Etching method and substrate processing device
By automatically controlling the pressure control valve in the etching method and using the pressure value in the gas exhaust pipe to adjust the pressure in the processing chamber, the problem of pressure fluctuation in the existing technology is solved, and a stable etching process and improved process performance are achieved.
Patent Information
- Application Number
- CN202110613525.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-06-02
AI Technical Summary
In existing etching methods, the drive of the pressure control valve cannot effectively follow the changes in pressure in the processing chamber, resulting in pressure fluctuations and unstable etching.
By automatically controlling the opening of the pressure control valve, the pressure value in the gas exhaust pipe is used to monitor and adjust the pressure in the processing chamber to ensure that a stable pressure is maintained during the etching process, especially by periodically adjusting the opening when etching the Al film. degree to avoid excessive pressure.
It achieves stable control of the pressure in the processing chamber, reduces pressure fluctuations and particle generation, and improves the process performance and stability of etching.
Smart Images

Figure CN113782412B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to an etching method and a substrate processing device. Background Art
[0002] For example, Patent Document 1 proposes the following scheme: a substrate having a stacked film including an upper titanium film, an aluminum film, and a lower titanium film and having a patterned photoresist layer formed on the stacked film is brought in to perform plasma etching on the stacked film. In Patent Document 1, a predetermined vacuum degree is adjusted inside a processing chamber by automatic control of a pressure control valve, and an etching gas containing a chlorine-containing gas is supplied into the processing chamber as a processing gas, and the processing gas is converted into plasma to perform plasma etching on the stacked film.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2018-41890 Summary of the invention
[0006] Problem that the invention aims to solve
[0007] The present disclosure provides an etching method and a substrate processing apparatus capable of stably controlling the pressure in a processing chamber.
[0008] Solutions for solving problems
[0009] According to one embodiment of the present disclosure, an etching method is provided, which includes the following steps: step (a), placing a substrate having a stacked film formed thereon in a processing chamber, the stacked film having a first titanium film and an aluminum film located below the first titanium film; step (b), etching the first titanium film with the aid of a mask made of an organic material while automatically controlling the opening of the pressure control valve in accordance with changes in pressure in the processing chamber connected to an exhaust device through an exhaust pipe via a pressure control valve or in accordance with changes in pressure in the exhaust pipe; and step (c), etching the first titanium film in accordance with the changes in pressure in step (b). ) to calculate a first opening value based on the value of the opening of the pressure control valve sampled in step (d); step (d), setting the opening of the pressure control valve to the first opening value when etching the aluminum film begins to etch the aluminum film; and step (e), monitoring the pressure in step (d), and when the pressure exceeds a predetermined threshold, changing the first opening value to a second opening value using a predetermined change amount, the etching method includes step (f), in which step (f), step (e) is performed one or more times during the period until the etching of the aluminum film is completed.
[0010] Effects of the Invention
[0011] According to one aspect, the pressure in the processing chamber can be stably controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic cross-sectional view showing an example of a substrate processing apparatus according to the embodiment.
[0013] Figure 2 This is a diagram showing an example of control of the pressure control valve according to the embodiment and pressure vibration in comparison with a reference example.
[0014] Figure 3 It is a diagram showing an example of arrangement of pressure gauges according to the embodiment.
[0015] Figure 4 1 is a flowchart showing an etching method according to an embodiment.
[0016] Figure 5 It is a diagram showing the EPD control according to the embodiment in comparison with the time control of a reference example.
[0017] Figure 6 It is a diagram showing another film structure to which the etching method according to the embodiment is applied.
[0018] Description of Reference Numerals
[0019] 10: processing container; 12: upper chamber; 12a: top plate; 13: lower chamber; 13a: side wall; 25: observation window; 13d: bottom plate; 13f: exhaust port; 30: shower head; 51: gas exhaust pipe; 52: pressure control valve; 53: exhaust device; 54: pressure gauge (CM); 55: luminescence spectrum analysis device; 60: substrate mounting table; 100: substrate processing device; G: substrate; S: processing chamber. DETAILED DESCRIPTION
[0020] Hereinafter, the mode for implementing the present disclosure will be described with reference to the accompanying drawings. In each of the drawings, the same components are sometimes denoted by the same reference numerals, and repeated descriptions are omitted.
[0021] [Substrate processing equipment]
[0022] First, refer to Figure 1 An example of a substrate processing apparatus according to an embodiment of the present disclosure will be described. Figure 1 It is a schematic cross-sectional view showing an example of a substrate processing apparatus according to the embodiment.
[0023] The substrate processing device 100 is an inductively coupled plasma (ICP) processing device for performing various substrate processing methods on a substrate G for FPD that is rectangular when viewed from above (hereinafter referred to as "substrate"). As the material of the substrate, glass is mainly used, and transparent synthetic resins are sometimes used depending on the purpose. Here, the substrate processing includes etching processing, film forming processing using CVD (Chemical Vapor Deposition) method, etc. As an FPD, a liquid crystal display (LCD) is shown as an example. It can also be electroluminescence (EL), plasma display panel (PDP), etc. The substrate G includes a supporting substrate in addition to the substrate in the form of a circuit pattern formed on its surface. In addition, the plane size of the substrate for FPD has become larger with the passage of generations. The planar dimensions of the substrate G processed by the substrate processing apparatus 100 range from about 1500 mm×1800 mm for the sixth generation to about 3000 mm×3400 mm for the 10.5th generation. The thickness of the substrate G is about 0.2 mm to several mm.
[0024] The substrate processing apparatus 100 includes a control unit 90, a rectangular box-shaped processing container 10, and a substrate mounting table 60 having a rectangular shape in a plan view and disposed in the processing container 10 for mounting the substrate G. The processing container 10 may also be in a cylindrical box-shaped, elliptical cylindrical box-shaped, or the like. In this case, the substrate mounting table 60 is also circular or elliptical, and the substrate G mounted on the substrate mounting table 60 is also circular.
[0025] The processing container 10 is divided into two spaces, upper and lower, by a dielectric plate 11. The antenna room as the upper space is formed by an upper chamber 12, and the processing chamber S as the lower space is formed by a lower chamber 13. The processing container 10 is formed of metal such as aluminum, and the dielectric plate 11 is formed of ceramics such as alumina (Al2O3) or quartz.
[0026] In the processing container 10, a rectangular ring-shaped support frame 14 is provided at the boundary between the lower chamber 13 and the upper chamber 12 so as to protrude into the processing container 10, and a dielectric plate 11 is placed on the support frame 14. The processing container 10 is grounded via a grounding wire 13e.
[0027] A loading / unloading port 13b for loading and unloading the substrate G into and out of the lower chamber 13 is provided on the side wall 13a of the lower chamber 13, and the loading / unloading port 13b can be opened and closed freely by a gate valve 20. The lower chamber 13 is adjacent to a transfer chamber (not shown) having a transfer mechanism therein, and the gate valve 20 is opened and closed to control the loading and unloading of the substrate G by the transfer mechanism through the loading / unloading port 13b.
[0028] In addition, a plurality of openings 13c are provided at intervals on the side wall 13a of the lower chamber 13, and an observation window 25 made of quartz is installed on the outside of each opening 13c so as to block the opening 13c. A light emission spectrometer 55 is installed on the outside of the observation window 25 via an optical fiber. The light emission spectrometer 55 receives the light emission of the plasma in the processing chamber S via the observation window 25 and measures the intensity of the light emission. The monitoring information of the light emission intensity of the plasma obtained by the light emission spectrometer 55 is sent to the control unit 90. The light emission spectrometer 55 only needs to be installed in the observation window 25 of the required opening 13c among the plurality of openings 13c.
[0029] In addition, a plurality of exhaust ports 13f are provided on the bottom plate 13d of the lower chamber 13. A gas exhaust pipe 51 is connected to the exhaust port 13f, and the gas exhaust pipe 51 is connected to the exhaust device 53 via the pressure control valve 52. The gas exhaust section 50 is formed by the gas exhaust pipe 51, the pressure control valve 52 and the exhaust device 53. The exhaust device 53 has a vacuum pump such as a turbomolecular pump, and during the process, the exhaust device 53 freely evacuates the lower chamber 13 until a predetermined vacuum degree is reached. A pressure gauge (CM) 54 is provided near the pressure control valve 52 and on the upstream side (lower chamber 13 side) of the pressure control valve 52. The pressure value at the upstream of the pressure control valve 52 in the gas exhaust pipe 51 is measured by the pressure gauge (CM) 54, and the pressure value is sent to the control unit 90. The control unit 90 controls the opening of the pressure control valve 52 based on the measured pressure value.
[0030] A support beam for supporting the dielectric plate 11 is provided on the lower surface of the dielectric plate 11, and the support beam also serves as a shower head 30. The shower head 30 may be formed of a metal such as aluminum, and may be subjected to a surface treatment based on anodization. A gas flow path 31 extending in a horizontal direction is formed in the shower head 30. The gas flow path 31 is connected to a gas ejection hole 32, and the gas ejection hole 32 extends downward to face the processing chamber S below the shower head 30.
[0031] A gas introduction pipe 45 connected to the gas flow path 31 is connected to the upper surface of the dielectric plate 11. The gas introduction pipe 45 airtightly penetrates the supply port 12b opened in the top plate 12a of the upper chamber 12, and is connected to the processing gas supply source 44 via the gas supply pipe 41 airtightly combined with the gas introduction pipe 45. An opening and closing valve 42 and a flow controller 43 such as a mass flow controller are provided at a midway position of the gas supply pipe 41. The gas introduction pipe 45, the gas supply pipe 41, the opening and closing valve 42, the flow controller 43 and the processing gas supply source 44 form a processing gas supply unit 40. The processing gas supplied from the processing gas supply unit 40 is supplied to the shower head 30 via the gas supply pipe 41 and the gas introduction pipe 45, and is ejected into the processing chamber S via the gas flow path 31 and the gas ejection hole 32.
[0032] A high frequency antenna 15 is disposed in the upper chamber 12 forming the antenna chamber. The high frequency antenna 15 is formed by winding an antenna wire 15a formed of a metal having good conductivity such as copper in a loop or spiral shape. For example, the loop-shaped antenna wire 15a may be disposed in multiple layers.
[0033] The terminal of the antenna wire 15a is connected to a power supply member 16 extending upward from the upper chamber 12, and the upper end of the power supply member 16 is connected to a power supply line 17, and the power supply line 17 is connected to a high-frequency power supply 19 via a matching device 18 for impedance matching. By applying a high-frequency power of, for example, 10 MHz to 15 MHz from the high-frequency power supply 19 to the high-frequency antenna 15, an induced electric field is formed in the lower chamber 13. The processing gas supplied from the shower head 30 to the processing chamber S is plasma-formed by the induced electric field, thereby generating an inductively coupled plasma, and providing ions in the plasma to the substrate G. The high-frequency power supply 19 is an ion source power supply for plasma generation, and the high-frequency power supply 73 connected to the substrate mounting table 60 is a bias power supply for attracting the generated ions to give kinetic energy to the ions. In this way, for the ion source power supply, inductive coupling is used to generate plasma, and the bias power supply as another power supply is connected to the substrate mounting table 60 to control the ion energy. As a result, the generation of plasma and the control of ion energy can be performed independently, thereby improving the degree of freedom of the process. The frequency of the high-frequency power output from the high-frequency power source 19 is preferably set within a range of 0.1 MHz to 500 MHz.
[0034] The substrate mounting table 60 has a substrate 63 and an electrostatic chuck 66 formed on the upper surface 63a of the substrate 63. The top view shape of the substrate 63 is rectangular, and the substrate 63 has a plane size of the same degree as the substrate G mounted on the substrate mounting table 60. The length of the long side of the substrate 63 can be set to a size of about 1800mm to 3400mm, and the length of the short side can be set to a size of about 1500mm to 3000mm. Relative to the plane size, the thickness of the substrate 63 can be, for example, about 50mm to 100mm. The substrate 63 is formed of stainless steel, aluminum, aluminum alloy, etc. A temperature adjustment medium flow path 62a is provided on the substrate 63 in a manner that covers the entire area of the rectangular plane. In addition, the temperature adjustment medium flow path 62a can also be provided on the electrostatic chuck 66, for example. In addition, the substrate 63 can also be formed as a laminate of two components instead of being a single body composed of one component as shown in the example.
[0035] The two ends of the temperature adjustment medium flow path 62a are connected with the feed pipe 62b and the return pipe 62c, and the feed pipe 62b is used to supply the temperature adjustment medium to the temperature adjustment medium flow path 62a, and the return pipe 62c is used to discharge the temperature adjustment medium that has been circulated in the temperature adjustment medium flow path 62a and heated. The feed pipe 62b is connected with the feed flow path 82, and the return pipe 62c is connected with the return flow path 83. The feed flow path 82 and the return flow path 83 are connected with the cooler 81. The cooler 81 has a main body for controlling the temperature and the ejection flow rate of the temperature adjustment medium and a pump for pressurizing and conveying the temperature adjustment medium (both are not shown). In addition, a refrigerant is used as the temperature adjustment medium, and the refrigerant is Galden (registered trademark), Fluorinert (registered trademark), etc. The temperature adjustment method of the example shown in the figure is a method in which the temperature adjustment medium is circulated in the substrate 63, but it can be a method in which the substrate 63 is built-in with a heater, etc. to use the heater to adjust the temperature, or it can be a method in which the temperature adjustment is performed by both the temperature adjustment medium and the heater. In addition, the temperature adjustment accompanying heating can be performed by circulating a high-temperature temperature adjustment medium instead of performing the temperature adjustment accompanying heating by the heater. In addition, the resistor heater is formed of tungsten, molybdenum, or a compound of any of these metals and aluminum oxide, titanium, etc. In addition, in the example shown in the figure, the temperature adjustment medium flow path 62a is formed on the substrate 63, but, for example, the electrostatic chuck 66 may also have a temperature adjustment medium flow path.
[0036] A box-shaped base 68 is fixed to the bottom plate 13 d of the lower chamber 13 . The base 68 is made of an insulating material and has a step portion inside. The substrate stage 60 is placed on the step portion of the base 68 .
[0037] An electrostatic chuck 66 for directly placing the substrate G is formed on the upper surface of the substrate 63. The electrostatic chuck 66 includes: a ceramic layer 64, which is a dielectric coating formed by spraying ceramics such as aluminum oxide; and a conductive layer 65 (electrode) buried inside the ceramic layer 64, and the conductive layer 65 has an electrostatic adsorption function. The conductive layer 65 is connected to a DC power supply 75 via a power supply line 74. When a switch (not shown) provided on the power supply line 74 is turned on by the control unit 90, a DC voltage is applied from the DC power supply 75 to the conductive layer 65, thereby generating a Coulomb force. The substrate G is electrostatically adsorbed on the upper surface of the electrostatic chuck 66 by the Coulomb force, and is held in a state of being placed on the upper surface of the substrate 63. The substrate placement table 60 forms a lower electrode for placing the substrate G in this way.
[0038] A temperature sensor such as a thermocouple is provided on the substrate 63, and monitoring information of the temperature sensor is sent to the control unit 90 at any time. The control unit 90 performs temperature adjustment control of the substrate 63 and the substrate G based on the sent temperature monitoring information. More specifically, the control unit 90 adjusts the temperature and flow rate of the temperature adjustment medium supplied from the cooler 81 to the feed flow path 82. Then, the temperature adjustment medium after temperature adjustment and flow adjustment is circulated to the temperature adjustment medium flow path 62a, thereby performing temperature adjustment control of the substrate mounting table 60. In addition, a temperature sensor such as a thermocouple may also be provided on the electrostatic chuck 66, for example.
[0039] A rectangular frame-shaped focus ring 69 is placed on the outer periphery of electrostatic chuck 66 and on the upper surface of base 68, and the upper surface of focus ring 69 is set lower than the upper surface of electrostatic chuck 66. Focus ring 69 is made of ceramic such as alumina or quartz.
[0040] The lower surface of the substrate 63 is connected to a power supply member 70. The lower end of the power supply member 70 is connected to a power supply line 71, and the power supply line 71 is connected to a high-frequency power supply 73 as a bias power supply via a matching device 72 for impedance matching. By applying a high-frequency power of, for example, 2 MHz to 6 MHz from the high-frequency power supply 73 to the substrate mounting table 60, ions generated by the high-frequency power supply 19 as an ion source power supply for plasma generation can be attracted to the substrate G. Therefore, in the plasma etching process, the etching rate and the etching selectivity can be improved together.
[0041] The control unit 90 controls the various components of the substrate processing apparatus 100, such as the operation of the cooler 81, the high frequency power supply 19, 73, the processing gas supply unit 40, and the gas exhaust unit 50 based on the monitoring information of the pressure measured by the pressure gauge (CM) 54. The control unit 90 has a memory such as a ROM (Read Only Memory), a RAM (Random Access Memory), and a CPU (Central Processing Unit). The CPU performs a prescribed process according to a process (process recipe) stored in a storage area of the memory. Control information of the substrate processing apparatus 100 for process conditions is set in the process. The control information includes, for example, a gas flow rate, a pressure in the processing container 10, a temperature in the processing container 10, a temperature of the substrate 63, a process time, and the like.
[0042] The process and the program used by the control unit 90 may be stored in a hard disk, an optical disk, a magneto-optical disk, etc. In addition, the process, etc. may be in the form of being stored in a portable and computer-readable storage medium such as a CD-ROM, a DVD, a memory card, etc., and set in the control unit 90 and read by the control unit 90. In addition, the control unit 90 also has a user interface such as an input device such as a keyboard and a mouse for inputting commands, a display device such as a display that visually displays the operating status of the substrate processing apparatus 100, and an output device such as a printer.
[0043] [Etching method]
[0044] Next, the etching method according to the present embodiment will be described in comparison with the etching methods according to Reference Examples 1 and 2. Figure 2 (a) shows the etching method involved in Reference Example 1, Figure 2 (b) shows the etching method involved in Reference Example 2, Figure 2 (c) shows the etching method involved in this embodiment. The etching target films of Reference Examples 1 and 2 and this embodiment have the same film structure, and a substrate G is etched with the help of a mask composed of a photoresist film of an organic material, and the substrate G has a stacked film with an Al film sandwiched between an upper Ti film and a lower Ti film. In addition, the upper Ti film is equivalent to the first titanium film, and the lower Ti film is equivalent to the second titanium film. The Al film can be either an Al monomer or an Al alloy such as Al-Si. In addition, the etching target film is not limited to the above-mentioned three-layer structure. For example, it can be a structure in which a mask composed of an organic material is formed on two layers of the upper Ti film and the lower Al film, or it can be a structure in which a mask composed of an organic material is formed on the Al film.
[0045] In addition, the process conditions of this embodiment are the same as those of reference examples 1 and 2, and an etching gas containing a chlorine-containing gas is supplied to the lower chamber 13. As the etching gas, in addition to the chlorine-containing gas, an inactive gas such as Ar gas or N2 gas may also be supplied. The stacked film of the upper Ti film, the Al film, and the lower Ti film is etched mainly by the plasma of the chlorine-containing gas in the etching gas.
[0046] In this embodiment and reference examples 1 and 2, the etching gas containing chlorine-containing gas for the upper Ti film and the lower Ti film is the same as the etching gas containing chlorine-containing gas for the Al film, and BCl3 gas and Cl2 gas are used as chlorine-containing gases. However, the present invention is not limited thereto, and the etching gas for the upper Ti film and the lower Ti film and the etching gas for the Al film only need to contain chlorine-containing gas, and part or all of the etching gas for the upper Ti film and the lower Ti film and the etching gas for the Al film may be different.
[0047] The etching results of each of this embodiment and Reference Examples 1 and 2 are described. Figure 2 The horizontal axis of each curve represents time (seconds), the vertical axis on the right represents the pressure value measured by the pressure gauge, and the vertical axis on the left represents the APC position (APC Position). The APC position is the position (angle) of the valve body of the pressure control valve 52, and is represented by the rotation angle / 1000 (= encoder value installed on the pressure control valve 52 / 1000).
[0048] The pressure gauge used in Reference Example 1 is arranged at a position different from that used in the present embodiment and Reference Example 2. Figure 3 The pressure of the processing chamber S is measured by a pressure gauge (CM2) 151 arranged at a CM port provided on a bottom plate 13d of the lower chamber 13. During the etching of the upper Ti film, the Al film, and the lower Ti film, the opening of the pressure control valve 52 is automatically controlled based on the pressure value of the processing chamber S measured by the pressure gauge (CM2) 151. Alternatively, the opening of the pressure control valve 52 may be automatically controlled based on the pressure value of the processing chamber S measured by the pressure gauge (CM1) 150 instead of the pressure gauge (CM2) 151.
[0049] Figure 2 (a) Figure 2 (b) and Figure 2 In (c), (1) indicates the timing when the etching target film is switched from the upper Ti film to the Al film, and (2) indicates the timing when the etching target film is switched from the Al film to the lower Ti film.
[0050] In the etching result of Reference Example 1, Figure 2In (a), during the etching of the Al film, the APC position represented by A1 vibrates and oscillates. The reason is that since there is a mechanical limit to the driving speed of the pressure control valve 52, the driving of the valve body of the pressure control valve 52 cannot follow the change in the pressure value in the processing chamber S measured by the pressure gauge (CM2) 151. In addition, the driving delay of the pressure control valve 52 results in an increase in the amplitude ΔP1 of the pressure value P1. During the etching of the Al film, the amplitude ΔP1 of the pressure value P1 measured by the pressure gauge (CM2) 151 is 2.8mT (about 0.373Pa). In addition, since the position of the pressure gauge (CM2) 151 is far away from the position of the pressure control valve 52, there is a delay until the pressure change measured by the pressure gauge (CM2) 151 is reflected in the pressure at the position of the pressure control valve 52, which is also a reason why the driving of the valve body cannot follow. Due to the oscillation of the pressure control valve 52 generated in this way during the etching process of the Al film, particles are generated, resulting in defects.
[0051] In Reference Example 2, using Figure 3 The pressure gauge (CM) 54 shown measures the pressure upstream of the pressure control valve 52 in the gas exhaust pipe 51. During the etching of the upper Ti film, the Al film, and the lower Ti film, the opening of the pressure control valve 52 is automatically controlled based on the pressure value of the gas exhaust pipe 51 measured by the pressure gauge (CM) 54.
[0052] As a result, in the etching result of Reference Example 2, Figure 2 In (b), during the etching of the Al film, the APC position represented by A2 vibrates and oscillates. However, the pressure control valve 52 is controlled based on the pressure P2 near the pressure control valve 52 in the gas exhaust pipe 51 instead of the pressure in the processing chamber S. Therefore, the transmission delay of the pressure change caused by the distance between the positions in Reference Example 1 is eliminated, and the responsiveness of the control of the pressure control valve 52 is improved. During the etching of the Al film, the amplitude ΔP2 of the pressure P2 in the gas exhaust pipe 51 is 1.1mT (about 0.14Pa). The position of the pressure gauge (CM) 54 is far away from the processing chamber S and is not easily affected by the pressure change in the processing chamber S, which is also one of the main reasons for the improvement.
[0053] Therefore, in the etching method involved in this embodiment, similarly to Reference Example 2, Figure 3The pressure gauge (CM) 54 shown measures the pressure upstream of the pressure control valve 52 in the gas exhaust pipe 51. In addition, the APC position is set to be automatically controlled during the etching of the upper Ti film and the lower Ti film, and different control is performed during the etching of the Al layer. That is, at the beginning of the etching of the Al layer, the APC position is set to an initial value. However, during the etching of the Al layer, the state in which the APC position is fixed to the initial value will not allow the APC position to follow the pressure changes in the processing chamber S or the gas exhaust pipe 51. As a result, the pressure in the processing chamber S gradually rises, which affects the process performance such as the characteristics of the etching performed on the substrate G.
[0054] In order to avoid the above-mentioned influence, in the etching method according to the present embodiment, during the etching of the Al layer, the pressure gauge (CM) 54 periodically measures the pressure in the gas exhaust pipe 51. And, when the measured pressure exceeds a predetermined threshold value, the APC position is controlled so that the APC position is opened by a predetermined change amount from the opening at the current time point.
[0055] That is, for the initial value of the APC position, the first opening value is calculated based on the value of the pressure control valve 52 sampled in the etching process of the upper Ti film, and the opening of the pressure control valve 52 is set to the first opening value when the etching of the Al film starts. In automatic control, the APC position is usually changed in sequence according to the pressure change to adjust the opening so that the pressure is always kept constant. However, in this embodiment, the opening is fixed without responding to the pressure change. In addition, in this embodiment, the difference from the usual automatic control is that the opening is adjusted only when a predetermined threshold is exceeded.
[0056] Next, during the etching process of the Al film, the pressure in the gas exhaust pipe 51 is monitored, and when the pressure exceeds a predetermined threshold, the first opening value is changed to a second opening value by a predetermined change amount. Furthermore, during the period until the etching of the Al film is completed, the process of changing the second opening value by adding the change amount to the second opening value each time the pressure exceeds the predetermined threshold is performed one or more times.
[0057] In addition, in the present embodiment, it is assumed that the etching of the Al layer progresses and the pressure value measured by the pressure gauge (CM) 54 becomes higher, and the control is performed in the following manner: the second opening value is changed by adding the change amount, and the APC position is further opened by the change amount each time the pressure exceeds a predetermined threshold. However, it is not limited to this, and it may be controlled in the following manner: the second opening value is changed by subtracting the change amount, and the APC position is further closed by the change amount each time the pressure is lower than a predetermined threshold as the etching of the Al layer progresses and the pressure value measured by the pressure gauge (CM) 54 becomes lower.
[0058] The results, such as Figure 2 As shown in the etching result of the present embodiment of (c), during the etching of the Al film, the APC position represented by A3 is controlled so that the APC position represented by A3 is gradually opened in stages from the first opening value, which is the opening of the initial value at the timing of (1). Thus, the oscillation of the APC position can be avoided. Thus, the amplitude ΔP3 of the pressure P3 in the gas exhaust pipe 51 during the etching of the Al film is reduced to 0.4mT (about 0.0533Pa), so that stable pressure control can be performed.
[0059] In addition, in the present embodiment, the average value of a plurality of sampling values is calculated as the first opening value, and the plurality of sampling values include the latest sampling value of the pressure control valve 52 sampled in the etching process of the upper Ti film. It is preferred that the plurality of sampling values including the latest sampling value are continuous sampling values. Alternatively, it may be a value sampled every other time or every predetermined number of times. However, the latest sampling value among the values of the pressure control valve 52 sampled in the etching process of the upper Ti film may be set as the first opening value. Furthermore, the initial value of the APC position may also be set to a value obtained by adding an offset value to the first opening value calculated in this way, and the offset value is a predetermined parameter. Regarding the offset value, a value obtained by experience according to the etching method involved in the present embodiment may also be pre-stored in the memory as a parameter.
[0060] [Etching treatment]
[0061] Reference Figure 4 A case where the etching method according to the present embodiment described above is executed by the substrate processing apparatus 100 will be described. Figure 4 The control unit 90 controls each unit of the substrate processing apparatus 100 to execute the etching method according to the embodiment. Figure 4 The etching method shown.
[0062] When starting Figure 4 When the etching method is used, the gate valve 20 is opened, and a substrate G having a stacked film of an upper Ti film, an Al film, and a lower Ti film is loaded through the loading and unloading port 13b, and the substrate G is arranged on the substrate mounting table 60 (step S1). After the substrate G is loaded, the gate valve 20 is closed.
[0063] Next, an etching gas containing chlorine-containing gas is supplied to the lower chamber 13, and the etching gas is plasmatized by high-frequency power applied from the high-frequency power supply 19, and the upper Ti film is etched while the pressure control valve 52 is automatically controlled (step S2). The automatic control of the pressure control valve 52 can be performed based on the pressure value of the processing chamber S measured by the pressure gauge (CM2) 151 or the pressure gauge (CM1) 150, or based on the pressure value in the gas exhaust pipe 51 measured by the pressure gauge (CM) 54. At this time, high-frequency power is applied from the high-frequency power supply 73 to the substrate mounting table 60, so that the substrate mounting table 60 is biased to control the energy of the ions incident on the substrate G.
[0064] While the upper Ti film is being etched, the opening degree of the pressure control valve 52 is sampled at a given period, and the sampled value is stored in the memory (step S3).
[0065] Next, the emission spectrum analyzer 55 detects the emission intensity of the plasma generated in the processing chamber S. Then, based on the emission intensity of the plasma, it is determined by EPD (End Point Detection) control whether the end point of the upper Ti film has been detected (step S4).
[0066] exist Figure 5 In the example of (c), the horizontal axis represents time (seconds), the vertical axis on the left represents the luminescence intensity of aluminum with a wavelength of 396nm, and the vertical axis on the right represents the luminescence intensity of chlorine with a wavelength of 838nm. As the etching of the upper Ti film progresses, when the Al film of the base is exposed, the luminescence intensity of aluminum with a wavelength of 396nm becomes higher. This can be used to detect the end point of the etching of the upper Ti film based on the luminescence intensity of the plasma. Specifically, it is judged that the end point has been reached based on the change in luminescence intensity being lower than a threshold value, and the change in luminescence intensity is represented by the slope (differential) of the curve (including the straight line portion) representing the change in luminescence intensity. For example, during the period when the slope of the curve of the change in luminescence intensity of aluminum with a wavelength of 396nm (hereinafter referred to as "slope") is above a preset threshold value, the control unit 90 determines that the end point of the upper Ti film has not been detected, returns to step S2, and repeats the processing of steps S2 to S4. Thus, the etching of the upper Ti film is promoted.
[0067] On the other hand, when the slope of the luminous intensity of aluminum at a wavelength of 396 nm is below a preset threshold, it is determined that the Al film of the base is fully exposed, and it is determined in step S4 that the end point of the upper Ti film is detected, and the process proceeds to step S5. Then, the first opening value is calculated based on the sampled value of the opening of the pressure control valve 52 stored in the memory (step S5). When there are multiple sampled values in the memory, it is preferred to calculate the average value of the multiple sampled values including the latest sampled value as the first opening value. However, the latest sampled value may also be used as the first opening value.
[0068] Next, the opening of the pressure control valve 52 is set to a first opening value, and the Al film is etched using an etching gas containing a chlorine-containing gas (step S6 ). At this time, the variable n is set to 1.
[0069] Next, the pressure in the gas exhaust pipe 51 is monitored by the pressure gauge (CM) 54 (step S7). However, the pressure in the processing chamber S may be monitored by the pressure gauge (CM2) 151. Next, it is determined whether the pressure value in the gas exhaust pipe 51 is greater than a predetermined threshold value (step S8).
[0070] When the pressure value in the gas exhaust pipe 51 is less than the threshold value, the process proceeds to step S11. When the pressure value in the gas exhaust pipe 51 is greater than the threshold value, the variable n is incremented by 1, and the nth opening value obtained by adding a predetermined change amount to the opening of the pressure control valve 52 at that time point is calculated (step S9). At that time point, the second opening value obtained by adding a predetermined change amount to the first opening value is calculated.
[0071] Next, the opening of the pressure control valve 52 is set to the nth (n=2) opening value to etch the Al film (step S10). Next, the emission spectrum analyzer 55 detects the emission intensity of the plasma, and based on the emission intensity of the plasma, it is determined by EPD control whether the end point of the Al film is detected (step S11).
[0072] exist Figure 5 In the example (c), while the slope of the luminescence intensity of aluminum at a wavelength of 396 nm is above a predetermined threshold, the control unit 90 determines that the end point of the Al film has not been detected, returns to step S7, and repeats the processing of steps S7 to S11. Thus, etching of the Al film is advanced.
[0073] On the other hand, as the etching of the Al film progresses, when the lower Ti film of the substrate is exposed, the luminous intensity of the aluminum with a wavelength of 396nm becomes lower and the slope of the change becomes larger. Therefore, when the slope of the luminous intensity of the aluminum with a wavelength of 396nm is below a preset threshold, the control unit 90 determines that the end point of the Al film is detected and enters step S12. In addition, here, since the change in luminous intensity is decreasing, the slope is expressed as a negative value. Therefore, the threshold is set to a negative value. In addition, the threshold in step S11 is set differently from the threshold in step S5.
[0074] Next, similarly to the upper Ti film, the lower Ti film is etched using etching gas containing chlorine gas while the pressure control valve 52 is automatically controlled (step S12). After the etching of the lower Ti film is completed, the processed substrate G is unloaded (step S13), and the present process is completed.
[0075] exist Figure 5 In the example of (c), when the slope of the luminescence intensity of chlorine with a wavelength of 838 nm is below a preset threshold, the end point of the lower Ti film is detected, and the base film of the lower Ti film is etched by overetching, and then the processed substrate G is removed to end the process. In addition, chlorine with a wavelength of 838 nm is an element contained in the chlorine-containing gas that is not consumed and remains in the etching of the lower Ti film. The threshold in step S12 is also set to a threshold different from that in step S5 and step S11.
[0076] In addition, regarding the values of the above-mentioned threshold values, for example, in the endpoint detection system used in the above-mentioned embodiment, when etching is transferred from the upper Ti layer to the Al layer, the threshold value is set to 200, and when it is less than 200, the etching of the upper Ti layer is deemed to be terminated. In addition, when etching is transferred from Al to the lower Ti layer, the threshold value is set to -10, and when it is less than -10, the etching of Al is deemed to be terminated. In addition, when etching is transferred from the lower Ti layer to the base film, the threshold value is set to 20, and when it is less than 20, the etching of the base Ti is deemed to be terminated. However, the values of these threshold values are not essential contents of the invention of this embodiment, but are contents that should be appropriately determined according to the endpoint detection system used, etc. In addition, these threshold values may also change according to etching conditions, etc.
[0077] As described above, according to the etching method involved in this embodiment, in the etching process of the Al film, the pressure control valve 52 is gradually opened according to the pressure value in the gas exhaust pipe 51 from the state where the opening (APC position) of the pressure control valve 52 is set to the first opening value. In addition, the first opening value as the initial value of the APC position is optimized based on the APC position sampled at the end of the etching process of the upper Ti film. As a result, the pressure fluctuation in the processing chamber S can be suppressed, thereby improving the process performance. In addition, the oscillation of the pressure control valve 52 can be prevented to suppress the generation of particles.
[0078] Ideally, in order to minimize the effect of pressure fluctuations in the processing chamber S on process performance, it is preferred to use Figure 3 The pressure gauge (CM1) 150 and the pressure gauge (CM2) 151 shown directly measure the pressure in the processing chamber S. However, the pressure of the processing chamber S measured by the pressure gauge (CM2) 151 is not necessarily the same as the pressure of the exhaust space. The pressure in the gas exhaust pipe 51 changes rapidly due to the control of the pressure control valve 52, but there will be a certain degree of time delay until the pressure in the processing chamber S changes. Therefore, in the control of the pressure control valve 52 involved in the present embodiment, the pressure near the pressure control valve 52 in the gas exhaust pipe 51 is monitored by the pressure gauge (CM) 54, and the pressure control valve 52 is controlled based on the pressure value measured by the pressure gauge (CM) 54. As a result, it is not easy to generate a delay from the control of the opening of the pressure control valve 52 to the pressure change in the gas exhaust pipe 51, so the pressure tracking performance is improved. However, in the application of the present embodiment, the pressure control valve 52 can also be controlled based on the pressure value measured by the pressure gauge (CM1) 150 or the pressure gauge (CM2) 151.
[0079] [EPD control]
[0080] In the etching method involved in this embodiment, the control method is switched from automatic control of the APC position when etching the upper Ti film to given control of the APC position when etching the Al film at the best timing through EPD control. Similarly, the control method is switched from control of the APC position when etching the Al film to automatic control of the APC position when etching the lower Ti film at the best timing through EPD control.
[0081] Figure 5 (a) is the etching result involved in Reference Example 3, Figure 5 (b) is the result of etching according to this embodiment. Figure 5In reference example 3 of (a), switching between the control methods of the APC position when etching the upper Ti film, when etching the Al film, and when etching the lower Ti film is controlled at predetermined timings. Figure 5 (a) shows the pressure P4 measured by the pressure gauge (CM2) 151 and the opening degree A4 of the pressure control valve 52 in Reference Example 3.
[0082] exist Figure 5 In (b), the control methods of the APC position are switched among when etching the upper Ti film, when etching the Al film, and when etching the lower Ti film by EPD control. Figure 5 (b) shows the pressure P5 measured by the pressure gauge (CM) 54 and the opening degree A5 of the pressure control valve 52 in this embodiment.
[0083] In addition, Figure 5 The process conditions for etching the upper Ti film, the Al film, and the lower Ti film in the experiment are the same. In addition, the control method of the APC position when etching the upper Ti film, etching the Al film, and etching the lower Ti film is as follows: Figure 4 As shown, the control method according to this embodiment is used.
[0084] As a result, in the case of reference example 3 in which the control method of controlling the APC position according to time is switched, as shown in FIG. Figure 5 As shown in the dotted frame of F1 in (a), the pressure P4 measured by the pressure gauge (CM2) 151 increases during the etching process of the Al film, and the pressure in the exhaust space and the processing chamber S becomes unstable.
[0085] On the other hand, in the case of the present embodiment in which the APC position control method is switched by EPD control, it is possible to switch from automatic control of the APC position when etching the upper Ti film to automatic control of the APC position when etching the Al film at the best timing. Similarly, it is possible to switch from automatic control of the APC position when etching the Al film to automatic control of the APC position when etching the lower Ti film at the best timing by EPD control. Figure 5 As shown in the dotted frame of F2 in (b), the pressure in the exhaust space and the processing chamber S can be stabilized.
[0086] [Application examples of other films]
[0087] In the etching method according to the present embodiment described above, the stacked film of the upper Ti film, the Al film, and the lower Ti film is used as the etching target film. However, the application range of the etching method according to the present embodiment is not limited to this. Figure 6 It is a diagram showing another film structure to which the etching method according to this embodiment is applied.
[0088] For example Figure 6As shown in (a), when a single Al film 1 is used as an etching target film and is etched through a mask 2 and the mask 2 contains carbon, the pressure control valve 52 vibrates during the etching of the Al film 1. As a result, Figure 6 As shown in (b), the pressure P in the processing chamber S vibrates. In view of this phenomenon, it is beneficial to apply the etching method according to this embodiment when etching the Al film 1.
[0089] Figure 6 (c) shows an example of the emission intensity I1 of Al with a wavelength of 396 nm and the emission intensity I2 of CCl with a wavelength of 278.8 nm among the emission intensities of the plasma detected by the emission spectrum analyzer 55. Figure 6 (b) and (c), when the pressure P is maximum, the luminescence intensity I1 of Al becomes the maximum peak, and the luminescence intensity I2 of CCl becomes the minimum peak. On the other hand, when the pressure P is minimum, the luminescence intensity I1 of Al becomes the minimum peak, and the luminescence intensity I2 of CCl becomes the maximum peak.
[0090] The reason for this phenomenon is that when the pressure P in the processing chamber S becomes higher, the Al film 1 is mainly etched, the etching rate of the Al film 1 increases, and the emission intensity I1 of Al becomes higher. On the other hand, when the pressure P in the processing chamber S becomes lower, the mask 2 is mainly etched, the etching rate of the mask 2 increases, and since the mask 2 contains carbon, the emission intensity I2 of CCl becomes higher. Therefore, the following phenomenon occurs: when the opening of the pressure control valve 52 is automatically controlled, the Al film 1 and the mask 2 are alternately etched in accordance with the periodic variation of the pressure P. The periodic variation of the pressure P is caused by the variation of the pressure caused by the progress of the etching itself in each of the etching of the Al film 1 and the etching of the mask 2.
[0091] In this case, during the etching of the Al film 1, the pressure control valve 52 is gradually opened or closed according to the pressure value from the state where the opening (APC position) of the pressure control valve 52 is set to the given initial value, similarly to the etching of the Al film between the upper Ti film and the lower Ti film. In this way, the pressure fluctuation in the processing chamber S can be suppressed, and the oscillation of the pressure control valve 52 can be prevented, thereby suppressing the generation of particles. The given initial value can be determined based on the results of, for example, preparatory etching performed in advance.
[0092] As described above, according to the etching method of this embodiment, the pressure in the processing chamber S can be stably controlled.
[0093] All aspects of the etching method and substrate processing device involved in the embodiments disclosed herein are illustrative and non-restrictive. The above embodiments can be modified and improved in various ways without departing from the scope of the claims and their main purpose. The matters described in the above multiple embodiments can also adopt other structures within the scope of non-contradiction, and the above matters can be combined within the scope of non-contradiction.
[0094] The substrate processing device disclosed in the present invention can also be applied as any type of device including atomic layer deposition (ALD: Atomic Layer Deposition) device, capacitively coupled plasma (CCP: Capacitively Coupled Plasma), inductively coupled plasma (ICP: Inductively Coupled Plasma), radial line slot antenna (RLSA: Radial Line Slot Antenna), electron cyclotron resonance plasma (ECR: Electron Cyclotron Resonance Plasma), and helicon wave plasma (HWP: Helicon Wave Plasma).
[0095] In addition, a plasma processing device is used as an example of a substrate processing device for explanation, but the substrate processing device is not limited to a plasma processing device as long as it is a device that performs a predetermined process (such as a film forming process, an etching process, etc.) on a substrate. When plasma is not used in etching, the etching process of Al may be controlled by incident probe light and monitoring the absorption rate instead of monitoring plasma light emission in EPD control.
Claims
1. An etching method, It is characterized in that Including the following processes: Step (a), placing a substrate having a stacked film formed thereon in a processing chamber, the stacked film having a first titanium film and an aluminum film located below the first titanium film; Step (b), etching the first titanium film by means of a mask made of an organic material while automatically controlling the opening of the pressure control valve in accordance with changes in pressure in the processing chamber connected to the exhaust device through an exhaust pipe via the pressure control valve or in accordance with changes in pressure in the exhaust pipe; Step (c), calculating a first opening value according to the value of the opening of the pressure control valve sampled in step (b); Step (d), setting the opening of the pressure control valve to the first opening value when etching the aluminum film begins, so as to etch the aluminum film; as well as step (e), monitoring the pressure in the step (d), and changing the first opening value to a second opening value by a predetermined change amount when the pressure exceeds a predetermined threshold value, The etching method includes step (f), in which step (e) is performed one or more times until the etching of the aluminum film is completed.
2. The etching method according to claim 1, It is characterized in that In the step (d), the pressure is the pressure in the exhaust pipe near the pressure control valve, and the pressure is measured on the upstream side of the pressure control valve.
3. The etching method according to claim 1 or 2, It is characterized in that The etching in the step (b) and the etching in the step (d) are performed by converting the chlorine-containing gas into plasma.
4. The etching method according to claim 1 or 2, It is characterized in that In the step (c), the first opening value is calculated based on a plurality of opening values of the pressure control valves, including the opening value of the pressure control valve last sampled in the step (b).
5. The etching method according to claim 1 or 2, It is characterized in that In the step (d), when etching of the aluminum film starts, the opening of the pressure control valve is set to a value obtained by adding a predetermined offset value to the first opening value.
6. The etching method according to claim 1 or 2, It is characterized in that The stacked film has a second titanium film under the aluminum film. The etching method further includes a step (g) of etching the second titanium film while automatically controlling the opening of the pressure control valve in accordance with changes in the pressure in the processing chamber or the exhaust pipe after the step (f).
7. The etching method according to claim 6, It is characterized in that The method further comprises a step (h), in which the light emission intensity of the plasma in the processing chamber is measured. The etching process is switched from the step (b) to the step (d), and the etching process is switched from the step (d) to the step (g) based on the emission intensity of the plasma.
8. A substrate processing device, comprising: a processing chamber in which a substrate is arranged; an exhaust device connected to the processing chamber via a pressure control valve and an exhaust pipe; a pressure gauge for measuring the pressure in the processing chamber or the exhaust pipe; and a control unit, wherein the substrate processing device is characterized in that: The control unit controls the following processes: Step (a), placing a substrate having a stacked film formed thereon in the processing chamber, the stacked film having a first titanium film and an aluminum film located below the first titanium film; Step (b) of etching the first titanium film through a mask made of an organic material while automatically controlling the opening of the pressure control valve in accordance with a change in the pressure in the processing chamber or in the exhaust pipe measured by the pressure gauge; Step (c), calculating a first opening value according to the value of the opening of the pressure control valve sampled in step (b); Step (d), setting the opening of the pressure control valve to the first opening value when etching the aluminum film begins, so as to etch the aluminum film; step (e), monitoring the pressure in the step (d), and changing the first opening value to a second opening value by a predetermined change amount when the pressure exceeds a predetermined threshold value, The control unit further controls step (f) so that in step (f), step (e) is performed one or more times until etching of the aluminum film is completed.
Citation Information
Patent Citations
Plasma etching method
JP2018041890A
Manufacturing a micro-system by deep reactive-ion etching, comprises e.g.: providing an etching tool for deep reactive-ion etching, carrying out multiple repeating-processing intervals of the deep ion etching including an etching step
DE102012202611A1
Plasma processing method, and plasma processing device
JP2012151325A
Method and apparatus for process control in time division multiplexed (TDM) etch processes
US20050263485A1