Silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material and preparation method thereof
The one-step hydrothermal method prepares silicon oxide@iron oxide/carbon composite materials, which solves the problems of high cost and poor cycle performance of lithium-ion battery anode materials, achieves improved conductivity and structural stability, and significantly improves electrochemical performance.
Patent Information
- Application Number
- CN202110535234.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-05-17
AI Technical Summary
Existing anode materials for lithium-ion batteries have problems such as high cost, difficulty in operation, and poor electrochemical performance. In particular, silicon oxide materials have large volume expansion during cycling, poor conductivity, and poor cycle performance.
Use a one-step hydrothermal method to mix silicon oxide, hydrated ferric chloride, urea, hydrochloric acid and sugar, add propanol or ethanol as the solvent, stir magnetically at room temperature and perform a hydrothermal reaction at 160 to 180°C, followed by washing and drying. The silicon oxide@iron oxide/carbon composite lithium-ion battery negative electrode material is prepared by maintaining the temperature at 400-600°C under a protective atmosphere.
This method has simple process and low cost, improves the conductivity and cycle performance of silicon oxide@iron oxide/carbon composite materials, alleviates the problem of volume expansion, and ensures structural stability and excellent electrochemical performance.
Smart Images

Figure CN113346056B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of negative electrode materials for lithium-ion batteries, and specifically relates to a silicon oxide@iron oxide / carbon composite negative electrode material for lithium-ion batteries and a preparation method thereof. Background Art
[0002] With the continuous advancement of science and technology, human demand for clean energy and energy storage equipment is gradually increasing. The emergence of new energy vehicles has pushed the demand for lithium-ion batteries to a new height. Lithium-ion batteries have attracted widespread attention as an emerging energy storage device. Since the commercialization of lithium-ion batteries, researchers have made great progress in improving battery capacity and energy density by optimizing the structure of lithium-ion batteries and using new electrode materials. Existing commercial negative electrode materials are mostly graphite-based negative electrode materials with reliable performance. However, their low specific capacity has led people to continue to look for new alternative high-capacity negative electrode materials.
[0003] Silicon oxide negative electrode materials have high capacity, low operating voltage, environmental friendliness and low price, and are considered to be one of the most promising new negative electrode materials. However, silicon oxide has problems such as large volume expansion (~200%), poor conductivity, low initial coulombic efficiency, easy crushing of multiple active materials and poor cycle performance during the cycle, which has attracted the attention of technicians in this field. The existing solutions mainly include nano-sizing, carbon composite and structural optimization.
[0004] At present, there are many kinds of materials prepared by carbon composites, such as the patented technology of "a method for preparing a graphene-coated silicon-carbon composite negative electrode material and a lithium-ion battery" (CN106058257A). The nano-silicon negative electrode material and the modified graphene are tightly combined to form an elastic network structure, which ensures the strength and flexibility of the electrode and has a certain porosity. However, the graphene raw materials used increase the cost of preparation and have limited improvement on the conductivity of the composite material; such as the patented technology of "silicon dioxide carbon composite negative electrode material and modified silicon dioxide carbon composite negative electrode material and its preparation method and application" (CN105789575B). The materials prepared by this method have good cycle stability, but the halloysite impurities used are many and need to be calcined at high temperature to remove impurities, which is a complicated process. The capacity of the final battery decays rapidly during the cycle process; for example, the patented technology of "A method for preparing a lithium-ion battery silicon oxide / carbon composite negative electrode material" (CN103236520B) uses resorcinol and formaldehyde as matrix raw materials and an organic silicon source to prepare a composite material. Although the product prepared by this technology has a small particle size and good cycle performance, the freeze-drying and high-temperature carbonization processes are relatively complex and costly, which limits industrialization.
[0005] In summary, the existing negative electrode materials for lithium-ion batteries not only have technical defects such as high cost, difficult operation and difficulty in industrialization, but also the electrochemical performance of the prepared products needs to be improved. Summary of the invention
[0006] The present invention aims to overcome the defects of the prior art and aims to provide a method for preparing a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material with low cost, simple process and convenient operation. The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared by this method has excellent electrochemical performance.
[0007] To achieve the above object, the technical solution adopted by the present invention is:
[0008] 1) 0.5-1.5 mol of silicon oxide, 0.5-1.5 mol of hydrated ferric chloride, 0.5-1.5 mol of urea, 0.1-0.3 mol of hydrochloric acid and 0.1-0.5 mol of sugar are mixed, and 1-5 mol of propanol or ethanol is added as a solvent, and magnetic stirring is performed at room temperature for 30-60 minutes to obtain a mixed solution.
[0009] 2) The mixed solution is transferred to a hydrothermal reaction kettle, subjected to a hydrothermal reaction at 160-180° C. for 10-12 h, and filtered to obtain a mixed material.
[0010] 3) The mixture is washed alternately with ethanol and deionized water for 3 to 5 times, dried at 60 to 80° C. for 6.0 to 8.0 hours, kept warm at 400 to 600° C. for 2 to 4 hours in a protective atmosphere, and cooled naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0011] The silicon oxide is one or more of silicon monoxide and silicon dioxide; the particle size of the silicon oxide is 1 to 3 μm, and the purity of the silicon oxide is ≥99%.
[0012] The particle size of the hydrated ferric chloride is 3-5 μm; the purity of the hydrated ferric chloride is ≥99%.
[0013] The sugar is one or more of glucose, sucrose and starch.
[0014] The protective atmosphere is argon or nitrogen.
[0015] Due to the adoption of the above technical solution, the present invention has the following positive effects compared with the prior art:
[0016] The present invention adopts a one-step hydrothermal method, mixing silicon oxide, hydrated ferric chloride, urea, hydrochloric acid and sugar, adding propanol or ethanol, magnetic stirring, hydrothermal reaction, washing, drying, keeping warm for 2 to 4 hours under a protective atmosphere and 400 to 600° C., and cooling naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material. The method is simple in process, easy to operate and low in cost.
[0017] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared by the one-step hydrothermal method of the present invention overcomes the defect of poor conductivity of silicon oxide itself, and the outer carbon layer has good conductivity. TEM test shows that the thickness of the carbon layer is 50 to 100 nm, thereby improving the conductivity of the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0018] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared by the present invention alleviates the problem of volume expansion. The iron oxide microspheres are uniformly agglomerated outside the silicon oxide particles and form a whole with the outermost carbon layer. The volume expansion of the silicon oxide during the cycle is transferred to the outer iron oxide and carbon layers, which buffers the internal stress generated by the volume expansion, ensures the stability of the structure, and improves the cycle performance of the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0019] The present invention applies the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material to a lithium ion battery, and conducts an electrochemical performance test: when the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is charged and discharged at 100mA / g, the discharge specific capacity is 1100-1550mAh / g; after 100 cycles, the discharge specific capacity is 590-670mAh / g.
[0020] Therefore, the present invention has the characteristics of low cost, simple process and convenient operation, and the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material has excellent electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is an XRD diagram of a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared by the present invention;
[0022] Figure 2 yes Figure 1 The SEM image of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material shown;
[0023] Figure 3 yes Figure 1 TEM image of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material shown;
[0024] Figure 4 yes Figure 1 The capacity decay diagram of silicon oxide@iron oxide / carbon composite lithium-ion battery negative electrode material is shown. DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, but is not intended to limit the scope of protection thereof.
[0026] In this specific implementation mode:
[0027] The particle size of the silicon oxide is 1-3 μm, and the purity of the silicon oxide is ≥99%.
[0028] The particle size of the hydrated ferric chloride is 3-5 μm; the purity of the hydrated ferric chloride is ≥99%.
[0029] This will not be described in detail in the embodiments.
[0030] Example 1
[0031] A silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material and its preparation method. The preparation method described in this embodiment is:
[0032] 1) 0.5 mol of silicon oxide, 1.5 mol of hydrated ferric chloride, 0.5 mol of urea, 0.1 mol of hydrochloric acid and 0.1 mol of sugar were mixed, and 1 mol of propanol was added as a solvent. The mixture was stirred magnetically for 30 minutes at room temperature to obtain a mixed solution.
[0033] 2) The mixed solution was transferred to a hydrothermal reactor, subjected to a hydrothermal reaction at 160° C. for 10 h, and filtered to obtain a mixed material.
[0034] 3) The mixture was washed alternately with ethanol and deionized water for 3 times, dried at 60° C. for 8.0 h, kept at 400° C. for 2 h in a protective atmosphere, and cooled naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0035] In this embodiment: the silicon oxide is silicon monoxide; the sugar is glucose; and the protective atmosphere is argon.
[0036] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in this embodiment is applied to a lithium ion battery, and an electrochemical performance test is performed: the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is used as a working electrode, metallic lithium is used as a counter electrode, and 1 mol / L LiF6 / EC-DMC (volume ratio 1: 1) is used as an electrolyte. A simulated battery is assembled in an argon atmosphere glove box, and a charge and discharge test is performed on the simulated battery. The voltage range is 0.01 ~ 3V (vs. Li + / Li), the current density is 100mA / g. The test results show that the specific capacity curve of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material when charged and discharged under 100mA / g is as follows Figure 4 As shown, the discharge capacity is 1125.5 mAh / g; after 100 cycles, the discharge capacity is 595 mAh / g;
[0037] Example 2
[0038] A silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material and its preparation method. The preparation method described in this embodiment is:
[0039] 1) 1.0 mol of silicon oxide, 1.0 mol of hydrated ferric chloride, 1.0 mol of urea, 0.2 mol of hydrochloric acid and 0.3 mol of sugar were mixed, and 3 mol of ethanol was added as a solvent. The mixture was stirred magnetically for 45 minutes at room temperature to obtain a mixed solution.
[0040] 2) The mixed solution was transferred to a hydrothermal reactor, subjected to a hydrothermal reaction at 170° C. for 11 h, and filtered to obtain a mixed material.
[0041] 3) The mixture was washed alternately with ethanol and deionized water for 4 times, dried at 70° C. for 7.0 h, kept at 500° C. for 3 h in a protective atmosphere, and cooled naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0042] In this embodiment: the silicon oxide is silicon dioxide; the sugar is sucrose; and the protective atmosphere is nitrogen.
[0043] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in this embodiment is applied to a lithium ion battery, and an electrochemical performance test is performed: the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is used as a working electrode, metallic lithium is used as a counter electrode, and 1 mol / L LiF6 / EC-DMC (volume ratio 1: 1) is used as an electrolyte. A simulated battery is assembled in an argon atmosphere glove box, and a charge and discharge test is performed on the simulated battery. The voltage range is 0.01 ~ 3V (vs. Li + / Li), the current density is 100mA / g. The test results show that the discharge capacity of the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is 1239.6mAh / g under 100mA / g conditions; after 100 cycles, the discharge capacity is 637mAh / g.
[0044] Example 3
[0045] A silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material and its preparation method. The preparation method described in this embodiment is:
[0046] 1) 1.5 mol of silicon oxide, 0.5 mol of hydrated ferric chloride, 1.5 mol of urea, 0.3 mol of hydrochloric acid and 0.5 mol of sugar were mixed, and 5 mol of propanol was added as a solvent. The mixture was magnetically stirred for 60 minutes at room temperature to obtain a mixed solution.
[0047] 2) The mixed solution was transferred to a hydrothermal reactor, subjected to hydrothermal reaction at 180° C. for 12 h, and filtered to obtain a mixed material.
[0048] 3) The mixture was washed alternately with ethanol and deionized water for 5 times, dried at 80° C. for 6.0 h, kept at 600° C. for 4 h in a protective atmosphere, and cooled naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0049] In this embodiment: the silicon oxide is silicon monoxide; the sugar is starch; and the protective atmosphere is argon.
[0050] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in this embodiment is applied to a lithium ion battery, and an electrochemical performance test is performed: the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is used as a working electrode, metallic lithium is used as a counter electrode, and 1 mol / L LiF6 / EC-DMC (volume ratio 1: 1) is used as an electrolyte. A simulated battery is assembled in an argon atmosphere glove box, and a charge and discharge test is performed on the simulated battery. The voltage range is 0.01 ~ 3V (vs. Li + / Li), the current density is 100mA / g. The test results show that the discharge capacity of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is 1532mAh / g under 100mA / g; after 100 cycles, the discharge capacity is 663mAh / g;
[0051] Compared with the prior art, this specific implementation has the following positive effects:
[0052] This specific embodiment adopts a one-step hydrothermal method, mixing silicon oxide, hydrated ferric chloride, urea, hydrochloric acid and sugar, adding propanol or ethanol, magnetic stirring, hydrothermal reaction, washing, drying, keeping warm for 2 to 4 hours at 400 to 600°C in a protective atmosphere, and cooling naturally to obtain silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material. The method is simple in process, easy to operate and low in cost.
[0053] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared by a one-step hydrothermal method in this specific embodiment is shown in the accompanying drawings. Figure 1 This is an XRD diagram of a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in Example 1; Figure 2 yes Figure 1 The SEM image of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material shown; Figure 3 yes Figure 1 TEM image of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material shown; Figure 4 yes Figure 1 The capacity decay diagram of silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is shown. Figure 1It can be seen that the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is a carbon composite material of amorphous silicon oxide and crystalline iron oxide; Figure 2 It can be seen that the structure of the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is uniform and coated with a carbon layer on the outside; Figure 3 It can be seen that the thickness of the carbon layer on the outside of the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is 50-100nm; Figure 4 It can be seen that the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material has excellent electrochemical performance and slow capacity decay. Therefore, the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material effectively overcomes the defect of poor conductivity of silicon oxide itself, and the outer carbon layer has good conductivity, which significantly improves the conductivity.
[0054] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in this specific embodiment alleviates the problem of volume expansion. The iron oxide microspheres are uniformly agglomerated outside the silicon oxide particles and form a whole with the outermost carbon layer. The volume expansion of silicon oxide during the cycle is transferred to the outer iron oxide and carbon layers, which buffers the internal stress generated by the volume expansion, ensures the stability of the structure, and improves the cycle performance of the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material.
[0055] The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared in this specific embodiment is applied to lithium ion batteries. The electrochemical performance test shows that when the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is charged and discharged under 100mA / g conditions, the discharge specific capacity is 1100 ~ 1550mAh / g; after 100 cycles, the discharge specific capacity is 590 ~ 670mAh / g.
[0056] Therefore, this specific implementation has the characteristics of low cost, simple process and convenient operation, and the prepared silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material has excellent electrochemical performance.
Claims
1. A method for preparing a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material, characterized in that The preparation method is: 1) Mix 0.5-1.5 mol of silicon oxide, 0.5-1.5 mol of hydrated ferric chloride, 0.5-1.5 mol of urea, 0.1-0.3 mol of hydrochloric acid and 0.1-0.5 mol of sugar, add 1-5 mol of propanol or ethanol as solvent, and stir magnetically for 30-60 min at room temperature to obtain a mixed solution; 2) transferring the mixed solution to a hydrothermal reactor, performing a hydrothermal reaction at 160-180° C. for 10-12 hours, filtering, and obtaining a mixed material; 3) washing the mixture with ethanol and deionized water alternately for 3 to 5 times, drying at 60 to 80° C. for 6.0 to 8.0 hours, keeping the mixture at 400 to 600° C. for 2 to 4 hours under a protective atmosphere, and cooling the mixture naturally to obtain a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material; The silicon oxide is one or more of silicon monoxide and silicon dioxide; the particle size of the silicon oxide is 1-3 μm, and the purity of the silicon oxide is ≥99%; The particle size of the hydrated ferric chloride is 3-5 μm; the purity of the hydrated ferric chloride is ≥99%; The sugar is one or more of glucose, sucrose and starch; The protective atmosphere is argon or nitrogen.
2. A silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material, characterized in that The silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material is a silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material prepared according to the preparation method of the silicon oxide @ iron oxide / carbon composite lithium ion battery negative electrode material according to claim 1.