Covering layer for bit line resistance reduction

Through low-temperature deposition and the use of silicon nitride or silicon carbonitride as diffusion barriers, the problems of high bit line resistivity and metal surface roughness in integrated circuits are solved, and a bit line stack structure with low resistance characteristics is achieved, improving the Operational integrity of integrated circuits.

CN112789724BActive Publication Date: 2024-10-18APPLIED MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN201980064979.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2019-10-18
Publication Date
2024-10-18
Estimated Expiration
2039-10-18

AI Technical Summary

Technical Problem

The conductive interconnect layers of modern integrated circuits increase bit line resistance due to high deposition temperatures, and the metal surface roughness is difficult to control, affecting operational integrity.

Method used

Using a low-temperature deposition method, a covering layer is used to prevent the surface roughness of the bit line metal from increasing, and silicon nitride or silicon carbonitride is used as a diffusion barrier to reduce the resistivity and form a bit line stack structure with low resistance characteristics.

Benefits of technology

Effectively reduces the resistivity of the bit line, prevents hard mask elements from migrating to the bit line metal layer, ensures a clean interface and low RC time constant, and improves the operational integrity of the integrated circuit.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN112789724B_ABST
    Figure CN112789724B_ABST
Patent Text Reader

Abstract

Memory elements and methods of forming memory elements are described herein. The memory element includes a substrate having at least one film stack. The film stack includes a polysilicon layer on the substrate; a bitline metal layer on the polysilicon layer; a capping layer on the bitline metal layer; and a hard mask on the capping layer. Some embodiments of the memory element include an optional barrier metal layer on the polysilicon layer, and the bitline metal layer is on the barrier metal layer. Methods of forming electronic elements are described herein, wherein one or more patterns are transferred through films of the film stack to provide bitlines of the memory element.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present disclosure relate to the field of electronic components and electronic component manufacturing. More particularly, embodiments of the present disclosure provide electronic components including bit lines with reduced resistance and methods of forming the same. Background Art

[0002] The conductive interconnect layers of modern integrated circuits typically have very fine pitches and high density. A single small defect in a precursor metal film that ultimately forms a metal interconnect layer of an integrated circuit may be located in a position that severely compromises the operational integrity of the integrated circuit.

[0003] Bitline stack deposition encounters a number of potential problems. Surface reactions of the metal and silicon nitride hard mask may occur due to the high deposition temperatures experienced during hard mask formation. Bitline resistance may increase due to interdiffusion of silicon into the bitline and metal atoms into the silicon nitride hard mask. Additionally, grain-grown metals may be difficult to use due to metal surface roughness caused by high temperature silicon nitride hard mask formation.

[0004] Therefore, there is a need in the art for bitline stacking and / or methods of forming bitlines having lower resistivity. Summary of the invention

[0005] One or more embodiments of the present disclosure are directed to a memory element, the memory element comprising a substrate having at least one film stack thereon, the film stack comprising a polysilicon layer on the substrate, a bit line metal layer on the polysilicon layer, a capping layer on the bit line metal layer, and a hard mask on the capping layer.

[0006] Additional embodiments of the present disclosure are directed to methods of forming a memory element. A substrate is provided having a conductive layer having a barrier layer thereon and a bit line metal layer on the barrier layer. A capping layer is formed on the bit line metal layer at a temperature of less than or equal to about 500° C. A hard mask is formed on the capping layer at a temperature of greater than or equal to about 650° C. Elements of the hard mask are substantially prevented from migrating into the bit line metal layer.

[0007] Another embodiment of the present disclosure is directed to a method of forming a memory element. A substrate is provided having a film stack thereon. The film stack includes a polysilicon layer, a barrier metal layer on the polysilicon layer, a barrier layer on the barrier metal layer, a bit line metal layer on the barrier layer, a capping layer on the bit line metal layer, a hard mask on the capping layer, a carbon hard mask on the hard mask, an anti-reflective coating (ARC) on the carbon hard mask, and a patterned spacer layer on the ARC. The ARC, the carbon hard mask, and the hard mask are etched to expose the capping layer. The capping layer, the bit line metal layer, the barrier layer, the barrier metal layer, and the polysilicon are etched to form a substrate having a plurality of DRAM film stacks. BRIEF DESCRIPTION OF THE DRAWINGS

[0008] Thus, a more particular description of the disclosure briefly summarized above may be obtained by reference to embodiments, some of which are illustrated in the accompanying drawings, in order to understand in detail the above-mentioned features of the disclosure. It should be noted, however, that the drawings illustrate only typical embodiments of the disclosure and, therefore, should not be considered limiting of the scope of the disclosure, as the disclosure may admit to other equally effective embodiments. The embodiments described herein are illustrated by way of example and not limitation in the figures of the accompanying drawings, in which like reference numerals indicate similar elements.

[0009] Figure 1 A circuit diagram illustrating a dynamic memory cell in a DRAM memory having improved properties according to one or more embodiments of the present disclosure;

[0010] Figure 2 illustrates a schematic diagram of a membrane stack according to one or more embodiments;

[0011] Figure 3 illustrates a flow chart of a method for forming a film stack according to one or more embodiments;

[0012] Figure 4 A flowchart illustrating a method for forming an electronic component according to one or more embodiments; and

[0013] FIG. 5A to FIG. 5J A schematic diagram illustrating a process for forming an electronic component according to one or more embodiments of the present disclosure. DETAILED DESCRIPTION

[0014] Before describing several exemplary embodiments of the present disclosure, it should be understood that the present disclosure is not limited to the details of construction or process steps set forth in the following description. The present disclosure is capable of other embodiments and can be practiced or carried out in various ways.

[0015] Bitline stacks and methods for forming bitline stacks having reduced resistance are provided. One or more embodiments of the present disclosure advantageously address the problem of resistivity reduction despite the need to shrink nodes. In some embodiments, the resistivity of the bitline is reduced by providing a cleaner interface with the existing bitline metal and by changing the bitline metal. Some embodiments of the present disclosure advantageously provide one or more of the following: flexibility in selecting the bitline metal; temperature flexibility for silicon nitride hard mask deposition; ensuring a clean metal / dielectric interface resulting in lower resistivity; or minimizing or eliminating the risk of contaminating the high temperature silicon nitride hard mask deposition chamber with the new bitline metal.

[0016] Some embodiments of the present disclosure provide low temperature deposition methods that use a capping layer to prevent the surface of the bit line metal from becoming rough when the selected metal exhibits grain growth characteristics. In some embodiments, a high density non-porous film is used to act as a good diffusion barrier at high temperatures. Some embodiments provide a dielectric material, such as silicon nitride (SiN) or silicon carbonitride (SiCN), to act as a capping film so as to minimize or eliminate the adverse effects on the RC time constant by acting as a good diffusion barrier for the bit line metal and SiN hard mask. The RC time constant is the time associated with charging a capacitor to a certain percentage of full charge or discharging a capacitor to a small fraction of the initial voltage through a resistor. The RC time constant is equal to the product of the circuit resistance and the circuit capacitance. Some embodiments of the present disclosure advantageously provide a deposition process at low temperatures (e.g., <500° C.). Some embodiments provide a deposition process compatible with the lower bit line metal to minimize or eliminate surface reactions during film deposition.

[0017] One or more embodiments of the present disclosure generally provide a structure including one or more low-resistivity features formed of a thin film refractory metal (e.g., tungsten) that can be implemented as a bitline structure and / or a gate stack. Some embodiments include methods for forming a bitline stack. By way of example, a bitline stack structure formed according to an embodiment of the present disclosure can be a memory-type semiconductor device, such as a DRAM-type integrated circuit.

[0018] Figure 1 A schematic circuit diagram illustrating a one transistor one capacitor cell such as may be used in a DRAM memory is shown. Figure 1The memory cell depicted in includes a storage capacitor 110 and a select transistor 120. The select transistor 120 is formed as a field effect transistor and includes a first source / drain electrode 121 and a second source / drain electrode 123, with an active region 122 arranged therebetween. Above the active region 122 is a gate insulating layer or dielectric layer 124 (typically a thermally grown oxide) and a gate electrode / metal 125 (referred to as a word line in memory elements), which together act as a plate capacitor and can affect the charge density in the active region 122 so as to form or block a current conduction path between the first source / drain electrode 121 and the second source / drain electrode 123.

[0019] The second source / drain electrode 123 of the select transistor 120 is connected to the first electrode 111 of the storage capacitor 110 via the metal wiring 114. The second electrode 112 of the storage capacitor 110 is in turn connected to a capacitor plate, which may be common to the storage capacitors of the DRAM memory cell arrangement. The second electrode 112 of the storage capacitor 110 may be electrically grounded via the metal wiring 115. The first source / drain electrode 121 of the select transistor 120 is additionally connected to the bit line 116 so that the information stored in the storage capacitor 110 in the form of charge can be written and read. The write or read operation is controlled via the word line 117 or the gate electrode 125 of the select transistor 120 and the bit line 116 connected to the first source / drain electrode 121. The write or read operation occurs by applying a voltage to create a current conduction channel in the active region 122 between the first source / drain electrode 121 and the second source / drain electrode 123.

[0020] Figure 2 A portion of a memory element 200 is shown in accordance with one or more embodiments of the present disclosure. Figure 3 Diagram used to form Figure 2 An exemplary processing method 300 of the illustrated memory element 200. The skilled person will recognize that the film stack illustrated in the figure is an exemplary portion (the bit line portion) of a memory element.

[0021] refer to Figure 2 and Figure 3 , formation of memory element 200 includes providing a substrate 210 on which film stack 205 may be formed at operation 310. As used in this specification and claims, the term "providing" means making the substrate available for processing (eg, positioned in a processing chamber).

[0022] As used in this specification and claims, the term "substrate" refers to a surface, or a portion of a surface, on which a process acts. It should also be understood by those skilled in the art that reference to a substrate may refer to only a portion of a substrate unless the context clearly indicates otherwise. In addition, references to deposition on a substrate may mean a bare substrate and a substrate having one or more films or features deposited or formed thereon.

[0023] As used herein, "substrate" refers to any substrate or material surface formed on a substrate on which film processing is performed during a manufacturing process. For example, depending on the application, the substrate surface on which processing may be performed includes materials such as silicon, silicon oxide, strained silicon, silicon on insulator (SOI), carbon-doped silicon oxide, amorphous silicon, doped silicon, germanium, gallium arsenide, glass, sapphire, and any other material such as metals, metal nitrides, metal alloys and other conductive materials. Substrates include, but are not limited to, semiconductor wafers. The substrate may be exposed to a pretreatment process to grind, etch, reduce, oxidize, hydroxylate, anneal and / or bake the substrate surface. In addition to performing film processing directly on the surface of the substrate itself, in the present disclosure, any of the disclosed film processing steps may also be performed on an underlying layer (as disclosed in more detail below) formed on the substrate, and the term "substrate surface" is intended to include the underlying layer, as indicated by the context. Thus, for example, where a film / layer or portion of a film / layer has been deposited on a substrate surface, the exposed surface of the most recently deposited film / layer becomes the substrate surface.

[0024] In some embodiments, the provided substrate 210 includes a film stack 205 including a polysilicon layer 215 and a bitline metal layer 240. In some embodiments, the provided substrate 210 includes a polysilicon layer 215 and the bitline metal layer 240 is formed as part of the method 300.

[0025] In some embodiments, substrate 210 includes an oxide layer (not shown) on a silicon wafer. In some embodiments, the oxide layer is a native oxide formed on the silicon wafer. In some embodiments, the oxide layer is intentionally formed on the silicon wafer and has a thickness greater than the thickness of the native oxide film. The oxide layer may be formed by any suitable technique known to a skilled artisan, including but not limited to thermal oxidation, plasma oxidation, and exposure to atmospheric conditions.

[0026] In some embodiments, the substrate 210 provided in operation 310 further includes a barrier metal layer 220 (also referred to as a conductive layer) on the polysilicon layer 215. The barrier metal layer 220 can be any suitable conductive material. In some embodiments, the barrier metal layer 220 includes one or more of titanium (Ti), tantalum (Ta), titanium silicide (TiSi), or tantalum silicide (TaSi). In some embodiments, the barrier metal layer 220 includes titanium. In some embodiments, the barrier metal layer 220 consists essentially of titanium. In some embodiments, the barrier metal layer 220 includes tantalum or consists essentially of tantalum. In some embodiments, the barrier metal layer 220 includes titanium silicide or consists essentially of titanium silicide. In some embodiments, the barrier metal layer 220 includes tantalum silicide or consists essentially of tantalum silicide. As used in this manner, the term "consisting essentially of" means that the subject film includes greater than or equal to about 95%, 98%, 99%, or 99.9% of the element or composition in terms of atoms. For example, a barrier metal layer 220 consisting essentially of titanium has a film of greater than or equal to approximately 95%, 98%, 99%, or 99.5% titanium when deposited.

[0027] In some embodiments, the substrate 210 provided in operation 310 further includes a barrier layer 230 on the conductive layer (barrier metal layer 220). The barrier layer 230 may be formed between the barrier metal layer 220 and the bit line metal layer 240. In some embodiments, the method 300 includes an operation prior to operation 310 in which the bit line metal layer 240 is formed on the barrier layer 230. The barrier layer 230 may be any suitable barrier layer material. In some embodiments, the barrier layer 230 includes one or more of a nitride or an oxide of the barrier metal layer 220. In some embodiments, the barrier layer 230 consists substantially of a nitride of the barrier metal layer 220. For example, a barrier layer 230 consisting essentially of titanium nitride means that when deposited, the sum of titanium and nitrogen atoms in the film constitutes greater than or equal to about 95%, 98%, 99%, or 99.5% (by atom) of the barrier layer 230.

[0028] In some embodiments, the barrier metal layer 220 includes titanium (Ti) and the barrier layer 230 includes titanium nitride (TiN). In some embodiments, the barrier metal layer 220 consists essentially of titanium and the barrier layer 230 consists essentially of titanium nitride. In one or more embodiments, the barrier metal layer 220 includes a metal selected from one or more of the following: cobalt (Co), copper (Cu), nickel (Ni), ruthenium (Ru), manganese (Mn), silver (Ag), gold (Au), platinum (Pt), iron (Fe), molybdenum (Mo), rhodium (Rh), titanium (Ti), tantalum (Ta), silicon (Si), or tungsten (W). In one or more specific embodiments, the barrier metal layer 220 (conductive material) includes one or more of titanium (Ti), copper (Cu), cobalt (Co), tungsten (W), or ruthenium (Ru). In some embodiments, the barrier layer 230 includes a nitride, an oxynitride, a carbonitride, or an oxycarbonitride of the metal in the barrier metal layer 220. In some embodiments, barrier metal layer 220 comprises (or consists essentially of) tantalum or tantalum silicide, and barrier layer 230 comprises (or consists essentially of tantalum nitride). In some embodiments, barrier metal layer 220 comprises (or consists essentially of) titanium or titanium silicide, and barrier layer 230 comprises (or consists essentially of) titanium nitride.

[0029] In some embodiments, the bit line metal layer 240 is included in the substrate provided in operation 310 of the method 300. The bit line metal layer 240 may be deposited by any suitable technique known to a skilled person. In some embodiments, the bit line metal layer 240 includes one or more of tungsten (W), ruthenium (Ru), iridium (Ir), platinum (Pt), rhodium (Rh), or molybdenum (Mo). In some specific embodiments, the bit line metal layer 240 includes or consists essentially of one or more of ruthenium or tungsten.

[0030] The thickness of the bit line metal layer 240 can vary. In some embodiments, the bit line metal layer 240 has a thickness of about to about in the range of, or about to about in the range of, or about to about in the range of, or about to about The thickness is in the range of

[0031] The bitline metal layer 240 may be deposited by any suitable technique known to skilled artisans. In some embodiments, the bitline metal layer 240 is deposited by one or more of chemical vapor deposition, atomic layer deposition, or physical vapor deposition.

[0032] At operation 320, a capping layer 250 is formed on the bit line metal layer 240. The capping layer 250 of some embodiments is deposited at a lower temperature than that typically used to form a subsequent hard mask 260 layer. Without being bound by any particular theory of operation, it is believed that the lower deposition temperature minimizes diffusion of capping layer 250 elements into the bit line metal layer 240. In some embodiments, it is believed that the low temperature deposition of the capping layer 250 minimizes grain growth at the bit line metal layer 240 interface and minimizes the effect of grain size and roughness on the resistivity of the resulting bit line metal layer 240.

[0033] The capping layer 250 may be deposited by any suitable technique known to a skilled artisan. In some embodiments, the capping layer 250 is deposited by one or more of chemical vapor deposition or atomic layer deposition.

[0034] The capping layer 250 of some embodiments comprises the same compound as the subsequent hard mask 260. In some embodiments, the capping layer 250 comprises one or more of silicon nitride, silicon carbonitride, or silicon carbide. In some embodiments, the capping layer 250 consists essentially of silicon nitride. In some embodiments, the capping layer 250 consists essentially of silicon carbonitride. In some embodiments, the capping layer 250 consists essentially of silicon carbide.

[0035] The thickness of the cover layer 250 may vary to minimize the effects of high temperature formation of the hard mask 260. In some embodiments, the cover layer 250 has a thickness of about to about The thickness is in the range of

[0036] The deposition temperature of the capping layer 250 can be controlled, for example, to preserve the thermal budget of the formed element. In some embodiments, the capping layer 250 is formed at a temperature less than or equal to about 500° C., or about 450° C., or about 400° C., or about 350° C., or about 300° C. In some embodiments, the capping layer 250 is formed at a temperature in the range of about 350° C. to about 550° C., or in the range of about 400° C. to about 500° C.

[0037] At operation 330, a hard mask 260 is formed on the capping layer 250. The hard mask 260 of some embodiments is formed in a furnace at a temperature greater than about 600°C, about 650°C, about 700°C, or about 750°C.

[0038] In some embodiments, hardmask 260 comprises the same composition as capping layer 250. In some embodiments, capping layer 250 and hardmask 260 comprise or consist essentially of silicon nitride, silicon oxide, or silicon nitride. In some embodiments, hardmask 260 has a different density than capping layer 250. In some embodiments, hardmask 260 has a different porosity than hardmask 260. In some embodiments, hardmask 260 has a different deposition temperature than capping layer 250.

[0039] In some embodiments, the bit line metal layer 240 includes or consists essentially of tungsten, and one or more of the capping layer 250 or the hard mask 260 includes or consists essentially of silicon nitride. In some embodiments, the bit line metal layer 240 includes or consists essentially of ruthenium, and one or more of the capping layer 250 or the hard mask 260 includes or consists essentially of silicon oxide or silicon nitride.

[0040] In some embodiments, elements of the hard mask 260 are substantially prevented from migrating into the bit line metal layer 240. For example, if the hard mask 260 includes silicon and nitrogen atoms, the silicon or nitrogen atoms are substantially prevented from migrating into the bit line metal layer 240. As used in this manner, the term "substantially prevented" means less than or equal to about 10% or 5% of the elements of the hard mask 260 migrate into the bit line metal layer 260 via the capping layer 250.

[0041] Additional embodiments of the present disclosure are directed to methods of forming a memory element. Skilled persons will recognize that the described methods may form a portion of a memory element (eg, a bit line), which may be part of a complete memory element. Figure 4 A process flow of an exemplary method 400 for forming a memory element is shown. FIG. 5A to FIG. 5J Shown in accordance with Figure 4 The method 400 forms an electronic component 500 (see Figure 5J ) is a schematic diagram of various layers and films during the process. A skilled person will recognize that method 400 can start with various configurations of substrates and films / layers thereon. For example, method 400 can FIG. 5B to FIG. 5I Starting with the configuration shown in any of Figure 5J The electronic component 500 shown in FIG. 4 ends. The described films / layers may be used in conjunction with Figure 2 The films / layers described are the same and the reference numerals used to describe the films / layers are the same as those used in the examples of FIG. Figure 2 The component numbers of the embodiments are consistent with those of the embodiments.

[0042] At operation 410, a substrate 210 is provided for processing. The substrate 210 has a film stack 204 formed thereon, such as Figure 5A The membrane stack 204 includes Figure 2The film stack 205 shown in FIG. 2 , together with additional layers / films formed thereon, such as Figure 5A . In some embodiments, film stack 204 includes a polysilicon layer 215 on (or directly on) substrate 210. As used in this manner, the term "directly on" means that the subject film is formed without intervening layers or films. The skilled artisan will recognize that any of the films / layers described as "on another film / layer" may be "directly on" another film / layer or may have intervening layers.

[0043] The optional barrier metal layer 220 is on the polysilicon layer 215 or directly on the polysilicon layer 215. In some embodiments, there is no barrier metal layer 220 in the film stack 204. The optional barrier layer 230 can be on the optional barrier metal layer 220, directly on the optional barrier metal layer 220, or directly on the polysilicon layer 215. The bit line metal layer 240 is on the optional barrier layer 230 or directly on the optional barrier layer 230, or directly on the barrier metal layer 220, or directly on the polysilicon layer 215. The capping layer 250 is on the bit line metal layer 240 or directly on the bit line metal layer 240. The hard mask 260 is on the capping layer 250 or directly on the capping layer 250.

[0044] The film stack 204 of some embodiments further includes one or more of a carbon hard mask 270, an anti-reflective coating (ARC) 280, or a spacer layer 290. In some embodiments, the carbon hard mask 270 is formed on or directly on the hard mask 260. The carbon hard mask 270 can be any suitable carbon-containing material that can be used as a hard mask for device patterning. In some embodiments, the carbon hard mask 270 includes a high-density carbon film.

[0045] In some embodiments, the carbon hard mask 270 includes a diamond-like carbon material. For diamond-like carbon materials, the bulk properties sought may include, but are not limited to, high density and modulus (e.g., higher sp3 content, more diamond-like) and low stress (e.g., <-500 MPa). Some embodiments of diamond-like carbon films have one or more of high density (e.g., >1.8 g / cc), high modulus (e.g., >150 GPa), and / or low stress (e.g., <-500 MPa). In some embodiments, the carbon hard mask 270 has low stress and high sp3 carbon content.

[0046] The carbon hard mask 270 may be formed by any suitable process known to a skilled artisan. The carbon hard mask 270 may be formed at any suitable temperature depending on, for example, the thermal budget of the device being formed, the process used for formation, and / or the reactive species used for film formation.

[0047] In some embodiments, an anti-reflective coating (ARC) 280 is formed on or directly on the carbon hard mask 270. In some embodiments, the ARC 280 is formed directly on the hard mask 260 without an intervening carbon hard mask 270. The anti-reflective coating 280 of some embodiments includes one or more of a silicon ARC (SiARC), a bottom ARC (BARC), or a dielectric ARC (DARC). In some embodiments, the ARC 280 and the carbon hard mask 270 are reversed such that the ARC 280 is directly on the hard mask 260 and the carbon hard mask 270 is directly on the ARC 280.

[0048] ARC 280 may be formed by any suitable process known to those skilled in the art. In some embodiments, ARC 280 is deposited using one of a number of deposition techniques, such as, but not limited to, chemical vapor deposition (CVD), physical vapor deposition (PVD), molecular beam epitaxy (MBE), metalorganic chemical vapor deposition (MOCVD), atomic layer deposition (ALD), spin coating, or other insulating deposition techniques known to those skilled in the art of microelectronic device fabrication.

[0049] The patterned spacer layer 290 is on the ARC 280 or directly on the ARC 280. In some embodiments, the patterned spacer layer 290 is directly on the carbon hard mask 270, with or without the ARC 280 below the carbon hard mask 270. The pattern of the patterned spacer layer 290 can be formed by any suitable patterning technique known to a skilled person, including but not limited to photolithography. The patterned spacer layer 290 has a pattern that exposes a portion of the top surface 282 of the ARC 280 or the top surface 272 of the carbon hard mask 270.

[0050] At operation 420, the film stack 204 is etched to expose the capping layer 250, such as Figure 5D Operation 420 may include any number of processes sufficient to etch ARC 280, carbon hard mask 270, and hard mask 260 to expose capping layer 250. A skilled person will recognize that Figure 4 The process shown represents only one possible process and series of operations.

[0051] In the illustrated embodiment, at operation 422, the pattern of the patterned spacer layer 290 is transferred to the ARC 280 to form a patterned ARC 281, as shown in FIG. Figure 5B . The pattern may be transferred to the ARC 280 by any suitable technique known to the skilled artisan, including but not limited to isotropic etching. The pattern of the patterned ARC 281 is substantially the same as the pattern of the patterned spacer layer 290, and exposes the top surface 272 of the carbon hard mask 270. As used in this manner, as will be understood by the skilled artisan, the term "substantially the same" means that the transferred pattern is aligned with the source pattern and slight imperfections are allowed to be transferred. Referring to a pattern as being "the same" as the previous pattern also recognizes that small variations and imperfections are expected and are within the scope of the present disclosure. In some embodiments, the ARC 280 is etched through the patterned spacer layer 290 to form the patterned ARC 281.

[0052] like Figure 5B As shown in , the height (thickness) of the patterned spacer layer 290 is reduced to form a reduced patterned spacer layer 291. The reduction in thickness of the patterned spacer layer can occur simultaneously with the pattern transfer, or in a separate process. In some embodiments, the patterned spacer layer 290 is etched simultaneously with the ARC 280 to form a reduced patterned spacer layer 291 and a patterned ARC 281. In some embodiments, the patterned spacer layer 290 is completely removed during the pattern transfer process.

[0053] In operation 424, as Figure 5C As shown in FIG. 2 , the pattern of the patterned ARC 281 is transferred into the carbon hard mask 270 to form a patterned carbon hard mask 271. The pattern of the patterned carbon hard mask 271 is substantially the same as the pattern of the patterned ARC 281, and exposes the top surface 262 of the hard mask 260. The pattern may be transferred to the carbon hard mask 270 by any suitable technique known to a skilled person, including but not limited to isotropic etching, selective etching, or anisotropic etching.

[0054] In the illustrated process, the reduced patterned spacer layer 291 is removed and the pattern is transferred into the carbon hard mask 270. The removal of the reduced patterned spacer layer 291 can occur in the same process as the pattern transfer or in a different process.

[0055] In operation 426, if Figure 5DAs shown in FIG, the pattern of the patterned carbon hard mask 271 is transferred into the hard mask 260 to form the patterned hard mask 261 and expose the top surface 252 of the capping layer 250. The pattern can be transferred from the patterned carbon hard mask 271 to the patterned hard mask 261 by any suitable technique known to a skilled person, including but not limited to isotropic etching, selective etching, or anisotropic etching.

[0056] exist Figure 5D , the thickness of the patterned carbon hard mask 271 is reduced to form a reduced patterned carbon hard mask 273. In some embodiments, reducing the thickness of the patterned carbon hard mask 271 occurs simultaneously with transferring the pattern to the hard mask 270. In some embodiments, reducing the thickness of the patterned carbon hard mask 271 occurs in a different process than pattern transfer.

[0057] At optional operation 430, the width W1 of the individual mandrels 265 of the patterned hard mask 261 is reduced to a smaller width W2. Figure 5E As shown in FIG, the trimmed mandrel 266 has a width W2 that is smaller than the width W1 of the reduced patterned carbon hard mask 272. The width of the mandrel 265 may be trimmed by any suitable trimming process known to a skilled artisan, including but not limited to plasma exposure.

[0058] At operation 435, as Fig. 5F As shown in , the reduced patterned carbon hard mask 272 is removed from the trimmed patterned hard mask 263 or from the patterned hard mask 261 (when the trimming operation 430 is omitted). The reduced patterned carbon hard mask 272 may be removed by any suitable process known to a skilled person, including but not limited to selective etching.

[0059] At operation 440, a substrate 210 having a plurality of DRAM film stacks 205 is formed, such as Figure 5J To reach the substrate 210 having the plurality of DRAM film stacks 205, the capping layer 250, the bit line metal layer 240, the barrier layer 230, the barrier metal layer 220 and the polysilicon layer 215 are etched.

[0060] At operation 442, if Figure 5G As shown in FIG. 2 , the pattern of the trimmed patterned hard mask 263 is transferred to the capping layer 250 and the bit line metal layer 240 to form a patterned capping layer 251 and a patterned bit line metal layer 241, respectively. Figure 5D If the mandrels 265 in the embodiment are not trimmed, the pattern of the patterned hard mask 261 is transferred to the capping layer 250 and the bit line metal layer 240. The difference in the process lies in the width of the patterned mandrels.

[0061] The illustrated embodiment shows that the pattern is transferred to the capping layer 250 and the bit line metal layer 240 at the same time. The method 400 shows that the pattern transfer is divided into operations 442 and 444. In some embodiments, as in operation 442, the pattern is transferred to the capping layer 250 to form a patterned capping layer 251 and expose the top surface (not shown) of the bit line metal layer 240. As in operation 444, the pattern of the patterned capping layer 251 can then be transferred to the bit line metal layer 240 to form a patterned bit line metal layer 241.

[0062] exist Figure 5G , the thickness of the patterned hard mask 263 is reduced to form a reduced patterned hard mask 267. In some embodiments, reducing the thickness of the patterned hard mask 263 occurs simultaneously with transferring the pattern to the capping layer 250 and / or the bit line metal layer 240. In some embodiments, reducing the thickness of the patterned hard mask 263 occurs in a different process than transferring the pattern to the capping layer 250 or the bit line metal layer 240.

[0063] At operation 446, the pattern of the patterned bit line metal layer 241 is transferred to the barrier layer 230 and the barrier metal layer 220 to form the patterned barrier layer 231 and the patterned metal layer 221. The pattern may be transferred to the barrier layer 230 and the barrier metal layer 220 simultaneously or in different processes. Figure 4 The method flow chart shows a single operation 446 for transferring a pattern to the barrier layer 230 and the barrier metal layer 220. The schematic diagrams shown show different processes. Figure 5H In the embodiment, the pattern is transferred to the barrier layer 231 to form a patterned barrier layer 231 and expose the top surface 222 of the barrier metal layer 220. Fig.5I In the embodiment, the pattern is transferred to the barrier metal layer 220 to form a patterned metal layer 221 and expose the top surface 217 of the polysilicon layer 215. The pattern transfer to the barrier layer 230 and the barrier metal layer 220 may be performed by any suitable technique known to those skilled in the art, including but not limited to selective etching.

[0064] In operation 448, if Figure 5J As shown in FIG. 2 , the pattern of the patterned metal layer 221 is transferred to the polysilicon layer 215 to form a patterned polysilicon layer 216. The resulting electronic device 500 has a similar Figure 2 205. In embodiments where some of the layers are omitted, the multiple film stacks will also omit the same layers. Transferring the pattern into the polysilicon layer may be performed by any suitable technique, including but not limited to selective etching.

[0065] In the context of describing the materials and methods discussed herein, (especially in the context of the following claims), the use of the terms "a" and "an" and "the" and similar indications should be interpreted as covering both the singular and the plural, unless otherwise indicated herein or clearly contradicted by the context. Unless otherwise indicated herein, the enumeration of value ranges herein is intended only to be used as a shorthand method of individually indicating each individual value within the range, and each individual value is incorporated into the specification as if it were individually described herein. All methods described herein can be performed in any suitable order, unless otherwise indicated herein or clearly contradicted by the context. Unless otherwise required, the use of any and all examples or illustrative language (e.g., "such as") provided herein is intended only to better illustrate the materials and methods, and is not intended to limit the scope. No language in the specification should be interpreted as indicating that any unrequired element is essential to the practice of the disclosed materials and methods.

[0066] References throughout this specification to "one embodiment," "certain embodiments," "one or more embodiments," or "an embodiment" mean that a particular feature, structure, material, or characteristic described in connection with the embodiment is included in at least one embodiment of the present disclosure. Thus, phrases such as "in one or more embodiments," "certain embodiments," "in an embodiment," or "in an embodiment" appearing in various places throughout this specification are not necessarily referring to the same embodiment of the present disclosure. Additionally, particular features, structures, materials, or characteristics may be combined in any suitable manner in one or more embodiments.

[0067] Although the disclosure herein has been described with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of the disclosure. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the disclosure without departing from the spirit and scope of the disclosure. Therefore, it is contemplated that the disclosure includes modifications and variations within the scope of the claims and their equivalents.

Claims

1. A method for forming a memory element, the method comprising the following steps: Providing a substrate, the substrate having a polysilicon layer, a barrier metal layer on the polysilicon layer, a barrier layer on the barrier metal layer, and a bit line metal layer on the barrier layer; forming a capping layer on the bit line metal layer at a temperature less than or equal to 500° C.; and forming a hard mask on the cover layer at a temperature greater than or equal to 650° C., wherein elements of the hard mask are prevented from migrating into the bit line metal layer, Wherein the cover layer and the hard mask comprise the same composition.

2. The method of claim 1, wherein the capping layer comprises one or more of silicon nitride or silicon carbonitride.

3. The method of claim 2, wherein the covering layer has to The thickness is in the range of The method of claim 3 , wherein the capping layer is deposited by a chemical vapor deposition or atomic layer deposition process. The method of claim 4 , wherein the hard mask comprises silicon nitride.

6. The method of claim 5, wherein the hard mask is deposited using a furnace at a temperature greater than or equal to 650°C.

7. The method of claim 1, further comprising the steps of: forming a carbon hard mask on the hard mask; forming an ARC (anti-reflective coating) on ​​the carbon hard mask; forming a patterned spacer layer on the ARC; etching the ARC, carbon hard mask, and hard mask to expose the capping layer; and The capping layer, the bit line metal layer, the barrier layer, the barrier metal layer and the polysilicon layer are etched to form a substrate having a plurality of DRAM film stacks.

8. The method of claim 7, wherein etching the ARC, carbon hard mask, and hard mask comprises: transferring the pattern of the patterned spacer layer into the ARC, reducing the thickness of the patterned spacer layer and forming a patterned ARC; transferring the pattern of the patterned ARC into the carbon hard mask, removing the patterned spacer layer and forming a patterned carbon hard mask; transferring the pattern of the patterned carbon hard mask into the hard mask to remove the ARC and reduce the thickness of the patterned carbon hard mask; trimming a width of the patterned hard mask; and The carbon hard mask is removed from the patterned hard mask.

9. The method of claim 8, wherein etching the capping layer, the bit line metal layer, the barrier layer, the barrier metal layer, and the polysilicon layer comprises: transferring the pattern of the patterned hard mask into the cover layer to form a patterned cover layer; transferring the pattern of the patterned capping layer into the bit line metal layer to form a patterned bit line metal layer; transferring the pattern of the patterned bit line metal layer into the barrier metal layer to form a patterned barrier metal layer; and The pattern of the patterned barrier metal layer is transferred into a polysilicon layer to form a patterned polysilicon layer on the substrate.

10. The method of claim 9, wherein: The bit line metal layer includes one or more of tungsten (W), ruthenium (Ru), iridium (Ir) or molybdenum (Mo), and has to Thickness in the range of The capping layer includes silicon nitride (SiN) having to thickness in the range of; and The hard mask includes silicon nitride (SiN).

11. A memory element formed by the method of claim 1, comprising: A substrate having at least one film stack thereon, the film stack comprising: a polysilicon layer on the substrate; a barrier metal layer on the polysilicon layer; a barrier layer on the barrier metal layer; a bit line metal layer on the barrier layer; a capping layer on the bit line metal layer; A hard mask on the overlay.

12. The memory device of claim 11, wherein the barrier metal layer comprises one or more of titanium (Ti), tantalum (Ta), titanium silicide (TiSi), or tantalum silicide (TaSi), and the barrier layer comprises titanium nitride (TiN).

13. The memory element of claim 11, wherein the bit line metal layer comprises one or more of tungsten (W), ruthenium (Ru), iridium (Ir), or molybdenum (Mo), platinum (Pt), or rhodium (Rh).

14. The memory element of claim 11, wherein the capping layer comprises silicon nitride, silicon carbonitride, or silicon carbide.

15. The memory element of claim 14, wherein the cover layer has to The thickness is in the range of 16. The memory element of claim 15, wherein the bit line metal layer has to The thickness is in the range of 17. The memory element of claim 11, wherein the hard mask comprises silicon nitride (SiN).

18. The memory element of claim 17, wherein the capping layer comprises silicon nitride, the capping layer having a different density and / or porosity than the hard mask.

Citation Information

Patent Citations

  • Bit line gate structure of dynamic random access memory (DRAM) and forming method thereof

    US20180190662A1

  • Semiconductor stack having a dielectric sidewall for prevention of oxidation of tungsten in tungsten capped poly-silicon gate electrodes

    US5796151A