Composite copper parts
By forming a metal layer other than copper on the surface of the copper foil, the problem that it is difficult to improve mechanical adhesion, acid resistance and heat resistance at the same time by treating the oxide layer, and the efficient adhesion and durability of composite copper components are achieved. in the manufacturing of electronic components.
Patent Information
- Application Number
- CN202080027104.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-09
- Filing Date
- 2020-05-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-05-07
AI Technical Summary
The oxide layer treatment on the surface of the existing copper foil is difficult to improve mechanical adhesion, acid resistance and heat resistance at the same time, and the adhesion of the plated cover is not sufficient to cope with the transmission requirements under high density and high frequency bands.
By forming a metal layer other than copper on the surface of the copper foil, metal atoms and oxygen atoms are detected by energy dispersion X-ray analysis method, X-ray photoelectron spectroscopy and continuous electrochemical reduction method to form a composite copper component with fine convex parts. Enhance the acid resistance and heat resistance of the oxide layer.
It realizes excellent peel strength, acid resistance and heat resistance of composite copper components, is suitable for the manufacturing of electronic components, and improves adhesion and durability with resin.
Smart Images

Figure BDA0003292558630000111 
Figure BDA0003292558630000131 
Figure HDA0003292558640000011
Abstract
Description
Technical Field
[0001] The invention relates to a composite copper component. Background Art
[0002] The copper foil used for printed circuit boards requires adhesion to resin. In order to improve the adhesion, a method of roughening the surface of the copper foil by etching, etc. is adopted to improve the mechanical adhesion caused by the so-called anchoring effect. However, from the perspective of high density of printed circuit boards and transmission loss under high frequency bands, the flattening of the copper foil surface is required. In order to meet such opposite requirements, a copper surface treatment method (International Publication No. 2014 / 126193) for performing oxidation processes and reduction processes has been developed. According to its description, the copper foil is pre-treated, and after oxidizing the copper foil surface by immersing it in a reagent containing an oxidant and forming the concave and convex of copper oxide, it is immersed in a reagent containing a reducing agent to reduce the copper oxide, thereby adjusting the concave and convex of the surface and trimming the roughness of the surface. In addition, as a method for improving the adhesion of copper foil in the treatment of oxidation and reduction, a method of adding surfactant molecules in the oxidation process (Japanese Patent Publication No. 2013-534054), or a method of forming a protective film on the surface of the copper foil using aminothiazole compounds after the reduction process (Japanese Patent Publication No. 8-97559) has been developed. A method of roughening the surface of a copper conductor pattern on an insulating substrate and forming a plated film having discretely distributed metal particles on the surface formed with a copper oxide layer by chemical plating has also been developed (Japanese Patent Publication No. 2000-151096).
[0003] It is generally believed that in addition to mechanical bonding, 1) physical bonding due to intermolecular forces between the resin and the metal and 2) chemical bonding due to covalent bonds between the functional groups of the resin and the metal also participate in the bonding between the resin and the metal. For example, there are also reports that the presence of an oxide layer containing cupric oxide and cuprous oxide on the surface of the copper foil has an effect on the affinity with the resin (International Publication No. 2017 / 150043).
[0004] On the other hand, the plating film is required to have a degree of adhesion that can withstand its use and environment and has no practical problems. As a method for this, a method is known to strengthen the metal bond by removing the oxide layer on the metal surface and to disperse the stress by roughening the surface to ensure adhesion ("Adhesion of Plating Film and Its Improvement Method" by Morikawa Mu, Nakaide Takuo, Yokoi Masayuki). Summary of the invention
[0005] Problems to be solved by the invention
[0006] Technical problem to be solved by the invention
[0007] The object of the present invention is to provide a novel composite copper component.
[0008] Technical solutions for solving technical problems
[0009] As a result of intensive research conducted by the inventors of the present invention, a novel composite copper component having excellent peel strength, acid resistance and heat resistance was successfully produced by maintaining an oxide layer containing copper oxide and / or cuprous oxide exposed on the surface and uniformly reinforcing the deficiencies in acid resistance and heat resistance of the oxide layer using a metal layer including metal atoms other than copper formed by plating or the like.
[0010] The present invention includes the following embodiments:
[0011] [1] A composite copper component, wherein a metal layer including other than copper is formed on at least a portion of the surface of the copper component, characterized in that the surface on which the metal layer is formed has fine protrusions, and when using energy dispersive X-ray analysis (EDX) using a transmission electron microscope (TEM), copper atoms and oxygen atoms are detected on the surface on which the metal layer is formed in addition to the metal atoms; preferably, when using the EDX method using a TEM, copper atoms and oxygen atoms are detected on the surface on which the metal layer is formed in any range of 1 nm, 3 nm or 10 nm in diameter in addition to the metal atoms.
[0012] [2] A composite copper component, wherein a metal layer other than copper is formed on at least a portion of the surface of the copper component, characterized in that the surface on which the metal layer is formed has fine protrusions, and when the outermost surface is analyzed by X-ray photoelectron spectroscopy (XPS), copper atoms and oxygen atoms are detected in addition to the metal atoms on the surface on which the metal layer is formed; preferably, when X-ray photoelectron spectroscopy (XPS) is used, copper atoms and oxygen atoms are detected in addition to the metal atoms within any range of 30 μm, 100 μm or 300 μm in diameter on the surface on which the metal layer is formed.
[0013] [3] A composite copper component, wherein a metal layer other than copper is formed on at least a portion of the surface of the copper component, characterized in that the surface on which the metal layer is formed has fine protrusions, and when a continuous electrochemical reduction method (SERA) is used, a spectrum originating from copper oxide is detected on the surface on which the metal layer is formed, in addition to a spectrum originating from the metal atoms; preferably, by the continuous electrochemical reduction method (SERA), a spectrum originating from copper oxide is detected within an arbitrary range of 1.6 mm or 3.2 mm in diameter on the surface on which the metal layer is formed, in addition to a spectrum originating from the metal atoms.
[0014] [4] The composite copper component as described in [1] to [3], wherein the metal other than copper is at least one metal selected from Sn, Ag, Zn, Al, Ti, Bi, Cr, Fe, Co, Ni, Pd, Au and Pt.
[0015] [5] The composite copper component as described in [1] to [4], wherein the average thickness of the metal layer other than copper in the vertical direction is greater than 10 nm and less than 70 nm, preferably greater than 20 nm and less than 50 nm.
[0016] [6] A composite copper component as described in [1] to [5], which has a protrusion containing copper oxide or cuprous oxide; preferably, the height of the protrusion is greater than 10nm and less than 1000nm; further preferably, the height of the protrusion is greater than 50nm and less than 500nm, and more preferably, greater than 100nm and less than 300nm.
[0017] [7] An electronic component produced using the composite copper component described in [1] to [6].
[0018] ==Cross-references to related literature==
[0019] The present invention claims priority based on Japanese patent application No. 2019-089121 filed on May 9, 2019, and the contents of the basic application are incorporated into this specification by reference. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1A This is a diagram showing the measurement site of the EDX analysis of Example 1 in the SEM cross-sectional image.
[0021] Figure 1B It is a graph showing the results of EDX analysis of Example 1, Comparative Example 1, and Comparative Example 2.
[0022] Figure 2 It is a graph showing the results of XPS analysis of Example 1 and Comparative Examples 1 to 3.
[0023] Figure 3 It is a graph showing the results of SERA analysis of Example 1, Comparative Examples 1 to 3, and Ni foil. DETAILED DESCRIPTION
[0024] Hereinafter, preferred embodiments of the present invention will be described in detail using the accompanying drawings, but are not necessarily limited thereto. Among them, through the description of this specification, the purpose, features, advantages and concepts of the present invention are clear to those skilled in the art, and as long as they are skilled in the art, they can easily reproduce the present invention according to the description of this specification. The embodiments of the invention described below and specific examples, etc. represent preferred embodiments of the present invention, and are intended to illustrate or explain, and the present invention is not limited thereto. Those skilled in the art can clearly know that various changes and modifications can be made based on the description of this specification within the intent and scope of the present invention disclosed in this specification.
[0025] ==Composite Copper Parts==
[0026] One embodiment of the present invention is a composite copper component in which a metal layer including metal atoms other than copper is formed on at least a portion of the surface of the copper component. The copper component refers to a material that is a part of the structure and contains Cu as a main component, including copper foil such as electrolytic copper foil, rolled copper foil, and copper foil with a carrier, copper wiring, copper plate, copper lead frame, etc., but is not limited thereto.
[0027] The surface of the copper component contains copper oxide and / or cuprous oxide. When the surface of the composite component is measured by various elemental analysis methods, copper atoms and oxygen atoms other than metal atoms constituting the metal layer, and / or molecules composed of them are detected on the surface. When copper foil is used as a copper component, the thickness of the copper foil is not particularly limited, and is preferably between 0.1 μm and 100 μm, and more preferably between 1 μm and 50 μm. The copper foil may have a metal layer on the surface of the copper foil of the copper foil with a carrier. The type of elemental analysis method is not particularly limited, and examples thereof include energy dispersive X-ray analysis (EDX), X-ray photoelectron spectroscopy (XPS), and continuous electrochemical reduction (SERA). These methods are described below.
[0028] Energy dispersive X-ray analysis is an elemental analysis method that uses characteristic X-rays generated when an object is irradiated with electron beams into a semiconductor detector to study the elements and concentrations that make up the object based on the energy and number of the generated electron:hole pairs. The analysis spot diameter (i.e., the diameter of the cross section when the cylindrical part that can be analyzed is cut so that the cross section becomes a circle) is preferably 1 nm or more and 100 nm or less. Energy dispersive X-ray analysis can be performed using a transmission electron microscope (TEM) or a scanning electron microscope (SEM).
[0029] X-ray photoelectron spectroscopy is a method of irradiating an object with X-rays and capturing the photoelectrons released as the object is ionized. -XPS is a method for energy analysis. Through XPS, the type, amount, chemical bonding state, etc. of elements present on the sample surface (for example, up to a depth of 6 nm) can be studied. The analysis spot diameter (i.e., the diameter of the cross section when the cylindrical part that can be analyzed is cut in a circular manner) is preferably 1 μm or more and 1 mm or less.
[0030] The continuous electrochemical reduction method is a method of making an electrolyte contact with the surface of an object, flowing a small current through the electrolyte, measuring the inherent reduction potential of the material constituting the object, and calculating the thickness and element content of each material by the time required for reduction. The analysis spot diameter (i.e., the diameter of the cross section when the cylindrical part that can be analyzed is cut in a circular manner) is not particularly limited, and is preferably 1 mm or more and 500 mm or less.
[0031] The type of metal constituting the metal layer is not particularly limited as long as it is a metal other than copper, but is preferably at least one metal selected from Sn, Ag, Zn, Al, Ti, Bi, Cr, Fe, Co, Ni, Pd, Au, and Pt. In particular, in order to obtain acid resistance and heat resistance, metals having higher acid resistance and heat resistance than copper, such as Ni, Pd, Au, and Pt, are preferred.
[0032] In the composite copper component, the average thickness of the metal other than copper contained in the metal layer in the vertical direction is not particularly limited, but is preferably 6 nm or more, more preferably 10 nm or more, 14 nm or more, 18 nm or more, or 20 nm or more. However, if it is too thick, copper oxide cannot be detected on the surface where the metal layer is formed, and the peel strength is also reduced, so it is preferably 80 nm or less, more preferably 70 nm or less, or 60 nm or less.
[0033] In addition, the average thickness of the metal other than copper contained in the metal layer in the vertical direction can be calculated by dissolving the metal layer with an acidic solution, measuring the amount of metal by ICP analysis, and dividing the amount by the area of the composite copper part. Alternatively, it can be calculated by dissolving the composite copper part itself and detecting and measuring only the amount of metal forming the metal layer.
[0034] When the average thickness of the metal layer in the vertical direction is thin, the metal layer is not uniform but exists discretely, so metals other than copper cannot be detected in some parts, and the surface is discolored due to oxidation, so discoloration occurs in the heat resistance test. On the other hand, when the average thickness of the metal layer in the vertical direction is thick, the surface unevenness of the composite copper part is buried by leveling, so the strength deteriorates. In addition, when the average thickness in the vertical direction is large, only metals other than copper can be detected in some parts.
[0035] A metal layer including metals other than copper can be formed on the surface of a copper part by plating. The plating method is not particularly limited, and examples thereof include electroplating, electroless plating, vacuum evaporation, chemical conversion treatment, etc. Since it is preferred to form a uniform and thin plating layer, electroplating is preferred. When electroplating is performed on the surface of a copper foil after oxidation treatment, the charge is first used to reduce the copper oxide (CuO) on the surface to cuprous oxide (Cu2O) or pure copper. Therefore, there is a time lag until plating, and then the metal forming the metal layer begins to precipitate. The amount of charge varies depending on the type of plating solution and the amount of copper oxide. For example, when Ni is plated on a copper part, in order to make its thickness within the preferred range, it is preferred to apply 15C / dm per unit area of the copper part to be electroplated. 2 Above~75C / dm 2 The charge is preferably 25C / dm 2 Above~65C / dm 2 the following.
[0036] In one embodiment of the present invention, a composite copper component having a metal layer formed thereon including a metal other than copper has fine protrusions on its surface. Such fine protrusions are formed by forming a film on the protrusions with a metal other than copper, and the protrusions are fine protrusions generated by roughening the surface of the copper component.
[0037] The roughening treatment includes a process of forming fine convex portions on the surface of the copper component. The roughening treatment may include a process of forming fine convex portions containing copper oxide (CuO) on the surface of the copper foil using an oxidizing agent. Furthermore, the process may include dissolving the oxidized copper foil surface using a dissolving agent to adjust the convex portions on the oxidized copper component surface. In addition, the process may include forming cuprous oxide (Cu2O) by performing a reduction treatment using a reducing agent to adjust the convex portions on the oxidized copper foil surface.
[0038] The average height of the convex portion on the surface of the composite component where the metal layer is formed is preferably 10 nm or more, more preferably 50 nm or more, and further preferably 100 nm or more, and preferably 1000 nm or less, more preferably 500 nm or less, and further preferably 300 nm or less. The height of the convex portion can be, for example, the distance between the midpoint of a line segment connecting the minimum points of adjacent concave portions sandwiching the convex portion and the maximum point of the convex portion located between the concave portions in a scanning electron microscope (SEM) image of a cross section of a composite copper foil produced by a focused ion beam (FIB).
[0039] ==Method for manufacturing composite copper component==
[0040] One embodiment of the present invention is a method for producing a composite copper part, including a first step of oxidizing a surface of a copper part, and a second step of plating the oxidized copper surface.
[0041] First, in the first step, an oxidant is used to oxidize the surface of the copper part to form a layer of copper oxide and to form convex portions on the surface. Copper oxides include CuO and Cu2O. Before the oxidation step, although it is not necessary to perform a roughening treatment step such as etching, it can be performed. In addition, before the oxidation treatment, a degreasing treatment or an acid cleaning to remove the natural oxide film for uniform treatment can be performed, or an alkali treatment to prevent the acid from being brought into the oxidation step can be performed after the acid cleaning. The method of the alkali treatment is not particularly limited, and a treatment of 30 to 50°C for about 0.5 to 2 minutes can be performed using an alkali aqueous solution preferably of 0.1 to 10 g / L, more preferably 1 to 2 g / L, such as an aqueous sodium hydroxide solution.
[0042] The oxidant is not particularly limited, and for example, aqueous solutions of sodium chlorite, sodium hypochlorite, potassium chlorate, potassium perchlorate, etc. can be used. Various additives (for example, phosphates such as trisodium phosphate dodecahydrate) and surfactant molecules can also be added to the oxidant. Examples of the surfactant molecule include porphyrin, porphyrin macrocycle, expanded porphyrin, ring-contracted porphyrin, linear porphyrin polymer, porphyrin sandwich coordination compound, porphyrin array (porphyrin array), silane, tetraorgano-silane, aminoethyl-aminopropyl-trimethoxysilane, (3-aminopropyl)trimethoxysilane, 1-[3-(trimethoxysilyl)propyl]urea (l-[3-(Trimethoxysilyl)propyl]urea), (3-aminopropyl)triethoxysilane, ((3-glycidyloxypropyl)trimethoxysilane), (3-chloropropyl)trimethoxysilane, (3-glycidyloxypropyl)trimethoxysilane, dimethyldichlorosilane, 3-(trimethoxysilyl)propylmethacrylate, ethyltriacetoxysilane, triethoxy(isobutyl)silane, triethoxy(octyl)silane, tri(2-methoxyethoxy)(vinyl)silane, chlorotrimethylsilane, methyltrichlorosilane, tetrachlorosilane, tetraethoxysilane, phenyltrimethoxysilane, chlorotriethoxysilane, vinyl-trimethoxysilane, amines, sugars, etc.
[0043] The oxidation reaction conditions are not particularly limited, but the liquid temperature of the oxidizing agent is preferably 40 to 95° C., more preferably 45 to 80° C. The reaction time is preferably 0.5 to 30 minutes, more preferably 1 to 10 minutes.
[0044] In the first step, the oxidized surface of the copper member may be dissolved using a dissolving agent to adjust the convex portions on the surface of the copper member.
[0045] The dissolving agent used in this step is not particularly limited, but is preferably a chelating agent, particularly a biodegradable chelating agent, examples of which include ethylenediaminetetraacetic acid, diethanolglycine, tetrasodium L-glutamate diacetate, ethylenediamine-N,N'-disuccinic acid, sodium 3-hydroxy-2,2'-iminodisuccinate, trisodium methylglycine diacetate, tetrasodium aspartic acid diacetate, disodium N-(2-hydroxyethyl)iminodiacetate, and sodium gluconate.
[0046] The pH of the dissolving agent is not particularly limited, but is preferably alkaline, more preferably pH 8 to 10.5, further preferably pH 9.0 to 10.5, and further preferably pH 9.8 to 10.2.
[0047] In the first step, the number and height of the protrusions may be adjusted by reducing the copper oxide formed on the copper member using a chemical containing a reducing agent (a reducing chemical).
[0048] As the reducing agent, DMAB (dimethylamine borane), diborane, sodium borohydride, hydrazine, etc. can be used. The reducing chemical solution is a liquid containing a reducing agent, an alkaline compound (sodium hydroxide, potassium hydroxide, etc.) and a solvent (pure water, etc.).
[0049] Next, in the second step, the surface of the copper part formed with fine protrusions is plated with a metal other than copper to manufacture a composite copper part. The plating method can adopt a known technology. For example, as a metal other than copper, Sn, Ag, Zn, Al, Ti, Bi, Cr, Fe, Co, Ni, Pd, Au, Pt or various alloys can be used. The plating process is not particularly limited, and the plating can be carried out by electroplating, electroless plating, vacuum evaporation, chemical conversion treatment, etc. Since it is preferred to form a uniform and thin plating layer, electroplating is preferred. At present, in order to form concave-convex on the copper surface of the copper part by copper plating and then impart heat resistance and chemical resistance, the plating treatment is carried out in layers, but in the present invention, the copper oxide formed by oxidation treatment is included, and the copper surface of the copper part having uniform and fine concave-convex parts is plated.
[0050] In the case of nickel plating, pure nickel plating and nickel alloy plating are preferred during electroplating. Pure nickel and nickel alloy plating include pure nickel, Ni-Cu alloy, Ni-Cr alloy, Ni-Co alloy, Ni-Zn alloy, Ni-Mn alloy, Ni-Pb alloy, Ni-P alloy, etc.
[0051] As the plating ion supply agent, for example, nickel sulfate, nickel sulfamate, nickel chloride, nickel bromide, zinc oxide, zinc chloride, dichlorodiammine palladium, iron sulfate, iron chloride, anhydrous chromic acid, chromium chloride, sodium chromium sulfate, copper sulfate, copper pyrophosphate, cobalt sulfate, manganese sulfate, sodium hypophosphite, etc. can be used.
[0052] As other additives including pH buffers, brighteners, etc., for example, boric acid, nickel acetate, citric acid, sodium citrate, ammonium citrate, potassium formate, malic acid, sodium malate, sodium hydroxide, potassium hydroxide, sodium carbonate, ammonium chloride, sodium cyanide, potassium sodium tartrate, potassium thiocyanate, sulfuric acid, hydrochloric acid, potassium chloride, ammonium sulfate, ammonium chloride, potassium sulfate, sodium sulfate, sodium thiocyanate, sodium thiosulfate, potassium bromate, potassium pyrophosphate, ethylenediamine, nickel ammonium sulfate, sodium thiosulfate, fluorosilicic acid, sodium fluorosilicic acid, strontium sulfate, cresolsulfonic acid, β-naphthol, o-sulfonylbenzoimide, 1,3,6-naphthalenetrisulfonic acid, naphthalene (di, tri), sodium sulfonate, sulfonamide, sulfinic acid, 1-4-butynediol, coumarin, sodium lauryl sulfate.
[0053] When nickel plating, the bath composition preferably contains nickel sulfate (100 g / L to 350 g / L), nickel sulfamate (100 g / L to 600 g / L), nickel chloride (0 g / L to 300 g / L) and mixtures thereof, and may contain sodium citrate (0 g / L to 100 g / L) and boric acid (0 g / L to 60 g / L) as additives.
[0054] In the case of electroless nickel plating, it is preferred to perform a treatment using a catalyst. As a catalyst, iron, cobalt, nickel, ruthenium, rhodium, palladium, osmium, iridium and their salts are preferably used. By performing a treatment using a catalyst, a uniform metal layer in which particles do not exist in a dotted form can be obtained. Thus, the heat resistance of the composite copper foil is improved. In the case of electroless nickel plating, as a reducing agent, it is preferred to use a reducing agent in which copper and copper oxide do not have catalytic activity. As a reducing agent in which copper and copper oxide do not have catalytic activity, hypophosphites such as sodium hypophosphite can be cited.
[0055] In conventional copper parts, the copper surface is generally plated with copper in the first stage to form unevenness, and then a second stage of plating is performed in layers using a metal other than copper in order to impart heat resistance or chemical resistance. In the first stage of plating, plating is performed on pure copper to obtain uniformity, and the plating is then formed into layers by the second stage of plating. Therefore, it is impossible to detect copper atoms and oxygen atoms or molecules composed of these in addition to the plated metal atoms at any position within a few nm. In the present invention, by performing the first and second steps on the copper part, plating is performed on the surface of the copper part that is uniform and contains fine copper oxide, and the thickness of the plating is adjusted, thereby being able to manufacture a composite copper foil having the following characteristics, that is, on the surface of the composite copper foil, copper atoms and oxygen atoms and / or molecules composed of these can be detected in addition to the metal atoms used for plating.
[0056] The composite copper foil produced through these steps may be subjected to a coupling treatment using a silane coupling agent or the like, or a rust-proofing treatment using a benzotriazole or the like.
[0057] ==How to use composite copper parts==
[0058] The composite copper member of the present invention can be used in electronic parts such as copper foil used for printed wiring boards, copper wires for wiring on substrates, and copper foil for negative electrode current collectors of LIBs.
[0059] For example, the composite copper foil of the present invention can be bonded to a resin in a layered form to produce a laminate for use in manufacturing a printed circuit board. The type of resin is not particularly limited, but is preferably polyphenylene ether, epoxy, PPO, PBO, PTFE, LCP or TPPI.
[0060] In addition, by using the composite copper foil of the present invention for the negative electrode collector of LIB, the adhesion between the copper foil and the negative electrode material can be improved, thereby obtaining a good lithium ion battery with small capacity degradation. The negative electrode collector for lithium ion batteries can be manufactured by a known method. For example, a negative electrode material containing a carbon-based active material is prepared and dispersed in a solvent or water to form an active material slurry. After the active material slurry is applied to the copper foil, it is dried to evaporate the solvent or water. Then, pressurized, and after drying again, the negative electrode collector is formed into a desired shape. In addition, the negative electrode material may contain silicon or silicon compounds, germanium, tin, lead, etc., whose theoretical capacity is larger than that of the carbon-based active material. In addition, as an electrolyte, it can be not only an organic electrolyte in which a lithium salt is dissolved in an organic solvent, but also an electrolyte using a polymer composed of polyethylene oxide or polyvinylidene fluoride, etc. The composite copper foil of the present invention can be used not only for lithium ion batteries, but also for lithium ion polymer batteries.
[0061] Example
[0062] <1. Manufacturing of composite copper foil>
[0063] In Example 1 and Comparative Examples 1 to 3, the shiny side (shiny side, which is a flatter side than the opposite side) of copper foil (DR-WS, thickness: 18 μm) manufactured by Furukawa Electric Co., Ltd. was used.
[0064] (1) Pretreatment
[0065] [Alkali degreasing treatment]
[0066] The copper foil was immersed in a 40 g / L sodium hydroxide aqueous solution at a liquid temperature of 50° C. for 1 minute, and then washed with water.
[0067] [Acid cleaning treatment]
[0068] The copper foil subjected to the alkali degreasing treatment was immersed in a 10 wt % sulfuric acid aqueous solution at a liquid temperature of 25° C. for 2 minutes, and then washed with water.
[0069] [Pre-impregnation treatment]
[0070] The copper foil after the acid cleaning treatment was immersed in a pre-dip agent having a liquid temperature of 40° C. and a sodium hydroxide (NaOH) content of 1.2 g / L for 1 minute.
[0071] (2) Oxidation treatment
[0072] The copper foil after the alkali treatment was oxidized in an aqueous oxidation treatment solution (NaClO2 60 g / L; NaOH 9 g / L) at 73° C. for 2 minutes. In Comparative Example 1, the copper foil was washed with water after the oxidation treatment.
[0073] (3) Reduction treatment
[0074] In Comparative Example 2, after the oxidation treatment, the sample was immersed in a reducing agent (5 g / L of dimethylamine borane and 5 g / L of sodium hydroxide) at room temperature for 1 minute to perform a reduction treatment.
[0075] (4) Plating treatment
[0076] In Example 1 and Comparative Example 3, the copper foil after oxidation treatment was plated. Specifically, in Example 1, electroplating was performed on the shiny surface of the copper foil using a nickel plating electrolyte (470 g of nickel sulfamate and 40 g / L of L-boric acid) (at 50 degrees and a current density of 0.5 A / dm 2 ×45 seconds (=22.5C / dm 2 In Comparative Example 3, except for the conditions of electroplating the shiny surface of the copper foil (at 50 degrees, current density 0.5 A / dm 2 The same as in Example 1 except for the time (×100 seconds).
[0077] Regarding Examples and Comparative Examples, a plurality of test pieces were prepared under the same conditions.
[0078] <2. Measurement of average thickness of metal layer in vertical direction by ICP>
[0079] 1. Methods
[0080] The test pieces of Example 1 and Comparative Example 3 were dissolved in 12% nitric acid, and the concentration of the metal component in the obtained liquid was measured using an ICP emission spectrometer 5100SVDV ICP-OES (manufactured by Agilent Technologies). The average thickness of the layered metal layer in the vertical direction was calculated by considering the density of the metal and the surface area of the metal layer.
[0081] 2. Results
[0082] The results are shown in Table 1.
[0083] [Table 1]
[0084]
[0085] <3. Surface analysis using EDX>
[0086] 1. Methods
[0087] The surfaces of the test pieces of Example 1 and Comparative Examples 1 to 3 were subjected to carbon treatment for the purpose of protecting the surfaces from damage caused by the FIB beam. After extracting any part by the FIB / sampling method, the thinned pieces were processed by FIB to a thickness that can be observed by a transmission electron microscope. Multiple measurement fields ( Figure 1A ), and elemental analysis was performed using a scanning electron microscope (HD-2300 (manufactured by Hitachi); accelerating voltage 200 kV; beam diameter 1 nm; irradiation area of 3 nm in diameter; systematic peaks: W, Mo, Ga) equipped with an energy dispersive X-ray analyzer (EDX).
[0088] 2. Results
[0089] The results are shown in Table 1 and Figure 1B . In any measurement point on the surface of the metal layer formed in Example 1, the spectra of nickel, copper and oxygen elements were detected. Since the spectra of each element can be detected, it is proved that the composite layer of Ni, Cu and O is coated in a uniform and non-discrete manner. When there are only two elements, Cu and O, as in Comparative Examples 1 and 2, oxidation is easy to occur, and the color change amount in the heat resistance test is large.
[0090] <4. Surface analysis using XPS>
[0091] 1. Methods
[0092] The outermost surface Narrow analysis of the obtained test pieces of Example 1 and Comparative Examples 1 to 3 was performed by the following steps using Quantera SPM (manufactured by ULVAC-PHI).
[0093] (1)Survey spectrum
[0094] First, the elements were detected under the following conditions.
[0095] X-ray beam diameter: 100μm (25w15kV)
[0096] Pass energy: 280eV, 1eV step
[0097] Line analysis:
[0098] Total times: 6 times
[0099] (2) Narrow spectrum
[0100] For the elements detected in (1), a Narrow Spectrum was acquired under the following conditions, and when the total amount of elements other than N and C among the detected components was set to 100%, the ratio of each detected component was calculated as a quantitative value.
[0101] X-ray beam diameter: 100μm (25w15kV)
[0102] Pass energy: 112eV, 0.1eV step
[0103] Line analysis:
[0104] 2. Results
[0105] The results are shown in Figure 2 and Table 1.
[0106] In Example 1, nickel, copper, and oxygen were detected at any measurement point on the surface where the metal layer was formed. However, in Comparative Example 3, which was subjected to the same nickel plating, since the plating thickness was thicker than that of Example 1, only nickel and oxygen were detected, and copper was not detected, and the three elements were not uniformly covered. This means that nickel was formed in a thick layer, and copper oxide with fine irregularities was completely covered by the nickel layer due to the leveling of the plating, and the fine irregularities could not be maintained, so that adhesion could not be obtained.
[0107] <5. Surface analysis by SERA>
[0108] 1. Methods
[0109] Surface element analysis was performed using QC-100 (manufactured by ECI).
[0110] The following electrolyte solutions were used in the measurement.
[0111] Electrolyte (pH = 0.6 ~ 0.7)
[0112]
[0113] The diameter of the gasket is 0.16 cm. The current density is 90 μA / cm 2 When the above electrolyte solution was used, the potential from -0.4 V to -0.15 V was determined as a peak derived from copper oxide, and the potential from -0.15 V to 0.1 V was determined as a peak derived from Ni. As a control, commercially available nickel foil (thickness 5 μm) was also measured simultaneously.
[0114] However, the peak derived from each element is defined as follows.
[0115] Peak from copper oxide: -0.5V to -0.1V
[0116] Peak from Ni: -0.1V to 0V
[0117] 2. Results
[0118] When there is no Ni as in Comparative Example 1, only the spectrum from copper oxide can be detected, and when Ni is too thick as in Comparative Example 3, only the spectrum from Ni can be detected. In Example 1, spectra from both copper oxide and Ni were detected. The case where both spectra were detected as in Example 1 is the case where only extremely thin Ni exists to the extent that the spectrum from copper oxide can be detected at a predetermined potential.
[0119] <6. Measurement of height and number of convex parts>
[0120] 1. Methods
[0121] Using a confocal scanning electron microscope controller MC-1000A (manufactured by Lasertec Co., Ltd.), the height and number of the protrusions of the test pieces of Example 1 and Comparative Examples 1 to 3 were measured. In the scanning electron microscope (SEM) image, the distance between the midpoint of the line segment connecting the adjacent minimum points sandwiching the protrusion and the maximum point of the protrusion located between the recesses is taken as the height of the protrusion. Using SEM images of 5 independent positions, 3 points are measured for each image, and the average value is calculated and set as the average height of the protrusion. Next, in the 5 SEM images, the number of protrusions with a height of more than 50nm within every 3.8μm is counted, and the average value of the 5 is calculated. When there are undulations in the original copper part, the length when the undulations of the original part are extended into a plane is measured and converted into a length per 3.8μm.
[0122] 2. Results
[0123] Table 1 shows the results of each measurement.
[0124] <7. Determination of peel strength, acid resistance and heat resistance>
[0125] 1. Methods
[0126] The peel strength before and after the acid treatment was measured for the test pieces of Example 1 and Comparative Examples 1 to 3. First, the prepreg (R5670KJ, manufactured by Panasonic Corporation) was laminated to each test piece, and a vacuum high-pressure press was used to heat and press-bond the laminate under the conditions of a press pressure of 2.9 MPa, a temperature of 210°C, and a press time of 120 minutes, thereby obtaining a laminate. For the embodiments and comparative examples, multiple laminates were made under the same conditions. In order to study the tolerance to acid, one laminate was taken as it was (normal state) and the other was immersed in acid solution (after acid resistance test) as a test sample. In addition, the acid solution immersion was carried out by immersing the laminate in 4N HCl at 60°C for 90 minutes. For these test samples, the peel strength (kgf / cm) was measured by a 90° peel test (Japanese Industrial Standard (JIS) C5016).
[0127] In addition, the heat resistance of the test pieces of Example 1 and Comparative Examples 1 to 3 was examined by the color change caused by heating. Specifically, the color difference (L * 、a * , b * ) and then treated in an oven at 225°C for 30 minutes, and the color difference of the test piece after heat treatment was measured. ΔE was calculated from the obtained value according to the following formula: * ab.
[0128] ΔE * ab=[(ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ] 1 / 2
[0129] 2. Results
[0130] The results are shown in Table 1. The composite copper foil of Example 1 is superior to the copper foils of Comparative Examples 1 to 3 in heat resistance and acid resistance. Comparative Example 1 is inferior in acid resistance and heat resistance. Comparative Examples 2 and 3 are acid resistant but inferior in heat resistance. On the other hand, the composite copper foil of Example 1 is superior in peel strength, heat resistance, and acid resistance.
[0131] Thus, the composite copper foil of Example 1 has fine concavoconvexities derived from copper oxide on its surface, and while maintaining the exposure of the oxide layer containing copper oxide and / or cuprous oxide, the oxide layer with poor resistance to heat and acid is uniformly and not discretely coated with a metal other than copper, thereby having excellent peel strength, acid resistance and heat resistance. Therefore, it can be suitably used in electronic components and the like.
[0132] Industrial Applicability
[0133] The present invention can provide a novel composite copper component.
Claims
1. A composite copper component, wherein a metal layer including metal atoms other than copper is formed on at least a portion of the surface of the copper component, characterized in that: The metal layer is a uniform and thin plating layer, The surface of the composite copper member on which the metal layer is formed has fine protrusions. By energy dispersive X-ray analysis (EDX) using a transmission electron microscope (TEM), copper atoms and oxygen atoms were detected in addition to the metal atoms within an arbitrary range of 10 nm in diameter on the surface of the composite copper member.
2. A composite copper component, wherein a metal layer including metal atoms other than copper is formed on at least a portion of the surface of the copper component, characterized in that: The metal layer is a uniform and thin plating layer, The surface of the composite copper member on which the metal layer is formed has fine protrusions. When the outermost surface of the surface of the composite copper member was analyzed by X-ray photoelectron spectroscopy (XPS), copper atoms and oxygen atoms were detected in addition to the metal atoms within any range of 300 μm in diameter on the surface where the metal layer was formed.
3. A composite copper component, wherein a metal layer including metal atoms other than copper is formed on at least a portion of the surface of the copper component, characterized in that: The metal layer is a uniform and thin plating layer, The surface of the composite copper member on which the metal layer is formed has fine protrusions. By a continuous electrochemical reduction method (SERA) method, a spectrum derived from copper oxide is detected on the surface of the composite copper member in addition to a spectrum derived from the metal atoms.
4. The composite copper component according to any one of claims 1 to 3, characterized in that: The metal atom is at least one metal atom selected from Sn, Ag, Zn, Al, Ti, Bi, Cr, Fe, Co, Ni, Pd, Au and Pt.
5. The composite copper component according to any one of claims 1 to 3, characterized in that: The average thickness of the metal layer in a vertical direction is greater than or equal to 10 nm and less than or equal to 70 nm.
6. The composite copper component according to any one of claims 1 to 3, characterized in that: The height of the fine protrusions is not less than 10 nm and not more than 1000 nm.
7. An electronic component produced using the composite copper component according to any one of claims 1 to 6.