Method for producing electrode foil for electrolytic capacitor
By adjusting the current density in two steps in the electrolytic etching process, the problem of uneven etching pit of electrolytic capacitors is solved, the electrostatic capacitance is improved, and the higher capacitance requirements are met.
Patent Information
- Application Number
- CN202011135517.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-30
- Filing Date
- 2020-10-21
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2040-10-21
AI Technical Summary
It is difficult for existing electrolytic capacitors to form uniform etching pits during the etching process, resulting in insufficient electrostatic capacitance and unable to meet the higher requirements in recent years.
The electrolytic etching process is used, which is divided into two steps: the first step flows through the current at the maximum current density when the etching starts to 30% of the total time, and the second step uses the current density to be more than 10% of the maximum current density in the remaining time. And etching is continued below 30%, eliminating current flow bias and forming a uniform etching pit.
Through this method, a more uniform etching pit can be formed on the metal foil, the electrostatic capacitance of the electrolytic capacitor can be improved, and the higher electrostatic capacitance needs can be met.
Smart Images

Figure CN112750625B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing an electrode foil for an electrolytic capacitor. Background Art
[0002] As the anode body of the capacitor element, a metal foil containing a valve metal can be used. In order to increase the capacitance of the capacitor element, etching is performed on all or part of the main surface of the metal foil. Patent document 1 teaches that a large current flows at the beginning of the electrolytic etching process and then gradually decreases.
[0003] Prior Art Literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2005-203529 Summary of the invention
[0006] Problems to be solved by the invention
[0007] According to Patent Document 1, the electrostatic capacitance of the electrolytic capacitor is improved by generating uniform etching pits in the aluminum foil. However, in recent years, electrolytic capacitors are required to have higher electrostatic capacitance.
[0008] Means for solving problems
[0009] The first aspect of the present invention relates to a method for manufacturing an electrode foil for an electrolytic capacitor, which includes an electrolytic etching step in which a current is passed through at least one main surface of a metal foil in an etching solution to etch the metal foil. The electrolytic etching step includes a first step of etching the metal foil from the start of etching of the metal foil until 30% of the total time T during which the metal foil is etched has passed; and a second step of etching the metal foil after the first step. In the first step, the current density of the current flowing through the metal foil reaches a maximum current density A1. In the second step, the current density of the current flowing through the metal foil is greater than 10% and less than 30% of the maximum current density A1 for more than 50% of the total time T.
[0010] Effects of the Invention
[0011] According to the present invention, more uniform etching pits can be formed in the metal foil. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a graph showing changes in current density in the electrolytic etching step according to one embodiment of the present invention.
[0013] Figure 2AThis is a graph showing an example of changes in current density in the first step according to one embodiment of the present invention.
[0014] Figure 2B This is a graph showing another example of the change in current density in the first step according to one embodiment of the present invention.
[0015] Figure 2C This is a graph showing still another example of the change in current density in the first step according to one embodiment of the present invention.
[0016] Figure 2D This is a graph showing still another example of the change in current density in the first step according to one embodiment of the present invention.
[0017] Figure 2E This is a graph showing still another example of the change in current density in the first step according to one embodiment of the present invention.
[0018] Figure 2F This is a graph showing still another example of the change in current density in the first step according to one embodiment of the present invention.
[0019] Figure 3 This is a graph showing an example of the change in current density in the second step according to one embodiment of the present invention.
[0020] Figure 4A This is a graph showing another example of the change in current density in the second step according to one embodiment of the present invention.
[0021] Figure 4B This is a graph showing still another example of the change in current density in the second step according to one embodiment of the present invention.
[0022] Figure 4C This is a graph showing still another example of the change in current density in the second step according to one embodiment of the present invention.
[0023] Figure 4D This is a graph showing still another example of the change in current density in the second step according to one embodiment of the present invention.
[0024] Figure 4E This is a graph showing still another example of the change in current density in the second step according to one embodiment of the present invention.
[0025] Figure 5 This is an explanatory diagram schematically showing an etching device used in the electrolytic etching process according to one embodiment of the present invention.
[0026] Figure 6It is a cross-sectional view schematically showing a capacitor element according to one embodiment of the present invention.
[0027] Figure 7 It is a cross-sectional view schematically showing an electrolytic capacitor according to one embodiment of the present invention.
[0028] Explanation of symbols
[0029] 20: Etching device;
[0030] 22: Electrode;
[0031] 23: Etching groove;
[0032] 24: AC power supply;
[0033] 25: Conveying roller;
[0034] 10: Metal foil;
[0035] 11: electrode foil (anode);
[0036] 100: electrolytic capacitor;
[0037] 110: capacitor element;
[0038] 110a: anode portion;
[0039] 110b: cathode portion;
[0040] 12: dielectric layer;
[0041] 13: cathode layer;
[0042] 13a: solid electrolyte layer;
[0043] 13b: cathode lead layer;
[0044] 120A: Anode lead terminal;
[0045] 120B: cathode lead terminal;
[0046] 130: Insulation material. DETAILED DESCRIPTION
[0047] The manufacturing method of the electrode foil involved in this embodiment includes: an electrolytic etching process, in which a current is passed through at least one main surface of the metal foil in an etching solution to etch the metal foil. The electrolytic etching process includes a first step and a second step. In the first step, the metal foil is etched from the start of etching of the metal foil until 30% of the total time T (hereinafter sometimes referred to as etching time T) during which the metal foil is etched has passed. In the second step, the metal foil is further etched after the first step.
[0048] The electrolytic etching process refers to the period from the start to the end of the etching process on the metal foil, and also includes the time when no current flows through the metal foil, that is, the current density is zero. On the other hand, the above-mentioned etching time T does not include the time when no current flows through the metal foil (hereinafter sometimes referred to as the non-electrolysis time). In addition, a small amount of current (for example, 0.0016A / cm 2 The time when the electrolyte flows through the metal foil may also be included in the electroless time.
[0049] The first step is an etching process performed from the start of current flow to the metal foil until the total current flow time (hereinafter sometimes referred to as electrolysis time) reaches 30% of the etching time T. The second step is an etching process performed after the first step until the current flow to the metal foil stops.
[0050] Figure 1 is a graph showing the change in current density during the electrolytic etching process. Figure 1 In the case of electrolysis time or not, the first step is performed until the electrolysis time (t1, t2, t3) is added and the total of them exceeds 30% of the etching time T. The etching time T is the total electrolysis time in the electrolytic etching process. Figure 1 In the case of , the etching time T is the sum of t1, t2, t3, t4, t5 and t6.
[0051] Sometimes, an oxide film is formed on the surface of the metal foil. Since the oxide film is a resistance component, when a current flows through the metal foil, the current flows unevenly. As a result, the etching pits formed on the surface of the metal foil are also uneven.
[0052] In this embodiment, in the first step, a current is passed so that the current density of the current flowing through the metal foil becomes the maximum current density A1, and in the second step, a current is passed so that the current density of the current flowing through the metal foil becomes 10% or more and 30% or less of the maximum current density A1 for more than 50% of the etching time T. In other words, a very large current flows through the metal foil at an early stage from the start of the etching process. As a result, the bias of the flow of current on the surface of the metal foil can be eliminated, thereby forming uniformly distributed etching pits. The etching pits formed on the surface of the metal foil are dug deeper by the subsequent weak current.
[0053] The time for which the current that can obtain the maximum current density A1 (hereinafter sometimes referred to as the large current A) flows is not particularly limited. The large current A may flow for a time of more than 0.5%, more than 3%, and especially more than 5% of the etching time T in the first step. In addition, the large current A may flow for a time of less than 25%, less than 20%, and especially less than 10% of the etching time T in the first step.
[0054] The large current A may start flowing during the period from the start of etching of the metal foil to 10% of the etching time T in the first step. As a result, the bias in the flow of current on the surface of the metal foil is eliminated at a very early stage, so that the etching pits become more easily distributed. It is preferred that the large current A starts flowing and ends flowing during the period from the start of etching of the metal foil to 10% of the etching time T.
[0055] In the first step, the current flowing through the metal foil may be constant or variable. For example, during the first step, a current may be passed such that the current density of the current flowing through the metal foil reaches the maximum current density A1. In the first step, it is preferred that the current flowing through the metal foil changes. As a result, the direction of the current flowing through the metal foil surface changes, and the bias of the current flow becomes easier to eliminate.
[0056] The electric current, i.e., the density of the electric current flowing through the electrode foil (hereinafter referred to simply as the current density), can change in stages or continuously. The continuous change can be either a linear function, a quadratic function, or a combination thereof. The current density can increase in stages or continuously until the maximum current density A1 is reached. The current density can also decrease in stages or continuously after reaching the maximum current density A1. Among them, the current density is preferably increased in stages until the maximum current density A1 is reached. As a result, the direction of the current flowing through the surface of the metal foil becomes easier to change.
[0057] FIG. 2A to FIG. 2F : is a graph showing an example of change in current density in the first step. In the example of the figure, for convenience, the change in current density in the second step is shown by a dotted line, but the present invention is not limited to this.
[0058] exist Figure 2A In the etching process, the current density increases from the initial current density A0 to the maximum current density A1 in one stage, and then decreases to the current density A0 again. The maximum current density A1 is maintained during about 10% of the etching time T. Figure 2B In the process, a large current A flows from the beginning, and the current density is the maximum current density A1. The maximum current density A1 is maintained from the start of etching of the metal foil to 10% of the etching time T. Then, the current density decreases to the current density A0.
[0059] exist Figure 2C In the process, the current density increases continuously from the initial current density A0 until it reaches the maximum current density A1. Figure 2D In the embodiment, the current density increases stepwise from the initial current density A0 until it reaches the maximum current density A1. In any case, the current density then decreases again to the current density A0.
[0060] exist Figure 2E In the example, after a large current A initially flows, the current density decreases continuously from A1 to A0. Figure 2F In the example, after a large current A initially flows, the current density decreases stepwise from A1 to A0.
[0061] In the second step, a current is passed through the metal foil so that the current density is 10% to 30% of the maximum current density A1 for 50% or more of the etching time T. Thus, the etching pit formed on the surface of the electrode foil in the first step is deepened.
[0062] The time during which the current density flows to a value that is 10% or more and 30% or less of the maximum current density A1 (hereinafter referred to as the base current) is 55% or more of the etching time T, and can be 60% or more and 70% or less. The current density based on the base current is preferably 15% or more of the maximum current density A1, and preferably 25% or less.
[0063] In the second step, the magnitude of the current may be varied. That is, in the second step, the density of the current flowing through the metal foil may be increased or decreased.
[0064] For example, a current smaller than the base current or a current larger than the base current may flow through the electrode foil at a time other than when the base current flows. Furthermore, a current larger than the large current A may flow through the electrode foil. Among them, it is preferred to flow a current larger than the base current and smaller than the large current A more than once in a short period of time. As a result, the current density increases intermittently, making it easier to form new etching pits. Therefore, the unevenness of the etching pits can be further suppressed.
[0065] The time for each time a current larger than the base current flows through the electrode foil is not particularly limited, but can be, for example, 0.1% or more, 0.2% or more, and especially 0.5% or more of the etching time T in the second step. In addition, the time for each time a current larger than the base current flows through the electrode foil can also be less than 5% or less than 3% or especially less than 2% of the etching time T in the second step. The current larger than the base current preferably flows intermittently more than twice. The current density at this time is, for example, greater than 30% of the maximum current density A1 and less than 75%.
[0066] Figure 3 is a graph showing the change in current density in the second step. In the example of the figure, for convenience, the change in current density in the first step is shown by a dotted line, but it is not limited to this. Figure 3 In the process, a current larger than the base current and smaller than the large current A flows intermittently multiple times.
[0067] In addition, by changing the magnitude of the base current, the current density can be increased or decreased within a range of 10% to 30% of the maximum current density Al. The current density can be increased or decreased in stages or continuously. The continuous change can be a linear function, a quadratic function, or a combination thereof.
[0068] FIG. 4A to FIG. 4E is a graph showing the change in current density in the second step. In the example of the figure, for convenience, the change in current density in the first step is shown by a dotted line, but it is not limited to this. FIG. 4A to FIG. 4E In the embodiment, the current density is changed within a range of 10% to 30% of the maximum current density A1.
[0069] exist Figure 4A In the case of , the current density decreases as a linear function. Figure 4B In the case of , the current density decreases as a quadratic function. Figure 4C In the case of Figure 4D In the process, the current density is maintained at a certain level and then decreases as a linear function. Figure 4E In the process, the current density is maintained at a certain level, then decreases as a linear function and is maintained at a certain level again.
[0070] [Electrolytic Etching Process]
[0071] With the electrode facing at least one main surface of the metal foil, an electric current is passed between the metal foil and the electrode in an etching solution to etch the metal foil.
[0072] The current flowing between the metal foil and the electrode may be either AC or DC. Etching may be performed on only one main surface of the metal foil or on both main surfaces. When an AC power source is used, the frequency is not particularly limited. The frequency of the AC power source is, for example, greater than 1 Hz and less than 500 Hz.
[0073] The current density flowing through the electrode foil is not particularly limited and can be appropriately set according to the thickness of the electrode foil, the depth of the desired etching pit, etc. The maximum current density A1 flowing through the metal foil in the first step can be, for example, 0.5 A / cm 2 Above, it can be 0.8A / cm 2 Above, especially 1A / cm 2 The maximum current density A1 flowing through the metal foil in the first step can be, for example, 10 A / cm 2 Below, and further can be 8A / cm 2 Below, in particular, can be 5A / cm 2 the following.
[0074] The etching time T is not particularly limited, and similarly to the above, it can be appropriately set according to the thickness of the electrode foil, the depth of the desired etching pit, etc. The etching time T can be, for example, more than 5 minutes, and further can be more than 10 minutes. The etching time T can be, for example, less than 60 minutes, and further can be less than 50 minutes.
[0075] In the electrolytic etching process, the etching of the metal foil is preferably performed intermittently. In other words, the electrolytic etching process preferably has a non-electrolysis time. As a result, the diffusion of metal ions originating from the metal foil generated in the etching pit is promoted, making it easy to improve the etching efficiency. The non-electrolysis time is, for example, the time for the metal foil to move between the electrodes when there are multiple electrodes, or the time for the metal foil to move between the etching grooves when there are multiple etching grooves.
[0076] In addition, the electrolysis-free time may be a cleaning step for cleaning the metal foil. For cleaning the metal foil, pure water (ion exchange water) is preferably used. This is to remove impurities and make the above-mentioned metal ions more easily diffused. The cleaning step may be performed midway during the etching in the first step, midway during the etching in the second step, or midway between the two steps.
[0077] The metal foil contains valve metals such as titanium, tantalum, aluminum and niobium. The metal foil contains one or more of the above-mentioned valve metals. Alternatively, the metal foil contains the above-mentioned valve metal in the form of an alloy or an intermetallic compound. The thickness of the metal foil is not particularly limited. The thickness of the metal foil is, for example, greater than 15 μm and less than 300 μm, or greater than 80 μm and less than 250 μm.
[0078] As the etching solution, a known etching solution used in electrolytic etching can be used. As the etching solution, for example, an aqueous solution containing sulfuric acid, nitric acid, phosphoric acid and / or oxalic acid and hydrochloric acid can be cited. Various additives such as a chelating agent may also be included in the aqueous solution. The concentration of hydrochloric acid in the etching solution, the concentration of other acids and the temperature are not particularly limited, as long as they are appropriately set according to the desired shape of the etching pit and the performance of the capacitor. The concentration of hydrochloric acid in the etching solution is, for example, greater than 1 mol / L and less than 10 mol / L. The concentration of other acids in the etching solution is, for example, greater than 0.01 mol / L and less than 1 mol / L. The temperature of the etching solution in the electrolytic etching process is not particularly limited, and is, for example, greater than 15°C and less than 60°C.
[0079] Figure 51 is an explanatory diagram schematically showing an etching device used in the electrolytic etching process according to the present embodiment. The etching device 20 includes an etching tank 23 for holding an etching solution, a plurality of conveying rollers 25 for conveying a metal foil 10, a pair of electrodes 22 facing the metal foil 10, and an AC power source 24 for passing a current through the electrodes 22. The metal foil 10 moves in the etching tank 23 while being conveyed by the plurality of conveying rollers 25. The metal foil 10 is etched while facing the electrodes 22 in the etching tank 23. Thus, the electrode foil 11 can be obtained.
[0080] exist Figure 5 In the figure, the etching of a long metal foil is shown, but the present invention is not limited to this. For example, the etching of a metal foil having a certain area which is stationary can also be performed. Figure 5 In the embodiment, a pair of electrodes is used, but it is not limited to this. For example, a metal foil may be placed opposite to an electrode, and the electrode and the metal foil may be connected to an AC power supply for etching. Furthermore, there may be multiple etching grooves. In one etching groove, there may be more than two pairs of electrodes.
[0081] [Capacitor elements]
[0082] The electrode foil obtained by etching the metal foil as described above is used as an anode body of a capacitor element. The long electrode foil is punched into a desired shape.
[0083] The capacitor element has an anode portion and a cathode portion. The anode portion includes a portion of the anode body. The cathode portion includes: the remaining portion of the anode body, a dielectric layer formed on at least a portion of the surface of the anode body, and a cathode layer formed on at least a portion of the surface of the dielectric layer. The cathode layer includes: a solid electrolyte layer formed on at least a portion of the dielectric layer, and a cathode lead layer formed on at least a portion of the solid electrolyte layer. Such a capacitor element is, for example, in the form of a sheet or a plate.
[0084] (Dielectric layer)
[0085] The dielectric layer is formed on at least a portion of the surface of the anode body. The dielectric layer is formed, for example, by anodizing the surface of the anode body through a chemical conversion treatment or the like. Therefore, the dielectric layer may contain an oxide of a valve metal. For example, when aluminum is used as the valve metal, the dielectric layer may contain Al2O3. In addition, the dielectric layer is not limited thereto, and any structure that functions as a dielectric may be used.
[0086] (Cathode layer)
[0087] The cathode layer includes, for example, a solid electrolyte layer and a cathode lead layer.
[0088] The solid electrolyte layer only needs to be formed to cover at least a portion of the dielectric layer, and may be formed to cover the entire surface of the dielectric layer.
[0089] The solid electrolyte layer can use, for example, a manganese compound or a conductive polymer. As the conductive polymer, polypyrrole, polyaniline, polythiophene, polyacetylene, derivatives thereof, etc. can be used. The solid electrolyte layer containing the conductive polymer can be formed, for example, by chemically polymerizing and / or electrolytically polymerizing the raw material monomer on the dielectric layer. Alternatively, it can be formed by applying a solution in which the conductive polymer is dissolved or a dispersion in which the conductive polymer is dispersed to the dielectric layer.
[0090] The cathode lead layer only needs to be formed so as to cover at least a portion of the solid electrolyte layer, and may be formed so as to cover the entire surface of the solid electrolyte layer.
[0091] The cathode lead layer includes, for example, a carbon layer and a metal (e.g., silver) paste layer formed on the surface of the carbon layer. The carbon layer includes a composition containing conductive carbon materials such as graphite. The metal paste layer includes, for example, a composition containing silver particles and resin. In addition, the structure of the cathode lead layer is not limited to this, as long as it has a current collection function.
[0092] Figure 6 1 is a cross-sectional view schematically showing a capacitor element according to the present embodiment. Capacitor element 110 is in a sheet shape. Anode portion 110a includes electrode foil (anode body) 11. Cathode portion 110b includes anode body 11, dielectric layer 12, and cathode layer 13. Cathode layer 13 includes solid electrolyte layer 13a and cathode extraction layer 13b.
[0093] [Electrolytic capacitors]
[0094] The capacitor element constitutes an electrolytic capacitor. The electrolytic capacitor may also include a plurality of capacitor elements. The plurality of capacitor elements are stacked. The number of stacked capacitor elements is not particularly limited, and is, for example, 2 or more and 20 or less.
[0095] The anode parts of the stacked capacitor elements are joined to each other by welding and / or riveting, so as to be electrically connected. An anode lead terminal is joined to the anode part of at least one capacitor element. The plurality of anode parts are riveted, for example, by a bent anode lead terminal. The anode part and the anode lead terminal may also be further laser welded. Thus, the connection reliability of the plurality of anode parts to each other and the connection reliability of the anode part and the anode lead terminal are improved.
[0096] In addition, the cathode portions of the stacked capacitor elements are also electrically connected. A cathode lead terminal is bonded to the cathode layer of at least one capacitor element. The cathode lead terminal is bonded to the cathode layer via a conductive adhesive, for example.
[0097] The capacitor element is sealed by an insulating material so that at least a portion of the anode lead terminal and the cathode lead terminal are exposed. As the insulating material, for example, a cured product of a thermosetting resin and an engineering plastic can be cited. As the thermosetting resin, for example, an epoxy resin, a phenolic resin, a silicone resin, a melamine resin, a urea resin, an alkyd resin, a polyurethane, and an unsaturated polyester can be cited. Engineering plastics include general engineering plastics and super engineering plastics. As engineering plastics, for example, polyimide and polyamide-imide can be cited.
[0098] Figure 7 The electrolytic capacitor 100 includes one or more capacitor elements 110, an anode lead terminal 120A joined to an anode portion 110a of the capacitor element 110, a cathode lead terminal 120B joined to a cathode portion 110b, and an insulating material 130 that seals the capacitor element.
[0099] In this embodiment, a solid electrolyte is used as an electrolyte, and an electrolytic capacitor in which a capacitor element is sealed by an insulating material is cited, but it is not limited to this. The electrode foil involved in this embodiment can be applied to the following electrolytic capacitor, for example, having an anode formed by a strip of electrode foil and a capacitor element wound with a separator and an electrolyte. In this case, the electrode foil involved in this embodiment is used for at least one of the anode and the cathode.
[0100] [Example]
[0101] Hereinafter, the present invention will be described in more detail based on Examples, but the present invention is not limited to the Examples.
[0102] 《Example 1》
[0103] Aluminum foil having a thickness of 100 μm and a purity of 99.98% was prepared and pre-treated by immersing the aluminum foil in an aqueous solution having a phosphoric acid concentration of 1.0 mass % and a temperature of 90° C. for 60 seconds.
[0104] Next, use Figure 5 The etching apparatus shown in the figure performed electrolytic etching as follows. As an etching solution, an aqueous solution containing 5 mass % hydrochloric acid, 2 mass % aluminum chloride, 0.1 mass % sulfuric acid, 0.5 mass % phosphoric acid, and 0.2 mass % nitric acid was used, and the liquid temperature was set to 35° C. The frequency of the AC power supply was set to 35 Hz. The etching time T was set to 5 minutes.
[0105] In step 1, follow Figure 2A The maximum current density of Al is 3A / cm 2 In step 2, follow Figure 4AThat is, the current density based on the base current is increased from 0.5A / cm 2 (about 17% of the maximum current density A1) and then continuously reduced to 0.3 A / cm 2 (10% of the maximum current density of Al).
[0106] Finally, the aluminum foil was immersed in a 60° C. aqueous solution containing 10 mass % sulfuric acid for 60 seconds, and then heat-treated at 250° C. for 120 seconds to produce an electrode foil for an electrolytic capacitor.
[0107] Comparative Example 1
[0108] In addition to setting the maximum current density to 0.5 A / cm in step 1 2 In other respects, the electrode foil was obtained in the same manner as in Example 1. That is, in the second step, the current density based on the base current was increased from 100% (0.5 A / cm 2 ) is continuously reduced until the maximum current density A1 is 60% (0.3A / cm 2 ).
[0109] The surfaces of the electrode foil obtained in Example 1 and the electrode foil obtained in Comparative Example 1 were confirmed by scanning electron microscopy. Within the observation field, the average etching pit diameter on the surface of the electrode foil of Example 1 was smaller than that of Comparative Example 1. Furthermore, within the observation field, the number of etching pits formed on the surface of the electrode foil of Example 1 was greater than that of Comparative Example 1, and the etching pits were more evenly distributed.
[0110] Industrial Applicability
[0111] The electrode foil produced by the method according to the present invention can achieve high electrostatic capacitance and thus can be used in capacitors for various purposes.
Claims
1. A method for manufacturing an electrode foil for an electrolytic capacitor, comprising: an electrolytic etching step of etching the metal foil by passing an electric current through at least one main surface of the metal foil in an etching solution, The electrolytic etching process comprises: In a first step, the metal foil is etched from the start of etching of the metal foil until 30% of the total time T during which the metal foil is etched has passed; and In the second step, after the first step, the metal foil is etched. In the first step, the current density of the current flowing through the metal foil reaches the maximum current density A1, In the second step, the current density of the base current flowing through the metal foil is 10% to 30% of the maximum current density A1 for 50% to 70% of the total time T. The current flowing to etch the metal foil in the electrolytic etching step is an alternating current.
2. The method for producing an electrode foil for an electrolytic capacitor according to claim 1, wherein: In the second step, after the base current flows for a certain period of time, a current that is larger than the base current and smaller than a current that gives the maximum current density A1 flows.
3. The method for producing an electrode foil for an electrolytic capacitor according to claim 1 or 2, wherein: During the period from the start of etching of the metal foil to 10% of the total time T, the current density of the current flowing through the metal foil reaches the maximum current density A1.
4. The method for producing an electrode foil for an electrolytic capacitor according to claim 1 or 2, wherein: In the first step, the current density of the current flowing through the metal foil is changed stepwise.
5. The method for producing an electrode foil for an electrolytic capacitor according to claim 1 or 2, wherein: In the first step, the current density of the current flowing through the metal foil is continuously changed.
6. The method for producing an electrode foil for an electrolytic capacitor according to claim 5, wherein: In the first step, the current density of the current flowing through the metal foil is continuously increased until it reaches the maximum current density A1.
7. The method for producing an electrode foil for an electrolytic capacitor according to claim 1 or 2, wherein: In the electrolytic etching step, the etching of the metal foil is performed intermittently.
8. The method for producing an electrode foil for an electrolytic capacitor according to claim 7, wherein: The electrolytic etching process includes a cleaning step of cleaning the metal foil.
9. The method for producing an electrode foil for an electrolytic capacitor according to claim 1 or 2, wherein: In the second step, the current density of the current flowing through the metal foil is increased or decreased.
Citation Information
Patent Citations
Method for manufacturing electrode foil for aluminum electrolytic capacitor
JP2005203529A
Method for etching holes by corroding aluminum foil
CN101752095A
Etching method for electrode of electrolytic capacitor
JP1991104207A
Manufacture of aluminum foil for electrolytic capacitor
JP1991270117A
Manufacture of aluminum foil for electrolytic capacitor
JP1992305911A