Evaluation method based on water vapor diffusion coefficient in asphalt mixture pores
By calculating the absorption content and mineral gap ratio of the asphalt mixture, combined with the aggregate stacking model and the Nussen diffusion formula, the problem of the inability to accurately calculate the pore diffusion coefficient of water gas in the asphalt mixture in the prior art is solved, and the problem of the inability to accurately calculate the pore diffusion coefficient of water gas in the asphalt mixture is achieved. Quantitative evaluation of the movement laws of water gas helps avoid water damage from asphalt mixture.
Patent Information
- Application Number
- CN202111334691.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-11
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2041-11-11
AI Technical Summary
The prior art lacks an effective evaluation method for the internal water gas movement laws of asphalt mixture, and it is difficult to accurately calculate the pore diffusion coefficient of water gas inside the asphalt mixture, resulting in the inability to effectively analyze the water damage caused by the movement of water gas.
By preparing asphalt mixture and placing it in a water gas environment, the content percentage of absorbed asphalt and mineral gap ratio are calculated, the relationship between the gap volume and the thickness of the asphalt film is established, and the water gas is calculated based on the aggregate stacking model and the Nussen diffusion formula. Pore diffusion coefficient inside the asphalt mixture.
The quantitative evaluation of the degree of diffusion of water gas inside the asphalt mixture is achieved, and the quantitative evaluation of the movement laws of water gas under different oil and stone ratios can be carried out, providing a direction to avoid water damage to asphalt mixture.
Smart Images

Figure CN113919182B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of road construction, in particular to an evaluation method based on the diffusion coefficient of water vapor in the pores of asphalt mixture. Background Art
[0002] At present, the diffusion of water vapor inside asphalt pavement is one of the factors causing water damage to pavement. The water vapor diffusion coefficient inside asphalt mixture can reflect the diffusion rate of water vapor in the mixture. The water vapor diffusion coefficient directly affects the internal relative humidity distribution law of asphalt mixture during service and the length of time required to reach the humidity equilibrium state. Therefore, determining the water vapor diffusion coefficient inside asphalt mixture is of great significance for analyzing the water damage caused by water vapor movement. At present, when studying the diffusion of water vapor inside asphalt mixture, asphalt mixture is mainly regarded as a single homogeneous material, and the diffusion coefficient is solved according to Fick's first law. Since asphalt mixture is a typical composite material composed of three materials: asphalt, aggregate, and air, its internal structure is complex, which makes the diffusion coefficient solved according to Fick's first law actually the effective diffusion coefficient and the effective diffusion path. When the diffusion coefficient of each basic material in the composite material is not in the same order of magnitude, the diffusion coefficient is related to the internal structure of the medium. At this time, the effective diffusion is different from the actual diffusion coefficient in the medium. It is found through experimental calculation that the actual diffusion coefficient of asphalt mixture is more than 2000 times the effective diffusion coefficient. Therefore, the effective diffusion coefficient of asphalt mixture cannot reflect the actual situation inside the asphalt mixture.
[0003] In order to study the actual diffusion coefficient and the actual effective diffusion path of asphalt mixture, the water vapor diffusion coefficient of the basic materials in the asphalt mixture should be tested separately. At present, the methods for testing and calculating the water vapor diffusion coefficient of asphalt and aggregate are relatively mature, but there are few methods for determining the diffusion coefficient of internal pores. The internal pores of asphalt mixture are important channels for water vapor movement, and the influence of internal pores on the water vapor movement of asphalt mixture cannot be ignored. However, the structure of the internal pores of asphalt mixture is complex, and it is difficult to directly measure the diffusion coefficient of water vapor in the internal pores of asphalt mixture through experiments. The existing technology lacks a method for calculating the diffusion coefficient of water vapor in the internal pores of asphalt mixture, making it difficult to effectively evaluate the movement law of water vapor in asphalt mixture. Therefore, it is necessary to propose a new method to effectively evaluate the movement law of water vapor in asphalt mixture. Summary of the invention
[0004] The purpose of the present invention is to provide an evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture, so as to solve the problem that the prior art lacks an effective method for evaluating the movement law of water vapor in asphalt mixture.
[0005] In order to solve the above technical problems, the present invention provides an evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture, the steps of which include:
[0006] (1) Prepare an asphalt mixture and place it in a water-vapor environment, and calculate the percentage of absorbed asphalt in the asphalt mixture and the mineral void ratio;
[0007] (2) absorbing asphalt to coat the surface of aggregate particles and form an asphalt film, establishing a first functional relationship between the internal gap volume of the asphalt mixture and the asphalt film thickness, and obtaining the value of the asphalt film thickness;
[0008] (3) performing differential processing on the asphalt film thickness based on the first functional relationship to obtain a second functional relationship between the internal gap surface area of the asphalt mixture and the asphalt film thickness;
[0009] (4) Establishing an aggregate stacking model, based on which a third functional relationship between the internal void volume, void surface area, and average radius of the model pores is obtained;
[0010] (5) Based on the first functional relationship, the second functional relationship and the third functional relationship, a fourth functional relationship between the average radius of the model pores and the thickness of the asphalt film is obtained;
[0011] (6) Based on the Knudsen diffusion formula and the relationship between asphalt film thickness and the fourth function, calculate the diffusion coefficient of water vapor in the pores of asphalt mixture;
[0012] (7) The water vapor diffusion coefficient in the pores of asphalt mixture is used to evaluate the movement law of water vapor in asphalt mixtures with different oil-stone ratios.
[0013] Furthermore, in step (1), based on the fact that the sum of the effective volume of the aggregate and the volume of the absorbed asphalt is equal to the gross volume of the aggregate, the calculation formula for the percentage content P of the absorbed asphalt is:
[0014] P=(G se -G sb ) / (G se ×G sb )×G b
[0015] Among them, G sb G is the relative density of aggregate bulk volume, dimensionless; b is the relative density of asphalt, dimensionless; G se is the effective relative density of aggregate, the effective relative density of aggregate G se The calculation formula is:
[0016]
[0017] Among them, Gf is the relative density of the specimen’s gross volume, dimensionless; P b is the percentage value of the total asphalt content in the asphalt mixture, and P b % is the percentage of total asphalt content in asphalt mixture.
[0018] Furthermore, in step (1), the calculation formula of the mineral material void ratio VMA is:
[0019] VMA=(1-G f / G sb ×P s / 100)×100
[0020] Among them, P s is the percentage of aggregate in the total mass of asphalt mixture, and P s =100-P b .
[0021] Furthermore, in step (2), the expression of the first functional relationship is:
[0022] e v (t) = (1-φ)exp[-(α1t+α2t 2 +α3t 3 )]
[0023] Among them, e v (t) is the internal void volume of the asphalt mixture, α1, α2, α3 represent the geometric characteristics of aggregate particles in the asphalt mixture, and are calculated by the following formulas: m1 is the average value of aggregate particle diameter, m2 is the average value of square of aggregate particle diameter, and m3 is the average value of cube of aggregate particle diameter, and the average calculation method is based on the number of aggregate particles; q satisfies the relationship φ is a function of the aggregate volume greater than the asphalt film thickness.
[0024] The expression of φ is:
[0025] φ=(1-VMA)(1-P d )
[0026] Among them, P d It represents the volume percentage of aggregate smaller than the thickness of the asphalt film, satisfying the relationship P 0.075 Indicates the passing rate through a 200-mesh sieve.
[0027] Furthermore, in step (2), the internal gap volume of the asphalt mixture is v (t) also satisfies the relationship:
[0028]
[0029] This formula is combined with the expression of the first functional relationship to obtain the relationship:
[0030] α1t+α2t 2 +α3t 3 =ln[(1-φ) / e v (t)]
[0031] And solve the value of asphalt film thickness.
[0032] Furthermore, in step (3), the expression of the second functional relationship is:
[0033]
[0034] Where S(t) represents the internal gap surface area of asphalt mixture.
[0035] Furthermore, in step (4), the aggregate stacking model is as follows: each aggregate particle is a cylindrical unit, a number of aggregate particles are stacked and arranged, model pores are formed between adjacent cylindrical units, and asphalt is filled in the model pores to form an asphalt mixture; the inner wall surface area of the model pores is equivalent to the internal gap surface area of the asphalt mixture, and the expression of the inner wall surface area of the model pores is: The model pore volume is equivalent to the internal gap volume of asphalt mixture. The expression of the model pore volume is: in, represents the average radius of the model pores, h represents the length of the cylindrical unit, and n represents the number of cylindrical units. Based on the expressions of the inner wall surface area of the model pores and the model pore volume, the expression of the third functional relationship is obtained as follows:
[0036] Furthermore, in step (5), based on the first functional relationship, the second functional relationship and the third functional relationship, the expression of the fourth functional relationship is obtained as follows:
[0037] Furthermore, in step (6), the Knudsen diffusion formula is:
[0038]
[0039] Among them, D t Indicates the diffusion coefficient of water vapor in the pores of asphalt mixture; D m It represents the diffusion coefficient of water vapor in the air. At normal temperature and pressure, the diffusion coefficient is about 0.26cm 2 / s;D K represents the Knudsen diffusion coefficient, which satisfies the relationship:
[0040]
[0041] in, represents the average pore radius, and R represents the molar gas constant, which is 8.314 j·mol -1 ·k -1 , M represents the molar mass of the molecule; based on the Knudsen diffusion formula, asphalt film thickness and the fourth function relationship, the pore diffusion coefficient of water vapor in the asphalt mixture is calculated.
[0042] The beneficial effects of the present invention are as follows: Different from the prior art, the present invention provides an evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture. By establishing an aggregate stacking model, the actual values of the internal gap parameters of the asphalt mixture are associated with the theoretical model, and combined with the Knudsen diffusion formula, a calculation method for the pore diffusion coefficient of water vapor in the asphalt mixture is obtained, thereby realizing the quantification of the diffusion degree of water vapor in the asphalt mixture, thereby being able to quantitatively evaluate the movement law of water vapor in the asphalt mixture under different oil-stone ratios, and pointing out the direction for avoiding the occurrence of water damage in asphalt mixtures. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 It is a flow chart of the evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture in the present invention;
[0044] Figure 2 It is a schematic diagram of the cross-sectional structure of the aggregate stacking model in the evaluation method based on the diffusion coefficient of water vapor in the pores of asphalt mixture according to the present invention. DETAILED DESCRIPTION
[0045] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] See also Figure 1 The evaluation method of the water vapor diffusion coefficient in the internal pores of asphalt mixture in the present invention comprises the following steps:
[0047] S1, prepare asphalt mixture and place it in a water vapor environment, calculate the percentage of absorbed asphalt in the asphalt mixture and the mineral gap ratio. In this step, the percentage of absorbed asphalt in the asphalt mixture and the mineral gap ratio are calculated. Since the sum of the effective volume of the aggregate and the volume of absorbed asphalt is equal to the gross volume of the aggregate, the calculation formula for the percentage of absorbed asphalt P is:
[0048] P=(G se -G sb) / (G se ×G sb )×G b (1)
[0049] (1) In the formula, G sb G is the relative density of aggregate bulk volume, dimensionless; b is the relative density of asphalt, dimensionless; G se is the effective relative density of aggregate, the effective relative density of aggregate G se The calculation formula is:
[0050]
[0051] (2) In the formula, G f is the relative density of the specimen’s gross volume, dimensionless; P b is the percentage value of the total asphalt content in the asphalt mixture, and P b % is the percentage of total asphalt content in asphalt mixture.
[0052] On the other hand, the calculation formula of the mineral void ratio VMA is:
[0053] VMA=(1-G f / G sb ×P s / 100)×100 (3)
[0054] Among them, P s is the percentage of aggregate in the total mass of asphalt mixture, and P s =100-P b .
[0055] S2, absorb asphalt to coat the surface of aggregate particles and form an asphalt film, establish a first functional relationship between the internal gap volume of the asphalt mixture and the asphalt film thickness, and obtain the value of the asphalt film thickness. In this step, the expression of the first functional relationship is:
[0056] e v (t) = (1-φ)exp[-(α1t+α2t 2 +α3t 3 )] (4)
[0057] (4) In the formula, e v (t) is the internal void volume of the asphalt mixture, α1, α2, α3 represent the geometric characteristics of aggregate particles in the asphalt mixture, and are calculated by the following formulas: m1 is the average value of aggregate particle diameter, m2 is the average value of square of aggregate particle diameter, and m3 is the average value of cube of aggregate particle diameter. The average is calculated based on the number of aggregate particles, not the mass ratio of aggregates. q satisfies the relationship φ is the function of the aggregate volume greater than the thickness of the asphalt film. The expression of φ is:
[0058] φ=(1-VMA)(1-P d ) (5)
[0059] (5) In the formula, P d It represents the volume percentage of aggregate smaller than the thickness of the asphalt film, satisfying the relationship P 0.075 Indicates the passing rate through a 200-mesh sieve.
[0060] On the other hand, the internal void volume of asphalt mixture e v (t) also satisfies the relationship:
[0061]
[0062] Combining equation (6) with equation (4) yields the following relationship:
[0063] α1t+α2t 2 +α3t 3 =ln[(1-φ) / e v (t)] (7)
[0064] The real root t of the equation group can be solved by equation (7), which is the value of the asphalt film thickness. It should be noted that the above equations (4) to (6) specifically refer to the document "Analytical Formulas for Film Thickness in Compacted Asphalt Mixture". The meanings and calculation processes of the relevant parameters have been recorded in detail in the corresponding document and will not be repeated here.
[0065] S3, based on the first functional relationship, the asphalt film thickness is differentiated to obtain a second functional relationship between the internal gap surface area of the asphalt mixture and the asphalt film thickness. In this step, the asphalt film thickness t is differentiated based on formula (7), and the expression of the obtained second functional relationship is:
[0066]
[0067] In formula (8), since it is the differentiation of thickness, S(t) represents the internal gap surface area of asphalt mixture.
[0068] S4, establish an aggregate stacking model, and obtain a third functional relationship between the internal gap volume, gap surface area and average radius of model pores of the asphalt mixture based on the aggregate stacking model. Figure 2 As shown, Figure 2 is a schematic diagram of the cross-sectional structure of the aggregate stacking model. The established aggregate stacking model is as follows: each aggregate particle is designed as a cylindrical unit, and a number of aggregate particles are stacked and arranged. Model pores are formed between adjacent cylindrical units, and asphalt is filled in the model pores to form an asphalt mixture; the inner wall surface area of the model pores is equivalent to the internal gap surface area of the asphalt mixture, and the expression of the inner wall surface area of the model pores is:
[0069]
[0070] The model pore volume is equivalent to the internal gap volume of asphalt mixture. The expression of the model pore volume is:
[0071]
[0072] in, represents the average radius of the model pores, h represents the length of the cylindrical unit, and n represents the number of cylindrical units. Based on the inner wall surface area of the model pores (9) and the model pore volume (10), the expression of the third functional relationship is obtained as follows:
[0073]
[0074] S5, based on the first functional relationship, the second functional relationship and the third functional relationship, obtain the fourth functional relationship between the average radius of the model pores and the thickness of the asphalt film. In this step, since the first functional relationship and the second functional relationship represent the actual values of the internal gap volume and gap surface area of the asphalt mixture, and the third functional relationship represents the theoretical model relationship between the internal gap volume and gap surface area of the asphalt mixture, the first functional relationship, the second functional relationship and the third functional relationship are combined to link the actual value with the theoretical model, thereby obtaining the average radius of the model pores The functional relationship between t and the asphalt film thickness; By combining equations (4), (8) and (11), the expression of the fourth functional relationship is obtained as follows:
[0075]
[0076] S6, based on the Knudsen diffusion formula, asphalt film thickness, and the fourth function relationship, calculate the diffusion coefficient of water vapor in the pores of the asphalt mixture. In this step, the Knudsen diffusion formula is:
[0077]
[0078] (13) Where Dt Indicates the diffusion coefficient of water vapor in the pores of asphalt mixture; D m It represents the diffusion coefficient of water vapor in the air. At normal temperature and pressure, the diffusion coefficient is about 0.26cm 2 / s;D K represents the Knudsen diffusion coefficient, which satisfies the relationship:
[0079]
[0080] (14) In the formula, represents the average pore radius, and R represents the molar gas constant, which is 8.314 j·mol -1 ·k -1 , M represents the molar mass of the molecule; Based on the Knudsen diffusion formula and the relationship between the thickness of the asphalt film and the fourth function, (12) is substituted into the above Knudsen diffusion formula to obtain the diffusion coefficient D of water vapor in the pores of the asphalt mixture. t The functional relationship between the asphalt film thickness t and the asphalt film thickness t is such that the water vapor diffusion coefficient in the pores of the asphalt mixture can be calculated from the asphalt film thickness t.
[0081] S7, using the pore diffusion coefficient of water vapor in asphalt mixture to evaluate the movement law of water vapor in asphalt mixture with different oil-stone ratios. In this step, since the pore diffusion coefficient of water vapor in asphalt mixture is obtained in the above step S6, the degree of diffusion of water vapor in asphalt mixture is quantified; and through experiments, it is determined that there is a certain change law between the pore diffusion coefficient of water vapor in asphalt mixture and the oil-stone ratio, so the movement law of water vapor in asphalt mixture with different oil-stone ratios can be quantitatively evaluated. Furthermore, it can also provide conditions for exploring the influence of the movement state of water vapor in asphalt mixture on the performance of asphalt mixture, and point out the direction for avoiding the occurrence of water damage in asphalt mixture.
[0082] The following is a detailed description of the embodiment of the method for evaluating the diffusion coefficient of water vapor in the pores of asphalt mixture in the present invention through specific embodiments.
[0083] Example 1
[0084] In this embodiment, the test uses limestone from Fang County, Hubei Province as the experimental ore. According to different grading curves, 5 groups of molding specimens are prepared according to the oil-stone ratio of 3.5, 4.0, 4.3, 4.5, and 5.0. The specific passing rate of each grade of aggregate is shown in Table 1, and the volume index is shown in Table 2.
[0085] Table 1 HMA specimen gradation
[0086]
[0087] Table 2 Apparent relative density and bulk relative density of aggregates of various grades
[0088]
[0089] According to the asphalt mixture specimens with different oil-to-stone ratios of 3.5, 4.0, 4.3, 4.5 and 5.0, the model pore radius of the asphalt mixture specimens with different oil-to-stone ratios was calculated according to the steps described in the aforementioned evaluation method based on the pore diffusion coefficient of water vapor in the asphalt mixture. The calculation results are shown in Table 3. Then, according to the aforementioned formulas (13) and (14), the pore diffusion coefficient of water vapor in the asphalt mixture was calculated. The calculation results are shown in Table 4.
[0090] Table 3 Model pore radius of asphalt mixture specimens with different asphalt-aggregate ratios
[0091]
[0092]
[0093] Table 4 Diffusion coefficient of water vapor in asphalt mixtures with different oil-to-stone ratios
[0094] Oil-stone ratio <![CDATA[Internal diffusion coefficient (cm 2 / s)]]> 3.5 0.200 4.0 0.203 4.3 0.204 4.5 0.201 5.0 0.197
[0095] From the data in Table 3 and Table 4, it can be seen that the thickness of the asphalt film increases with the increase of the oil-stone ratio, but the model pore radius shows a trend of first increasing and then decreasing with the increase of the oil-stone ratio. This shows that for asphalt mixtures, there is an oil-stone ratio corresponding to the maximum internal model pore radius; and with the increase of the oil-stone ratio, the diffusion coefficient of water vapor in the asphalt mixture also shows a trend of first increasing and then decreasing, which also shows that there is an oil-stone ratio that maximizes the internal diffusion coefficient. In practical applications, considering the avoidance of water damage, the oil-stone ratio corresponding to the maximum internal diffusion coefficient can be used as a reference value, and the diffusion degree of water vapor in the asphalt mixture under different oil-stone ratios can be quantitatively compared, and the actual selection of the oil-stone ratio close to the reference value can be avoided as much as possible, thereby reducing the impact of internal water vapor diffusion.
[0096] In addition, in the actual experiment, under different asphalt film conditions, the influence degree between the model pore radius of the asphalt mixture and the asphalt film thickness is different. Specifically, when the asphalt film is small, the model pore radius in the asphalt mixture is mainly affected by the gradation of the mineral aggregate, so the change of the model pore radius with the thickness of the asphalt film is not obvious; when the asphalt film is large, the aggregate wrapped by the asphalt film increases, and the size of the model pore radius of the asphalt mixture is mainly affected by the thickness of the oil film, so the model pore radius decreases very significantly with the increase of the asphalt film thickness.
[0097] Different from the prior art, the present invention provides an evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture. By establishing an aggregate stacking model, the actual values of the internal gap parameters of the asphalt mixture are associated with the theoretical model, and combined with the Knudsen diffusion formula, a calculation method for the pore diffusion coefficient of water vapor in the asphalt mixture is obtained, thereby realizing the quantification of the diffusion degree of water vapor in the asphalt mixture. Therefore, the movement law of water vapor in the asphalt mixture under different oil-stone ratios can be quantitatively evaluated, and a direction for avoiding the occurrence of water damage in asphalt mixture is pointed out.
[0098] The above-mentioned embodiments only express the implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. An evaluation method based on the pore diffusion coefficient of water vapor in asphalt mixture, characterized in that: The steps include: (1) Prepare asphalt mixture and place it in a water-gas environment, and calculate the percentage of absorbed asphalt in the asphalt mixture and the void ratio of the mineral aggregate; (2) The absorption asphalt coats the surface of aggregate particles and forms an asphalt film, a first functional relationship between the internal gap volume of the asphalt mixture and the thickness of the asphalt film is established, and a value of the asphalt film thickness is obtained; (3) performing a differential process on the asphalt film thickness based on the first functional relationship to obtain a second functional relationship between the internal gap surface area of the asphalt mixture and the asphalt film thickness; (4) establishing an aggregate stacking model, and obtaining a third functional relationship between the internal gap volume, gap surface area and average radius of model pores of the asphalt mixture based on the aggregate stacking model; (5) Based on the first functional relationship, the second functional relationship and the third functional relationship, a fourth functional relationship between the average radius of the pores in the model and the thickness of the asphalt film is obtained; (6) Calculating the diffusion coefficient of water vapor in the pores of the asphalt mixture based on the Knudsen diffusion formula, the asphalt film thickness, and the fourth functional relationship; (7) Using the water vapor pore diffusion coefficient in asphalt mixture to evaluate the water vapor movement law in asphalt mixtures with different asphalt-aggregate ratios; In the step (1), based on the fact that the sum of the effective volume of the aggregate and the volume of the absorbed asphalt is equal to the gross volume of the aggregate, the calculation formula for the percentage content P of the absorbed asphalt is: in, G sb is the relative density of aggregate bulk volume, dimensionless; G b is the relative density of asphalt, dimensionless; G se is the effective relative density of the aggregate, the effective relative density of the aggregate G se The calculation formula is: in, G f is the relative density of the specimen’s gross volume, dimensionless; P b is the percentage value of the total asphalt content in the asphalt mixture, and P b % is the percentage of total asphalt content in asphalt mixture; In the step (1), the calculation formula of the mineral material void ratio VMA is: in, P s is the percentage of aggregate in the total mass of asphalt mixture, and P s =100- P b ; In the step (2), the expression of the first functional relationship is: in, is the internal void volume of the asphalt mixture, α 1. α 2. α 3 represents the geometric characteristics of aggregate particles in asphalt mixture, which are calculated by the following formulas: , , ; m 1 is the average diameter of aggregate particles, m 2 is the average value of the square of aggregate particle diameter, m 3 is the average value of the cube of the aggregate particle diameter, and is calculated based on the number of aggregate particles; q Satisfy the relationship , ϕ is a function of the volume of aggregate greater than the thickness of the asphalt film; Said ϕ The expression is: in, P d It represents the volume percentage of aggregate smaller than the thickness of the asphalt film, satisfying the relationship , Indicates the passing rate through a 200-mesh sieve; In step (2), the internal gap volume of the asphalt mixture It also satisfies the relationship: This formula is combined with the expression of the first functional relationship to obtain the relationship: And solve to obtain the value of the asphalt film thickness; In step (3), the expression of the second functional relationship is: in, It represents the internal interstitial surface area of asphalt mixture; In step (4), the aggregate stacking model is as follows: each aggregate particle is a cylindrical unit, a plurality of aggregate particles are stacked and arranged, model pores are formed between adjacent cylindrical units, and asphalt is used to fill the model pores to form an asphalt mixture; The inner wall surface area of the model pores is equivalent to the internal gap surface area of the asphalt mixture. The expression of the inner wall surface area of the model pores is: ; The model pore volume is equivalent to the internal gap volume of the asphalt mixture, and the expression of the model pore volume is: ,in, represents the average radius of the model pores, h represents the length of the cylindrical unit, and n represents the number of cylindrical units; Based on the expressions of the inner wall surface area of the model pore and the model pore volume, the expression of the third functional relationship is obtained as follows: ; In the step (5), based on the first functional relationship, the second functional relationship and the third functional relationship, the expression of the fourth functional relationship is obtained as follows: ; In step (6), the Knudsen diffusion formula is: in, It represents the diffusion coefficient of water vapor in the pores of asphalt mixture; It represents the diffusion coefficient of water vapor in air; represents the Knudsen diffusion coefficient, which satisfies the relationship: in, represents the average pore radius, represents the molar gas constant, which is 8.314 j·mol -1 ·k -1 , It represents the molar mass of a molecule; Based on the Knudsen diffusion formula, the asphalt film thickness, and the fourth functional relationship, the diffusion coefficient of water vapor in the pores of the asphalt mixture is calculated.
Citation Information
Patent Citations
Method for determining water vapor motion parameters of road asphalt mixture
CN110595935A
Asphalt mixture water-gas motion parameter calculation method, storage medium and system