Liquid crystal compounds
By adjusting its optical anisotropy through side-substituted curable liquid crystal compounds, it solves the shortcomings of existing LCP films in low melting point, supercooling ability and alignment performance, achieves high birefringence and improves film performance, and is suitable for Preparation of optical and optoelectronic devices.
Patent Information
- Application Number
- CN202080024794.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-16
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-03-16
AI Technical Summary
When preparing optical and optoelectronic devices, it is difficult for existing LCP films to meet the requirements of low melting point, good supercooling ability, high-definition bright spots and good alignment properties at the same time, and high optical anisotropy materials often lead to the formation of smectic mesophase and enhanced crystallization tendency. , reduced solubility and inhomogeneity of disclination in tilted microregions, affecting optical properties.
Provide a laterally substituted curable liquid crystal compound, which can reduce the formation of tilted microdomains and disclinations by adjusting its optical anisotropy, and improve the miscibility and solubility with other LCPs, using the compound of formula (I) and an organic solvent Mix to form an LCP mixture to prepare films with high birefringence.
Achieving a wide range of optical anisotropy in fewer chemical steps reduces film thickness, improves the performance of optical structures, reduces material usage, and maintains good alignment properties and solubility.
Smart Images

Figure CN113631686B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to laterally substituted curable liquid crystals (LCPs) having mesogenic properties or properties which render these LCPs compatible with mesogenic molecular structures. In particular, the present invention relates to laterally substituted curable liquid crystals (LCPs) having adjustable optical anisotropy and simultaneously having a low melting point or good supercooling capability, a relatively high clearing point and good alignment properties, and to the use of such LCPs for the preparation of substantially uniform or patterned films, wherein the orientation of the LCP molecules in the plane and relative to the plane of the substrate can be controlled. Background Art
[0002] Films made of curable liquid crystals (LCP films) are well known to those skilled in the art and are used to prepare optical and optoelectronic devices. US5650534 discloses compounds and mixtures for preparing components suitable for nonlinear optical (NLO) applications. These compounds are optically active and exhibit chiral smectic or chiral nematic mesophases. US5707544 also discloses compounds and mixtures suitable for NLO applications. However, these compounds are characterized by relatively high melting points. US5593617 discloses photochemically polymerizable liquid crystal compounds and mixtures, which are used to prepare optical and electronic components. However, these mixtures have a relatively narrow operating range and are not suitable for use at higher temperatures.
[0003] LCP films are usually manufactured by using known coating and printing techniques. This includes coating an organic solution of a cross-linkable LCP or LCP mixture onto a substrate equipped with an orientation layer. The organic solvent is then removed to obtain a well-oriented, solvent-free mesogenic LCP layer, which is cross-linked to fix the ordered structure of liquid crystal properties. The ideal optical properties of such films depend critically on some physical parameters that the LCP material must simultaneously meet. Such properties are nematic mesophase, high-definition bright spots, low melting point or low crystallization tendency when cooled to below the melting point (supercooling), good solubility in organic solvents, good miscibility with other LCPs, good alignment properties on the orientation layer, and the ability to form an adjustable tilt with substantially no tilt microdomains and disclinations relative to (out of) the substrate plane. Tilt microdomains are regions within the LCP film in which the major axes of the LCP molecules form tilt angles of equal size but opposite directions relative to the substrate plane. Disclinations are the boundary lines of adjacent tilt microdomains, where LCP molecules with opposite tilt angles are adjacent. These tilted domains and disclinations lead both to a disturbance in the uniform appearance of the film and to inhomogeneous optical properties.
[0004] Retardation films are a type of optical element that changes the polarization state of light passing through it. When light passes through a phase retarder, its polarization direction is changed due to the birefringence and thickness of the phase retarder. One of the biggest problems in the preparation of phase retarders is the preparation of high-performance films with small feed amounts. When using liquid crystals with high birefringence, the necessary retardation values can be achieved with small amounts of liquid crystal compounds.
[0005] In order to adjust the optical properties of layers and films (e.g. retardation films) prepared from LCP, it is also necessary to use various LCP materials with different optical anisotropies (mainly high optical anisotropies). It is known that LCPs that exhibit high optical anisotropy often show a negative impact on a variety of the above-mentioned properties. In particular, the formation of smectic mesophases, high melting points, an enhancement of the tendency to crystallize, low solubility in organic solvents or a reduction in miscibility with other LCPs are observed. In addition, the ability to uniformly align without tilted microdomains and disclinations is often reduced.
[0006] Therefore, there is a need for new LCP materials that can be used to prepare LCP mixtures, which significantly reduce the above-mentioned disadvantages. The present invention addresses this need. Summary of the invention
[0007] A first aspect of the present invention provides a compound of formula (I).
[0008]
[0009] in
[0010] G 1 and G 2 independently represent polymerizable mesogenic residues;
[0011] Ar represents an aromatic group selected from phenyl or naphthalene diyl;
[0012] w is 1 or 2;
[0013] X represents a group selected from -CH2-, -O-, -CO-, -COO-, -OOC-, -CONR'-, -OCOO- and -OCONR';
[0014] Sp represents the formula -(CH2) p -, wherein p is an integer from 1 to 18, and one or two non-adjacent -CH2- groups are optionally replaced by -CH=CH-; or one or two -CH2- groups are optionally replaced by one or two groups selected from -O-, -CO-, -COO-, -OOC-, -CONR'-, -OCOO-, -OCONR', with the proviso that: firstly, the spacer group does not contain two adjacent heteroatoms, and secondly, when X is -CH2-, p can also be 0; and
[0015] M represents an achiral group of formula (II)
[0016]
[0017] in
[0018] A and B independently represent an optionally substituted six-membered carbocyclic or heterocyclic group or naphthalene diyl;
[0019] C is selected from a five-membered and six-membered carbocyclic or heterocyclic group or naphthalene diyl;
[0020] n 1 and n 2 is 0 or 1, with the following conditions: First, 1≤n 1 +n 2 ≤2, and secondly, when C is naphthalene diyl, 0≤n 1 +n 2 ≤2;
[0021] Z 1 is selected from -O-, -COO-, -OOC-, -CO-, -CONR'-, -NR'CO-, OCOO-, -OCONR'-, -NR'COO- and a single bond;
[0022] in
[0023] R' is selected from hydrogen, a lower achiral alkyl group and a lower achiral alkenyl group;
[0024] Z 2 and Z 3 are independently selected from a single bond, -COO-, -OOC-, -CH2-CH2-, -CH2O-, -OCH2-, -CH=CH-, -C≡C-, -(CH2)4-, and -(CH2)3O-; and
[0025] R 1 is selected from H, -CN, -COR, -COOR, -OCOR, -CONR'R, -NR'COR, OCOOR, -OCONR'R, -NR'COOR, -F, -Cl, -CF3, -OCF3, -OR and -R
[0026] in
[0027] R is selected from hydrogen, achiral C 1-18 Alkyl groups and achiral C 4-18 alkenyl groups wherein the double bond is at the 3-position or higher; and
[0028] R' is as defined above.
[0029] In addition to the above-mentioned lateral substituted mesogen compounds, such compounds are also disclosed in WO00 / 55110. However, many of these compounds are not suitable for preparing LCP films for optical films. It has been found that by using the compounds of the present invention, thinner phase retarders compared with those of the prior art can be prepared. In addition, LCP according to the present invention generally shows good alignment properties and shows a reduced trend of forming tilted micro-regions and disclinations. In addition, the compounds of the present invention have better solubility in organic solvents, and high miscibility with other LCP compounds. In addition, the compounds of the present invention show higher birefringence, and therefore require less material in the optical structure.
[0030] The optical anisotropy of the compounds of the invention can be easily adjusted to suit the requirements simply by choosing different M groups of formula I without changing the main core of the molecule. This allows a wide range of LCPs showing different optical anisotropies to be obtained economically with a minimum of chemical steps in their preparation.
[0031] The polymerizable mesogenic residue G 1 and G 2 Can be the same or different.
[0032] The group X is preferably selected from -CH2-, -O-, -COO-, -OOC- and -OCOO-.
[0033] The spacer group Sp may optionally be substituted by one or more fluorine or chlorine atoms. Preferred are groups in which no substituents are present. Particularly preferred are groups in which the integer p has a value of 1 to 12 and in which no more than two -CH2- groups are replaced by -O- and no more than one -CH2- group is replaced by a group selected from -CH=CH-, -CO-, -COO-, -OOC-, -CONR'-, -OCOO- and -OCONR'.
[0034] Group A and B are saturated, unsaturated or aromatic. They are optionally substituted by one or two substituents selected from F, Cl, CN, low alkyl, low alkenyl, low alkoxy and low alkenyloxy. Preferably, group A and B contain no more than one substituent separately. Especially preferred is that group A and B do not contain any replacement.
[0035] Preferably, the radicals A and B are selected from 1,4-phenylene, pyridine-2,5-diyl, pyrimidine-2,5-diyl, trans-1,4-cyclohexylene or trans-1,3-dioxane-2,5-diyl, 1,4-naphthalenediyl and 2,6-naphthalenediyl. Particularly preferably, A and B are selected from 1,4-phenylene, trans-1,4-cyclohexylene and 2,6-naphthalenediyl.
[0036] The group C is saturated, unsaturated or aromatic. It is optionally substituted by one or two substituents selected from F, Cl, CN, lower alkyl, lower alkenyl, lower alkoxy and lower alkenyloxy. Preferably, the group C contains at most one substituent. It is especially preferred that the group C does not contain any substitution.
[0037] Preferably, the radical C is selected from furan-2,4-diyl, furan-2,5-diyl, tetrahydrofuran-2,4-diyl, tetrahydrofuran-2,5-diyl, dioxolane-2,4-diyl, dioxolane-2,5-diyl, Oxazole-2,4-diyl, oxadiazole-2,5-diyl, cyclopentane-1,3-diyl, cyclopentane-1,4-diyl, 1,4-phenylene, pyridine-2,5-diyl, pyrimidine-2,5-diyl, trans-1,4-cyclohexylene or dioxane-2,5-diyl, 1,4-naphthalenediyl, 1,3-naphthalenediyl, 1,5-naphthalenediyl, 1,6-naphthalenediyl, 1,7-naphthalenediyl, 2,3-naphthalenediyl, 2,4-naphthalenediyl, 2,5-naphthalenediyl, 2,6-naphthalenediyl, 2,7-naphthalenediyl and 2,8-naphthalenediyl. In particular, C is preferably selected from furan-2,5-diyl, tetrahydrofuran-2,5-diyl, oxadiazole-2,5-diyl, 1,4-phenylene, trans-1,4-cyclohexylene and 2,6-naphthalenediyl.
[0038] Group Z 1 It is preferably selected from -O-, -COO-, -OOC- and a single bond. Z is particularly preferably 1 Selected from -O- or a single bond.
[0039] Group Z 2 and Z 3 It is preferably selected from -COO-, -OOC-, -CH2CH2-, -CH2O-, -OCH2-, -CH=CH-, -C≡C- and a single bond. Z is particularly preferably 2 and Z 3 Selected from -COO-, -OOC-, -C≡C- and a single bond.
[0040] Group R 1 Preferably, it is selected from H, -CN, -COOR, -OCOR, F, Cl, CF3, OCF3, OR, R, wherein R represents C 1-12 Achiral alkyl, C 4-12 Achiral alkenyl groups wherein the double bond is at the 3-position or higher, or hydrogen. Particularly preferred are R 1 Selected from -CN, F, Cl, CF3, OCF3, OR, R, wherein R represents C 1-8 An achiral alkyl group or hydrogen.
[0041] The term "lower alkyl" should be understood to include C1-6 Achiral, branched or straight-chain alkyl groups. Examples of lower alkyl groups that may be present in the compounds of the invention include methyl, ethyl, propyl, butyl, pentyl, hexyl and the like.
[0042] The term "lower alkenyl" should be understood to include C 3-6 Achiral, branched or straight-chain alkenyl groups, wherein the double bond is located at the 2-position or higher. Examples of lower alkenyl groups that may be present in the compounds of the invention include 2-propenyl, 3-butenyl, 3-isopentenyl, 4-pentenyl, 5-hexenyl, 4-isohexenyl and similar groups.
[0043] The term "lower alkoxy" is understood to include C 1-6 Achiral, branched or straight-chain alkoxy groups. Examples of lower alkoxy groups which may be present in the compounds of the invention include methoxy, ethoxy, propoxy, butoxy, pentyloxy, hexyloxy and the like.
[0044] The term "alkenyloxy" is to be understood to include C 3-6 Achiral, branched or straight-chain alkenyloxy groups in which the double bond is located at the 2-position or higher. Examples of lower alkenyloxy groups that may be present in the compounds of the invention include 2-propenyloxy, 3-butenyloxy, 4-pentenyloxy, 5-hexenyloxy and similar groups.
[0045] Preferably, the polymerizable mesogenic residue G 1 and G 2 Each independently represented by a group of formula III
[0046]
[0047] in
[0048] D is selected from 1,4-naphthalenediyl, 2,6-naphthalenediyl and 1,5-naphthalenediyl;
[0049] E is selected from optionally substituted 1,4-phenylene, pyridine-2,5-diyl, pyrimidine-2,5-diyl, trans-1,4-cyclohexylene, trans-1,4-cyclohexane, trans-1,3-dioxane-2,5-diyl, 1,4-naphthalenediyl, 2,6-naphthalenediyl and 1,5-naphthalenediyl;
[0050] m is 1 or 0,
[0051] Z 4 and Z 5 independently selected from a single bond, -COO-, -OOC- and -OCOO-, -CH2-CH2-, -CH2O-, -OCH2-, -CH=CH-, -C≡C-, -(CH2)4- and -(CH2)3O-;
[0052] Z 6 Represents a single bond or formula -(CH2) q X-, wherein q is an integer ranging from 1 to 18, and X is as defined above, and one or two non-adjacent -CH2- groups may optionally be replaced by -CH=CH-, or one or two -CH2- groups may be replaced by one or two additional linking groups X, with the proviso that: first, the group Z 6 does not contain two adjacent heteroatoms, and secondly, when X is -CH2, q can also take the value of 0.
[0053] R 2 represents a polymerizable group selected from CH2=C(Ph)-, CH2=CW-COO-, CH2=CH-COO-Ph-, CH2=CW-CO-NH-, CH2=CH-O-, CH2=CH-OOC-, Ph-CH=CH-, CH2=CH-Ph-, CH2=CH-Ph-O-, R 3 -Ph-CH=CH-COO-, R 3 -OOC-CH=CH-Ph-O- and 2-W-epoxyethyl
[0054] in
[0055] W represents H, Cl, Ph or a lower alkyl group,
[0056] R 3 represents a lower alkyl group, with the condition that: when R 3 When attached to a phenylene group (-Ph-) it may also represent hydrogen or lower alkoxy.
[0057] The terms "Ph" and "Ph-" will be understood to refer to a phenyl group. The term "-Ph-" will be understood to mean any isomer of phenylene, ie, 1,2-phenylene, 1,3-phenylene or 1,4-phenylene, unless the context requires otherwise.
[0058] It is particularly preferred that the radicals D and E do not contain any substitutions.
[0059] Preferred groups Z 4 and Z 5 is selected from a single bond, -COO-, -OOC-, -OCOO-, -CH2-CH2-, -CH2O-, -OCH2-, -CH=CH- and -C≡C-. Z is particularly preferred 4 and Z 5 Represents a single bond, -C≡C-, -COO-, -OCOO- or -OOC-.
[0060] Z 6It may be optionally substituted by one or more halogen atoms, preferably one or more fluorine atoms. Preferably, q is 1 to 11. Also preferably, Z 6 It is further preferred that for group Z 6 , X is selected from -CH2-, -O-, -COO-, OCOO and -OOC-, especially -CH2- or -O-.
[0061] Preferred groups R 2 Selected from CH2=CW-COO- and CH2=CH-O-.
[0062] Preferably, for group G 1 and G 2 In each of the two integers m, the sum of the two integers m is 0 or 1. It is particularly preferred that for G 1 and G 2 In both cases, the value of m is 0.
[0063] The compounds of the present invention can be readily prepared using procedures well known to those skilled in the art.
[0064] The starting materials are either commercially available or can be readily prepared and are well known to those skilled in the art.
[0065] The compounds of the invention are preferably prepared by forming a ring including the side groups and then attaching the mesogenic residues. Alternatively, the compounds may be prepared by forming a ring including a polymerizable mesogenic residue and then attaching the side groups. Thus, a second aspect of the invention provides a method for preparing a compound of formula (I), the method comprising forming a ring including the side groups and then attaching the mesogenic residues thereto. If the mesogenic residue G 1 and G 2 are the same, then G 1 and G 2 Also connect to the center ring.
[0066] LCP material as used in the context of this application shall mean a liquid crystal material comprising liquid crystal monomers and / or liquid crystal oligomers and / or liquid crystal polymers and / or cross-linked liquid crystals. In the case where the liquid crystal material comprises liquid crystal monomers, such monomers may be polymerized, typically after anisotropy has been generated in the LCP material, for example due to contact with an alignment layer. Polymerization may be initiated by heat treatment or by exposure to actinic light, which preferably includes UV light. LCP material may comprise only one single type of liquid crystal compound, but may also comprise additional polymerizable and / or non-polymerizable compounds, not all of which necessarily have to be liquid crystal compounds. In addition, the LCP material may contain additives including, but not limited to, antioxidants, initiators such as photoinitiators, promoters, dyes, inhibitors, activators, fillers, chain transfer inhibitors, pigments, antistatic agents, flame retardants, thickeners, thixotropic agents, surfactants, viscosity modifiers, extender oils, plasticizers, tackifiers, catalysts, sensitizers, stabilizers such as phenol derivatives such as 4-ethoxyphenol or 2,6-di-tert-butyl-4-methylphenol (BHT), lubricants; dispersants; polymer binders and / or monomeric compounds that can be converted into polymer binders by polymerization, or In the case of emulsion coatings and printing inks, dispersing aids, such as those disclosed in U.S. Pat. No. 5,798,147; hydrophobing agents, binders, flow improvers, defoamers, deaerators, diluents, auxiliaries, colorants, dyes and pigments, curing inhibitors, such as hydroquinone, p-tert-butylcatechol; 2,6-di-tert-butyl-p-methylphenol; phenothiazine; N-phenyl-2-naphthylamine; or photo-orientable monomers or oligomers or polymers as described in EP 1 090 325 B, chiral additives, isotropic or anisotropic fluorescent and / or non-fluorescent dyes, in particular dichroic dyes.
[0067] It will be appreciated that compounds of the present invention can be used to prepare LCP mixtures. Such mixtures can be prepared by mixing compounds of formula (I) with one or more additional components. Organic solvents can also be used in the preparation of these mixtures. Therefore, a third aspect of the present invention provides a kind of LCP mixture, which comprises compounds of formula (I) and one or more additional components. The one or more additional components present in the LCP mixture can be other compounds of formula (I), other mesogenic compounds, compounds compatible with the mesogenic molecular architecture or chiral dopants for inducing helical pitch. The LCP mixture can also include suitable organic solvents. Examples of solvents that can be used to prepare such liquid crystal mixtures include, but are not limited to, acetone, cyclopentanone (CP), cyclohexanone (CH), methyl isobutyl ketone (MIBK), methyl ethyl ketone (MEK), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), N-ethylpyrrolidone, N-vinylpyrrolidone, N,N-dimethylacetamide (AN), tetrahydrofuran (THF), 1,3-dioxolane (DXG), ethylene glycol, dipropylene glycol, butyl carbitol, ethyl carbitol acetate, dipropylene glycol monomethyl ether, ethyl acetate (EA), 1-methoxy-2-propanol acetate (MPA), γ-butyrolactone (BL), propylene glycol monoacetate, propylene glycol diacetate, dipropylene glycol monomethyl ether, and dimethyl sulfoxide (DMSO).
[0068] The most preferred are cyclopentanone (CP), cyclohexanone (CH), methyl isobutyl ketone (MIBK), methyl ethyl ketone (MEK), ethyl acetate (EA), 1-methoxy-2-propanol acetate (MPA), 1,3-dioxolane (DXG), and dimethyl sulfoxide (DMSO).
[0069] A dichroic dye is a dye in which the absorbance is different between the longer axis direction and the shorter axis direction of the molecule. Dichroic dyes preferably absorb visible light. Examples of dichroic dyes include azo dyes, acridine dyes, The dichroic dyes may be used alone or in combination. The dichroic dyes may be used in an amount of 0.01 to 40 parts by mass, and preferably 0.05 to 15 parts by mass, relative to 100 parts by mass of the liquid crystal mixture.
[0070] The compounds of the present invention can also be used to form an LCP layer by casting the LCP compound according to the first aspect of the present invention or the LCP mixture according to the third aspect of the present invention onto a substrate. Therefore, a fourth aspect of the present invention provides a method for forming an LCP network, the method comprising forming an LCP layer comprising a compound of formula (I) and crosslinking the layer. The LCP mixture according to the third aspect of the present invention can also be used to manufacture an LCP network in a similar manner.
[0071] In a fifth aspect of the invention, the present invention also comprises a crosslinked LCP network comprising the compound of formula (I) in crosslinked form. A crosslinked LCP network comprising the mixture according to the third aspect of the invention in crosslinked form may also be comprised in this aspect of the invention.
[0072] The sixth aspect of the present invention provides the use of the compound of formula (I) for preparing an optical or optoelectronic device. The use of the liquid crystal mixture according to the third aspect of the present invention for preparing an optical or optoelectronic device is also included in this aspect of the present invention.
[0073] The seventh aspect of the present invention provides an optical or optoelectronic device comprising a compound of formula (I) in a crosslinked state. An optical or optoelectronic device comprising an LCP liquid crystal mixture according to the third aspect of the present invention in a crosslinked state is also included in this aspect of the present invention.
[0074] The LCP mixture can be applied to a carrier. The carrier can be rigid or flexible and can have any form or shape. For example, it can be an object with a complex surface. In principle, it can be composed of any material. Preferably, the carrier comprises plastic, glass or metal or is a silicon wafer. In the case where the carrier is flexible, preferably the carrier is plastic or metal foil. Preferably, the surface of the carrier is flat. For some applications, the carrier may comprise a topographical surface structure, such as a microstructure, such as a microlens or a microprism, or a structure exhibiting a sudden change in shape, such as a rectangular structure. Preferably, the carrier is transparent.
[0075] During the deposition of the LCP mixture, the carrier may be mobile. For example, the layer of the LCP mixture may be prepared in a continuous roll-to-roll process by depositing the material composition onto a moving flexible foil, which is preferably plastic or metal. The resulting film may then be wound on a drum together with the carrier foil, or the film may be detached from the carrier and then wound as a self-supporting film without a carrier.
[0076] The carrier may have additional layers, such as organic layers, dielectric layers or metal layers. These layers may have different functions, for example, an organic layer may be applied as a primer layer, which increases the compatibility of the material to be applied with the carrier. The metal layer can be used as an electrode, for example when used in an optoelectronic device such as a display, or the metal layer may have the function of a reflector. The carrier may also be an optical element or device with certain functions, such as a substrate for an LCD, which may, for example, contain a thin film transistor, an electrode or a color filter. In another example, the carrier is a device comprising an OLED layer structure. The carrier may also be a retardation film, a polarizer, such as a polarizing film or sheet polarizer, a reflective polarizer, such as the commercially available Vikuity TM DBEF membrane.
[0077] The LCP mixture can be applied to the carrier by any suitable method, such as extrusion, casting, molding, 2D- or 3D-printing or coating. Suitable coating methods are, for example, spin coating, blade coating, knife coating, kiss roll coating, die coating, dipping, brush coating, rod casting, roller coating, flow coating, line coating, spray coating, dip coating, curtain coating, air knife coating, reverse roller coating, gravure coating, metering rod (Meyer bar) coating, slot die (extrusion) coating, roller coating, flexographic coating. Suitable printing methods include: screen printing, relief printing, such as flexographic printing, inkjet printing, gravure printing, such as direct gravure printing or offset gravure printing, lithography, such as offset printing, or stencil printing, such as screen printing.
[0078] A layer of the LCP mixture does not necessarily cover the entire surface of the support. On the contrary, the layer may be applied in the form of a pattern, for example by printing, or may be processed after deposition, for example by photolithographic methods, to have the form of a pattern.
[0079] The alignment of the LCP can be achieved by any known means for aligning liquid crystals. For example, the carrier may have an alignment surface, which is intended to mean that the surface has the ability to align liquid crystals. The carrier may already provide the alignment without further treatment. For example, if a plastic substrate is used as a carrier, it can provide alignment on the surface due to the manufacturing method, such as extrusion or stretching of the substrate. The carrier can also be brushed or embossed with oriented microstructures to produce alignment capabilities. Alternatively, a thin layer of material can be applied to a carrier specifically designed for alignment performance. The layer can be further brushed or, for example, processed by embossing to provide oriented microstructures on the surface. If the thin layer contains a photo-orientable substance, alignment can be produced by exposure to aligning light.
[0080] The alignment surface of the substrate may exhibit a pattern of alignment directions in order to define an orientation pattern for the liquid crystals in the LCP layer. Preferably, an alignment layer comprising a photo-alignable substance is used for this purpose and the alignment pattern is produced by selective exposure to aligning light with different polarization planes. DETAILED DESCRIPTION
[0081] The present invention will now be described with reference to the following non-limiting examples. These embodiments are provided by way of illustration only. Variations of these embodiments falling within the scope of the present invention will be apparent to those skilled in the art.
[0082] Example
[0083] Definitions used in the examples:
[0084] 1 H NMR: 1 H NMR spectroscopy
[0085] DMSO-d6: deuterated dimethyl sulfoxide
[0086] 300MHz: 300 megahertz
[0087] m: multiplet, d: doublet, dd: doublet of doublets, t: triplet, s: singlet
[0088] DMF: dimethylformamide
[0089] HCl solution (25%): volume percentage
[0090] CH2Cl2: dichloromethane
[0091] THF: Tetrahydrofuran
[0092] In the following examples, the thermotropic phases are abbreviated as follows:
[0093] T (Cr-N) : Transition temperature from crystalline phase to nematic phase
[0094] T (N-I) : Transition temperature from nematic phase to isotropic phase
[0095] Example 1: Preparation of 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile compound 1
[0096] A mixture of 39.1 g (0.2 mol) of 4-(4-cyanophenyl)phenol, 34.5 g (0.26 mol) of potassium carbonate, 4.35 g (0.026 mol) of potassium iodide and 35.5 g (0.26 mol) of 6-chlorohexanol in DMF was heated at 80° C. for 18 hours. The solution was then cooled and poured into 1.2 L of water. The precipitate obtained was filtered off and washed twice with 2 L of water. The solid was then recrystallized from acetonitrile to give 50.4 g of 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile as a white crystalline powder.
[0097] Example 2: Preparation of 4-[4-(8-hydroxyoctyloxy)phenyl]benzonitrile compound 2
[0098] Compound 2 was prepared according to the method described for compound 1 in Example 1, with the proviso that 6-chlorohexanol was replaced by 8-chlorooctanol.
[0099] Example 3: Preparation of 4-[4-(10-hydroxydecyloxy)phenyl]benzonitrile compound 3
[0100] Compound 3 was prepared according to the method described for compound 1 in Example 1, with the proviso that 6-chlorohexanol was replaced by 10-chlorodecanol.
[0101] Example 4: Preparation of 4-[4-(11-hydroxyundecyloxy)phenyl]benzonitrile compound 4
[0102] Compound 4 was prepared according to the method described for compound 1 in Example 1, with the proviso that 6-chlorohexanol was replaced by 11-chloroundecanol.
[0103] Example 5: Preparation of 2,5-dihydroxybenzoic acid 6-[4-(4-cyanophenyl)phenoxy]hexyl ester compound 5
[0104] 52.1 g (0.51 mol) of triethylamine was added dropwise to a solution of 50.4 g (0.17 mol) of 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile dissolved in 450 mL of THF. The mixture was cooled to 0°C and 23.5 g (0.204 mol) of methanesulfonyl chloride was slowly added. After stirring for 3 hours, the mixture was filtered off under silica and dried by removing the solvent under reduced pressure to give 70.7 g of 6-[4-(4-cyanophenyl)phenoxy]hexyl methanesulfonate as a yellow oil. 27.2 g (0.175 mol) of 2,3,4,6,7,8,9,10-octahydropyrimido[1,2-a]azepine Add to a solution of 28.1 g (0.179 mol) of 2,5-dihydroxybenzoic acid in 190 mL DMF. 7.65 g of sodium iodide, 70.7 g (0.170 mol) of methanesulfonic acid 6-[4-(4-cyanophenyl)phenoxy]hexyl ester in 190 mL DMF are introduced into the mixture. After 4 hours, the resulting mixture is poured into 2 L of cold water. Filter out the precipitate and wash it twice with water. The light yellow solid is recrystallized in CH3CN to obtain 57.7 g of 2,5-dihydroxybenzoic acid 6-[4-(4-cyanophenyl)phenoxy]hexyl ester as a white powder.
[0105] Example 6: Preparation of 2,5-dihydroxybenzoic acid 8-[4-(4-cyanophenyl)phenoxy]octyl ester compound 6
[0106] Compound 6 was prepared according to the method described for compound 5 in Example 5, with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by 4-[4-(8-hydroxyoctyloxy)phenyl]benzonitrile compound 2.
[0107] Example 7: Preparation of 2,5-dihydroxybenzoic acid 10-[4-(4-cyanophenyl)phenoxy]decyl ester compound 7
[0108] Compound 7 was prepared according to the method described for compound 5 in Example 5, with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by compound 3.
[0109] Example 8: 2,5-dihydroxybenzoic acid 11-[4-(4-cyanophenyl)phenoxy]undecyl ester compound 8 preparation
[0110] Compound 8 was prepared according to the method described for compound 5 in Example 5, with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by compound 4.
[0111] Example 9: Preparation of 6-(6-hydroxyhexyloxy)naphthalene-2-carboxylic acid compound 9
[0112] A mixture of 76.3 g (0.377 mol) of 6-hydroxynaphthalene-2-carboxylic acid methyl ester, 68.5 g (0.49 mol) of potassium carbonate, 8.2 g (0.049 mol) of potassium iodide and 67 g (0.49 mol) of 6-chlorohexanol in 250 mL of DMF was heated to 80 ° C for 18 hours. The solution was then cooled and poured into 2.6 L of cold water. The precipitate was filtered out and washed twice with water. The product was then recrystallized from acetonitrile to obtain 94.2 g of white powder. The mixture formed by this solid in 680 mL of DMF, 37.95 g of sodium hydroxide, 340 mL of methanol and 75 mL of water was stirred at 60 ° C for 4 hours. 122.2 g of hydrochloric acid in 782 mL of water was added dropwise. The suspended matter was filtered out to obtain 85.8 g of white solid 6-(6-hydroxyhexyloxy)naphthalene-2-carboxylic acid.
[0113] Example 10: Preparation of 6-(8-hydroxyoctyloxy)naphthalene-2-carboxylic acid compound 10
[0114] Compound 10 was prepared according to the procedure described for compound 9 in Example 9, with the proviso that 6-chlorohexanol was replaced by 8-chlorooctanol.
[0115] Example 11: Preparation of 6-(8-hydroxydecyloxy)naphthalene-2-carboxylic acid compound 11
[0116] Compound 11 was prepared according to the procedure described for compound 9 in Example 9, with the proviso that 6-chlorohexanol was replaced by 10-chlorodecanol.
[0117] Example 12: Preparation of 6-(11-hydroxyundecyloxy)naphthalene-2-carboxylic acid compound 12
[0118] Compound 12 was prepared according to the procedure described for compound 9 in Example 9, with the proviso that 6-chlorohexanol was replaced by 11-chloroundecanol.
[0119] Example 13: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[6-[4-(4-cyanophenyl)benzene Oxy]hexyloxycarbonyl]-4-[6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl]oxy-phenyl]ester compound 13 Preparation
[0120] 45.3 g (0.357 mol) of chloropropionyl chloride in 50 mL of N-methyl-2-pyrrolidone was added dropwise to 85.8 g (0.297 mol) of 6-(6-hydroxyhexyloxy)naphthalene-2-carboxylic acid in 220 mL of N-methyl-2-pyrrolidone. The mixture was stirred at room temperature for 2 hours. The solution was then poured onto 810 mL of water and the solid was filtered off and dried under vacuum to give 105.25 g.
[0121] 6.1 g (0.0161 mol) of the previous product, 3 g (0.0070 mol) of 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate, 0.2 g of 4-(dimethylamino)-pyridine and 3.65 g of dicyclohexylcarbodiimide (0.0175 mol) were mixed in 120 mL of CH2Cl2 and stirred overnight at room temperature. The solution was filtered through hyflo silica and the solution was dried under vacuum to obtain a white solid. The solid was dissolved in 50 mL of CH2Cl2 along with 3.2 g of triethylamine. The mixture was stirred overnight at 40°C, filtered out and dried under vacuum. The white solid was recrystallized from acetonitrile to obtain 5.95 g of white solid 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[6-[4-(4-cyanophenyl)phenoxy]hexyloxycarbonyl]-4-[6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl]oxy-phenyl] ester compound 13.
[0122] Liquid crystal phase transition: Compound 13 was observed under crossed polarizers using a polarizing microscope to determine its phase transition temperature. The result was that when the temperature was increased, the crystalline phase was at 105°C (T (Cr-N)) and the isotropic phase appears above 150°C (T (N-I) ).
[0123] In DMSO-d6 1 H NMR (300 MHz): in DMSO-d6 1 H NMR (300MHz): 8.80(s,2H),8.11(m,4H),7.95(m,3H),7.86(d,4H),7.80(d,1H),7.76(d,2H),7.58(d,1H),7.43(d ,2H),7.28(d,2H),6.94(d,2H),6.32(m,2H),6.13(m,2H),5.93(m,2H),4.10(m,10H),3.73(t,2H),2-0.8(m,24H).
[0124] Example 14: (acry6-8) 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[8-[4-(4-cyano 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl)oxy-phenyl] Preparation of ester compound 14
[0125] Compound 14 was prepared according to the method described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 8-[4-(4-cyanophenyl)phenoxy]octyl 2,5-dihydroxybenzoate.
[0126] Liquid crystal phase transition: T (Cr-N) : 96℃, T (N-I) >150℃
[0127] In DMSO-d6 1 H NMR (300 MHz): in DMSO-d6 1 H NMR (300MHz): 8.80(s,2H),8.09(m,4H),7.94(m,3H),7.83(d,4H),7.80(d,1H),7.66(d,2H),7.58(d,1H),7.45(d, 2H),7.28(d,2H),7.02(d,2H),6.30(m,2H),6.16(m,2H),5.92(m,2H),4.14(m,10H),3.90(t,2H),1.9-0.7(m,28H).
[0128] Example 15: (acry6-10) 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[10-[4-(4- [(6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl)oxy]benzene] Preparation of ester compound 15
[0129] Compound 15 was prepared according to the method described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 10-[4-(4-cyanophenyl)decyloxy]octyl 2,5-dihydroxybenzoate.
[0130] Liquid crystal phase transition: T (Cr-N) : 107℃, T (N-I) >150℃
[0131] In DMSO-d6 1 H NMR (300MHz): 8.68(d,2H),7.98(m,4H),7.84(m,3H),7.73(d,4H),7.67(dd,1H),7.58(d,2H),7.47(d,1H),7.36(d, 2H),7.17(d,2H),6.92(d,2H),6.24(m,2H),6.10(m,2H),5.81(m,2H),3.98(m,10H),3.85(t,2H),1.9-0.7(m,32H).
[0132] Example 16: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[11-[4-(4-cyanophenyl)benzene [6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl]oxy-phenyl] ester Preparation of Compound 16
[0133] Compound 16 was prepared according to the procedure described for compound 13 in Example 13, with the proviso that 2,5-dihydroxybenzoic acid 6-[4-(4-cyanophenyl)phenoxy]hexyl ester was replaced by 2,5-dihydroxybenzoic acid 11-[4-(4-cyanophenyl)undecyloxy]octyl ester.
[0134] Liquid crystal phase transition: T (Cr-N) : 90℃, T (N-I) : 141℃
[0135] Example 17: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[6-[4-(4-cyanophenyl)benzene oxy]hexyloxycarbonyl]-4-[6-(11-prop-2-enoyloxyundecyloxy)naphthalene-2-carbonyl]oxy-phenyl] esterification Preparation of Compound 17
[0136] Compound 17 was prepared according to the procedure described for compound 13 in Example 13, with the proviso that 6-(6-hydroxyhexyloxy)naphthalene-2-carboxylic acid was replaced by 6-(11-hydroxyundecyloxy)naphthalene-2-carboxylic acid.
[0137] Liquid crystal phase transition: T (Cr-N) : 120℃, T (N-I) >150℃
[0138] Example 18: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[8-[4-(4-cyanophenyl)benzene Oxy]octyloxycarbonyl]-4-[6-(11-prop-2-enoyloxyundecyloxy)naphthalene-2-carbonyl]oxy-phenyl] esterification Preparation of Compound 18
[0139] Compound 18 was prepared according to the procedure described for compound 17 in Example 17, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 8-[4-(4-cyanophenyl)phenoxy]octyl 2,5-dihydroxybenzoate.
[0140] Liquid crystal phase transition: T (Cr-N) :109℃,T (N-I) >150℃
[0141] Example 19: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[10-[4-(4-cyanophenyl)benzene oxy]decyloxycarbonyl]-4-[6-(11-prop-2-enoyloxyundecyloxy)naphthalene-2-carbonyl]oxy-phenyl] esterification Preparation of Compound 19
[0142] Compound 19 was prepared according to the procedure described for compound 17 in Example 17, with the proviso that 2,5-dihydroxybenzoic acid 6-[4-(4-cyanophenyl)phenoxy]hexyl ester was replaced by 2,5-dihydroxybenzoic acid 10-[4-(4-cyanophenyl)phenoxy]decyl ester.
[0143] Liquid crystal phase transition: T (Cr-N) : 98℃, T (N-I) >150℃.
[0144] In DMSO-d6 1 H NMR (300MHz): 8.82(d,2H),8.15(m,4H),7.95(m,6H),7.85(d,4H),7.71(m,3H),7.60(d,1H),7.48(s,2H),7. 30(d,2H),7.15(d,2H),6.35(m,2H),6.20(m,2H),5.94(m,2H),4.10(m,10H),3.95(t,2H),1.9-0.7(m,54H).
[0145] Example 20: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[10-[4-(4-cyanophenyl)benzene Oxy]decyloxycarbonyl]-4-[6-(10-prop-2-enoyloxydecyloxy)naphthalene-2-carbonyl]oxy-phenyl]ester compound Preparation of 20
[0146] Compound 20 was prepared according to the procedure described for compound 19 in Example 19, with the proviso that 6-(11-hydroxyundecyloxy)naphthalene-2-carboxylic acid was replaced by 6-(10-hydroxydecyloxy)naphthalene-2-carboxylic acid.
[0147] Liquid crystal phase transition: T (Cr-N) : 80℃, T (N-I) >150℃
[0148] Example 21: 6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carboxylic acid [3-[6-[4-(4-cyano phenyl)phenoxy]hexyloxycarbonyl]-4-[6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carbonyl]oxy- Preparation of phenyl] ester compound 21
[0149] 5g (0.0140mol) 6-(4-propane-2-enoyloxy butoxycarbonyloxy) naphthalene-2-carboxylic acid (prepared according to the method described in patent US7670505B2) and 35mg BHT are mixed in 50mL CH2Cl2. 3.5ml DMF and 1.9g (0.0145mol) oxalyl chloride are added to the solution. Subsequently the reaction mixture is stirred at room temperature for 1 hour, and then excessive oxalyl chloride is removed under reduced pressure. The product is dissolved in CH2Cl2 and added dropwise to 2.7g (0.0062mol) 2,5-dihydroxybenzoic acid 6-[4-(4-cyanophenyl) phenoxy] hexyl ester compound 5, 3.85g N, N-dimethylcyclohexylamine and 5mg 2,6-di-tert-butyl-4-methylphenol in 50mL CH2Cl2. The resulting mixture is stirred at room temperature for 4 hours. Then, 3 g of 25% hydrochloric acid and 100 mL of water were added, and phase separation occurred. The organic phase was washed twice with saturated sodium chloride aqueous solution, dried over anhydrous sodium sulfate and concentrated under reduced pressure. The residue was recrystallized from CH3CN to obtain 2.45 g of white solid compound 21.
[0150] Liquid crystal phase transition: T (Cr-N) : 99℃, T (N-I) >150℃
[0151] In DMSO-d6 1 H NMR (300MHz): 8.95(s,2H),8.32(m,2H),8.16(m,4H),7.96(d,3H),7.80(m,5H),7.57(m,5H),6.96(d,2H),6.34(m ,2H),6.20(m,2H),5.96(m,2H),4.26(m,4H),4.09(m,6H),3.77(t,2H),1.75(m,8H),1.6-1.2(m,4H),1.15(m,4H).
[0152] Example 22: 6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carboxylic acid [3-[8-[4-(4-cyano phenyl)phenoxy]octyloxycarbonyl]-4-[6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carbonyl]oxy- Preparation of phenyl] ester compound 22
[0153] Compound 22 was prepared according to the procedure described for compound 21 in Example 21 with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 8-[4-(4-cyanophenyl)phenoxy]octyl 2,5-dihydroxybenzoate.
[0154] Liquid crystal phase transition: T (Cr-N) : 103℃, T (N-I) >150℃
[0155] Example 22A: Preparation of 10-(4-phenylphenoxy)decan-1-ol Compound 22A
[0156] Compound 22A was prepared according to the procedure described for compound 3 in Example 3, with the proviso that 4-(4-cyanophenyl)phenol was replaced by 4-phenylphenol.
[0157] Example 22B: Preparation of 10-[4-(p-methylphenyl)phenoxy]decan-1-ol Compound 22B
[0158] Compound 22B was prepared according to the procedure described for compound 3 in Example 3, with the proviso that 4-(4-cyanophenyl)phenol was replaced by 4-(p-tolyl)phenol.
[0159] Example 22C: Preparation of 6-(10-hydroxydecyloxy)naphthalene-2-carbonitrile Compound 22C
[0160] Compound 22C was prepared according to the procedure described for compound 3 in Example 3, with the proviso that 4-(4-cyanophenyl)phenol was replaced by 6-hydroxynaphthalene-2-carbonitrile.
[0161] Example 22D: Preparation of 6-(3-hydroxypropoxy)naphthalene-2-carboxylic acid compound 22D
[0162] Compound 22D was prepared according to the procedure described for compound 9 in Example 9, with the proviso that 6-chlorohexanol was replaced by 3-bromopropanol.
[0163] Example 22E: Preparation of 2,5-dihydroxybenzoic acid 10-(4-phenylphenoxy)decyl ester Compound 22E
[0164] Compound 22E was prepared according to the procedure described for compound 5 in Example 5, with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by 10-(4-phenylphenoxy)decan-1-ol compound.
[0165] Example 22F: Preparation of 2,5-dihydroxybenzoic acid 10-[4-(p-tolyl)phenoxy]decyl ester
[0166] Compound 22F was prepared according to the procedure described for compound 5 in Example 5, with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by 10-[4-(p-tolyl)phenoxy]decan-1-ol compound.
[0167] Example 22G: Preparation of 2,5-dihydroxybenzoic acid 10-[(6-cyano-2-naphthyl)oxy]decyl ester Compound 22G Preparation.
[0168] Compound 22G was prepared according to the procedure described for compound 5 in Example 5 with the proviso that 4-[4-(6-hydroxyhexyloxy)phenyl]benzonitrile was replaced by 6-(10-hydroxydecyloxy)naphthalene-2-carbonitrile Compound 22G.
[0169] Example 22H: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[10-(4-phenylphenoxy)decyl Preparation of [oxycarbonyl]-4-[6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl]oxy-phenyl] ester compound 22H
[0170] Compound 22H was prepared according to the procedure described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 10-(4-phenylphenoxy)decyl 2,5-dihydroxybenzoate.
[0171] Liquid crystal phase transition: T (Cr-N) : 90℃, T (N-I) : 127℃
[0172] In DMSO-d6 1 H NMR(300MHz): 8.78(d,2H),8.12(m,4H),7.96(m,3H),7.75(dd,1H),7.57(m,5H),7.42(dd,4H),7.28(m ,3H),6.97(d,2H),6.32(m,2H),6.18(m,2H),5.89(m,2H),4.10(m,10H),3.93(t,2H),1.9-0.7(m,32H).
[0173] Example 22I: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [4-[6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid Compound 22I Preparation.
[0174] Compound 22I was prepared according to the procedure described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 10-[4-(p-tolyl)phenoxy]decyl 2,5-dihydroxybenzoate.
[0175] Liquid crystal phase transition: T (Cr-N) : 93℃, T (N-I) :152℃
[0176] In DMSO-d6 1 H NMR(300MHz): 8.80(d,2H),8.12(m,4H),7.94(m,3H),7.76(dd,1H),7.52(m,7H),7.24(dd,4H),6.96(d ,2H),6.30(m,2H),6.17(m,2H),5.95(m,2H),4.13(m,10H),3.93(t,2H),2.32(s,3H),1.9-0.7(m,32H).
[0177] Example 22J: 6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carboxylic acid [3-[10-[(6-cyano-2-naphthyl) Oxy] decyloxycarbonyl]-4-[6-(6-prop-2-enoyloxyhexyloxy)naphthalene-2-carbonyl]oxy-phenyl] ester compound Preparation of 22J
[0178] Compound 22J was prepared according to the procedure described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 10-[(6-cyano-2-naphthyl)oxy]decyl 2,5-dihydroxybenzoate.
[0179] Liquid crystal phase transition: T (Cr-N) : 71℃, T (N-I) : 137℃
[0180] In DMSO-d6 1 H NMR (300MHz): 8.80(d,2H),8.45(d,1H),8.11(m,4H),7.96(m,5H),7.75(m,2H),7.58(d,1H),7.45(dd, 3H),7.29(d,3H),6.30(m,2H),6.19(m,2H),5.94(m,2H),4.10(m,12H),3.85(t,2H),1.9-0.6(m,32H).
[0181] Example 22K: 6-(3-prop-2-enoyloxypropoxy)naphthalene-2-carboxylic acid [3-[10-[4-(4-cyanophenyl) Phenoxy]decyloxycarbonyl]-4-[6-(3-prop-2-enoyloxypropoxy)naphthalene-2-carbonyl]oxy-phenyl]ester compound Preparation of 22K
[0182] Compound 22K was prepared according to the method described for compound 13 in Example 13, with the proviso that 6-[4-(4-cyanophenyl)phenoxy]hexyl 2,5-dihydroxybenzoate was replaced by 10-[(6-cyano-2-naphthyl)oxy]decyl 2,5-dihydroxybenzoate, and 6-(6-hydroxyhexyloxy)naphthalene-2-carboxylic acid was replaced by 6-(3-hydroxypropoxy)naphthalene-2-carboxylic acid.
[0183] Liquid crystal phase transition: T (Cr-N) :110.4℃,T (N-I) >160℃
[0184] In DMSO-d6 1 H NMR(300MHz): 8.79(d,2H),8.10(m,4H),7.94(m,3H),7.81(d,5H),7.66(d,2H),7.57(d,1H),7.48(d,2H),7.29(d,2H),7.02(d,2H),6 .35(m,2H),6.16(m,2H),5.95(m,2H),4.33(m,6H),4.25(t,2H),4.07(t,2H),3.95(t,2H),2.17(m,4H),1.64(t,2H),1.5-0.5(m,14H).
[0185] Example 23A: Preparation of an alignment layer using a photoalignment material
[0186] A glass substrate was spin-coated with a photoalignment composition (2% solid content of photoalignment material in cyclopentanone as described in patent publication WO2012 / 085048). The film was dried at 80°C for 30 seconds and the resulting film thickness was about 100 nm. The film was then exposed to alignment light, which was collimated and linearly polarized UV (LPUV) light (280-320 nm) with a flux of 250 mJ / cm 2 The polarization plane is 0° relative to a reference edge on the substrate.
[0187] Embodiment 23:
[0188] A 15.0 wt% solution was prepared by mixing 14.79 wt% of compound 16, 0.03 wt% of 2,6-di-tert-butyl-4-methylphenol, and 0.18 wt% of Irgacure 369 in cyclohexanone, and the solution was stirred thoroughly until the solid was completely dissolved at room temperature. The above polymer solution was spin-coated onto a glass plate having an alignment layer of Example 23A to form a liquid crystal film. The film was dried on a temperature-controlled hot plate at 90°C for 5 minutes. The sample was cooled to room temperature and then photopolymerized by irradiating with UV light for about 2 minutes using a mercury lamp at room temperature under a N2 atmosphere to fix the alignment state of the liquid crystal.
[0189] The resulting films exhibit a very well oriented nematic mesophase at room temperature.
[0190] Embodiment 24:
[0191] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 21. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0192] Embodiment 25:
[0193] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 22. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a well-oriented nematic mesophase at room temperature.
[0194] Embodiment 26:
[0195] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 15. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0196] Example 26B:
[0197] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 22H. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0198] Example 26C:
[0199] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 221. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0200] Example 26D:
[0201] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 22J. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0202] Example 26E:
[0203] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by compound 22K. The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0204] Comparative Example 1:
[0205] The film was prepared as in Example 23, with the only difference that compound 16 was replaced by 2,5-bis[[4-(6-prop-2-enoyloxyhexyloxy)]benzoyl]oxy]benzoic acid 10-[4-(4-cyanophenyl)phenoxy]decyl ester described in patent application WO2011 / 003846A1. The film was dried on a temperature-controlled hot plate at 90°C for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0206] Comparative Example 2:
[0207] Films were prepared as in Example 23 except that compound 16 was obtained from 6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carboxylic acid [4-[6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carbonyl]oxyphenyl] ester ( The film was dried on a temperature-controlled hot plate at 100° C. for 5 minutes. The resulting film exhibited a very well oriented nematic mesophase at room temperature.
[0208] Embodiment 27:
[0209] The retardation at 550 nm of the samples described in Example 23, Example 25, Example 26, in Comparative Example 1 and in Comparative Example 2 was measured with an ellipsometer. The thickness of the samples was measured by a contact stylus profilometer. The birefringence (Δn) was obtained from the determined retardation and thickness values according to the formula (Δn=retardation / thickness). These values are listed in Table 1.
[0210] Example Thickness(μm) Retardation at 550nm Δn 23 1.05 236 0.23 25 1.04 233 0.22 26 1.06 256 0.24 26B 1.07 221 0.21 26C 1.12 250 0.22 26D 1.16 271 0.23 26E 1.14 322 0.28 Comparative Example 2 1.03 206 0.20 Comparative Example 1 1.03 205 0.20
[0211] Table 1
[0212] The films of Examples 23, 25, 26, 26B, 26C, 26D and 26E have higher birefringence than the films of Comparative Examples 1 and 2. These new LCPs can be used to prepare phase retarder optical films as quarter wave plates (QWP) and half wave plates (HWP). Retarder transmits light and changes its polarization state, and it is widely used in various display applications or for security elements. The particularly high birefringence of these new LCPs leads to a significant reduction in the thickness of the retarder film. As an example, Table 2 shows the thickness required for obtaining a half wave plate (λ / 2) retarder (HWP) at 550nm using compounds 15, 16, 22, 22H, 22I, 22J, 22K used in Examples 26, 23, 25, 26B, 26C, 26D and 26E, respectively.
[0213] Example Required thickness of HWP at 550nm (μm) 23 1.20 25 1.25 26 1.15 26B 1.31 26C 1.23 26D 1.2 26E 0.98 Comparative Example 2 1.38 Comparative Example 1 1.38
[0214] Table 2
[0215] Example 28: Formation of Polarizing Film Comparative Example 3
[0216] The composition is obtained by mixing the following components:
[0217] 29.26 parts of the 2,5-bis[[4-(6-prop-2-enoyloxyhexyloxy)benzoyl]oxy]benzoic acid 10-[4-(4-cyanophenyl)phenoxy]decyl ester compound described in patent application WO2011 / 003846A1 were mixed with 1.24 parts of A black mixture of X13, 0.95 parts of Irgacure OXE03 produced by BASF and 0.016 parts of 2,6-di-tert-butyl-4-methylphenol were mixed and the mixture was dissolved in 68.5 parts of cyclohexanone.
[0218] The solution was coated by K-rod coating with an N°3 rod on a 100 nm photoalignment layer coated on a glass (D263) substrate that had been exposed to 250 mJ of linearly polarized light. The substrate was then heated in an oven at 90°C for 5 minutes and cooled to room temperature. The coated LCP layer was then photopolymerized by irradiation with UV light using a mercury lamp under N2 atmosphere at room temperature for about 2 minutes to fix the orientation state of the liquid crystal.
[0219] Example 29: Forming a polarizing film using Comparative Example 4
[0220] The composition is obtained by mixing the following components:
[0221] 29.33 parts of 6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carboxylic acid [4-[6-(4-prop-2-enoyloxybutoxycarbonyloxy)naphthalene-2-carbonyl]oxyphenyl] ester (described in US Pat. No. 7,670,505 B2) obtained from US Pat. No. 7,670,505 B2 LC1057) and 1.18 parts of A black mixture of X13, 0.95 parts of Irgacure OXE03 produced by BASF and 0.016 parts of 2,6-di-tert-butyl-4-methylphenol were mixed and the mixture was dissolved in 68.5 parts of cyclohexanone.
[0222] The solution was coated by K-rod coating with an N°3 rod on a 100 nm photoalignment layer coated on a glass (D263) substrate that had been exposed to 250 mJ of linearly polarized light. The substrate was then heated in an oven at 90°C for 5 minutes and cooled to room temperature. The coated LCP layer was then photopolymerized by irradiation with UV light using a mercury lamp under N2 atmosphere at room temperature for about 2 minutes to fix the orientation state of the liquid crystal.
[0223] Example 30: Formation of a polarizing film using the compound from Example 15
[0224] The composition is obtained by mixing the following components:
[0225] 29.45 parts of the compound of Example 15 were mixed with 1.06 parts of A black mixture of X13, 0.95 parts of Irgacure OXE03 produced by BASF and 0.016 parts of 2,6-di-tert-butyl-4-methylphenol were mixed and the mixture was dissolved in 68.5 parts of cyclohexanone.
[0226] The solution was coated by K-rod coating with an N°3 rod on a 100 nm photoalignment layer coated on a glass (D263) substrate that had been exposed to 250 mJ of linearly polarized light. The substrate was then heated in an oven at 90°C for 5 minutes and cooled to room temperature. The coated LCP layer was then photopolymerized by irradiation with UV light using a mercury lamp under N2 atmosphere at room temperature for about 2 minutes to fix the orientation state of the liquid crystal.
[0227] Example 31: Formation of a polarizing film using the compound from Example 15
[0228] The composition is obtained by mixing the following components:
[0229] 16.42 parts of the compound of Example 15 were mixed with 1.00 parts of A black mixture of X13, 0.95 parts of Irgacure OXE03 produced by BASF and 0.016 parts of 2,6-di-tert-butyl-4-methylphenol were mixed and the mixture was dissolved in 82 parts of cyclohexanone.
[0230] The solution was coated by K-rod coating with an N°3 rod on a 100 nm photoalignment layer coated on a glass (D263) substrate that had been exposed to 250 mJ of linearly polarized light. The substrate was then heated in an oven at 90°C for 5 minutes and cooled to room temperature. The coated LCP layer was then photopolymerized by irradiation with UV light using a mercury lamp under N2 atmosphere at room temperature for about 2 minutes to fix the orientation state of the liquid crystal.
[0231] Example 32: Formation of a polarizing film using the compound from Example 22K
[0232] The composition is obtained by mixing the following components:
[0233] 16.42 parts of the compound of Example 22K were mixed with 1.00 parts of A black mixture of X13, 0.54 parts of Irgacure OXE03 produced by BASF and 0.009 parts of 2,6-di-tert-butyl-4-methylphenol were mixed and the mixture was dissolved in 82 parts of cyclohexanone.
[0234] The solution was coated by K-rod coating with an N°3 rod on a 100 nm photoalignment layer coated on a glass (D263) substrate that had been exposed to 250 mJ of linearly polarized light. The substrate was then heated in an oven at 100°C for 5 minutes and cooled to room temperature. The coated LCP layer was then photopolymerized by irradiation with UV light using a mercury lamp under N2 atmosphere at room temperature for about 2 minutes to fix the orientation state of the liquid crystal.
[0235] Example 33: Polarizing Film Properties
[0236] The dichroic ratio (DR) of absorbance can define the polarization performance of the polarizing film. DR is a material property and therefore it is independent of the thickness of the polarizer. The DR of absorbance can be measured by polarization spectroscopy and is defined as follows:
[0237] DR=Log(1 / T 垂直 ) / (Log(1 / T 平行 ))
[0238] T 垂直 It is the transmittance of light entering perpendicular to the transmission axis of the polarizing film. 平行 is the transmittance of light entering parallel to the transmission axis of the polarizing film. The transmittance T of Examples 28 to 32 垂直 and T 平行 The λ values were measured using an AxoScan polarimeter and they were used to determine the dichroic ratio (DR) at wavelengths of 450 nm, 550 nm, 650 nm.
[0239] The thickness of the polarizing films of Examples 28 to 32 was determined by an Alpha-Step stylus profilometer.
[0240] The results of thickness and DR of the polarizing films of Examples 28 to 32 are summarized in Table 3.
[0241]
[0242] Table 3
[0243] It can be said that when the dichroic ratio is high, the polarizing film is more effective. By using the composition of the present invention, a polarizing film with a high dichroic ratio can be obtained. In fact, the polarizing film made of compound 15 and compound 22K of the present invention exhibits a dichroic ratio higher than 13, while the DR of the polarizing film of comparative example 3 and comparative example 4 has a maximum DR of 10.2.
Claims
1. Compounds of formula (I) in G 1 and G 2 independently represent a polymerizable mesogenic residue, wherein the polymerizable mesogenic residue G 1 and G 2 Each independently represented by a group of formula III in D is selected from 1,4-naphthalenediyl, 2,6-naphthalenediyl and 1,5-naphthalenediyl; E is selected from optionally substituted 1,4-phenylene, pyridine-2,5-diyl, pyrimidine-2,5-diyl, trans-1,4-cyclohexylene, trans-1,4-cyclohexane, trans-1,3-dioxane-2,5-diyl, 1,4-naphthalenediyl, 2,6-naphthalenediyl and 1,5-naphthalenediyl; m is 0, Z 4 and Z 5 are independently selected from a single bond, -COO-, -OOC- and -OCOO-; Z 6 Representative formula -(CH2) q X-, wherein q is an integer ranging from 1 to 18, and X is as defined below, and one or two non-adjacent -CH2- groups may optionally be replaced by -CH=CH-, or one or two -CH2- groups may be replaced by one or two additional linking groups X, with the proviso that the group Z 6 Does not contain two adjacent heteroatoms; R 2 is selected from CH2=CW-COO-, wherein W represents H or a methyl group, Ar represents phenyl; w is 1 or 2; X is selected from -O-, -COO-, -OOC- and -OCOO-; Sp represents the formula -(CH2) p -, wherein p is an integer from 1 to 12; or one or two -CH2- groups are optionally replaced by one or two groups selected from -O-, -CO-, -COO-, -OOC-, -OCOO-, with the proviso that the spacer group does not contain two adjacent heteroatoms; and M represents an achiral group of formula (II) in A and B represent 1,4-phenylene; C is selected from 1,4-phenylene and naphthalene diyl; n 1 and n 2 is 0 or 1, with the proviso that if C is 1,4-phenylene, then n 1 is 0 and n 2 is 1, or if C is naphthalene diyl, then n 1 and n 2 is 0; Z 1 is selected from -O-, -COO-, -OOC-, -OCOO- and a single bond; Z 2 and Z 3 are independently selected from -COO-, -OOC-, -CH2CH2-, -CH2O-, -OCH2-, -CH=CH-, -C≡C-, and a single bond; and R 1 is selected from -CN and -R, wherein R is selected from hydrogen, achiral C 1-8 Alkyl group.
2. A compound according to claim 1, wherein the group Z 2 and Z 3 It is a single bond.
3. An LCP mixture comprising a compound of formula (I) according to claim 1 or 2.
4. An LCP network comprising a compound according to claim 1 or 2 or a mixture according to claim 3 in crosslinked or polymerized form.
5. Use of a compound according to claim 1 or 2 or a mixture according to claim 3 for producing an optical or optoelectronic device.
6. An optical or optoelectronic device comprising a compound according to claim 1 or 2, a mixture according to claim 3 or a network according to claim 4.
Citation Information
Patent Citations
Optical component, orientation layer, and layerable polymerisable mixture
EP1090325A1
Photochemically polymerizable liquid crystals
US5593617A
Optically active smectic photo-cross-linkable liquid crystals
US5650534A
Chromophore-containing photo cross-linkable liquid crystals
US5707544A
Process for coating and printing substrates
US5798147A