Non-destructive testing method and device for tube sheet plug weld penetration uniformity and cracks
By heating in the center of the welding plug surface and using temperature difference detection, the lossless problems of weld melting depth uniformity and crack defect detection in the prior art are solved, and effective evaluation of the quality of welding plugs is achieved, providing rapid and The non-destructive detection method reduces the risk of defects in welding plugs during use.
Patent Information
- Application Number
- CN202111035536.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-03
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2041-09-03
AI Technical Summary
The prior art lacks effective non-destructive testing methods to evaluate the weld melting depth uniformity and crack defects of pipe plate welding plugs, resulting in the risk of potential defects in the welding plugs during use.
By heating in the center of the welding plug surface, temperature differences are used to detect weld melting depth uniformity and crack defects, ceramic insulation fibers are used to cover it and temperature field test is used to judge the weld melting depth and The existence of cracks.
Non-destructive testing of welding plugs is realized, providing effective evaluation of the quality of new products and in-service pipe plate welding plugs. The test process does not damage the welding structure, and the equipment is small and the hardware requirements are simple. It can quickly obtain semi-quantitative results of defect size. .
Smart Images

Figure CN113567501B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material engineering, and in particular relates to a non-destructive testing method and device for uniformity of penetration and cracks of a tube sheet plug weld. Background Art
[0002] Tube-sheet heat exchangers manufactured by welding methods are widely used in power generation, petrochemical, pharmaceutical and other fields. The connection methods between heat exchange tubes and tube sheets include expansion joints, welding and expansion welding. Steam generators are one of the core equipment of thermal power and nuclear power technology, and are typical application representatives of welded tube-sheet heat exchangers. The quality of the welded joints between tubes and tube sheets is of great significance to the safe production of power plants.
[0003] The welded joint between the tube and the tube sheet is the weak link of thermal power and nuclear power steam generators. Long-term high-temperature steam corrosion, mechanical vibration, and external abrasive wear will cause the tube to break, eventually leading to mixing of the heat exchange medium and reduced heat exchange efficiency. For nuclear power steam generators, there is also a huge risk of radioactive leakage. Therefore, once the tube fails, the inlet and outlet of the damaged tube are usually blocked to achieve the purpose of short-circuiting the failed tube. The main blocking methods include mechanical expansion blocking, welding blocking, and expansion and welding composite blocking. Among them, welding blocking is a recently developed high-reliability blocking method. However, the corresponding detection technology is relatively lacking, which is a bottleneck problem affecting its wide application and post-service quality tracking. The quality inspection of post-weld and in-service plugs needs to be completed on site. The characteristics of weld excess height and appearance can be detected by existing methods. However, for defects such as weld penetration and internal cracks in the weld, due to the limitation of site space and tube sheet position, the commonly used methods such as radiographic detection and eddy current detection cannot be implemented. The current method is usually to use destructive testing methods to detect and evaluate the above defects during the optimization and solidification stages of the welding process, and finally obtain optimized process parameters. However, there are problems such as testing without use and use without testing, which makes the plugs used have the risk of defects. Therefore, it is urgent to develop a non-destructive testing method for the uniformity / consistency of weld penetration and weld cracks of tube-to-sheet welding plugs. Summary of the invention
[0004] In view of the bottleneck problem that there is currently no effective non-destructive testing method for detecting and evaluating the uniformity of weld penetration and weld crack defects of tube sheet welding plugs, the purpose of the present invention is to provide a non-destructive testing method and device for the uniformity of weld penetration and cracks of tube sheet welding plugs. This method can perform non-destructive testing of weld penetration uniformity and weld crack defects without destroying the welding structure, based on the principle that the defect hinders the radial conduction of heat flow at the center of the plug, causing an obvious temperature difference on both sides of the defect. This method can provide a new and effective method for quality evaluation of new and in-service tube sheet welding plugs.
[0005] The present invention is achieved through the following technical solutions:
[0006] A non-destructive testing method for uniformity of penetration and cracks of a tube sheet plug weld comprises the following steps:
[0007] 1) Clean the surface of the tube sheet welding plug sample to remove the oxidation products and oily attachments on the surface to prevent their influence on the evolution and measurement of the plug surface temperature field;
[0008] 2) Measure and obtain the center of the plug sample surface and mark it, bring a heating body with a diameter between 1 / 8 and 1 / 2 of the plug diameter into close contact with and fix it to the center area of the plug surface, heat the center area of the plug sample surface, and cover the surface with ceramic insulation fiber;
[0009] 3) After heating for a preset time, take out the ceramic insulation fiber and test the temperature field on the surface of the plug sample. If the temperature inside and outside the weld is lower than a certain value of the temperature in the area with the same diameter, it is judged that the weld penetration in this area is shallow or there is a crack in the weld;
[0010] Taking advantage of the fact that shallow weld penetration and crack defects will reduce or partially block the heat conduction path from the center of the plug along the diameter direction outward, heat exchange can only be carried out by more inefficient thermal radiation, resulting in the temperature of the shallow weld penetration or crack defect near the center of the heat source being higher than other areas with the same radius, and the temperature of the shallow weld penetration or crack defect far from the center of the heat source being lower than other areas with the same radius, a semi-quantitative detection of weld penetration uniformity and crack defects is performed.
[0011] Preferably, the heating of the central area of the plug surface by the heating body in step 2) is heat conduction heating by an electric heating rod, or irradiation heating in the form of laser or xenon lamp.
[0012] Preferably, the heating body in step 2) heats the plug to no less than 150°C so that the temperature difference caused by shallow fusion depth and crack defects can be detected, and the upper limit of heating temperature is no higher than the temperature that does not change the material structure and properties.
[0013] Preferably, the preset heating time in step 3) is between 1 and 15 minutes. The higher the thermal conductivity of the plug and the weld material or the deeper the set weld penetration, the shorter the heating time is set; the lower the thermal conductivity of the plug and the weld material or the shallower the set weld penetration, the longer the heating time is set.
[0014] Preferably, the temperature field test in step 3) adopts a thin film thermocouple, a mesh thermocouple, an infrared thermometer or an infrared camera, and the temperature resolution is not less than 2°C and the plane resolution is not less than 0.2°C / mm.
[0015] Preferably, when judging in step 3) that the fusion depth is shallow or a crack defect occurs, the temperature difference on both sides of the target area needs to be greater than 5°C.
[0016] Preferably, the heat source temperature, heating time and thermal conductivity of the material are combined, and the results of the calculation of the non-steady-state heat transfer relationship of the point heat source in a semi-infinite area are used to infer the weld penetration and defect size in different areas.
[0017] Preferably, the method is not only applicable to new tube sheet welding plugs, but also applicable to quality inspection of in-service tube sheet welding plugs.
[0018] The test device for realizing the non-destructive test method for the uniformity of penetration depth and cracks of the tube sheet plug weld comprises a three-point support frame 2 of the automated test device, a magnetic fixing device 3 fixed at the bottom of the three-point support frame 2 of the automated test device for fixing with the welding plug test sample 1, an XY two-dimensional moving platform 4 fixed at the inner side of the top of the three-point support frame 2 of the automated test device, a horizontal rotating platform 5 fixed at the bottom of the XY two-dimensional moving platform 4, a first vertical direction slide rail 9 and a second vertical direction slide rail 10 fixed at both ends of the lower part of the horizontal rotating platform 5, and the first vertical direction slide rail 9 and the second vertical direction slide rail 10 are respectively fixed at the first vertical direction slide rail 9 and the second vertical direction slide rail 10. An infrared camera 8 and a laser heating device 7 at the bottom of the second vertical slide rail 10, two positioning cameras 6 fixed at the bottom of the horizontal rotating platform 5 and located between the first vertical slide rail 9 and the second vertical slide rail 10, a data and power transfer interface 11 arranged on the three-point support skeleton 2 of the automated testing device, a process monitoring and control device 12 and a power supply 13 connected to the XY two-dimensional mobile platform 4, the horizontal rotating platform 5, the positioning camera 6, the laser heating device 7, the infrared camera 8, the first vertical slide rail 9 and the second vertical slide rail 10 through the data and power transfer interface 11.
[0019] The test device is implemented according to the following test steps: first, mechanical grinding and organic solvent cleaning are used to remove oxides and organic matter and other attachments on the surface of the plugs 1-3 and the surrounding areas of the welding plug test sample 1 to ensure that the center of the plug is flat; the test device is fixed to the surface of the welding plug test sample 1 by a magnetic fixing device 3; secondly, the test device is turned on, and two non-parallel positioning cameras 6 are driven by the process monitoring and control device 12 to determine the geometric center of the plug to be tested by the image method to obtain its plane coordinates; the XY two-dimensional moving platform 4 and the horizontal rotating platform 5 are driven by the process monitoring and control device 12 to align the laser heating device 7 with the geometric center of the plug 1-3 plane; laser focusing or The second vertical slide rail 10 is driven to heat the surface center of the plug 1-3 with a diameter between 1 / 8 and 1 / 2 of the plug diameter by means of a laser or a heating rod, and the surface is covered with a ceramic thermal insulation fiber blanket; finally, after heating for a certain period of time, the ceramic thermal insulation fiber is taken out, and the process monitoring and control device 12 is used to drive the XY two-dimensional mobile platform 4 and the horizontal rotating platform 5 to align the infrared camera 8 with the geometric center of the plug 1-3 plane, and the first vertical slide rail 9 is driven to test the temperature field on the surface of the welding plug test sample 1 under a reasonable field of view. If there are areas inside and outside the weld with a temperature lower than a certain value of the temperature of the area with the same diameter, it can be judged that the weld penetration is shallow or there are cracks in the weld.
[0020] Compared with the prior art, the present invention has the following advantages:
[0021] 1) The testing process will not affect the quality of the plug, the testing equipment is small in size and the hardware requirements are simple.
[0022] 2) The test time of a single plug is short.
[0023] 3) Semi-quantitative results of defect size can be obtained through theoretical calculation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 It is a typical device for a non-destructive testing method of uniform penetration and cracks of a tube sheet plug weld; in the figure, 1-welding plug test specimen (1-1 tube sheet, 1-2 tube, 1-3 plug, 1-4 weld), 2-three-point support frame of automated testing device, 3-magnetic fixing device, 4-XY two-dimensional mobile platform, 5-horizontal rotating platform, 6-positioning camera, 7-laser heating device, 8-infrared camera, 9-first vertical slide rail, 10-second vertical slide rail, 11-data and power transfer interface, 12-process monitoring and control device, 13-power supply. DETAILED DESCRIPTION
[0025] The following is a detailed description of the embodiments and the attached Figure 1The present invention is further described in detail, which is intended to explain the present invention rather than to limit it.
[0026] Figure 1 The device for realizing the non-destructive testing method of the penetration uniformity and crack of the tube sheet plug weld of the present invention comprises a three-point supporting frame 2 of an automated testing device, a magnetic fixing device 3 fixed at the bottom of the three-point supporting frame 2 of the automated testing device for fixing with a welding plug test sample 1, an XY two-dimensional moving platform 4 fixed at the inner side of the top of the three-point supporting frame 2 of the automated testing device, a horizontal rotating platform 5 fixed at the bottom of the XY two-dimensional moving platform 4, a first vertical direction slide rail 9 and a second vertical direction slide rail 10 fixed at both ends of the lower part of the horizontal rotating platform 5, and the first vertical direction slide rail 9 and the second vertical direction slide rail 10 are respectively fixed at the first vertical direction slide rail 9 and the second vertical direction slide rail 10. An infrared camera 8 and a laser heating device 7 at the bottom of the second vertical slide rail 10, two positioning cameras 6 fixed at the bottom of the horizontal rotating platform 5 and located between the first vertical slide rail 9 and the second vertical slide rail 10, a data and power transfer interface 11 arranged on the three-point support skeleton 2 of the automated testing device, a process monitoring and control device 12 and a power supply 13 connected to the XY two-dimensional mobile platform 4, the horizontal rotating platform 5, the positioning camera 6, the laser heating device 7, the infrared camera 8, the first vertical slide rail 9 and the second vertical slide rail 10 through the data and power transfer interface 11.
[0027] The present invention discloses a non-destructive testing method for welding plug weld penetration uniformity and cracks, which is implemented by the following steps:
[0028] First, mechanical grinding and organic solvent cleaning are used to remove oxides and organic matter and other attachments on the surface of plugs 1-3 and nearby areas to ensure that the center of the plug is flat and the roughness is not higher than Ra 4.5μm; Figure 1The automated testing device shown is fixed to the surface of the welding plug test sample 1 by a magnetic fixing device 3. Secondly, turn on the automated testing device, and drive two non-parallel positioning cameras 6 through the process monitoring and control device 12 to determine the geometric center of the plug to be tested by the image method to obtain its plane coordinates. The XY two-dimensional moving platform 4 and the horizontal rotating platform 5 are driven by the process monitoring and control device 12 to align the laser heating device 7 with the geometric center of the plug 1-3 plane. The surface center of the plug 1-3 with a diameter between 1 / 8 and 1 / 2 of the plug diameter is heated by laser focusing or driving the second vertical slide rail 10 using a laser or a heating rod, and the surface is covered with a ceramic thermal insulation fiber blanket. Finally, after heating for a certain period of time, the ceramic thermal insulation fiber is taken out, and the process monitoring and control device 12 drives the XY two-dimensional mobile platform 4 and the horizontal rotating platform 5 to align the infrared camera 8 with the geometric center of the plug 1-3 plane, and drives the first vertical slide rail 9 to test the temperature field on the surface of the welding plug test sample 1 under a reasonable field of view. If there are areas inside and outside the weld where the temperature is lower than a certain value of the temperature of the area with the same diameter, it can be judged that the weld penetration is shallow or there are cracks in the weld.
[0029] The specific embodiments are as follows:
[0030] Embodiment 1: Specific embodiment is as follows:
[0031] Example 1: A TIG welding joint of an Incolly 800H alloy tube with an outer diameter of 19 mm and a wall thickness of 3 mm and an Incolly 800H alloy tube sheet with a thickness of 200 mm is selected, and an Incolly 800H plug with a diameter of 12.85 mm is selected to seal the tube. After sealing, the following is obtained by mechanical processing: Figure 1 The welding plug test sample 1 shown in the figure. First, the oxides and organic matter attached to the surface of the plugs 1-3 and the surrounding areas were removed by grinding with an angle grinder and cleaning with acetone to ensure that the center of the plug was flat and the roughness was not higher than Ra 4.5μm; secondly, Figure 1The automated testing device shown is fixed to the surface of the welding plug test sample 1 by a magnetic fixing device 3. Secondly, turn on the automated testing device, and drive two non-parallel positioning cameras 6 through the process monitoring and control device 12 to determine the geometric center of the plug to be tested by the image method to obtain its plane coordinates. The XY two-dimensional mobile platform 4 and the horizontal rotating platform 5 are driven by the process monitoring and control device 12 to align the laser heating device 7 with the geometric center of the plug 1-3 plane. The surface center of the plug 1-3 with a diameter between 1 / 8 and 1 / 2 of the plug diameter is heated by laser focusing or driving the second vertical slide rail 10 using a laser or a heating rod. The heating temperature is set to 450°C by adjusting the laser power, and the surface is covered with a ceramic thermal insulation fiber blanket. Finally, after heating for 3.5 minutes, the ceramic insulation fiber is taken out, and the process monitoring and control device 12 drives the XY two-dimensional moving platform 4 and the horizontal rotating platform 5 to align the infrared camera 8 with the geometric center of the plug 1-3 plane, and the temperature field of the sample surface is tested under a reasonable field of view by driving the first vertical direction slide rail 9. The area inside and outside the weld where the temperature is lower than the temperature of the same diameter area by a certain value can be judged as a shallow weld penetration or a weld crack. A total of 3 samples under different welding parameters were tested, and no welding cracks were found in the 3 samples. In one sample, there was a strip area on both sides of the weld that was parallel to the annular weld and the temperature difference on both sides was between 15-29°C, with a length of 8.2mm. According to its morphology, it was judged to be a defect of too shallow weld penetration. At the same time, the destructive metallographic method was used to dissect and observe the samples after non-destructive testing. The observation results were consistent with the non-destructive testing results. No defects were found in 2 samples, and there was a too shallow weld area in 1 sample, and the length test result was 7.4mm.
Claims
1. A non-destructive testing device for the uniformity of weld penetration and cracks of tube sheet plugs. It is characterized in that The invention comprises a three-point support frame (2) of an automated testing device, a magnetic fixing device (3) fixed at the bottom of the three-point support frame (2) of the automated testing device and used for fixing to a welding plug test sample (1), an XY two-dimensional moving platform (4) fixed to the inner side of the top of the three-point support frame (2) of the automated testing device, a horizontal rotating platform (5) fixed to the bottom of the XY two-dimensional moving platform (4), a first vertical direction slide rail (9) and a second vertical direction slide rail (10) fixed to both ends of the bottom of the horizontal rotating platform (5), an infrared camera (8) and a laser heating device (7) respectively fixed to the bottom of the first vertical direction slide rail (9) and the second vertical direction slide rail (10), and a laser heating device (7) fixed to the horizontal rotating platform ( 5) two positioning cameras (6) located at the bottom and between the first vertical slide rail (9) and the second vertical slide rail (10), a data and power transfer interface (11) arranged on the three-point support frame (2) of the automated test device, a process monitoring and control device (12) and a power supply (13) connected to the XY two-dimensional mobile platform (4), the horizontal rotation platform (5), the positioning camera (6), the laser heating device (7), the infrared camera (8), the first vertical slide rail (9) and the second vertical slide rail (10) through the data and power transfer interface (11); the test steps are implemented as follows: first, the welding plug test sample 1 is removed by mechanical grinding and organic solvent cleaning. The surface of the plug (1-3) and the surrounding area are free of oxides, organic matter and other attachments to ensure that the center of the plug is flat; the test device is fixed to the surface of the welding plug test sample (1) by a magnetic fixing device (3); secondly, the test device is turned on, and two non-parallel positioning cameras (6) are driven by a process monitoring and control device (12) to determine the geometric center of the plug to be tested by an image method to obtain its plane coordinates; the XY two-dimensional moving platform (4) and the horizontal rotating platform (5) are driven by the process monitoring and control device (12) to align the laser heating device (7) with the geometric center of the plug (1-3) plane; laser focusing or driving the second vertical slide rail (10) to use laser or heating The center of the surface of the plug (1-3) with a diameter between 1 / 8 and 1 / 2 of the plug diameter is heated by a hot rod, and the surface is covered with a ceramic thermal insulation fiber blanket; finally, after heating for a certain period of time, the ceramic thermal insulation fiber is taken out, and the process monitoring and control device (12) drives the XY two-dimensional moving platform (4) and the horizontal rotating platform (5) to align the infrared camera (8) with the geometric center of the plug (1-3) plane, and the temperature field of the surface of the welding plug test sample (1) is tested under a reasonable field of view by driving the first vertical direction slide rail (9). If the temperature inside and outside the weld is lower than a certain value of the temperature of the same diameter area, it can be judged that the weld penetration is shallow or there is a crack in the weld.
2. A non-destructive testing method for uniform penetration and cracks of tube sheet plug welds. It is characterized in that The method is based on a non-destructive testing device for uniformity of weld penetration and cracks of a tube sheet plug according to claim 1, and comprises the following steps: 1) Clean the surface of the tube-to-sheet welded plug sample to remove the oxidation products and oily attachments on the surface to prevent their influence on the evolution and measurement of the plug surface temperature field; 2) Measure and obtain the center of the plug sample surface and mark it, place a heating body with a diameter between 1 / 8 and 1 / 2 of the plug diameter in close contact with the center area of the plug surface and fix it, heat the center area of the plug sample surface, and cover the surface with ceramic insulation fiber; 3) After heating for a preset time, take out the ceramic insulation fiber and test the temperature field on the surface of the plug sample. If the temperature inside and outside the weld is lower than a certain value of the temperature in the area with the same diameter, it is judged that the weld penetration in this area is shallow or there is a crack in the weld; Taking advantage of the fact that shallow weld penetration and crack defects will reduce or partially block the heat conduction path from the center of the plug along the diameter direction outward, heat exchange can only be carried out by more inefficient thermal radiation, resulting in the temperature of the shallow weld penetration or crack defect near the center of the heat source being higher than other areas with the same radius, and the temperature of the shallow weld penetration or crack defect far from the center of the heat source being lower than other areas with the same radius, a semi-quantitative detection of weld penetration uniformity and crack defects is performed.
3. A non-destructive testing method for uniform penetration and cracks of a tube sheet plug weld according to claim 2, It is characterized in that The heating of the central area of the plug surface by the heating body in step 2) is conducted by an electric heating rod, or irradiated by a laser or a xenon lamp.
4. A non-destructive testing method for uniform penetration and cracks of a tube sheet plug weld according to claim 2, It is characterized in that The heating body in step 2) heats the plug to no less than 150°C so that the temperature difference caused by shallow fusion depth and crack defects can be detected, and the upper limit of heating temperature is no higher than the temperature that does not change the material structure and properties.
5. A non-destructive testing method for uniform penetration and cracks of a tube sheet plug weld according to claim 2, It is characterized in that The preset heating time in step 3) is between 1 and 15 minutes. The higher the thermal conductivity of the plug and the weld material or the deeper the set weld penetration, the shorter the heating time is set. The lower the thermal conductivity of the plug and the weld material or the shallower the set weld penetration, the longer the heating time is set.
6. A non-destructive testing method for tube sheet plug weld penetration uniformity and cracks according to claim 2, It is characterized in that Step 3) The temperature field is tested using thin film thermocouples, mesh thermocouples, infrared thermometers or infrared cameras, with a temperature resolution of no less than 2°C and a plane resolution of no less than 0.2°C / mm.
7. A non-destructive testing method for tube sheet plug weld penetration uniformity and cracks according to claim 2, It is characterized in that When judging shallow melting depth or crack defects in step 3), the temperature difference on both sides of the target area needs to be greater than 5°C.
8. A non-destructive testing method for tube sheet plug weld penetration uniformity and cracks according to claim 2, It is characterized in that Combining the heat source temperature, heating time and thermal conductivity of the material, and using the results of the non-steady-state heat transfer relationship of a point heat source in a semi-infinite area, the weld penetration and defect size in different areas can be inferred.
9. A non-destructive testing method for tube sheet plug weld penetration uniformity and cracks according to claim 2, It is characterized in that This method is not only applicable to new tube sheet welding plugs, but also to the quality inspection of in-service tube sheet welding plugs.