Method for depositing chromium or chromium alloy layer and electroplating device

By dissolving solid trivalent chromium formate in an aqueous deposition bath, combining trivalent chromium ions and formate ions, the anion accumulation problem is solved, and the deposition of high wear resistance and stability is achieved, thereby improving the sustainability of the chromium deposition process Sex and efficiency.

CN113166961BActive Publication Date: 2024-11-19ATOTECH DEUT GMBH & CO KG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN201980081806.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2018-12-11
Filing Date
2019-12-11
Publication Date
2024-11-19
Estimated Expiration
2039-12-11

AI Technical Summary

Technical Problem

In the existing chromium deposition method based on trivalent chromium, anion accumulation leads to precipitate formation, affecting the roughness of the chromium layer and the stability of the deposition process. The existing method is difficult to avoid anion accumulation, limiting the lifetime of the deposition bath and the chromium layer. wear resistance.

Method used

The concentration of trivalent chromium ions is increased by dissolving solid trivalent chromium formate in the aqueous deposition bath in the range of pH 4.1 to 6.9. , avoid anion accumulation and use expensive membrane structures.

Benefits of technology

Chromium deposition without the influence of anion accumulation is achieved for a long time, and a functional chromium layer with high wear resistance and desired thickness is obtained, which improves the stability and current efficiency of the aqueous deposition bath.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113166961B_ABST
    Figure CN113166961B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for depositing a chromium or chromium alloy layer on at least one substrate, the method comprising the steps of: (a) providing an aqueous deposition bath having a pH in the range of 4.1 to 6.9, the bath comprising: -trivalent chromium ions, -formate ions, and -optionally sulfate ions, (b) providing at least one substrate and at least one anode, (c) immersing the at least one substrate in the aqueous deposition bath and applying an electric current so that the chromium or chromium alloy layer is deposited on the substrate, the substrate being the cathode, wherein, if during or after step (c), the trivalent chromium ions have a concentration below a target concentration of trivalent chromium ions, then (d) adding dissolved trivalent chromium formate to the aqueous deposition bath so that the trivalent chromium ions are present in a higher concentration than before step (d), but with the proviso that -solid trivalent chromium formate is dissolved in a separated partial volume taken from the aqueous deposition bath to obtain the dissolved trivalent chromium formate for step (d).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method and a specially designed electroplating device for depositing a chromium or chromium alloy layer on at least one substrate. Background Art

[0002] Functional chromium layers generally have a much higher average layer thickness (at least 1 μm to several hundred micrometers) than decorative chromium layers (generally below 1 μm) and are characterized by very good hardness and wear resistance.

[0003] Functional chromium layers obtained from deposition baths containing hexavalent chromium are known in the art and are an accepted standard.

[0004] In recent decades, chromium deposition methods that rely on hexavalent chromium have been increasingly replaced by deposition methods that rely on trivalent chromium. Such trivalent chromium-based methods are healthier and more environmentally friendly.

[0005] However, it has been observed that trivalent chromium-based processes often result in the accumulation of inorganic counter anions such as sulfate or chloride. This occurs due to the need to replenish the consumed trivalent chromium, usually from common commercially available trivalent chromium sources. Very common trivalent chromium sources are chromium (III) sulfate and chromium (III) chloride.

[0006] This accumulation is a fundamental problem. In contrast to hexavalent chromium deposition baths using chromium trioxide, which cannot cause undesirable accumulation of anions and can therefore be operated continuously, the life of trivalent chromium deposition baths is naturally limited by this accumulation. If the interfering maximum concentration of anions (e.g., sulfate) is reached or even exceeded, usually undesirable precipitation can be seen, blocking pipes and pumps. In addition, the entire deposition process is adversely affected, resulting in (for example) undesirable roughness of the deposited chromium layer. In addition, the tendency to form precipitates in each deposition bath increases significantly. Typically, this precipitate is covering the anode, which promotes the undesirable anode formation of hexavalent chromium. Continuously regenerating this bath and artificially reducing the concentration of the anions is very economically inefficient. In some cases, even toxic and / or dangerous degradation products are formed. For example, if trivalent chromium chloride is used for supplementation, the chloride ion accumulation is even as high as the concentration of toxic chlorine gas. Therefore, it is highly desirable to have a deposition method that can be operated for a long time like a deposition method that relies on hexavalent chromium.

[0007] In the prior art, it has been described that the accumulation of anions can be avoided by using volatile anions, which are usually organic anions.

[0008] For example, WO 2015 / 110627 A1 relates to an electroplating bath for depositing chromium and to a method for depositing chromium on a substrate using the electroplating bath. WO'627 also discloses electrolytically consumable anions that will not accumulate in the electrolyte. Among these anions, formate ions, acetate ions, propionate ions, glycolate ions, oxalate ions, carbonate ions, citrate ions and combinations thereof are disclosed. WO'627 also indicates the use of a membrane to limit the accumulation of undesirable anions throughout the electrolyte.

[0009] However, own experiments have shown that these anions generally have the disadvantage of too low a solubility and, therefore, cannot be practically used in recognized deposition methods that rely on trivalent chromium or do not coordinate well with the complexing agent in the respective deposition bath. It is generally preferred that the trivalent chromium source and the anion of the complexing agent in the deposition bath are identical. Very common complexing agents are weak carboxylic acids. With regard to membranes, own experiments have shown that membranes are very expensive and decompose rapidly at high current densities.

[0010] US 4,054,494 discloses a method for maintaining a trivalent chromium electroplating bath. However, this disclosure is not applicable to functional chromium deposits deposited in a weakly acidic pH range.

[0011] Purpose of the invention

[0012] The object of the present invention is therefore to overcome the above mentioned disadvantages. In particular, the object of the present invention is to provide a method for depositing chromium or chromium alloy layers based on trivalent chromium ions, which method completely prevents the accumulation of ultimately interfering anions (or even completely avoids these anions), which method can be operated for a longer time without intensive regeneration, most preferably as long as a deposition bath of hexavalent chromium is used, and provides an excellent functional chromium deposit with the desired thickness and wear resistance. For this purpose, it is desirable not to use a membrane. Summary of the invention

[0013] The object is solved by a method for depositing a chromium or chromium alloy layer on at least one substrate, the method comprising the following steps:

[0014] (a) providing an aqueous deposition bath having a pH in the range of 4.1 to 6.9, said bath comprising:

[0015] - trivalent chromium ions,

[0016] -formate ion, and

[0017] - optionally sulfate ions,

[0018] (b) providing at least one substrate and at least one anode,

[0019] (c) immersing said at least one substrate in said aqueous deposition bath and applying an electric current so that a chromium or chromium alloy layer is deposited on said substrate, said substrate being a cathode,

[0020] Wherein, if during or after step (c), the trivalent chromium ions have a concentration lower than the target concentration of trivalent chromium ions, then

[0021] (d) adding dissolved trivalent chromium formate to the aqueous deposition bath such that trivalent chromium ions are present at a higher concentration than before step (d),

[0022] But the prerequisite is

[0023] - dissolving solid trivalent chromium formate in the separated partial volume taken from the aqueous deposition bath to obtain the dissolved trivalent chromium formate for step (d).

[0024] Furthermore, the object is solved by an electroplating device for depositing a chromium or chromium alloy layer on at least one substrate, the device comprising:

[0025] (A) a first compartment 110 for an aqueous deposition bath,

[0026] It comprises at least one heating unit 112 and at least one anode 113,

[0027] (B) a second compartment 120 for receiving a partial volume of the aqueous deposition bath,

[0028] It comprises optionally at least one stirring unit 121, and optionally at least one heating unit 122,

[0029] (C) a feeding unit 130 functionally connected to the second compartment 120,

[0030] (D) at least one analysis unit 150,

[0031] (E) at least one transport member 140 connecting the first compartment 110 and the second compartment 120 to transport a partial volume of the aqueous deposition bath to the second compartment 120 and to transport a modified partial volume from the second compartment 120 back to the first compartment 110,

[0032] in

[0033] - the at least one transport member 140 comprises at least one conveying unit 180,

[0034] the at least one analyzing unit 150, the feeding unit 130 and the at least one conveying unit 180 are connected to each other by an electrical connection 160 comprising a control unit 170 adapted such that the at least one analyzing unit 150, the feeding unit 130, the at least one conveying unit 180 and the control unit 170 are suitable for communicating with each other,

[0035] - if the control unit 170 communicates a feed signal, the feed unit 130 is adjusted to add a defined amount of dry powder or suspension into the second compartment 120, and

[0036] If the control unit 170 communicates a delivery signal, the at least one delivery unit 180 is adapted to deliver the modified partial volume into the first compartment 110 . BRIEF DESCRIPTION OF THE DRAWINGS

[0037] exist Figure 1 , the deposition apparatus is described in detail. Figure 1 The reference symbols in have the following meanings:

[0038] 100 Electroplating equipment

[0039] 110 First compartment

[0040] 112 Heating unit

[0041] 113 Anode

[0042] 120 Second compartment

[0043] 121 Mixing unit

[0044] 122 Heating unit

[0045] 130 Feeding unit

[0046] 140 At least one transport component

[0047] 150 At least one analysis unit

[0048] 160 Electrical connection

[0049] 170 Control Unit

[0050] 180 at least one delivery unit (comprising at least one valve and one pump)

[0051] The drawings are schematic and do not necessarily represent actual size, arrangement and proportion. DETAILED DESCRIPTION

[0052] Although trivalent chromium formate generally has a very low and even insufficient solubility in water, the process of the invention allows the use of trivalent chromium formate to replenish trivalent chromium ions and formate ions as a complexing agent for the trivalent chromium ions. Since formate anions are excellent complexing agents for trivalent chromium ions, the complexing agent can be replenished together with the trivalent chromium, i.e. in one source. This is economically most preferred and allows an easy-to-handle process. Since formate ions generally decompose during the process of the invention, no accumulation of formate ions occurs.

[0053] In the method of the present invention, the chromium or chromium alloy layer deposited in step (c) is preferably a functional chromium or functional chromium alloy layer (often also referred to as a hard chromium layer or a hard chromium alloy layer) and a non-decorative chromium or decorative chromium alloy layer. Therefore, preferred is the method of the present invention, wherein the average layer thickness of the chromium or chromium alloy layer deposited in step (c) is 1.0 μm or more, preferably 2 μm or more, more preferably 4 μm or more, even more preferably 5 μm or more, most preferably the average layer thickness is in the range of 5 μm to 200 μm, preferably 6 μm to 150 μm. These are typical average layer thicknesses of functional chromium or chromium alloy layers. These thicknesses are required to provide the desired wear resistance that is generally required. In some cases, the lower limit preferably and explicitly includes 10 μm, 15 μm or 20 μm.

[0054] In contrast, decorative chromium / chromium alloy layers generally have an average layer thickness of well below 1 μm. Furthermore, the substrates used for decorative purposes generally have a relatively short residence time in the respective deposition bath compared to the residence time of the substrates used for functional purposes. This means that for decorative purposes, in the deposition method, the respective deposition bath undergoes a relatively high volume loss by means of a delay. This differs significantly from the deposition method for functional purposes. The substrates used for functional purposes stay in the respective deposition bath for a relatively long time, i.e. without significant delay and therefore undergo a volume loss. This has significant consequences, since it means that only relatively small volumes of, for example, water can be replenished. Otherwise, an undesirable dilution of the deposition bath occurs. This means that the desired compound for replenishment cannot be dissolved in advance in a large volume of fresh electrolyte or water. In the method according to the invention, this fact is taken into account by utilizing solid trivalent chromium formate, which is dissolved in a separated partial volume taken from the aqueous deposition bath utilized in the method according to the invention. This allows the concentrations of trivalent chromium ions and formate ions to be increased to the desired target concentrations and, at the same time, keep the total volume of the aqueous deposition bath fairly constant over a longer period of time.

[0055] Furthermore, due to the process of the invention, the stability and the current efficiency of the aqueous deposition bath are improved (ie increased).

[0056] In the context of the present invention, the term "at least one" means "one, two, three or more than three" (and is interchangeable with them). In addition, the term "trivalent chromium ion" refers to Cr in free or complexed form. 3+ Likewise, "hexavalent chromium" refers to chromium having an oxidation number of +6 and related compounds thereof (including related compounds containing ions of chromium in a hexavalent state).

[0057] The method of the present invention comprises steps (a) and (b), wherein the order is (a) followed by (b) or vice versa. Step (c) is usually carried out after both steps (a) and (b) have been carried out.

[0058] In step (a), an aqueous deposition bath is provided. This means that the main solvent is water. Preferably, water is the only solvent. Therefore, preferably, the aqueous deposition bath does not contain an organic solvent.

[0059] The method of the invention is specifically designed for aqueous deposition baths with a pH in the range of 4.1 to 6.9. The method is incompatible with the same deposition bath which differs only in having a pH below 4.1, since, if the pH is below 4.1, undesired precipitation occurs. Furthermore, if the pH is below 4.1 or above 6.9, a functional chromium layer or chromium alloy layer having sufficient wear resistance and hardness cannot be obtained.

[0060] Preferred is the process of the invention, wherein the pH is in the range of 4.6 to 6.5, preferably in the range of 5.1 to 6.1, most preferably in the range of 5.5 to 5.9. Very good functional chromium and chromium alloy layers are obtained at a pH in the range of 5.1 to 6.1; excellent results are obtained at a pH in the range of 5.5 to 5.9. Functional chromium and chromium alloy layers obtained from a deposition bath having this pH show good or even excellent wear resistance and hardness. The pH ranges and values ​​mentioned above are with reference to a temperature of 20°C.

[0061] The method of the invention is based on the discovery that trivalent chromium ions can be replenished very well if solid trivalent chromium formate is dissolved in a separated partial volume taken from an aqueous sediment. This promotes the dissolution of the trivalent chromium formate and prevents the direct addition of solid trivalent chromium formate into the aqueous deposition bath, which would cause undesirable particles in the deposition bath. These undesirable particles can lead to undesirable roughness of the deposited chromium or chromium alloy layer.

[0062] To enhance the solubility of the trivalent chromium formate, defined temperatures in the aqueous deposition bath and in the separated partial volume are advantageous.

[0063] Preference is given to the process according to the invention, wherein the aqueous deposition bath has a temperature in the range of 20° C. to 80° C., preferably in the range of 30° C. to 70° C., more preferably in the range of 40° C. to 60° C., most preferably in the range of 45° C. to 55° C. A very preferred temperature of the aqueous deposition bath is 50° C. If the temperature significantly exceeds 80° C., undesired evaporation occurs, which adversely affects the concentration of bath components (even up to the risk of precipitation). In addition, the formation of hexavalent chromium is significantly less suppressed. If the temperature is significantly below 20° C., the deposition is insufficient. Most preferably, the above temperature range is applied during step (c) of the process according to the invention.

[0064] Furthermore, preference is given to the process of the invention, wherein the temperature of the separated partial volume taken from the aqueous deposition bath is 3.1°C to 30°C higher, preferably 3.3°C to 26°C, more preferably 3.5°C to 21°C, even more preferably 3.7°C to 15°C, most preferably 3.9°C to 11°C, even most preferably 4°C to 8°C higher than the temperature of the aqueous deposition bath in step (c). In this preferred case, the temperature of the separated partial volume taken from the aqueous deposition bath is always significantly higher than the temperature of the aqueous deposition bath in step (c), which has a favorable effect on the dissolution of the solid trivalent chromium formate. The above temperatures include the precondition that the resulting temperature in the separated partial volume does not exceed 95°C to avoid boiling and excessive gas evolution. If the temperature of the separated partial volume is not sufficiently higher than the temperature of the aqueous deposition bath, insufficient amounts of trivalent chromium formate are dissolved in the separated partial volume, leaving a large amount of undissolved solid trivalent chromium formate. However, if the temperature of the separated partial volume is too high compared to the temperature of the aqueous deposition bath, undesired evaporation of the solvent occurs. Furthermore, introducing the strongly heated separated partial volume back into the aqueous deposition bath would adversely affect the deposition process and undesirably disturb the temperature equilibrium in the aqueous deposition bath.

[0065] The process of the present invention is most preferred, wherein in step (c), the aqueous deposition bath has a temperature in the range of 45°C to 55°C and the temperature of the separated partial volume taken from the aqueous deposition bath is 5°C to 15°C higher than the temperature of the aqueous deposition bath.

[0066] Most preferably, the separated partial volume taken from the aqueous deposition bath has a temperature in the range of 50 to 65°C, preferably irrespective of the temperature of the aqueous deposition bath.

[0067] Alternatively, in some cases, it is preferred that the separated partial volume taken from the aqueous sedimentation has essentially the same temperature as the aqueous sedimentation bath. Thus, preference is given to the process of the invention, wherein the temperature of the separated partial volume taken from the aqueous sedimentation bath is within the range of ±3°C of the temperature of the aqueous sedimentation bath in step (c), preferably within the range of +0°C to +3°C, more preferably within the range of +0°C to +2°C. In this preferred case, the temperature of the separated partial volume taken from the aqueous sedimentation bath is preferably the same as the temperature of the aqueous sedimentation bath in step (c), or preferably only slightly different, i.e. within a small temperature variation.

[0068] In this latter (alternative) case, the dissolution of the trivalent chromium formate is achieved primarily by mechanical influence, preferably by stirring and / or circulation / convection.

[0069] In each case, preference is given to the process of the invention, wherein the separated partial volume taken from the water sediment is agitated, preferably by stirring, most preferably by constant stirring. Most preferably, the separated partial volume is agitated, preferably by stirring, most preferably by constant stirring, and in addition, the separated partial volume is heated, preferably as described above.

[0070] Due to the limited solubility of chromium formate, the dissolution of the solid trivalent chromium formate in the separated partial volume requires a certain time. Preferred is the process of the present invention, wherein the solid trivalent chromium formate is dissolved within 1 minute to 120 minutes, preferably within 10 minutes to 80 minutes, most preferably within 40 minutes to 70 minutes.

[0071] As soon as the trivalent chromium formate has been dissolved, the separated partial volume comprising said dissolved chromium formate is returned to the aqueous deposition bath as quickly as possible. Preferred is the process of the invention, wherein said dissolved trivalent chromium formate is added in step (d) at the latest 8 hours after dissolving said solid trivalent chromium formate in the separated partial volume taken from the aqueous deposition bath, preferably at the latest 4 hours, more preferably at the latest 5 minutes to 3 hours after dissolving said solid trivalent chromium formate in the separated partial volume taken from the aqueous deposition bath, most preferably at the latest 6 to 60 minutes. Depending on the amount dissolved, if said dissolved trivalent chromium formate is returned after a time significantly longer than 8 hours, undesirable precipitate formation is generally visible in the separated partial volume, since the high concentration of trivalent chromium ions promotes precipitation.

[0072] Preference is given to the process according to the invention, wherein the trivalent chromium ions in the aqueous deposition bath have a concentration in the range of 15 g / L to 35 g / L, preferably in the range of 16 g / L to 30 g / L, more preferably in the range of 17 g / L to 26 g / L, even more preferably in the range of 18 g / L to 23 g / L, based on the total volume of the deposition bath. If the total amount is significantly below 15 g / L in many cases, insufficient deposition is seen and the deposited chromium or chromium alloy layer is generally of poor quality. If the total amount is significantly above 35 g / L, the deposition bath is no longer stable, which includes disturbing the formation of precipitates.

[0073] In each case, the target concentration of trivalent chromium ions is within the aforementioned concentration range, preferably within the range of 16 g / L to 30 g / L, more preferably within the range of 17 g / L to 26 g / L, most preferably within the range of 18 g / L to 23 g / L. If the trivalent chromium ions in the aqueous deposition bath have a concentration lower than this target concentration, and preferably still within any one of the aforementioned concentration ranges, most preferably still within 18 g / L to 23 g / L, step (d) of the method of the present invention is performed.

[0074] In step (d) of the method of the present invention, the concentration of trivalent chromium ions in the aqueous deposition bath is increased by adding dissolved trivalent chromium formate, because during step (c), the concentration of trivalent chromium ions in the deposition bath generally decreases due to the deposition of metallic chromium. Preferably, in the method of the present invention, after step (d), the concentration of trivalent chromium ions in the deposition bath does not exceed 35 g / L, preferably does not exceed 30 g / L, more preferably does not exceed 26 g / L, and most preferably does not exceed 23 g / L, based on the total volume of the deposition bath.

[0075] Preferred is the process of the present invention, wherein in step (d) in the separated partial volume taken from the aqueous deposition bath comprising dissolved solid chromium formate, the trivalent chromium ions have a higher concentration than the trivalent chromium ions in the aqueous deposition bath (preferably during or after step (c)), based on the total volume of the separated partial volume comprising dissolved solid chromium formate, preferably up to 15 g / L higher, more preferably up to 10 g / L higher, even more preferably up to 8 g / L higher, most preferably up to 6 g / L higher, even most preferably up to 4 g / L higher.

[0076] Preferred is the process of the present invention, wherein in step (d) in the separated partial volume taken from the aqueous deposition bath comprising dissolved solid chromium formate, the trivalent chromium ions have a concentration in the range of 20 g / L to 35 g / L, preferably in the range of 20.5 g / L to 30 g / L, more preferably in the range of 21 g / L to 28 g / L, even more preferably in the range of 21.5 g / L to 25 g / L, based on the total volume of the separated partial volume comprising dissolved solid chromium formate, but with the proviso that in the separated partial volume comprising dissolved solid chromium formate, the trivalent chromium ions have a higher concentration than in the aqueous deposition bath, preferably during or after step (c).

[0077] Most preferred is the process of the present invention, wherein after carrying out step (d), the trivalent chromium ions in the aqueous deposition bath have a concentration above the respective target concentration, said target concentration preferably being in the range of 18 g / L to 23 g / L, and the concentration of the trivalent chromium ions is preferably again in any one of the aforementioned concentration ranges, most preferably again in the range of 18 g / L to 23 g / L.

[0078] The preferred target concentration is in the range of 19 g / L to 21 g / L.

[0079] In the method of the present invention, step (d) is performed at least once. In other words, the method of the present invention comprises at least one step (d), which is performed if during or after step (c), the trivalent chromium ions have a concentration lower than the target concentration of the trivalent chromium ions.

[0080] The process of the present invention is preferably a continuous process. This means:

[0081] A: Repeat steps (a) to (d) repeatedly, and / or

[0082] B: Step (c) is repeated once or more than once using another substrate, and then step (d) is performed.

[0083] Scheme "B" preferably comprises that step (c) is repeated several times with other substrates and then step (d) is carried out. After completion of step (d), the deposition bath obtained after step (d) is provided in step (a) for another series of steps. Therefore, preferred is the process of the present invention, wherein after step (d), an aqueous deposition bath for at least one further step (a) is produced and steps (a) to (d) are repeated with at least one further substrate and this deposition bath.

[0084] Although after each step (c), the trivalent chromium ions are generally present in a lower concentration than before step (c), it is not necessary to add dissolved trivalent chromium formate during or after each step (c), because the trivalent chromium ions in the aqueous deposition bath have a concentration below the target concentration not after each step (c). The skilled person knows that if the concentration falls below the target concentration, the concentration must be increased. Therefore, it is preferred that the process of the invention wherein step (d) is carried out after each step (c) or not after each step (c) but after at least one step (c).

[0085] As mentioned above, in the method of the present invention, step (d) is performed at least once, preferably several times. This means that the method of the present invention comprises at least one step:

[0086] (c) immersing at least one substrate in an aqueous deposition bath and applying an electric current so that a chromium or chromium alloy layer is deposited on said substrate, said substrate being the cathode,

[0087] wherein during or after step (c), the trivalent chromium ions have a concentration that is less than a target concentration of trivalent chromium ions, and then

[0088] (d) adding dissolved trivalent chromium formate to the aqueous deposition bath such that trivalent chromium ions are present at a higher concentration than before step (d),

[0089] But the prerequisite is

[0090] - dissolving solid trivalent chromium formate in the separated partial volume taken from said aqueous deposition bath to obtain said dissolved trivalent chromium formate for step (d). Preferably, the preferred features of the process of the invention described throughout this document also apply.

[0091] In some cases, preference is given to the process of the invention, wherein the aqueous deposition bath does not contain sulfate ions, preferably neither in step (a) nor after step (d). This means that during the process of the invention, neither a source of chromium ions containing sulfate nor any other compound containing sulfate is utilized. In this case, preference is given to utilizing alternative conductive anions, more preferably chloride ions.

[0092] However, the aqueous deposition bath may contain sulfate ions, preferably, for example, conductive anions. Therefore, in some cases, preferred is the method of the present invention, wherein the aqueous deposition bath contains sulfate ions. The source of sulfate ions is preferably trivalent chromium sulfate, typically chromium sulfate used for the first establishment of the aqueous deposition bath, hereinafter referred to as "fresh aqueous deposition bath". In this case, the concentration of sulfate ions remains relatively constant, since sulfate ions do not degrade. However, over time, due to the delay, the concentration of sulfate ions decreases. Since in these preferred cases, sulfate ions are an essential component of the aqueous deposition bath, a constant concentration needs to be maintained, preferably by a source other than trivalent chromium sulfate. Therefore, in these cases, it is far more preferred not to add any type of chromium sulfate to the aqueous deposition bath.

[0093] Preferred is the process of the present invention, wherein in step (a), the aqueous deposition bath contains sulfate ions and the sulfate ions have a concentration in the range of 5 g / L to 120 g / L, preferably in the range of 20 g / L to 100 g / L, more preferably in the range of 35 g / L to 90 g / L, even more preferably in the range of 50 g / L to 85 g / L, based on the total volume of the deposition bath. Most preferably, this applies to each step (a). In general, it is most preferred to keep the concentrations of all ingredients in the aqueous deposition bath constant.

[0094] Preferred is the process of the invention, wherein in each step (a), the sulfate ions have a concentration within ±10 g / L, preferably within ±5 g / L, compared to the concentration of the sulfate ions in the first step (a), preferably with the proviso that the concentration of the sulfate ions in each step (a) is in the range of 5 g / L to 120 g / L, preferably in the range of 20 g / L to 100 g / L, more preferably in the range of 35 g / L to 90 g / L, even more preferably in the range of 50 g / L to 85 g / L, based on the total volume of the deposition bath. The first step (a) most preferably refers to a fresh aqueous deposition bath. Preferably, the process of the invention comprises two or more steps (a).

[0095] The fresh aqueous deposition bath also comprises formate ions as complexing agent. Since formate ions are strongly degraded during the deposition process, formate ions must be replenished relatively frequently. Therefore, it is advantageous to replenish trivalent chromium ions together with formate ions as defined in the method of the invention. However, it is preferred to also utilize other sources of formate ions.

[0096] Preferred is the process of the present invention, wherein in step (a), the aqueous deposition bath comprises ammonium ions, preferably in a concentration of 30 g / L to 150 g / L, preferably 70 g / L to 120 g / L, even more preferably 80 g / L to 100 g / L, based on the total volume of the deposition bath.

[0097] In some cases, preference is given to the process of the invention, wherein in the aqueous deposition bath the sum of the total weight of trivalent chromium ions and the total weight of ammonium ions corresponds to 90% by weight or more, preferably 95% by weight or more, more preferably 98% by weight or more of the total weight of all cations in the aqueous deposition bath. Thus, substantially the entire amount of cations in the deposition bath is formed by the trivalent chromium ions and the ammonium ions.

[0098] Preferred is the process of the present invention, wherein in step (a), the aqueous deposition bath contains bromide ions, preferably in a total concentration of at least 0.06 mol / L, preferably at least 0.1 mol / L, more preferably at least 0.15 mol / L, based on the total volume of the deposition bath. Bromide ions effectively inhibit the formation of hexavalent chromium formed at the anode.

[0099] Preferred is the process of the invention, wherein the trivalent chromium ions and the formate ions form a molar ratio in the range of 1:0.5 to 1:14, preferably in the range of 1:1 to 1:12, more preferably in the range of 1:4 to 1:11, even more preferably in the range of 1:5 to 1:10. Only within this molar ratio, especially within the more preferred and even more preferred ranges, an excellent functional chromium or functional chromium alloy layer is obtained. If the molar ratio is in the range of 1:5 to 1:10, especially in combination with the pH of the aqueous deposition bath, most preferably in combination with the preferred and more preferred pH ranges defined above, an excellent stability is obtained.

[0100] Preference is given to the process of the invention, wherein the aqueous deposition bath contains no sulfur-containing compounds and no boron-containing compounds having sulfur atoms with an oxidation number below +6.

[0101] It is assumed that the absence of said sulphur-containing compounds leads to an amorphous chromium layer and a chromium alloy layer, respectively. Therefore, preferred is the process of the invention, wherein the layer deposited in step (c) is amorphous as determined by X-ray diffraction. This applies to the chromium or chromium alloy layer obtained during step (c) of the process of the invention and before any other post-deposition surface treatment affecting the atomic structure of said deposited layer, causing it to change from amorphous to crystalline or partially crystalline. Furthermore, it is assumed that these sulphur-containing compounds adversely affect the hardness of the functional chromium or functional chromium alloy layer deposited in step (c).

[0102] In the context of the present invention, the term "does not contain" a target (e.g., a compound, a material, etc.) independently means that the target is not present at all or is present only in a very small and non-interfering amount (degree) without affecting the intended purpose of the present invention. For example, this target may be added or utilized unintentionally, for example, as an unavoidable impurity. Based on the total weight of the aqueous deposition bath utilized in the method of the present invention, if defined for the bath, the term "does not contain" preferably limits the target to 0 (zero) ppm to 50 ppm, preferably 0 ppm to 25 ppm, more preferably 0 ppm to 10 ppm, even more preferably 0 ppm to 5 ppm, and most preferably 0 ppm to 1 ppm. Most preferably, the target is undetectable, which includes the target being present in zero ppm, which is most preferred.

[0103] In some cases, it is preferred that the process of the invention wherein the aqueous deposition bath contains no additional NH + and nitrogen-containing compounds other than NH3.

[0104] Preferred is the process of the present invention wherein the aqueous deposition bath does not contain formaldehyde, glyoxal, formaldehyde bisulfite, glyoxal bisulfite, sodium formaldehyde sulfoxylate, and mixtures thereof, preferably does not contain aldehydes (including monoaldehydes and dialdehydes), sulfites (including bisulfites), sulfoxylates, and mixtures thereof, and most preferably does not contain soluble reducing agents.

[0105] In the process of the present invention, no hexavalent chromium is intentionally added to the aqueous deposition bath.

[0106] The aqueous deposition bath utilized in the process of the present invention is sensitive to a number of metal cations which are undesirable and may cause undesirable discoloration. Therefore, preferred is the process of the present invention, wherein in step (a), the aqueous deposition bath does not contain copper ions, zinc ions, nickel ions and iron ions. This preference also includes compounds containing said metal cations. Most preferably, any of the above mentioned metal cations is not present at all.

[0107] Most preferably, in the aqueous deposition bath utilized in the method of the present invention, chromium is the only sub-group element according to the periodic table.

[0108] Furthermore, preference is given to the process according to the invention, wherein the aqueous deposition bath does not comprise glycine, aluminum ions and tin ions.

[0109] Preferred is the process of the invention, wherein in step (a), the aqueous deposition bath comprises alkali metal cations in a total concentration in the range of 0 mol / L to 0.8 mol / L, preferably in the range of 0 mol / L to 0.6 mol / L, more preferably in the range of 0 mol / L to 0.4 mol / L, even more preferably in the range of 0 mol / L to 0.2 mol / L, based on the total volume of the deposition bath. Most preferably, the aqueous deposition bath comprises alkali metal cations in a total concentration of 0 mol / L to 0.08 mol / L, and even most preferably does not contain any alkali metal cations at all. According to own experiments, a low total concentration of alkali metal cations in the aqueous deposition bath as described above leads to a very smooth deposited chromium or chromium alloy layer.

[0110] Preferred is the process of the present invention, wherein in step (d), the solid trivalent chromium formate contains no alkali metal cations. This means that preferably, in step (d) of the process of the present invention, no alkali metal cations are added to the aqueous deposition bath, preferably independently of the total concentration of alkali metal cations in the aqueous deposition bath (i.e., alkali metal cations may already be present in the aqueous deposition bath or not present in the aqueous deposition bath).

[0111] The term "alkali metal cations in total concentration" refers to the sum of the individual amounts of metal cations of lithium, sodium, potassium, rubidium, cesium and francium. Typically, rubidium, francium and cesium ions are not utilized in the aqueous deposition bath. Therefore, in most cases (and most preferably) the total concentration of alkali metal cations as defined above refers to metal cations of lithium, sodium and potassium, more preferably to metal cations of sodium and potassium.

[0112] In step (b) of the method of the present invention, at least one substrate and at least one anode are provided, wherein the substrate is a cathode. Preferably, more than one substrate is utilized simultaneously in the method of the present invention.

[0113] Preferred is the method of the present invention, wherein the at least one substrate provided in step (b) is a metal or metal alloy substrate, preferably a metal or metal alloy substrate independently comprising one or more than one metal selected from the group consisting of copper, iron, nickel and aluminum, more preferably a metal or metal alloy substrate comprising iron. Most preferably, the at least one substrate is a steel substrate, which is a metal alloy substrate comprising iron. In many technical applications, a steel substrate having a smooth, wear-resistant, functional chromium or chromium alloy layer is desired. This can be achieved in particular by the method of the present invention.

[0114] In some cases, at least one substrate is preferably a coated substrate, more preferably a coated metal substrate. The coating is preferably a metal or metal alloy layer, preferably a nickel or nickel alloy layer, most preferably a semi-bright nickel layer. Especially preferably, a steel substrate coated with a nickel or nickel alloy layer is preferred. However, preferably, other coatings are alternative or additionally present. In many cases, this coating significantly increases corrosion resistance compared to a metal substrate without this coating. However, in some cases, the substrate is not easily corroded due to a corrosive inert environment (e.g., for use in an oil bath). In this case, a coating (preferably a nickel or nickel alloy layer) is not necessarily required.

[0115] Therefore, preferred is the method of the present invention, wherein

[0116] In step (c), a chromium or chromium alloy layer is deposited directly on at least one substrate, or

[0117] At least one substrate defined in step (b) additionally comprises a nickel or nickel alloy layer and in step (c) said chromium or chromium alloy layer is deposited on said substrate.

[0118] Preferred is the process of the present invention, wherein at least one anode is independently selected from the group consisting of graphite anodes and mixed metal oxide anodes (MMO), preferably independently selected from the group consisting of graphite anodes and mixed metal oxide anodes on titanium. These anodes have shown sufficient resistance in the aqueous deposition baths utilized in the process of the present invention.

[0119] Preferably, at least one anode does not contain any lead or chromium.

[0120] In step (c) of the process of the invention, at least one substrate is immersed in an aqueous deposition bath, an electric current is applied and as a result of which a chromium or chromium alloy layer is deposited on said substrate.

[0121] In step (c) of the method of the present invention, a chromium layer or a chromium alloy layer is deposited. In most cases, preference is given to the method of the present invention, wherein the layer deposited in step (c) is a chromium alloy layer. Preferred alloying elements are carbon and oxygen. Carbon is usually present due to formate ions. Preferably, the chromium alloy layer does not contain one, more than one or all elements selected from the group consisting of sulfur, nickel, copper, aluminum, tin and iron. More preferably, the only alloying elements are carbon and / or oxygen, most preferably carbon and oxygen. Preferably, the chromium alloy layer contains 88% by weight of chromium or more, more preferably 91% by weight or more, even more preferably 93% by weight or more, most preferably 96% by weight or more, based on the total weight of the chromium alloy layer.

[0122] Preferred is the process of the present invention, wherein in step (c), the electric current is direct current (DC), preferably having a current of about 5 A / dm 2 Up to 100A / dm 2In the range of 10A / dm 2 Up to 80A / dm 2 In the range of 15A / dm 2 Up to 70A / dm 2 The most preferred range is 20A / dm 2 Up to 60A / dm 2 Direct current within the range of current density.

[0123] Preferably, the direct current is applied in step (c) without interruption during step (c). Thus, the direct current is preferably non-pulsed (non-pulsed DC). Furthermore, the direct current preferably does not comprise a reverse pulse.

[0124] During step (c), the aqueous deposition bath is preferably constantly agitated, preferably by stirring.

[0125] Preferred is the process of the invention, wherein at least one substrate comprising a deposited chromium or chromium alloy layer obtained after step (c) exhibits a thermal conductivity of at least 700 HV (0.05) The wear resistance is preferably as good as that obtained by means of a deposition process based on hexavalent chromium.

[0126] In the method of the present invention, preferably at least one substrate and at least one anode are present in the aqueous deposition bath such that the trivalent chromium ions are in contact with the at least one anode. In this preferred method, a membrane or diaphragm can be completely avoided to separate the trivalent chromium ions from the anode (i.e. no additional compartment is formed in the aqueous deposition bath). In other words, in the method of the present invention, no separation means are utilized to separate the trivalent chromium ions in the deposition bath from the anode. This reduces costs, maintenance work and allows for simplified operation of the method of the present invention. Own experiments have shown that these separation means are not required in the method of the present invention.

[0127] In step (d), the trivalent chromium ions and formate ions are replenished with the aid of dissolved solid trivalent chromium formate. The solid trivalent chromium formate is preferably a dry powder or a suspension. The suspension is preferably obtained by mixing a small amount of liquid with a dry powder so that most of the powder remains undissolved. This prevents the raising of undesirable dust while providing solid chromium formate. It is also most preferred that the small amount of liquid is part of the volume of the aqueous deposition bath. Alternatively, if a small amount of water has to be replenished to the aqueous deposition bath (e.g. due to losses caused by delays), this water is preferably used to obtain the suspension.

[0128] In the method of the present invention, if step (d) is started during or after step (c), the trivalent chromium ions have a concentration lower than the target concentration of trivalent chromium ions. In some cases, it is preferred to directly determine the concentration of trivalent chromium ions and then compare it with the target concentration.

[0129] However, in other cases, preferred is the method of the present invention, wherein the concentration of trivalent chromium ions in the aqueous deposition bath is determined indirectly, most preferably by monitoring and / or determining the total current applied to the aqueous deposition bath. Taking into account the total current and the current efficiency, the reduction in concentration and the concentration of trivalent chromium ions, respectively, can be calculated and compared with the target concentration.

[0130] Therefore, preferred is the process of the present invention wherein, prior to step (d), in the aqueous deposition bath, an ampere-hour meter is used to measure the ampere-hour value. This ampere-hour value is most preferably the trigger for initiating step (d) of the process of the present invention.

[0131] In addition to the addition of dissolved trivalent chromium formate in step (d), preferred is the process of the present invention wherein during the process of the present invention, additional NH4OH, NH3 and / or one or more than one ammonium salt are added, most preferably to adjust the pH of the aqueous deposition bath, to add sulfate ions, and / or to add additional formate ions. Thus, the one or more than one ammonium salt is preferably ammonium formate and ammonium sulfate. Preferably, no other hydroxides than NH4OH are used in the process of the present invention. Preferably, in the process of the present invention, NH4OH, NH3 and formic acid are the only compounds that adjust the pH of the aqueous deposition bath.

[0132] The present invention also relates to the use of solid trivalent chromium formate to replenish trivalent chromium ions and formate anions in an aqueous deposition bath for depositing a chromium or chromium alloy layer on at least one substrate, preferably in combination with a molar ratio between trivalent chromium ions and formate ions as defined above for the process of the invention.

[0133] The present invention relates to the use of solid trivalent chromium formate for replenishing trivalent chromium ions and formate anions in an aqueous deposition bath for depositing a chromium or chromium alloy layer on at least one substrate, wherein the aqueous deposition bath has a pH in the range of 4.1 to 6.9, preferably in combination with a molar ratio between trivalent chromium ions and formate ions as defined above for the process of the invention.

[0134] The present invention therefore relates to the use of a very specific trivalent chromium salt (i.e. chromium formate) in a specific form (i.e. solid) for a very specific purpose (for replenishing an aqueous deposition bath for electrolytic deposition of a chromium or chromium alloy layer). Despite the poor solubility of trivalent chromium formate, the use of solid trivalent chromium formate allows the replenishment of trivalent chromium ions and formate ions as a complexing agent at the same time. This is very preferred, economical and prevents the accumulation of undesirable anions (e.g. sulfate ions), or even avoids the presence of sulfate completely. In addition, this is particularly advantageous for the deposition of functional chromium or functional chromium alloy layers (see above for functional layers). In these cases (and as mentioned above in this article), the replenishment must be carefully controlled to avoid dilution of the aqueous deposition bath. If relatively low solubilities are to be dealt with, solid trivalent chromium formate is an excellent tool to overcome this problem. This is achieved by the method of the present invention.

[0135] More preferred is the use according to the invention, wherein the solid trivalent chromium formate is dissolved before replenishment in the separated partial volume taken from the aqueous deposition bath.

[0136] The use of the present invention in an aqueous deposition bath utilized in the process of the present invention is most preferred.Thus, where applicable, the aforementioned features with respect to the process of the present invention preferably also apply to the aforementioned use of the present invention.

[0137] The use according to the invention is particularly preferred, wherein the aqueous deposition bath for depositing the chromium or chromium alloy layer on the at least one substrate has a pH in the range of 4.6 to 6.5, more preferably in the range of 5.1 to 6.1, most preferably in the range of 5.5 to 5.9. This is particularly preferred in combination with the molar ratio between trivalent chromium ions and formate ions as defined above for the process according to the invention.

[0138] The invention also relates to an electroplating device for depositing a chromium or chromium alloy layer on at least one substrate, the device comprising:

[0139] (A) a first compartment 110 for an aqueous deposition bath,

[0140] It comprises at least one heating unit 112 and at least one anode 113,

[0141] (B) a second compartment 120 for receiving a partial volume of the aqueous deposition bath,

[0142] It comprises optionally at least one stirring unit 121, and optionally at least one heating unit 122,

[0143] (C) a feeding unit 130 functionally connected to the second compartment 120,

[0144] (D) at least one analysis unit 150,

[0145] (E) at least one transport member 140 connecting the first compartment 110 and the second compartment 120 to transport a partial volume of the aqueous deposition bath to the second compartment 120 and to transport a modified partial volume from the second compartment 120 back to the first compartment 110,

[0146] in

[0147] - the at least one transport member 140 comprises at least one conveying unit 180,

[0148] the at least one analyzing unit 150, the feeding unit 130 and the at least one conveying unit 180 are connected to each other by an electrical connection 160 comprising a control unit 170 adapted such that the at least one analyzing unit 150, the feeding unit 130, the at least one conveying unit 180 and the control unit 170 are suitable for communicating with each other,

[0149] - if the control unit 170 communicates a feed signal, the feed unit 130 is adjusted to add a defined amount of dry powder or suspension into the second compartment 120, and

[0150] If the control unit 170 communicates a delivery signal, the at least one delivery unit 180 is adapted to deliver the modified partial volume into the first compartment 110 .

[0151] Most preferably, the first compartment of the electroplating apparatus is a plating tank, most preferably a plating tank containing an aqueous deposition bath having a pH in the range of 4.1 to 6.9, the bath comprising:

[0152] - trivalent chromium ions,

[0153] -formate ion, and

[0154] -Optionally sulfate ions.

[0155] The aforementioned features of the aqueous deposition bath utilized in the method of the present invention preferably also apply to the aqueous deposition bath utilized in the electroplating apparatus of the present invention, and most preferably, the aforementioned features of the method of the present invention preferably also apply to the electroplating apparatus of the present invention (if applicable).

[0156] Preferably, the second compartment is a replenishment tank.

[0157] Preferably, at least one transport member is a pipe.

[0158] Preferably, at least one transport member comprises a first transport member to transport a partial volume of the aqueous deposition bath to the second compartment 120, and a second transport member to transport the modified partial volume from the second compartment 120 back to the first compartment 110. More preferably, each transport member comprises a conveying unit individually. This ensures that in each transport member, only one flow direction is applied. In the context of the present invention, "transport member" also means a connecting member suitable for conveying liquids (and therefore interchangeable with the connecting member).

[0159] Very preferably, at least one transport member additionally comprises at least one filter unit. These filter units are very advantageous if the solid trivalent chromium formate is not completely dissolved or if other precipitates are formed and thus prevent particles from entering the deposition bath. Alternatively or additionally, the conveying unit 180 comprises a filter unit.

[0160] The modified partial volume is preferably a separated partial volume taken from the first compartment (preferably taken from the aqueous deposition bath) which comprises undissolved dry powder (preferably undissolved solid chromium formate).

[0161] Furthermore, the electroplating device of the invention preferably comprises means for applying an electric current in the first compartment. As regards the details regarding the electric current, see above.

[0162] In some cases, it is preferred that the electroplating apparatus of the present invention has a volume of the second compartment that is at least 5% by volume, preferably at least 9% by volume, of the volume of the first compartment.

[0163] The volume of the second compartment is determined primarily by / based on the average current flux per hour (h) in ampere-hours (Ah) applied to the total volume of the aqueous deposition bath in the first compartment. Therefore, the second compartment must have a total volume suitable for absorbing the desired volume of the partial volume. Preferred is the electroplating device of the present invention, wherein the second compartment is suitable for absorbing a volume varying in the range of 15L to 100L of the partial volume per 1000Ah / h of current applied to the aqueous deposition bath in the first compartment, preferably a volume varying in the range of 25L to 80L, most preferably this applies, but with the proviso that the temperature of the partial volume of the aqueous deposition bath is in the range of 45°C to 65°C, most preferably in the range of 50°C to 60°C. Under these conditions, optimized charging can be achieved, i.e. sufficient time is given to dissolve the solid trivalent chromium formate and to properly add the dissolved trivalent chromium formate to the aqueous deposition bath. Sufficient time is also allowed for maintenance. The foregoing also applies to the method of the present invention.

[0164] For example, the method of the present invention is by means of Figure 1 The electroplating device 100 schematically shown in FIG.

[0165] A fresh aqueous deposition bath is set up in the first compartment 110, which is a plating tank. The fresh aqueous deposition bath contains 18 g / L to 23 g / L of trivalent chromium ions, sulfate ions, formate ions, bromide ions and ammonium ions and has a pH in the range of 5.5 to 5.9, referenced to 20° C. The target concentration is within a concentration of 19 g / L to 21 g / L.

[0166] The deposition bath was maintained at a temperature of about 50° C. by using a heating unit 112. The steel substrate coated with the nickel alloy layer was immersed in the deposition bath while applying about 40 A / dm 2 A direct current of about 100° is applied for about 45 minutes to electrolytically deposit a functional chromium alloy layer. The anode 113 is a graphite anode. The deposition of this chromium alloy layer is repeated several times with additional substrates until the concentration of trivalent chromium ions is below the target concentration. The concentration of trivalent chromium ions is indirectly analyzed by a last analyzing unit 150, which is an ampere-hour meter that analyzes the total current applied to the deposition bath. In this case, the last analyzing unit 150 is located outside the first compartment 110. However, alternatively and if the total concentration of trivalent chromium ions is directly analyzed, the at least one analyzing unit 150 is in direct contact with the deposition bath.

[0167] For replenishment of trivalent chromium ions and formate ions, solid trivalent chromium formate as a dry powder (or as a suspension) is added manually or automatically to the feed unit 130. A partial volume is separated from the aqueous deposition bath in the first compartment by means of at least one transport member 140, which is a pipe, and transported to the second compartment, i.e. into the replenishment tank.

[0168] If the concentration of trivalent chromium ions analyzed by at least one analysis unit 150 (the analysis unit 150 is electrically connected to the control unit 170 and the feeding unit 130 by means of an electrical connection 160) is below the target concentration, a feeding signal is generated in the control unit 170 and communicated to the feeding unit 130. The feeding unit 130 automatically adds the dry powder (or suspension) to the second compartment 120 in a defined amount. The second compartment is heated to a temperature of about 60° C. by means of a heating unit 122 and the separated partial volume is continuously stirred by the stirring unit 121 for about 60 minutes to dissolve the dry powder, i.e. to obtain dissolved trivalent chromium formate. In the context of the present invention, the control unit 170 is preferably a control and / or regulating unit; a feeding unit 130 "functionally connected" to the second compartment also means "integrated" with the second compartment.

[0169] Regardless of whether the feeding unit 130 is adding a dry powder or a suspension, in each case the feeding unit is adapted to at least add (ie transport, provide, etc.) a solid to the second compartment. In the case of a suspension, the solid is accompanied by a liquid.

[0170] After the added solid trivalent chromium formate is dissolved, a modified partial volume is obtained in the second compartment 120. Then, the control unit 170 communicates a transport signal to at least one transport unit 180 so that the at least one transport unit 180 transports the modified partial volume back into the first compartment. As a result, the concentration of trivalent chromium ions in the first compartment (i.e., the aqueous deposition bath) increases and is above the target concentration. Deposition of functional chromium alloy layers continues with other substrates until the concentration is again below the target concentration. In this case, the replenishment as described above is repeated.

[0171] In the context of the present invention, the term "conveyor unit" means (and is interchangeable with) a "transport unit", i.e. a unit that is primarily responsible for processing individual communication signals so that the transport of partial volumes and modified partial volumes is facilitated / performed. Typically, it is an active component in the transport member 140.

[0172] Preferred is the process of the invention, wherein in step (d) the dissolved trivalent chromium ions are added batchwise to the aqueous deposition bath. In other cases, a process is preferred, wherein in step (d) the dissolved trivalent chromium ions are added continuously or semi-continuously to the aqueous deposition bath.

[0173] It is believed that the method of the present invention is substantially applicable to similar sparingly soluble chromium salts, preferably sparingly soluble chromium salts comprising anions selected from the group consisting of acetate ions, propionate ions, glycolate ions, oxalate ions, carbonate ions, citrate ions and combinations thereof. However, formate ions are the most preferred and therefore the most preferred complexing agent for trivalent chromium ions, and therefore trivalent chromium formate is the most preferred sparingly soluble chromium salt utilized in step (d) of the method of the present invention. Therefore, firstly preferred is the method of the present invention, wherein in step (d), no chromium salt comprising anions selected from the group consisting of acetate ions, propionate ions, glycolate ions, oxalate ions, carbonate ions, citrate ions and combinations thereof is utilized, more preferably the aqueous deposition bath does not contain acetate ions, propionate ions, glycolate ions, oxalate ions, carbonate ions and citrate ions at all. Most preferably, formate ions are the only organic complexing agent for the trivalent chromium ions.

Claims

1. A method for depositing a chromium or chromium alloy layer on at least one substrate, the method comprising the following steps: (a) providing an aqueous deposition bath having a pH in the range of 4.1 to 6.9, said bath comprising: - trivalent chromium ions, -formate ion, - sulfate ions, and Ammonium ions, (b) providing said at least one substrate and at least one anode, (c) immersing said at least one substrate in said aqueous deposition bath and applying an electric current so that said chromium or chromium alloy layer is deposited on said substrate, said substrate being a cathode, wherein during or after step (c), when the trivalent chromium ions have a concentration that is already lower than a target concentration of trivalent chromium ions, (d) adding dissolved trivalent chromium formate to the aqueous deposition bath such that trivalent chromium ions are present at a higher concentration than before step (d), provided that - solid trivalent chromium formate is dissolved in the separated partial volume taken from the aqueous deposition bath to obtain the higher concentration of trivalent chromium ions for step (d), wherein in step (a), the sulfate ions have a concentration in the range of 35 g / L to 90 g / L based on the total volume of the deposition bath, Wherein in step (a), the aqueous deposition bath comprises ammonium ions at a concentration of 30 g / L to 150 g / L based on the total volume of the deposition bath.

2. The method according to claim 1, wherein the aqueous deposition bath has a temperature in the range of 20°C to 80°C.

3. The method according to claim 1 or 2, wherein the temperature of the separated partial volume taken from the aqueous deposition bath is 3.1°C to 30°C higher than the temperature of the aqueous deposition bath in step (c).

4. The method according to claim 1 or 2, wherein the temperature of the separated partial volume taken from the aqueous deposition bath is within ± 3°C of the temperature of the aqueous deposition bath in step (c).

5. The method according to claim 1 or 2, wherein the dissolved trivalent chromium formate is added in step (d) at the latest 8 hours after dissolving the solid trivalent chromium formate in the separated partial volume taken from the aqueous deposition bath.

6. The method according to claim 1 or 2, wherein the trivalent chromium ions in the aqueous deposition bath have a concentration in the range of 15 g / L to 35 g / L based on the total volume of the deposition bath.

7. The process according to claim 1 or 2, wherein in step (d), in the separated partial volume taken from the aqueous deposition bath comprising the dissolved solid chromium formate, the trivalent chromium ions have a higher concentration than the trivalent chromium ions in the aqueous deposition bath, based on the total volume of the separated partial volume comprising the dissolved solid chromium formate.

8. The method according to claim 1 or 2, wherein in step (d), in the separated partial volume taken from the aqueous deposition bath comprising the dissolved solid chromium formate, the trivalent chromium ions have a concentration in the range of 20 g / L to 35 g / L based on the total volume of the separated partial volume comprising the dissolved solid chromium formate, but with the proviso that in the separated partial volume comprising the dissolved solid chromium formate, the trivalent chromium ions have a higher concentration than the trivalent chromium ions in the aqueous deposition bath.

9. The method according to claim 1 or 2, wherein after step (d), an aqueous deposition bath is produced for at least one further step (a) and steps (a) to (d) are repeated with at least one further substrate and this deposition bath.

10. The method according to claim 1 or 2, wherein in step (a), the aqueous deposition bath contains sulfate ions and the sulfate ions have a concentration in the range of 50 g / L to 85 g / L based on the total volume of the deposition bath.

11. The method according to claim 10, wherein in each step (a), the sulfate ion has a concentration within a deviation of ±10 g / L compared to the concentration of the sulfate ion in the first step (a).

12. The method according to claim 1 or 2, wherein in step (a), the aqueous deposition bath comprises ammonium ions at a concentration of 70 g / L to 120 g / L based on the total volume of the deposition bath.

13. The method according to claim 1 or 2, wherein before step (d), in the aqueous deposition bath, an ampere-hour value is measured using an ampere-hour meter.