Secondary battery and method for manufacturing the same
By covering the non-uniform coating part on the first electrode in the secondary battery and using the second electrode active material to form the inactive coating part, the precipitation problem caused by non-uniform coating in battery manufacturing is solved and the stability of the battery is improved. sex and performance.
Patent Information
- Application Number
- CN202080017252.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-08
- Filing Date
- 2020-03-31
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-03-31
AI Technical Summary
When manufacturing secondary batteries, over-coating of the first electrode active material results in non-uniform coating portions, resulting in precipitation on the second electrode, affecting stability and battery performance.
Form a non-uniform coating part at the beginning or end of coating of the first electrode active material, and cover the inactive coating part at the beginning or end of coating of the second electrode active material to cover the non-uniformity on the first electrode Coated parts to prevent precipitation.
By covering the non-uniform coating part, the stability and performance of the secondary battery are improved, lithium is prevented from being precipitated on the second electrode, and the overall performance of the battery is improved.
Smart Images

Figure CN113767503B_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the benefit of priority from Korean Patent Application No. 10-2019-0040973, filed on Apr. 8, 2019, which is hereby incorporated by reference in its entirety. Technical Field
[0003] The present invention relates to a secondary battery and a method for manufacturing the same, and more particularly, to a secondary battery in which precipitation is prevented from being generated due to a non-uniform coating portion occurring when an electrode active material is applied and a method for manufacturing the same. Background Art
[0004] Generally, a secondary battery refers to a battery that is both rechargeable and dischargeable, unlike a primary battery that is non-rechargeable. Secondary batteries are widely used in high-tech electronic fields such as mobile phones, laptop computers, and camcorders.
[0005] Such a secondary battery includes an electrode assembly in which electrodes and separators are alternately stacked, and a case accommodating the electrode assembly, and the electrode assembly has a structure in which a plurality of electrodes and a plurality of separators are alternately stacked.
[0006] Here, the plurality of electrodes include a first electrode and a second electrode. The first electrode includes a first current collector and a first electrode active material applied on the first current collector, and the second electrode includes a second current collector and a second electrode active material applied on the second current collector.
[0007] The first electrode is a positive electrode, and the second electrode is a negative electrode.
[0008] A method for manufacturing a secondary battery having the above configuration includes: an electrode manufacturing step of manufacturing a first electrode and a second electrode; and an electrode assembly manufacturing step of manufacturing an electrode assembly by stacking the first electrode and the second electrode in a state where a separator is located between the first electrode and the second electrode. The electrode manufacturing step includes a first electrode manufacturing process in which a first active material is applied from a coating start portion to a coating end portion of a first current collector to manufacture the first electrode, and a second electrode manufacturing process in which a second active material is applied from a coating start portion to a coating end portion of a second current collector to manufacture the second electrode.
[0009] Here, the first electrode manufacturing process has the following problem: when applying the first active material from the coating start portion to the coating end portion of the first current collector, the first active material is excessively applied to any one of the coating start portion and the coating end portion of the first current collector, thereby causing a non-uniform coating portion, i.e., bulging. As a result, there is a problem that precipitation occurs on the second electrode as a negative electrode due to the bulging, thereby deteriorating stability and battery performance. Summary of the invention
[0010] Technical issues
[0011] The present invention is invented to solve the above problems. Therefore, the present invention provides a secondary battery and a method for manufacturing the same. In the secondary battery, an inactive coating portion is formed on a second electrode serving as a negative electrode, and the inactive coating portion covers the non-uniform coating portion generated on a first electrode serving as a positive electrode to stably cover the non-uniform coating portion generated on the first electrode, thereby preventing precipitation from occurring on the second electrode, thereby improving stability and battery performance.
[0012] Technical Solution
[0013] A secondary battery according to the present invention for achieving the above purpose includes: a first electrode, which is provided with a first current collector and a first electrode active material applied on at least one surface of the first current collector; and a second electrode, which is provided with a second current collector and a second electrode active material applied on at least one surface of the second current collector, wherein a non-uniform coating portion is provided on at least one of the coating start portion or the coating end portion of the first electrode active material, at which the first electrode active material is irregularly increased in amount and applied, and an inactive coating portion is provided on at least one of the coating start portion or the coating end portion of the second electrode active material, and the inactive coating portion is constructed to cover the non-uniform coating portion.
[0014] The inactive coating portion may be made of the same material as the second electrode active material.
[0015] The inactive coating portion may be provided by coating with the second electrode active material in a state where at least one of a coating start portion or a coating end portion of the second electrode active material extends to cover the non-uniform coating portion.
[0016] The thickness of the inactive coating portion may be greater than the thickness of the second electrode active material from the coating start portion to the coating end portion.
[0017] The coating thickness of the inactive coating portion may correspond to the coating thickness of the non-uniform coating portion.
[0018] The first electrode may be a positive electrode, and the second electrode may be a negative electrode.
[0019] The first electrode may further include a non-reactive tape attached to the non-uniformly coated portion.
[0020] The non-reactive tape may be attached to surround the entire non-uniformly coated portion.
[0021] A method for manufacturing a secondary battery according to the present invention includes: a first electrode manufacturing step (S10), which applies a first electrode active material on one surface of a first current collector from a coating start portion to a coating end portion, and applies the first electrode active material on another surface of the first current collector from a coating start portion to a coating end portion to manufacture a first electrode; and a second electrode manufacturing step (S20), which applies a second electrode active material on one surface of a second current collector from a coating start portion to a coating end portion, and applies the second electrode active material on another surface of the second current collector from a coating start portion to a coating end portion to manufacture a second electrode, wherein, in the first electrode manufacturing step (S10), due to an increase in the loading amount of the first electrode active material, a non-uniform coating portion is formed on at least one of the coating start portion or the coating end portion of the first electrode active material, and in the second electrode manufacturing step (S20), an inactive coating portion covering the non-uniform coating portion is further formed on at least one of the coating start portion or the coating end portion of the second electrode active material.
[0022] In the second electrode manufacturing step ( S20 ), after at least one of the coating start portion or the coating end portion of the second electrode active material is coated, the loading amount of the second electrode active material may be increased to be applied on the inactive coating portion covering the non-uniform coating portion.
[0023] The thickness of the inactive coating portion may be greater than the thickness of the second electrode active material from the coating start portion to the coating end portion.
[0024] The inactive coating portion may be applied to a thickness corresponding to the thickness of the non-uniform coating portion.
[0025] The method may further include: after the second electrode manufacturing step (S20), an electrode rolling step (S30) of rolling surfaces of the first electrode and the second electrode.
[0026] The method may further include: after the electrode rolling step ( S30 ), a tape attaching step ( S40 ) of attaching a non-reactive tape to the non-uniform coating portion formed on the first electrode.
[0027] The method may further include: after the tape attaching step ( S40 ), a secondary battery manufacturing step ( S60 ) of interposing a separator between the first electrode and the second electrode to manufacture a secondary battery.
[0028] Beneficial effects
[0029] The secondary battery according to the present invention may include an inactive coating portion that covers a non-uniform coating portion generated on the first electrode when manufacturing the second electrode as the negative electrode. Therefore, the non-uniform coating portion can be continuously covered to prevent precipitation from occurring on the second electrode, thereby improving the stability and performance of the secondary battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 is a perspective view of a secondary battery according to a first embodiment of the present invention.
[0031] Figure 2 is a cross-sectional view of an electrode assembly of a secondary battery according to a first embodiment of the present invention.
[0032] Figure 3 is a cross-sectional view illustrating an inactive tape of a secondary battery according to a first embodiment of the present invention.
[0033] Figure 4 is a flowchart illustrating a method for manufacturing a secondary battery according to a first embodiment of the present invention.
[0034] Figure 5 is a process diagram illustrating a method for manufacturing a secondary battery according to a first embodiment of the present invention.
[0035] Figure 6 The table shown shows values obtained by measuring the thicknesses of the second electrode active material and the inactive coating portion of the second electrode manufactured by the method for manufacturing the secondary battery according to the first embodiment of the present invention.
[0036] Figure 7 is a graph illustrating thicknesses of a second electrode manufactured by the method for manufacturing a secondary battery according to the first embodiment of the present invention before and after rolling. DETAILED DESCRIPTION
[0037] Hereinafter, embodiments of the present invention will be described in detail with reference to the accompanying drawings so that those skilled in the art can easily implement the technical ideas of the present invention. However, the present invention can be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. In the accompanying drawings, for the sake of clarity, any unnecessary content for describing the present invention will be omitted, and the same reference numerals in the accompanying drawings also represent the same elements.
[0038] [Secondary Battery According to First Embodiment of the Invention]
[0039] like Figure 1 As shown in , a secondary battery 100 according to a first embodiment of the present invention includes an electrode assembly 110 , a can 120 accommodating the electrode assembly 110 , and a cap assembly 130 installed in an opening of the can 120 .
[0040] like Figure 2 As shown in , the electrode assembly 110 has a structure in which a plurality of electrodes and a plurality of separators are alternately stacked. The plurality of electrodes include a first electrode 111 and a second electrode 112. That is, the electrode assembly 110 includes the first electrode 111 and the second electrode 112 stacked downward and the separator 113 disposed between the first electrode 111 and the second electrode 112.
[0041] The first electrode 111 includes a first current collector 111 a and a first electrode active material 111 b applied from a coating start portion A of the first current collector 111 a to a coating end portion B of the first current collector 111 a .
[0042] The second electrode 112 includes a second current collector 112 a and a second electrode active material 112 b applied from a coating start portion C to a coating end portion D of the second current collector 112 a .
[0043] Here, the first electrode is a positive electrode, and the second electrode is a negative electrode.
[0044] The first electrode 111 as a positive electrode is coated while applying the first electrode active material 111b from the coating start portion A to the coating end portion B of the first current collector 111a by using a coating device (not shown). Here, since the coating device moves uniformly between the coating start portion A and the coating end portion B in addition to the coating start portion A and the coating end portion B, the first electrode active material can be uniformly applied. However, although the first electrode active material is applied with a uniform thickness, since the coating is started on the coating start portion A or completed on the coating end portion B in a state where the coating device is stopped, the first electrode active material 111b is excessively applied, thereby forming a non-uniform coating portion 111c. That is, as Figure 2 As shown in FIG. 1 , since the first electrode active material 111 b is excessively applied from the coating start portion A of the first current collector 111 a to the coating end portion B of the first current collector 111 a , a non-uniform coating portion 111 c is formed.
[0045] Since the non-uniform coating portion 111c formed as described above is unintentionally coated when manufacturing the first electrode, when the first electrode 111 and the second electrode 112 are stacked, lithium may be precipitated on the second electrode 112 due to the non-uniform coating portion 111c, thereby deteriorating stability and battery performance.
[0046] In order to solve the above problem, the second electrode 112 includes an inactive coating portion 112c, which covers the non-uniform coating portion 111c generated on the first electrode 111. Therefore, the non-uniform coating portion 111c can be stably covered by the inactive coating portion 112c to prevent lithium from being precipitated on the electrode, thereby preventing stability and battery performance from being deteriorated.
[0047] That is, the inactive coating portion 112c is formed on any one of the coating start portion C and the coating end portion D of the second current collector 112a included in the second electrode 112, which corresponds to the non-uniform coating portion 111c formed on the first electrode. Therefore, the non-uniform coating portion 111c formed on the first electrode 111 may be covered by the inactive coating portion 112c formed on the second electrode 112.
[0048] The inactive coating portion 112c is made of the same material as the second electrode active material 112b. That is, the inactive coating portion 112c is made of the same material as the second electrode active material 112b applied on the second current collector 112a. Therefore, the ease of manufacturing can be improved, and in particular, the inactive coating portion 112c and the non-uniform coating portion 111c are unintentionally coated, but due to the increase of active materials, the battery performance can be improved.
[0049] That is, the inactive coating portion 112c is coated with the second electrode active material 112b from the coating start portion C of the second current collector 112a to the coating end portion D. Here, the loading amount of the second electrode active material 112b increases at the coating start portion C and the coating end portion D of the second current collector 112a, and thus, the second electrode active material 112b applied to the coating start portion C and the coating end portion D is widely spread to form the inactive coating portion 112c.
[0050] In summary, the inactive coating portion 112c may be provided by coating with the second electrode active material 112b in a state where at least one of the coating start portion C or the coating end portion D of the second electrode active material 112b extends to cover the non-uniform coating portion 111c. Therefore, the second electrode active material 112b and the inactive coating portion 112c may be made of the same material to increase ease of manufacturing.
[0051] The thickness of the coated inactive coating portion 112c may be greater than the thickness from the coating start portion C to the coating end portion D of the second electrode active material 112b. That is, since the non-uniform coating portion 111c is generated due to the increase in the loading amount of the first electrode active material 111b, the thickness of the coated inactive coating portion 112c may be greater than the thickness from the coating start portion C to the coating end portion D of the second electrode active material 112b to stably cover the non-uniform coating portion 111c.
[0052] In particular, the coating thickness of the inactive coating portion 112c corresponds to the coating thickness of the non-uniform coating portion 111c. That is, when the coating thickness of the inactive coating portion 112c is less than the coating thickness of the non-uniform coating portion 111c, the non-uniform coating portion 111c may not be stably covered by the inactive coating portion 112c, thereby causing precipitation on the second electrode 112. Moreover, when the thickness of the inactive coating portion 112c is greater than the thickness of the non-uniform coating portion 111c, although the non-uniform coating portion 111c is stably covered, the second electrode active material 112b may still be excessively used, thereby significantly increasing the manufacturing cost. Therefore, the thickness of the inactive coating portion 112c may correspond to the thickness of the non-uniform coating portion 111c to reduce the manufacturing cost and stably cover the non-uniform coating portion 111c.
[0053] The surface of the inactive coating portion 112c corresponding to the non-uniform coating portion 111c may be set as a flat horizontal surface 112c-1. Therefore, even if the surface of the non-uniform coating portion 111c is non-uniform, the friction between the non-uniform coating portion 111c and the inactive coating portion 112c may be minimized, and the non-uniform coating portion 111c may be stably covered.
[0054] The connection portion between the second electrode active material 112b and the inactive coating portion 112c may be set as an inclined surface so as not to form a step portion. Therefore, the separator 113 may be prevented from being damaged due to interference with the connection portion between the second electrode active material 112b and the inactive coating portion 112c. In particular, the first electrode or the second electrode may be prevented from being folded or damaged due to interference with the non-uniform coating portion 111c at the connection portion between the second electrode active material 112b and the inactive coating portion 112c.
[0055] The secondary battery 100 having the above-described configuration according to the first embodiment of the present invention includes an inactive coating portion 112 c located on the second electrode 112 as a negative electrode to stably cover the non-uniform coating portion 111 c generated on the first electrode 111 and prevent lithium from being precipitated on the second electrode 112, thereby improving stability and preventing battery performance from being deteriorated.
[0056] like Figure 3 As shown in , the secondary battery 100 according to the first embodiment of the present invention may further include an inactive tape 114, which is attached to the non-uniform coating portion 111c formed on the first electrode 111. That is, when a meandering failure occurs in the first and second electrodes stacked downward, the first electrode 111 and the second electrode 112 are stacked at different angles, and therefore, the inactive coating portion 112c of the second electrode 112 may not cover the non-uniform coating portion 111c formed on the first electrode 111. In order to prevent this phenomenon, the inactive tape 114 may be attached to the non-uniform coating portion 111c formed on the first electrode 111 to cover the non-uniform coating portion 111c. Therefore, even if the first electrode 111 and the second electrode 112 are stacked at different angles, the non-uniform coating portion 111c can be stably covered.
[0057] The non-reactive tape 114 may be attached to completely surround the non-uniform coating portion 111 c to stably cover the entire non-uniform coating portion 111 c .
[0058] In the secondary battery 100 according to the first embodiment of the present invention, in order to increase the adhesion of the edge surface of the inactive tape, an adhesive 115 may be applied between the edge surface of the inactive tape 114 and the first electrode 111 to improve the adhesion of the edge surface of the inactive tape 114 through the adhesive 115.
[0059] In particular, the non-reactive tape may be provided as a double-sided tape. As a result, the non-uniform coating portion 111 c and the separator 113 corresponding to each other may be attached to be connected to each other to prevent the first electrode 111 having the non-uniform coating portion 111 c from having a bending failure.
[0060] Hereinafter, a method for manufacturing the secondary battery according to the first embodiment of the present invention will be described.
[0061] [ Method for manufacturing a secondary battery according to a first embodiment of the present invention ]
[0062] like Figure 4 and 5 As shown in , the method for manufacturing a secondary battery according to the first embodiment of the present invention includes: a first electrode manufacturing step ( S10 ) of manufacturing a first electrode 111 ; and a second electrode manufacturing step ( S20 ) of manufacturing a second electrode 112 .
[0063] First electrode manufacturing step
[0064] refer to Figure 5(a), in the first electrode manufacturing step (S10), from the coating start portion A to the coating end portion B, on one surface of the first current collector 111a (when Figure 5 (a), the first electrode active material 111b is applied on the top surface of the first current collector. Next, from the coating start portion A to the coating end portion B, the other surface of the first current collector 111a (when the Figure 5 (a), the first electrode active material 111b is applied on the bottom surface of the first current collector. The first electrode 111 may be manufactured through the above process.
[0065] Here, in the first electrode manufacturing step ( S10 ), the non-uniform coating portion 111 c is formed on at least one of the coating start portion A or the coating end portion B due to an increase in the loading amount of the first electrode active material 111 b .
[0066] Second electrode manufacturing step
[0067] refer to Figure 5 (b) In the second electrode manufacturing step (S20), from the coating start portion C to the coating end portion D, on one surface of the second current collector 112a (when Figure 5 (b), the second electrode active material 112b is applied to the top surface of the second current collector. Next, from the coating start portion C to the coating end portion D, the other surface of the second current collector 112a (when the Figure 5 (b), the second electrode active material 112b is applied to the bottom surface of the second current collector. The second electrode 112 may be manufactured through the above process.
[0068] Here, in the second electrode manufacturing step (S20), the inactive coating portion 112c covering the non-uniform coating portion 111c is further formed on at least one of the coating start portion C or the coating end portion D of the second electrode active material 112b. That is, in the second electrode manufacturing step (S20), when at least one of the coating start portion C or the coating end portion D of the second electrode active material 112b is coated, the loading amount of the second electrode active material 112b is increased to be applied on the inactive coating portion 112c covering the non-uniform coating portion 111c.
[0069] In particular, in the second electrode manufacturing step (S20), the thickness of the applied inactive coating portion 112c is greater than the thickness of the second electrode active material 112b applied from the coating start portion C to the coating end portion D of the second electrode active material 112b to stably cover the non-uniform coating portion 111c. In addition, the coated thickness of the inactive coating portion 112c may correspond to the thickness of the non-uniform coating portion 111c to stably cover the non-uniform coating portion 111c.
[0070] After the second electrode manufacturing step ( S20 ), an electrode rolling step ( S30 ) of rolling the surface of each of the first electrode 111 and the second electrode 112 is further performed.
[0071] Electrode rolling steps
[0072] refer to Figure 5 (c) In the electrode rolling step ( S30 ), the first electrode 111 and the second electrode 112 are pressed using the roller 20 to uniformly adjust the coating thickness of each of the first electrode active material 111 b of the first electrode 111 and the second electrode active material 112 b of the second electrode 112 .
[0073] Particularly, in the electrode rolling step (S30), the excessively protruding non-uniform coating portion 111c and the inactive coating portion 112c covering the non-uniform coating portion 111c are rolled together with each other to reduce the thickness of each of the non-uniform coating portion 111c and the inactive coating portion 112c.
[0074] After the electrode rolling step ( S30 ), a tape attaching step ( S40 ) of attaching a non-reactive tape to the non-uniform coating portion formed on the first electrode is further performed.
[0075] Tape Attachment Steps
[0076] refer to Figure 5 (d) The tape attaching step (S40) attaches the non-reactive tape 114 to surround the entire non-uniform coating portion 111c formed on the first electrode 111. Then, even if a stacking error of the first electrode 111 and the second electrode 112 occurs, the non-uniform coating portion 111c can be stably covered by the non-reactive tape 114.
[0077] An adhesive 115 is further applied to a boundary between the inactive tape 114 and the non-uniformly coated portion 111 c to increase adhesion of an edge surface of the inactive tape 114 .
[0078] After the tape attaching step ( S40 ), a secondary battery manufacturing step ( S60 ) for completing the secondary battery 100 is further performed.
[0079] Secondary battery manufacturing steps
[0080] refer to Figure 5 (e), in the secondary battery manufacturing step ( S60 ), the separator 113 is interposed between the first electrode 111 and the second electrode 112 to manufacture the electrode assembly 110 .
[0081] Moreover, if Figure 1 As shown in , the electrode assembly 110 is accommodated in the can 120 , and the cap assembly 130 is installed in the opening of the can 120 to manufacture the secondary battery 100 .
[0082] Here, since the non-uniform coating portion 111c formed on the first electrode 111 and the inactive coating portion 112c of the second electrode 112 are disposed to correspond to each other, precipitation may be prevented from occurring on the second electrode 112 to improve stability and prevent battery performance from being deteriorated.
[0083] Experimental example
[0084] Three second electrodes were prepared, which were negative electrodes manufactured by the method for manufacturing a secondary battery of the present invention, and the thickness and loading of the prepared second electrodes were measured. In particular, the thickness at a portion of the second electrode active material applied to each of the second electrodes and the thickness at a portion of the inactive coating portion were measured.
[0085] Here, the electrode thickness can be measured up to about 30 μm, and the loading can be measured up to about 20 mg / 25 cm 2 Moreover, in the second electrode as the negative electrode, the nitrogen / phosphorus ratio can be increased from 104% to 110%, and the supply rate can be increased from 23.6% to 42.6%, compared with the first electrode as the positive electrode. This can prevent lithium from being precipitated on the second electrode even if a non-uniform coating portion is formed on the first electrode as the positive electrode.
[0086] Measurement results
[0087] As a result of the measurement as described above, it is possible to obtain Figure 6 Experimental table shown.
[0088] That is, when the thickness and loading of the three second electrodes 112 manufactured by the method for manufacturing a secondary battery according to the present invention are compared, it is seen that the thickness and loading of the inactive coating portion 112c as a single-side coating portion are greater than the thickness and loading of the second electrode active material 112b as a double-side coating portion. Therefore, the inactive coating portion 112c for covering the non-uniform coating portion 111c formed on the first electrode 111 can be stably formed.
[0089] and, Figure 7 (a) illustrates the thickness of three second electrodes 112 manufactured by the method for manufacturing a secondary battery according to the present invention before rolling, and Figure 7 (b) illustrates thicknesses of three second electrodes 112 manufactured by the method for manufacturing a secondary battery according to the present invention after rolling.
[0090] refer to Figure 7 In the graph of the second electrode 112, it is seen that the thickness of each of the second electrode active material and the inactive coating portion applied on the second electrode 112 is reduced, and in particular, it is seen that the portion between the second electrode active material and the inactive coating is changed to a gently inclined surface. Therefore, the separator can be prevented from being damaged due to interference between the second electrode active material and the inactive coating portion.
[0091] Accordingly, the scope of the present invention is more defined by the appended claims than by the foregoing description and the exemplary embodiments described therein. Various modifications made within the meaning of the claims equivalent to the present invention and within the claims are considered to be within the scope of the present invention.
Claims
1. A secondary battery comprising: a first electrode provided with a first current collector and a first electrode active material applied to at least one surface of the first current collector; and a second electrode provided with a second current collector and a second electrode active material applied on at least one surface of the second current collector, wherein a non-uniform coating portion is provided on at least one of a coating start portion or a coating end portion of the first electrode active material, at which the first electrode active material is irregularly increased in amount and applied, An inactive coating portion is provided on at least one of a coating start portion or a coating end portion of the second electrode active material, the inactive coating portion being configured to cover the non-uniform coating portion, and The inactive coating portion is made of the same material as the second electrode active material, The thickness of the inactive coating portion is greater than the thickness of the second electrode active material from the coating start portion to the coating end portion, The connection portion between the second electrode active material and the inactive coating portion is provided as an inclined surface so as not to form a step portion, and The surface of the inactive coating portion corresponding to the non-uniform coating portion is set to a flat horizontal surface, The first electrode is a positive electrode, and the second electrode is a negative electrode.
2. The secondary battery according to claim 1, wherein The inactive coating portion is provided by coating with the second electrode active material in a state where at least one of the coating start portion or the coating end portion of the second electrode active material extends to cover the non-uniform coating portion.
3. The secondary battery according to claim 1, wherein The coating thickness of the inactive coating portion corresponds to the coating thickness of the non-uniform coating portion.
4. The secondary battery according to claim 1, wherein The first electrode further includes a non-reactive tape attached to the non-uniformly coated portion.
5. The secondary battery according to claim 4, wherein The non-reactive tape is attached to surround the entire non-uniformly coated portion.
6. A method for manufacturing a secondary battery, the method comprising: A first electrode manufacturing step (S10): applying a first electrode active material on one surface of a first current collector from a coating start portion to a coating end portion, and applying the first electrode active material on another surface of the first current collector from the coating start portion to the coating end portion to manufacture a first electrode; and A second electrode manufacturing step (S20): applying a second electrode active material on one surface of a second current collector from a coating start portion to a coating end portion, and applying the second electrode active material on another surface of the second current collector from the coating start portion to the coating end portion to manufacture a second electrode, wherein, in the first electrode manufacturing step (S10), due to an increase in the loading amount of the first electrode active material, a non-uniform coating portion is formed on at least one of the coating start portion or the coating end portion of the first electrode active material, In the second electrode manufacturing step (S20), an inactive coating portion covering the non-uniform coating portion is further formed on at least one of the coating start portion or the coating end portion of the second electrode active material, and The inactive coating portion is made of the same material as the second electrode active material, The thickness of the inactive coating portion is greater than the thickness of the second electrode active material from the coating start portion to the coating end portion, The connection portion between the second electrode active material and the inactive coating portion is provided as an inclined surface so as not to form a step portion, and The surface of the inactive coating portion corresponding to the non-uniform coating portion is set to a flat horizontal surface, The first electrode is a positive electrode, and the second electrode is a negative electrode.
7. The method according to claim 6, wherein: In the second electrode manufacturing step (S20), after at least one of the coating start portion or the coating end portion of the second electrode active material is coated, a loading amount of the second electrode active material is increased to be applied on the inactive coating portion covering the non-uniform coating portion.
8. The method according to claim 7, wherein: The inactive coating portion is applied to a thickness corresponding to a thickness of the non-uniform coating portion.
9. The method according to claim 6, further comprising: After the second electrode manufacturing step ( S20 ), an electrode rolling step ( S30 ) of rolling the surfaces of the first electrode and the second electrode is performed.
10. The method according to claim 9, further comprising: After the electrode rolling step ( S30 ), a tape attaching step ( S40 ) of attaching a non-reactive tape to the non-uniformly coated portion formed on the first electrode is performed.
11. The method according to claim 10, further comprising: After the tape attaching step ( S40 ), a secondary battery manufacturing step ( S60 ) of interposing a separator between the first electrode and the second electrode to manufacture the secondary battery is performed.