Negative electrode active material, lithium ion secondary battery and method for producing the same, mixed negative electrode active material, negative electrode
By using a mixed negative active material of specifically screened silicon compound particles and carbon materials in lithium-ion secondary batteries, the problem of expansion and fragmentation of the silicon negative active material is solved, achieving the same performance as carbon material batteries, and improving Battery capacity and cycling characteristics.
Patent Information
- Application Number
- CN202110480492.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2015-11-18
- Filing Date
- 2016-11-04
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2036-11-04
AI Technical Summary
When existing lithium-ion secondary batteries use silicon as the negative active material, they are prone to expansion and fragmentation, resulting in poor cycle characteristics and initial efficiency, and fail to achieve the same performance as carbon material batteries.
A negative active material containing silicon compound particles is used. The silicon compound particles contain SiOx (0.5≤x≤1.6), and the particles containing Li2SiO3 are screened out through the 29Si-MAS-NMR spectrum to meet a specific peak intensity ratio to increase battery capacity. and cyclic properties.
The battery capacity and initial charge and discharge characteristics of lithium-ion secondary batteries are significantly improved, the cycle life of the battery is extended, and the stability and safety of the battery are improved.
Smart Images

Figure CN113178559B_ABST
Abstract
Description
[0001] The present application is a divisional application of an application with a filing date of November 4, 2016, an application number of 201680067722.6, and an invention name of “Negative electrode active material, lithium-ion secondary battery and method for manufacturing the same, mixed negative electrode active material, negative electrode”. Technical Field
[0002] The present invention relates to a negative electrode active material, a mixed negative electrode active material, a negative electrode for a non-aqueous electrolyte secondary battery, a lithium ion secondary battery, a method for producing the negative electrode active material, and a method for producing the lithium ion secondary battery. Background Art
[0003] In recent years, small electronic devices such as mobile terminals have become widely popular, and there is a strong demand for further miniaturization, lightness, and longevity. In response to this market demand, the development of a secondary battery has been promoted, which is particularly small and light and can obtain a high energy density. The application of this secondary battery is not limited to small electronic devices, and the application of large electronic devices such as automobiles and power storage systems such as houses is also being studied.
[0004] Among them, lithium-ion secondary batteries are expected to be small and have high capacity, and can achieve higher energy density than lead batteries and nickel-cadmium batteries.
[0005] The lithium ion secondary battery includes a positive electrode, a negative electrode, a separator, and an electrolyte solution, and the negative electrode includes a negative electrode active material involved in charge and discharge reactions.
[0006] As the negative electrode active material, carbon materials are widely used. On the other hand, the recent market demands further improvement of battery capacity. In order to increase the battery capacity, the use of silicon as the negative electrode active material is being studied. The reason is that the theoretical capacity of silicon (4199mAh / g) is more than 10 times greater than the theoretical capacity of graphite (372mAh / g), so a significant increase in battery capacity can be expected. The development of silicon materials as negative electrode active material is being studied not only for silicon monomers, but also for compounds represented by alloys and oxides. In addition, the shape of the active material is being studied from a standard coating type implemented by carbon materials to an integrated type directly deposited on the collector.
[0007] However, if silicon is used as the main raw material of the negative electrode active material, the negative electrode active material will expand and shrink during charge and discharge, so it is easy to break mainly near the surface of the negative electrode active material. In addition, ionic substances will be generated inside the active material, making the negative electrode active material a substance that is easy to break. If the surface of the negative electrode active material breaks, it will lead to the generation of a new surface, and the reaction area of the active material will increase. At this time, a decomposition reaction of the electrolyte will occur on the new surface, and the decomposition product of the electrolyte, that is, a film, will be formed on the new surface, thereby consuming the electrolyte. Therefore, the cycle characteristics are easily reduced.
[0008] To date, various studies have been conducted on negative electrode materials and electrode structures for lithium-ion secondary batteries using silicon materials as the main material in order to improve the initial efficiency and cycle characteristics of the battery.
[0009] Specifically, in order to obtain good cycle characteristics and high safety, a vapor phase method is used to deposit silicon and amorphous silicon dioxide simultaneously (see, for example, Patent Document 1). In addition, in order to obtain high battery capacity and safety, a carbon material (conductive material) is provided on the surface of the silicon oxide particles (see, for example, Patent Document 2). Furthermore, in order to improve the cycle characteristics and obtain high input-output characteristics, an active material containing silicon and oxygen is prepared, and an active material layer with a high oxygen ratio is formed near the collector (see, for example, Patent Document 3). In addition, in order to improve the cycle characteristics, oxygen is contained in the silicon active material, and is formed in the following manner: the average oxygen content is less than 40at%, and the oxygen content near the collector is high (see, for example, Patent Document 4).
[0010] In addition, in order to improve the initial charge and discharge efficiency, a silicon (Si) phase, SiO2, M y O metal oxide nanocomposite (see, for example, Patent Document 5). In addition, in order to improve the cycle characteristics, SiO x(0.8≤x≤1.5, particle size range = 1μm~50μm) is mixed with a carbon material and calcined at a high temperature (see, for example, Patent Document 6). In addition, in order to improve the cycle characteristics, the molar ratio of oxygen to silicon in the negative electrode active material is set to 0.1~1.2, and the active material is controlled within the range where the difference between the maximum and minimum values of the molar ratio of the active material near the collector interface is less than 0.4 (see, for example, Patent Document 7). In addition, in order to improve the battery load characteristics, a metal oxide containing lithium is used (see, for example, Patent Document 8). In addition, in order to improve the cycle characteristics, a hydrophobic layer such as a silane compound is formed on the surface of the silicon material (see, for example, Patent Document 9). In addition, in order to improve the cycle characteristics, silicon oxide is used, and a graphite film is formed on its surface to impart conductivity (see, for example, Patent Document 10). In Patent Document 10, regarding the shift value obtained from the Raman spectrum associated with the graphite film, at 1330cm -1 and 1580cm -1 Broad peaks appear at the 1330 / I 1580 1.5<I 1330 / I 1580 <3. In order to increase the battery capacity and improve the cycle characteristics, a particle having a silicon microcrystalline phase dispersed in silicon dioxide is used (see, for example, Patent Document 11). In order to improve the overcharge and overdischarge characteristics, a silicon oxide in which the atomic ratio of silicon to oxygen is controlled to 1:y (0<y<2) is used (see, for example, Patent Document 12).
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Application Publication No. 2001-185127;
[0014] Patent document 2: Japanese Patent Application Publication No. 2002-042806;
[0015] Patent Document 3: Japanese Patent Application Publication No. 2006-164954;
[0016] Patent Document 4: Japanese Patent Application Publication No. 2006-114454;
[0017] Patent Document 5: Japanese Patent Application Publication No. 2009-070825;
[0018] Patent Document 6: Japanese Patent Application Publication No. 2008-282819;
[0019] Patent Document 7: Japanese Patent Application Publication No. 2008-251369;
[0020] Patent Document 8: Japanese Patent Application Publication No. 2008-177346;
[0021] Patent Document 9: Japanese Patent Application Publication No. 2007-234255;
[0022] Patent Document 10: Japanese Patent Application Publication No. 2009-212074;
[0023] Patent Document 11: Japanese Patent Application Publication No. 2009-205950;
[0024] Patent document 12: Japanese Patent No. 2997741. Summary of the invention
[0025] As mentioned above, in recent years, the high performance and multifunctionality of small mobile devices represented by electronic machines have been continuously developed, and the main power source, that is, lithium-ion secondary batteries, requires an increase in battery capacity. As one of the methods to solve this problem, it is expected to develop a lithium-ion secondary battery, which is composed of a negative electrode using a silicon-based active material as the main material. In addition, it is expected that the initial efficiency and cycle characteristics of the lithium-ion secondary battery using silicon-based active materials are similar to those of the lithium-ion secondary battery using carbon materials. However, a negative electrode active material has not yet been proposed, which shows the same initial efficiency and cycle stability as the lithium-ion secondary battery using carbon materials.
[0026] The present invention is completed in view of the above-mentioned problems, and its purpose is to provide a negative electrode active material, a mixed negative electrode active material containing the negative electrode active material, a negative electrode for a non-aqueous electrolyte secondary battery containing the mixed negative electrode active material, and a lithium ion secondary battery. When the negative electrode active material is used as a negative electrode active material of a lithium ion secondary battery, the battery capacity can be increased and the cycle characteristics and initial charge and discharge characteristics can be improved.
[0027] Another object of the present invention is to provide a method for producing a negative electrode active material having excellent battery characteristics as described above, and a method for producing a lithium ion secondary battery.
[0028] In order to achieve the above object, the present invention provides a negative electrode active material, which comprises negative electrode active material particles, wherein the negative electrode active material particles contain silicon compound particles, and the silicon compound particles contain silicon compound SiO x , wherein 0.5≤x≤1.6; at least a portion of the negative electrode active material particles contain crystalline Li2SiO3, and the negative electrode active material particles are composed of 29The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by the Si-MAS-NMR spectrum satisfy the following formula 1 or formula 2:
[0029] A>B>D···(1),
[0030] A>C>D···(2).
[0031] The negative electrode active material of the present invention comprises negative electrode active material particles, and the negative electrode active material particles comprise silicon compound particles, so that the battery capacity can be improved. In addition, SiO2, which is a part of the silicon compound and reacts with lithium to become an irreversible component when the secondary battery is charged, is modified into crystalline lithium silicate such as Li2SiO3 in advance, so that the irreversible capacity generated during charging can be reduced. In addition, when the negative electrode active material particles satisfy the above formula 1 or formula 2, it can be considered that the negative electrode active material particles contain less SiO2 based on Li2SiO3 and Si, or less SiO2 based on Li2SiO3 and Li2S2iO5. Therefore, the initial efficiency and cycle characteristics of the battery can be improved. In addition, if A>B is satisfied as in formula 1, it can be considered that most of the SiO2 is deteriorated into Li2SiO3, so the irreversible capacity of the battery is reduced. Further, if B>D is satisfied as in formula 1, it can be considered that there is a sufficient amount of silicon (Si), and the Si can absorb lithium when the battery is charged and discharged, so a higher battery capacity can be obtained. In addition, if A>C is satisfied as in Formula 2, it can be considered that in the lithium silicate obtained by changing SiO2, there are more stable Li2SiO3 than Li2S2iO5 which is easily eluted into aqueous slurry and unstable, so the stability of the aqueous slurry used in making the electrode is improved, and the cycle characteristics of the battery are also improved. In addition, if A>C and C>D are satisfied as in Formula 2, it can become a negative electrode active material, which is stable and can reduce the irreversible capacity caused by SiO2.
[0032] At this time, it is preferred that the 29 The Si-MAS-NMR spectrum obtained had a peak near -130 ppm as a chemical shift value.
[0033] The peak obtained at a position near the chemical shift value of -130ppm is presumed to be a peak derived from amorphous silicon (hereinafter also referred to as a-Si). When a peak derived from amorphous silicon is detected in this way, it can be considered that SiO2 is more fully modified and can thus become a negative electrode active material, which can further improve the initial efficiency and cycle characteristics of the secondary battery.
[0034] In addition, at this time, it is preferred that the29 The Si-MAS-NMR spectrum obtained has a peak at -40 to -60 ppm as a chemical shift value.
[0035] The peak that appears in the range of -40 to -60 ppm as a chemical shift value is also a peak derived from amorphous silicon. Therefore, similarly to the above, it is possible to obtain a negative electrode active material that can further improve the initial efficiency and cycle characteristics of a secondary battery.
[0036] In addition, the silicon compound particles preferably have a half-value width (2θ) of a diffraction peak due to the Si (111) crystal plane obtained by X-ray diffraction of 1.2° or more, and a crystallite size corresponding to the crystal plane of 7.5 nm or less.
[0037] When a negative electrode active material whose silicon compound particles have the above silicon crystallinity is used as a negative electrode active material for a lithium ion secondary battery, better cycle characteristics and initial charge and discharge characteristics can be obtained.
[0038] In addition, it is preferred that: a test battery consisting of a negative electrode and a counter electrode lithium is prepared, the negative electrode contains a mixture of the aforementioned negative electrode active material and a carbon-based active material, and the test battery is subjected to 30 cycles of charge and discharge consisting of charging and discharging, the charging is to cause current to flow in a manner that causes lithium to be inserted into the aforementioned negative electrode active material, and the discharging is to cause current to flow in a manner that causes lithium to be separated from the aforementioned negative electrode active material, and a graph is drawn, the graph showing the relationship between the differential value dQ / dV obtained by differentiating the discharge capacity Q in each charge and discharge using the potential V of the aforementioned negative electrode based on the aforementioned counter electrode lithium and the aforementioned potential V, at this time, during the discharge after the Xth time, where 1≤X≤30, the aforementioned negative electrode has a peak in the range of the potential V of 0.4V to 0.55V.
[0039] The peak in the V-dQ / dV curve is similar to that of silicon material, and the discharge curve on the higher potential side rises sharply, so it is easy to show the capacity when implementing battery design. In addition, if the peak appears during charge and discharge within 30 times, it can become a negative electrode active material that can form a stable bulk.
[0040] Furthermore, the negative electrode active material particles preferably have a median particle size of 1.0 μm or more and 15 μm or less.
[0041] When the median particle size is 1.0 μm or more, the increase in irreversible capacity of the battery due to the increase in surface area per unit mass can be suppressed. On the other hand, when the median particle size is 15 μm or less, the particles are less likely to break, so new surfaces are less likely to appear.
[0042] Furthermore, the negative electrode active material particles preferably contain a carbon material in the surface layer portion.
[0043] In this way, the negative electrode active material particles contain the carbon material in the surface layer portion thereof, thereby achieving improved electrical conductivity.
[0044] Furthermore, the average thickness of the carbon material is preferably not less than 10 nm and not more than 5000 nm.
[0045] If the average thickness of the carbon material is 10 nm or more, the conductivity can be improved. In addition, if the average thickness of the carbon material used for coating is 5000 nm or less, the negative electrode active material containing such negative electrode active material particles can be used in a lithium ion secondary battery to ensure a sufficient amount of silicon compound particles, thereby suppressing the decrease in battery capacity.
[0046] The present invention provides a mixed negative electrode active material, characterized in that it comprises the above-mentioned negative electrode active material and a carbon-based active material.
[0047] In this way, as a material for forming a negative electrode active material layer, the negative electrode active material (silicon-based negative electrode active material) of the present invention and a carbon-based active material are simultaneously included, thereby improving the conductivity of the negative electrode active material layer and relieving the expansion stress caused by charging. In addition, by mixing the silicon-based negative electrode active material into the carbon-based active material, the battery capacity can be increased.
[0048] In addition, in order to achieve the above-mentioned purpose, the present invention provides a negative electrode for a non-aqueous electrolyte secondary battery, characterized in that the negative electrode contains the above-mentioned mixed negative electrode active material, and the mass ratio of the above-mentioned negative electrode active material is greater than 6 mass% relative to the total mass of the above-mentioned negative electrode active material and the above-mentioned carbon-based active material.
[0049] If the mass ratio of the negative electrode active material (silicon-based negative electrode active material) to the total mass of the negative electrode active material (silicon-based negative electrode active material) and the carbon-based active material is 6 mass % or more, the battery capacity can be further increased.
[0050] In addition, in order to achieve the above-mentioned purpose, the present invention provides a negative electrode for a non-aqueous electrolyte secondary battery, characterized in that the negative electrode has a negative electrode active material layer and a negative electrode collector, and the negative electrode active material layer is formed by the above-mentioned mixed negative electrode active material material; the aforementioned negative electrode active material layer is formed on the aforementioned negative electrode collector; and the aforementioned negative electrode collector contains carbon and sulfur, and their contents are both less than 100 mass ppm.
[0051] In this way, the negative electrode current collector constituting the negative electrode contains the above-mentioned amounts of carbon and sulfur, thereby suppressing deformation of the negative electrode during charging.
[0052] In order to achieve the above object, the present invention provides a lithium ion secondary battery characterized by using a negative electrode containing the above negative electrode active material.
[0053] A lithium ion secondary battery using a negative electrode including such a negative electrode active material has a high capacity and can obtain good cycle characteristics and initial charge and discharge characteristics.
[0054] In addition, in order to achieve the above-mentioned object, the present invention provides a method for manufacturing a negative electrode active material, which is a method for manufacturing a negative electrode active material containing negative electrode active material particles, wherein the negative electrode active material particles contain silicon compound particles, and the method for manufacturing the negative electrode active material is characterized in that it comprises the following steps: a step of preparing negative electrode active material particles, wherein the negative electrode active material particles contain silicon compound SiO x Silicon compound particles, wherein 0.5≤x≤1.6; and, a screening step, wherein the following negative electrode active material particles are screened out from the aforementioned negative electrode active material particles, that is, at least a portion of which contains crystalline Li2SiO3 and is 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by the Si-MAS-NMR spectrum satisfy the following formula 1 or formula 2:
[0055] A>B>D···(1),
[0056] A>C>D···(2);
[0057] Then, the negative electrode active material is manufactured by using the screened negative electrode active material particles.
[0058] By manufacturing a negative electrode active material by screening silicon-based active material particles in this manner, it is possible to manufacture a negative electrode active material that has a high capacity and good cycle characteristics and initial charge and discharge characteristics when used as a negative electrode active material for a lithium ion secondary battery.
[0059] In addition, in order to achieve the above-mentioned purpose, the present invention provides a method for manufacturing a lithium-ion secondary battery, characterized in that a negative electrode is made using a negative electrode active material manufactured by the above-mentioned method for manufacturing a negative electrode active material, and a lithium-ion secondary battery is manufactured using the manufactured negative electrode.
[0060] By using the negative electrode active material produced in the above manner, it is possible to produce a lithium ion secondary battery having a high capacity and excellent cycle characteristics and initial charge and discharge characteristics.
[0061] The negative electrode active material of the present invention, when used as a negative electrode active material of a secondary battery, has high capacity and can obtain good cycle characteristics and initial charge and discharge characteristics. In addition, a mixed negative electrode active material, a negative electrode, and a lithium ion secondary battery containing this negative electrode active material can also obtain the same effect. In addition, if it is a method for manufacturing a negative electrode active material of the present invention, a negative electrode active material can be manufactured, and the negative electrode active material has good cycle characteristics and initial charge and discharge characteristics when used as a negative electrode active material of a secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 It is a cross-sectional view showing the structure of the negative electrode for lithium ion secondary battery of the present invention.
[0063] Figure 2 It is a diagram showing a configuration example (laminated film type) of the lithium ion secondary battery of the present invention.
[0064] Figure 3 is used 29 Si-MAS-NMR was used to determine the SiO x An example of the spectrum obtained when .
[0065] Figure 4 The results of the tests in Example 1-1, Example 1-2 and Comparative Example 1-1 are as follows: 29 Si-MAS-NMR spectroscopy.
[0066] Figure 5 This is a graph showing the increase rate of the battery capacity in Example 8-1 and Comparative Example 8-1. DETAILED DESCRIPTION
[0067] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following description.
[0068] As mentioned above, as one of the methods for increasing the battery capacity of lithium-ion secondary batteries, the following method is being studied: using a negative electrode using a silicon-based active material as the main material. The lithium-ion secondary battery using this silicon-based active material is expected to have initial charge and discharge characteristics and cycle characteristics that are similar to those of a lithium-ion secondary battery using a carbon material, but a silicon-based active material that shows the same initial efficiency and cycle stability as a lithium-ion secondary battery using a carbon material has not been proposed.
[0069] Therefore, the present inventors have conducted intensive studies to obtain a negative electrode active material that has a high battery capacity and good cycle characteristics and primary efficiency when used in a secondary battery, thereby completing the present invention.
[0070] The negative electrode active material of the present invention comprises negative electrode active material particles. Furthermore, the negative electrode active material particles contain silicon compound particles, and the silicon compound particles contain silicon compound SiO x , wherein 0.5≤x≤1.6. At least a portion of the negative electrode active material particles contain crystalline Li2SiO3, and are 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by the Si-MAS-NMR spectrum satisfy the following formula 1 or formula 2:
[0071] A>B>D···(1),
[0072] A>C>D···(2).
[0073] The negative electrode active material of the present invention comprises negative electrode active material particles, and the negative electrode active material particles comprise silicon compound particles, so that the battery capacity can be improved. In addition, SiO2, which will react with lithium to become an irreversible component when the secondary battery is charged, is modified into lithium silicate in advance, so that the irreversible capacity generated during charging can be reduced. In addition, when the negative electrode active material particles satisfy the above formula 1 or formula 2, it can be considered that the negative electrode active material particles contain less SiO2 based on Li2SiO3 and Si, or less SiO2 based on Li2SiO3 and Li2S2iO5. Therefore, the initial efficiency and cycle characteristics of the battery can be improved. In addition, if A>B is satisfied as in formula 1, it can be considered that most of the SiO2 is deteriorated into Li2SiO3, so the irreversible capacity of the battery is reduced. Further, if B>D is satisfied as in formula 1, it can be considered that there is a sufficient amount of Si, and the Si can absorb lithium when the battery is charged and discharged, so a higher battery capacity can be obtained. In addition, if A>C is satisfied as in Formula 2, it can be considered that in the lithium silicate obtained by changing SiO2, there are more stable Li2SiO3 than Li2S2iO5 which is easily eluted into the aqueous slurry and unstable, so the stability of the aqueous slurry used in making the electrode is improved, and the cycle characteristics of the battery are also improved. In addition, if A>C and C>D are satisfied as in Formula 2, it can become a negative electrode active material, which is stable and can reduce the irreversible capacity caused by SiO2.
[0074] <Non-aqueous electrolyte secondary battery negative electrode>
[0075] First, the negative electrode for a nonaqueous electrolyte secondary battery will be described. Figure 1 The cross-sectional structure of a negative electrode for a nonaqueous electrolyte secondary battery (hereinafter also referred to as “negative electrode”) in one embodiment of the present invention is shown.
[0076] [Constitution of negative electrode]
[0077] like Figure 1 As shown, the negative electrode 10 is constituted by having a negative electrode active material layer 12 on a negative electrode current collector 11. The negative electrode active material layer 12 may be provided on both sides of the negative electrode current collector 11, or may be provided on only one side of the negative electrode current collector 11. Furthermore, if the negative electrode using the negative electrode active material of the present invention is used, the negative electrode current collector 11 may not be required.
[0078] [Negative electrode current collector]
[0079] The negative electrode current collector 11 is an excellent conductive material and is composed of a material having excellent mechanical strength. Examples of conductive materials that can be used for the negative electrode current collector 11 include copper (Cu) and nickel (Ni). This conductive material is preferably a material that does not form an intermetallic compound with lithium (Li).
[0080] The negative electrode current collector 11 preferably contains carbon (C) and sulfur (S) in addition to the main elements. The reason is that the physical strength of the negative electrode current collector can be improved. In particular, when there is an active material layer that expands during charging, if the current collector contains the above elements, it has the effect of suppressing deformation of the electrode containing the current collector. The content of the above-mentioned elements is not particularly limited, and it is preferably less than 100 mass ppm respectively. The reason is that a higher deformation suppression effect can be obtained. According to such deformation suppression effect, the cycle characteristics can be further improved.
[0081] In addition, the surface of the negative electrode current collector 11 may be roughened or not. A roughened negative electrode current collector may be, for example, a metal foil that has been electrolytically treated, embossed, or chemically etched. An unroughened negative electrode current collector may be, for example, a rolled metal foil.
[0082] [Negative Electrode Active Material Layer]
[0083] The negative electrode active material layer 12 includes the negative electrode active material of the present invention that can absorb and release lithium ions. From the perspective of battery design, it may further include other materials such as a negative electrode adhesive (binder) or a conductive aid. The negative electrode active material includes negative electrode active material particles, and the negative electrode active material particles include silicon compound particles, and the silicon compound particles contain silicon compound SiO x , where 0.5≤x≤1.6.
[0084] In addition, the negative electrode active material layer 12 may include a mixed negative electrode active material, wherein the mixed negative electrode active material includes the negative electrode active material (silicon-based negative electrode active material) of the present invention and a carbon-based active material. Accordingly, the resistance of the negative electrode active material layer can be reduced, and the expansion stress caused by charging can be alleviated. As the carbon-based active material, for example, pyrolytic carbon, coke, glassy carbon fiber, organic polymer compound calcined body, carbon black, etc. can be used.
[0085] In addition, the negative electrode of the present invention is preferably: relative to the total mass of the silicon-based negative electrode active material and the carbon-based active material, the mass ratio of the silicon-based negative electrode active material is 6 mass% or more. If the mass ratio of the negative electrode active material of the present invention is 6 mass% or more relative to the total mass of the silicon-based negative electrode active material and the carbon-based active material, the battery capacity can be reliably improved.
[0086] In addition, as described above, the negative electrode active material of the present invention comprises silicon compound particles, wherein the silicon compound particles contain a silicon compound (SiO x : 0.5≤x≤1.6), preferably x is close to 1. The reason is that high cycle characteristics can be obtained. In addition, the composition of the silicon compound in the present invention does not necessarily mean 100% purity, and may contain trace amounts of impurity elements.
[0087] In addition, in the negative electrode active material of the present invention, the silicon compound particles may further contain Li4SiO4 in addition to crystalline Li2SiO3. This lithium silicate is also obtained by pre-modifying the SiO2 component in the silicon compound, which becomes unstable when inserting and removing lithium during battery charging and discharging, into other lithium silicates, thereby reducing the irreversible capacity generated during charging.
[0088] In addition, when Li4SiO4 and Li2SiO3 coexist in the bulk of silicon compound particles, the battery characteristics can be further improved. Furthermore, these lithium silicates can be quantified using nuclear magnetic resonance (NMR) and X-ray photoelectron spectroscopy (XPS). The determination of XPS and NMR can be carried out according to the following conditions, for example.
[0089] XPS
[0090] Device: X-ray photoelectron spectroscopy device;
[0091] X-ray source: monochromatized Al Kα rays;
[0092] X-ray spot diameter: 100 μm;
[0093] Ar ion gun sputtering conditions: 0.5 kV / 2 mm × 2 mm.
[0094] 29 Si MAS NMR (Magic Angle Spinning Nuclear Magnetic Resonance)
[0095] Apparatus: 700NMR nuclear magnetic resonance spectrometer manufactured by Bruker;
[0096] Probe: 4 mm HR-MAS rotor 50 μL;
[0097] Sample rotation speed: 10kHz;
[0098] Measurement environment temperature: 25℃.
[0099] In addition, in the present invention, the negative electrode active material particles are preferably composed of 29 The Si-MAS-NMR spectrum has a peak near -130ppm as a chemical shift value. The peak obtained at a position near the chemical shift value of -130ppm is presumed to be a peak derived from amorphous silicon. When a peak derived from amorphous silicon is detected in this way, it can be considered that SiO2 is more fully modified and can thus become a negative electrode active material that can further improve the initial efficiency and cycle characteristics of the secondary battery.
[0100] In addition, in the present invention, the negative electrode active material particles are preferably composed of 29 The Si-MAS-NMR spectrum has a peak at -40 to -60 ppm as a chemical shift value. The peak that appears in the range of -40 to -60 ppm as a chemical shift value is also a peak derived from amorphous silicon. Therefore, similarly to the above, it can become a negative electrode active material that can further improve the initial efficiency and cycle characteristics of the secondary battery.
[0101] Furthermore, an example of a peak derived from amorphous silicon is shown in Figure 3 .like Figure 3 As shown in Figure 2, the peak originating from amorphous silicon appears as a gentle peak. 29 The chemical shift values of the Si-MAS-NMR spectrum are in the region of -40 to -60 ppm. Furthermore, a peak derived from amorphous silicon also appears at a position near the chemical shift value of -130 ppm.
[0102] In addition, the silicon compound particles preferably have a half-value width (2θ) of a diffraction peak caused by a (111) crystal plane obtained by X-ray diffraction of 1.2° or more, and a crystallite size corresponding to the crystal plane of 7.5 nm or less. The lower the silicon crystallinity of the silicon compound in the silicon compound particles, the better. In particular, if the amount of silicon crystals present is small, the battery characteristics can be improved, and a stable lithium compound can be generated.
[0103] In addition, in the negative electrode active material of the present invention, the negative electrode active material particles preferably contain carbon material in the surface layer. By using the negative electrode active material to contain carbon material in its surface layer, the conductivity can be improved. Therefore, when the negative electrode active material containing such negative electrode active material particles is used as the negative electrode active material of the secondary battery, the battery characteristics can be improved.
[0104] In addition, the average thickness of the surface layer of the negative electrode active material particles is preferably greater than 10 nm and less than 5000 nm. If the average thickness of the carbon material is greater than 10 nm, the conductivity can be improved; if the average thickness of the coated carbon material is less than 5000 nm, when the negative electrode active material containing such negative electrode active material particles is used as the negative electrode active material of the secondary battery, the battery capacity can be suppressed from decreasing.
[0105] The average thickness of this carbon material can be calculated, for example, using the following sequence. First, observe the negative electrode active material particles at an arbitrary magnification using a TEM (transmission electron microscope). This magnification is preferably the following magnification: a magnification at which the thickness of the carbon material can be visually confirmed in a manner that allows the thickness to be measured. Then, the thickness of the carbon material is measured at any 15 points. At this time, it is preferred that the measurement positions are set widely and randomly without concentrating on a specific location as much as possible. Finally, the average value of the thickness of the carbon material at the above 15 points is calculated.
[0106] The coverage of the carbon material is not particularly limited, but is preferably as high as possible. A coverage of 30% or more is preferred because the conductivity can be further improved. The coating method of the carbon material is not particularly limited, but preferably a sugar carbonization method or a hydrocarbon gas thermal cracking method. The reason is that the coverage can be improved.
[0107] In addition, it is preferred that the median particle size (D 50 : Particle size when the cumulative volume becomes 50%) is greater than 1.0μm and less than 15μm. The reason is that if the median particle size is within the above range, lithium ions are easily absorbed and released during charge and discharge, and the particles are not easy to break. If the median particle size is greater than 1.0μm, the surface area per unit mass can be reduced, and the increase in irreversible capacity of the battery can be suppressed. On the other hand, if the median particle size is set to less than 15μm, the particles are not easy to break, so new surfaces are not easy to appear.
[0108] In addition, the negative electrode active material (silicon-based active material) of the present invention is preferably: a test cell composed of a negative electrode and a counter electrode lithium is prepared, the negative electrode contains a mixture of the silicon-based active material and a carbon-based active material, and the test cell is subjected to 30 cycles of charge and discharge, wherein the charge is to flow a current in a manner that lithium is inserted into the silicon-based active material, and the discharge is to flow a current in a manner that lithium is separated from the silicon-based active material, and a graph is drawn showing the relationship between the differential value dQ / dV obtained by differentiating the discharge capacity Q in each charge and discharge by the potential V of the negative electrode with respect to the counter electrode lithium and the potential V, wherein, in the discharge after the Xth time, where 1≤X≤30, the negative electrode has a peak in the range of the potential V of 0.4V to 0.55V. The peak in the V-dQ / dV curve is similar to the peak of the silicon material, and the discharge curve rises sharply on the higher potential side, so that the capacity is easily displayed when the battery design is implemented. In addition, if the negative electrode active material can show the above peak during charge and discharge within 30 cycles, it can be judged that a stable bulk can be formed.
[0109] As the negative electrode binder contained in the negative electrode active material layer, for example, any one or more of a polymer material and a synthetic rubber can be used. The polymer material includes, for example, polyvinylidene fluoride, polyimide, polyamide-imide, aramid, polyacrylic acid, lithium polyacrylate, carboxymethyl cellulose, etc. The synthetic rubber includes, for example, styrene butadiene rubber, fluorine rubber, ethylene propylene diene, etc.
[0110] As the negative electrode conductive additive, for example, one or more carbon materials such as carbon black, acetylene black, graphite, Ketjen black, carbon nanotubes, and carbon nanofibers can be used.
[0111] The negative electrode active material layer is formed by, for example, a coating method, which is a method of mixing negative electrode active material particles with the above-mentioned binder, and optionally with a conductive additive and a carbon material, dispersing the mixture in an organic solvent or water, and applying the mixture.
[0112] The negative electrode can be manufactured according to the following procedure, for example. First, a method for manufacturing a negative electrode active material used for the negative electrode is described. First, negative electrode active material particles containing silicon compound particles are prepared. The silicon compound particles contain a silicon compound (SiO x :0.5≤x≤1.6) Then, the following negative electrode active material particles are selected from the negative electrode active material particles: at least a part of which contains crystalline Li2SiO3 and is composed of 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by the Si-MAS-NMR spectrum satisfy the following formula 1 or formula 2:
[0113] A>B>D···(1),
[0114] A>C>D···(2).
[0115] Then, the negative electrode active material is produced using the screened negative electrode active material particles.
[0116] In addition, when preparing the negative electrode active material particles, a step of coating the silicon compound particles with a carbon material may be further included. The negative electrode active material particles obtained by coating the surface of the silicon compound particles with a carbon material have excellent electrical conductivity.
[0117] More specifically, the negative electrode active material can be manufactured in the following manner. First, a raw material capable of generating silicon oxide gas is heated in the presence of an inert gas and under reduced pressure within a temperature range of 900°C to 1600°C to generate silicon oxide gas. Considering the presence of surface oxygen of the metal silicon powder and trace oxygen in the reactor, the mixing molar ratio is preferably within the range of 0.8 < metal silicon powder / silicon dioxide powder < 1.3.
[0118] The generated gas solidifies and deposits on the adsorption plate. Then, the temperature in the reaction furnace is lowered to below 100°C, and the deposit is taken out and crushed and powdered using a ball mill, a jet mill, etc. The above method can be used to produce silicon compound particles. Furthermore, the silicon microcrystals in the silicon compound particles can be controlled by changing the vaporization temperature or heat treatment after generation.
[0119] Here, the carbon material layer can be formed on the surface layer of the silicon compound particles. As a method for forming the carbon material layer, a thermal chemical vapor deposition method (thermal CVD method) is preferably used. A method for forming the carbon material layer using the thermal CVD method will be described.
[0120] First, silicon compound particles are loaded into a furnace. Then, hydrocarbon gas is introduced into the furnace, and the temperature in the furnace is raised. The decomposition temperature is not particularly limited, but is preferably below 1200°C, and more preferably below 950°C. By setting the decomposition temperature below 1200°C, unexpected disproportionation of silicon compound particles can be suppressed. After the temperature in the furnace is raised to a specific temperature, a carbon layer is formed on the surface of the silicon compound particles. In this way, negative electrode active material particles can be manufactured. In addition, the hydrocarbon gas used as the raw material of the carbon material is not particularly limited, but is preferably at C n H m In the composition, n ≤ 3. When n ≤ 3, the production cost can be reduced and the physical properties of the decomposition product can be improved.
[0121] Then, the negative electrode active material particles prepared in the above manner may be modified by inserting lithium. In this case, the negative electrode active material particles may contain crystalline lithium silicate such as Li2SiO3 and Li4SiO4.
[0122] The insertion of lithium is preferably carried out according to a thermal doping method. At this time, the modification can be carried out, for example, by mixing the negative electrode active material particles with lithium hydride powder or lithium powder and heating them in a non-oxidizing atmosphere. As a non-oxidizing atmosphere, for example, an argon (Ar) atmosphere can be used. More specifically, first, lithium hydride powder or lithium powder is fully mixed with silicon oxide powder under an argon atmosphere, and sealed, and then the entire sealed container is stirred to homogenize it. Then, the modification is carried out by heating in the range of 700°C to 750°C. In addition, at this time, to separate lithium from the silicon compound, the following method can be used: the heated powder is fully cooled, and then washed with alcohol or alkaline water, weak acid or pure water.
[0123] In addition, lithium can also be inserted into the negative electrode active material particles according to the redox method. In the modification using the redox method, for example, first, the silicon oxide particles are immersed in a solution A obtained by dissolving lithium in an ether solvent, thereby enabling the insertion of lithium. This solution A can further contain a polycyclic aromatic compound or a linear polyphenylene compound. After the insertion of lithium, the silicon oxide particles are immersed in a solution B containing a polycyclic aromatic compound or a derivative thereof, thereby enabling the active lithium to be separated from the negative electrode active material particles. The solvent of this solution B can be, for example: an ether solvent, a ketone solvent, an ester solvent, an alcohol solvent, an amine solvent, or a mixed solvent of these solvents. Furthermore, after being immersed in solution B, the negative electrode active material particles are immersed in a solution C containing an alcohol solvent, a carboxylic acid solvent, water, or a mixed solvent of these solvents, thereby enabling more active lithium to be separated from the negative electrode active material particles. In addition, solution C' can be used instead of solution C, wherein solution C' contains a compound having a quinone structure in the molecule as a solute, and contains an ether solvent, a ketone solvent, an ester solvent, or a mixed solvent of these solvents as a solvent. In addition, the negative electrode active material particles can be repeatedly immersed in solutions B, C, and C'. If this is done, after the lithium is inserted and the active lithium is separated, a negative electrode active material with higher water resistance can be formed. Then, the following methods can be used for cleaning: using alcohol, alkaline water containing lithium carbonate, weak acid or pure water for cleaning.
[0124] In addition, by performing modification according to two modification methods, a negative electrode active material can be produced, wherein the modification of the negative electrode active material is further advanced and the battery characteristics are further improved. More specifically, it is better to first perform modification using a thermal doping method and then perform modification according to a redox method. At this time, the silicon dioxide part that is not fully modified by the thermal doping method can be selectively modified by the redox method.
[0125] Then, the following negative electrode active material particles are selected from the modified negative electrode active material particles: at least a portion of which contains crystalline Li2SiO3 and is composed of 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by the Si-MAS-NMR spectrum satisfy the following formula 1 or formula 2:
[0126] A>B>D···(1),
[0127] A>C>D···(2).
[0128] 29 Si-MAS-NMR can be carried out under the following conditions.
[0129] 29 Si MAS NMR
[0130] Apparatus: 700NMR nuclear magnetic resonance spectrometer manufactured by Bruker;
[0131] Probe: 4 mm HR-MAS rotor 50 μL;
[0132] Sample rotation speed: 10kHz;
[0133] Measurement environment temperature: 25℃.
[0134] in addition, 29 In the Si-MAS-NMR spectrum, the peaks appearing near the chemical shift values of -72 to -75 ppm are peaks derived from Li2SiO3, and the peaks appearing near -83 ppm are peaks derived from Si. In addition, the peaks appearing near the chemical shift values of -93 ppm are peaks derived from Li2Si2O5, and the peaks appearing near -110 ppm are peaks derived from SiO2.
[0135] Furthermore, there are peaks of lithium silicate other than Li2SiO3 and Li4SiO4 in the range of -80 to -100 ppm. Also, a peak derived from Li4SiO4 may appear around -63 ppm.
[0136] The peak intensity is given by 29The peak height calculated from the baseline of the Si-MAS-NMR spectrum is expressed as follows. In this case, the baseline can be calculated according to a general method.
[0137] In addition, sometimes the peak near -72 to -75ppm originating from Li2SiO3 does not achieve a maximum value. In this case, the peak intensity A is set to the maximum value of the spectrum intensity at -72ppm. In addition, when the peak near -83ppm originating from Si does not have a maximum value, the peak intensity B is set to the intensity at -83ppm. In addition, when the peak near -93ppm originating from Li2Si2O5 does not have a maximum value, the peak intensity C is set to the intensity at -93ppm. In addition, when the peak near -110ppm originating from SiO2 does not have a maximum value, the peak intensity D is set to the intensity at -110ppm.
[0138] Furthermore, the screening of negative electrode active material particles does not necessarily need to be carried out every time the negative electrode active material is manufactured. As long as the manufacturing conditions satisfying the above formula 1 and formula 2 are found and selected, the negative electrode active material can be manufactured using the same conditions as the selected conditions.
[0139] The negative electrode active material produced in the above manner is mixed with other materials such as a negative electrode adhesive and a conductive aid to make a negative mixed electrode mixture, and then an organic solvent or water is added to make a slurry. Then, the surface of the negative electrode collector is coated with the above slurry and dried to form a negative electrode active material layer. At this time, hot pressing can also be performed as needed. In addition, if the negative electrode collector contains 100 mass ppm of carbon and sulfur each, the effect of suppressing the deformation of the negative electrode can be obtained. In the above manner, a negative electrode can be made.
[0140] <Lithium-ion secondary battery>
[0141] Next, the lithium ion secondary battery of the present invention is described. The lithium ion secondary battery of the present invention uses a negative electrode containing the negative electrode active material of the present invention. Here, as a specific example, a laminated thin film type lithium ion secondary battery can be cited as an example.
[0142] [Construction of laminated thin film type lithium ion secondary battery]
[0143] like Figure 2 The laminated thin film type lithium ion secondary battery 20 shown mainly contains a wound electrode body 21 inside a sheet-like outer casing 25. This wound electrode body is wound with a separator between the positive electrode and the negative electrode. In addition, there is also the following situation: a separator is provided between the positive electrode and the negative electrode and a laminate is contained. In any electrode body, a positive electrode lead 22 is installed on the positive electrode, and a negative electrode lead 23 is installed on the negative electrode. The outermost periphery of the electrode body is protected by a protective tape.
[0144] The positive and negative electrode leads are led out in one direction, for example, from the inside to the outside of the outer casing 25. The positive electrode lead 22 is made of a conductive material such as aluminum, and the negative electrode lead 23 is made of a conductive material such as nickel or copper.
[0145] The outer member 25 is, for example, a laminated film formed by sequentially laminating a fusion layer, a metal layer, and a surface protective layer, and the fusion layer and the electrode body 21 are opposed to each other, and the outer peripheral portions of the fusion layers of the two films are fused to each other or bonded by an adhesive or the like. The fusion portion is, for example, a film of polyethylene or polypropylene, and the metal layer is, for example, aluminum foil. The protective layer is, for example, nylon or the like.
[0146] An adhesive film 24 is inserted between the outer casing 25 and the positive and negative electrode leads to prevent the intrusion of external gas. The material of the adhesive film 24 is, for example, polyethylene, polypropylene, or polyolefin resin.
[0147] [positive electrode]
[0148] Positive electrode, such as Figure 1 Similarly, the negative electrode 10 has positive electrode active material layers on both surfaces or on one surface of the positive electrode current collector.
[0149] The positive electrode current collector is formed of a conductive material such as aluminum.
[0150] The positive electrode active material layer includes any one or more of the positive electrode materials capable of absorbing and releasing lithium ions, and may include other materials such as a binder, a conductive aid, and a dispersant according to the design. In this case, the detailed information about the binder and the conductive aid is the same as that of the negative electrode binder and the negative electrode conductive aid already described.
[0151] As the positive electrode material, lithium-containing compounds are more preferred. Examples of such lithium-containing compounds include composite oxides composed of lithium and transition metal elements, or phosphate compounds containing lithium and transition metal elements. Among these positive electrode materials, compounds containing at least one of nickel, iron, manganese, and cobalt are preferred. The chemical formula of these positive electrode materials is, for example, Li x M1O2 or Li y In the above formula, M1 and M2 represent at least one transition metal element. The values of x and y vary with the charge and discharge state of the battery. Generally, they are represented by 0.05≤x≤1.10 and 0.05≤y≤1.10.
[0152] Examples of composite oxides containing lithium and transition metal elements include lithium cobalt composite oxides (Li x CoO2), lithium nickel composite oxide (Li xNiO2), etc. As phosphoric acid compounds containing lithium and transition metal elements, examples include lithium iron phosphate compound (LiFePO4) or lithium iron manganese phosphate compound (LiFe 1-u Mn u PO4 (0 < u < 1)), etc. The reason is that if these positive electrode materials are used, high battery capacity can be obtained, and excellent cycle characteristics can also be obtained.
[0153] [Negative electrode]
[0154] The negative electrode has the same structure as the negative electrode 10 for the lithium ion secondary battery described above. For example, negative electrode active material layers 12 are provided on both sides of the current collector 11. This negative electrode is preferably such that the negative electrode charging capacity is larger than the capacitance obtained from the positive electrode active material agent (as the charging capacity of the battery). The reason is that lithium metal precipitation on the negative electrode can be suppressed.
[0155] The positive electrode active material layer is provided on a part of both sides of the positive electrode current collector, and the negative electrode active material layer is also provided on a part of both sides of the negative electrode current collector. At this time, for example, in the negative electrode active material layer provided on the negative electrode current collector, there is a region where there is no opposing positive electrode active material layer. The reason is to implement a stable battery design.
[0156] In the non-opposing region, that is, in the region where the negative electrode active material layer and the positive electrode active material layer do not oppose each other, it is hardly affected by charge and discharge. Therefore, the state of the negative electrode active material layer can be maintained after formation. Accordingly, the composition of the negative electrode active material, etc. can be investigated reproducibly and correctly in a manner independent of the presence or absence of charge and discharge.
[0157] [Separator]
[0158] The separator isolates the positive electrode and the negative electrode to prevent a current short circuit caused by the two electrodes coming into contact, and allows lithium ions to pass through. This separator is formed using, for example, a porous membrane made of a synthetic resin or ceramic, and may have a laminated structure formed by laminating two or more porous membranes. Examples of the synthetic resin include polytetrafluoroethylene, polypropylene, polyethylene, etc.
[0159] [Electrolyte solution]
[0160] In at least a part of the active material layer or the separator, a liquid electrolyte (electrolyte solution) is impregnated. This electrolyte solution has an electrolyte salt dissolved in a solvent and may contain other materials such as additives.
[0161] Solvents, such as non-aqueous solvents, can be used. Examples of non-aqueous solvents include ethyl carbonate, propyl carbonate, butyl carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, methyl propyl carbonate, 1,2-dimethoxyethane, or tetrahydrofuran. Among them, it is more desirable to use at least one of ethyl carbonate, propyl carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate. The reason is that better properties can be obtained. In addition, at this time, by combining high-viscosity solvents such as ethyl carbonate and propyl carbonate with low-viscosity solvents such as dimethyl carbonate, ethyl methyl carbonate, and diethyl carbonate, more advantageous properties can be obtained. The reason is that the dissociation and ion mobility of the electrolyte salt can be improved.
[0162] When using an alloy-based negative electrode, in particular, as a solvent, it is more desirable to contain at least one of a halogenated chain carbonate or a halogenated cyclic carbonate. Accordingly, especially when charging, a stable film can be formed on the surface of the negative electrode active material. Here, a halogenated chain carbonate refers to a chain carbonate having a halogen as a constituent element (at least one hydrogen is replaced by a halogen). In addition, a halogenated cyclic carbonate refers to a cyclic carbonate having a halogen as a constituent element (that is, at least one hydrogen is replaced by a halogen).
[0163] The type of halogen is not particularly limited, but fluorine is preferred. The reason is that it can form a better film than other halogens. In addition, the more halogens there are, the better. The reason is that the obtained film is more stable and can reduce the decomposition reaction of the electrolyte.
[0164] Examples of the halogenated chain carbonate include fluoromethyl methyl carbonate and difluoromethyl methyl carbonate, and examples of the halogenated cyclic carbonate include 4-fluoro-1,3-dioxolane-2-one and 4,5-1,3-dioxolane-2-one.
[0165] Preferably, as the solvent additive, an unsaturated carbon-bonded cyclic carbonate is included. The reason is that a stable film can be formed on the surface of the negative electrode during charge and discharge, and the decomposition reaction of the electrolyte can be suppressed. Examples of the unsaturated carbon-bonded cyclic carbonate include vinylene carbonate and vinyl ethyl carbonate.
[0166] In addition, it is preferable to include sultone (cyclic sulfonate) as a solvent additive because the chemical stability of the battery can be improved. Examples of sultone include propane sultone and propene sultone.
[0167] Furthermore, the solvent preferably contains an acid anhydride because the chemical stability of the electrolyte can be improved. Examples of the acid anhydride include propane disulfonic anhydride.
[0168] The electrolyte salt may include at least one of light metal salts such as lithium salts. Examples of the lithium salts include lithium hexafluorophosphate (LiPF6) and lithium tetrafluoroborate (LiBF4).
[0169] The content of the electrolyte salt is preferably 0.5 mol / kg or more and 2.5 mol / kg or less relative to the solvent, because high ion conductivity can be obtained.
[0170] [Method for producing laminated thin film secondary battery]
[0171] In the present invention, a negative electrode is produced using the negative electrode active material produced by the method for producing a negative electrode active material of the present invention, and a lithium ion secondary battery is produced using the produced negative electrode.
[0172] At the beginning, the positive electrode is made by using the above-mentioned positive electrode material. First, the positive electrode active material is mixed with an adhesive, a conductive aid, etc. as needed to make a positive electrode mixture, and then dispersed in an organic solvent to make a positive electrode mixture slurry. Then, a coating device such as a die coater with a knife roller or a die head is used to coat the mixture slurry on the positive electrode collector, and hot air drying is performed to obtain a positive electrode active material layer. Finally, a roller press is used to compression-mold the positive electrode active material layer. At this time, heating can be performed, and heating or compression can be repeated multiple times.
[0173] Next, the negative electrode active material layer was formed on the negative electrode collector using the same operation procedure as that used to prepare the negative electrode 10 for the lithium ion secondary battery, thereby preparing the negative electrode.
[0174] When manufacturing the positive electrode and the negative electrode, each active material layer is formed on both sides of the positive electrode and the negative electrode current collector. At this time, in any electrode, the active material coating lengths on both sides may be different (refer to Figure 1 ).
[0175] Then, an electrolyte is prepared. Then, ultrasonic welding is used to Figure 2In a manner, the positive electrode lead 22 is installed on the positive electrode collector, and the negative electrode lead 23 is installed on the negative electrode collector. Then, the positive electrode and the negative electrode are stacked or wound with a separator to produce a wound electrode body 21, and a protective tape is adhered to its outermost periphery. Then, the wound body is formed in a flat shape. Then, the wound electrode body is sandwiched between the folded film-like outer packaging members 25, and then the insulating parts of the outer packaging members are bonded to each other by a thermal fusion method, and only one direction is set to an open state to seal the wound electrode body. An adhesive film is inserted between the positive electrode lead and the negative electrode lead and the outer packaging member. A specific amount of the above-prepared electrolyte is added from the open part, and vacuum impregnation is performed. After impregnation, the open part is bonded by a vacuum thermal fusion method. In the above manner, a laminated thin film secondary battery 20 can be manufactured.
[0176] [Example]
[0177] Hereinafter, the present invention will be described in more detail with reference to Examples and Comparative Examples of the present invention; however, the present invention is not limited to these Examples.
[0178] (Example 1-1)
[0179] Use the following procedure to create Figure 2 A laminated thin film type lithium ion secondary battery 20 is shown.
[0180] First, the positive electrode is made. The positive electrode active material is a mixture of 95% by mass of lithium nickel cobalt composite oxide (NCA), namely LiNi 0.7 Co 0.25 Al 0.05 O, 2.5 mass % of positive electrode conductive aid, and 2.5 mass % of positive electrode adhesive (polyvinylidene fluoride, PVDF) to make a positive electrode mixture. Then, the positive electrode mixture is dispersed in an organic solvent (N-methyl-2-pyrrolidone, NMP) to make a paste slurry. Then, a coating device with a die head is used to apply the slurry on both sides of the positive electrode collector, and a hot air drying device is used to dry it. At this time, the positive electrode collector uses a positive electrode collector with a thickness of 15μm. Finally, compression molding is performed by roller pressing.
[0181] Next, the negative electrode was prepared in the following manner. The raw material obtained by mixing metal silicon and silicon dioxide was introduced into a reaction furnace, vaporized in a vacuum environment of 10 Pa, and then deposited on an adsorption plate. After being fully cooled, the deposit was taken out and crushed using a ball mill. The SiO2 of the silicon compound particles obtained in this way x The x value is 1.0. Then, the particle size of the silicon compound particles is adjusted by classification. Then, the surface of the silicon compound particles is coated with carbon material by performing thermal CVD. This is used as negative electrode active material particles.
[0182] Then, the negative electrode active material particles are modified by inserting lithium by performing a thermal doping method. First, lithium hydride powder and negative electrode active material particles are mixed under an argon atmosphere and stirred with an oscillator (shaker), wherein the mass of the lithium hydride powder is equivalent to 4% by mass relative to the negative electrode active material particles (silicon compound particles coated with carbon material). Then, the stirred powder is subjected to a heat treatment at 740°C in an atmosphere controlled furnace to perform modification.
[0183] After modification, the negative electrode active material particles are washed with alcohol, alkaline water, weak acid or pure water.
[0184] The negative electrode active material particles produced in this manner contain crystalline Li 2 SiO 3 .
[0185] Here, according to 29 After Si-MAS-NMR was used to measure the negative electrode active material particles prepared in Example 1-1, the following was obtained: Figure 4 The spectrum shown. Figure 4 After setting the baseline in the spectrum and calculating the peak intensities, the peak intensity A originating from Li2SiO3, the peak intensity B originating from Si, the peak intensity C originating from Li2Si2O5, and the peak intensity D originating from SiO2 satisfy formula 2 (A>C>D), but do not satisfy formula 1 (A>D>B).
[0186] Depend on Figure 4 It can be seen that a peak is also obtained at a position near the chemical shift value of -130 ppm. Furthermore, only a gentle peak is observed at a position of the chemical shift value of -40 to -60 ppm.
[0187] Then, the negative electrode active material particles and the carbon active material were mixed at a mass ratio of 1:9 to prepare the negative electrode active material. Here, as the carbon active material, the following carbon active material was used: natural graphite coated with a pitch layer and artificial graphite were mixed at a mass ratio of 5:5. In addition, the median particle size of the carbon active material was 20 μm.
[0188] Then, the prepared mixed negative electrode active material, conductive aid 1 (carbon nanotube, CNT), conductive aid 2 (carbon microparticles with a median particle size of about 50 μm), styrene butadiene rubber (styrene butadiene copolymer, hereinafter referred to as SBR), carboxymethyl cellulose (hereinafter referred to as CMC) were mixed at a dry mass ratio of 92.5:1:1:2.5:3, and diluted with pure water to prepare a negative electrode mixture slurry. In addition, the above-mentioned SBR and CMC are negative electrode binders (negative electrode binders).
[0189] In addition, as the negative electrode collector, an electrolytic copper foil with a thickness of 15 μm is used. This electrolytic copper foil contains carbon and sulfur at a concentration of 100 mass ppm each. Finally, the negative electrode mixture slurry is coated on the negative electrode collector and dried at 100°C for 1 hour in a vacuum environment. After drying, the deposition amount of the negative electrode active material layer per unit area on a single side of the negative electrode (also known as the area density) is 5 mg / cm 2 .
[0190] Then, after mixing the solvent (4-fluoro-1,3-dioxolane-2-one (FEC), ethyl carbonate (EC) and dimethyl carbonate (DMC)), the electrolyte salt (lithium hexafluorophosphate, LiPF6) was dissolved to prepare the electrolyte solution. At this time, the composition of the solvent was set to FEC:EC:DEC=10:20:70 by volume, and the content of the electrolyte salt was set to 1.2 mol / kg relative to the solvent.
[0191] Then, assemble the secondary battery in the following manner. First, ultrasonically weld an aluminum lead to one end of the positive electrode collector, and weld a nickel lead to the negative electrode collector. Then, stack the positive electrode, separator, negative electrode, and separator in sequence, and then wind them longitudinally to obtain a wound electrode body. Fix the end of the winding with a PET protective tape. The separator uses a laminated film (12μm), which is composed of a film with porous polypropylene as the main component, sandwiched between a film with porous polyethylene as the main component. Then, after the electrode body is sandwiched between the outer packaging components, the outer peripheral portions are heat-fused to each other except one side, and the electrode body is housed inside. The outer packaging component uses an aluminum laminated film stacked by nylon film, aluminum foil, and polypropylene film. Then, the prepared electrolyte is injected from the opening, impregnated in a vacuum environment, and then sealed by heat fusion.
[0192] The cycle characteristics and initial charge and discharge characteristics of the secondary battery produced in the above manner were evaluated.
[0193] The cycle characteristics were investigated in the following manner. Initially, in order to stabilize the battery, two cycles of charge and discharge were performed at 0.2C at 25°C, and the discharge capacity of the second cycle was measured. Then, charge and discharge were performed until the total number of cycles reached 499 cycles, and the discharge capacity was measured each time. Finally, the discharge capacity of the 500th cycle obtained by charging and discharging at 0.2C was divided by the discharge capacity of the second cycle to calculate the capacity retention rate (hereinafter referred to as the retention rate). The general cycle, that is, from the 3rd cycle to the 499th cycle, is performed by charging at 0.7C and discharging at 0.5C.
[0194] When investigating the initial charge and discharge characteristics, the initial efficiency (hereinafter sometimes referred to as the initial efficiency) is calculated. The initial efficiency is calculated by the following formula: initial efficiency (%) = (initial discharge capacity / initial charge capacity) × 100. The atmosphere and temperature are set to be the same as when investigating the cycle characteristics.
[0195] In addition, a 2032-size button cell type test battery was made from the negative electrode and the counter electrode lithium prepared in the above manner, and its discharge behavior was evaluated. More specifically, the counter electrode lithium was charged at a constant current and constant voltage until 0 V. When the current density reached 0.05 mA / cm 2 Then, discharge at a constant current until the voltage reaches 1.2V. The current density at this time is 0.2mA / cm 2 . This charge and discharge was repeated 30 times, and the data obtained during each charge and discharge were plotted with the vertical axis set to the rate of change of capacity (dQ / dV) and the horizontal axis set to voltage (V), and then it was confirmed whether a peak was obtained in the V range of 0.4 to 0.55 (V). As a result, a peak was obtained in the V range of 0.4 to 0.55 (V) during charge and discharge within 30 times, and this peak was obtained in all charge and discharges from the charge and discharge when this peak first appeared to the 30th charge and discharge.
[0196] In addition, the silicon-based active material alone (SiO x First, the negative electrode active material particles prepared above were mixed with polyacrylic acid at a mass ratio of 85:15, and the mixture was coated on a copper foil. At this time, the area density of the coated mixture was about 2 mg / cm 2 After vacuum drying at 90°C for 1 hour, the battery was placed in a 2032-size button cell format using a lithium counter electrode at a voltage of 0 V and a current density of 0.2 mA / cm 2 Then, the constant current constant voltage charging is started. Then, the constant current constant voltage charging is terminated when the current value reaches 0.1 mA. Then, the constant current discharge is performed, and the discharge is terminated when the voltage reaches 1.2 V. The current density during discharge is set to be the same as that during charging. At this time, when the condition for inputting lithium to the negative electrode is set to charging, and the condition for taking lithium out of the negative electrode is set to discharging, the silicon-based active material alone (SiO x The initial efficiency of SiO is (discharge capacity) / (charge capacity)×100(%). x Unique primary efficiency. As a result, SiO x The primary efficiency alone is 80.5%.
[0197] (Example 1-2)
[0198] like Figure 4 As shown, use29 The negative electrode active material particles whose peak intensities A, B, C, and D in the Si-MAS-NMR spectrum satisfy Formula 1 and Formula 2 are prepared in the same manner as in Example 1-1. Figure 4 It can be seen that a peak is also obtained at a position near the chemical shift value of -130 ppm, and a gentle peak appears at a position of the chemical shift value of -40 to -60 ppm.
[0199] In Example 1-2, the negative electrode active material particles modified by the hot doping method are further modified by the redox method. Specifically, first, the negative electrode active material particles modified by the hot doping method are immersed in a solution (solution A1), which is obtained by dissolving lithium sheets and biphenyl in tetrahydrofuran (hereinafter also referred to as THF). Solution A1 of Example 1-1 is prepared in the following manner: after dissolving biphenyl in THF solvent at a concentration of 1 mol / L, a lithium sheet with a mass fraction of 10% is added to the mixed solution of THF and biphenyl. In addition, when immersing the negative electrode active material particles, the temperature of the solution is 20°C, and the immersion time is set to 10 hours. Then, the negative electrode active material particles are obtained by filtration. According to the above treatment, lithium is inserted into the negative electrode active material particles.
[0200] Then, the negative electrode active material particles after lithium insertion were immersed in a solution (solution B), which was obtained by dissolving naphthalene in THF. Solution B of Example 1-2 was prepared by dissolving naphthalene in THF solvent at a concentration of 2 mol / L. In addition, when immersing the negative electrode active material particles, the temperature of the solution was 20°C and the immersion time was set to 20 hours. Then, the negative electrode active material particles were filtered to obtain the negative electrode active material particles.
[0201] Then, the negative electrode active material particles after contact with solution B are immersed in a solution (solution C) obtained by dissolving p-benzoquinone in THF at a concentration of 1 mol / L. The immersion time is set to 2 hours. Then, the negative electrode active material particles are filtered. Then, after the washing treatment, the silicon compound is dried under reduced pressure. After modification, the negative electrode active material particles are washed using alcohol or alkaline water, weak acid or pure water.
[0202] In addition, a 2032-size button cell type test battery was prepared using the same negative electrode and counter electrode lithium as the secondary battery prepared in Example 1-2, and its discharge behavior was evaluated in the same manner as in Example 1-1. As a result, a peak was obtained in the range of V 0.4 to 0.55 (V) during charge and discharge within 30 cycles. In addition, SiO x After the initial efficiency of the SiO x The initial efficiency alone was 85.3%.
[0203] (Comparative Example 1-1)
[0204] like Figure 4 As shown, use 29 The peak intensities A, B, C, and D in the Si-MAS-NMR spectrum do not satisfy the negative electrode active material particles of Formula 1 and Formula 2. Otherwise, the secondary battery is manufactured in the same manner as in Example 1-1. Figure 4 It can be seen that Comparative Example 1-1 has a spectrum in which the peak intensity D derived from the silicon dioxide region obtained at a position near the chemical shift value of -110 ppm is the largest. 29 Does the Si-MAS-NMR spectrum have a peak at a chemical shift value of -130 ppm? 29 The Si-MAS-NMR spectrum showed no peak at a chemical shift value of -40 to -60 ppm. In Comparative Example 1-1, the modification of Example 1-1 was not performed, but negative electrode active material particles prepared by the same procedure as Example 1-1 were used.
[0205] In addition, a 2032-size button cell type test battery was prepared using the same negative electrode and counter electrode lithium as the secondary battery prepared in Comparative Example 1-1, and its discharge behavior was evaluated in the same manner as in Example 1-1. As a result, a peak was obtained in the range of V 0.4 to 0.55 (V) during charge and discharge within 30 cycles. In addition, for particles that were not modified, SiO x After the initial efficiency of the SiO x The initial efficiency alone is 71%.
[0206] At this time, the negative electrode active material particles of Examples 1-1, 1-2 and Comparative Example 1-1 have the following properties. Median particle size D of the negative electrode active material particles 50 The average thickness of the carbon material on the surface of the negative electrode active material particles was 100 nm.
[0207] In addition, the half-value width (2θ) of the diffraction peak due to the Si (111) crystal plane obtained by X-ray diffraction of the silicon compounds of Examples 1-1 and 1-2 was 1.755°, and the crystallite size due to the Si (111) crystal plane was 4.86 nm.
[0208] Table 1 shows the results of Examples 1-1, 1-2 and Comparative Example 1-1.
[0209] [Table 1]
[0210] SiO x :x=1,D 50 =4μm; copper foil: carbon 100ppm, sulfur 100ppm; SiOx Ratio: 10% by mass;
[0211] Positive electrode NCA; average thickness of carbon material 100nm; with dQ / dV peak;
[0212]
[0213] The negative electrode active material of Example 1-1, that is, when the negative electrode active material particles are modified according to the hot doping method in the manner of Example 1-1, a certain amount of silicon dioxide equivalent to the irreversible component can be reduced and changed into lithium silicate, etc., thereby obtaining negative electrode active material particles satisfying Formula 2. At this time, as shown in Table 1, compared with Comparative Example 1-1, which does not satisfy both Formulas 1 and 2, the capacity retention rate and initial efficiency are improved. In addition, in the manner of Example 1-2, after the hot doping method is implemented, the remaining silicon dioxide component is further modified using a redox method, thereby obtaining a negative electrode active material satisfying both Formulas 1 and 2. At this time, the capacity retention rate and initial efficiency are further improved than those of Example 1-1.
[0214] (Examples 2-1, 2-2, Comparative Examples 2-1, 2-2)
[0215] The secondary battery was manufactured in the same manner as in Example 1-2 except that the oxygen content in the bulk of the silicon compound was adjusted. At this time, the oxygen content was adjusted by changing the ratio of metal silicon to silicon dioxide in the raw material of the silicon compound and the heating temperature. x Table 2 shows the x values of the silicon compounds represented by .
[0216] [Table 2]
[0217] SiO x :D 50 =4μm; copper foil: carbon 100ppm, sulfur 100ppm; SiO x Ratio: 10% by mass;
[0218] Positive electrode NCA; average thickness of carbon material 100nm; Si(111) half-value width 1.755°, crystallite 4.86nm; satisfying equations 1 and 2; peak at -130ppm; peak at -40~-60ppm
[0219] As shown in Table 2, in the case of SiO xIn the silicon compound represented by , when the x value is in the range of 0.5≤x≤1.6, the battery characteristics are further improved. As shown in Comparative Example 2-1, when the oxygen is insufficient (x=0.3), although the initial efficiency is improved, the capacity retention rate is significantly deteriorated. On the other hand, as shown in Comparative Example 2-2, when the oxygen content is large (x=1.8), it is not easy to cause the absorption and separation of lithium because the oxygen content is too much, so the capacity of silicon oxide cannot be substantially manifested, so the evaluation is stopped.
[0220] (Example 3-1)
[0221] by 29 In order to prevent the peak from appearing at the position of the chemical shift value of -40 to -60 ppm in the Si-MAS-NMR spectrum, the modification conditions of the negative electrode active material particles were changed, and the secondary battery was manufactured in the same manner as in Example 1-1. At this time, the heat treatment temperature in the hot doping, the particle size of lithium hydride, and the heat treatment time were changed.
[0222] [Table 3]
[0223] SiO x :x=1,D 50 =4μm; copper foil: carbon 100ppm, sulfur 100ppm; SiO x Ratio: 10% by mass;
[0224] Positive electrode NCA; average thickness of carbon material 100nm; Si(111) half-value width 1.755°, crystallite 4.86nm; does not satisfy equation 1 but satisfies equation 2; has a peak at -130ppm; has a dQ / dV peak
[0225]
[0226] When a peak appears at a position where the chemical shift value is -40 to -60 ppm, the capacity retention rate and the initial efficiency are improved.
[0227] (Examples 4-1 to 4-5)
[0228] The crystallinity of silicon microcrystals in silicon compound particles was changed as shown in Table 4. Otherwise, secondary batteries were prepared under the same conditions as in Example 1-2, and the cycle characteristics and initial efficiency were evaluated. Furthermore, the crystallinity of silicon microcrystals in silicon compound particles can be controlled by changing the vaporization temperature of the raw material or by heat treatment after the silicon compound particles are generated.
[0229] [Table 4]
[0230] SiO x : x = 1; copper foil: carbon 100ppm, sulfur 100ppm; SiO x Ratio: 10% by mass;
[0231] There is a dQ / dV peak; positive electrode NCA; average thickness of carbon material is 100nm; satisfying equations 1 and 2; there is a peak at -130ppm; there is a peak at -40 to -60ppm
[0232]
[0233] The capacity retention rate and initial efficiency vary with the crystallinity of silicon microcrystals in the silicon compound particles. In particular, low-crystalline materials with a half-value width of 1.2° or more and a microcrystal size of 7.5nm or less due to the Si(111) plane can achieve a higher capacity retention rate.
[0234] (Examples 5-1 to 5-5)
[0235] The median particle size of the silicon compound was changed as shown in Table 5. Otherwise, secondary batteries were prepared under the same conditions as in Example 1-2, and the cycle characteristics and primary efficiency were evaluated.
[0236] [Table 5]
[0237] SiO x : x = 1; copper foil: carbon 100ppm, sulfur 100ppm; SiO x Ratio: 10 mass%; with dQ / dV peak;
[0238] Positive electrode NCA; average thickness of carbon material 100nm; Si(111) half-value width 1.755°, crystallite 4.86nm; satisfying equations 1 and 2; peak at -130ppm; peak at -40~-60ppm
[0239] If the median particle size of the silicon compound is 1.0 μm or more, the retention rate can be improved. This is believed to be because the surface area per unit mass of the silicon compound will not be too large, and the area where side reactions occur can be reduced, and the consumption of the electrolyte can be suppressed. On the other hand, if the median particle size is less than 15 μm, the particles are not easy to break during charging, and it is not easy to generate SEI (solid electrolyte interface) caused by the new surface during charging and discharging, so the loss of reversible lithium can be suppressed. In addition, if the median particle size of the silicon-based active material particles is less than 15 μm, the expansion amount of the silicon compound particles during charging will not increase, so the physical and electrical damage of the negative electrode active material layer caused by expansion can be prevented.
[0240] (Example 6-1)
[0241] A secondary battery was produced under the same conditions as in Example 1-1 except that the surfaces of the silicon compound particles were not coated with the carbon material, and the cycle characteristics and the initial efficiency were evaluated.
[0242] (Examples 6-2 to 6-5)
[0243] A secondary battery was produced under the same conditions as in Example 1-1 except that the average thickness of the carbon material coated on the surface of the silicon compound particles was changed, and the cycle characteristics and initial efficiency were evaluated. The average thickness of the carbon material can be adjusted by changing the CVD conditions.
[0244] [Table 6]
[0245] SiO x :x=1,D 50 =4μm; copper foil: carbon 100ppm, sulfur 100ppm; SiO x Ratio: 10% by mass;
[0246] Positive NCA; Si(111) half-value width 1.755°, microcrystal 4.86nm; dQ / dV peak; satisfying equations 1 and 2; peak at -130ppm; peak at -40~-60ppm
[0247]
[0248] As can be seen from Table 6, when the average thickness of the carbon material is 10 nm or more, the conductivity is particularly improved, so the capacity retention rate and initial efficiency can be improved. On the other hand, if the average thickness of the carbon material is 5000 nm or less, the amount of silicon compound particles can be sufficiently ensured in the battery design, so the battery capacity can be fully ensured.
[0249] (Example 7-1)
[0250] A secondary battery was produced under the same conditions as in Example 1-1 except that a copper foil containing no carbon or sulfur was used as the current collector of the negative electrode, and the cycle characteristics and the initial efficiency were evaluated.
[0251] [Table 7]
[0252] SiO x :x=1,D 50 =4μm; SiO x Ratio: 10 mass%; with dQ / dV peak;
[0253] Positive electrode NCA; average thickness of carbon material 100nm; Si(111) half-value width 1.755°, crystallite 4.86nm; satisfying equations 1 and 2; peak at -130ppm; peak at -40~-60ppm
[0254] When the negative electrode contains less than 100 mass ppm of carbon and sulfur, the strength of the current collector is improved. Therefore, when using a silicon-based negative electrode active material that expands and contracts greatly during the charge and discharge of a secondary battery, the deformation and distortion of the current collector caused by it can be suppressed, so as shown in Example 1-1, the battery characteristics are improved, especially the cycle characteristics are improved.
[0255] (Example 8-1)
[0256] A secondary battery was produced under the same conditions as in Example 1-1 except that the mass ratio of the negative electrode active material particles (silicon-based active material particles) in the negative electrode active material was changed, and the rate of increase in battery capacity was evaluated.
[0257] Furthermore, when no carbon-based active material is used (when the proportion of silicon-based active material in the negative electrode active material is set to 100% by mass), silicon-based active material particles, conductive aid 1 (carbon nanotubes, CNT), conductive aid 2 (carbon microparticles with a median particle size of about 50 nm), and precursors of negative electrode adhesives are mixed at a dry weight ratio of 83:10:2.5, and then diluted with NMP to make a paste-like negative electrode mixture slurry. At this time, NMP is used as a solvent for polyamic acid. Subsequently, the negative electrode mixture slurry is applied to both sides of the negative electrode collector using a coating device and then dried. As this negative electrode collector, electrolytic copper foil (thickness = 15 μm) is used. Finally, calcination is performed at 400°C in a vacuum environment for 1 hour. This forms a negative electrode adhesive (polyimide).
[0258] (Comparative Example 8-1)
[0259] A secondary battery was produced under the same conditions as in Comparative Example 1-1 except that the mass ratio of the negative electrode active material particles (silicon-based active material particles) in the negative electrode active material was changed, and the rate of increase in battery capacity was evaluated.
[0260] Figure 5 A graph showing the relationship between the ratio of the silicon-based active material particles to the total amount of the negative electrode active material and the rate of increase in the battery capacity of the secondary battery in Example 8-1 and Comparative Example 8-1 is shown. Figure 5 It can be seen that in Example 8-1, when the ratio of the silicon-based compound is 6 mass % or more, the rate of increase in battery capacity becomes larger than that in Comparative Example 8-1, and the volume energy density increases particularly significantly.
[0261] The present invention is not limited to the above-described embodiments. The above-described embodiments are merely examples, and any technical solutions having substantially the same structure and exhibiting the same functions and effects as the technical concept described in the claims of the present invention are all within the technical scope of the present invention.
Claims
1. A negative electrode active material comprising negative electrode active material particles, wherein the negative electrode active material is characterized in that: The negative electrode active material particles contain silicon compound particles, and the silicon compound particles contain silicon compound SiO x , 0.5≤x≤1.6; At least a portion of the negative electrode active material particles contains crystalline Li2SiO3, The negative electrode active material particles are composed of 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by Si-MAS-NMR spectrum satisfy the following equations 1 and 2, A>B>D···(1), A>C>D···(2).
2. The negative electrode active material according to claim 1, wherein Said by 29 The Si-MAS-NMR spectrum obtained had a peak near -130 ppm as a chemical shift value.
3. The negative electrode active material according to claim 1, wherein The silicon compound particles have a diffraction peak due to a Si (111) crystal plane obtained by X-ray diffraction with a half-value width 2θ of 1.2° or more, and a crystallite size corresponding to the crystal plane of 7.5 nm or less.
4. The negative electrode active material according to claim 1, wherein A test battery consisting of a negative electrode and a counter electrode lithium is prepared, wherein the negative electrode comprises a mixture of the negative electrode active material and the carbon active material, and the test battery is subjected to 30 cycles of charge and discharge, wherein the charge is to cause current to flow in a manner that lithium is inserted into the negative electrode active material, and the discharge is to cause current to flow in a manner that lithium is separated from the negative electrode active material, and a graph is drawn, wherein the graph shows the relationship between the differential value dQ / dV obtained by differentiating the discharge capacity Q in each charge and discharge and the potential V of the negative electrode with respect to the counter electrode lithium, wherein, at the time of discharge after the Xth time, wherein 1≤X≤30, the negative electrode has a peak in the range of the potential V of 0.4V to 0.55V.
5. The negative electrode active material according to claim 1, wherein The negative electrode active material particles have a median particle size of 1.0 μm or more and 15 μm or less.
6. The negative electrode active material according to claim 1, wherein The negative electrode active material particles contain a carbon material in the surface layer portion.
7. The negative electrode active material according to claim 6, wherein The average thickness of the carbon material is greater than or equal to 10 nm and less than or equal to 5000 nm.
8. A mixed negative electrode active material, characterized in that: The negative electrode active material comprises the negative electrode active material according to any one of claims 1 to 7, and a carbon-based active material.
9. A negative electrode for a non-aqueous electrolyte secondary battery, characterized in that: The negative electrode comprises the mixed negative electrode active material according to claim 8, and the mass ratio of the negative electrode active material to the total mass of the negative electrode active material and the carbon-based active material is 6 mass % or more.
10. A negative electrode for a non-aqueous electrolyte secondary battery, characterized in that: The negative electrode comprises a negative electrode active material layer and a negative electrode current collector, wherein the negative electrode active material layer is formed by the mixed negative electrode active material according to claim 8; The negative electrode active material layer is formed on the negative electrode current collector; Furthermore, the negative electrode current collector contains carbon and sulfur, and the content of these carbon and sulfur is both 100 mass ppm or less.
11. A lithium ion secondary battery, characterized in that: As the negative electrode, a negative electrode including the negative electrode active material according to any one of claims 1 to 7 is used.
12. A method for producing a negative electrode for a non-aqueous electrolyte secondary battery, characterized in that: The process includes the following steps: The process of preparing negative electrode active material particles, wherein the negative electrode active material particles contain a silicon compound SiO x Silicon compound particles, 0.5≤x≤1.6; The step of modifying the silicon compound particles by a thermal doping method and then modifying them by a redox method, thereby causing at least a portion of the silicon compound particles to contain crystalline Li2SiO3; and A screening step, wherein the following negative electrode active material particles are screened out from the negative electrode active material particles, that is, at least a portion of which contains crystalline Li2SiO3 and is 29 The peak intensity A derived from Li2SiO3, the peak intensity B derived from Si, the peak intensity C derived from Li2Si2O5, and the peak intensity D derived from SiO2 obtained by Si-MAS-NMR spectrum satisfy the following equations 1 and 2, A>B>D···(1), A>C>D···(2); Furthermore, the negative electrode active material particles screened out are used to manufacture the negative electrode active material. A negative electrode for a non-aqueous electrolyte secondary battery is produced using the negative electrode active material produced as described above.