Fuel cell module, fuel cell stack, and method for manufacturing fuel cell module

By forming gaps or through-holes on the outer periphery of the gas diffusion layer of the fuel cell module, the stress is dispersed and the problem of stress concentration in the electrolyte membrane where the electrode layer and the protective layer overlap is solved, thereby realizing a fuel cell module with high durability and miniaturization.

CN113169341BActive Publication Date: 2024-10-11PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN201980081646.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-02
Filing Date
2019-11-28
Publication Date
2024-10-11
Estimated Expiration
2039-11-28

AI Technical Summary

Technical Problem

In existing fuel cell modules, the stress concentration at the overlapping portions of the electrode layer and protective layer causes damage or deterioration of the electrolyte membrane, and it is difficult to achieve miniaturization or thinning.

Method used

Gaps or through-holes are formed on the outer periphery of the gas diffusion layer to reduce overlap with the sealing member. This structure allows the gas diffusion layer to deform when a load is applied in the thickness direction, thereby dispersing stress and preventing deterioration of the electrolyte membrane.

Benefits of technology

It effectively prevents damage or deterioration of the electrolyte membrane, achieves high durability and miniaturization of the fuel cell module, and reduces external gas leakage and cross-leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113169341B_ABST
    Figure CN113169341B_ABST
Patent Text Reader

Abstract

A fuel cell module is provided that suppresses degradation of a polymer electrolyte membrane. The fuel cell module comprises: a membrane-electrode assembly; a pair of separators sandwiching the membrane-electrode assembly; and a sealing member that bonds and seals the membrane-electrode assembly and the pair of separators, respectively, wherein the membrane-electrode assembly comprises: a polymer electrolyte membrane; an anode catalyst layer disposed on a first main surface of the polymer electrolyte membrane; a cathode catalyst layer disposed on a second main surface of the polymer electrolyte membrane; and a pair of gas diffusion layers, one of which is stacked on the anode catalyst layer and the other is stacked on the cathode catalyst layer, wherein the gas diffusion layer of one of the pair of gas diffusion layers and the sealing member overlap in the thickness direction in a region including an end edge on the center side of the sealing member, and a portion of a portion of the gas diffusion layer of one of the pair of gas diffusion layers corresponding to the region is cut through in the thickness direction.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a fuel cell module and a fuel cell stack, and a method for manufacturing the fuel cell module. Background Art

[0002] In the fuel cell module described in Patent Document 1, a membrane-electrode assembly is sandwiched between a pair of separators, and the membrane-electrode assembly and the pair of separators are bonded to each other via a resin portion containing fibers at least in part, thereby being integrally joined.

[0003] The membrane-electrode assembly described in Patent Document 2 has a protective layer formed on the peripheral edge of the electrode layer, and has an overlapping portion where the electrode layer and the protective layer overlap in the thickness direction.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: JP Patent No. 6149260

[0007] Patent Document 2: Japanese Patent Application Publication No. 2009-217999 Summary of the invention

[0008] Problems to be solved by the invention

[0009] In recent years, there has been a demand for a fuel cell module that suppresses damage or degradation of the electrolyte membrane.

[0010] Means for solving problems

[0011] The fuel cell module disclosed in the present invention comprises: a membrane-electrode assembly; a pair of separators sandwiching the membrane-electrode assembly; and a sealing member that adheres and seals the membrane-electrode assembly and the pair of separators respectively, wherein the membrane-electrode assembly has: a polymer electrolyte membrane; an anode catalyst layer provided on the first main surface of the polymer electrolyte membrane; a cathode catalyst layer provided on the second main surface of the polymer electrolyte membrane; and a pair of gas diffusion layers, one of which is stacked on the anode catalyst layer and the other is stacked on the cathode catalyst layer, the gas diffusion layer of one of the pair of gas diffusion layers and the sealing member overlap in the thickness direction in an area including the end edge on the center side of the sealing member, and a part of the portion of the gas diffusion layer of one of the pair of gas diffusion layers corresponding to the area is cut through in the thickness direction.

[0012] The fuel cell stack disclosed in the present invention has a plurality of the above-mentioned fuel cell modules.

[0013] The manufacturing method of the fuel cell module disclosed in the present invention includes: a gas diffusion layer processing step, in which the volume of at least a portion of the outer periphery of at least one of the gas diffusion layers in a pair of gas diffusion layers is reduced; a configuration step, in which the membrane-electrode assembly including the pair of gas diffusion layers and the sealing member are configured so that at least a portion of the outer periphery overlaps with the sealing member in the thickness direction; and a bonding step, in which the sealing member and the membrane-electrode assembly are sandwiched by a pair of separators, and the membrane-electrode assembly and the pair of separators are bonded.

[0014] Effects of the Invention

[0015] According to the present disclosure, it is possible to provide a fuel cell module and a fuel cell stack in which damage or degradation of an electrolyte membrane is suppressed, and a method for manufacturing a fuel cell module. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is an exploded perspective view of the fuel cell stack according to Embodiment 1 of the present disclosure.

[0017] Figure 2 It is a plan view of a membrane-electrode assembly and a sealing member of a fuel cell module according to Embodiment 1 of the present disclosure.

[0018] Figure 3 yes Figure 2 AA line cross-sectional view of the membrane-electrode assembly.

[0019] Figure 4 It is a plan view of a cathode gas diffusion layer of a fuel cell module according to Embodiment 1 of the present disclosure.

[0020] Figure 5 It is a plan view of an anode gas diffusion layer of a fuel cell module according to Embodiment 1 of the present disclosure.

[0021] Figure 6 Yes Figure 4 as well as Figure 5 An enlarged view of a portion of the outer circumference of the gas diffusion layer processed into a serrated shape.

[0022] Figure 7 Yes Figure 4 as well as Figure 5 An enlarged view of a portion of the outer peripheral portion of the through hole formed in the gas diffusion layer.

[0023] Figure 8 It is a cross-sectional view showing the positional relationship of the structural members of the fuel cell module according to Embodiment 1 of the present disclosure.

[0024] Fig. 9 This is a partial cross-sectional view of a fuel cell module according to Embodiment 1 of the present disclosure.

[0025] Fig.10 This is a partial cross-sectional view of a fuel cell module according to Embodiment 1 of the present disclosure.

[0026] Fig.11 This is an exemplary flow chart of a method for manufacturing a fuel cell module according to Embodiment 1 of the present disclosure.

[0027] Fig.12 It is a plan view of a cathode sealing member according to Embodiment 2 of the present disclosure.

[0028] Fig.13 It is a plan view of an anode sealing member according to Embodiment 2 of the present disclosure.

[0029] Fig.14 It is a top view of a cathode gas diffusion layer according to Embodiment 2 of the present disclosure.

[0030] Fig.15 It is a plan view of an anode gas diffusion layer according to Embodiment 2 of the present disclosure.

[0031] Fig.16 This is a partial cross-sectional view of a fuel cell module according to Embodiment 2 of the present disclosure.

[0032] Fig.17 It is a plan view of an electrolyte membrane-electrode assembly and a sealing member in a fuel cell module according to Embodiment 3 of the present invention.

[0033] Fig.18 yes Fig.17 AA line cross-sectional view of the electrolyte membrane-electrode assembly.

[0034] Fig.19 This is a partial cross-sectional view of a fuel cell module according to Embodiment 3 of the present invention.

[0035] Fig. 20 It is a partial cross-sectional view showing the positional relationship of fuel cell module components according to Embodiment 3 of the present invention.

[0036] Fig.21 It is a plan view of a gas diffusion layer according to Embodiment 3 of the present invention.

[0037] Fig. 22 This is a top view of a gas diffusion layer whose outer periphery is processed into a serrated shape.

[0038] Fig.23 This is a plan view of a gas diffusion layer having through holes formed on the outer periphery.

[0039] Fig.24This is a partial cross-sectional view of a fuel cell module according to Embodiment 3 of the present invention.

[0040] Fig.25 This is an exemplary flow chart of a method for manufacturing a fuel cell module according to Embodiment 3 of the present invention.

[0041] Fig.26 This is a cross-sectional view of components of a conventional solid polymer fuel cell.

[0042] Fig. 27 Partial cross-sectional view of a conventional fuel cell module. DETAILED DESCRIPTION

[0043] (The process of this disclosure)

[0044] A polymer electrolyte fuel cell is a device that generates electricity and heat simultaneously by electrochemically reacting a fuel gas containing hydrogen with an oxidant gas containing oxygen, such as air. Hereafter, a polymer electrolyte fuel cell will be referred to as a PEFC (Polymer Electrolyte Fuel Cell). Fig.26 The cross-sectional view of FIG. 1 shows the basic structure of PEFC. PEFC includes an electrolyte membrane 1500 that selectively transports hydrogen ions, and an anode electrode 1900 and a cathode electrode 2000 formed on both surfaces of the electrolyte membrane 1500 .

[0045] The anode electrode 1900 includes: an anode catalyst layer 1600 formed on the first main surface 1510 of the electrolyte membrane 1500; and an anode gas diffusion layer 1810 stacked on the outside of the anode catalyst layer 1600. The cathode electrode 2000 includes: a cathode catalyst layer 1700 formed on the second main surface 1520 of the electrolyte membrane 1500; and a cathode gas diffusion layer 1820 stacked on the outside of the cathode catalyst layer 1700. The anode gas diffusion layer 1810 and the cathode gas diffusion layer 1820 have the functions of air permeability and electronic conductivity.

[0046] In this way, a product in which the electrolyte membrane 1500 and the electrodes 1900 and 2000 are integrally joined and assembled is a membrane-electrode assembly 1000. Hereinafter, the membrane-electrode assembly may also be referred to as MEA (Membrane Electrode Assembly).

[0047] exist Fig. 271 shows a cross-sectional view of MEA1000. An anode separator 1110 is provided on the anode electrode 1900 side of MEA1000, and a cathode separator 1120 is provided on the cathode electrode 2000 side of MEA1000. The anode separator 1110 and the cathode separator 1120 mechanically sandwich and fix the MEA1000. In this way, the structure in which the MEA1000 is sandwiched by a pair of separators 1110 and 1120 is a fuel cell module (single cell module) 2100. In addition, the separators 1110 and 1120 are components for electrically connecting adjacent fuel cell modules 2100 in series. A gas flow path groove 1310 for supplying a reaction gas to the anode electrode 1900 and carrying away generated water and excess gas is formed in the portion of the anode separator 1110 that contacts the MEA1000. A gas flow path groove 1320 is also formed in the portion of the cathode separator 1120 that contacts the MEA1000.

[0048] Therefore, in fuel cells, improving the utilization efficiency of the reaction gas is one of the important issues. Factors that reduce the utilization efficiency include external leakage of gas, cross leakage of gas, and shortcut of gas.

[0049] In order to supply the reaction gas to the gas flow channels 1310 and 1320, manifold holes are provided at the edges of the separators 1110 and 1120 to distribute the reaction gas. Furthermore, in order to prevent the reaction gas supplied to the gas flow channels 1310 and 1320 from leaking to the outside or mixing, a sealing member 900 is provided between the pair of separators 1110 and 1120 so as to surround the electrode forming portion in the MEA 1000, that is, the outer periphery of the power generation region.

[0050] exist Fig.26 The outer edge of the MEA1000 shown is embedded in the frame. The sealing member 900 (gasket) is embedded in the outer edge (peripheral portion) of the MEA1000. Conductive separators 1110 and 1120 are arranged on both sides of the thickness direction of the MEA1000. The sealing member 900 between the separators 1110 and 1120 uses a resin frame and an elastomer gasket for holding the MEA1000. In this case, it is necessary to fill the gap between the resin frame and the electrolyte membrane 1500 with an elastomer gasket, requiring high component dimensional accuracy and assembly accuracy. For this reason, a complex gasket shape is formed so that no gap will be generated within the tolerance range, and since the tolerance will not become too small, it is difficult to make the elastomer gasket thin. Miniaturization or thinning is required for a fuel cell stack that can obtain a high voltage by stacking and connecting a plurality of fuel cell modules 2100 in series, but it is difficult to miniaturize or thin it when a resin frame and an elastomer gasket are used in the sealing member 900. Therefore, as in Patent Document 1, there is known a method of realizing a thin module by using an insulating thermosetting resin as the sealing member 900 .

[0051] In addition, if the electrolyte membrane 1500, or the anode catalyst layer 1600 and the cathode catalyst layer 1700 are directly exposed to the reaction gas at the end of the surface direction of the MEA 1000, the degradation of the electrolyte membrane 1500 will be accelerated, which will affect the durability. For this reason, as in Patent Document 2, there is also a method of forming a protective layer as a sealing member so that the electrolyte membrane 1500, the anode catalyst layer 1600 and the cathode catalyst layer 1700 are not exposed.

[0052] However, in the case of Patent Document 2, since the protective layer (sealing member) has an overlapping portion that overlaps with the electrode layer (gas diffusion layer), when the MEA is sandwiched between the separators to apply a load, stress is concentrated on the separator and the electrolyte membrane at the overlapping portion where the protective layer and the electrode layer overlap, and there is a possibility of damage to the separator or rupture of the electrolyte membrane. In addition, in the case of a design in which the protective layer is stepped to avoid stress concentration, or in the case of a dimensional design of the electrode layer without the overlapping portion with the protective layer, the electrolyte membrane and the electrode layer may be exposed due to alignment and assembly tolerances.

[0053] Therefore, the inventors of the present invention conducted intensive studies to prevent stress concentration on the separator and the electrolyte membrane and suppress degradation of the electrolyte membrane even when the electrode layer and the protective layer have an overlapping portion, and as a result, obtained the following findings.

[0054] In a fuel cell module having an MEA such as that disclosed in Patent Document 2, if a load is applied in a state where the sealing member and the gas diffusion layer have overlapping portions, stress concentration will occur on structural members of the fuel cell module such as the separator and the electrolyte membrane. In view of this, for example, it is considered that the overlapping portion overlapping with the sealing member in the gas diffusion layer is made of a softer material than the non-overlapping portion that does not overlap with the sealing member. However, since it is difficult to manufacture the overlapping portion in the gas diffusion layer with a material different from that of the non-overlapping portion, problems such as an increase in the manufacturing cost of the gas diffusion layer may occur.

[0055] In view of this, the inventors of the present invention have found a structure for forming a gap (space) in the outer periphery of the gas diffusion layer. Specifically, the following structure is found: the gas diffusion layer and the sealing member are overlapped in the region of the end edge of the sealing member having an opening, so as to form a gap that penetrates at least a part of the portion overlapping with the sealing member in the gas diffusion layer in the thickness direction. Thus, a gap can be formed for the gas diffusion layer to deform in the surface direction. For this reason, when a load is applied to the gas diffusion layer in the thickness direction, the gas diffusion layer can deform toward the gap. Thus, it is found that even when a load is applied in a state where the gas diffusion layer and the portion stacked on the gas diffusion layer overlap in the thickness direction, stress concentration on the structural member can be prevented. As a result, it is found that even in the case of a portion where the outer periphery of the gas diffusion layer overlaps with the sealing member, stress concentration on the structural member can be prevented and degradation of the electrolyte membrane can be suppressed.

[0056] Based on these new findings, the inventors of the present invention have completed the following invention.

[0057] According to one embodiment of the present disclosure, a fuel cell module is provided, comprising: a membrane-electrode assembly; a pair of separators sandwiching the membrane-electrode assembly; and a sealing member that adheres and seals the membrane-electrode assembly and the pair of separators, respectively, wherein the membrane-electrode assembly has: a polymer electrolyte membrane; an anode catalyst layer provided on the first main surface of the polymer electrolyte membrane; a cathode catalyst layer provided on the second main surface of the polymer electrolyte membrane; and a pair of gas diffusion layers, one of which is stacked on the anode catalyst layer and the other is stacked on the cathode catalyst layer, the gas diffusion layer of one of the pair of gas diffusion layers and the sealing member overlap in the thickness direction in an area including the end edge on the center side of the sealing member, and a portion of the portion of the gas diffusion layer of one of the pair of gas diffusion layers corresponding to the area is cut through in the thickness direction.

[0058] With such a structure, a portion of the portion (inner region) corresponding to the region in one gas diffusion layer is cut through in the thickness direction, so that a space for the first diffusion layer to deform in the surface direction can be formed. Thus, when a load is applied to the first diffusion layer in the thickness direction, the first diffusion layer can deform toward the space. Thus, even when a load is applied in a state where the gas diffusion layer and the sealing member overlap in the thickness direction, stress concentration on the structural member can be prevented. As a result, even when the outer periphery of the gas diffusion layer and the sealing member overlap, stress concentration on the structural member can be prevented, thereby suppressing the degradation of the polymer electrolyte membrane.

[0059] According to a second aspect of the present disclosure, there may be provided a fuel cell module wherein a plurality of through holes penetrating in the thickness direction are provided in a portion of the one gas diffusion layer corresponding to the region.

[0060] With such a structure, when a load is applied to the first diffusion layer in the thickness direction, the first diffusion layer can be deformed toward the through hole.

[0061] According to a third aspect of the present disclosure, there may be provided a fuel cell module, wherein a portion of the one gas diffusion layer corresponding to the region is provided with a serration portion formed in a serration shape in a plan view.

[0062] With such a structure, when a load is applied to the first diffusion layer in the thickness direction, the first diffusion layer can be deformed toward the space between the sawtooth portions.

[0063] According to a fourth embodiment of the present disclosure, the following fuel cell module is provided, wherein the pair of gas diffusion layers are an anode gas diffusion layer stacked on the anode catalyst layer, and a cathode gas diffusion layer stacked on the cathode catalyst layer, the pair of separators are an anode separator arranged on the anode gas diffusion layer side of the membrane-electrode assembly, and a cathode separator arranged on the cathode gas diffusion layer side of the membrane-electrode assembly and paired with the anode separator to sandwich the membrane-electrode assembly, the sealing member comprises: an anode sealing member having an opening, bonding and sealing the membrane-electrode assembly and the anode separator; and a cathode sealing member having an opening, bonding and sealing the membrane-electrode assembly and the cathode separator, when viewed from a direction perpendicular to the first main surface, the anode gas The body diffusion layer has an anode side inner region overlapping with the anode sealing member in a region including the end edge on the opening side of the anode sealing member, and the cathode gas diffusion layer has a cathode side inner region overlapping with the cathode sealing member in a region including the end edge on the opening side of the cathode sealing member when viewed from a direction perpendicular to the first main surface, a gap penetrating in the thickness direction of the anode gas diffusion layer is formed in at least a portion of the anode gas diffusion layer including the anode side inner region, and a gap penetrating in the thickness direction of the cathode gas diffusion layer is formed in at least a portion of the cathode gas diffusion layer including the cathode side inner region, and when viewed from a direction perpendicular to the first main surface, the anode side inner region and the cathode side inner region do not overlap.

[0064] With such a structure, by forming a gap in at least a portion of the inner region on the anode side and the inner region on the cathode side, it is possible to prevent stress concentration on the structural member when a load is applied in the thickness direction of the fuel cell module. As a result, it is possible to suppress damage or degradation of the polymer electrolyte membrane.

[0065] According to the fifth embodiment of the present disclosure, a fuel cell module may be provided in which, when viewed from a direction perpendicular to the first main surface, the inner region on the anode side has: an outer portion located further outward than the inner region on the cathode side; and an inner portion located further inward than the inner region on the cathode side.

[0066] With this structure, since the inner region on the anode side and the inner region on the cathode side do not overlap, it is possible to prevent stress concentration when a load is applied in the thickness direction of the fuel cell module.

[0067] According to a sixth aspect of the present disclosure, there may be provided a fuel cell module in which at least one of the space formed in the anode gas diffusion layer and the space formed in the cathode gas diffusion layer includes a plurality of through holes.

[0068] With such a structure, when a load is applied in the thickness direction of the fuel cell module, the gas diffusion layer can deform toward the through-holes, thereby preventing stress concentration.

[0069] According to the seventh aspect of the present disclosure, a fuel cell module may be provided in which at least one of the gap formed in the anode gas diffusion layer and the gap formed in the cathode gas diffusion layer is formed by a serrated notch when viewed in a direction perpendicular to the first main surface.

[0070] With such a structure, when a load is applied in the thickness direction of the fuel cell module, the gas diffusion layer can be deformed toward the notch between the serrations, thereby preventing stress concentration.

[0071] According to an eighth aspect of the present disclosure, there can be provided a fuel cell stack in which a plurality of fuel cell modules according to any one of the first to seventh aspects are connected in series and stacked.

[0072] With such a structure, it is possible to prevent stress from concentrating on structural members of the fuel cell stack, thereby providing a fuel cell stack with high durability.

[0073] According to the 9th embodiment of the present disclosure, a method for manufacturing a fuel cell module can also be provided, comprising: a gas diffusion layer processing step, in which the volume of at least a portion of the outer peripheral portion of at least one of the gas diffusion layers in a pair of gas diffusion layers is reduced; a configuration step, in which the membrane-electrode assembly including the pair of gas diffusion layers and the sealing member are configured so that at least a portion of the outer peripheral portion overlaps with the sealing member in the thickness direction; and a bonding step, in which the sealing member and the membrane-electrode assembly are sandwiched by a pair of partitions, and the membrane-electrode assembly and the pair of partitions are bonded.

[0074] According to such a method, even when the outer peripheral portion of the gas diffusion layer overlaps with the sealing member, it is possible to prevent stress concentration on the structural member, thereby suppressing degradation of the polymer electrolyte membrane.

[0075] According to the tenth embodiment of the present disclosure, the following method for manufacturing a fuel cell module can also be provided, the method further comprising: a preparation step, preparing a polymer electrolyte membrane having an anode catalyst layer on a first main surface and a cathode catalyst layer on a second main surface, an anode gas diffusion layer and a cathode gas diffusion layer, an anode separator and a cathode separator, and an anode sealing member and a cathode sealing member; in the gas diffusion layer processing step, forming a gap in at least a portion of the outer periphery of the anode gas diffusion layer and the cathode gas diffusion layer; in the configuration step, stacking the anode gas diffusion layer on the anode catalyst layer side of the polymer electrolyte membrane, and stacking the anode gas diffusion layer on the cathode catalyst layer side of the polymer electrolyte membrane. The cathode gas diffusion layer is stacked on the catalyst layer side to form a membrane-electrode assembly, the anode sealing member is arranged to overlap with at least a portion of the outer periphery of the anode gas diffusion layer, and the cathode sealing member is arranged to overlap with at least a portion of the outer periphery of the cathode gas diffusion layer. In the bonding step, the anode gas diffusion layer and the anode separator of the membrane-electrode assembly are bonded via the anode sealing member, the cathode gas diffusion layer and the cathode separator of the membrane-electrode assembly are bonded via the cathode sealing member, and the membrane-electrode assembly is sandwiched by the anode separator and the cathode separator.

[0076] By adopting such a method, even in the case where there is a region where the gas diffusion layer and the sealing member overlap, it is possible to prevent stress concentration on the structural members of the fuel cell module, thereby suppressing degradation of the polymer electrolyte membrane.

[0077] The following describes a fuel cell module and a fuel cell stack according to each embodiment, and a method for manufacturing a fuel cell module, with reference to the drawings.

[0078] (Implementation Method 1)

[0079] Figure 1 : is an exploded perspective view of the fuel cell stack according to the first embodiment. Figure 1 , a portion of the fuel cell stack is exploded and schematically shown. Figure 2 It is a plan view of a membrane-electrode assembly and a sealing member in a fuel cell module according to the present embodiment. Figure 3 yes Figure 2 AA line cross-sectional view of the membrane-electrode assembly.

[0080] [Overall structure]

[0081] The fuel cell stack 1 according to the present embodiment is, for example, a polymer electrolyte fuel cell (PEFC), which generates electricity, heat, and water simultaneously by electrochemically reacting a fuel gas containing hydrogen and an oxidant gas containing oxygen such as air. Figure 1 As shown, the fuel cell stack 1 includes, for example, a fuel cell module (monomer) 2 as a single cell module, a current collector 3, an end plate 4, and a spring 5. In the fuel cell stack 1, a plurality of fuel cell modules 2 are stacked and connected in series. Figure 1 The figure shows a state where one fuel cell module 2 is disassembled and the remaining fuel cell modules 2 are stacked. Collector plates 3, end plates 4, and springs 5 ​​are installed on the outermost layers at both ends of the fuel cell stack 1. End plates 4 and collector plates 3 arranged on the inner side of the end plates 4 are installed at both ends of the fuel cell stack 1, and a plurality of springs 5 ​​are arranged on the inner surface of the end plates 4, that is, on the surface on the fuel cell module 2 side. The fuel cell stack 1 is fastened with fastening bolts 7 and nuts 8 inserted through bolt holes 6 from both ends.

[0082] Fuel cell module 2 Figure 1 to Figure 3 As shown in the figure, the membrane-electrode assembly 10, the anode separator 11A, the cathode separator 11C, the anode sealing member 9A and the cathode sealing member 9C are provided. The membrane-electrode assembly 10 includes: an anode catalyst layer 16 provided on the first main surface 15a of the polymer electrolyte membrane 15; a cathode catalyst layer 17 provided on the second main surface 15b of the polymer electrolyte membrane 15; an anode gas diffusion layer 18A stacked on the anode catalyst layer 16; and a cathode gas diffusion layer 18C stacked on the cathode catalyst layer 17. The anode separator 11A is arranged on the anode gas diffusion layer 18A side of the membrane-electrode assembly 10. The cathode separator 11C is arranged on the cathode gas diffusion layer 18C side of the membrane-electrode assembly 10, and forms a pair with the anode separator 11A, thereby sandwiching the membrane-electrode assembly 10. The anode sealing member 9A has an opening, and bonds the membrane-electrode assembly 10 and the anode separator 11A. The cathode sealing member 9C has an opening and bonds the membrane-electrode assembly 10 and the cathode separator 11C. A cooling water separator 11W may be disposed outside the anode separator 11A and the cathode separator 11C.

[0083] In addition, in the present embodiment, the membrane-electrode assembly is sometimes referred to as MEA. In addition, the anode sealing member 9A and the cathode sealing member 9C are sometimes referred to as the sealing member 9. In addition, the anode separator 11A, the cathode separator 11C and the cooling water separator 11W are sometimes referred to as the separator 11. In addition, the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C are sometimes referred to as the gas diffusion layer 18.

[0084] <Current Collector Plate>

[0085] The collector plate 3 is arranged outside the stack of the fuel cell module 2. In order to efficiently collect the electricity generated in the fuel cell module 2, the collector plate 3 can be, for example, a collector plate obtained by gold-plating a copper plate. The collector plate 3 can be made of a metal material with good electrical conductivity, such as iron, nickel, stainless steel, or aluminum. In addition, a surface treatment such as tin plating or nickel plating can be applied.

[0086] <End plate>

[0087] The end plate 4 is arranged on the outer side of the collector plate 3. The end plate 4 is formed of, for example, an electrically insulating material and also functions as an insulating plate. The end plate 4 can be formed by injection molding using, for example, a polyphenylene sulfide resin. The piping integrated with the end plate 4 is pushed into the manifold hole 12 of the stack of fuel cell modules 2, for example, via a gasket not shown in the figure. A spring 5 for applying a load to the fuel cell module 2 is arranged on the inner surface of the end plate 4, that is, the surface on the fuel cell module 2 side. The spring 5 is concentrated on the portion that overlaps with the MEA 10 of the fuel cell module 2 when stacked. The fuel cell stack 1 is tightened by tightening the bolts 7 and the nuts 8 so that the force of the spring 5 becomes a given value.

[0088] <Polymer Electrolyte Membrane>

[0089] A solid polymer material showing proton conductivity, such as a perfluorosulfonic acid membrane, can be used as the polymer electrolyte membrane 15. As the perfluorosulfonic acid membrane, for example, a Nafion membrane manufactured by DuPont can be used.

[0090] <Membrane-Electrode Assembly>

[0091] MEA10 has an anode catalyst layer 16 formed mainly of, for example, carbon powder that retains and adsorbs a platinum-ruthenium alloy catalyst, on the first main surface 15a, which is the surface on the anode side of the polymer electrolyte membrane 15 that selectively transports hydrogen ions. In addition, a cathode catalyst layer 17 formed mainly of, for example, carbon powder that retains and adsorbs a platinum catalyst, is formed on the second main surface 15b, which is the surface on the cathode side of the polymer electrolyte membrane 15. An anode gas diffusion layer 18A is stacked on the anode catalyst layer 16, and a cathode gas diffusion layer 18C is stacked on the cathode catalyst layer 17.

[0092] <Gas Diffusion Layer>

[0093] The anode gas diffusion layer 18A is stacked on the anode catalyst layer 16 and has the functions of gas permeability and point electrical conductivity of the fuel gas. In addition, the cathode gas diffusion layer 18C is stacked on the cathode catalyst layer 17 and has the functions of gas permeability and point electrical conductivity of the oxidant gas. For example, carbon paper or carbon cloth is used for the gas diffusion layer 18.

[0094] <Partition>

[0095] The anode separator 11A and the cathode separator 11C are formed in a flat plate shape. The surfaces of the anode separator 11A and the cathode separator 11C that are in contact with the MEA 10, that is, the surfaces of the anode separator 11A and the cathode separator 11C, which will be described later, Figure 8 as well as Fig. 9 The inner surface 11Ai and the inner surface 11Ci shown are formed with fuel gas flow channels 13A and oxidant gas flow channels 13C corresponding to the shape of the MEA 10. The inner surface 11Ai of the anode separator 11A is formed to be aligned with the gas diffusion layer 18A ( Figure 3 The inner surface 11Ci of the cathode separator 11C is formed to contact with the gas diffusion layer 18C ( Figure 3 ) contact. Figure 8 as well as Fig. 9 The outer surfaces 11Ao and 11Co of the anode separator 11A and the cathode separator 11C shown and the both surfaces of the cooling water separator 11W form cooling water flow path grooves 13W.

[0096] The separator 11 is formed of a gas-impermeable conductive material and is obtained by cutting a resin-impregnated carbon material into a predetermined shape, molding a mixture of carbon powder and a resin material, or molding a metal.

[0097] <Sealing member>

[0098] Figure 2 This is a diagram of the MEA 10 and the sealing member 9 viewed from a direction perpendicular to the first main surface 15a. Hereinafter, the direction perpendicular to the first main surface 15a is sometimes referred to as the thickness direction. In addition, the state viewed from a direction perpendicular to the first main surface 15a is sometimes referred to as a top view. Figure 2 As shown in FIG. 1 , an opening 26 is provided in the sealing member 9. The opening 26 is formed in the central portion of the sealing member 9 in the thickness direction. Figure 2 The sealing member 9 uses, for example, a fiber sheet contained in an insulating resin. The fiber sheet contained in the resin in consideration of insulation, heat resistance, and gas permeability may be, for example, a prepreg material in which glass fibers are impregnated with epoxy resin. In addition, the fiber corresponds to strength, thickness, linear expansion coefficient, and contained substances, and for example, inorganic fibers such as ceramic fibers may also be used. In addition, the resin may be other thermosetting resins such as phenolic resin, unsaturated polyester resin, or polyurethane resin. In addition, it may be a structure in which a fiber-containing resin is multi-layered with other resins, or a structure in which the partial composition is different. In the present embodiment, a fiber sheet contained in an insulating resin is used, but an adhesive sheet in which an adhesive layer is formed on both sides of a substrate such as a polyethylene naphthalate film may also be used.

[0099] like Figure 1 as well as Figure 2As shown, manifold holes 12 and bolt holes 6 are respectively provided in the peripheral portion of the separator 11 and the sealing member 9 so as to penetrate in the thickness direction. The manifold hole 12 is a through hole through which the fuel gas, the oxidant gas, and the cooling water flow respectively. When a plurality of fuel cell modules 2 are stacked, the manifold holes 12 of the respective fuel cell modules 2 are stacked and combined to form a fuel gas manifold, an oxidant gas manifold, and a cooling water manifold.

[0100] The anode sealing member 9A is configured to overlap with the anode gas diffusion layer 18A in the thickness direction. In the present embodiment, the anode sealing member 9A is configured to overlap with the anode gas diffusion layer 18A in the thickness direction in the region including the edge 26a on the side of the opening 26. At this time, the portion of the anode sealing member 9A overlapping with the anode gas diffusion layer 18A is referred to as region F1. The cathode sealing member 9C is also configured to overlap with the cathode gas diffusion layer 18C in the region including the edge 26a on the side of the opening 26. In the present embodiment, region F1 is a region from the edge 26a of the opening 26 of the sealing member 9 to a position away from a given length in the surface direction outside when viewed from above, indicating a region where the sealing member 9 overlaps with the gas diffusion layer 18. In addition, the sealing member 9 is configured to cover the outer periphery of the gas diffusion layer 18.

[0101] refer to Figures 4 to 7 To explain in more detail Figure 3 The gas diffusion layer 18 is shown. Figure 4 It is a top view of the cathode gas diffusion layer 18C. Figure 5 It is a top view of the anode gas diffusion layer 18A. Figure 6 The outer periphery of the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C is processed as follows: Figure 4 X1 and Figure 5 X2 magnified image. Figure 7 Another example of processing the outer periphery of the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C is to Figure 4 X1 and Figure 5 The X2 magnified image. Figures 4 to 7 In the figure, some emphasized parts are included for the purpose of explanation.

[0102] When viewed from a direction perpendicular to the first main surface 15a, the cathode gas diffusion layer 18C has a cathode side inner region F2 overlapping with the cathode sealing member 9C in a region including an edge 26Ca on the opening 26C side of the cathode sealing member 9C. Figure 2 The portion corresponding to the region F1 in FIG. 1 is the portion where the cathode sealing member 9C overlaps with the cathode gas diffusion layer 18C. Figure 4As shown in the figure, the cathode gas diffusion layer 18C includes: the outer peripheral portion of the cathode gas diffusion layer 18C including the cathode side inner region F2, namely the first cathode gas diffusion layer 18Ce; and the inner portion of the first cathode gas diffusion layer 18Ce, namely the second cathode gas diffusion layer 18Cd. That is, the first cathode gas diffusion layer 18Ce is the outermost portion in the surface direction of the cathode gas diffusion layer 18C. In addition, the cathode gas diffusion layer 18C has a portion, namely the cathode side inner region F2, which overlaps with the cathode sealing member 9C in the thickness direction at least in a portion of the outer peripheral portion. In the present embodiment, the first cathode gas diffusion layer 18Ce is a portion including the cathode side inner region F2. That is, the cathode sealing member 9C overlaps in the thickness direction at a portion of the first cathode gas diffusion layer 18Ce.

[0103] When viewed from a direction perpendicular to the first main surface 15a, the anode gas diffusion layer 18A has an anode side inner region F3 overlapping with the anode sealing member 9A in a region including the edge 26Aa on the opening portion 26A side of the anode sealing member 9A. Figure 2 The portion corresponding to the region F1 in FIG. 1 is the portion where the anode sealing member 9A overlaps with the anode gas diffusion layer 18A. Figure 5 As shown in the figure, the anode gas diffusion layer 18A includes: the outer peripheral portion of the anode gas diffusion layer 18A including the anode side inner region F3, namely the first anode gas diffusion layer 18Ae; and the inner portion of the first anode gas diffusion layer 18Ae, namely the second anode gas diffusion layer 18Ad. That is, the first anode gas diffusion layer 18Ae is a portion located at the outer peripheral portion of the anode gas diffusion layer 18A. In addition, the anode gas diffusion layer 18A has a portion, namely the anode side inner region F3, overlapping with the anode sealing member 9A in the thickness direction in at least a portion of the outer peripheral portion. In the present embodiment, the first anode gas diffusion layer 18Ae is a portion including the anode side inner region F3. That is, the anode sealing member 9A overlaps in the thickness direction on a portion of the first anode gas diffusion layer 18Ae.

[0104] In addition, the cathode gas diffusion layer 18C has a gap extending through the cathode gas diffusion layer 18C in the thickness direction thereof, at least in a portion including the cathode side inner region F2. Similarly, the anode gas diffusion layer 18A has a gap extending through the anode gas diffusion layer 18A in the thickness direction thereof, at least in a portion including the anode side inner region F3. The gaps formed in the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C are, for example, Figure 6As shown in the figure, the gap 22a is formed by the sawtooth portions 24A and 24C which are formed into a sawtooth shape in a plan view. The sawtooth portions 24A and 24C are portions where a plurality of notches and a plurality of sharp points are formed along the end of the gas diffusion layer 18. In addition, the sawtooth portions 24A and 24C are provided in the first anode gas diffusion layer 18Ae of the anode gas diffusion layer 18A, or the first cathode gas diffusion layer 18Ce of the cathode gas diffusion layer 18C. In the present embodiment, the gap 22a is formed between the sawtooth portions 24A and 24C in the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce. The sawtooth portions 24A and 24C may be provided on the entire periphery of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce.

[0105] In addition, the gaps formed in the gas diffusion layer 18 may be Figure 7 As shown in the figure, a plurality of through holes 22Ab and 22Cb are provided in the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce. The through holes 22Ab and 22Cb are holes that penetrate the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction. The through holes 22Ab and 22Cb can be formed in a circular shape, for example, in a plan view.

[0106] The through hole 22Ab may be, for example, Figure 7 As shown in FIG. 1 , the through holes 22Ab are arranged to be evenly distributed in the first anode gas diffusion layer 18Ae. In addition, the size of the through holes 22Ab can be formed to be larger than the thickness of the first anode gas diffusion layer 18Ae. The through holes 22Cb can also be formed to be Figure 7 As shown in FIG. 1 , the through holes 22Cb are arranged to be evenly distributed in the first cathode gas diffusion layer 18Ce. In addition, the size of the through holes 22Cb can be formed to be larger than the thickness of the first cathode gas diffusion layer 18Ce, for example.

[0107] The second anode gas diffusion layer 18Ad and the second cathode gas diffusion layer 18Cd are portions adjacent to the inner sides of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the surface direction.

[0108] In the present embodiment, the gas diffusion layer 18 is manufactured using a roll-to-roll method, and a process of punching the gas diffusion layer 18 continuously formed in a sheet form with the same composition into a given size is provided to form a gap. For this purpose, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce, and the second anode gas diffusion layer 18Ad and the second cathode gas diffusion layer 18Cd are formed with the same composition. In addition, as a method for processing the gap portion, for example, a method of changing the composition of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce, and the second anode gas diffusion layer 18Ad and the second cathode gas diffusion layer 18Cd when manufacturing the gas diffusion layer 18 can also be adopted.

[0109] In order to prevent the polymer electrolyte membrane 15, the anode catalyst layer 16 and the cathode catalyst layer 17 from being exposed on both the anode and cathode sides of the MEA 10, Figure 8 The sealing member 9 and the gas diffusion layer 18 are arranged as shown. Specifically, the sealing member 9 is arranged so that the cathode sealing member 9C and the cathode side inner region F2 of the cathode gas diffusion layer 18C overlap in the thickness direction, and the anode sealing member 9A and the anode side inner region F3 of the anode gas diffusion layer 18A overlap in the thickness direction. Furthermore, the sealing member 9 is arranged so that the cathode side inner region F2 and the anode side inner region F3 do not overlap in the thickness direction.

[0110] like Figure 8 As shown in FIG. 1 , after the sealing member 9 is disposed on the MEA 10, the MEA 10 and the sealing member 9 are sandwiched between the cathode separator 11C and the anode separator 11A. Fig. 9 As shown in FIG. 1 , by clamping with the separator 11, if a load is applied in the thickness direction, stress is concentrated in the cathode side inner region F2 and the anode side inner region F3 which are the overlapping parts of the gas diffusion layer 18 and the sealing member 9. In the present embodiment, due to the formation of the void, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce are deformed in the surface direction toward the void 22a or the through holes 22Ab and 22Cb, and are compressed in the thickness direction. That is, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce are deformed in the surface direction toward the void 22a or the through holes 22Ab and 22Cb. Figure 6 or Figure 7 Specifically, by receiving a load in the thickness direction, the Figure 6 The first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce of the sawtooth portions 24A and 24C are transformed from the solid line shape to the single-dot chain line shape, so that the gap 22a becomes smaller. Figure 7In the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce, the through hole 22Cb is deformed from the shape of the solid line to the shape of the single-point dashed line, so that the size of the through holes 22Ab and 22Cb is reduced. By deforming the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the surface direction, it becomes difficult to apply force to the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction. For this reason, the stress concentration on the portion where the sealing member 9 and the gas diffusion layer 18 overlap, that is, the anode side inner region F3 and the cathode side inner region F2 can be alleviated. Therefore, the damage of the separator 11 can be prevented.

[0111] Furthermore, if Figure 8 As shown in FIG. 1 , the anode side inner region F3 and the cathode side inner region F2 do not overlap in a plan view, thereby alleviating stress concentration. For example, the anode side inner region F3 and the cathode side inner region F2 can be prevented from overlapping by making the outer dimensions of the anode gas diffusion layer 18A larger than the outer dimensions of the cathode gas diffusion layer 18C.

[0112] The widths of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce of the gas diffusion layer 18 can be determined in consideration of the positional deviation accuracy when the gas diffusion layer 18 and the sealing member 9 are overlapped. Specifically, even if the positional deviation accuracy deteriorates and the deviation amount increases, in order to prevent damage to the separator, it is preferably determined that the gas diffusion layer and the sealing member 9 do not overlap in the portion other than the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce. In addition, in order to prevent degradation or membrane rupture of the polymer electrolyte membrane 15, it is preferably determined that the widths of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce do not generate a gap between the gas diffusion layer and the sealing member 9.

[0113] For example, if the arrangement accuracy of the sealing member relative to the gas diffusion layer 18 is ±0.5 mm, the design is such that even if the overlap size is reduced by 1 mm when the overlap is at its maximum, the overlap area does not disappear. Also, for example, if the overlap is at its minimum at 0.2 mm, the separator can be prevented from being damaged by setting the width of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce to 1.2 mm or more.

[0114] In addition, you can also Fig.10 As shown in FIG. 1 , the area ratio of the anode side inner region F3 to the cathode side inner region F2 is Fig. 9 Since the overlapping area of ​​the sealing member 9 and the gas diffusion layer 18, i.e., the inner region F3 on the anode side and the inner region F2 on the cathode side, is smaller than that of the gas diffusion layer 18, Fig. 9 The situation is smaller than that of Fig.10In the case of Fig.10 In, with Fig. 9 Compared with the case of , the deformation portions of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce are smaller. Fig.10 In this way, even if the size of the anode side inner region F3 and the cathode side inner region F2 is reduced, Fig. 9 In the same manner as in the case of FIG. 1 , the gap between the gas diffusion layer 18 and the sealing member 9 is eliminated.

[0115] [Manufacturing method]

[0116] Next reference Fig.11 A method for manufacturing the fuel cell module 2 will be described. Fig.11 FIG. 2 is an exemplary flow chart of a method for manufacturing a fuel cell module 2. Fig.11 As shown, the method for manufacturing the fuel cell module 2 includes a preparation step ST10 , a gas diffusion layer processing step ST20 , a placement step ST30 , and a bonding step ST40 .

[0117] In the preparation step ST10, the polymer electrolyte membrane 15 having the anode catalyst layer 16 on the first main surface 15a and the cathode catalyst layer 17 on the second main surface 15b, the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C are prepared. In addition, the anode separator 11A and the cathode separator 11C, the anode sealing member 9A and the cathode sealing member 9C are prepared.

[0118] In the gas diffusion layer processing step ST20, a gap is formed in at least a portion of the outer periphery of the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C. For example, the gap is formed in at least a portion of the outer periphery of each of the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C by punching. The gap may be Figure 6 The sawtooth portions 24A and 24C shown. Alternatively, Figure 7 The through hole shown.

[0119] In the arrangement step ST30, the anode gas diffusion layer 18A is stacked on the anode catalyst layer 16 side of the polymer electrolyte membrane 15, and the cathode gas diffusion layer 18C is stacked on the cathode catalyst layer 17 side to form the membrane-electrode assembly 10. In addition, the anode sealing member is arranged so as to overlap with at least a portion of the outer periphery of the anode gas diffusion layer 18A, and the cathode sealing member 9C is arranged so as to overlap with at least a portion of the outer periphery of the cathode gas diffusion layer 18C.

[0120] In the bonding step ST40, the anode gas diffusion layer 18A and the anode separator 11A of the membrane-electrode assembly 10 are bonded via the anode sealing member 9A, and the cathode gas diffusion layer 18C and the cathode separator 11C of the membrane-electrode assembly 10 are bonded. In this way, the gas diffusion layer 18 and the separator 11 are bonded by the sealing member 9, so that the membrane-electrode assembly 10 is sandwiched by the anode separator 11A and the cathode separator 11C. The MEA 10 is sandwiched by the anode separator 11A and the cathode separator 11C and heated, so that the MEA 10 and the separator 11 are bonded.

[0121] As described above, the fuel cell module 2 according to the present embodiment is manufactured through the preparation step ST10, the gas diffusion layer processing step ST20, the placement step ST30, and the bonding step ST40. The fuel cell stack 1 is completed by stacking and fastening the fuel cell modules 2 manufactured in this way.

[0122] [Effect]

[0123] The fuel cell module 2 involved in the present embodiment 1 includes a membrane-electrode assembly 10, a separator 11, and a sealing member 9. The membrane-electrode assembly 10 includes a polymer electrolyte membrane 15, an anode catalyst layer 16, a cathode catalyst layer 17, an anode gas diffusion layer 18A stacked on the anode catalyst layer 16, and a cathode gas diffusion layer 18C stacked on the cathode catalyst layer 17. The anode catalyst layer 16 is provided on the first main surface 15a of the polymer electrolyte membrane 15. The cathode catalyst layer 17 is provided on the second main surface 15b of the polymer electrolyte membrane 15. The anode separator 11A and the cathode separator 11C sandwich the membrane-electrode assembly 10 as a pair of separators 11. In a plan view in which the sealing member 9 adheres the membrane-electrode assembly 10, the anode separator 11A, and the cathode separator 11C, respectively, an opening 26 is provided in the sealing member 9. The anode gas diffusion layer 18A and the anode sealing member 9A overlap in the anode side inner region F3 including the edge 26a of the opening portion 26 of the anode sealing member 9A. In addition, the cathode gas diffusion layer 18C and the cathode sealing member 9C overlap in the cathode side inner region F2 including the edge 26a of the opening portion 26 of the cathode sealing member 9C. The anode gas diffusion layer 18A forms a void penetrating in the thickness direction in a portion including at least the anode side inner region F3, and the cathode gas diffusion layer 18C forms a void penetrating in the thickness direction in a portion including at least the cathode side inner region F2.

[0124] According to this structure, by forming the voids penetrating in the thickness direction in a portion of the first anode gas diffusion layer 18Ae including at least the anode side inner region F3, the voids 22a or the through holes 22Ab for deforming the first anode gas diffusion layer 18Ae in the plane direction can be formed. Similarly, by forming the voids penetrating in the thickness direction in a portion of the first cathode gas diffusion layer 18Ce including at least the cathode side inner region F2, the voids 22a or the through holes 22Cb for deforming the first cathode gas diffusion layer 18Ce in the plane direction can be formed. Thus, when a load is applied to the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce can be deformed toward the voids 22a or the through holes 22Ab and 22Cb. Therefore, even when a load is applied in a state where the gas diffusion layer 18 and the sealing member 9 overlap in the thickness direction, stress concentration on the anode side inner region F3 and the cathode side inner region F2, which are overlapping regions, can be prevented. As a result, even in the case where the outer periphery of the gas diffusion layer 18 and the sealing member 9 overlap the anode side inner region F3 and the cathode side inner region F2, stress concentration on the anode side inner region F3 and the cathode side inner region F2 can be prevented, thereby suppressing degradation of the polymer electrolyte membrane 15. In addition, since there is a region where the gas diffusion layer 18 overlaps with the sealing member 9, exposure of the anode catalyst layer 16 and the cathode catalyst layer 17 can be prevented.

[0125] Furthermore, a plurality of through holes 22Ab and 22Cb penetrating in the thickness direction are provided in the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce.

[0126] According to this structure, when a load is applied to the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce deform in the direction of reducing the pore diameters of the through holes 22Ab and 22Cb, thereby dispersing the stress.

[0127] In addition, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce are provided with serrations 24A and 24C formed in a serration shape in a plan view.

[0128] According to this structure, when a load is applied to the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction, the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce deform toward the gaps 22a between the serrations 24A and 24C, thereby dissipating the stress.

[0129] In addition, the fuel cell stack 1 according to the first embodiment is a stack of a plurality of fuel cell modules 2 connected in series.

[0130] According to this structure, it is possible to prevent stress concentration on the structural members of the fuel cell stack 1 .

[0131] In addition, the manufacturing method of the fuel cell module 2 involved in the present embodiment 1 includes a preparation step ST10, a gas diffusion layer processing step ST20, a configuration step ST30 and a bonding step ST40. In the preparation step ST10, a polymer electrolyte membrane 15 provided with an anode catalyst layer 16 and a cathode catalyst layer 17, a gas diffusion layer 18, a sealing member 9, and a separator 11 are prepared. In the gas diffusion layer processing step ST20, a gap is formed in at least a portion of the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce. In the configuration step ST30, the sealing member 9 is configured on the MEA 10 so that the outer periphery of the gas diffusion layer 18 overlaps with the sealing member 9 at least in part. In the bonding step ST40, the MEA 10 and the sealing member 9 are sandwiched by the separator 11, and the MEA 10 and the separator 11 are bonded by the sealing member 9.

[0132] According to this manufacturing method, even when the outer periphery of the gas diffusion layer 18 overlaps the sealing member 9 , stress concentration on the structural members of the fuel cell module 2 can be prevented, thereby suppressing degradation of the polymer electrolyte membrane 15 .

[0133] In addition, the present disclosure is not limited to the above-mentioned embodiment 1, and can also be implemented in various other ways. In the above-mentioned embodiment, the structure in which the outer dimensions of the anode gas diffusion layer 18A are larger than the cathode gas diffusion layer 18C and the cathode side inner region F2 and the anode side inner region F3 do not overlap in the thickness direction is illustrated, but the structure of the fuel cell module 2 is not limited to this. For example, the fuel cell module 2 can also be a structure in which the outer dimensions of the cathode gas diffusion layer 18C are larger than the anode gas diffusion layer 18A. Through this structure, it is also possible to prevent stress concentration on the structural components of the fuel cell module 2 in the case of a portion where the outer periphery of the gas diffusion layer 18 overlaps with the sealing member 9, thereby suppressing the degradation of the polymer electrolyte membrane 15.

[0134] Furthermore, although the cavities are formed in the first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce by punching, the processing method is not limited thereto as long as the cavities are formed in at least a part of the outer periphery of the gas diffusion layer 18 .

[0135] In addition, the first cathode gas diffusion layer 18Ce and the first anode gas diffusion layer 18Ae form sawtooth-shaped gaps, i.e., sawtooth portions 24C and 24A, when viewed from above, but the shape of the gaps is not limited thereto. For example, the gaps may be formed by bending along the outer circumference of the first cathode gas diffusion layer 18Ce and the first anode gas diffusion layer 18Ae. In this case, even when a load is applied in a state where the gas diffusion layer 18 and the sealing member 9 overlap in the thickness direction, stress concentration on the structural members of the fuel cell module 2 can be prevented.

[0136] In addition, the through holes 22Ab and 22Cb are formed in a circular shape in a plan view, but the shapes of the through holes 22Ab and 22Cb are not limited thereto. For example, the through holes 22Ab and 22Cb may be other shapes such as an ellipse or a polygon in a plan view.

[0137] In addition, the first anode gas diffusion layer 18Ae and the anode sealing member 9A, and the first cathode gas diffusion layer 18Ce and the cathode sealing member 9C partially overlap, but the present invention is not limited thereto. For example, the anode sealing member 9A and the cathode sealing member 9C may overlap the entire first anode gas diffusion layer 18Ae and the first cathode gas diffusion layer 18Ce in the thickness direction when viewed from above. That is, the anode side inner region F3 and the first anode gas diffusion layer 18Ae, and the cathode side inner region F2 and the first cathode gas diffusion layer 18Ce may coincide with each other when viewed from above.

[0138] (Implementation Method 2)

[0139] A fuel cell module according to Embodiment 2 of the present disclosure is described. In Embodiment 2, the differences from Embodiment 1 are mainly described. In Embodiment 2, the same or equivalent structures as those in Embodiment 1 are described by being denoted by the same reference numerals. In Embodiment 2, the descriptions that overlap with those in Embodiment 1 are omitted.

[0140] In the first embodiment, the cathode gas diffusion layer 18C and the anode gas diffusion layer 18A are changed in the outer dimensions so that the cathode side inner region F2 and the anode side inner region F3 do not overlap. In the second embodiment, the anode gas diffusion layer 18A and the cathode gas diffusion layer 18C are changed in the shapes so that the anode side inner region F3 and the cathode side inner region F2 do not overlap.

[0141] Fig.12 It is a plan view of cathode sealing member 9C in fuel cell module 2 according to Embodiment 2. Fig.13 It is a plan view of anode sealing member 9A in fuel cell module 2 according to Embodiment 2. Fig.14It is a plan view of a cathode gas diffusion layer 18C according to the second embodiment. Fig.15 It is a plan view of an anode gas diffusion layer 18A in a fuel cell module 2 according to Embodiment 2.

[0142] like Fig.12 as well as Fig.13 As shown in the figure, an opening 26C is provided in the cathode sealing member 9C, and an opening 26A is provided in the anode sealing member 9A. The opening 26C provided in the cathode sealing member 9C is a polygonal shape in which two vertices 28a and 28c facing each other are arranged outside the square 27C serving as a reference. In addition, the opening 26A provided in the anode sealing member 9A is a polygonal shape in which two vertices 29b and 29d facing each other are arranged outside the square 27A serving as a reference. The openings 26C and 26A are formed so that when the cathode sealing member 9C and the anode sealing member 9A are overlapped, the squares 27C and 27A overlap, but the vertices 28a to 28d and the vertices 29a to 29d among the vertices of the openings 26C and 26A do not overlap, respectively.

[0143] The cathode sealing member 9C covers the outer periphery of the cathode gas diffusion layer 18C, so that the portion of the edge 26Ca of the opening 26C in the region F1C of the cathode sealing member 9C overlaps with the cathode gas diffusion layer 18C in the thickness direction. Similarly, the portion of the edge 26Aa of the opening 26A in the region F1A of the anode sealing member 9A covers the outer periphery of the anode gas diffusion layer 18A. In this case, it is preferable to set the configuration such that the inner region F3 on the anode side and the inner region F2 on the cathode side do not overlap when viewed from above. For example, if Fig.13 As shown, by providing the region F1A of the anode sealing member 9A as a plurality of individually provided regions rather than a continuous region, it is possible to achieve a configuration in which the anode side inner region F3 and the cathode side inner region F2 do not overlap.

[0144] like Fig.14 as well as Fig.15As shown in FIG. 1 , the cathode gas diffusion layer 18C has the same shape as the opening 26C of the cathode sealing member 9C, but is formed larger than the opening 26C. In addition, the cathode gas diffusion layer 18C includes: a first cathode gas diffusion layer 18Ce, which is the outer peripheral portion thereof; and a second cathode gas diffusion layer 18Cd, which is the inner portion of the first cathode gas diffusion layer 18Ce. The anode gas diffusion layer 18A has the same shape as the opening 26A of the anode sealing member 9A, but is formed larger than the opening 26A. In addition, the anode gas diffusion layer 18A includes: a first anode gas diffusion layer 18Ae, which is the outer peripheral portion thereof; and a second anode gas diffusion layer 18Ad, which is the inner portion of the first anode gas diffusion layer 18Ae. The first cathode gas diffusion layer 18Ce has a cathode side inner region F2, which is a portion overlapping with the cathode sealing member 9C. In addition, the anode side inner region F3 of the first anode gas diffusion layer 18Ae is four discontinuous individual regions, similar to the region F1A of the anode sealing member 9A. like Fig.15 As shown, when viewed from a direction perpendicular to the first main surface 15 a , the anode side inner region F3 has an outer portion F31 located outside the cathode side inner region F2 and an inner portion F32 located inside the cathode side inner region F2 .

[0145] For example, a first cathode gas diffusion layer 18Ce and a first anode gas diffusion layer 18Ae are formed with Figure 6 That jagged, or Figure 7 The cathode gas diffusion layer 18C and the cathode sealing member 9C overlap within the range of region F1C, taking into account the assembly tolerance. Similarly, the anode gas diffusion layer 18A and the anode sealing member 9A overlap within the range of region F1A. Figure 12 to Figure 15 Such a shape is configured so that the anode side inner region F3 and the cathode side inner region F2 do not overlap in a plan view.

[0146] Fig.16 2 is a cross-sectional view of a fuel cell module 2 in Embodiment 2. The anode sealing member 9A and the cathode sealing member 9C are portions that are in contact with the fuel gas flow path groove 13A and the oxidant gas flow path groove 13C when the anode separator 11A and the cathode separator 11C are bonded. The sealing member 9 uses a fiber sheet that is contained by an insulating resin, but it is possible that the resin of the anode sealing member 9A melts and blocks the fuel gas flow path groove 13A. For this purpose, the resin of the portion of the anode sealing member 9A that is in contact with the fuel gas flow path groove 13A, i.e., the pre-hardened portion 9Ae, can be pre-hardened. At this time, if the region where the cathode sealing member 9C overlaps with the cathode gas diffusion layer 18C, i.e., the cathode side inner region F2, is located further inward in the surface direction than the pre-hardened portion 9Ae, the concentration of stress can be suppressed.

[0147] On the other hand, a pre-hardened portion (not shown) is also provided at the portion where the cathode sealing member 9C and the oxidant gas flow channel 13C are in contact. In this case, the anode side inner region F3 is preferably located inside the pre-hardened portion of the cathode sealing member 9C.

[0148] The fuel cell module 2 according to the second embodiment has an anode-side inner region F3 of the anode gas diffusion layer 18A, when viewed from a direction perpendicular to the first main surface 15a, an outer portion F31 located outside the cathode-side inner region F2 of the cathode gas diffusion layer 18C, and an inner portion F32 located inside the cathode-side inner region F2 of the cathode gas diffusion layer 18C. That is, when viewed from a direction perpendicular to the first main surface 15a, there is no region where the anode-side inner region F3 and the cathode-side inner region F2 overlap.

[0149] According to this structure, even if the positions of the structural members are deviated during assembly, the cathode gas diffusion layer 18C and the cathode sealing member 9C, and the anode gas diffusion layer 18A and the anode sealing member 9A do not overlap when viewed from above, thereby preventing damage to the structural members of the fuel cell module 2 due to stress concentration.

[0150] In addition, in the present embodiment, the region F1A of the anode sealing member 9A and the anode side inner region F3 are set as discontinuous individual regions, but the region F1C of the cathode sealing member 9C and the cathode side inner region F2 may also be set as the same structure. That is, the cathode side inner region F2 may have an outer portion located outside the anode side inner region F3 and an inner portion located inside the anode side inner region F3.

[0151] In the present embodiment, the shapes of the opening 26A of the anode sealing member 9A and the opening 26C of the cathode sealing member 9C are polygonal, but the shapes of the openings 26A and 26C are not limited thereto and may be, for example, elliptical.

[0152] (Implementation 3)

[0153] A fuel cell module according to Embodiment 3 of the present disclosure will be described. Fig.17 This is a plan view of the MEA 100 and the sealing member 90 in the fuel cell module 20 as viewed from the outside in the thickness direction. Fig.18 yes Fig.17 AA line cross-sectional view of MEA100. Fig.17 A top view of Fig.18 The partial cross-sectional view shows the structure of MEA 100 in which a sealing member 90 is provided at the peripheral edge of separator 110 and MEA 100. Fig.17In the embodiment, the sealing member 90 having the bolt holes 60 and the manifold hole 120 is arranged so that the outer edge of the MEA 100 is not exposed.

[0154] The sealing member 90 is arranged to overlap with at least one of the gas diffusion layers 180A and 180C in the thickness direction. Specifically, the sealing member 90 is arranged to overlap with at least one of the gas diffusion layers 180A and 180C in the thickness direction in the region including the edge of the central side of the sealing member 90. Here, the edge of the central side of the sealing member 90 refers to the edge of the gas diffusion layer 180 side (the central side of the gas diffusion layer 180) configured in the surface direction of the sealing member 90. In the present embodiment, the sealing member 90 covers the outer periphery of the gas diffusion layer 180 so that the region F4 including the edge 260a of the opening 260 overlaps with the gas diffusion layer 180 in the thickness direction. In the present embodiment, the region F4 represents the region from the edge 260a of the opening 260 to the position of a given length away from the outside in the surface direction when viewed from above.

[0155] use Fig.19 The cross-sectional view of FIG. 1 shows a schematic structure of a fuel cell module 20 in this embodiment. Fig. 20 The details of the boundary between the gas diffusion layer 180 and the sealing member 90 are shown in a schematic cross section of the outer periphery of one of the stacked fuel cell modules 20 .

[0156] In order to prevent the polymer electrolyte membrane 150 and the catalyst layers 160 and 170 from being exposed on at least one side, for example Fig. 20 As shown in FIG. 1 , the cathode sealing member 90C and the cathode gas diffusion layer 180C are overlapped in the thickness direction of the fuel cell module 20. The structure of the case where the cathode gas diffusion layer 180C overlaps the cathode sealing member 90C is described below. As for the case where the anode gas diffusion layer 180A overlaps the sealing member 90A, since it is the same structure as the cathode gas diffusion layer 180C, the description is omitted here.

[0157] exist Fig. 20 In the state, if Fig.19 As shown in the cross-sectional view of FIG. 1 , the cathode separator 110C and the anode separator 110A are clamped. Before the MEA 100 is clamped by the cathode separator 110C and the anode separator 110A, the outer periphery of the cathode gas diffusion layer 180C is processed to form a space along the outer periphery. Thus, when a load is applied in the stacking direction, stress concentration at the portion where the cathode sealing member 90C and the cathode gas diffusion layer 180C overlap and damage to the cathode separator 110C can be prevented.

[0158] As a method for processing the outer peripheral portion of the cathode gas diffusion layer 180C, for example, there is a method of changing the composition of the outer peripheral portion and the rest of the cathode gas diffusion layer 180C when manufacturing the cathode gas diffusion layer 180C. In the present embodiment, in order to apply to a roll-to-roll process in which the cathode gas diffusion layer 180C is continuously manufactured in a sheet form, a method of processing the outer peripheral portion in a process of punching a portion continuously formed in a sheet form with the same composition into a predetermined size is used.

[0159] Next, use Figure 21 to Figure 23 The cathode gas diffusion layer 180C (gas diffusion layer 180 ) will be described in detail. Fig.21 180C is a top view of the cathode gas diffusion layer 180C. Fig. 22 When the outer periphery of the cathode gas diffusion layer 180C is processed into a sawtooth shape Fig.21 An enlarged view of the X3 section. Fig.23 This is when the through hole 220b is processed in the outer periphery of the cathode gas diffusion layer 180C. Fig.21 In addition, Figure 21 to Figure 23 Some parts are emphasized for the purpose of explanation.

[0160] The cathode gas diffusion layer 180C and the region F4 ( Fig.17 ) is cut through in the thickness direction. Here, the cathode gas diffusion layer 180C corresponding to the region F4 ( Fig.17 ) indicates an inner region F5 located inwardly (on the polymer electrolyte membrane 150 side) of the region F4 in the thickness direction of the cathode gas diffusion layer 180C. The inner region F5 is a region including spaces 220a and 220b described later.

[0161] like Fig.21 As shown, the cathode gas diffusion layer 180C (gas diffusion layer 180) includes a first diffusion layer 180Ce and a second diffusion layer 180Cd.

[0162] The first diffusion layer 180Ce is formed on the periphery of the cathode gas diffusion layer 180C. Specifically, the first diffusion layer 180Ce is the outermost portion of the cathode gas diffusion layer 180C in the surface direction. More specifically, the first diffusion layer 180Ce is a portion of the cathode gas diffusion layer 180C having spaces 220a and 220b, which are described later, formed along the periphery. The cathode gas diffusion layer 180C is configured to overlap with the sealing member 90C in the thickness direction at least in a portion of the periphery. In the present embodiment, the first diffusion layer 180Ce includes an inner region F5 in a portion of the peripheral region. That is, in a portion of the first diffusion layer 180Ce, the sealing member 90A overlaps in the thickness direction. The first diffusion layer 180Ce is configured to overlap with the sealing member 90C when the MEA 100 and the sealing members 90A and 90C are sandwiched by a pair of separators 110A and 110C (refer to Fig. 20 ).

[0163] The second diffusion layer 180Cd is a portion adjacent to the inner side of the first diffusion layer 180Ce in the plane direction. In the present embodiment, the first diffusion layer 180Ce and the second diffusion layer 180Cd are formed with the same composition.

[0164] The first diffusion layer 180Ce is located in the inner region F5 ( Fig.19 ) are provided with a gap. The first diffusion layer 180Ce is, for example, Fig. 22 As shown in FIG. 1 , the inner region F5 has a sawtooth portion 240 formed in a sawtooth shape in a plan view. In the first diffusion layer 180Ce, a space 220a is formed between the sawtooth portions 240. In the present embodiment, the sawtooth portion 240 is provided on the entire periphery of the first diffusion layer 180Ce. Here, the so-called plan view refers to a state when viewed from the thickness direction.

[0165] The first diffusion layer 180Ce may be, for example, Fig.23 As shown, in the inner area F5 ( Fig.19 ) has a plurality of through holes (spaces) 220b. The through holes 220b are holes that penetrate the first diffusion layer 180Ce in the thickness direction. The through holes 220b are formed, for example, in a circular shape when viewed from above. The through holes 220b are provided, for example, in the first diffusion layer 180Ce in the same manner along the outer circumference.

[0166] When the outer peripheral portion of the cathode gas diffusion layer 180C (first diffusion layer 180Ce) and the cathode sealing member 90C are overlapped, pressed, and fastened, a load is applied to the first diffusion layer 180Ce in the thickness direction. Fig. 22 or Fig.23 As shown in FIG. 1 , the first diffusion layer 180Ce is easily deformed and compressed in the surface direction toward the spaces 220a and 220b (for example, in the direction of the arrow). Fig. 22 as well as Fig.23 In FIG. 1 , the solid line indicates the outer edge of the first diffusion layer 180Ce before deformation, and the dashed line indicates the outer edge of the first diffusion layer 180Ce after deformation. Fig. 22 In the embodiment, the first diffusion layer 180Ce is deformed to narrow the space 220a between the sawtooth portions 240. Fig.23 In the embodiment, the first diffusion layer 180Ce is deformed toward the inside of the through hole 220b to reduce the size of the through hole 220b. Since the first diffusion layer 180Ce is deformed in the surface direction, it becomes difficult to apply force to the first diffusion layer 180Ce in the thickness direction. Therefore, stress concentration can be relieved at the portion where the cathode sealing member 90C overlaps with the cathode gas diffusion layer 180C. Thus, damage to the cathode separator 110C can be prevented.

[0167] Thus, in the fuel cell module 20 according to the present embodiment, even if the outer peripheral portion of the cathode gas diffusion layer 180C (first diffusion layer 180Ce) and the cathode sealing member 90C are overlapped, pressed and fastened, damage to the member due to stress concentration can be prevented, thereby preventing the catalyst layer from being exposed.

[0168] In addition, the width of the processing of the outer peripheral portion of the cathode gas diffusion layer 180C is determined in consideration of the positional deviation accuracy when the cathode gas diffusion layer 180C and the cathode sealing member 90C are overlapped. Specifically, in order to prevent damage to the member even if the positional deviation accuracy deteriorates and the deviation amount increases, the processing width is determined so that the cathode gas diffusion layer 180C and the cathode sealing member 90C do not overlap in the portion not subjected to processing. In addition, in order to prevent degradation, membrane rupture, etc. of the polymer electrolyte membrane 150, the processing width is determined so that no gap is generated between the cathode gas diffusion layer 180C and the cathode sealing member 90C.

[0169] For example, if the arrangement accuracy of the cathode sealing member 90C relative to the cathode gas diffusion layer 180C is set to ±0.5 mm, the overlapping area will not disappear even if the overlapping size is reduced by 1 mm for the case where the overlap is the largest. In addition, for example, if the overlap is the smallest, it is possible to prevent damage to the member by processing the outer periphery above 1.2 mm.

[0170] If the case where the overlap is the largest is set as the aforementioned Fig.19 , then in Fig.24 The schematic cross-sectional view shows the case where the overlap is minimized. Although the deformation of the cathode gas diffusion layer 180C is smaller than that of the case where the overlap is maximized, the gap in the surface direction between the cathode gas diffusion layer 180C and the sealing member 90 can be eliminated in either case.

[0171] Next, use Fig.25 A method of manufacturing the fuel cell module 20 will be described. Fig.25 FIG. 2 is a flow chart showing an exemplary method of manufacturing the fuel cell module 20. Fig.25 As shown, the method for manufacturing the fuel cell module 20 includes a preparation step ST100 , a gas diffusion layer processing step ST200 , a placement step ST300 , and a bonding step ST400 .

[0172] In the preparation step ST100 , the polymer electrolyte membrane 150 provided with the anode catalyst layer 160 and the cathode catalyst layer 170 , the pair of gas diffusion layers 180A and 180C, the pair of sealing members 90A and 90C, and the pair of separators 110A and 110C are prepared.

[0173] In the gas diffusion layer processing step ST200, the volume of at least one of the gas diffusion layers 180 (e.g., the cathode gas diffusion layer 180C) out of the pair of gas diffusion layers 180A and 180C is reduced. The volume of at least one of the gas diffusion layers 180 is reduced by punching, for example. For example, when punching into a rectangular shape, such as Fig. 22 As shown in the figure, the volume can be reduced by cutting off the outer periphery into a serrated shape. Alternatively, Fig.23 As shown, during punching, for example, a plurality of through holes 220b are provided around the entire periphery to reduce the volume.

[0174] In the arrangement step ST300 , the MEA 100 including the pair of gas diffusion layers 180A and 180C and the sealing member 90 are arranged so that at least a portion of the outer periphery of at least one of the gas diffusion layers 180 overlaps with the sealing member 90 in the thickness direction.

[0175] In the bonding step ST400 , the sealing members 90A and 90C and the MEA 100 are sandwiched between the pair of separators 110A and 110C, and the MEA 100 and the pair of separators 110A and 110C are bonded to each other.

[0176] The processing for reducing the volume of a part of the outer periphery of the cathode gas diffusion layer 180C is performed as described above. Then, the MEA 100 including the cathode gas diffusion layer 180C and the cathode sealing member 90C are arranged so that the first diffusion layer 180Ce of the cathode gas diffusion layer 180C overlaps with the sealing member 90 in the thickness direction. Then, the sealing member 90 and the MEA 100 are sandwiched by the separator 110 (the anode separator 110A and the cathode separator 110C) and heated, thereby bonding the MEA and the separator 110. Thus, the fuel cell module 20 involved in this embodiment is manufactured.

[0177] The fuel cell modules 20 formed in this way are stacked and fastened to complete a fuel cell stack.

[0178] The fuel cell module according to the present embodiment includes a membrane-electrode assembly 100, a pair of separators 110A, 110C, and a sealing member 90. The membrane-electrode assembly 100 includes: a polymer electrolyte membrane 150; an anode catalyst layer 160; a cathode catalyst layer 170; and a pair of gas diffusion layers 180A, 180C, one of which is stacked on the anode catalyst layer 16 and the other is stacked on the cathode catalyst layer 170. The anode catalyst layer 160 is provided on the first main surface of the polymer electrolyte membrane 150. The cathode catalyst layer 170 is provided on the second main surface of the polymer electrolyte membrane 150. The pair of separators 110A, 110C sandwich the membrane-electrode assembly 100. The sealing member 90 bonds the membrane-electrode assembly 100 and the pair of separators 110A, 110C, respectively. In a plan view, the sealing member 90 is provided with an opening 260, and the gas diffusion layer 180 of one of the pair of gas diffusion layers 180A and 180C and the sealing member 90 overlap in the thickness direction in a region F4 including an edge 260a of the opening 260. A portion of the portion (inner region F5) corresponding to the region F4 of the gas diffusion layer 180 is cut through in the thickness direction.

[0179] According to this structure, by cutting through a part of the inner region F5 in the thickness direction, it is possible to form spaces 220a, 220b for the first diffusion layer 180Ce to deform in the surface direction. Thus, when a load is applied to the first diffusion layer 180Ce in the thickness direction, the first diffusion layer 180Ce can deform toward the spaces 220a, 220b. Thus, even when a load is applied in a state where the gas diffusion layer 180 and the sealing member 90 overlap in the thickness direction, stress concentration on the structural member can be prevented. As a result, even when the outer periphery of the gas diffusion layer 180 and the sealing member 90 overlap, stress concentration on the structural member can be prevented, thereby suppressing the degradation of the polymer electrolyte membrane 150.

[0180] In addition, a portion (inner region F5 ) of the gas diffusion layer 180 corresponding to the region F4 is provided with a plurality of through holes 220 b penetrating in the thickness direction.

[0181] According to this structure, when a load is applied to the first diffusion layer 180Ce in the thickness direction, the first diffusion layer 180Ce can be deformed toward the through hole 220b.

[0182] In addition, a serration portion 240 formed in a serration shape in a plan view is provided in a portion (inner region F5 ) corresponding to the region F4 in one gas diffusion layer 180 .

[0183] According to this structure, when a load is applied to the first diffusion layer 180Ce in the thickness direction, the first diffusion layer 180Ce can be deformed toward the space 220 a between the sawtooth portions 240 .

[0184] Furthermore, the fuel cell stack according to the present embodiment includes a plurality of fuel cell modules 20 .

[0185] According to this structure, it is possible to prevent stress concentration on the members of the fuel cell stack.

[0186] In addition, the manufacturing method of the fuel cell module according to the present embodiment includes a processing step ST200, a placement step ST300, and a bonding step ST400. In the processing step ST200, the volume of at least a portion of the outer periphery of at least one of the pair of gas diffusion layers 180A and 180C is reduced. In the placement step ST300, the membrane-electrode assembly 100 including the pair of gas diffusion layers 180A and 180C and the sealing member 90 are placed so that at least a portion of the outer periphery of at least one of the gas diffusion layers 180 overlaps with the sealing member 90 in the thickness direction. In the bonding step ST400, the sealing member 90 and the membrane-electrode assembly 100 are sandwiched by a pair of separators 110A and 110C, and the membrane-electrode assembly 100 and the pair of separators 110A and 110C are bonded.

[0187] According to this manufacturing method, even when the outer peripheral portion of the gas diffusion layer 180 overlaps with the sealing member 90 , stress concentration on the structural member can be prevented, thereby suppressing degradation of the polymer electrolyte membrane 150 .

[0188] In addition, the present invention is not limited to the above-described embodiment and can be implemented in various other ways. In the above-described embodiment, the structure in which the cathode gas diffusion layer 180C and the cathode sealing member 90C are overlapped on the cathode side is described as an example, but the fuel cell module 20 is not limited thereto. The fuel cell module 20 can also be configured to have a structure in which the anode gas diffusion layer 180A and the anode sealing member 90A are overlapped on the anode side. Specifically, a portion of the portion corresponding to the region F4 can be cut through in the thickness direction in the anode gas diffusion layer 180A. Through this structure, even if the outer periphery of the gas diffusion layer 180 overlaps with the sealing member 90, stress concentration on the structural member can be prevented, thereby suppressing the degradation of the polymer electrolyte membrane 150.

[0189] In addition, a portion of the portion corresponding to the region F4 may be cut through in the thickness direction of both the anode gas diffusion layer 180A and the cathode gas diffusion layer 180C. With this structure, even when the outer periphery of the gas diffusion layer 180 overlaps with the sealing member 90, stress concentration on the structural member can be prevented, thereby suppressing the degradation of the polymer electrolyte membrane 150.

[0190] In addition, at least one of the gas diffusion layers 180 is punched to reduce the volume of at least a portion of the outer peripheral portion. However, the method is not limited to punching as long as the volume of at least a portion of the outer peripheral portion can be reduced.

[0191] In addition, the first diffusion layer 180Ce is provided with the sawtooth portion 240 formed in a sawtooth shape in a plan view, but the present invention is not limited to this as long as at least one of the pair of gas diffusion layers 180A and 180C has a portion corresponding to the region F4 cut through in the thickness direction. The first diffusion layer 180Ce may be formed, for example, by bending in the surface direction along the outer periphery. With this structure, even when a load is applied when the gas diffusion layers 180A and 180C and the sealing members 90A and 90C overlap in the thickness direction, it is possible to prevent stress concentration on the structural member.

[0192] In addition, the through hole 220b is formed in a circular shape in a plan view, but the present invention is not limited thereto. The through hole 220b may also be in other shapes such as an ellipse or a polygon in a plan view.

[0193] In addition, the sealing member 90A overlaps a portion of the first diffusion layer 180Ce in the thickness direction, but the sealing member 90A may overlap the entire first diffusion layer 180Ce in the thickness direction in a plan view. That is, in a plan view, the inner edge ( Fig.21 The two-dot chain line) and the inner edge of the first diffusion layer 180Ce ( Fig.21 The dotted line) is consistent.

[0194] Industrial Applicability

[0195] According to the fuel cell module, fuel cell stack, and fuel cell module manufacturing method disclosed herein, external leakage or cross leakage of fuel gas and oxidant gas can be suppressed, and a highly durable thin fuel cell module can be realized. Therefore, the fuel cell is useful as a portable power source, a power source for electric vehicles, or a fuel cell used in a home cogeneration system, etc.

[0196] Description of Reference Numerals

[0197] 1 Fuel cell stack

[0198] 2.20 Fuel cell module (monomer)

[0199] 3. Collector plate

[0200] 4 End plate

[0201] 5 Spring

[0202] 6, 60 bolt holes

[0203] 7 Fastening bolts

[0204] 8 Nut

[0205] 9, 90 Sealing components

[0206] 9A, 90A anode sealing components

[0207] 9C, 90C cathode sealing component

[0208] 9Ae Pre-hardened part

[0209] 10, 100 MEA (Membrane-Electrode Assembly)

[0210] 11.110 Partition

[0211] 11A, 110A anode separator

[0212] 11C, 110C cathode separator

[0213] 12, 120 manifold holes

[0214] 13 Gas flow channel

[0215] 13A Fuel gas flow channel

[0216] 13C Oxidant gas flow channel

[0217] 13W Cooling water flow channel

[0218] 15, 150 Polymer electrolyte membrane

[0219] 16.160 Anode catalyst layer

[0220] 17, 170 cathode catalyst layer

[0221] 18, 180 Gas Diffusion Layer

[0222] 18A, 180A Anode gas diffusion layer

[0223] 18C, 180C cathode gas diffusion layer

[0224] 18Ad 2nd anode gas diffusion layer

[0225] 18Ae 1st anode gas diffusion layer

[0226] 18Cd 2nd cathode gas diffusion layer

[0227] 18Ce 1st cathode gas diffusion layer

[0228] 180Ce 1st diffusion layer

[0229] 180Cd 2nd diffusion layer

[0230] 22a, 220a gap

[0231] 220b Through hole

[0232] 22Ab Through hole

[0233] 22Cb Through hole

[0234] 24A Serration

[0235] 24C Serration

[0236] 240 Sawtooth

[0237] 26A Opening

[0238] 26C Opening

[0239] 260 Opening

[0240] 26Aa Edge

[0241] 26Ca terminal edge

[0242] 260a Edge

[0243] F1, F4 area

[0244] F2 Cathode side inner area

[0245] F3 Anode side inner area

[0246] F5 medial region.

Claims

1. A fuel cell module comprising: Membrane-electrode junction; A pair of separators sandwiching the membrane-electrode assembly; and A sealing member for bonding and sealing the membrane-electrode assembly and the pair of separators, respectively; in, The membrane-electrode assembly comprises: Polymer electrolyte membrane; an anode catalyst layer disposed on the first main surface of the polymer electrolyte membrane; a cathode catalyst layer provided on the second main surface of the polymer electrolyte membrane; and a pair of gas diffusion layers, one of which is stacked on the anode catalyst layer and the other of which is stacked on the cathode catalyst layer, One of the pair of gas diffusion layers and the sealing member overlap in the thickness direction in a region including an edge on the center side of the sealing member. A portion of the portion corresponding to the region in the one gas diffusion layer is cut through in the thickness direction.

2. The fuel cell module according to claim 1, wherein: A portion of the one gas diffusion layer corresponding to the region is provided with a plurality of through holes penetrating in the thickness direction.

3. The fuel cell module according to claim 1 or 2, wherein: A portion of the one gas diffusion layer corresponding to the region is provided with a serrated portion formed in a serrated shape in a plan view.

4. The fuel cell module according to any one of claims 1 to 3, wherein: The pair of gas diffusion layers are an anode gas diffusion layer stacked on the anode catalyst layer, and a cathode gas diffusion layer stacked on the cathode catalyst layer. The pair of separators are an anode separator disposed on the anode gas diffusion layer side of the membrane-electrode assembly, and a cathode separator disposed on the cathode gas diffusion layer side of the membrane-electrode assembly and forming a pair with the anode separator to sandwich the membrane-electrode assembly. The sealing member comprises: an anode sealing member having an opening and bonding and sealing the membrane-electrode assembly and the anode separator; and a cathode sealing member having an opening, for bonding and sealing the membrane-electrode assembly and the cathode separator, The anode gas diffusion layer has an anode side inner region overlapping with the anode sealing member in a region including an edge of the anode sealing member on the opening side when viewed in a direction perpendicular to the first main surface. When viewed from a direction perpendicular to the first main surface, the cathode gas diffusion layer has a cathode side inner region overlapping with the cathode sealing member in a region including an edge of the cathode sealing member on the opening side. The anode gas diffusion layer has a void formed in at least a portion including the anode side inner region, penetrating in the thickness direction of the anode gas diffusion layer. The cathode gas diffusion layer has a gap formed in at least a portion including the cathode side inner region, which passes through the cathode gas diffusion layer in a thickness direction. When viewed from a direction perpendicular to the first main surface, the anode-side inner region and the cathode-side inner region do not overlap.

5. The fuel cell module according to claim 4, wherein: When viewed in a direction perpendicular to the first main surface, the anode-side inner region includes an outer portion located outside the cathode-side inner region and an inner portion located inside the cathode-side inner region.

6. The fuel cell module according to claim 4 or 5, wherein: At least one of the voids formed in the anode gas diffusion layer and the voids formed in the cathode gas diffusion layer includes a plurality of through holes.

7. The fuel cell module according to claim 4 or 5, wherein: At least one of the voids formed in the anode gas diffusion layer and the voids formed in the cathode gas diffusion layer is formed by a sawtooth-shaped notch portion when viewed in a direction perpendicular to the first main surface. 8 . A fuel cell stack comprising a plurality of the fuel cell modules according to claim 1 connected in series and stacked.

9. A method for manufacturing a fuel cell module, comprising: a gas diffusion layer processing step of forming a gap in at least a portion of an outer periphery of at least one of the pair of gas diffusion layers; an arrangement step of arranging a membrane-electrode assembly including the pair of gas diffusion layers and a sealing member so that at least a portion of the outer peripheral portion overlaps with the sealing member in a thickness direction; and The bonding step includes sandwiching the sealing member and the membrane-electrode assembly with a pair of separators to bond the membrane-electrode assembly to the pair of separators.

10. The method for manufacturing a fuel cell module according to claim 9, wherein: The method for manufacturing the fuel cell module further comprises: A preparation step, comprising: preparing: a polymer electrolyte membrane having an anode catalyst layer on a first main surface and a cathode catalyst layer on a second main surface; an anode gas diffusion layer and a cathode gas diffusion layer, an anode separator and a cathode separator; and an anode sealing member and a cathode sealing member, In the gas diffusion layer processing step, a gap is formed in at least a portion of the outer periphery of the anode gas diffusion layer and the cathode gas diffusion layer. In the arrangement step, the anode gas diffusion layer is stacked on the anode catalyst layer side of the polymer electrolyte membrane, and the cathode gas diffusion layer is stacked on the cathode catalyst layer side to form a membrane-electrode assembly, the anode sealing member is arranged so as to overlap with at least a portion of the outer peripheral portion of the anode gas diffusion layer, and the cathode sealing member is arranged so as to overlap with at least a portion of the outer peripheral portion of the cathode gas diffusion layer, In the bonding step, the anode gas diffusion layer and the anode separator of the membrane-electrode assembly are bonded via the anode sealing component, the cathode gas diffusion layer and the cathode separator of the membrane-electrode assembly are bonded via the cathode sealing component, and the membrane-electrode assembly is sandwiched between the anode separator and the cathode separator.

Citation Information

Patent Citations

  • Membrane-electrode assembly

    JP2009217999A

  • Method and apparatus for fabricating roll good fuel cell subassemblies

    CN101563804A

  • Fuel cell end plate combination, far end plate combination, entrance end plate combination and electric stack

    CN107146904A

  • Fuel cell electrode structure, metal separator, fuel cell employing said fuel cell electrode structure and said metal separator, and die for fabricating said fuel cell electrode structure

    CN107710483A

  • Fuel cell with gas manifold

    CN1278367A