Composition for electron transport layer and preparation method and application thereof

By using a mixture of ZnCaO and ZnO as the electron transport layer, the problem of electron and hole transport balance in quantum dot electroluminescent devices is solved, and the efficiency and performance of the device are improved.

CN113707821BActive Publication Date: 2024-10-25上饶小姆软件中心(个人独资)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110771996.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-07-08
Publication Date
2024-10-25
Estimated Expiration
2041-07-08

AI Technical Summary

Technical Problem

The conversion efficiency of electronic light-emitting devices of existing quantum dot electroluminescent devices is low, mainly because the problem of electron and hole transport balance has not been effectively solved, especially the stability of the ZnO electron transport layer and the defective state causing spontaneous electron transfer that hinders the device. Improvement of efficiency.

Method used

A mixture of ZnCaO and ZnO is used as the electron transport layer. Ca doping is used to raise the conduction band, prevent electrons from transferring from quantum dots to the transport layer, achieve electron/hole injection balance, maintain the electrical neutrality of the quantum dot film, and promote electron transfer. Fast transfer.

Benefits of technology

It improves the charge balance and efficiency of quantum dot devices, realizes rapid electron transmission, and improves the overall performance of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0003153979830000011
    Figure HDA0003153979830000011
Patent Text Reader

Abstract

The present invention discloses a composition for an electron transport layer, a preparation method and an application thereof, wherein the composition comprises: ZnO; ZnCaO; and a first solvent. The present invention uses a mixture of ZnCaO and ZnO as an electron transport layer, which can effectively prevent the transfer of charges from quantum dots to the electron transport layer compared to an electron transport layer of pure ZnO or pure ZnCaO, is conducive to the transmission of electrons and maintains the electrical neutrality of the quantum dot film, so that a quantum dot device using the composition has a high charge balance and can also achieve rapid electron transmission, thereby improving the efficiency of the quantum dot device using the composition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of quantum dot electroluminescent devices, and in particular relates to a composition for an electron transport layer and a preparation method and application thereof. Background Art

[0002] Quantum dots have characteristics such as adjustable energy bands. By controlling the size and composition of quantum dots, the entire visible light region, even the near-infrared region, can be covered. Quantum dot-based quantum dot light-emitting diode materials have unique photoelectric properties of quantum dots and are the most promising lighting and display technology after LCD and OLED. In particular, the new generation of core display technology based on quantum dots has gradually begun to advance from the laboratory to commercialization.

[0003] There are still many technical challenges to be solved for the full commercialization of quantum dot electroluminescent devices, one of which is how to improve the efficiency of electroluminescent devices. At present, the quantum yields of red, green and blue quantum dots are already very high, but the device conversion efficiency of electronic light-emitting devices based on these quantum dots is much lower than the quantum yield of their quantum dots. The main reason is that the problem of electron and hole transport balance inside the device has not been effectively solved.

[0004] The existing technology for the electron transport layer of quantum dot light-emitting diodes has a more mainstream method of using metal oxides such as ZnO with a large electron mobility as the electron transport layer material. However, the stability of the ZnO electron transport layer is relatively low, and there are many surface defect states of ZnO. When ZnO is in direct contact with the quantum dot layer, the spontaneous transfer of electrons between the quantum dots and the electron transport layer ZnO hinders further improvement of the device efficiency. Therefore, the existing technology needs to be improved. Summary of the invention

[0005] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to propose a composition for an electron transport layer, a preparation method and an application thereof. The present invention uses a mixture of ZnCaO and ZnO as an electron transport layer. Compared with the electron transport layer of pure ZnO or pure ZnCaO, it can effectively prevent the transfer of charge from quantum dots to the electron transport layer, which is beneficial to the transmission of electrons and maintains the electrical neutrality of the quantum dot film, so that the quantum dot device using the composition has a high charge balance while also achieving rapid transmission of electrons, thereby improving the efficiency of the quantum dot device using the composition.

[0006] In one aspect of the present invention, the present invention provides a composition for an electron transport layer. According to an embodiment of the present invention, the composition for an electron transport layer comprises:

[0007] ZnO;

[0008] ZnCaO; and

[0009] The first solvent.

[0010] According to the composition for the electron transport layer of the embodiment of the present invention, Ca-doped ZnO can effectively widen the band gap of ZnO by raising the conduction band. Since the difference between the quantum dots and the conduction band of ZnO is small, electrons can easily undergo spontaneous charge transfer at the interface between the quantum dots and ZnO. By adding ZnCaO, ZnCaO with a higher conduction band can hinder the injection of electrons into the quantum dot layer, thereby easily achieving electron / hole injection balance. Using a mixture of ZnCaO and ZnO as the electron transport layer, compared with the electron transport layer of pure ZnO or pure ZnCaO, it can effectively prevent electrons from transferring from quantum dots to the electron transport layer, which is beneficial to the transmission of electrons in the device and maintains the electrical neutrality of the quantum dot film, so that the quantum dot device using the composition has a high charge balance while also achieving rapid transmission of electrons in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0011] In addition, the composition for the electron transport layer according to the above embodiment of the present invention may also have the following additional technical features:

[0012] In some embodiments of the present invention, the molar ratio of the ZnO to the ZnCaO is 1:(1-10).

[0013] In some embodiments of the present invention, the concentration of ZnO in the composition is (0.1-100) mg / mL, preferably (15-30) mg / mL.

[0014] In some embodiments of the present invention, the concentration of ZnCaO in the composition is (0.1-100) mg / mL, preferably (15-30) mg / mL.

[0015] In some embodiments of the present invention, the first solvent is selected from at least one of methanol, ethanol, propanol, butanol, petroleum ether, ethyl ether, n-butyl ether, octane, hexane, heptane, acetone, ethyl acetate, toluene, chlorobenzene, chloroform, dichloromethane and chlorobenzene.

[0016] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned composition for an electron transport layer. According to an embodiment of the present invention, the method comprises:

[0017] (1) Preparation of ZnO;

[0018] (2) mixing the calcium-containing inorganic substance, the zinc-containing inorganic substance, the second solvent and the base, and reacting them to obtain ZnCaO;

[0019] (3) The ZnO, the ZnCaO and a first solvent are mixed to obtain a composition for an electron transport layer.

[0020] According to the method for preparing the above-mentioned composition for electron transport layer according to the embodiment of the present invention, Ca-doped ZnO can effectively widen the band gap of ZnO by raising the conduction band. Since the difference between the conduction band of quantum dots and ZnO is small, electrons can easily undergo spontaneous charge transfer at the interface of quantum dots and ZnO. By adding ZnCaO, ZnCaO with a higher conduction band can hinder the injection of electrons into the quantum dot layer, thereby easily achieving electron / hole injection balance. Using a mixture of ZnCaO and ZnO as the electron transport layer, compared with the electron transport layer of pure ZnO or pure ZnCaO, it can effectively prevent electrons from transferring from quantum dots to the electron transport layer, which is beneficial to the transmission of electrons in the device and maintains the electrical neutrality of the quantum dot film, so that the quantum dot device using the composition has a high charge balance while also achieving rapid transmission of electrons in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0021] In addition, the method for preparing the composition for an electron transport layer according to the above embodiment of the present invention may also have the following additional technical features:

[0022] In some embodiments of the present invention, in step (1), the specific process of preparing ZnO is as follows: reacting an alkali with a zinc salt solution to obtain ZnO.

[0023] In some embodiments of the present invention, in step (1), the base is selected from at least one of tetramethylammonium hydroxide, potassium hydroxide, sodium hydroxide and lithium hydroxide.

[0024] In some embodiments of the present invention, in step (1), the zinc salt in the zinc salt solution is selected from at least one of zinc acetate, zinc nitrate and zinc chloride.

[0025] In some embodiments of the present invention, in step (1), the solvent in the zinc salt solution is selected from at least one of dimethyl sulfoxide, ethanol and ethyl acetate.

[0026] In some embodiments of the present invention, in step (1), the Zn in the zinc salt solution 2+ With the OH in the base - The molar ratio is 1:(0.1-10).

[0027] In some embodiments of the present invention, in step (1), the Zn in the zinc salt solution 2+ The concentration is (0.1-100) mg / mL.

[0028] In some embodiments of the present invention, in step (2), the molar ratio of the calcium-containing inorganic substance to the zinc-containing inorganic substance is 1:(0.01-100), preferably 1:(0.1-10).

[0029] In some embodiments of the present invention, in step (2), the calcium-containing inorganic substance reacts with OH in the base. - The molar ratio is 1:(2-10).

[0030] In some embodiments of the present invention, in step (2), the calcium-containing inorganic substance is selected from at least one of calcium nitrate, calcium fluoride, calcium chloride, calcium bromide, calcium iodide and calcium sulfate.

[0031] In some embodiments of the present invention, in step (2), the zinc-containing inorganic substance is selected from at least one of zinc nitrate, zinc fluoride, zinc chloride, zinc bromide, zinc iodide and zinc sulfate.

[0032] In some embodiments of the present invention, in step (2), the second solvent is selected from at least one of methanol, ethanol, propanol, butanol and deionized water.

[0033] In some embodiments of the present invention, in step (2), the base is selected from at least one of sodium hydroxide, magnesium hydroxide and potassium hydroxide.

[0034] In the third aspect of the present invention, the present invention provides an electron transport layer. According to an embodiment of the present invention, the electron transport layer is prepared by solution spin coating using the composition for the electron transport layer or the composition for the electron transport layer prepared by the above method. Thus, using a mixture of ZnCaO and ZnO as the electron transport layer can effectively prevent the transfer of charges from quantum dots to the electron transport layer compared to the electron transport layer of pure ZnO or pure ZnCaO, thereby achieving electron / hole injection balance.

[0035] In a fourth aspect of the present invention, the present invention provides a quantum dot light-emitting device. According to an embodiment of the present invention, the quantum dot light-emitting device has an electron transport layer as described above. As a result, the quantum dot device using the composition has a high charge balance and can also achieve rapid electron transport in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0036] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description, or will be learned through practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0038] Figure 1 Schematic diagram of the structure of a quantum dot light-emitting device according to an embodiment of the present invention. DETAILED DESCRIPTION

[0039] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.

[0040] In one aspect of the present invention, the present invention proposes a composition for an electron transport layer. According to an embodiment of the present invention, the composition for an electron transport layer includes: ZnO; ZnCaO; and a first solvent. Thus, Ca-doped ZnO can effectively widen the band gap of ZnO by raising the conduction band. Since the difference between the quantum dots and the ZnO conduction band is small, electrons can easily undergo spontaneous charge transfer at the interface between the quantum dots and ZnO. By adding ZnCaO, ZnCaO with a higher conduction band can hinder the injection of electrons into the quantum dot layer, thereby easily achieving electron / hole injection balance. Using a mixture of ZnCaO and ZnO as an electron transport layer, compared with an electron transport layer of pure ZnO or pure ZnCaO, it can effectively prevent the transfer of charges from quantum dots to the electron transport layer, which is beneficial to the transmission of electrons in the device and maintains the electrical neutrality of the quantum dot film, so that the quantum dot device using the composition has a high charge balance while also achieving rapid transmission of electrons in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0041] According to a specific embodiment of the present invention, the molar ratio of the ZnO to the ZnCaO is 1:(1-10), such as 1:1, 1:3, 1:5, 1:7, 1:10, etc. Thus, within this ratio range, while maintaining faster electron transmission, the electrical neutrality of the film is also well maintained. The inventors found that if the content of ZnCaO is too little, it will cause the ability to hinder electron injection into the quantum dot layer to be weak, and more electrons will be spontaneously transferred from the electron transport layer to the quantum dot light-emitting layer. The quantum dot layer is difficult to maintain electrical neutrality, and the electron and hole transmission is unbalanced, thereby affecting the efficiency of the device; if the content of ZnCaO is too much, because the electron transmission rate of ZnCaO is lower than that of ZnO, it will cause the electron transmission rate to be too low, which will also affect the efficiency of the device.

[0042] According to another specific embodiment of the present invention, the concentration of ZnO in the composition is (0.1-100) mg / mL (e.g., 0.1 mg / mL, 10 mg / mL, 20 mg / mL, 40 mg / mL, 60 mg / mL, 80 mg / mL, 100 mg / mL, etc.), preferably (15-30) mg / mL, which is further conducive to the transfer of electrons. The inventors have found that if the concentration of ZnO in the composition is too high or too low, it is not conducive to the transfer of electrons. If the concentration is too high, it will cause the electron transfer to be too fast, and if the concentration is too low, it will cause the electron transfer to be too slow.

[0043] According to another specific embodiment of the present invention, the concentration of ZnCaO in the composition is (0.1-100) mg / mL (e.g., 0.1 mg / mL, 10 mg / mL, 20 mg / mL, 40 mg / mL, 60 mg / mL, 80 mg / mL, 100 mg / mL, etc.), preferably (15-30) mg / mL. The inventors found that if the concentration of ZnCaO in the composition is too low, the content of ZnCaO will be too little, thereby causing more electrons to spontaneously transfer from the electron transport layer to the quantum dot light-emitting layer, and the quantum dot layer is difficult to maintain electrical neutrality, and the electron and hole transmission is unbalanced, affecting the efficiency of the device; if the concentration of ZnCaO in the composition is too high, the content of ZnCaO will be too much, because the electron transmission rate of ZnCaO is less than that of ZnO, then the electron transmission rate will be too low, thereby affecting the efficiency of the device.

[0044] In an embodiment of the present invention, the first solvent refers to an organic solvent that can disperse ZnO and ZnCaO and will not decompose ZnO and ZnCaO. The specific type is not particularly limited, and those skilled in the art can choose it at will according to actual conditions. As a preferred solution, the first solvent is selected from at least one of methanol, ethanol, propanol, butanol, petroleum ether, ethyl ether, n-butyl ether, octane, hexane, heptane, acetone, ethyl acetate, toluene, chlorobenzene, chloroform, dichloromethane and chlorobenzene, more preferably ethanol.

[0045] In another aspect of the present invention, the present invention provides a method for preparing the above-mentioned composition for an electron transport layer. According to an embodiment of the present invention, the method comprises:

[0046] S100: Preparation of ZnO

[0047] In this step, the alkali reacts with the zinc salt solution to obtain ZnO, the reaction temperature is room temperature, and the reaction environment is an atmospheric environment. Further, the prepared ZnO is cleaned with a specific reagent, and the specific reagent is selected from at least one of methanol, ethanol, propanol, butanol, petroleum ether, ether, n-butyl ether, octane, hexane, heptane, acetone, ethyl acetate, toluene, chlorobenzene, chloroform, dichloromethane, chlorobenzene, etc., but not limited thereto; among them, ethyl acetate and heptane are preferred.

[0048] In the embodiments of the present invention, the specific type of the above-mentioned base is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a preferred scheme, the base is selected from at least one of tetramethylammonium hydroxide, potassium hydroxide, sodium hydroxide and lithium hydroxide.

[0049] In the embodiments of the present invention, the specific type of the zinc salt in the zinc salt solution is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a preferred embodiment, the zinc salt in the zinc salt solution is selected from at least one of zinc acetate, zinc nitrate and zinc chloride.

[0050] In the embodiments of the present invention, the specific type of the solvent in the zinc salt solution is not particularly limited, and those skilled in the art can select it at will according to actual needs. As a preferred embodiment, the solvent in the zinc salt solution is selected from at least one of dimethyl sulfoxide, ethanol and ethyl acetate.

[0051] According to a specific embodiment of the present invention, Zn in the zinc salt solution 2+ With the OH in the base - The molar ratio is 1:(0.1-10), for example 1:0.1, 1:0.5, 1:1, 1:5, 1:10, etc., thereby being able to effectively control the size ratio.

[0052] According to another specific embodiment of the present invention, Zn in the zinc salt solution 2+ The concentration is (0.1-100) mg / mL (e.g., 0.1 mg / mL, 10 mg / mL, 20 mg / mL, 40 mg / mL, 60 mg / mL, 80 mg / mL, 100 mg / mL, etc.).

[0053] S200: Mixing the calcium-containing inorganic substance, the zinc-containing inorganic substance, the second solvent and the base, and reacting them to obtain ZnCaO

[0054] In this step, calcium-containing inorganic substance, zinc-containing inorganic substance, second solvent and alkali are mixed, reacted, so as to obtain ZnCaO, the reaction temperature is room temperature, and the reaction environment is atmospheric environment. The order in which calcium-containing inorganic substance, zinc-containing inorganic substance, second solvent and alkali are mixed is not particularly limited, and calcium-containing inorganic substance, zinc-containing inorganic substance and second solvent mixture can be added with alkali to mix, or alkali and second solvent mixture can be added with calcium-containing inorganic substance, zinc-containing inorganic substance to mix. Preferably, calcium-containing inorganic substance and zinc-containing inorganic substance are dissolved in an amount of second solvent with a certain molar ratio, a mixed liquid is prepared, and then an amount of alkaline aqueous solution is dripped in the mixed liquid to prepare ZnCaO.

[0055] Furthermore, the prepared ZnCaO is cleaned with a specific reagent, and the specific reagent is selected from at least one of deionized water, methanol, ethanol, propanol, butanol, etc., but not limited thereto; among them, deionized water and ethanol are preferred.

[0056] According to another specific embodiment of the present invention, the molar ratio of the calcium-containing inorganic substance to the zinc-containing inorganic substance is 1:(0.01-100), for example, 1:0.01, 1:0.1, 1:1, 1:10, 1:50, 1:100, preferably 1:(0.1-10), thereby further effectively controlling the doping ratio. The inventors have found that if the content of the calcium-containing inorganic substance is too high, the conduction band of ZnCaO will be too high, which is not conducive to electron transfer. If the content of the calcium-containing inorganic substance is too low, the difference between the conduction bands of ZnCaO and ZnO will be too small, which will not play a role in improving the conduction band.

[0057] According to another specific embodiment of the present invention, the calcium-containing inorganic substance and the OH in the alkali - The molar ratio is 1:(2-10).

[0058] In the embodiments of the present invention, the specific type of the above-mentioned calcium-containing inorganic substance is not particularly limited, and those skilled in the art can choose it at will according to actual conditions. As a preferred scheme, the calcium-containing inorganic substance is selected from at least one of calcium nitrate, calcium fluoride, calcium chloride, calcium bromide, calcium iodide and calcium sulfate.

[0059] In the embodiments of the present invention, the specific type of the above-mentioned zinc-containing inorganic substance is not particularly limited, and those skilled in the art can choose it at will according to actual conditions. As a preferred scheme, the zinc-containing inorganic substance is selected from at least one of zinc nitrate, zinc fluoride, zinc chloride, zinc bromide, zinc iodide and zinc sulfate.

[0060] In an embodiment of the present invention, the specific type of the above-mentioned second solvent is not particularly limited, and those skilled in the art can choose it at will according to actual conditions. As a preferred scheme, the second solvent is selected from at least one of methanol, ethanol, propanol, butanol and deionized water.

[0061] In the embodiments of the present invention, the specific type of the above-mentioned base is not particularly limited, and those skilled in the art can select it at will according to actual conditions. As a preferred scheme, the base is selected from at least one of sodium hydroxide, magnesium hydroxide and potassium hydroxide.

[0062] S300: Mixing the ZnO, the ZnCaO and the first solvent to obtain a composition for an electron transport layer

[0063] In this step, the ZnO, the ZnCaO and the first solvent are mixed to obtain a composition for an electron transport layer, which is used to prepare an electron transport layer. The specific process of mixing the ZnO, the ZnCaO and the first solvent is not particularly limited. ZnO and ZnCaO can be added to the first solvent together for mixing, or ZnO can be first added to part of the first solvent to form a first mixed solution, and then ZnCaO is added to the remaining part of the first solvent to form a second mixed solution, and then the first mixed solution and the second mixed solution are mixed to obtain a composition for an electron transport layer. The latter mixing method is preferred.

[0064] According to the method for preparing the above-mentioned composition for electron transport layer according to the embodiment of the present invention, Ca-doped ZnO can effectively widen the band gap of ZnO by raising the conduction band. Since the difference between the quantum dots and the conduction band of ZnO is small, electrons can easily undergo spontaneous charge transfer at the interface between the quantum dots and ZnO. By adding ZnCaO, ZnCaO with a higher conduction band can hinder the injection of electrons into the quantum dot layer, thereby easily achieving electron / hole injection balance. Using a mixture of ZnCaO and ZnO as the electron transport layer, compared with the electron transport layer of pure ZnO or pure ZnCaO, it can effectively prevent the transfer of charges from quantum dots to the electron transport layer, which is beneficial to the transmission of electrons in the device and maintains the electrical neutrality of the quantum dot film, so that the quantum dot device using the composition has a high charge balance while also achieving rapid transmission of electrons in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0065] In the third aspect of the present invention, the present invention provides an electron transport layer. According to an embodiment of the present invention, the electron transport layer is prepared by solution spin coating using the composition for the electron transport layer or the composition for the electron transport layer prepared by the above method. Thus, using a mixture of ZnCaO and ZnO as the electron transport layer can effectively prevent the transfer of charges from quantum dots to the electron transport layer compared to the electron transport layer of pure ZnO or pure ZnCaO, thereby achieving electron / hole injection balance.

[0066] In a fourth aspect of the present invention, the present invention provides a quantum dot light-emitting device. According to an embodiment of the present invention, the quantum dot light-emitting device has an electron transport layer as described above. As a result, the quantum dot device using the composition has a high charge balance and can also achieve rapid electron transport in the device, thereby improving the efficiency of the quantum dot device using the composition.

[0067] In an embodiment of the present invention, the quantum dots of the above-mentioned quantum dot light-emitting device may include but are not limited to at least one of II-V compounds, II-VI compounds, III-V compounds, III-VI compounds, IV-VI compounds, I-III-VI compounds, II-IV-VI compounds or IV simple substances. As a specific example, the material of the quantum dot light-emitting layer may include but is not limited to ZnSe, ZnS, ZnTe, InP, InAs, CuInS2, AgInS2, C, Si, Ge. Further, the ligands on the surface of the oil-soluble quantum dots include oleic acid (OA), oleylamine (OAm), octylamine, trioctylphosphine (TOP), trioctylphosphine oxide (TOPO), octadecylphosphonic acid (ODPA) and tetradecylphosphonic acid (TDPA), etc., but are not limited thereto.

[0068] In the embodiment of the present invention, the conventional packaging method of the quantum dot light-emitting device is frame glue packaging, that is, the UV glue is not in contact with the electrode (cathode) of the quantum dot light-emitting device. Figure 1 As shown, the quantum dot light-emitting device includes ITO (anode), a hole injection layer, a hole transport layer, a quantum dot light-emitting layer, a ZnCaO:ZnO electron transport layer and a cathode.

[0069] The embodiments of the present invention are described in detail below. It should be noted that the embodiments described below are exemplary and are only used to explain the present invention, and cannot be interpreted as limiting the present invention. In addition, if not explicitly stated, all reagents used in the following embodiments are commercially available, or can be synthesized according to this article or known methods, and the reaction conditions not listed are also easily available to those skilled in the art.

[0070] Example 1

[0071] This embodiment takes PVK and CdSe / ZnS green quantum dots as an example for detailed description:

[0072] 1) Preparation of ZnO

[0073] A 3M tetramethylammonium hydroxide ethanol solution was gradually added dropwise to a 3.8M zinc acetate dimethyl sulfoxide (DMSO) solution at room temperature, and after stirring for 30 minutes, the solution was washed with ethyl acetate and heptane to obtain ZnO.

[0074] Disperse ZnO at a concentration of 20 mg / mL in an ethanol solvent for preparing an electron transport layer. Take ZnO and ethanol to prepare a ZnO electron transport layer mixed solution.

[0075] 2) Preparation of ZnCaO

[0076] A 0.4 M zinc nitrate aqueous solution and a 0.1 M calcium nitrate aqueous solution were mixed, and a 1 M sodium hydroxide aqueous solution was added to the mixed solution and stirred until a milky white solution was formed.

[0077] The precipitate was washed three times with deionized water and ethanol respectively, and after drying, a ZnCaO electron transport layer mixed solution with a concentration of 20 mg / mL was prepared, and the solvent was ethanol.

[0078] 3) Mix ZnO and ZnCaO and prepare quantum dot devices by conventional solution spin coating method

[0079] The ZnO electron transport layer mixed solution and the ZnCaO electron transport layer mixed solution were mixed at a volume ratio of 1:2 to prepare a ZnO and ZnCaO electron transport layer mixed solution.

[0080] The filtered PEDPOT:PSS (AI4083) solution was spin coated on the cleaned ITO glass substrate at a speed of 3500rpm for 40s, followed by annealing at 150℃ for 20min. The hole transport layer PVK chlorobenzene solution (6mg / mL) was spin coated on PEDPOT:PSS (AI4083) at a speed of 1800rpm for 40s and annealed at 110℃ for 10min. The prepared CdSe / ZnS green quantum dot solution (30mg / mL, octane) of a certain concentration was spin coated at a speed of 2000rpm for 60s and annealed at 60℃ for 30min. The electron transport layer ZnCaO and ZnO mixed solution was spin coated at a speed of 2500rpm for 60s and annealed at 60℃ for 30min. Finally, in a high vacuum of 2×10 4 Pa pressure, a 150nm thick aluminum electrode was deposited by thermal evaporation through a mask, and the area of ​​the prepared QLED device was 4cm 2 .

[0081] Comparative Example 1

[0082] The electron transport layer of this comparative example is spin-coated with a ZnO mixed solution, and other contents are the same as those of Example 1.

[0083] The QLED devices prepared in the above-mentioned Example 1 and Comparative Example 1 were tested for device efficiency (EQE) using the same test method. The results are shown in Table 1. It can be seen from Table 1 that the device efficiency of Example 1 is higher than that of Comparative Example 1, with an improvement of nearly 12%.

[0084] Table 1

[0085] Device Category Device efficiency (EQE) Comparative Example 1 9.5% Example 1 10.6%

[0086] Example 2

[0087] This embodiment takes PVK, InP / ZnSe / ZnS red quantum dots as an example for detailed description:

[0088] 1) Preparation of ZnO

[0089] A 3M tetramethylammonium hydroxide ethanol solution was gradually added dropwise to a 3.8M zinc acetate dimethyl sulfoxide (DMSO) solution at room temperature, and after stirring for 30 minutes, the solution was washed with ethyl acetate and heptane to obtain ZnO.

[0090] Disperse ZnO at a concentration of 10 mg / mL in an ethanol solvent for preparing an electron transport layer. Take ZnO and ethanol to prepare a ZnO electron transport layer mixed solution.

[0091] 2) Preparation of ZnCaO

[0092] A 0.6 M zinc nitrate aqueous solution and a 0.1 M calcium nitrate aqueous solution were mixed, and a 1 M sodium hydroxide aqueous solution was added to the mixed solution and stirred until a milky white solution was formed.

[0093] The precipitate was washed three times with deionized water and ethanol respectively, and after drying, a ZnCaO electron transport layer mixed solution with a concentration of 8 mg / mL was prepared, and the solvent was ethanol.

[0094] 3) Mix ZnO and ZnCaO and prepare quantum dot devices by conventional solution spin coating method

[0095] The ZnO electron transport layer mixed solution and the ZnCaO electron transport layer mixed solution were mixed at a volume ratio of 1:2 to prepare a ZnO and ZnCaO electron transport layer mixed solution.

[0096] The filtered PEDPOT:PSS (AI4083) solution was spin coated on the cleaned ITO glass substrate at a speed of 3500rpm for 40s, followed by annealing at 150℃ for 20min. The hole transport layer PVK chlorobenzene solution (6mg / mL) was spin coated on PEDPOT:PSS (AI4083) at a speed of 1800rpm for 40s and annealed at 110℃ for 10min. The prepared InP / ZnSe / ZnS red quantum dot solution (30mg / mL, octane) of a certain concentration was spin coated at a speed of 2000rpm for 60s and annealed at 60℃ for 30min. The electron transport layer ZnCaO:ZnO was spin coated at a speed of 2500rpm for 60s and annealed at 60℃ for 30min. Finally, in a high vacuum of 2×10 4 Pa pressure, a 150nm thick aluminum electrode was deposited by thermal evaporation through a mask, and the area of ​​the prepared QLED device was 4cm 2 .

[0097] Comparative Example 2

[0098] The electron transport layer of this comparative example is spin-coated with a ZnO mixed solution, and other contents are the same as those of Example 2.

[0099] The QLED devices prepared in the above-mentioned Example 2 and Comparative Example 2 were tested for device efficiency (EQE) using the same test method. The results are shown in Table 2. It can be seen from Table 2 that the device efficiency of Example 2 is higher than the device efficiency of Comparative Example 2.

[0100] Table 2

[0101] Device Category Device efficiency (EQE) A 11.9% B 12.3%

[0102] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0103] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A composition for an electron transport layer, characterized in that: include: ZnO; ZnCaO; as well as The first solvent, The molar ratio of the ZnO to the ZnCaO is 1:(1-10), The concentration of ZnO in the composition is (0.1-100) mg / mL, The concentration of ZnCaO in the composition is (0.1-100) mg / mL.

2. The composition for an electron transport layer according to claim 1, characterized in that The concentration of ZnO in the composition is (15-30) mg / mL.

3. The composition for an electron transport layer according to claim 1, characterized in that: The concentration of ZnCaO in the composition is (15-30) mg / mL.

4. The composition for an electron transport layer according to claim 1, characterized in that The first solvent is selected from at least one of methanol, ethanol, propanol, butanol, petroleum ether, ethyl ether, n-butyl ether, octane, hexane, heptane, acetone, ethyl acetate, toluene, chlorobenzene, chloroform, dichloromethane and chlorobenzene.

5. A method for preparing the composition for an electron transport layer according to any one of claims 1 to 4, characterized in that: include: (1) Preparation of ZnO; (2) mixing the calcium-containing inorganic substance, the zinc-containing inorganic substance, the second solvent and the base, and reacting them to obtain ZnCaO; (3) The ZnO, the ZnCaO and a first solvent are mixed to obtain a composition for an electron transport layer.

6. The method according to claim 5, characterized in that In step (1), the specific process of preparing ZnO is as follows: A base is reacted with the zinc salt solution to obtain ZnO.

7. The method according to claim 6, characterized in that In step (1), the base is selected from at least one of tetramethylammonium hydroxide, potassium hydroxide, sodium hydroxide and lithium hydroxide.

8. The method according to claim 6, characterized in that In step (1), the zinc salt in the zinc salt solution is selected from at least one of zinc acetate, zinc nitrate and zinc chloride.

9. The method according to claim 6, characterized in that In step (1), the solvent in the zinc salt solution is selected from at least one of dimethyl sulfoxide, ethanol and ethyl acetate.

10. The method according to claim 6, characterized in that In step (1), the Zn in the zinc salt solution 2+ With the OH in the base - The molar ratio is 1:(0.1-10).

11. The method according to claim 6, characterized in that In step (1), the Zn in the zinc salt solution 2+ The concentration is (0.1-100) mg / mL.

12. The method according to claim 5, characterized in that In step (2), the molar ratio of the calcium-containing inorganic substance to the zinc-containing inorganic substance is 1:(0.01-100).

13. The method according to claim 12, characterized in that In step (2), the molar ratio of the calcium-containing inorganic substance to the zinc-containing inorganic substance is 1:(0.1-10).

14. The method according to claim 5, characterized in that In step (2), the calcium-containing inorganic substance reacts with OH in the alkali. - The molar ratio is 1:(2-10).

15. The method according to claim 5, characterized in that In step (2), the calcium-containing inorganic substance is selected from at least one of calcium nitrate, calcium fluoride, calcium chloride, calcium bromide, calcium iodide and calcium sulfate.

16. The method according to claim 5, characterized in that In step (2), the zinc-containing inorganic substance is selected from at least one of zinc nitrate, zinc fluoride, zinc chloride, zinc bromide, zinc iodide and zinc sulfate.

17. The method according to claim 5, characterized in that In step (2), the second solvent is selected from at least one of methanol, ethanol, propanol, butanol and deionized water.

18. The method according to claim 5, characterized in that In step (2), the base is selected from at least one of sodium hydroxide, magnesium hydroxide and potassium hydroxide.

19. An electron transport layer, characterized in that The electron transport layer is prepared by a solution spin coating method using the composition according to any one of claims 1 to 4 or a composition prepared by the method according to any one of claims 5 to 18.

20. A quantum dot light-emitting device, characterized in that: The quantum dot light-emitting device has the electron transport layer as claimed in claim 19.