A preparation method and product of carbon nanotube-loaded iron oxide and its application
By calcining carbon nanotubes in an oxygen atmosphere and using surfactant to assist dispersion, the problem of using strong acids and strong oxidants in the prior art was solved, and iron oxides supported by carbon nanotubes containing high oxygen content and high adhesion amounts were prepared. Complex, suitable for lithium-ion batteries and other fields, realizes a safe, environmentally friendly and efficient preparation process.
Patent Information
- Application Number
- CN202110828238.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-07-22
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-07-22
AI Technical Summary
The existing preparation methods for carbon nanotube-loaded iron oxides require the use of a large number of corrosive strong acids and strong oxidants, which leads to high environmental pollution and experimental risks, and is not suitable for large-scale production.
By calcining carbon nanotubes in an oxygen atmosphere, oxygen-containing groups are attached to the surface of their surfaces, and surfactant assists dispersed in polar solvents, the iron oxide precursor is added to attach it through electrostatic action and converted into iron oxidation in situ and prepare carbon nanotube-loaded iron oxide composite.
This method avoids the use of strong acids and strong oxidants, improves the specific surface area and oxygen content of carbon nanotubes, and the adhesion of iron oxides reaches 70 wt.%, and significantly improves the circulation capacity and Coulomb efficiency of lithium-ion batteries. Simple, safe, environmentally friendly, suitable for large-scale preparation.
Smart Images

Figure CN113548658B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material preparation, and relates to a composite modification technology of carbon nanotube materials, in particular to a preparation method of a composite of carbon nanotubes and iron oxides. Background Art
[0002] Carbon materials have excellent properties such as high electrical conductivity, corrosion resistance, high temperature resistance, and light weight, and have been widely studied and reported in the fields of electrochemistry and electromagnetic compatibility. Carbon nanotubes (CNTs) are one-dimensional hollow tubular carbon materials formed by curling single or multi-layer graphene. They have excellent electrical, thermal, and mechanical properties and are widely used in electromagnetic interference shielding materials and stealth materials, CNTs composite materials, electrochemical devices, catalyst carriers, and sewage treatment. In the field of carbon nanotube composite materials, it is generally necessary to first attach oxygen-containing groups, hydroxyl groups (-OH), carboxyl groups (-COOH), and ethers (COC) on the surface of CNTs, and then load metal oxides, metals, non-metals, etc. to obtain CNTs composites. In the past, the method of attaching oxygen-containing groups was mainly through oxidation with reagents such as nitric acid, a mixture of sulfuric acid and nitric acid, a mixture of sulfuric acid and hydrogen peroxide, and ozone. The attachment of oxygen-containing groups to CNTs can increase its polarity, making it soluble in polar solvents such as water, and can adsorb positively charged load precursors in the solution on its surface and convert them into target products. Based on the characteristics of ferroferric oxide (Fe3O4) such as low price, environmental friendliness, superparamagnetism and excellent electrochemical properties, it has been widely studied and reported in the fields of lithium-ion batteries, supercapacitors, electromagnetic interference, magnetic recording, catalysis, and medicine. The composite of Fe3O4 and CNTs will show more excellent characteristics in some related fields.
[0003] In the reports of preparing CNTs loaded with Fe3O4, it is generally first oxidized by a highly corrosive acid such as nitric acid and sulfuric acid to attach oxygen-containing groups, and finally obtain a Fe3O4 / CNTs complex. Chinese patent CN 109119625A discloses that CNTs are dispersed in concentrated nitric acid with a mass fraction of 65%-68% and then subjected to high-temperature acid treatment, and then the acidified CNTs are dispersed in deionized water, and ferric chloride hexahydrate, urea and potassium sodium tartrate are added to prepare a Fe3O4 / CNTs complex by hydrothermal reaction. Chinese patent CN 102671661A discloses that multi-walled carbon nanotubes (MWCNTs) are refluxed in at least one strong oxidant selected from concentrated sulfuric acid, concentrated nitric acid, hydrogen peroxide, saturated aqueous solution of ammonium persulfate and aqueous solution of potassium dichromate to obtain oxidized MWCNTs, and then mixed with water, an iron-containing compound and a reducing agent, and then a Fe3O4 / CNTs complex is prepared by hydrothermal reaction.
[0004] However, in the preparation of the above-mentioned Fe3O4 / CNTs composite, a large amount of corrosive strong acid and strong oxidant are needed to oxidize CNTs, which not only pollutes the environment but also increases the danger of the experiment. Summary of the invention
[0005] The purpose of the present invention is to overcome the shortcomings of the prior art and seek to design a simple, safe and large-scale production method for preparing carbon nanotubes (CNTs) loaded with iron oxide, a product and an application thereof. First, CNTs are calcined in an oxygen-containing atmosphere so that oxygen-containing groups are attached to their surfaces. Then, the CNTs with oxygen-containing groups attached are dispersed in a polar solvent such as water with the assistance of a surfactant. Then, an iron oxide precursor is added. The iron oxide precursor is attached to the surface of the CNTs through the electrostatic force generated between the two. Under the action of a surface additive, the iron oxide precursor is converted into iron oxide in situ through a liquid phase reaction to obtain a CNTs loaded with iron oxide composite.
[0006] In order to achieve the above object, the present invention provides a method for preparing carbon nanotube-loaded iron oxide in a first aspect, the method comprising the following steps:
[0007] (1) subjecting CNTs to a thermogravimetric test at a certain heating rate in an oxygen atmosphere to determine the initial weight loss temperature of CNTs;
[0008] (2) placing CNTs in a high-temperature furnace, heating the temperature to or above the initial weight loss temperature at a certain heating rate, introducing a small flow of oxygen-containing atmosphere, and maintaining this temperature for several hours to prepare CNTs with attached oxygen-containing groups;
[0009] (3) adding a certain amount of CNTs attached with oxygen-containing groups into a certain volume of polar solvent, obtaining a dispersion of CNTs attached with oxygen-containing groups by ultrasonic dispersion, and adding a certain amount of surfactant to assist dispersion according to the needs of dispersion conditions;
[0010] (4) adding a certain amount of iron oxide precursor and additives to the CNTs dispersion liquid attached with oxygen-containing groups, stirring and standing for a period of time to allow the iron oxide precursor to adhere to the surface of the CNTs attached with oxygen-containing groups through electrostatic action, and then preparing the CNTs-loaded iron oxide composite by a liquid phase method;
[0011] (5) The CNTs-loaded iron oxide composite is subsequently calcined in a high-temperature inert atmosphere to further improve the conductivity of the CNTs and the crystallinity of the iron oxide.
[0012] The second aspect of the present invention provides a composite material of CNTs loaded with iron oxides prepared by the above method.
[0013] The third aspect of the present invention provides the application of the above-mentioned CNTs-loaded iron oxide composite material in the fields of lithium-ion batteries, supercapacitors, electromagnetic interference, magnetic recording, catalysis, and medicine, especially in lithium-ion batteries.
[0014] Through the above technical solution, the present invention has the following beneficial effects:
[0015] The oxygen-containing groups attached to CNTs are obtained by heat treatment in an oxygen-containing atmosphere. The oxygen exists mainly in the form of carbon-oxygen double bonds connecting aromatic carbons, carbon-oxygen single bonds connecting aliphatic carbons, and carbon-oxygen single bonds connecting aromatic carbons. Heat treatment can greatly increase the oxygen content in CNTs. The mass fraction of oxygen in CNTs with attached oxygen-containing groups reaches more than 10wt.%, and can reach 15wt.%; the specific surface area of CNTs increases by at least 1.3 times.
[0016] The oxygen-containing groups on the surface of CNTs are helpful to load iron oxides. The precursor of iron oxides is uniformly attached to the surface of CNTs in the form of nanoparticles. The content of attached iron oxides can be as high as 70wt.%.
[0017] Furthermore, the obtained CNTs-loaded iron oxide composite material is used in lithium-ion batteries, which can significantly improve the cycle capacity while still maintaining a high coulombic efficiency and good cycle stability. Iron oxide and CNTs have a synergistic effect. On the one hand, the CNTs with oxygen-containing groups attached to the iron oxide can buffer the volume change of the iron oxide during the charge and discharge process. On the other hand, the CNTs with oxygen-containing groups attached provide a high-speed electron transmission channel. Furthermore, the porous characteristics of the CNTs with oxygen-containing groups attached are conducive to the transmission and diffusion of lithium ions.
[0018] In addition, the present invention avoids the use of corrosive strong acids and strong oxidants, and the process is simple, safe, environmentally friendly, and suitable for large-scale preparation; the CNTs-loaded iron oxide composite prepared by the present invention has broad application potential in lithium-ion batteries, supercapacitors, electromagnetic interference, magnetic recording, catalysis, medicine and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A thermogravimetric analysis curve of MWCNTs used in the present invention in an oxygen atmosphere;
[0020] Figure 2 X-ray photoelectron spectroscopy (XPS) diagram of MWCNTs with attached oxygen-containing groups and their raw materials prepared in Example 1 of the present invention;
[0021] Figure 3 This is a photograph of MWCNTs with attached oxygen-containing groups prepared in Example 1 of the present invention uniformly dispersed in water (1 mg / mL) after standing for 3 months;
[0022] Figure 4 This is a photo of the raw material MWCNTs prepared in Comparative Example 1 of the present invention dispersed in water;
[0023] Figure 5 This is a scanning electron microscope (SEM) image of heat-treated MWCNTs loaded with Fe3O4 prepared in Example 1 of the present invention;
[0024] Figure 6 X-ray diffraction (XRD) diagram of the heat-treated MWCNTs and the Fe3O4-loaded composite thereof prepared in Example 1 of the present invention;
[0025] Figure 7 This is a thermogravimetric analysis curve of the heat-treated MWCNTs-loaded Fe3O4 composite prepared in Example 1 of the present invention in an oxygen atmosphere;
[0026] Figure 8 This is a SEM image of heat-treated MWCNTs loaded with Fe2O3 prepared in Example 2 of the present invention;
[0027] Fig. 9 This is a SEM image of Fe2O3 loaded on MWCNTs raw material prepared in Comparative Example 1 of the present invention;
[0028] Fig.10 XRD diagram of heat-treated MWCNTs and Fe2O3-loaded composites prepared in Example 2 of the present invention;
[0029] Fig.11 Thermogravimetric analysis diagram of heat-treated MWCNTs loaded with Fe2O3 prepared in Example 2 of the present invention in an oxygen atmosphere;
[0030] Fig.12 These are the charge and discharge curves of the Fe2O3 / raw material MWCNTs composite and the Fe2O3 / heat-treated MWCNTs composite prepared in Example 2 of the present invention. DETAILED DESCRIPTION
[0031] The specific contents of the present invention are further illustrated by examples below.
[0032] A first aspect of the present invention provides a method for preparing CNTs loaded with iron oxide, the method comprising the following steps:
[0033] CNTs are heat-treated in an oxygen-containing atmosphere so that oxygen-containing groups are attached to the surface of the CNTs, and then the CNTs with oxygen-containing groups attached are added to a polar solvent, and a certain amount of surfactant is added thereto as needed, and a dispersion of CNTs with oxygen-containing groups attached is obtained by ultrasonic dispersion, and a certain amount of iron oxide precursor and additives are added to the dispersion of CNTs with oxygen-containing groups attached, and the mixture is stirred and allowed to stand so that the iron oxide precursor is attached to the surface of CNTs with oxygen-containing groups attached through electrostatic action, and then a CNTs-loaded iron oxide composite material is prepared by a liquid phase method; the CNTs-loaded iron oxide composite material is subsequently calcined in a high-temperature inert atmosphere to further improve the conductivity of the CNTs and the crystallinity of the iron oxide.
[0034] In the present invention, the purpose of heat treatment is to slowly oxidize CNTs at a suitable temperature. It should be pointed out that the carbon element in some CNTs reacts with oxygen to form gaseous carbon oxides, and leaves holes in situ. Therefore, the heat treatment process will increase the specific surface area of CNTs, and there will be a large number of oxygen-containing groups connected to the carbon element that have not been separated from the CNTs, so that the CNTs are attached with a large number of oxygen-containing groups, and porous CNTs with attached oxygen-containing groups are obtained. Therefore, the heat treatment process will not only greatly increase the specific surface area of CNTs, but also cause a large number of oxygen-containing functional groups to be attached to the surface of CNTs. The inventors have found that the oxygen-containing groups attached to CNTs are obtained by heat treatment in an oxygen-containing atmosphere, and the existence of oxygen mainly includes carbon-oxygen double bonds connected to aromatic carbons, carbon-oxygen single bonds connected to aliphatic carbons, and carbon-oxygen single bonds connected to aromatic carbons. Heat treatment can significantly increase the oxygen content in CNTs. The mass fraction of oxygen in CNTs with attached oxygen-containing groups reaches more than 10wt.%, and can reach 15wt.%; the specific surface area of CNTs increases by at least 1.3 times.
[0035] Since the reaction between carbon and oxygen is an exothermic reaction, the control of the heat treatment temperature and the oxygen content and flow rate of the introduced oxygen-containing atmosphere is very important and critical for the preparation of porous CNTs with attached oxygen-containing groups.
[0036] In the present invention, the oxygen-containing atmosphere includes: air, oxygen, a mixture of air and an inert atmosphere, and a mixture of oxygen and an inert atmosphere; the inert atmosphere is nitrogen and argon.
[0037] In the present invention, the flow rate of the oxygen-containing atmosphere is 0-5 mL / min. The small flow rate of the oxygen-containing atmosphere is used to control the concentration of oxygen in the oxygen-containing atmosphere, thereby controlling the reaction efficiency of CNTs and oxygen.
[0038] In the present invention, the initial weight loss temperature is determined by the physical properties of the CNTs material and is determined by thermogravimetric analysis at a heating rate of 5 to 10°C / min in an oxygen atmosphere. The temperature range of the heat treatment is the initial weight loss temperature and up to 100°C above; the heating rate is controlled to be 1 to 10°C / min; based on the initial weight loss temperature, the set temperature ensures that the CNTs react with oxygen at this temperature, and the rate at which the CNTs react with oxygen can be controlled by the set temperature.
[0039] In the present invention, the heat treatment is maintained for 0.1 to 5 hours. If the time is too short, the oxygen content of the attached particles is low, while if the time is too long, it is difficult for the CNTs to maintain a complete skeleton structure.
[0040] In the present invention, the heat treatment is carried out in a high temperature furnace, which includes a tubular furnace and a muffle furnace.
[0041] In the present invention, the laboratory dosage of the CNTs powder is 0.03-0.3 g.
[0042] According to the present invention, CNTs attached with oxygen-containing groups are added into a polar solvent and ultrasonically dispersed to obtain a dispersion of CNTs attached with oxygen-containing groups.
[0043] Furthermore, the surfactant is selected from one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate or hexadecyl trimethyl ammonium bromide. It should be noted that the CNTs attached with oxygen-containing groups are highly dispersed in the polar solvent and do not settle or attach for a long time; preferably, no surfactant is added; the ultrasonic power is 300 to 1000 W; the ultrasonic dispersion time is 30 to 100 minutes; the polar solvent is one of water, N,N-dimethylformamide, and N-methylpyrrolidone.
[0044] In the present invention, the inventors have found that the precursor of iron oxide is uniformly attached to the surface of CNTs in the form of nanoparticles, and the content of attached iron oxide can be as high as 70wt.%, while the CNTs that have not been heat-treated only load a small amount of iron oxide nanoparticles, less than 10wt.%. This confirms the importance of oxygen-containing groups on the surface of CNTs to their loading of Fe3O4. In addition, the inventors have found that the content of oxygen-containing groups on the surface of CNTs has an important influence on the loading of iron oxide. If the oxygen content is too low, it cannot be effectively loaded. In the CNTs with attached oxygen-containing groups obtained by the above-mentioned heat treatment method, the mass fraction of oxygen reaches more than 10.0wt.%, which is sufficient to form an effective load.
[0045] In the present invention, the iron oxide precursor is selected from one or a mixture of two of Fe(OH)3 sol, ferric nitrate, ferric acetate, FeCl3, and FeCl2.
[0046] In the present invention, the usage ratio of CNTs with attached oxygen-containing groups, surfactant, iron oxide precursor and polar solvent is 30-60 mg: 0-0.16 g: 10-200 mg: 20-70 mL.
[0047] In the present invention, an auxiliary agent may be optionally added to the solution of the iron oxide precursor, wherein the auxiliary agent includes a pH regulator, a Fe 3+ Reduction to Fe 2+ One or more of the reducing agent A or the reducing agent B for further reducing the CNTs attached with oxygen-containing groups. The reducing agent A is selected from ascorbic acid or trisodium citrate; the reducing agent B is selected from hydrazine hydrate or ethylene glycol; the pH adjusting agent is selected from one or more of ammonia water, sodium hydroxide and sodium bicarbonate; the amount of reducing agent A is 0.5 to 2 times the molar amount of the iron oxide precursor, and the amount of reducing agent B is 3 to 30 vol.% of the total volume of the solvent; the pH adjusting agent adjusts the pH value of the reaction solution to about 11.
[0048] In the present invention, the stirring and standing are both carried out at room temperature to 45°C. The stirring and standing are to make the iron oxide precursor better adhere to the surface of CNTs. The stirring speed is 10-200 rpm, the stirring time is 1-5 minutes, and the standing time is 3-30 minutes. The appropriate high temperature below 45°C accelerates the Brownian motion so that the iron oxide precursor and the CNTs attached with oxygen-containing groups are more efficiently electrostatically adsorbed.
[0049] According to the present invention, the iron oxide precursor attached to the surface of CNTs is converted into iron oxide in situ by a subsequent liquid phase method, and the iron oxide is Fe2O3 and / or Fe3O4. The liquid phase method mainly comprises that the iron oxide precursor reacts chemically with ions in the liquid phase under liquid phase reaction conditions at a certain temperature and finally converts into iron oxide in situ; or the iron oxide precursor does not react chemically with ions in the liquid phase and converts into iron oxide in situ under liquid phase reaction conditions at a certain temperature.
[0050] In the present invention, the liquid phase method is a hydrothermal reaction or a coprecipitation reaction. The conditions of the hydrothermal reaction are 120-180° C. for 10-14 hours, and the conditions of the coprecipitation reaction are 80° C. for 2-5 minutes.
[0051] Furthermore, the CNTs-loaded iron oxide composite material is subsequently calcined in a high-temperature inert atmosphere to further improve the conductivity of the CNTs and the crystallinity of the iron oxide. The calcination temperature is 400-500° C. and the calcination time is 0.5-5 hours.
[0052] In the present invention, the CNTS includes MWCNTs and single-walled carbon nanotubes (SWCNTs).
[0053] Embodiment 1:
[0054] Preparation of CNTs loaded with iron oxide:
[0055] (1) First, MWCNTs (purity: 99%, model: CNTs099, manufacturer: Shenzhen Suiheng Graphene Technology) were subjected to thermogravimetric analysis at a heating rate of 10°C / min in an oxygen atmosphere to determine their initial weight loss temperature;
[0056] (2) heating the MWCNTs to 500°C in a tube furnace at a heating rate of 5°C / min in an air atmosphere with a flow rate of 0.5 mL / min and maintaining the temperature for 3 h, and then taking them out after natural cooling to obtain MWCNTs loaded with oxygen-containing groups;
[0057] (3) Weighing 25 mg of the above-mentioned MWCNTs with attached oxygen-containing groups into 25 mL of water, and ultrasonically dispersing for 30 min to obtain an aqueous dispersion of MWCNTs with attached oxygen-containing groups;
[0058] (4) 15 mL of Fe(OH)3 hydrosol containing about 50 mg of Fe(OH)3 colloidal particles was added to the aqueous dispersion of the MWCNTs attached with oxygen-containing groups, and after stirring and standing for a period of time, 80 mg of ascorbic acid was weighed and added thereto, and then the pH value of the reaction solution was adjusted to about 11 with ammonia water, and then hydrothermally reacted at 180°C for 12 hours, and then centrifuged, washed and dried to obtain a MWCNTs-loaded Fe3O4 composite. The mass ratio of Fe3O4 in the MWCNTs-loaded Fe3O4 composite was 54.0 wt.%.
[0059] Embodiment 2:
[0060] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that ascorbic acid was not added, and the prepared product was a MWCNTs loaded with Fe2O3 composite, wherein the mass ratio of Fe2O3 was 51.9wt.%.
[0061] Embodiment 3:
[0062] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that the mass of Fe(OH)3 colloidal particles in the added Fe(OH)3 aqueous sol was about 25 mg, and the prepared product was a MWCNTs loaded with Fe3O4 composite, in which the mass ratio of Fe3O4 was about 29wt.%.
[0063] Embodiment 4:
[0064] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that the mass of Fe(OH)3 colloidal particles in the added Fe(OH)3 hydrosol was about 75 mg, and the prepared product was a MWCNTs loaded with Fe3O4 composite, in which the mass ratio of Fe3O4 was about 70wt.%.
[0065] Embodiment 5:
[0066] A composite material of CNTs loaded with iron oxide was prepared according to the method of Example 1, except that single-walled carbon nanotubes (SWCNTs) with attached oxygen-containing groups having an oxygen content of about 10 wt.% were used, and the prepared product was a SWCNTs loaded with Fe3O4 composite, in which the mass ratio of Fe3O4 was about 50 wt.%.
[0067] Embodiment 6:
[0068] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that ascorbic acid was not used, but an equimolar amount of trisodium citrate was used, and the prepared product was a MWCNTs loaded with Fe3O4 composite, wherein the mass ratio of Fe3O4 was about 53wt.%.
[0069] Embodiment 7:
[0070] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that no Fe(OH)3 colloidal particles were added, and an equimolar amount of FeCl3 (76 mg) was added. The prepared product was a MWCNTs loaded Fe3O4 composite, in which the mass ratio of Fe3O4 was about 52wt.%.
[0071] Embodiment 8:
[0072] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that the prepared MWCNTs loaded with Fe3O4 composite was further calcined in an argon atmosphere at 500°C for 2h to enhance the degree of reduction of the MWCNTs, thereby improving the conductivity of the composite and the crystallinity of Fe3O4, wherein the mass ratio of Fe3O4 was about 57wt.%.
[0073] Embodiment 9:
[0074] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 1, except that no ammonia water was added, and 1.25 mL of hydrazine hydrate was added. The prepared product was a MWCNTs loaded with Fe3O4 composite, in which the mass ratio of Fe3O4 was about 54 wt.%.
[0075] Embodiment 10:
[0076] The steps of this embodiment are the same as those of embodiment 1, except that in step (4), no Fe(OH)3 colloidal particles are added, but 0.24 mmol of FeCl3 and 0.24 mmol of FeCl2 are added. The reaction solution is heated to 80°C while stirring, and then the pH value of the reaction solution is adjusted to about 11 with ammonia water. Stirring is continued for 5 minutes, and a MWCNTs-loaded Fe3O4 composite is obtained by centrifugation, washing and drying, in which the mass ratio of Fe3O4 is about 51wt.%.
[0077] Embodiment 11:
[0078] A composite material of MWCNTs loaded with iron oxide was prepared according to the method of Example 2, except that the mass of Fe(OH)3 colloidal particles in the added Fe(OH)3 aqueous sol was about 25 mg, and the prepared product was a MWCNTs loaded with Fe2O3 composite, in which the mass ratio of Fe2O3 was about 27wt.%.
[0079] Embodiment 12:
[0080] The steps of this embodiment are the same as those of embodiment 7, except that MWCNTs are not added, and an equal mass of SWCNTs with an oxygen content of about 10 wt.% is added. The prepared product is a SWCNTs-loaded Fe3O4 composite, in which the mass ratio of Fe3O4 is about 55 wt.%.
[0081] Comparative Example 1:
[0082] The same as Example 2, except that the heat treatment of steps (1) and (2) is not performed, and steps (3) and (4) are directly performed using the raw material oxygen content of MWCNTs.
[0083] Comparative Example 2:
[0084] The same as Example 1, except that: the MWCNTs were heated to 610°C and heat treated for 0.5h. After the heat treatment, the oxygen content in the MWCNTs was only about 3wt.%, and the morphology of some MWCNTs collapsed. The content of loaded Fe3O4 nanoparticles was about 8wt.%, and no effective load could be formed.
[0085] Figure 1 This is a thermogravimetric analysis curve of the MWCNTs raw material used in Example 1 of the present invention. It can be seen from the figure that its initial weight loss temperature is about 470°C.
[0086] Figure 2The X-ray photoelectron spectroscopy (XPS) diagram of the MWCNTs with attached oxygen-containing groups prepared in Example 1 of the present invention and its raw materials. From the XPS diagram, it can be seen that the oxygen content of the MWCNTs increased from 1.9wt.% to 10.8wt.% after heat treatment in an air atmosphere, which indicates that the heat treatment under such conditions causes a large number of oxygen-containing groups to be attached to the surface of the MWCNTs;
[0087] Figure 3 This is a photograph of the MWCNTs with attached oxygen-containing groups prepared in Example 1 of the present invention being uniformly dispersed in water (1 mg / mL) without adding a dispersant after standing for 3 months. It can be seen from the figure that even after 3 months of standing, the MWCNTs with attached oxygen-containing groups prepared in Example 1 of the present invention can still be uniformly dispersed in water, which provides convenient conditions for it to generate electrostatic force on the positively charged load precursor. Figure 4 This is a photograph of the raw material MWCNTs prepared in Comparative Example 1 of the present invention dispersed in water. It can be seen from the figure that the raw material MWCNTs are difficult to be uniformly dispersed in water.
[0088] Figure 5 This is a scanning electron microscope (SEM) image of the heat-treated MWCNTs loaded with Fe3O4 prepared in Example 1 of the present invention. It can be seen from the image that the heat-treated MWCNTs are loaded with a large amount of nanoparticles; Figure 6 The X-ray diffraction (XRD) diagram of the heat-treated MWCNTs and the Fe3O4-loaded composite prepared in Example 1 of the present invention shows that the diffraction peaks of the heat-treated MWCNTs-loaded Fe3O4 composite include the diffraction peaks of Fe3O4 and the heat-treated MWCNTs. The diffraction peaks at 2θ=30.1°, 35.4°, 43.1°, 53.4°, 56.9° and 62.5° correspond to the (220), (311), (400), (422), (511) and (440) crystal planes of Fe3O4, respectively. The peak of the heat-treated MWCNTs and the Fe3O4-loaded composite at about 26.4° corresponds to the (002) crystal plane of graphite, while the peak at 22.0° corresponds to the interlayer spacing of 0.40 nm, which is due to the expansion of the interlayer spacing of MWCNTs caused by the generation of oxygen-containing groups.
[0089] Figure 7 This is a thermogravimetric analysis curve of the heat-treated MWCNTs-loaded Fe3O4 composite prepared in Example 1 of the present invention. Since Fe3O4 is converted into Fe2O3 during the thermogravimetric analysis process, the heat-treated MWCNTs are converted into gaseous carbon oxides. Based on the remaining mass of 55.9wt.%, it is calculated that the mass ratio of Fe3O4 in the MWCNTs-loaded Fe3O4 composite is 54.0wt.%, and the mass ratio of the heat-treated MWCNTs is 46.0wt.%.
[0090] Figure 8 This is a SEM image of heat-treated MWCNTs loaded with Fe2O3 prepared in Example 2 of the present invention. It can be seen from the image that a large number of nanoparticles are attached to the heat-treated MWCNTs; Fig. 9 This is a SEM image of the raw material MWCNTs loaded with Fe2O3 prepared in Comparative Example 1 of the present invention. It can be seen from the image that only a small amount of nanoparticles are attached to the surface of the raw material MWCNTs.
[0091] Fig.10 The XRD pattern of the heat-treated MWCNTs and the Fe2O3-loaded composite prepared in Example 2 of the present invention shows that the diffraction peaks at 2θ=24.1°, 33.15°, 35.61°, 40.85°, 49.48°, 54.09°, 57.6°, 62.45°, 63.99° and 71.9° correspond to the (012), (104), (110), (113), (024), (116), (018), (214), (300) and (1010) crystal planes of cubic α-Fe2O3, respectively. The diffraction peaks at around 26.4° and 22.0° are attributed to the heat-treated MWCNTs, which are consistent with the XRD pattern of the heat-treated MWCNTs and the Fe2O3-loaded composite prepared in Example 2 of the present invention. Figure 6 Consistent.
[0092] Fig.11 This is the thermogravimetric analysis diagram of MWCNTs loaded with Fe2O3 prepared in Example 2 of the present invention. Based on the fact that the heat-treated MWCNTs are converted into gaseous carbon oxides during the thermogravimetric analysis process, and the remaining substance is Fe2O3 in the composite, it can be concluded that the mass ratio of Fe2O3 in the heat-treated MWCNTs loaded with Fe2O3 composite is 48.1wt.%, and the mass ratio of the heat-treated MWCNTs is 51.9wt.%.
[0093] The MWCNTs-loaded Fe2O3 composite (Fe2O3 / heat-treated MWCNTs composite) prepared in Example 2 of the present invention and the Fe2O3 / raw material MWCNTs composite prepared in Comparative Example 1 of the present invention were used for the assembly of button-type lithium batteries, wherein the mass ratio of active material: conductive additive (carbon black): binder (polyvinylidene fluoride) was 8:1:1, the electrolyte was 1M LiPF6, and the solvent was ethylene carbonate, dimethyl carbonate and ethyl methyl carbonate in a volume ratio of 1:1:1. The cycle capacity was tested and characterized by a Xinwei battery test system (model: CT-3008W, manufacturer: Shenzhen Xinwei Electronics Co., Ltd.).
[0094] Fig.12Figure 2 is the charge-discharge curve of the Fe2O3 / heat-treated MWCNTs composite prepared in Example 2 of the present invention and the Fe2O3 / raw material MWCNTs composite prepared in Comparative Example 1 of the present invention. It can be seen from the figure that the charge-discharge specific capacity of the heat-treated MWCNTs loaded with Fe2O3 prepared in Example 2 is significantly higher than that of the raw material MWCNTs loaded with Fe2O3 prepared in Comparative Example 1. In the charge-discharge voltage range of 0.01 to 3V, at a current density of 0.5A / g, after 55 charge-discharge cycles, the discharge specific capacity of the heat-treated MWCNTs loaded with Fe2O3 is maintained at 605.3mAh g -1 On the one hand, the heat-treated MWCNTs can buffer the volume change of Fe2O3 during the charge and discharge process, and on the other hand, the heat-treated MWCNTs can make up for the lack of electrical conductivity of Fe2O3. The good charge and discharge cycle performance shows that Fe2O3 is firmly attached to the heat-treated MWCNTs. However, the corresponding discharge capacity of raw MWCNTs loaded with Fe2O3 is only 243.0mAh g -1 This is mainly because Fe2O3 has a higher theoretical capacity and the amount of Fe2O3 that can be loaded by the raw material MWCNTs is small.
Claims
1. A method for preparing carbon nanotube-loaded iron oxide, characterized in that: The method comprises the following steps: (1) CNTs were subjected to thermogravimetric testing at a heating rate of 5-10 °C / min in an oxygen atmosphere to determine the initial weight loss temperature of CNTs; (2) placing the CNTs in a high temperature furnace, heating the temperature at a rate of 1 to 10 °C / min to a temperature at most 100 °C above the initial weight loss temperature, while introducing an oxygen-containing atmosphere at a flow rate of 0 to 5 mL / min, and heat treating at this temperature for 0.1 to 5 hours to prepare CNTs with attached oxygen-containing groups; the mass fraction of oxygen in the CNTs with attached oxygen-containing groups is greater than 10.0 wt.%; The oxygen-containing atmosphere includes: air, oxygen, a mixture of air and an inert atmosphere, and a mixture of oxygen and an inert atmosphere; the inert atmosphere is nitrogen and argon; (3) adding a certain amount of CNTs attached with oxygen-containing groups into a certain volume of polar solvent, and obtaining a dispersion of CNTs attached with oxygen-containing groups by ultrasonic dispersion; (4) A certain amount of iron oxide precursor and additives were added to the dispersion of CNTs attached with oxygen-containing groups, stirred and allowed to stand for a period of time to allow the iron oxide precursor to adhere to the surface of CNTs attached with oxygen-containing groups through electrostatic action, and then a CNTs-loaded iron oxide composite was prepared by a liquid phase method. The iron oxide precursor was uniformly attached to the surface of CNTs in the form of nanoparticles, and the content of the attached iron oxide was 70 wt.%.
2. The method for preparing carbon nanotube-loaded iron oxide according to claim 1, characterized in that: The polar solvent is one of water, N,N-dimethylformamide and N-methylpyrrolidone; The ultrasonic power is 300-1000 W; the ultrasonic dispersion time is 30-100 min.
3. The method for preparing carbon nanotube-loaded iron oxide according to claim 1, characterized in that: In step (3), a certain amount of surfactant is added thereto to assist in dispersion according to the dispersion requirements; The surfactant is selected from one of polyvinyl pyrrolidone, sodium dodecylbenzene sulfonate or hexadecyltrimethylammonium bromide.
4. The method for preparing carbon nanotube-loaded iron oxide according to claim 3, characterized in that: The iron oxide precursor is selected from one or a mixture of two of Fe(OH)3 sol, ferric nitrate, ferric acetate, FeCl3, and FeCl2; The amount ratio of CNTs attached with oxygen-containing groups, surfactant, iron oxide precursor and polar solvent is 30~60 mg: 0~0.16 g: 10~200 mg: 20~70 mL.
5. The method for preparing carbon nanotube-loaded iron oxide according to claim 1, characterized in that: The auxiliary agent includes a pH regulator, Fe 3+ Reduction to Fe 2+ One or more of a reducing agent A or a reducing agent B for further reducing the CNTs attached with oxygen-containing groups; The reducing agent A is selected from ascorbic acid or trisodium citrate; the reducing agent B is selected from hydrazine hydrate or ethylene glycol; the pH adjusting agent is selected from one or more of ammonia water, sodium hydroxide and sodium bicarbonate; The amount of reducing agent A used is 0.5 to 2 times the molar amount of the iron oxide precursor, the amount of reducing agent B used is 3 to 30 vol.% of the total volume of the solvent; and the pH value of the reaction solution is adjusted to 11 by the pH adjuster.
6. The method for preparing carbon nanotube-loaded iron oxide according to claim 1, characterized in that: The stirring and standing are both performed at room temperature to 45°C, the stirring speed is 10-200 rpm, the stirring time is 1-5 min, and the standing time is 3-30 min; The liquid phase method is a hydrothermal reaction or a coprecipitation reaction. The conditions of the hydrothermal reaction are 120-180°C for 10-14 h, and the conditions of the coprecipitation reaction are 80°C for 2 min-5 min.
7. The method for preparing carbon nanotube-loaded iron oxide according to claim 1, characterized in that: The method also includes further improving the conductivity of CNTs and the crystallinity of iron oxide by subsequently calcining the composite material of CNTs loaded with iron oxide in a high-temperature inert atmosphere; the calcination temperature is 400-500°C and the calcination time is 0.5-5 h.
8. A composite material of CNTs loaded with iron oxides prepared by the method according to any one of claims 1 to 7, characterized in that: The iron oxide is Fe2O3 and / or Fe3O4; In the CNTs with attached oxygen-containing groups, the mass fraction of oxygen is above 10.0 wt.%; The precursor of iron oxide is uniformly attached to the surface of CNTs in the form of nanoparticles, and the content of the attached iron oxide is 70wt.%.
9. Application of the composite material of CNTs loaded with iron oxide according to claim 8 in the fields of lithium ion batteries, supercapacitors, electromagnetic interference, magnetic recording, catalysis, and medicine.