is also formed on the opposite surface in the same manner as the above-mentioned image forming step.
[0221] The paper on which the toner has been fixed in the fixing member 14 is discharged from the image forming apparatus body 2 to the outside of the apparatus via the paper discharge roller constituting the paper discharge member 15 and stored in the paper storage portion 151 such as a paper discharge tray.
[0222] Example
[0223] Hereinafter, the present disclosure will be described by way of examples. However, the present disclosure should not be construed as being limited to these examples. In the examples, "parts" and "%" mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Various physical properties of the toners of the examples and comparative examples measured by the aforementioned methods are summarized and listed in Table 1.
[0224] (Example 1)
[0225] <Preparation of aqueous phase>
[0226] Water (963 parts), a 48.3% aqueous solution of sodium dodecyldiphenyl ether disulfonate (ELEMINOL MON-7 available from Sanyo Chemical Industries, Ltd.) (37 parts) and ethyl acetate (90 parts) were mixed and stirred to obtain an emulsion, which was used as [aqueous phase 1].
[0227] <Synthesis of Non-Crystallized Intermediate Polyester>
[0228] Into a reaction vessel equipped with a condenser, a stirrer and a nitrogen introduction tube, bisphenol A-ethylene oxide 2 mol adduct (200 parts), bisphenol A-propylene oxide 2 mol adduct (563 parts), terephthalic acid (283 parts), trimellitic anhydride (22 parts) and dibutyltin oxide (2 parts) were added, and they were reacted at 230° C. for 7 hours under normal pressure, and then further reacted under a reduced pressure of 10 mmHg to 15 mmHg for 5 hours to obtain [non-crystalline intermediate polyester 1].
[0229] Next, [non-crystalline intermediate polyester 1] (410 parts), isophorone diisocyanate (89 parts) and ethyl acetate (500 parts) were added to a reaction vessel equipped with a condenser, a stirrer and a nitrogen introduction tube, and they were reacted at 100° C. for 5 hours to obtain [prepolymer 1].
[0230] <Synthesis of Ketimine Compound>
[0231] Isophoronediamine (170 parts) and methyl ethyl ketone (75 parts) were added to a reaction container equipped with a stirring bar and a thermometer, and reacted at 45°C for 5 hours and 30 minutes to obtain [ketimine compound 1].
[0232] <Synthesis of Crystalline Polyester Resin>
[0233] Stearic acid (248 parts), ethylene glycol (27 parts) and dihydroxybis(triethanolamine)titanium (0.5 parts) as a condensation catalyst were added to a reaction vessel equipped with a condenser, a thermometer, a stirrer, a dehydrator and a nitrogen introduction tube. They were reacted at 180° C. for 2 hours under a nitrogen stream while removing the generated water, and then further reacted under a reduced pressure of 5 mmHg to 20 mmHg for 3 hours to obtain [Crystalline Polyester Resin 1].
[0234] <Preparation of Resin for Dispersing Crystalline Polyester Resin>
[0235] Sebacic acid (6.0 parts), ethylene glycol (5.4 parts), fumaric acid (3.4 parts) and xylene (9.9 parts) were added to a 5L-four-necked flask equipped with a nitrogen introduction tube, a dehydration tube, a stirrer and a thermocouple. The above materials were reacted at 180°C for 10 hours. Then, the temperature was raised to 200°C and the materials were reacted for 3 hours, followed by further reaction at a pressure of 8.3KPa for 2 hours. A solution obtained by dissolving styrene (38.3 parts), methacrylic acid (0.3 parts) and di-tert-butyl peroxide (1.2 parts) in xylene (3.9 parts) was added dropwise thereto for 3 hours. The resulting product was kept at 170°C for 30 minutes, and the solvent was removed to obtain [resin 1 for dispersing crystalline polyester resin].
[0236] <Preparation of Crystalline Polyester Resin Dispersion>
[0237] [Crystalline polyester resin 1] (446 parts), ethyl acetate (1,894 parts) and [resin 1 for dispersing crystalline polyester resin] (446 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 85% to prepare a mixture of crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of standard state). As a result, [crystalline polyester resin dispersion 1] was obtained.
[0238] <Preparation of Oil Phase>
[0239] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 1] (446 parts) and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. Under stirring, the material was warmed to 80° C., maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 1].
[0240] [Material dissolved liquid 1] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads loaded to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 1].
[0241] <Emulsification and solvent removal>
[0242] [Pigment / wax dispersion 1] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 1].
[0243] [Emulsified slurry 1] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours. The resultant was left to stand at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 1].
[0244] <Washing and Drying>
[0245] [Dispersion slurry 1] (100 parts) was filtered under reduced pressure and subjected to a series of washing treatments described below.
[0246] Specifically, ion exchange water (100 parts) was added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, followed by filtering. Then, 10% hydrochloric acid (100 parts) was added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, followed by filtering. Ion exchange water (300 parts) was added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, followed by filtering. The aforementioned operation was performed twice to obtain [filter cake 1].
[0247] [Filter Cake 1] was dried at 45°C for 48 hours using a circulation dryer, and the resultant was sieved using a mesh having an opening of 75 μm to obtain [Toner Base Particles 1].
[0248] Next, to the obtained toner mother particles (100 parts), silica having a large particle diameter (HSP160A obtained from FUSOCHEMICAL CO., Ltd., RX40 obtained from NIPPON AEROSIL CO., Ltd.) (2.20 parts) was added, followed by mixing using a Henschel mixer. Furthermore, silica having a small diameter (R972) (0.6 parts) was mixed using a Henschel mixer, and coarse particles were removed using a sieve having an opening of 37 μm to prepare [Toner 1].
[0249] The domain diameter of the crystalline resin of [Toner 1] was 0.60 μm, and the coverage of the crystalline resin on the toner surface was 8%.
[0250] (Example 2)
[0251] [Toner 2] was obtained in the same manner as in Example 1, except that [Pigment / Wax Dispersion Liquid 1] was changed to the following [Pigment / Wax Dispersion Liquid 2].
[0252] The domain diameter of the crystalline resin of [Toner 2] was 0.50 μm, and the coverage of the crystalline resin on the toner surface was 7%.
[0253] <Production of Non-Crystalline Resin A>
[0254] To a 5L-four-necked flask equipped with a nitrogen introduction tube, a dehydration tube, a stirrer and a thermocouple, propylene glycol as a diol and dimethyl terephthalate and dimethyl adipate as dicarboxylic acids were added so that the molar ratio between dimethyl terephthalate and dimethyl adipate (dimethyl terephthalate / dimethyl adipate) would be 90 / 10 and the ratio between OH groups and COOH groups (OH / COOH) would be 1.2. The added material was reacted in the presence of 300ppm of titanium tetraisopropoxide relative to the mass of the added material while methanol was flowing out. The temperature was finally raised to 230°C, and the resultant was reacted until the acid value of the resin reached 5mg KOH / g or less. Then, it was reacted under a reduced pressure of 20mmHg to 30mmHg until Mw reached 15,000. The reaction temperature was lowered to 180° C., and trimellitic anhydride was added thereto to obtain [non-crystalline resin A], which was a non-crystalline polyester resin to which carboxylic acid was imparted at its terminal.
[0255] <Production of Crystalline Polyester Resin B>
[0256] To a 5L-four-necked flask equipped with a nitrogen introduction tube, a dehydration tube, a stirrer and a thermocouple, 1,10-decanediol and decanedioic acid were added so that the ratio between the OH group and the COOH group (OH / COOH) would be 1.1. The added material was reacted with 300 ppm of titanium tetraisopropoxide relative to the mass of the added material while water was allowed to flow out. The temperature was finally raised to 230° C., and the resultant was reacted until the acid value of the resin reached 5 mg KOH / g or less. Then, it was reacted under a reduced pressure of 10 mmHg or less for 6 hours to obtain [Crystalline Polyester Resin B].
[0257] <Preparation of Dispersant 1>
[0258] [Non-crystalline resin A] (800 parts) and [crystalline polyester resin B] (200 parts) were mixed using a Henschel mixer (available from Mitsui Mining Co., Ltd.) and kneaded using a twin roll at 100° C. for 10 minutes. After the resultant was rolled and cooled, it was pulverized by a pulverizer to obtain [Dispersant 1].
[0259] <Preparation of Oil Phase>
[0260] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion 1] (335 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. Under stirring, the material was warmed to 80° C., maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 2].
[0261] [Material dissolved liquid 2] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 2].
[0262] (Example 3)
[0263] [Toner 3] was obtained as follows.
[0264] <Preparation of Crystalline Polyester Resin Dispersion>
[0265] [Crystalline polyester resin 1] (446 parts), ethyl acetate (1,894 parts) and [resin 1 for dispersing crystalline polyester resin] (446 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 94% to prepare a mixture of crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of standard state). As a result, [crystalline polyester resin dispersion 3] was obtained.
[0266] <Preparation of Oil Phase>
[0267] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion 3] (446 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. Under stirring, the material was warmed to 80° C., maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 3].
[0268] [Material dissolved liquid 3] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, by filling 0.5 mm-zirconia beads to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 3].
[0269] <Emulsification and solvent removal>
[0270] [Pigment / wax dispersion 3] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 3].
[0271] [Emulsified slurry 3] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was allowed to stand at 30° C. for 2 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 3].
[0272] <Washing and Drying>
[0273] [Dispersion slurry 3] (100 parts) was filtered under reduced pressure and subjected to the following series of washing treatments.
[0274] Specifically, ion exchange water (100 parts) is added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, then filtered. Then, 10% hydrochloric acid (100 parts) is added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, then filtered. Ion exchange water (300 parts) is added to the filter cake obtained and mixed (with 12,000rpm revolutions, 10 minutes) using a TK homomixer, then filtered. The aforementioned operation is carried out twice to obtain [filter cake 3].
[0275] [Filter Cake 3] was dried at 45°C for 48 hours using a circulation dryer, and the resultant was sieved using a mesh having an opening of 75 μm to obtain [Toner Base Particles 3].
[0276] Next, silica having a large particle diameter (HSP160A obtained from FUSOCHEMICAL CO., Ltd., RX40 obtained from NIPPON AEROSIL CO., Ltd.) (2.20 parts) was added to the obtained toner mother particles (100 parts), followed by mixing using a Henschel mixer. Furthermore, silica having a small diameter (R972) (0.6 parts) was mixed using a Henschel mixer, and coarse particles were removed using a sieve having an opening of 37 μm to prepare [Toner 3]. The domain diameter of the crystalline resin of [Toner 3] was 0.10 μm, and the coverage of the crystalline resin on the toner surface was 12%.
[0277] (Example 4)
[0278] [Toner 4] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 4].
[0279] The domain diameter of the crystalline resin of [Toner 4] was 0.20 μm, and the coverage of the crystalline resin on the toner surface was 11%.
[0280] <Preparation of Oil Phase>
[0281] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion 3] (335 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. Under stirring, the material was warmed to 80° C., maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 4].
[0282] [Material dissolved liquid 4] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 4].
[0283] <Emulsification and solvent removal>
[0284] [Pigment / wax dispersion 4] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 4].
[0285] [Emulsified slurry 4] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours. The resultant was allowed to stand at 30° C. for 2 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 4].
[0286] (Example 5)
[0287] [Toner 5] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 5].
[0288] The domain diameter of the crystalline resin of [Toner 5] was 0.60 μm, and the coverage of the crystalline resin on the toner surface was 14%.
[0289] <Preparation of Crystalline Polyester Resin Dispersion>
[0290] [Crystalline polyester resin 1] (446 parts) and ethyl acetate (1,894 parts) were added to a pressure-resistant container in which stirring was performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 85% to prepare a mixture of the crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of standard state). As a result, [Crystalline polyester resin dispersion 5] was obtained.
[0291] <Preparation of Oil Phase>
[0292] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 5] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 5].
[0293] [Material dissolved liquid 5] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion liquid 5].
[0294] <Emulsification and solvent removal>
[0295] [Pigment / wax dispersion 5] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 5].
[0296] [Emulsified slurry 5] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 5].
[0297] (Example 6)
[0298] [Toner 6] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 6].
[0299] The domain diameter of the crystalline resin of [Toner 6] was 0.50 μm, and the coverage of the crystalline resin on the toner surface was 13%.
[0300] <Preparation of Oil Phase>
[0301] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 5] (335 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 6].
[0302] [Material dissolved liquid 6] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, by filling 0.5 mm-zirconia beads to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 6].
[0303] <Emulsification and solvent removal>
[0304] [Pigment / wax dispersion 6] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 6].
[0305] [Emulsified slurry 6] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 6].
[0306] (Example 7)
[0307] [Toner 7] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 7].
[0308] The domain diameter of the crystalline resin of [Toner 7] was 0.60 μm, and the coverage of the crystalline resin on the toner surface was 14%.
[0309] <Preparation of Oil Phase>
[0310] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 5] (112 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 7].
[0311] [Material dissolved liquid 7] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, by filling 0.5 mm-zirconia beads to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 7].
[0312] <Emulsification and solvent removal>
[0313] [Pigment / wax dispersion 7] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 7].
[0314] [Emulsified slurry 7] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 7].
[0315] (Example 8)
[0316] [Toner 8] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 8]. The domain diameter of the crystalline resin of [Toner 8] was 0.10 μm, and the coverage of the crystalline resin on the toner surface was 13%.
[0317] <Preparation of Crystalline Polyester Resin Dispersion>
[0318] [Crystalline polyester resin 1] (446 parts) and ethyl acetate (1,894 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 94% to prepare a mixture of the crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of a standard state). As a result, [Crystalline polyester resin dispersion 8] was obtained.
[0319] <Preparation of Oil Phase>
[0320] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 8] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 8].
[0321] [Material dissolved liquid 1] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads loaded to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 8].
[0322] <Emulsification and solvent removal>
[0323] [Pigment / wax dispersion 8] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 8].
[0324] [Emulsified slurry 8] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left to stand at 30° C. for 2 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 8].
[0325] (Example 9)
[0326] [Toner 9] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 9].
[0327] The domain diameter of the crystalline resin of [Toner 9] was 0.20 μm, and the coverage of the crystalline resin on the toner surface was 14%.
[0328] <Preparation of Oil Phase>
[0329] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 8] (335 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 9].
[0330] [Material dissolved liquid 9] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRAVISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disc peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion liquid 9].
[0331] <Emulsification and solvent removal>
[0332] [Pigment / wax dispersion 9] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 9].
[0333] [Emulsified slurry 9] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours. The resultant was left to stand at 30° C. for 2 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 9].
[0334] (Example 10)
[0335] [Toner 10] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 10].
[0336] The domain diameter of the crystalline resin of [Toner 10] was 1.10 μm, and the coverage of the crystalline resin on the toner surface was 25%.
[0337] <Preparation of Crystalline Polyester Resin Dispersion>
[0338] [Crystalline polyester resin 1] (446 parts) and ethyl acetate (1,894 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 75% to prepare a mixture of the crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of a standard state). As a result, [Crystalline polyester resin dispersion 10] was obtained.
[0339] <Preparation of Oil Phase>
[0340] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 10] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 10].
[0341] [Material dissolved liquid 10] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 10].
[0342] <Emulsification and solvent removal>
[0343] [Pigment / wax dispersion 10] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 10].
[0344] [Emulsified slurry 10] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed at 30° C. for 8 hours. The resultant was left to stand at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 10].
[0345] (Example 11)
[0346] [Toner 11] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 11].
[0347] The domain diameter of the crystalline resin of [Toner 11] was 1.50 μm, and the coverage of the crystalline resin on the toner surface was 26%.
[0348] <Preparation of Crystalline Polyester Resin Dispersion>
[0349] [Crystalline polyester resin 1] (446 parts) and ethyl acetate (1,894 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 73% to prepare a mixture of the crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of a standard state). As a result, [Crystalline polyester resin dispersion 11] was obtained.
[0350] <Preparation of Oil Phase>
[0351] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 11] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 11].
[0352] [Material dissolved liquid 11] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, by filling 0.5 mm-zirconia beads to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 11].
[0353] <Emulsification and solvent removal>
[0354] [Pigment / wax dispersion 11] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 11].
[0355] [Emulsified slurry 11] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left to stand at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 11].
[0356] (Example 12)
[0357] [Toner 12] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 12].
[0358] The domain diameter of the crystalline resin of [Toner 12] was 0.08 μm, and the coverage of the crystalline resin on the toner surface was 10%.
[0359] <Preparation of Crystalline Polyester Resin Dispersion>
[0360] [Crystalline polyester resin 1] (401 parts) and ethyl acetate (1,894 parts) were added to a pressure-resistant container in which stirring was performed, followed by stirring at 180 rpm for 4 hours using an apparatus. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 73% to prepare a mixture of the crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of standard state). As a result, [Crystalline polyester resin dispersion 12] was obtained.
[0361] <Preparation of Oil Phase>
[0362] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 12] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 12].
[0363] [Material dissolved liquid 12] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 12].
[0364] <Emulsification and solvent removal>
[0365] [Pigment / wax dispersion 12] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 12].
[0366] [Emulsified slurry 12] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 12].
[0367] (Comparative Example 1)
[0368] [Toner 13] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 13].
[0369] The domain diameter of the crystalline resin of [Toner 13] was 1.90 μm, and the coverage of the crystalline resin on the toner surface was 14%.
[0370] <Preparation of Oil Phase>
[0371] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin 1] (669 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 13].
[0372] [Material dissolved liquid 13] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 13].
[0373] <Emulsification and solvent removal>
[0374] [Pigment / wax dispersion 13] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 13].
[0375] [Emulsified slurry 13] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was aged at 40° C. for 72 hours to obtain [Dispersion slurry 13].
[0376] (Comparative Example 2)
[0377] [Toner 14] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 14].
[0378] The domain diameter of the crystalline resin of [Toner 14] was 2.1 μm, and the coverage of the crystalline resin on the toner surface was 13%.
[0379] <Preparation of Oil Phase>
[0380] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin 1] (446 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 14].
[0381] [Material dissolved liquid 14] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 14].
[0382] <Emulsification and solvent removal>
[0383] [Pigment / wax dispersion 14] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 14].
[0384] [Emulsified slurry 14] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left to stand at 30° C. for 1 hour for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 14].
[0385] (Comparative Example 3)
[0386] [Toner 15] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 15].
[0387] The domain diameter of the crystalline resin of [Toner 15] was 0.90 μm, and the coverage of the crystalline resin on the toner surface was 35%.
[0388] <Emulsification and solvent removal>
[0389] [Pigment / wax dispersion 14] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 15].
[0390] [Emulsified slurry 15] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was aged at 40° C. for 72 hours to obtain [Dispersion slurry 15].
[0391] (Comparative Example 4)
[0392] [Toner 16] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 16].
[0393] The domain diameter of the crystalline resin of [Toner 16] was 2.00 μm, and the coverage of the crystalline resin on the toner surface was 36%.
[0394] <Preparation of Oil Phase>
[0395] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin 1] (491 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 16].
[0396] [Material dissolved liquid 16] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 16].
[0397] <Emulsification and solvent removal>
[0398] [Pigment / wax dispersion 16] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 16].
[0399] [Emulsified slurry 16] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 16].
[0400] (Comparative Example 5)
[0401] [Toner 17] was obtained in the same manner as in <Emulsification and Solvent Removal> and <Washing and Drying> of Example 1, except that [Pigment / Wax Dispersion Liquid 1] was changed to the following [Pigment / Wax Dispersion Liquid 17].
[0402] The domain diameter of the crystalline resin of [Toner 17] was 0.60 μm, and the coverage of the crystalline resin on the toner surface was 8%.
[0403] <Preparation of Oil Phase>
[0404] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin 1] (112 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 17].
[0405] [Material dissolved liquid 17] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads loaded to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 17].
[0406] (Comparative Example 6)
[0407] [Toner 18] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 18].
[0408] The domain diameter of the crystalline resin of [Toner 18] was 0.10 μm, and the coverage of the crystalline resin on the toner surface was 12%.
[0409] <Preparation of Oil Phase>
[0410] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin 1] (178 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 18].
[0411] [Material dissolved liquid 18] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion liquid 18].
[0412] <Emulsification and solvent removal>
[0413] [Pigment / wax dispersion 18] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 18].
[0414] [Emulsified slurry 18] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left to stand at 30° C. for 2 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 18].
[0415] (Comparative Example 7)
[0416] [Toner 19] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 19].
[0417] The domain diameter of the crystalline resin of [Toner 19] was 2.10 μm, and the coverage of the crystalline resin on the toner surface was 37%.
[0418] <Preparation of Oil Phase>
[0419] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion liquid 1] (669 parts), and ethyl acetate (1,894 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 19].
[0420] [Material dissolved liquid 19] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, by filling 0.5 mm-zirconia beads to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion liquid 19].
[0421] <Emulsification and solvent removal>
[0422] [Pigment / wax dispersion 19] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 19].
[0423] [Emulsified slurry 19] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed over 8 hours at 30° C. The resultant was left standing at 30° C. for 10 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 19].
[0424] (Comparative Example 8)
[0425] [Toner 20] was obtained in the same manner as in <Washing and Drying> of Example 1, except that [Dispersion Slurry 1] was changed to the following [Dispersion Slurry 20].
[0426] The domain diameter of the crystalline resin of [Toner 20] was 0.65 μm, and the coverage of the crystalline resin on the toner surface was 7%.
[0427] <Preparation of Crystalline Polyester Resin Dispersion>
[0428] [Crystalline polyester resin 1] (446 parts), ethyl acetate (1,894 parts) and [resin 1 for dispersing crystalline polyester resin] (446 parts) were added to a pressure-resistant container in which stirring could be performed, followed by stirring at 180 rpm for 4 hours using a device. Carbon dioxide as a supercritical fluid was made to flow under the following conditions so that the volume ratio of carbon dioxide would be 85% to prepare a mixture of crystalline polyester resin and supercritical carbon dioxide: 150° C.; 60 MPa; and a flow rate of 5.0 L / min (value in terms of standard state). As a result, [crystalline polyester resin dispersion 20] was obtained.
[0429] <Preparation of Oil Phase>
[0430] Paraffin wax (melting point: 90° C.) (120 parts), [crystalline polyester resin dispersion 20] (335 parts), ethyl acetate (1,894 parts), and [dispersant 1] (6 parts) were added to a container equipped with a stirring rod and a thermometer. The material was warmed to 80° C. under stirring, maintained at 80° C. for 5 hours, and then cooled to 30° C. over 1 hour. Next, cyan pigment (CI Pigment Blue 15:3) (250 parts) and ethyl acetate (1,000 parts) were added to the container, and the resultant was mixed for 1 hour to obtain [material dissolved liquid 20].
[0431] [Material dissolved liquid 20] (1,324 parts) was transferred to another container, and the pigment and wax were dispersed using a bead mill (ULTRA VISCOMILL, available from Imex Co., Ltd.) at a liquid delivery rate of 1 kg / hr, at a disk peripheral speed of 6 m / sec, through 0.5 mm-zirconia beads filled to 80% by volume, and in 5 passes to obtain [Pigment / wax dispersion 20].
[0432] <Emulsification and solvent removal>
[0433] [Pigment / wax dispersion 20] (375 parts), [prepolymer 1] (500 parts) and [ketimine compound 1] (15 parts) were added to a container and mixed at 5,000 rpm for 5 minutes using a TK homomixer (available from Tokushu Kika Kogyo Co., Ltd.). Then, [aqueous phase 1] (1,200 parts) was added to the container, followed by mixing at 10,000 rpm for 1.5 hours using a TK homomixer to obtain [emulsified slurry 20].
[0434] [Emulsified slurry 20] was added to a container equipped with a stirrer and a thermometer, and the solvent was removed in 8 hours at 30° C. The resultant was left to stand at 30° C. for 12 hours for annealing, and aged at 40° C. for 72 hours to obtain [Dispersion slurry 20].
[0435] (Manufacturing of carrier)
[0436] The following coating materials are dispersed for 10 minutes using an agitator to prepare a coating liquid. The coating liquid (920 parts) and the core material (Mn ferrite particles, weight average diameter: 35 μm) (5,000 parts) are added to a coating device to coat the coating liquid on the core material. Here, the coating device includes a rotating bottom plate disc and a paddle in a fluidized bed and is configured to coat while generating a vortex. The obtained coating product is baked at 250° C. in an electric furnace for 2 hours to obtain a ferrite carrier having an average particle size of 35 μm and coated with a silicone resin (average thickness of 0.5 μm).
[0437] <Coating material>
[0438] ·Toluene…450 parts
[0439] · Silicone resin SR2400 ... 450 parts (obtained from DuPont Toray Specialty Materials K.K., non-volatile component: 50%)
[0440] · Aminosilane SH6020 (obtained from DuPont Toray Specialty Materials KK) ... 10 parts
[0441] Carbon black…10 parts
[0442] (Preparation of two-component developer)
[0443] The prepared carrier (100 parts) and each toner of Examples and Comparative Examples (7 parts) were uniformly mixed to be charged using a TURBULA mixer configured to roll and flip its container for stirring. As a result, a two-component developer was prepared.
[0444] <Evaluation method>
[0445] The items (1) cold offset temperature, (2) hot offset temperature, (3) minimum scraping temperature and (4) cleaning failure were evaluated in the following manner using the prepared toners for evaluation of Examples 1 to 12 and Comparative Examples 1 to 8. The results are listed in Table 2 below.
[0446] <Evaluation Items>
[0447] (1) Cold offset temperature
[0448] The toner (5 parts) and the silicone-coated carrier (95 parts) having a weight average particle size of 60 μm were uniformly mixed to prepare a two-component developer for evaluation. An unfixed image developed by a developer using a commercial copier (imagio NEO450: obtained from Ricoh Company, Ltd.) was fixed at a process speed of 230 mm / sec using a commercial copier (imagio NEO450: obtained from Ricoh Company, Ltd.) in which the fixing unit had been modified and the temperature of the heat roller was variable.
[0449] The image after fixing was visually observed, and the fixing roller temperature at which cold offset did not occur was defined as the minimum fixing temperature.
[0450] [Evaluation criteria for cold offset resistance]
[0451] A: The minimum fixing temperature is 130° C. or less.
[0452] B: The minimum fixing temperature is more than 130° C. but 135° C. or less.
[0453] C: The minimum fixing temperature is greater than 135° C. but 140° C. or less.
[0454] D: The minimum fixing temperature is more than 140°C.
[0455] (2) Thermal offset temperature
[0456] The fixing evaluation was performed in the same manner as in the above minimum fixing temperature. Whether or not thermal offset occurred on the fixed image was visually evaluated.
[0457] The temperature of the fixing roller at which the hot offset occurs is defined as the hot offset temperature.
[0458] [Evaluation criteria for thermal offset resistance]
[0459] A: The maximum fixing temperature is 200° C. or more.
[0460] B: The maximum fixing temperature is 195°C or more but less than 200°C.
[0461] C: The maximum fixing temperature is 190°C or more but less than 195°C.
[0462] D: The maximum fixing temperature is less than 190°C.
[0463] (3) Minimum scratching temperature
[0464] A HEIDON scratch sapphire needle was set in a scratch tester. The radius of the circle scratched by the needle was set to 8 mm, and the load was set to 50 g.
[0465] The image on the paper that has passed through the fixing device is fixed on the plate of the scratch tester, and the handle is turned about ten times. The number of turns of the handle is about 1 time / second to about 2 times / second. The scratched sample is rubbed back and forth vigorously 5 times using HONECOTTO #440 or its equivalent.
[0466] At this time, the temperature at which peeling does not occur is defined as the minimum scratch temperature.
[0467] [Evaluation criteria]
[0468] A: The minimum scratch temperature is 100°C or less.
[0469] B: The minimum scratch temperature is 100°C or more but less than 105°C.
[0470] C: The minimum scratch temperature is 105°C or more but less than 110°C.
[0471] D: The minimum scratch temperature is 110° C. or more.
[0472] (4) Poor cleaning
[0473] Printing was performed on 10K (1K=1000) sheets of paper using a developer (prepared two-component developer) by an existing Ricoh copier. Then, the developer was exposed to an environment (temperature of 10° C. and humidity of 15% RH). Under this condition, printing was performed on 1K sheets of paper.
[0474] Then, when a white paper image is fed, the photoreceptor stops immediately after the white paper image passes through the cleaning blade. After the photoreceptor passes through the cleaning blade, the residual toner on the photoreceptor is transferred to a piece of tape. Then, the difference between the image density of the untransferred tape and the image density of the transferred tape is measured and judged using a spectral densitometer (obtained from X-Rite).
[0475] [Evaluation criteria]
[0476] A: The difference between the image density of the untransferred tape and the image density of the transferred tape was less than 0.01.
[0477] B: The difference between the image density of the untransferred tape and the image density of the transferred tape is 0.01 or more but less than 0.05.
[0478] C: The difference between the image density of the untransferred tape and the image density of the transferred tape is 0.05 or more but less than 0.11.
[0479] D: The difference between the image density of the untransferred tape and the image density of the transferred tape is 0.11 or more.
[0480]
[0481] [Table 2]
[0482]
[0483] For example, aspects of the present disclosure are as follows.
[0484] <1> Toner for developing electrostatically charged images,
[0485] wherein the spin-spin relaxation time of the colorant at 90°C is 0.30 msec or greater but 1.50 msec or less, and the spin-spin relaxation time of the colorant at 50°C is 0.0185 msec or greater but 0.0300 msec or less, and the spin-spin relaxation time of the colorant at 90°C and the spin-spin relaxation time of the colorant at 50°C are obtained by a Hahn echo method of pulsed NMR analysis.
[0486] <2> according to <1> Toner for developing electrostatic charge images,
[0487] wherein the toner has a spin-spin relaxation time at 90° C. of 1.0 msec or more but 1.5 msec or less.
[0488] <3> according to <1> or <2> A toner for electrostatic charge image development, further comprising:
[0489] non-crystalline polyester resin; and crystalline polyester resin.
[0490] <4> according to <3> Toner for developing electrostatic charge images,
[0491] The toner has a domain-matrix structure in which a non-crystalline polyester resin is a matrix and a crystalline polyester resin is a domain.
[0492] <5> according to <4> Toner for developing electrostatic charge images,
[0493] wherein the domain diameter of the crystalline polyester resin is 0.10 μm or more but 1.0 μm or less.
[0494] <6> according to <3> to <5> Any toner for developing an electrostatic charge image,
[0495] wherein the coverage of the crystalline polyester resin on the surface of the toner is less than 20%, the coverage being measured by observing a cross section of the toner.
[0496] <7> according to <3> to <6> Any toner for developing an electrostatic charge image,
[0497] wherein the amount of the crystalline polyester resin is 1% by mass or more but 20% by mass or less relative to the amount of the toner.
[0498] <8> A toner storage unit comprising:
[0499] Unit; and
[0500] According to the unit stored <1> to <7> Any toner.
[0501] <9> An image forming apparatus comprising:
[0502] Electrostatic latent image bearing body;
[0503] an electrostatic latent image forming unit configured to form an electrostatic latent image on an electrostatic latent image bearing body; and
[0504] a developing unit including a toner and configured to develop an electrostatic latent image formed on an electrostatic latent image bearing member using the toner to form a toner image,
[0505] The toner is based on <1> to <7> Any toner for developing an electrostatic charge image.
[0506] <10> An image forming method, comprising:
[0507] forming an electrostatic latent image on an electrostatic latent image bearing member; and
[0508] developing the electrostatic latent image formed on the electrostatic latent image bearing member using a toner to form a toner image,
[0509] The toner is based on <1> to <7> Any toner for developing an electrostatic charge image.
[0510] according to <1> to <7> Toner for electrostatic charge image development, according to <8> toner storage unit, according to <9> Image forming apparatus and according to <10> The image forming method can solve the conventional problems and can achieve the purpose of the present disclosure.
Claims
1. Toner for developing electrostatic charge images, wherein the spin-spin relaxation time of the toner at 90° C. is 0.30 milliseconds or more but 1.50 milliseconds or less, and the spin-spin relaxation time of the toner at 50° C. is 0.0185 milliseconds or more but 0.0300 milliseconds or less, the spin-spin relaxation time of the toner at 90° C. and the spin-spin relaxation time of the toner at 50° C. being obtained by a Hahn echo method of pulsed NMR analysis, The toner further comprises: Non-crystalline polyester resin; and crystalline polyester resin, and wherein the coverage of the crystalline polyester resin on the surface of the toner, as measured by observing a cross section of the toner, is less than 20%, The toner has a domain-matrix structure in which the non-crystalline polyester resin is a matrix and the crystalline polyester resin is a domain.
2. The toner for developing an electrostatic charge image according to claim 1, wherein the toner has a spin-spin relaxation time at 90° C. of 1.0 msec or more but 1.5 msec or less.
3. The toner for developing an electrostatic charge image according to claim 1, wherein the domain diameter of the crystalline polyester resin is 0.10 μm or more but 1.0 μm or less.
4. The toner for developing an electrostatic charge image according to any one of claims 1 to 3, wherein the amount of the crystalline polyester resin is 1% by mass or more but 20% by mass or less relative to the amount of the toner.
5. A toner storage unit comprising: unit; and The toner according to any one of claims 1 to 4 stored in the unit.
6. An image forming apparatus comprising: Electrostatic latent image bearing body; an electrostatic latent image forming unit configured to form an electrostatic latent image on the electrostatic latent image bearing body; and a developing unit including a toner and configured to develop the electrostatic latent image formed on the electrostatic latent image bearing member using the toner to form a toner image, The toner is the toner for developing an electrostatic charge image according to any one of claims 1 to 4.
7. An image forming method comprising: forming an electrostatic latent image on an electrostatic latent image bearing body; and developing the electrostatic latent image formed on the electrostatic latent image bearing member using a toner to form a toner image, The toner is the toner for developing an electrostatic charge image according to any one of claims 1 to 4.