A fuel cell proton exchange membrane and preparation method thereof
Through the composite preparation method of polybenzimidazole and nitrogen-containing heteroaromatic ring-substituted halogenated alkanes, the contradiction between the conductivity and mechanical strength of traditional proton exchange membranes and the loss of phosphoric acid are solved, achieving high performance and long life of high-temperature fuel cells, and promoting commercial application of fuel cells.
Patent Information
- Application Number
- CN202010113178.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-02-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-02-24
AI Technical Summary
The proton conductivity and mechanical strength of traditional high-temperature proton exchange membrane fuel cells are in conflict. The loss of phosphoric acid leads to battery performance degradation and shortened service life. There is a lack of proton exchange membranes with high proton conductivity, high mechanical strength, and low phosphoric acid loss rate.
Polybenzimidazole type compounds are compounded with nitrogen-containing heteroaromatic ring-substituted halogenated alkanes as raw materials, and proton exchange membranes are prepared through specific molar ratios and preparation methods to form membranes with high proton conductivity, mechanical strength and antioxidant properties.
It achieves high proton conductivity, mechanical strength and antioxidant properties of the proton exchange membrane at high temperatures, extends the service life of the battery, and promotes the commercial development of high-temperature fuel cells.
Smart Images

Figure BDA0002390693690000021 
Figure BDA0002390693690000031 
Figure BDA0002390693690000032
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of fuel cells, and in particular relates to a fuel cell proton exchange membrane and a preparation method thereof. Background Art
[0002] A fuel cell is a device that converts the chemical energy between a fuel and an oxidant directly into electrical energy through an electrode reaction. Due to its advantages of high efficiency, low pollution, short construction time, good reliability and maintainability, it is known as a fourth-generation power generation technology after hydropower, thermal power and nuclear power. Among them, the proton exchange membrane fuel cell (PEMFC) uses a proton exchange membrane as a solid electrolyte, has no electrolyte corrosion problem, has high energy conversion efficiency, is pollution-free, can be quickly started at room temperature, has a long life and high power density. Therefore, as a new type of military and civilian dual-use power source, it shows huge market potential and broad application prospects. The development of proton exchange membrane fuel cells is of great significance to the upgrading of the current industrial structure, environmental protection and sustainable economic development. In view of its importance, fuel cells have been listed by the United States as one of the 27 key technologies that must be developed to maintain the economic prosperity and national security of the United States, and have been recognized by developed countries such as the United States and Canada as the preferred clean energy system in the 21st century. In 2000, fuel cells were also rated by the American "Time" magazine as one of the top ten technologies that have a significant impact on human society in the 21st century.
[0003] The proton exchange membrane of traditional PEMFC widely uses perfluorosulfonic acid membrane (PFSA, such as Nafion membrane produced by Dupont). The proton conductivity of this membrane is heavily dependent on liquid water. It generally works at 60-90°C. Too high a temperature will cause PEM dehydration, a sharp drop in proton conductivity, and serious attenuation of battery performance. The low operating temperature brings various disadvantages to PEMFC and becomes its development bottleneck. In order to solve the above problems of the proton exchange membrane fuel cell of traditional PEMFC, the development of high temperature proton exchange membrane fuel cell (HT-PEMFC) has become inevitable.
[0004] At present, the most widely used high-temperature proton exchange membrane is the PBI (polybenzimidazole) type proton exchange membrane. However, since the membrane is doped with inorganic phosphoric acid, it has obvious disadvantages: (a) Since the system relies on phosphoric acid to conduct protons, and water is produced when the fuel cell is working and discharged from the membrane, this will cause the inorganic phosphoric acid to be lost along with the removal of the produced water, thereby causing the proton conductivity of the membrane to decrease; and it also leads to the attenuation of battery performance and shortens the service life of the battery. (b) The proton conductivity of the membrane is inconsistent with the mechanical strength of the membrane; since the system conducts protons through phosphoric acid, in order to increase the proton conductivity of the membrane, the phosphoric acid content in the membrane is generally increased. However, the increase in phosphoric acid content will lead to a decrease in the mechanical stability and antioxidant properties of the membrane, resulting in a shortened service life of the membrane.
[0005] Therefore, the art still lacks a proton exchange membrane that has high proton conductivity, high mechanical strength, high oxidation resistance, low phosphate loss rate, and long stable life. Summary of the invention
[0006] The object of the present invention is to provide a fuel cell proton exchange membrane and a preparation method thereof.
[0007] In a first aspect of the present invention, a fuel cell proton exchange membrane is provided, wherein the proton exchange membrane is composited with a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring as raw materials, wherein the molar ratio of A to B is nA:nB=1:0.1-6.0; and the polybenzimidazole polymer A is selected from the following group:
[0008]
[0009] Wherein, n=2-10000;
[0010] R is selected from the group consisting of O, S, NH, C(O), S(O)2, unsubstituted or halogenated C1-C6 alkylene, unsubstituted or halogenated C2-C6 alkenylene;
[0011] R 1 Select from the following group:
[0012]
[0013] The nitrogen-containing heteroaromatic ring substituted halogenated alkane B is a C1-C10 halogenated alkane, and the nitrogen-containing heteroaromatic ring is a 5-7 membered nitrogen-containing heteroaromatic ring.
[0014] In another preferred embodiment, the polybenzimidazole type compound A is selected from the following group:
[0015]
[0016] Where R 1 The definition of is as described above.
[0017] In another preferred embodiment, the structure of the nitrogen-containing heteroaromatic ring-substituted halogenated alkane B is:
[0018] R 2 -(CH2) m X or R 2 -(CF2) m X
[0019] in:
[0020] m = 1-9;
[0021] X=Cl or Br;
[0022] —R 2 Select from the following group:
[0023]
[0024] In another preferred embodiment, the molar ratio of A to B is nA:nB=1:0.5-3.
[0025] The second aspect of the present invention provides a method for preparing a fuel cell proton exchange membrane according to the first aspect of the present invention, the method comprising the steps of:
[0026] (i) dissolving a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring in an organic solvent to form a mixed solution;
[0027] (ii) filtering to remove insoluble matter to obtain a mixed filtrate;
[0028] (iii) degassing the mixed filtrate;
[0029] (iv) forming a membrane of the mixed filtrate subjected to the deaeration treatment to obtain a proton exchange membrane.
[0030] In another preferred embodiment, the step (iv) comprises: dissolving a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring in an organic solvent, dissolving them in an organic solvent under the protection of an inert gas, and refluxing at 150-170° C. for a period of time to form a mixed solution.
[0031] In another preferred embodiment, the step (i) comprises: casting the degassed mixed filtrate into a membrane, and then further drying at 80-100° C. and 180-220° C. in sequence to obtain a proton exchange membrane.
[0032] In another preferred embodiment, the preparation method comprises the steps of:
[0033] (1) dissolving a polybenzimidazole type compound A in a first organic solvent, and then adding a base to form a mixed solution;
[0034] (2) adding a halogenated alkane B substituted with a heteroaromatic ring to the mixed solution obtained in the above step (1), heating the mixture for reaction, and obtaining a reaction mixture;
[0035] (3) pouring the reaction mixture into water to precipitate solid;
[0036] (4) dissolving the solid in a second organic solvent to prepare a solution with a certain solid content;
[0037] (5) filtering the solution to remove insoluble matter to obtain a filtrate;
[0038] (6) degassing the filtrate to obtain a degassed filtrate;
[0039] (7) Casting the degassed filtrate into a membrane to obtain a proton exchange membrane.
[0040] In another preferred embodiment, the step (1) comprises: providing a polybenzimidazole type compound A, dissolving it in an organic solvent under the protection of an inert gas to prepare a mixed solution with a certain solid content, then adding a certain amount of alkali, and refluxing at 160° C. for 24 hours.
[0041] In another preferred embodiment, the solid precipitated in step (3) is first washed with water, then washed with ethanol, and then dried.
[0042] In another preferred embodiment, the step (7) comprises: casting the degassed mixed filtrate into a membrane, and then further drying at 80-100° C. and 180-220° C. in sequence to obtain a proton exchange membrane.
[0043] In another preferred embodiment, in the method, the molar ratio of the polybenzimidazole type compound A to the heteroaromatic ring substituted halogenated alkane B is 1:0.1-6.
[0044] In another preferred embodiment, the organic solvent, the first organic solvent and the second organic solvent are each independently a strongly polar organic solvent. More preferably, the organic solvent, the first organic solvent and the second organic solvent are each independently selected from the following group: DMSO (dimethyl sulfoxide), DMF (N,N-dimethylformamide), DMAC (N,N-dimethylacetamide), or NMP (N-methylpyrrolidone), or a combination thereof.
[0045] In another preferred embodiment, the solid content of the mixed solution is 1-40wt%.
[0046] In another preferred embodiment, in the step (1), the base is selected from the following group: NaH, LiH, KH, Na2CO3, K2CO3, or a combination thereof; preferably, the molar ratio of the polybenzimidazole type compound A to the base is 1:0.1-3.
[0047] It should be understood that within the scope of the present invention, the above-mentioned technical features of the present invention and the technical features specifically described below (such as embodiments) can be combined with each other to form a new or preferred technical solution. Due to space limitations, they will not be described one by one here. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] Figure 1 This is a graph showing the change of proton conductivity with temperature.
[0049] Figure 2 The Fenton reagent oxidation degradation curves of different membranes. DETAILED DESCRIPTION
[0050] After long-term and in-depth research, the inventor unexpectedly found that by using a polybenzimidazole type compound A and another nitrogen-containing heteroaromatic ring substituted halogenated alkane B as raw materials, preparing a solution and then forming a membrane, a high-temperature proton exchange membrane with high proton conductivity, high mechanical strength, high oxidation resistance, and low phosphoric acid loss rate can be prepared, so it is very suitable for use as a proton exchange membrane for a high-temperature proton conductive membrane fuel cell. Based on the above discovery, the inventor completed the present invention.
[0051] Fuel cell proton exchange membrane
[0052] The present invention provides a fuel cell proton exchange membrane, which is composited with a polybenzimidazole type compound A and another nitrogen-containing heteroaromatic ring substituted halogenated alkane B as raw materials, wherein the molar ratio of A to B is nA:nB=1:0.1-6.0.
[0053] The polybenzimidazole polymer A can be a commercially available polybenzimidazole polymer, or a polymer prepared by an existing method in the art (such as the polymer described in patent application No. 201710084102.X). A preferred class of polybenzimidazole polymers is selected from the following group:
[0054]
[0055] Wherein, n=2-10000;
[0056] R is selected from the group consisting of O, S, NH, C(O), S(O)2, unsubstituted or halogenated C1-C6 alkylene, unsubstituted or halogenated C2-C6 alkenylene;
[0057] R1 Select from the following group:
[0058]
[0059] The nitrogen-containing heteroaromatic ring substituted halogenated alkane B is a C1-C10 halogenated alkane, and the nitrogen-containing heteroaromatic ring is a 5-7 membered nitrogen-containing heteroaromatic ring.
[0060] The polybenzimidazole type compound A is selected from the following group:
[0061]
[0062] Where R 1 The definition of is as described above.
[0063] In a preferred embodiment of the present invention, the structure of the nitrogen-containing heteroaromatic ring-substituted halogenated alkane B is:
[0064] R 2 -(CH2) m X or R 2 -(CF2) m X
[0065] Wherein, m = 1-9;
[0066] X=Cl or Br;
[0067] Among them, “—R 2 "Selected from the following group:
[0068]
[0069] In a more preferred embodiment, the molar ratio of A to B is nA:nB=1:0.1-6.
[0070] The proton exchange membrane can be prepared by a common membrane forming method in the art, and the preferred preparation method is as follows:
[0071] Method (a):
[0072] According to a certain molar ratio, a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring are weighed, dissolved in an organic solvent under the protection of an inert gas, and refluxed at 160° C. for a period of time to prepare a mixed solution with a certain solid content;
[0073] Filter to remove insoluble matter to obtain a mixed filtrate;
[0074] Degassing the mixed filtrate;
[0075] The mixed filtrate subjected to the degassing treatment is cast into a membrane, first dried at 80-100° C., and then further dried at 180-220° C. to obtain a proton exchange membrane.
[0076] Method (b):
[0077] Providing a polybenzimidazole type compound A, dissolving it in an organic solvent under the protection of an inert gas to prepare a mixed solution with a certain solid content, then adding a certain amount of alkali, and refluxing at 160° C. for 24 hours;
[0078] Then, a certain proportion of the heteroaromatic ring-substituted halogenated alkane B is added, and the heating reaction is continued for 24 hours;
[0079] The reaction solution was poured into water to precipitate a solid, which was first washed with water, then with ethanol, and then dried;
[0080] Under the protection of inert gas, the dried solid is dissolved in an organic solvent to prepare a solution with a certain solid content;
[0081] Filter and remove insoluble matter to obtain a filtrate;
[0082] Degassing the filtrate;
[0083] Casting the degassed filtrate into a membrane, first drying at 80° C., and then drying at 120° C. to obtain a proton exchange membrane;
[0084] Wherein, in the method (a) and the method (b), the molar ratio of the polybenzimidazole type compound A to the heteroaromatic ring substituted halogenated alkane B is 1:0.1-6.
[0085] The organic solvent can be a solvent suitable for dissolving the polybenzimidazole type compound A and the heteroaromatic ring-substituted halogenated alkane B, such as a strongly polar organic solvent, preferably selected from the following group: DMSO (dimethyl sulfoxide), DMF (N,N-dimethylformamide), DMAC (N,N-dimethylacetamide), or NMP (N-methylpyrrolidone), or a combination thereof.
[0086] In the methods (a) and (b), the solid content of the prepared solution is 1-40 wt%.
[0087] In a preferred embodiment of the present invention, the base used in method (b) is NaH, LiH, KH, Na2CO3, K2CO3. More preferably, the molar ratio of the polybenzimidazole type compound A used in method (b) to the base is 1:0.1-3.
[0088] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by weight.
[0089] Compared with the existing high-temperature proton exchange membrane, the fuel cell proton exchange membrane of the present invention has the following advantages:
[0090] 1) The retention of nitrogen-containing heteroaromatic rings maintains the high proton conductivity and low phosphate loss rate of the membrane;
[0091] 2) There is no saturated full carbon main chain of polyethylene structure in the molecular structure of the membrane material polymer, which enhances the antioxidant performance of the membrane;
[0092] 3) Due to the introduction of the halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring, the active "NH" sites in the molecular structure of the polybenzimidazole polymer are reduced, and the antioxidant properties of the polymer are further enhanced;
[0093] Therefore, the fuel cell proton exchange membrane using the present invention will have higher antioxidant performance, higher proton conductivity, higher operating stability and durability, which is conducive to promoting the commercial development of high-temperature fuel cells.
[0094] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise stated, percentages and parts are calculated by weight.
[0095] Example 1
[0096] Preparation of membrane No. 1 [Method (a)]:
[0097]
[0098] According to the molar ratio of 1:2, dry m-PBI (616.7 mg, 2 mmol) and 1-(2-bromotetrafluoroethyl)imidazole (988.0 mg, 4 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMSO (dimethyl sulfoxide, 30.489 g), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 100°C for two hours, and then further heated to 200°C for 4 hours to obtain proton exchange membrane No. 1. The thickness of the membrane is 32 μm (micrometers), and the DSC test shows that its glass transition temperature T g =298℃, mechanical properties test shows that its tensile strength is 121MPa.
[0099] Example 2
[0100] Preparation of membrane No. 2 [Method (a)]:
[0101]
[0102] According to the molar ratio of 1:1.5, dry m-PBI (616.7 mg, 2 mmol) and 1-(bromodifluoromethyl)-1,2,3-triazole (593.9 mg, 3 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N,N-dimethylacetamide, 29.054 g), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 4%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 90°C for two hours, and then further heated to 200°C for 5 hours to obtain proton exchange membrane No. 2. The thickness of the membrane is 29 μm (micrometer), and the DSC test shows that its glass transition temperature T g =310℃, mechanical properties test shows that its tensile strength is 129MPa.
[0103] Example 3
[0104] Preparation of membrane No. 3 [Method (a)]:
[0105]
[0106] According to the molar ratio of 1:1, dry Py-O-PBI (710.8 mg, 2 mmol) and 1-(2-bromotetrafluoroethyl)-1,2,4-triazole (495.96 mg, 2.0 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMF (22.928 g of N,N-dimethylformamide), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80°C for two hours, and then further heated to 200°C for 4 hours to obtain proton exchange membrane No. 3. The thickness of the membrane is 26 μm (micrometer), and the DSC test shows that its glass transition temperature T g =318℃, mechanical properties test shows that its tensile strength is 132MPa.
[0107] Example 4
[0108] Preparation of membrane No. 4 [Method (a)]:
[0109]
[0110] According to the molar ratio of 1:0.8, dry OO-PBI (987.1 mg, 2 mmol) and 1-(2-bromotetrafluoroethyl) tetrazole (398.4 mg, 1.6 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry NMP (12.469 g of N-methylpyrrolidone), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 10%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80°C for two hours, and then further heated to 200°C for 5 hours to obtain a No. 4 proton exchange membrane. The thickness of the membrane is 38 μm (micrometer), and the DSC test shows that its glass transition temperature T g =323℃, mechanical properties test shows that its tensile strength is 137MPa.
[0111] Example 5
[0112] Preparation of No. 5 membrane [Method (a)]:
[0113]
[0114] According to the molar ratio of 1:0.6, dry F6-PBI (1069.0 mg, 2 mmol) and 2-(bromodifluoromethyl) tetrazole (238.8 mg, 1.2 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N, N-dimethylacetamide, 24.847 g), heated to 160 ° C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast on a 10 cm × 10 cm glass plate, and then placed in a blast oven at 90 ° C for two hours, and then further heated to 200 ° C for 4 hours to obtain a proton exchange membrane No. 5. The thickness of the membrane is 29 μm (micrometer), and the DSC test shows that its glass transition temperature T g =296℃, mechanical properties test shows that its tensile strength is 124MPa.
[0115] Example 6
[0116] Preparation of No. 6 membrane [Method (a)]:
[0117]
[0118] According to the molar ratio of 1:2.4, dry O-PBI (800.9 mg, 2 mmol) and 1-(chloromethyl)imidazole (559.4 mg, 4.8 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N, N-dimethylacetamide, 12.243 g), heated to 160 ° C and refluxed for a period of time to prepare a solution with a solid content of 10%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast on a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80 ° C for two hours, and then further heated to 200 ° C for 3 hours to obtain a No. 6 proton exchange membrane. The thickness of the membrane is 32 μm (micrometer), and the DSC test shows that its glass transition temperature T g =309℃, mechanical properties test shows that its tensile strength is 131MPa.
[0119] Example 7
[0120] Preparation of No. 7 membrane [Method (a)]:
[0121]
[0122] According to the molar ratio of 1:3, dry SO2-PBI (987.1 mg, 2 mmol) and 1-(2-chloroethyl)pyrazole (783.5 mg, 6.0 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N, N-dimethylacetamide, 33.641 g), heated to 160 ° C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast on a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80 ° C for two hours, and then further heated to 200 ° C for 5 hours to obtain a No. 7 proton exchange membrane. The thickness of the membrane is 33 μm (micrometer), and the DSC test shows that its glass transition temperature T g =297℃, mechanical properties test shows that its tensile strength is 126MPa.
[0123] Example 8
[0124] Preparation of No. 8 membrane [Method (a)]:
[0125]
[0126] According to the molar ratio of 1:2.4, dry Py-PBI (309.1 mg, 1 mmol) and 1-(2-bromoethyl)imidazole (420.1 mg, 2.4 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N,N-dimethylacetamide, 11.827 g), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After the filtrate was degassed, it was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80°C for two hours, and then further heated to 200°C for 4 hours to obtain a No. 8 proton exchange membrane. The thickness of the membrane is 15 μm (micrometer), and the DSC test shows that its glass transition temperature T g =315℃, mechanical properties test shows that its tensile strength is 135MPa.
[0127] Example 9
[0128] Preparation of No. 9 membrane [Method (a)]:
[0129]
[0130] According to the molar ratio of 1:3, dry S-PBI (416.1 mg, 1 mmol) and 1-(2-bromoethyl)-1,2,4-triazole (528.1 mg, 3 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N,N-dimethylacetamide, 15.404 g), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven at 80°C for two hours, and then further heated to 200°C for 4 hours to obtain a No. 9 proton exchange membrane. The thickness of the membrane is 23 μm (micrometer), and the DSC test shows that its glass transition temperature T g =299℃, mechanical properties test shows that its tensile strength is 128MPa.
[0131] Example 10
[0132] Preparation of membrane No. 10 [Method (a)]:
[0133]
[0134] According to the molar ratio of 1:1.8, dry poly[2,2′-(m-phenylene)-5,5′-di(benzimidazolyl)sulfone] (372.1 mg, 1 mmol) and 1-(2-chloroethyl)-1,2,3-triazole (236.8 mg, 1.8 mmol) were weighed. Under the protection of nitrogen, the mixture of the two was dissolved in dry DMAC (N,N-dimethylacetamide, 11.569 g), heated to 160°C and refluxed for a period of time to prepare a solution with a solid content of 5%, filtered, and the insoluble matter was filtered out. After degassing, the filtrate was cast onto a 10 cm×10 cm glass plate, and then placed in a blast oven at 80°C for two hours, and then further heated to 200°C for one hour to obtain a No. 10 proton exchange membrane. The thickness of the membrane is 21 μm (micrometer), and the DSC test shows that its glass transition temperature T g =306℃, mechanical properties test shows that its tensile strength is 127MPa.
[0135] Embodiment 11
[0136] Preparation of membrane No. 11 [Method (b)]:
[0137]
[0138] Weigh dry poly[2,2′-(2″,7″-naphthylene)-5,5′-bibenzimidazole] (358.1 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 17.547 g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add LiH (19.08 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 1-(2-bromoethyl)tetrazolyl (389.4 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solids, filter to obtain solids, wash the solids three times with water, then wash them twice with ethanol, and then put them into a vacuum oven and dry them at 100°C for 5 hours. The obtained solid was dissolved again in dry DMAC (N, N-dimethylacetamide) to prepare a solution with a solid content of 5%, and the insoluble matter was filtered off. The filtrate was degassed and then cast onto a 10 cm × 10 cm glass plate, and then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for 2 hours to obtain proton exchange membrane No. 11. The thickness of the membrane is 20 μm (micrometers), and the DSC test shows that its glass transition temperature T g =311℃, mechanical properties test shows that its tensile strength is 138MPa.
[0139] Example 12
[0140] Preparation of membrane No. 12 [Method (b)]:
[0141]
[0142] Weigh dry poly[2,2′-[4″,4″′-diphenylmethane]-5,5′-bibenzimidazole] (398.2 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 19.512 g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add NaH (57.6 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 2-(2-chloroethyl)tetrazolyl (291.6 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solid, filter to obtain solid, wash the solid three times with water, then wash it twice with ethanol, and then put it into a vacuum oven and dry it at 100°C for 5 hours. The obtained solid was dissolved again in dry DMAC (N, N-dimethylacetamide) to prepare a solution with a solid content of 5%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain a No. 12 proton exchange membrane. The thickness of the membrane is 21μm (micrometers), and the DSC test shows that its glass transition temperature T g =289℃, mechanical properties test shows that its tensile strength is 129MPa.
[0143] Example 13
[0144] Preparation of membrane No. 13 [Method (b)]:
[0145]
[0146] Weigh dry poly[2,2′-(m-phenylene)-5,5′-di(benzimidazolyl)ketone] (336.1 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 16.469 g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add KH (96.3 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 1-(2-chloroethyl)imidazole (287.3 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solids, filter to obtain solids, wash the solids three times with water, then wash them twice with ethanol, and then put them into a vacuum oven and dry them at 100°C for 5 hours. The obtained solid was dissolved again in dry DMAC (N, N-dimethylacetamide) to prepare a solution with a solid content of 4%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain proton exchange membrane No. 13. The thickness of the membrane is 26μm (micrometers), and the DSC test shows that its glass transition temperature T g =316℃, mechanical properties test shows that its tensile strength is 135MPa.
[0147] Embodiment 14
[0148] Preparation of membrane No. 14 [Method (b)]:
[0149]
[0150] Weigh dry poly[2,2′-(m-phenylene)-5,5′-di(benzimidazolyl)methane] (322.1 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 15.783 g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add LiH (19.08 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 1-(2-chloroethyl)-1,2,4-triazole (289.4 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solids, filter to obtain solids, wash the solids three times with water, then wash them twice with ethanol, and then put them in a vacuum oven and dry them at 100°C for 5 hours. The obtained solid was dissolved in dry DMAC (N, N-dimethylacetamide) again to prepare a solution with a solid content of 5%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain No. 14 proton exchange membrane. The thickness of the membrane is 21μm (micrometers), and the DSC test shows that its glass transition temperature T g =305℃, mechanical properties test shows that its tensile strength is 129MPa.
[0151] Embodiment 15
[0152] Preparation of membrane No. 15 [Method (b)]:
[0153]
[0154] Weigh dry poly[2,2′-(m-phenylene)-5,5′-di(benzimidazolyl)sulfide](340.1mg, 1mmol) and dissolve it in dry DMAC(N,N-dimethylacetamide, 16.665g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add LiH(19.08mg, 2.4mmol), heat to 160℃ and reflux for 24 hours, then add 1-(2-chloroethyl)tetrazolyl(291.6mg, 2.2mmol) and continue to react for 24 hours. Then pour the reaction solution into 500mL deionized water, precipitate solid, filter to obtain solid, wash the solid three times with water, then wash twice with ethanol, and then put it into a vacuum oven and dry it at 100℃ for 5 hours. The obtained solid was dissolved again in dry DMAC (N, N-dimethylacetamide) to prepare a solution with a solid content of 4%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain No. 15 proton exchange membrane. The thickness of the membrane is 24μm (micrometers), and the DSC test shows that its glass transition temperature T g =303℃, mechanical properties test shows that its tensile strength is 138MPa.
[0155] Example 16
[0156] Preparation of membrane No. 16 [Method (b)]:
[0157]
[0158] Weigh dry poly[2,2′-[4″,4″′-(methyldiphenylphosphine oxide)]-5,5′-di(benzimidazole) ether] (462.4 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 22.658 g) under nitrogen protection to prepare a solution with a solid content of 2%. Then add KH (96.3 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 1-(2-chloroethyl)pyrazole (287.3 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solids, filter to obtain solids, wash the solids three times with water, then wash them twice with ethanol, and then put them into a vacuum oven and dry them at 100°C for 5 hours. The obtained solid was dissolved again in dry DMAC (N, N-dimethylacetamide) to prepare a solution with a solid content of 4%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain No. 16 proton exchange membrane. The thickness of the membrane is 25μm (micrometers), and the DSC test shows that its glass transition temperature T g =294℃, mechanical properties test shows that its tensile strength is 130MPa.
[0159] Embodiment 17
[0160] Preparation of membrane No. 17 [Method (b)]:
[0161]
[0162] Weigh dry ABPBI (116.1 mg, 1 mmol) and dissolve it in dry DMAC (N,N-dimethylacetamide, 5.689 g) under the protection of nitrogen to prepare a solution with a solid content of 2%. Then add NaH (57.6 mg, 2.4 mmol), heat to 160°C and reflux for 24 hours, then add 1-(chloromethyl)imidazole (256.4 mg, 2.2 mmol), and continue to react for 24 hours. Then pour the reaction solution into 500 mL of deionized water, precipitate solids, filter to obtain solids, wash the solids three times with water, then wash them twice with ethanol, and then put them into a vacuum oven and dry them at 100°C for 5 hours. The obtained solid was dissolved in dry DMAC (N, N-dimethylacetamide) again to prepare a solution with a solid content of 5%, filtered to remove insoluble matter, and the filtrate was degassed and cast onto a 10cm×10cm glass plate, then placed in a blast oven and dried at 80°C for two hours, and then further heated to 120°C and dried for one hour to obtain No. 17 proton exchange membrane. The membrane has a thickness of 18μm (micrometers), and DSC test shows that its glass transition temperature T g =315℃, mechanical properties test shows that its tensile strength is 146MPa.
[0163] Test Example:
[0164] The proton conductivity of commercial PBI membranes and membrane No. 1 (Example 1), membrane No. 2 (Example 2), membrane No. 3 (Example 3), membrane No. 4 (Example 4), membrane No. 5 (Example 5), membrane No. 6 (Example 6), membrane No. 7 (Example 7), and membrane No. 8 (Example 8) in this patent were tested using a two-electrode method using a Membrane Test System 740 device.
[0165] Test method:
[0166] (1) Pre-test processing:
[0167] Each group of membranes was immersed in 85% phosphoric acid at 160° C. for 6 hours, then taken out and dried for testing.
[0168] (2) Formal test (test equipment: Membrane Test System 740):
[0169] Cut the sample film to be tested into a 1cm×3cm shape;
[0170] Use conductive adhesive to glue the GDE with Pt / C catalyst on the metal sheets of the two electrode fixtures, one on the top and one on the bottom, and install the cut film to be tested in the middle of the GDE, and clamp the fixture;
[0171] Turn on the power of MTS 740 and place the fixture containing the film to be tested into the test chamber of the device.
[0172] Open the instrument test program and connect the pipeline connecting the gas cylinder to the instrument. Adjust the N2 pipeline pressure to 0.5MPa and the H2 pipeline pressure to 0.4MPa. Check that the indicator lights in the program indicate normal operation and check the connection between the chemical workstation and the 740 operating chamber. The instrument schematic diagram is as follows:
[0173] When testing the membrane sample, N2 should be blown in for 10 minutes to remove the air in the chamber at a blowing rate of 500 sccm / min. During the operation of the instrument, when the temperature and humidity (relative humidity is 2%) reach the set values and stabilize, the test can be started.
[0174] The impedance spectrum was automatically obtained using the MTS740 program, and the membrane resistance value R was obtained from the spectrum.
[0175] Data processing: The conductivity is calculated by ρ = L / (Rs×A).
[0176] L: film thickness;
[0177] Rs: membrane resistance read by impedance spectroscopy
[0178] A: Measured area
[0179] At the end of the test, N2 must be purged for 15 minutes to remove moisture from the instrument, and finally the program and instrument power must be turned off.
[0180] Conductivity test data
[0181]
[0182]
[0183] The results are shown in Table 1 and Figure 1 As shown in . The results show that the conductivity of the proton exchange membranes prepared by the various polymers of the present application is significantly higher than that of the commercial PBI membrane of the control group. This shows that the polybenzimidazole polymer of the present application has higher proton conductivity and is more suitable for use as a proton exchange membrane material for fuel cells.
[0184] Fenton reagent oxidative degradation experiment:
[0185] This experiment tested the oxidation degradation of membrane No. 7 (Example 7), membrane No. 8 (Example 8), imported PBI membrane, membrane No. 1 (Example 1), and membrane No. 6 (Example 6) in the patent (201710084102.X) previously applied by our group in Fenton's reagent. The test was considered to be over when the membrane ruptured.
[0186] The test conditions are: Fenton reagent: 3% H2O2, 4ppm FeSO4.7H2O, test temperature is 70℃, and new Fenton reagent is replaced every 24 hours. Record the change of membrane weight with oxidation time [Note: When recording the weight, first take the membrane out of the solution and wash it with deionized water several times, then dry it in a vacuum oven at 100℃ for two hours, weigh it after cooling to room temperature, and record the percentage of the initial weight].
[0187] The test results are as follows Figure 2 As shown, the antioxidant capacity of the membrane in this patent application is significantly higher than that of the membrane sample in the patent (201710084102.X) previously applied by the applicant, and is also stronger than the antioxidant capacity of the imported PBI membrane. This shows that the proton exchange membrane in this application has a higher antioxidant capacity and is more suitable for use as a proton exchange membrane material for fuel cells.
[0188] All documents mentioned in the present invention are cited as references in this application, just as each document is cited as reference individually. In addition, it should be understood that after reading the above teachings of the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.
Claims
1. A fuel cell proton exchange membrane, characterized in that: The proton exchange membrane is composited with a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring as raw materials, wherein the molar ratio of A to B is nA:nB=1:0.1-6.0; and the polybenzimidazole polymer A is selected from the following group: Wherein, n=2-10000; R is selected from the group consisting of O, S, NH, C(O), S(O)2, unsubstituted or halogenated C1-C6 alkylene, unsubstituted or halogenated C2-C6 alkenylene; R 1 Select from the following group: The nitrogen-containing heteroaromatic ring-substituted halogenated alkane B is a C1-C10 halogenated alkane, and the nitrogen-containing heteroaromatic ring is a 5-7-membered nitrogen-containing heteroaromatic ring; The polybenzimidazole type compound A is selected from the following group: The structure of the nitrogen-containing heteroaromatic ring-substituted halogenated alkane B is: R 2 -(CH2) m X or R 2 -(CF2) m X in: m=1-9; X=Cl or Br; —R 2 Select from the following group:
2. The fuel cell proton exchange membrane according to claim 1, characterized in that: The molar ratio of A to B is nA:nB=1:0.5-3.
3. The method for preparing a fuel cell proton exchange membrane according to any one of claims 1 to 2, characterized in that: The preparation method comprises the steps of: (i) dissolving a polybenzimidazole type compound A and a halogenated alkane B substituted with a nitrogen-containing heteroaromatic ring in an organic solvent to form a mixed solution; (ii) filtering to remove insoluble matter to obtain a mixed filtrate; (iii) degassing the mixed filtrate; (iv) forming a membrane of the mixed filtrate subjected to the deaeration treatment to obtain a proton exchange membrane.
4. The method for preparing a fuel cell proton exchange membrane according to any one of claims 1 to 2, characterized in that: The preparation method comprises the steps of: (1) dissolving a polybenzimidazole type compound A in a first organic solvent, and then adding a base to form a mixed solution; (2) adding a halogenated alkane B substituted with a heteroaromatic ring to the mixed solution obtained in the above step (1), heating the mixture for reaction, and obtaining a reaction mixture; (3) pouring the reaction mixture into water to precipitate solid; (4) dissolving the solid in a second organic solvent to prepare a solution with a certain solid content; the solid content of the mixed solution is 1-40 wt %; (5) filtering the solution to remove insoluble matter to obtain a filtrate; (6) degassing the filtrate to obtain a degassed filtrate; (7) Casting the degassed filtrate into a membrane to obtain a proton exchange membrane.
5. The preparation method according to claim 3 or 4, characterized in that: In the method, the molar ratio of the polybenzimidazole type compound A to the heteroaromatic ring substituted halogenated alkane B is 1:0.1-6.
6. The preparation method according to claim 3 or 4, characterized in that: The organic solvent, the first organic solvent and the second organic solvent are independently strong polar organic solvents.
7. The preparation method according to claim 3 or 4, characterized in that: The organic solvent, the first organic solvent and the second organic solvent are each independently selected from the following group: DMSO, DMF, DMAC, NMP, or a combination thereof.
8. The preparation method according to claim 4, characterized in that: In the step (1), the base is selected from the following group: NaH, LiH, KH, Na2CO3, K2CO3, or a combination thereof.
9. The preparation method according to claim 4, characterized in that: The molar ratio of the polybenzimidazole type compound A to the base is 1:0.1-3.