A simple method for electrosynthesis of graphene from CO2

By electrolyzing CO2 in molten carbonate, combining electrochemical peeling and transition metal nucleation inhibition technology, the problems of high cost and high carbon footprint of graphene are solved, and graphene production with low cost and low carbon footprint are achieved, which improves the Yield and purity.

CN113924269BActive Publication Date: 2024-11-29C2CNT LLC
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202080039399.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-05-28
Publication Date
2024-11-29
Estimated Expiration
2040-05-28

AI Technical Summary

Technical Problem

The existing high cost and high carbon footprint production methods of graphene limit their wide application and are difficult to achieve low-cost, low-carbon footprint graphene synthesis.

Method used

By electrolysis in molten carbonate, CO2 is used as the only reactant, graphene is generated by electrochemical peeling method, and transition metal nucleation inhibition technology is used to promote the growth of carbon nanomaterials to form high-yield graphene.

Benefits of technology

The low-cost, low-carbon footprint graphene production has been achieved, which improves the yield and purity of graphene, reduces greenhouse gas emissions, and provides the possibility of large-scale synthesis of graphene.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113924269B_ABST
    Figure CN113924269B_ABST
Patent Text Reader

Abstract

The present invention relates to the production of graphene from CO2 by electrolysis and stripping processes. One embodiment is a method for producing graphene, comprising (i) electrolysis between an electrolysis anode and an electrolysis cathode in a molten carbonate electrolyte to generate a carbon nanomaterial on the cathode, and (ii) electrochemically stripping the carbon nanomaterial from a second anode to produce graphene. Compared with thicker conventional graphite stripping reactions, the stripping step produces graphene in high yield. CO2 can be the only reactant for producing a valuable product as graphene. This can promote the utilization of CO2, and unlike alternative products made from CO2 such as carbon monoxide or other fuels such as methane, the use of graphene products will not release this greenhouse gas back into the atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims the benefit of U.S. Provisional Application No. 62,938,135, filed on November 20, 2019, U.S. Provisional Application No. 62 / 890,719, filed on August 23, 2019, and U.S. Provisional Application No. 62 / 853,473, filed on May 28, 2019, the entire contents of each of which are incorporated herein by reference. Field of the Invention

[0003] The present invention relates to the production of graphene from CO2 by an electrolysis and exfoliation process. The exfoliation step produces graphene in high yields compared to thicker conventional graphite exfoliation reactions. CO2 can be the only reactant used to produce a valuable product as graphene. This can facilitate the utilization of CO2, and unlike alternative products made from CO2 (such as carbon monoxide) or other fuels (such as methane), the use of graphene products does not release this greenhouse gas back into the atmosphere. Background of the Invention

[0005] Graphene has unique properties that can be used in a variety of applications. However, the cost of synthesis and the difficulty in isolating the graphene product of its natural two-dimensional structure lead to a high current cost of graphene, which is valued at about $1 million per ton. See Price and Market of Materials, Carbon XPrize Standards Data Summary Set, Draft V1.2, (Sept. 12, 2017)).

[0006] Graphene has high surface area, high thermal and electrical conductivity, strength, surface tailorability, and high charge carrier conductivity, which makes it uniquely suitable for energy storage devices and electronic devices. See, e.g., et al., Front. Mat. Sci., 2019, 13, 23; Agudosi et al., Crit. Rev. Mat. Sci., 2019, 1040-8436, 1; Bai et al., Electrochem. Energy Rev., 2019, doi.org / 10.1007 / s41918-019-00042-6; and Zhang et al., Adv. Sci., 2017, 1700087, 4.

[0007] Graphene's ability to carry plasmons allows it to interact strongly with light in a nonlinear manner and act as both a transducer and a transmitter in optoelectronic devices. 2The crystal structure has an extremely high intrinsic charge mobility (250,000cm 2 / Vs), high specific surface area (2630m 2 / g), high thermal conductivity (5000 W / mK), high Young's modulus (1.0 TPa) and high optical transmittance (97.7%).

[0008] Methods for producing graphene include thermal annealing (see, e.g., Li et al., J. Nanomat., 2011, 319624), pulling nanotubes (see, e.g., Tanaka et al., Sci. Rep., 2015, 5, 12341), solvothermal and thermal decomposition (see, e.g., Singh et al., Int. J. Nanosci., 10, 39; Berger et al., J. Phys. Chem. B, 2004, 108, 19912), ball milling and chemical exfoliation (see, e.g., Del Tio-Castillo et al., Nano Res., 2014, 7, 963; Liu et al., Chem. Eng. J., 2019, 355, 181) and chemical vapor deposition (CVD) (see, for example, Shukla et al., Appl. Phys. Rev., 2019, 6, 021331; Azam et al., ECS J Solid State Science Technology, 2017 6(6)M3035; Lee et al., RSC Adv, 2017, 7, 15644; and Zhang et al., Adv. Sci., 2017, 1700087, 4).

[0009] Chemical vapor deposition (CVD) is a popular method for producing graphene using transition metal catalysts from a variety of organometallic compounds or other carbon sources. However, conventional CVD can have a huge carbon footprint of more than 600 tons of CO2 per ton of nanocarbon produced (see, e.g., Khanna et al., J. Ind. Ecology, 2008, 12, 394).

[0010] In a 2003 paper investigating processes detrimental to lithium-ion battery anodes, it was noted that electrochemical alkali ion insertion can cause layers to peel off from graphite anodes (see, e.g., Buqa et al., US DOE Tech Rep, 2003, 63; see also Spahr et al., J. Electrochem. Soc., 151, 2004, 181).

[0011] In 2007, it was discovered that single-atom-thick graphene layers were observed by electrochemical exfoliation (see, for example, Penicaud et al., Compos. Sci. Technol., 67, 2007, 795; Mansour et al., Carbon, 45, 2007, 1651; and Valles et al., J. Am. Chem. Soc., 130, 2008, 15802).

[0012] Electrochemically exfoliated graphene prepared from graphite has received increasing attention today and is often mechanistically explained as an anodic process in which intercalated ions between graphite layers are oxidized to form gases that break the weak interlayer van der Waals bonds and release thin monolayer or multilayer graphene sheets into the electrolyte (see, e.g., Hashimoto et al., Electrochem. Comm., 104, 2019, 106475; Xia et al., Nanoscale, 11, 2019, 5265; Bakunin et al., Inorg. Mat.: Appl. Res., 10, 2019, 249; and Khahpour et al., Appl. Energy Mat., 2, 2019, 4813). In 2017, it was observed that compressing graphite sheets before exfoliation, for example using graphite powder confined by a wax coating, increases the yield of graphene (see, for example, Wang et al., Appl. Mat. Interfaces, 9, 2017, 34456).

[0013] Low carbon footprint carbon nanomaterials can be produced by electrolysis of molten carbonates, at low cost and using CO2 as a reactant, such as C2CNT (CO2 to carbon nanotube) synthesis. However, technical challenges have prevented the amplification of the process, and nanomaterials are still insufficient. Although the examples of carbon nanotubes (CNTs) prepared by C2CNT synthesis are referred to as "straight", each example of the synthetic, grouped CNTs shown is clearly entangled, and twisted or hooked, but less twisted than the CNTs marked as "entangled". Entangled and twisted CNTs tend to agglomerate, so it is difficult to evenly disperse them in composite materials. In the examples of C2CNT synthesis, "straight" specifically refers to containing less sp between carbon defects. 3 bonded CNTs, and the “entangled” CNTs contain more sp 3defect. Exemplary methods for producing carbon nanomaterials from molten carbonates by electrolysis are disclosed in, for example, Licht et al., J. CO2 Utilization, 2017, vol. 18, 335-344; Nano Lett., 2015, vol. 15, 6142-6148; Materials Today Energy, 2017, 230-236; Data in Brief, 2017, vol. 14, 592-606; Scientific Reports, Nature, 2016, vol. 6, 1-10; ACSCent. Sci., 2015, vol. 2, 162-168; RSC Adv., 2016, vol. 6, 27191-27196; Carbon, 2016, vol. 106, 208-217; Energy Convers. Manag., 2016, vol. 122, 400-410; J. CO2 Utilization, 2017, vol. 18, 378–389; J. CO2 Utilization, 2017, vol. 18, 335–344; J. Phys. Chem. Lett., . 2010, vol. 1, 2363–2368; J. Phys. Chem. C, 2009, vol. 113, 16283-16292; J. CO2 Utilization, 2019, vol. 34, 303-312; Adv. Sustainable Syst., 2019, vol. 3, 1900056; and Mater. Today Sustainability, 2019, vol. 6, 100023; U.S. Patent Nos. 9,758,881 and 9,683,297, U.S. Publication No. 2019 / 36040, and WO International Publication No. 16 / 138469, International Publication No. WO 18 / 093942 and International Publication No. WO 18 / 156642.

[0014] However, there remains a need for a convenient and facile, low-cost, low-carbon footprint synthesis of graphene. Summary of the invention

[0015] The present invention describes a new and simple method for electrosynthesizing graphene from CO2 at low cost. The method comprises (i) performing electrolysis between an electrolysis anode and an electrolysis cathode in a molten carbonate electrolyte to generate carbon nanomaterials on the cathode; and (ii) electrochemically exfoliating the carbon nanomaterials from a second anode to produce graphene.

[0016] The electrosynthesized carbon sheets are nano-thin, which promotes a higher graphene yield compared to that observed using thicker conventional graphite exfoliation methods. CO2 can be the only reactant for producing graphene products. Using CO2 as the only reactant produces graphene as a low carbon footprint product. This stimulates the utilization and consumption of CO2, and unlike alternative products (such as carbon monoxide) or other fuels (such as methane) prepared by CO2, the use of graphene products does not require combustion and does not release greenhouse gases back into the atmosphere. The cost of the electrochemical method described herein is low and consumes carbon dioxide in the formation of graphene. Before the work described herein, it was believed that graphene could only be produced in large quantities with high carbon footprint and high cost. The sheet CO2 electrolysis in molten carbonate produces a simple linear increase in proportion to the area of ​​the electrolysis electrode, which contributes to the large-scale synthesis of graphene.

[0017] Graphene produced by the methods described herein typically exhibits relatively small lateral dimensions (on the order of about 2 μm to 8 μm). Such lateral dimensions are beneficial for use, for example, of graphene as a lubricant in battery anodes and in graphene blend applications. However, with further changes in electrochemical growth parameters (including, for example, electrolysis duration, current density, temperature, electrode and electrolyte composition), larger lateral dimensions can be expected and will extend the utility of the molten carbonate electrolysis process described herein.

[0018] Electrosynthesized carbon sheets and other non-CNT graphene layered forms (e.g., carbon nano-onions) containing uniquely arranged nanographene layers can be synthesized by the methods described herein. The inventors have discovered the molten carbonate electrosynthesis of two types of carbon nano products. The first type is formed when a transition metal nucleating agent is included in the electrolysis and produces carbon nanotubes and carbon nanofibers. In the present invention, the second type is formed when a transition metal nucleating agent is suppressed or excluded in the electrolysis, producing unique nanostructures, including, for example, nanosheets, nano-onions, and nano-scaffolds. Each nanostructure described herein contains layered graphene and can be peeled off to form a graphene sheet.

[0019] Without being bound by any particular theory, the inventors believe that carbon nanotubes are more thermodynamically stable and easier to grow than other graphene layered nanomaterial products. One result of this stability is that CNTs exhibit the highest material strength of any material measured to date. See, for example, Yu et al., Science, 287 (2000) 637–640 and Chang et al., ACS Nano 4 (2010) 5095-5100. Therefore, CNTs provide a low energy pathway for specific carbon nanomaterial products.

[0020] Electrocatalysis promotes nanotube growth in molten carbonates by transition metal nucleation. When nucleation is interrupted by, for example, suppression, repulsion and / or prevention, it is observed that alternative carbon nanoforms occur. In order to support the dominant growth of unique graphene layered carbon nano-nano-scaffolds, a group of experimental conditions that hinder transition metal nucleation pathways have been determined. For example, several electrolysis conditions are described herein, which reliably and consistently suppress CNT nucleation and promote the growth of other graphene layer-based carbon nanomaterials, even in the presence of transition metal nucleating agents such as Ni, Cr and Fe.

[0021] The first is direct cathode deposition rejection of transition metals that may be present in the electrolysis system (e.g., blocking, inhibiting or preventing deposition of transition metals on the cathode). For example, this can be achieved by selecting electrolysis conditions that inhibit the solubility of transition metal nucleating agents in the electrolyte. Reduced solubility minimizes their concentration in the electrolyte or near the cathode surface to inhibit their diffusion and inhibit the development of nucleation seeds required for CNT growth. Examples of these physicochemical conditions include, for example, (i) using nucleating metals, such as iron, in binary carbonates (i.e., mixtures of carbonates, such as a combination of lithium carbonate and potassium carbonate and / or sodium carbonate, rather than pure lithium carbonate), where the nucleating metal solubility is low, and (ii) the metal cation concentration is balanced with the oxide; an increase in one reduces the solubility of the other, and therefore adding oxides to carbonate electrolytes will reduce the solubility and availability of transition metal nucleating agents.

[0022] Compared with CNT, other physicochemical conditions that are conducive to the morphology of layered graphene include: (i) reduction of electrolysis temperature, (ii) reduction of lithium concentration in molten carbonate electrolyte is replaced by increase of material greater than lithium, and even at higher temperature, lithium concentration is reduced, and (iii) condition of higher electrolysis current density. Consistent with these observations is the mechanism meaning of suppressing nucleation, i.e., the reduction of temperature will reduce the rate of carbonate mass transport to nucleation point source, which will have a greater inhibitory effect than the wide-area diffusion to the growing nano carbon structure (i.e., providing less material for reduction and carbon growth). When trying to penetrate nucleation site and grow CNT wall to provide required charge compensation in the ongoing growth process, cations larger than lithium will face larger energy barriers. Similarly, the larger mass transport required under higher current density will be conducive to two-dimensional diffusion consistent with most of the planar growth of the support, rather than point source diffusion consistent with the nucleation point growth process. Each of these technologies can be used alone or in any combination to stop, suppress or prevent transition metal nucleation.

[0023] According to one aspect, the present invention relates to a method for producing graphene carbon nanomaterials. In one embodiment, the method comprises:

[0024] (i) performing electrolysis in a molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode to generate a carbon nanomaterial on the cathode; and

[0025] (ii) electrochemically exfoliating carbon nanomaterial (eg, from a second anode) to produce graphene.

[0026] In one embodiment of any of the methods described herein, step (i) is performed in the absence of a transition metal on or near the surface of the cathode.

[0027] In one embodiment of any of the methods described herein, the electrolysis anode and the molten carbonate electrolyte in step (i) do not contain transition metals. In another embodiment of any of the methods described herein, the electrolysis anode, the electrolysis cathode and the molten carbonate electrolyte in step (i) do not contain transition metals that melt above the melting point of the electrolyte, such as zinc, tin, lead, cadmium, mercury or aluminum.

[0028] In another embodiment, the electrolysis is performed in the absence of an oxide such as an alkali metal oxide (eg, lithium oxide).

[0029] In one embodiment of any of the methods described herein, the electrolysis in step (i) is performed in the absence of a transition metal. In one embodiment of any of the methods described herein, the electrolysis in step (i) is performed in the absence of a transition metal other than zinc.

[0030] In one embodiment of any of the methods described herein, step (i) comprises

[0031] (a) heating a carbonate electrolyte to obtain a molten carbonate electrolyte;

[0032] (b) placing a molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in the cell; and

[0033] (c) applying an electric current to an electrolytic cathode and an electrolytic anode in the cell to electrolyze the carbonate and generate carbon nanomaterials (eg, carbon nanosheets) on the electrolytic cathode.

[0034] In one embodiment of any of the methods described herein, step (ii) comprises performing an electrolysis wherein the electrolysis cathode having carbon nanomaterial from step (i) is used as an anode to produce graphene.

[0035] In one embodiment of any of the methods described herein, the electrolytic cathode having the carbon nanomaterial is cooled prior to stripping.

[0036] In one embodiment of any of the methods described herein, step (ii) comprises (a) placing the cathode having carbon nanomaterial from the electrolysis cathode of step (i) as a stripping anode in an electrochemical cell containing the stripping cathode and a stripping electrolyte, (b) applying a voltage between the stripping anode and the stripping cathode to strip graphene from the stripping anode, and (c) optionally, collecting the graphene stripped from the stripping anode.

[0037] In one embodiment of any of the methods described herein, the carbonate being electrolyzed in step (i) is supplemented by the addition of carbon dioxide.

[0038] In one embodiment of any of the methods described herein, the source of the added carbon dioxide is one of air, pressurized CO2, concentrated CO2, an industrial process for power generation, an industrial process for iron production, an industrial process for steel production, a cement forming process, an ammonia forming process, an aluminum forming process, a manufacturing process, an oven, a chimney, or an internal combustion engine.

[0039] In one embodiment of any of the methods and systems described herein, the electrolytic cathode comprises stainless steel, cast iron, a nickel alloy such as, but not limited to, C276 (UNS N10276 - nickel-molybdenum-chromium alloy containing tungsten), (nickel-chromium based high temperature alloy) (available from Special Metals Co., New Hartford, NY, USA) or Nichrome, or a material resistant to corrosion in the presence of a molten carbonate electrolyte, such as alumina ceramic, or any combination of the foregoing.

[0040] In one embodiment of any of the methods and systems described herein, the electrolysis anode comprises iridium, platinum, a material that is electrocatalytically active for carbonate oxidation while being resistant to corrosion in the presence of a molten carbonate electrolyte, or any combination of the foregoing.

[0041] In one embodiment of any of the methods described herein, the electrolytic cathode is coated with zinc, for example, stainless steel coated with zinc.

[0042] In one embodiment of any of the methods described herein, in step (i), the current is applied stepwise or in any other manner of gradual current increase. For example, in certain embodiments of any of the methods described herein, the current is first applied at, for example, about 0.01 A / cm 2 , then at about 0.02A / cm 2 , then at about 0.04A / cm 2 , then at about 0.08A / cm 2 The electrolysis current is applied for about 3 minutes to about 30 minutes, followed by a longer duration, higher constant current density, such as about 0.1 A / cm 2 , about 0.2A / cm2 or about 0.5A / cm 2 .

[0043] In another embodiment of any of the methods described herein, the carbon nanomaterial growth comprises carbon nanosheets.

[0044] In another embodiment of any of the methods described herein, the carbon nanosheets comprise less than about 125 graphene layers, e.g., less than about 100 graphene layers, less than about 75 graphene layers, less than about 50 graphene layers, less than about 25 graphene layers, less than about 10 graphene layers, or less than about 5 graphene layers.

[0045] In another embodiment of any of the methods described herein, the carbonate electrolyte comprises an alkali metal carbonate, an alkaline earth metal carbonate, or any combination thereof.

[0046] In another embodiment of any of the methods described herein, the alkali metal carbonate or alkaline earth metal carbonate is lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate, francium carbonate, beryllium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, radium carbonate, or any mixture thereof.

[0047] In one embodiment of any of the methods described herein, the molten carbonate electrolyte comprises lithium carbonate. In another embodiment of any of the steps described herein for producing nanomaterials (e.g., nanosheets), the molten carbonate electrolyte comprises at least about 70%, 80%, 90%, 95%, 98%, 99%, or 100% lithium carbonate based on 100% total weight of carbonates in the electrolyte.

[0048] In another embodiment of any of the methods described herein, the molten carbonate electrolyte further comprises one or more oxides, and / or one or more inorganic salts containing oxygen, sulfur, halide ions, nitrogen, or phosphorus.

[0049] In another embodiment of any of the methods described herein, step (ii) is performed in the presence of a stripping electrolyte, and the stripping electrolyte comprises an aqueous solution.

[0050] In another embodiment of any of the methods described herein, the stripping electrolyte comprises an aqueous solution of ammonium sulfate.

[0051] In another embodiment of any of the methods described herein, the stripping electrolyte comprises a non-aqueous solution, such as a chlorinated hydrocarbon, such as chloroform, or an alcohol, such as isopropyl alcohol, or any combination thereof.

[0052] In another embodiment of any of the methods described herein, the stripping electrolyte further comprises a carbonate dissolving solution.

[0053] In another embodiment of any of the methods described herein, stripping is performed by electrolysis in a stripping electrolyte between a stripping anode and a stripping cathode, wherein the stripping anode and the stripping cathode are separated by a membrane, filter, diaphragm or porous separator to separate the graphene produced near the anode.

[0054] In another embodiment of any of the methods described herein, the graphene produced comprises less than 10 graphene layers, such as less than 5 graphene layers. In another embodiment of any of the methods described herein, the graphene produced comprises a single layer of graphene.

[0055] In another embodiment of any method described herein, the coulombic efficiency of the method described in step (i) of any embodiment herein is greater than about 80%, such as greater than about 85%, greater than about 90%, or greater than about 95%. In another embodiment of any method described herein, the coulombic efficiency of the method described in step (i) of any embodiment herein is about 100%.

[0056] In another embodiment of any of the methods described herein, the electrolysis reaction described in step (i) of the embodiments herein is carried out at about 5 mA cm 2 to about 5000mA cm 2 , for example about 50 mA cm 2 to about 1000mA cm 2 , or about 100mA cm 2 to about 600mA cm 2 carried out at a current density of .

[0057] In another embodiment of any of the methods described herein, the graphene carbon nanomaterial has a purity greater than about 80%, such as greater than about 85%, greater than about 90%, greater than about 95%, greater than about 97.5%, or greater than about 99%.

[0058] In another embodiment of any of the methods described herein, the graphene carbon nanomaterial exhibits a Raman spectrum at less than 2720 cm -1 In another embodiment of any of the methods described herein, the graphene carbon nanomaterial exhibits a 2D peak at 2679 cm in the Raman spectrum. -1 Up to 2698cm -1 In yet another embodiment of any of the methods described herein, the graphene carbon nanomaterial exhibits a 2D peak at 2679 cm in the Raman spectrum. -1 The 2D peak at .

[0059] One embodiment is a method for forming a graphene carbon nanomaterial, comprising (i) heating a carbonate electrolyte to obtain a molten carbonate electrolyte; (ii) placing the molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell; (iii) applying an electric current to the electrolysis cathode and the electrolysis anode in the cell to electrolyze carbonate and produce carbon nanomaterials on the electrolysis cathode, wherein the carbonate to be electrolyzed is supplemented by adding carbon dioxide; (iv) placing the electrolysis cathode on which the carbon nanomaterial has been formed as a stripping anode in an electrochemical cell containing a stripping cathode and a stripping electrolyte; (v) applying a voltage between the stripping anode and the stripping cathode to strip graphene from the stripping anode; and (vi) optionally collecting the graphene stripped from the cathode of the cell. In one embodiment, the electrolysis in step (iii) is performed in the absence of an oxide such as an alkali metal oxide (e.g., lithium oxide).

[0060] Another embodiment is directed to a system for producing graphene carbon nanomaterials, the system comprising:

[0061] a furnace chamber receiving a carbonate, the furnace chamber being heated to produce a molten carbonate; and

[0062] an electrolysis device having an anode and a cathode for applying electrolysis to a molten carbonate,

[0063] wherein the system is configured to (i) initially form carbon nanosheets on a cathode of the electrolysis device, and (ii) subsequently use the cathode as an anode in an electrochemical exfoliation process to produce graphene carbon nanomaterials. In one embodiment, the carbon nanosheets are formed on the cathode in the absence of an oxide such as an alkali metal oxide (e.g., lithium oxide).

[0064] Another embodiment is directed to a method for producing carbon nanosheets (e.g., a two-dimensional layered graphene product), the method comprising:

[0065] (a) heating a carbonate electrolyte to obtain a molten carbonate electrolyte, wherein the molten carbonate may optionally further comprise a metal (e.g. zinc) which is molten at the temperature at which step (c) of electrolysis is carried out;

[0066] (b) placing a molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in the cell; and

[0067] (c) applying an electric current to an electrolysis cathode and an electrolysis anode in the cell to electrolyze carbonate and generate carbon nanosheets on the electrolysis cathode without forming transition metal nucleation sites on the cathode. The formation of transition metal nucleation sites can be blocked, inhibited or prevented by any of the techniques described herein.

[0068] In one embodiment, the electrolysis anode and molten carbonate electrolyte do not include a transition metal nucleating agent (eg, the electrolyte and anode do not release a transition metal reagent that promotes nucleation of carbon at the cathode).

[0069] In another embodiment, the cathode (before and / or during the reaction provided in step (c)) also does not include a transition metal nucleating agent. In yet another embodiment, the cathode comprises one or more transition metals, but the transition metals are not conducive to the formation of nucleation sites for the formation of carbon products in step (c) (e.g., by adding oxides to reduce the solubility of the transition metal in the electrolyte and at or near the cathode). In another embodiment, the method also includes electrochemically exfoliating carbon nanosheets (e.g., from a second anode) to produce graphene.

[0070] Another embodiment is directed to a method for producing a carbon onion (e.g., a three-dimensional concentric spherical layered graphene product), the method comprising:

[0071] (a) heating a carbonate electrolyte containing an oxide additive (e.g., an alkali metal oxide such as lithium oxide) to obtain a molten carbonate electrolyte;

[0072] (b) disposing a molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell, wherein the electrolysis anode and the molten carbonate electrolyte do not include a transition metal nucleating agent;

[0073] (c) applying an electric current to an electrolytic cathode and an electrolytic anode in the cell to electrolyze carbonate and generate carbon nano-onions on the electrolytic cathode without forming transition metal nucleation sites on the cathode.

[0074] In one embodiment, the electrolysis anode and molten carbonate electrolyte do not include a transition metal nucleating agent (eg, the electrolyte and anode do not release a transition metal reagent that promotes nucleation of carbon at the cathode).

[0075] In another embodiment, the cathode (before and / or during the reaction provided in step (c)) also does not include a transition metal nucleating agent. In yet another embodiment, the cathode comprises one or more transition metals, but the transition metal is not conducive to the formation of nucleation sites for the formation of carbon products in step (c) (e.g., by adding oxides to reduce the solubility of the transition metal in the electrolyte and at or near the cathode).

[0076] In another embodiment, the method further comprises electrochemically exfoliating the carbon nano-onions (eg, from the second anode) to produce graphene.

[0077] Another embodiment is a system for producing a carbon nano-onion (e.g., a three-dimensional concentric spherical layered graphene product) comprising:

[0078] a furnace chamber receiving a carbonate, the furnace chamber being heated to produce a molten carbonate containing an oxide additive (e.g., an alkali metal oxide such as lithium oxide); and

[0079] an electrolysis device having an anode and a cathode for applying electrolysis to a molten carbonate,

[0080] The system is configured to form carbon nano-onions on a cathode of an electrolyzer without forming transition metal nucleation sites on the cathode.

[0081] In one embodiment, the anode and molten carbonate electrolyte do not include a transition metal nucleating agent (eg, the electrolyte and anode do not release a transition metal reagent that promotes nucleation of carbon at the cathode).

[0082] In another embodiment, the cathode (before and / or during the reaction provided in step (c)) also does not include a transition metal nucleating agent.

[0083] In yet another embodiment, the cathode comprises one or more transition metals, but the transition metals do not facilitate the formation of nucleation sites for the formation of carbon products during electrolysis.

[0084] In one embodiment, the system is further configured to subject the carbon nano-onions to an electrochemical exfoliation process to produce graphene carbon nanomaterials (eg, by subsequently using the cathode of the electrolysis device as an anode in the electrochemical exfoliation process).

[0085] Another embodiment is directed to a method for producing a carbon nano-onion (e.g., a three-dimensional concentric spherical layered graphene product), the method comprising:

[0086] (a) heating a carbonate electrolyte comprising an oxide additive to obtain a freshly molten carbonate electrolyte;

[0087] (b) placing a fresh molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell, wherein the electrolysis anode and / or the molten carbonate electrolyte optionally further comprises a transition metal nucleating agent;

[0088] (c) applying an electric current to an electrolytic cathode and an electrolytic anode in the cell to electrolyze the newly molten carbonate and generate carbon nano-onions on the electrolytic cathode (eg, without forming transition metal nucleation sites on the cathode).

[0089] In one embodiment of the method described herein for producing nano-onions, a constant current is applied during the electrolysis process.

[0090] In another embodiment of the methods described herein for producing nano-onions, the method further comprises electrochemically exfoliating the carbon nano-onions (eg, from a second anode) to produce graphene.

[0091] Another embodiment relates to a method for producing graphene carbon nanoscaffolds, which can be achieved by, for example, suppressing the concentration of lithium in the electrolyte, such as by replacing a portion of the lithium carbonate with a non-lithium carbonate containing a cation greater than lithium (e.g., sodium or potassium), and simultaneously preventing the formation of transition metal nucleation sites on the cathode, the method comprising:

[0092] (a) heating carbonate to obtain a molten carbonate electrolyte rich in non-lithium salt;

[0093] (b) disposing a molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell, wherein the electrolysis anode and / or the molten carbonate electrolyte optionally further comprises a transition metal nucleating agent; and

[0094] (c) applying an electric current to an electrolytic cathode and an electrolytic anode in the cell to electrolyze carbonate and generate carbon nanoscaffolds,

[0095] Wherein, if a transition metal nucleating agent is present, activation of the transition metal nucleating agent is prevented during step (c).

[0096] In one embodiment, the suppression of lithium salts in the electrolyte is achieved by performing the following method in an electrolyte comprising a carbonate: based on 100% total weight of the carbonate in the electrolyte, the carbonate contains less than about 50%, 60%, 70%, 75%, 80%, 90% or 100% lithium carbonate and is rich in non-lithium carbonate (e.g., Na2CO3 or K2CO3, or a combination thereof). For example, based on 100% total weight of the carbonate in the electrolyte, the electrolyte may contain about 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90% lithium carbonate. Based on 100% total weight of the carbonate in the electrolyte, the electrolyte may contain about 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80% or 90% non-lithium salt (e.g., Na2CO3 or K2CO3 or a combination thereof).

[0097] In one embodiment, the formation of transition metal nucleation sites is suppressed by conducting step (c) at a temperature below about 700°C.

[0098] In one embodiment of the above method and system, the cathode (before and / or during the reaction provided in step (c)) also does not include a transition metal nucleating agent. In another embodiment, the cathode includes one or more transition metals, but the transition metals are not conducive to the formation of nucleation sites for the formation of carbon products in step (c). In another embodiment, the electrolysis anode and the molten carbonate electrolyte do not include a transition metal nucleating agent. In yet another embodiment, the electrolysis is carried out at a high current density (e.g., at least 0.4A cm -2 or higher) to suppress the formation of transition metal nucleation sites.

[0099] Other aspects and features of the present invention will become apparent to those of ordinary skill in the art after reading the following description of specific embodiments of the invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0101] In the accompanying drawings, embodiments of the invention are shown by way of example only:

[0102] Figure 1 An exemplary illustration of a method for electrosynthesis of graphene from CO2 is depicted. Figure 1 In A, CO2 from air or flue gas is electrolyzed into carbon nanosheets by molten carbon electrolysis. Figure 1 In B, a carbonate synthesis cathode is placed in a cellulose tube containing, for example, an aqueous solution of (NH4)2SO4. Figure 1 C, the cellulose tubes were placed in a (NH4)2SO4 bath and stripped.

[0103] Figure 2 is a scanning electron microscope (SEM) image of electrolysis products formed by decomposition of CO2 in molten carbonate in the absence of nickel nucleation and in the presence of zinc. Figure 2 Showing the formation of carbon sheets.

[0104] Figure 3 Photograph showing electrolysis products formed by decomposition of CO2 in molten carbonate using a galvanized stainless steel cathode ( Figure 3 A and Figure 3 C, electrodes before and after electrolysis), SEM ( Figure 3 D and Figure 3 E), Raman spectroscopy ( Figure 3 F) and X-ray diffraction (XRD) ( Figure 3 G) illustrates the electrosynthesis of carbon sheets from CO2. Figure 3 B depicts the cell potential measured during electrolysis.

[0105] Figure 4 Shown is the solubility of Li2CO3 in water (top) and various (NH4)2SO4 aqueous solutions (bottom) as a function of temperature.

[0106] Figure 5 The tunneling electron microscope (TEM) of the graphene product prepared according to the present invention is shown ( Figure 5 A and Figure 5 B, before and after stripping), Raman spectra ( Figure 5 C) and atomic force microscopy (ASM) images ( Figure 5 D).

[0107] Figure 6 is a SEM image of electrolysis products formed by decomposition of CO2 in molten carbonate in the absence of a transition metal nucleating agent and in the presence of lithium oxide. Figure 6 The formation of carbon nano-onion is shown.

[0108] Figure 7 TEM images showing the carbon nano-onion product are shown. Figure 7 The bottom of the graphene layer shows the interlayer space between each CNT wall in adjacent SEM, and the distance between the 8 walls is 2.841nm, and the distance between the layers totals 0.255nm.

[0109] Figure 8 Shown are SEM images showing the carbon nano-onion product after extended duration electrolysis.

[0110] Fig. 9 SEM images of electrolysis products produced in various pure or mixed electrolytes are shown.

[0111] Fig.10 The formation of carbon nanoscaffolds is shown. Fig.10 A shows a scheme of the electrolytic cell. Fig.10 B shows the electrolysis electrodes before and after electrolysis. Fig.10 C1 to Fig.10 C6 shows an SEM image of the electrolysis product produced under the conditions of reduced electrolysis temperature and reduced lithium carbonate concentration.

[0112] Fig.11 SEM images of electrolysis products produced in different binary carbonate electrolytes at different temperatures under high or low current density conditions are shown. DETAILED DESCRIPTION

[0113] It is to be understood that any range of values ​​described herein is intended to specifically include any intervening value or sub-range within the given range, and that all such intervening values ​​and sub-ranges are individually and specifically disclosed.

[0114] It should also be understood that the words “a” or “an” are intended to mean “one or more” or “at least one” and that any singular form herein is intended to include the plural.

[0115] It will also be understood that the term "including" (including any variations thereof) is intended to be open ended, and means "including, but not limited to," unless specifically indicated to the contrary.

[0116] When a list of items is given herein with an "or" before the last item, any one of the listed items or any suitable combination of two or more of the listed items can be selected and used.

[0117] The term "nanomaterial" generally refers to (i) a material having at least one limiting dimension that is less than 1000 nm in size, although other dimensions of the material may be larger (e.g., a carbon nanotube with a length much greater than 1000 nm is still a carbon nanomaterial when its diameter (but not its length) is less than 1000 nm), (ii) a material in which the structure of the material may be a material in which nanometer-sized building blocks (e.g., many graphene layers) are repeated to a size greater than 1000 nm, or (iii) a material composed of walls having nanometer-scale thickness (even if the material has a diameter greater than 1000 nm).

[0118] The methods described herein include the synthesis of carbon nanomaterials and their subsequent conversion to graphene.

[0119] The method of the present invention decomposes carbon dioxide by electrolysis in molten carbonate. Isotopes 13 C tracing can be used to track the consumption of CO2 as it dissolves in molten carbonate and decomposes by electrolysis to form carbon nanomaterials, such as carbon nanosheets. CO2 dissolution in molten lithium carbonate is exothermic and rapid, which together with the heat generated by electrolysis provides a heat balance during carbon deposition on the cathode. A process in which electrolysis with lithium carbonate (in the absence of a transition metal nucleating agent) forms carbon nanomaterials (CNM), oxygen and dissolved lithium oxide:

[0120] Electrolysis: Li2CO3→C CNM +O2+Li2O (1a)

[0121] The electrolyte used in the electrolysis step of preparing carbon nanomaterials can be pure lithium carbonate (Li2CO3) or can contain lithium carbon and one or more added oxides, added sodium carbonate, calcium carbonate or barium carbonate, or added boron, sulfur, phosphorus or nitrogen dopants, or any combination of any of the foregoing. The CO2 added to the electrolyte dissolves and chemically reacts with lithium oxide to renew and reform Li2CO3:

[0122] Chemical dissolution: CO2+Li2O→Li2CO3 (2)

[0123] In the methods described herein, carbon nanomaterials, such as carbon nanosheets, are formed by molten carbonate electrolysis when no transition metal nucleating agent (e.g., a transition metal other than zinc) is included. The methods described herein can be facilitated by increasing the electrolysis current in a stepwise manner prior to constant current electrolysis:

[0124] Electrolysis: Li2CO3→C 片 +O2+Li2O (1b)

[0125] In one embodiment, to avoid the formation of carbon nanotubes (CNTs), the electrolyte and cathode surfaces are substantially free of or free of transition metal nucleating agents, such as nickel or chromium, which would form CNT nuclei.

[0126] Carbon nanomaterials such as carbon sheets are then converted into graphene through exfoliation:

[0127] Stripping (DC voltage): C 片 →C 石墨烯 (3)

[0128] In addition to forming carbon nanomaterials (e.g., carbon sheets), the second product of the electrolysis of molten carbonate CO2 in Formula 3 is pure oxygen, O2, released during the electrolysis process. Figure 1 As shown, the net reaction of Formula 1b, Formula 2 and Formula 3 is that CO2 is decomposed into graphene and oxygen by electrolysis:

[0129] CO2→C 石墨烯 +O2 (4)

[0130] The CO2 electrolysis of molten carbonate produced by carbon nanomaterials increases linearly with the area of ​​the electrolysis electrode, which is conducive to larger-scale graphene synthesis. The anode of the molten carbonate carbon nanomaterial electrolysis is not consumed and releases oxygen. Molten carbonate electrolysis does not consume carbon as a reactant, but uses cost-free oxides as reactants to be reduced.

[0131] The carbon nanomaterial product resides on the cathode and can therefore be stacked vertically with a low physical coverage structure. The carbon nanomaterial molten carbonate electrolysis method can be operated at a potential of 0.8V to 2V in a molten carbonate electrolyte under relatively mild conditions (e.g., 770°C). The electricity cost per ton is estimated to be $360, compared to the known cost of $602 per ton of aluminum. These cheap costs provide a significant motivation for using greenhouse gas carbon dioxide as a reactant to produce graphene. The methods described herein provide a useful way to help disrupt the anthropogenic carbon cycle to mitigate climate change.

[0132] Example

[0133] Embodiment 1

[0134] Small transition metal clusters including nickel, chromium, etc. act as nucleation sites to promote high yield C2CNT carbon nanotube growth. Zinc, although liquid at molten carbonate temperatures, reduces the energy of initial carbon deposition. In the absence of solid transition metals as nucleating agents (nucleation sites), galvanized (zinc-coated) steel still appears to be an effective cathode for carbon growth, but CNTs are scarce, including <1% carbon products. In contrast, as Figure 2As shown, the product is an impure mixture of ultrathin carbon flakes, other carbon nanostructures, and amorphous carbon. Figure 2 Shown is an SEM image of the washed cathode product obtained from a 90 minute, 1 A constant current electrolysis of molten Li2CO3 with 6 m (6 mol / kg Li2CO3) Li2O (Alfa Aesar 99.5%) at 730°C without nickel. The electrolysis used a 5 cm 2 Pt foil anode and 5cm 2 0.12 cm diameter coiled galvanized steel wire cathode.

[0135] The noble metal iridium / platinum anode used in this embodiment is intentionally selected to suppress the formation of carbon nanotubes (CNT). This is by preventing the introduction, migration, reduction and formation of nickel or chromium nucleation sites (which are conducive to forming alternative CNT products) from the anode on the cathode to enhance the formation of the desired graphene product observed. However, iridium, platinum or iridium alloy anodes are not prerequisites for high yield sheets or graphene growth. It is feasible to suppress the migration of low-level nickel from nickel or nickel-containing alloy anodes or use thin films (e.g., about 10nm to about 100,000nm thick, such as about 50nm to about 10,000nm thick, or about 100nm to about nm thick) iridium anodes. The following references describe thin film iridium deposition: Grushina et al., J. Appl. Chem. USSR, 2015, 1992, 65; Kamegaya et al., Electrochimica Acta, 1995, 40, 889; Ohsaka et al., Int. J. Surface Eng. Coatings 2007, 85, 260; Ohsaka et al., Electrochem, Solid-State Lett., 2010, 13, D65; Shuxin et al., Rare Metal Mat. Eng., 2015, 44, 1816; Lopez et al., Int. J. Electrochem. Sci., 2015, 10, 9933; Allahyarzadeh et al., Surface Rev. Lett., 2016, 23, 1630001; and Sheela et al., Int. J. Surface Eng.Coatings,2017,8:5,191.

[0136] A mixture of nanostructures, including most of the sheets, formed during the first few minutes of electrolysis (e.g., 5 minutes), even in the presence of nickel. However, in the presence of nickel, with extended electrolysis times (e.g., 15 minutes), the products rapidly dissociated into carbon nanotubes. Over a wide range of lithiated electrolytes, a wide range of metal cathodes were used, including galvanized steel and copper, and over an electrolysis temperature range of 730°C to 790°C. Higher temperatures, not used in this study, increasingly favored the two-electron reduction of CO2 to CO, and by 950°C, the product was pure carbon monoxide.

[0137] Example II

[0138] In this example, it is shown that electrolysis in the absence of other transition metal nucleating agents but in the presence of zinc forms carbon nanosheets rather than carbon nanoonions (CNO) or carbon nanotubes (CNT). The zinc is present as a surface coating on a (galvanized) steel cathode. When the electrolyte is pure Li2CO3 rather than 6m (6 mole) Li2O, Figure 2 The yield of carbon sheets observed in the experiment increased to 70% when an increasing constant current step was first applied before the constant current step ( Figure 3 B), the yield of carbon sheets increased to more than 95%. Specifically, in this electrolysis, in Li2CO3 at 770°C, with a 5 cm 2 5cm of Pt Ir foil anode 2 Graphite flakes were grown on a galvanized (zinc-coated) steel cathode while the electrolysis current was increased stepwise to 0.05 A and 0.10 A for 10 minutes, then to 0.2 A and 0.4 A for 5 minutes, followed by a constant 1 A for 2 hours. These experimental conditions (zinc on the cathode, pure Li2CO3 electrolyte, neither Ni nor Cr in the anode, and increasing constant current steps) were chosen to increase the yield of carbon flakes. Repeated experiments produced similar results with over 95% carbon flake yield. 2 hours of constant current electrolysis at 0.2 A cm -2 During the 2-hour electrolysis, 0.82 g CO2 was consumed and 0.21 g carbon flakes were produced. The potential and electrolysis products of the step-current electrolysis are shown in Figure 4 B. The product purity is over 95%. The remainder includes smaller particles, which also contain smaller flakes. The X-ray diffraction (XRD) of the product ( Figure 3 G) shows a sharp peak at 26.3°2θ, indicating high crystallinity of graphite allotrope. Raman spectrum ( Figure 3 F) and TEM( Figure 3A) shows that the sheets have a relatively low number (25 to 125) of graphene layers. Without wishing to be bound by theory, the inventors electrochemically exfoliated these ultra-thin sheets into higher quality (thinner) graphene by starting with fewer graphene layers than graphite according to Formula 5 for the overall production of graphene from CO2 by electrolysis and electrochemical exfoliation.

[0139] With graphite (2720cm -1 ), an important feature of the conversion of graphite to graphene is the red shift of the 2D peak in the Raman spectrum (see, for example, Zhou et al., Mat. Lett., 2019, 235, 153). The 2D band is highly sensitive to the number of graphene layers, with a single layer showing a red shift at 2679 cm -1 and layers 1 to 4 show a peak at 2698 cm -1 Even before electrochemical exfoliation, ultrathin carbon sheets produced by molten carbonate synthesis ( Figure 3 F) shows a significant red shift to 2708 cm -1 .exist Figure 3 F, the intensity is better than I D / I D ' is 1.3, indicating that for I D / I D ', the defect level is always below the benchmark of graphene boundary defects (I D / I D '=3.5). (Ratio I D / I D ' represents D peak (1350cm -1 ) and D' peak (1620cm -1 ) The ratio of the Raman D or 2D to G peaks is related to the number of defects and the degree of graphitization, respectively. Figure 3 F, Raman I D / I G The intensity ratio of the peaks is low (0.4), and the Raman I 2D / I G The intensity ratio of is 0.6, both of which indicate a small amount of defects. D / I G Representative D peak (1350cm -1 ) and G peak (1583cm -1 )’s strength ratio.

[0140] Example III

[0141] In this example, it is shown that lithium carbonate with entrained carbon flakes produced during the electrolysis process described in Example II can be easily removed by dissolution in aqueous ammonium sulfate.

[0142] Unlike Na2CO3 and K2CO3, which are highly soluble in water, Li2CO3 has a low solubility (30.6, 113, and 1.2 g / 100 g H2O, respectively, at 25°C). Aqueous ammonium sulfate is one of the few media in which the solubility of Li2CO3 is enhanced.

[0143] Aqueous media capable of sustaining the dissolution of excess lithium carbonate electrolyte that can sustain stripping and aid in condensation on the cathode during the production and extraction and cooling of the cathode containing the carbon product by molten lithium carbon electrolysis were studied. The results of these solubility measurements are summarized below. Solubility was measured by incrementally adding lithium carbonate (Alfa Aesar) to an aqueous solution of water or ammonium sulfate (Alfa Aesar) until excess lithium carbonate was observed, and by diluting the excess lithium carbonate until complete dissolution was observed.

[0144] Interestingly, while the water solubility of sodium carbonate and potassium carbonate is high (30.6 and 113 / 100 g H2O at 25 °C, respectively) and increases with temperature (43.9 / 46 and 140 / 156 g H2O at 80 / 100 °C, respectively), the water solubility of lithium carbonate was measured to be low and decreases with increasing temperature, as shown in Figure 2. Figure 4 The water solubility of lithium carbonate (1.2 g / 100 g H2O at 25°C) is low compared to that of lithium chloride and lithium bromide (18.0 g and 17.5 g / 100 g H2O at 25°C, respectively), and increases with increasing temperature (112 / 128 and 245 / 266 g H2O at 80 / 100°C, respectively).

[0145] Then, the dissolution of ammonium sulfate in water (without lithium carbonate) was verified at room temperature and at temperatures close to the boiling point of the solution. See Table 1. These measurements were made to verify dissolution rather than to establish ammonium sulfate solubility limits, which were estimated to be 15% to 20% higher than the maximum dissolution observed at each temperature. The solubility of lithium carbonate in 100 ml of 1.07, 2.33, 4.06 or 6.64 molar (NH4)2SO4 (mass measured in grams) is shown in Figure 4 In the figure below. Figure 5 The 100°C and 108.9°C data in the lower trace are the measured solubility limits of lithium carbonate in 6.45 or 6.64 molar ammonium sulfate, respectively. Increasing the concentration of the aqueous ammonium sulfate solution can significantly increase the solubility of lithium carbonate.

[0146] Table 1: Dissolution of ammonium sulfate aqueous solution as a function of temperature

[0147]

[0148]

[0149] Example IV

[0150] In this example, it is shown that the carbon sheet formed in Example II is converted into graphene by electrochemical exfoliation.

[0151] The electrochemical exfoliation electrode is fixed in the cellulose dialysis membrane to separate the graphene product from the bulk electrolyte. The electrode in the cellulose membrane module is used as the anode in a two-compartment electrochemical cell, but instead of using graphite, a cooled cathode is used, i.e., an unwashed (carbon nanosheet) cathode in 0.1 M (NH4)2SO4, such as Figure 1 C. Specifically, the cathode containing the product of carbonate synthesis is cooled and placed in a cellulose tube containing a 0.1M (NH4)2SO4 aqueous solution. The cellulose tube is an inexpensive, high-quality commercially available cellulose dialysis membrane (see, for example, https: / / www.amazon.com / s?k=Premium-Dialysis-Tubing-Regenerated-Cellulose), listed as having a cutoff value of 12 to 14 kdal, equivalent to a pore size of 1 to 2 nm. Figure 1 C, a cellulose tube is placed in a 0.1M (NH4)2SO4 bath with a counter electrode. A DC voltage is then applied, which creates bursts of gas between the graphene layers, causing the thin sheets to peel off and produce graphene. As the graphene layers peel off, the cellulose captures them in the anode compartment.

[0152] Before exfoliation, the sheets ranged from 25 to 125 graphene layers as measured by TEM (see, e.g., Figure 5 A). This is consistent with the measured Raman spectrum at 2708 cm -1 After exfoliation, the lateral size of the exfoliated layer was 3 μm to 8 μm, as measured by SEM ( Figure 5 B). After stripping, the product was filtered, rinsed and freeze-dried to remove water, and then analyzed by TEM, atomic force microscopy (AFM) and Raman spectroscopy. The stripping product yield was 83% by mass of the original carbon sheet. The product yield may increase with longer stripping time (e.g., more than 10 hours).

[0153] Raman spectra of sample carbon nanosheets produced by C2CNT technology show Figure 5 In the top trace of C, the Raman spectrum of the sample graphene produced by the C2CNT technique is shown in Figure 5 In the bottom trace of C, the presence of the D' band indicates lamellar monolayer and multilayer (sheet) graphene layers, and the left shift of the 2-D band indicates thin graphene layers.

[0154] With graphite (2720cm -1), an important feature of the conversion of graphite to graphene is the red shift of the 2D peak in the Raman spectrum (see, for example, Zhou et al., Mat. Lett., 2019, 235, 153). The 2D band is highly sensitive to the number of graphene layers, with a single layer showing a red shift at 2679 cm -1 The peak at 2698 cm-1 is shown in Figure 1, and layers 1 to 4 show a peak at 2698 cm-1. -1 Even before electrochemical exfoliation, ultrathin carbon sheets produced by molten carbonate synthesis ( Figure 3 F) shows a significant red shift to 2708 cm -1 .exist Figure 3 F, the intensity is better than I D / I D ' is 1.3, indicating that for I D / I D ', the defect level is always below the benchmark of graphene boundary defects (I D / I D '=3.5). (Ratio I D / I D ' represents D peak (1350cm -1 ) and D' peak (1620cm -1 ) The ratio of the Raman D or 2D to G peaks is related to the number of defects and the degree of graphitization, respectively. Figure 3 F, Raman I D / I G The intensity ratio of the peaks is low (0.4), and the Raman I 2D / I G The intensity ratio of is 0.6, both of which indicate a small amount of defects. D / I G Representative D peak (1350cm -1 ) and G peak (1583cm -1 ) strength ratio.

[0155] Raman spectra of sample carbon nanosheets produced by the method described herein show Figure 5 C and compared with the Raman spectrum of sample graphene produced by the method described in this paper. The D' band (1620 cm -1 ) indicates lamellar single and multilayer (sheet) graphene layers, and the left shift of the 2-D band indicates thin graphene layers. The Raman spectrum of the sample carbon nanosheet produced by the method described herein shows Figure 5 C and compared with the Raman spectrum of sample graphene produced by the method described in this paper. The D' band (1620 cm -1 ) indicates lamellar monolayer and multilayer (sheet-like) graphene layers, and the left shift of the 2-D band indicates thin graphene layers.

[0156] exist Figure 5 C, the Raman 2D peak shows a peak from 2708 cm -1 Up to 2690cm -1 The significant red shift from flake (before exfoliation) to graphene (after exfoliation) products. Both flake (before exfoliation) and graphene (after exfoliation) are from graphite (2720cm -1 ) redshift. This -1 The shift of indicates that the graphene thickness ranges from 1 to 5 graphene layers. The edge TEM cross-section of the exfoliated product also shows a range from 1 layer (in Figure 5 B) to 5 layers of graphene. This was verified by AFM (see Figure 5 D). Dispersion of graphene products for AFM characterization remains a challenge. Sonication and freeze drying effectively disperse the product but are overly aggressive and convert the graphene from a continuous sheet to a "Swiss cheese" pattern, which has the benefit of providing additional locations for depth determination (see Figure 5 D) For comparison, using graphite foil as the exfoliation reactant instead of molten carbonate synthesized carbon nanosheets in the same experimental configuration produced multilayer graphene that was about 5 times thicker and ranged in thickness from 6 to 25 graphene layers at ∼2703 cm -1 The wavelength of 2690 cm-1 is not observed in the carbon nanosheet exfoliation product of Example II. -1 Raman 2D band peak is shown at .

[0157] It is expected that the graphene products prepared by the methods described herein can provide improved structural materials. For example, it is observed that the key measurable property related to strength is low defectivity, as evidenced by order (G peak (1583 cm) in the Raman spectrum. -1 ), reflecting the cylindrical planes sp in carbon 2 bond) and disorder (D peak (1350cm -1 ), reflecting the cylindrical out-of-plane sp 3 Tetrahedral bonds) compared to the ratio.

[0158] Raman spectroscopy of graphene products prepared according to the methods described herein shows that the exfoliated products show increased defects compared to the thicker pre-exfoliated sheets formed during electrolysis in molten carbonate, but the defect levels remain low and within tolerable levels for graphene. Figure 6 C, Comparison of the peak ratio of graphene with that of sheets: I D / I D ' is 1.5 (for graphene products, compared to 1.3 for nanosheets), again demonstrating that for I D / I D', the defect level is always lower than the graphene boundary defect ratio I D / I D ' = 3.5 standard. Raman I D / I G The intensity ratio of the peaks is 0.64 (for the graphene product, compared to 0.4 for the nanosheets), and the Raman I 2D / I G The intensity ratio is 0.70 (for the graphene product, compared to 0.6 for the nanosheets), both of which indicate a small number of defects.

[0159] Most of the applied stripping voltage is lost through the resistance drop across the 0.1 M ammonium sulfate solution. This can be avoided by placing the electrodes closer together and / or higher ionic strength to reduce the energy requirements. The temperature can be increased and the cellulose membrane can also be changed to minimize the voltage drop and also increase the sustainable current density (and stripping rate).

[0160] Example V

[0161] The methods and systems described herein can also be improved and used to produce other carbon nanomaterials (CNMs), including graphene, nano-onions, nanosheets, nano-scaffolds, and helical carbon nanotubes. It was observed that each of these CNMs exhibited unusual and valuable physicochemical properties before being added to structural materials, such as lubrication (nano-onions), batteries (graphene), and environmental adsorbents (nano-carbon aerogels), as well as enhanced properties, including improved conductivity and sensing capabilities for CNM-structural material composites. In each case, the product can be synthesized to a high Coulombic efficiency of over 95%, and in most cases, the product has a purity of over 95%.

[0162] Example VI

[0163] In this example, it is shown that in the absence of nickel and transition metal nucleating agents that almost exclude any other impurity levels, and in the absence of a step-wise current increase, but in the presence of lithium oxide, which can be used to reduce the solubility of other transition metals present as impurities, another graphene-based morphology consisting of concentric spherical layers of graphene is formed, and a high yield of carbon nano-onions (CNO) is formed. Unlike the carbon nanosheets containing two planar layered graphene observed in Example II. Zinc is present as a surface coating on a (galvanized) steel cathode. Figure 6The yield of carbon nano-onions shown in is over 95%. Applications of cheap CNO include supercapacitors, battery anodes and solid lubricants. The geological (graphite-like durability) stability of graphene allotropic carbon materials can provide a long-term storage reservoir for atmospheric CO2. SEM, EDS and TEM characterization provide basic evidence of the high yield and purity of CNO synthesis. Specifically, in this electrolysis, when the electrolysis current is 1A (0.2A / cm 2 ) was kept constant for 1.5 hours, in 770℃ Li2CO3 containing 5.9 mol Li2O, in a 5cm 2 5cm of Pt Ir foil anode 2 Highly uniform carbon spheroids grow on the galvanized (zinc-coated) steel cathode. The carbon content of the product is above 99%, the purity of the carbon spheroids in the product is above 95%, and the coulombic efficiency of electrolysis is above 95%, as determined by EDS. Figure 6 A shows the SEM traces of the products after 5, 15, or 90 minutes of electrolysis. It can be seen that even when the electrolysis duration is 15 minutes or less, the different carbon sphere shapes are evident. Figure 6 C presents Figure 6 Overview (lower magnification SEM) of various syntheses presented (at higher magnification) in B. In each case, the product was carbon spheroids of highly uniform diameter. Figure 6 Each spheroid in B is in turn formed by clusters of nano-onions.

[0164] Figure 7 TEM showing the carbon nano onion (CNO) product after 30 minutes of electrolysis. The distinct concentric shell morphology of the carbon nano onion with a typical layered graphite structure of 0.35nm interlayer spacing is evident. Not shown in the figure is that the isolated and single bundled nano onions in the spheres have an average diameter that increases with increasing electrolysis time, as measured by ImageJ SEM automatic optical counting software. After 5, 30 and 90 minutes of electrolysis, respectively, each CNO has an increased diameter of 38±10nm, 66±6nm and 96±2nm, while the spheroids (bundled nano onions) have a ten-fold higher respective diameter of 400nm, 600nm and 900nm, as shown in Figure 1. Figure 6 B. Although the nano-onions formed by short-duration electrolysis (5 min) have unique sizes, unlike the synthesis with longer duration, the products after 5 min of electrolysis do not show Figure 7 Unique concentric spherical graphene shells are evident in the graphene.

[0165] like Figure 8 The SEM of A shows that at a lower current density (0.1, instead of 0.2, A / cm 2), extended electrolysis (15 h instead of 1.5 h) produced more carbon nano-onion products, but the size of the carbon nano-onion products was not significantly larger.

[0166] Figure 8 The SEM tracking shown in B depicts the product of the method of forming carbon nano onions even in the presence of transition metals that have been inhibited from promoting carbon nucleation. Typically, in an aged lithium carbonate electrolyte, a high-purity, uniform CNT product is obtained at a controlled temperature in the range of 700°C during electrolysis, and the extent to which the carbon nanotube product is entangled or straight, long or short, or thick or thin can be controlled by the additives added to the lithium carbonate electrolyte, the current density, the duration of electrolysis, and the selection of anode or cathode materials. However, when the electrolyte is not aged, the product can be a partial or pure carbon nano onion product. Aging refers to a period of time in which the electrolyte is allowed to stand in a molten state for several hours to several days before use. After electrolysis is started in a newly molten solution, it is observed that there is a period of time, such as 1 hour, before CO2 is completely absorbed by the electrolyte. After this period of time, CO2 is completely absorbed to a rate of 4 farads per mole of CO2 equivalent to a constant current applied in the electrolysis. It is observed that when Li2O is added to a lithium carbonate electrolyte, the activation time for absorbing CO2 during electrolysis startup can be shortened by 2 to 3 times. This time period appears to correlate with the time required for the molten carbonate to reach a steady-state concentration of Li2O, consistent with the equilibrium reaction, for example:

[0167]

[0168] Without wishing to be bound by any theory, it is proposed that transition metal nucleation inhibits carbon nanotube growth during the initial stage of electrolyte activation. Specifically, electrolysis was performed in freshly molten Li2CO3 at 770°C using a Montz brass cathode and an Inconel 718 anode, both with an effective area of ​​2450 cm 2 . Electrolysis at 0.2A / cm 2 The duration of the test is 16 hours. Figure 8 As shown in B, the washed cathode product is pure carbon nano-onions without any evidence of carbon nanotubes.

[0169] Example VII

[0170] In this embodiment, it is shown that electrolysis in a high concentration of molten sodium carbonate or potassium carbonate electrolyte forms an alternative graphene product, a carbon nanoscaffold. The carbon nanoscaffold consists of a morphology in which multiple layers of graphene are stacked at sharp angles in an open structure, rather than a flat multilayer graphene sheet morphology. The open structure is not only aesthetically different, but also exposes a larger graphene surface area, which has the potential to increase activity in graphene capacitors, batteries, EMF shielding and catalytic applications. In addition, the conditions for the growth of the carbon nanoscaffold are different from the sheet growth conditions described above. Specifically, unlike avoiding transition metals to prevent competitive growth of alternative carbon nanotube products, here (i) transition metal ions are allowed, such as introduced through the anode, and the molten carbonate CO2 electrolysis is carried out under (ii) electrolyte and / or (iii) temperature conditions that are particularly unfavorable for carbon nanotube (CNT) growth.

[0171] It has been shown (see, e.g., Wu et al., Carbon., 2016, 106, 208) that temperatures above 700° C. are more favorable for CNT growth during molten carbonate electrolysis. Here, it is also demonstrated that electrolyte electrolysis in which the fraction of Na2CO3 or K2CO3 is increased in the mixed Li2CO3 is less favorable for CNT growth even in the presence of nucleating transition metals. Fig. 9 The SEM images of the electrolysis products in various mixed electrolytes after 5 hours of electrolysis are shown. Fig. 9 Comparison of SEM images of electrolysis products in pure Li2CO3 electrolyte aged for 24 hours at 770°C in A. Each electrolysis reaction was conducted at 0.2 A / cm 2 The results were performed at a current density of 1.5 Å with a cathode of Monds brass (an alloy of 60% Cu and 40% Zn) and an anode of Inconel 718 (an alloy of 50-55% Ni, 17-21% Cr, 2,4.75-5.5% Nb&Ta, 2.8-3.3% Mo, the balance being Fe and low concentrations of Ti, Co, Al, Mn, Cu, Si and C). The addition of 8% LiBO2 to the electrolyte further improved the morphology, uniformity and purity of the carbon nanotube product. For example, the addition of 8% LiBO2 to pure Li2CO3 increased the aspect ratio (length to diameter) of the CNT product (not shown), and this LiBO2 was added to each mixed electrolyte to improve the lower quality of the CNT product. (As described below, H3BO3 can partially or completely replace LiBO2 after water is allowed to leave the system.) Fig. 9 The scale bars of A and 9F are 50 μm. Fig. 9 The scale bar of D is 20 μm. Fig. 9 B. Fig. 9 The scale bars in C and 9E are 10 μm. Fig. 9 A to Fig. 9F Comparison at the same ratio shows that there are no easily observable CNTs in the 60% Na2CO3 / 40% Li2CO3 electrolysis product, while the product is high-purity CNTs in the 100% Li2CO3 electrolysis product. The 10% or 20% Na2CO3 electrolysis product contains more than 90% CNTs, while 30% Na2CO3 (not shown) and 50% Na2CO3 show reduced CNT yields and increased fractions of carbon nanospheres and carbon sheets. The CNT aspect ratio decreases and the diameter increases with increasing Na2CO3 percentage in the electrolyte (10% Na2CO3: ~80nm, 20%% Na2CO3: ~100nm, 30%% Na2CO3: ~200nm, 50%% Na2CO3: ~1μm). For 20wt% K2CO3 in Li2CO3, Fig. 9 SEM shown in D and electrolysis with 20wt% K2CO3 (not shown), the loss of aspect ratio in CNT purity occurs more rapidly with increasing K2CO3 weight fraction than with increasing Na2CO3 fraction in electrosynthesis. Energy dispersive X-ray spectroscopy (EDS) testing was used to probe the elemental analysis of the products from mixed electrolyte electrolysis. The EDS of the 20% Na2CO3 and 20% K2CO3 samples were both 100% carbon, while the 50% Na2CO3 and 50% K2CO3 spectra were 97.0% carbon (and 3.0% Na) and 97.8% carbon (and 2.2% K), respectively; the boron in the CNTs is below the limit of EDS detection. The calculated thermodynamic potential for the reduction of alkali carbonates is given by E Li2CO3 <E Na2CO3 <E K2CO3 The higher voltage of the latter salt with increasing concentration will increase the probability of alkali metal cation reduction to alkali metal rather than the desired carbonate reduction to carbon. For the three cases of the 100% Li2CO3, 10% Na2CO3 and 20% Na2CO3 electrolyte experiments, the mass of the product is compared with the applied charge per mole 4e-, and the Coulombic efficiency is close to 100% (98-100%). The Coulombic efficiency is still high, but decreases in binary lithium-carbon electrolytes containing more than 20% sodium carbonate or potassium carbonate. For example, for 30% Na2CO3 electrolyte, the Coulombic electrolysis efficiency drops from 95% to 93% 50% Na2CO3 electrolyte, and for 60% Na2CO3 electrolyte, the Coulombic electrolysis efficiency drops to 90%. Carbonate electrolysis has a diminishing benefit for CNT products in CNT-containing electrolytes. >20wt% Na2CO3 or >20wt% K2CO3.

[0172] exist Fig.10The unique carbon nanoscaffold products are shown in Figure 1 when electrolysis is carried out in a similar 50% Na2CO3 / 50% Li2CO3 electrolyte at 670°C instead of 770°C. Although transition metal elements can again be released from the Inconel 718 anode and the Montz brass cathode consists of copper and zinc, there is no evidence that the carbon nanoscaffold growth is based on transition metal nucleation. 10wt% H3BO3 is added to the electrolyte instead of LiBO2 as a cost-saving measure. After allowing water to leave the system, H3BO3 can partially or completely replace LiBO2. The scheme of the electrolytic cell is shown in Figure 11. Fig.10 A, and the electrolysis electrodes before and after electrolysis are shown in Fig.10 B. SEM images of the product at various magnifications are shown in Fig.10 C1 to Fig.10 C6. The electrolyte consisted of 250 g of Na2CO3, 250 g of Li2CO3, and 50 g of H3BO3 in total. The electrolysis was performed at 670°C for 4.0 hours with a 5 cm × 5 cm electrode at a constant current of 5 A. The voltage throughout the electrolysis was consistently 2.0 V, and more than 85% of the theoretically calculated CO2 was converted into carbon. More than 80% of the product was an unusual carbon nanoscaffold morphology. The morphology consisted of a series of asymmetric 50 nm to 200 nm thick, 2 μm to 20 μm long flat multilayer graphene sheets oriented in a 3D tumor-like geometry.

[0173] Fig.11 Shown are SEMs of electrolysis products produced in different binary carbonate electrolytes at different temperatures under high (Panels D to F) and low (Panel G) current density conditions. Fig.11 D to Fig.11 F shows the results of the thermal conductivity test at a higher current density (0.4 A / cm2) at a different anode, Nichrome C (61% Ni, 15% Cr, 24% Fe, same cathode), and without any borate additives over a range of temperatures. 2 ) under the carbon product. Fig.11 D and Fig.11 As shown in E1, even at the higher temperature of 750°C, there is a significant carbon nanoscaffold product. At this temperature and current density, the products of the 30% Na2CO3 electrolysis are a large proportion of both carbon nanoscaffolds and carbon nanoonions. Not shown is that carbon nanoscaffolds are also observed in the 70wt% Na2CO3 electrolyte, but the structure is smaller and surrounded by amorphous carbon. At this temperature and current density, as shown in Fig.11 E1 and Fig.11As shown in E2, the product of 30% K2CO3 electrolysis is mainly composed of carbon nanoscaffolds and ~10% very thick carbon nanotubes. EDS confirmed that the carbon nanoscaffold structure is mainly carbon (98.3%) and a small amount of potassium (1.7%). Carbon nanoscaffolds were observed under 50wt% K2CO3 (not shown), but as shown in Fig.11 F1 to Fig.11 As shown in F3, no carbon nanoscaffolds were observed in an electrolyte with a high wt% K2CO3 (70% K2CO3 / 30% Li2CO3). In this electrolyte, at 570°C, the product of panel F1 consisted of small round carbon assemblies, at 650°C, the product of panel F2 consisted of coral-like carbon assemblies, and at 750°C, the product of panel F3 consisted of larger but less defined coral-like carbon structures. At temperatures of 650°C or higher (e.g., 750°C or higher), carbonate electrolysis favors carbon nanoscaffold products in electrolytes containing 30 to 70 wt% Na2CO3 or 30 to 50 wt% K2CO3. Although transition metal elements can be included in the electrolysis system that produces nanoscaffold products, there is no evidence that carbon nanoscaffold growth is based on transition metal nucleation. Fig.11 The inset of D shows the electrolyte at 0.4 A / cm 2 At high current density (0.4 A / cm 2 The cross-sectional width of each scaffold unit is about 3 times smaller than that in Figures C1 to C6 when synthesized at a higher temperature (670°C) and with more lithium carbonate (50%) in the electrolyte. When the temperature is further reduced to 570°C, the carbon nanoscaffold can also be synthesized at 0.1A / cm 2 The synthesis under low current density, such as Fig.11 As shown in small figure G.

[0174] Of course, the above embodiments are intended to be illustrative only and not limiting in any way. Many modifications may be made to the form, arrangement of parts, details, and order of operation of the described embodiments. On the contrary, the present invention is intended to encompass all such modifications within its scope as defined by the claims.

Claims

1. A method for producing graphene having 1 to 5 layers, the method comprising: include: (i) performing electrolysis between an electrolysis anode and an electrolysis cathode in a molten carbonate electrolyte containing a metal carbonate to generate carbon nanosheets with condensed metal carbonate on the electrolysis cathode; as well as (ii) electrochemically exfoliating the carbon nanosheets from the electrolytic cathode serving as a second anode to produce graphene having 1 to 5 layers; wherein transition metal nucleating agents are suppressed or excluded from the electrolysis in step (i), in: (a) the molten carbonate electrolyte in step (i) comprises a metal carbonate, and (b) step (ii) comprises performing exfoliation, wherein the electrolysis cathode having the carbon nanosheets from step (i) is used as a second anode to produce the graphene, and the condensed metal carbonate from step (i) on the second anode present on the second anode is dissolved in an exfoliation electrolyte; Wherein, the metal carbonate is lithium carbonate.

2. The method of claim 1, wherein step (i) is performed in the absence of a transition metal on or near the surface of the cathode.

3. The method according to claim 1 or 2, wherein the electrolysis anode and the molten carbonate electrolyte comprising metal carbonate in step (i) do not contain transition metals.

4. The method of claim 1 or 2, wherein the electrolysis in step (i) is performed in the absence of (a) a transition metal, (b) lithium oxide, or (c) both.

5. The method according to claim 1 or 2, wherein step (i) comprises (a) heating a carbonate electrolyte to obtain a molten carbonate electrolyte; (b) placing the molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell; (c) applying an electric current to the electrolysis cathode and the electrolysis anode in the cell to electrolyze the carbonate and generate carbon nanosheets on the electrolysis cathode.

6. The method according to claim 1 or 2, wherein step (ii) comprises performing an electrolysis, wherein the electrolysis cathode with the carbon nanosheets from step (i) is used as an anode to produce graphene. The method according to claim 6 , wherein the electrolytic cathode having the carbon nanosheets is cooled before the exfoliation is performed.

8. The method according to claim 1 or 2, wherein step (ii) comprises (a) placing the cathode having carbon nanosheets from the electrolysis cathode of step (i) as a stripping anode in an electrochemical cell containing a stripping cathode and a stripping electrolyte, (b) applying a voltage between the stripping anode and the stripping cathode to strip graphene from the stripping anode, and (c) collecting the graphene stripped from the stripping anode.

9. The method according to claim 1 or 2, wherein the carbonate electrolyzed in step (i) is supplemented by adding carbon dioxide.

10. The method according to claim 9, wherein the source of the added carbon dioxide is air, pressurized CO 2 , Concentrated CO 2 , an industrial process for generating electricity, an industrial process for producing iron, an industrial process for producing steel, a cement forming process, an ammonia forming process, an aluminum forming process, a manufacturing process, an oven, a chimney or an internal combustion engine.

11. The method of claim 1 or 2, wherein the electrolysis cathode comprises stainless steel, cast iron, a nickel alloy, a material that is resistant to corrosion in the presence of the molten carbonate electrolyte comprising a metal carbonate, or any combination of the foregoing.

12. The method of claim 1 or 2, wherein the electrolytic cathode is coated with zinc.

13. The method according to claim 1 or 2, wherein in step (i), the current is applied in a stepwise increasing manner.

14. The method of claim 1, wherein the carbon nanosheet comprises less than 125 graphene layers.

15. The method of claim 1 or 2, wherein the molten carbonate electrolyte comprises an alkali metal carbonate, an alkaline earth metal carbonate, or any combination thereof.

16. The method of claim 15, wherein the alkali metal carbonate or alkaline earth metal carbonate is lithium carbonate, sodium carbonate, potassium carbonate, rubidium carbonate, cesium carbonate, francium carbonate, beryllium carbonate, magnesium carbonate, calcium carbonate, strontium carbonate, barium carbonate, radium carbonate, or any mixture thereof.

17. The method of claim 1 or 2, wherein the molten carbonate electrolyte further comprises one or more oxides, and / or one or more inorganic salts containing oxygen, sulfur, halide ions, nitrogen or phosphorus.

18. The method of claim 1, wherein step (ii) is performed in the presence of a stripping electrolyte, and the stripping electrolyte comprises an aqueous solution or a non-aqueous solution.

19. The method of claim 18, wherein the stripping electrolyte comprises an aqueous solution of ammonium sulfate.

20. The method of claim 18, wherein the stripping electrolyte comprises a non-aqueous solution.

21. The method of any one of claims 18 to 20, wherein the stripping electrolyte further comprises a carbonate dissolving solution.

22. The method of claim 1 or 2, wherein the stripping is performed by electrolysis between a stripping anode and a stripping cathode in a stripping electrolyte, wherein the stripping anode and the stripping cathode are separated by a membrane, a filter, a diaphragm or a porous partition to separate the graphene produced within the vicinity of the anode.

23. The method of claim 1 or 2, wherein the graphene produced comprises less than 5 graphene layers.

24. The method of claim 1 or 2, wherein the graphene produced comprises a single layer of graphene.

25. The method of claim 1 or 2, wherein the method produces a Coulombic efficiency greater than 80%.

26. The method of claim 1 or 2, wherein the coulombic efficiency is 100%.

27. The method according to claim 1 or 2, wherein the electrolysis reaction is carried out at 5 mA cm 2 Up to 1000mA cm 2 carried out at a current density of .

28. The method of claim 1 or 2, wherein the graphene carbon nanomaterial has a purity greater than 95%.

29. The method according to claim 1 or 2, wherein the graphene carbon nanomaterial shows a Raman spectrum of less than 2720 cm -1 The 2D peak at .

30. The method according to claim 1 or 2, wherein the graphene produced shows a Raman spectrum of 2679 cm -1 Up to 2698cm -1 2D peaks.

31. The method according to claim 1 or 2, wherein the graphene produced shows a Raman spectrum at 2679 cm -1 The 2D peak at .

32. The method according to claim 1 or 2, wherein step (i) also produces molecular oxygen (O 2 ).

33. A method for producing carbon nanosheets, include: (a) heating a carbonate electrolyte to obtain a molten carbonate electrolyte; (b) placing the molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell; as well as (c) applying an electric current to the electrolysis cathode and the electrolysis anode in the cell to electrolyze the carbonate and generate carbon nanosheets on the electrolysis cathode without forming transition metal nucleation sites on the cathode, The molten carbonate electrolyte comprises one or more transition metal nucleating agents, and the conditions for electrolysis reduce the solubility of one or more of the transition metal nucleating agents by: (i) using an electrolyte comprising lithium carbonate and one or both of sodium carbonate and potassium carbonate, (ii) lowering the electrolysis temperature, (iii) lowering the concentration of lithium in the electrolyte, (iv) increasing the electrolysis current density, or (v) any combination of any of the foregoing.

34. A method for producing carbon nano-onions, include: (a) heating a carbonate electrolyte comprising an oxide additive to obtain a freshly molten carbonate electrolyte; (b) placing the fresh molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell, wherein the electrolysis anode and / or the molten carbonate electrolyte further comprises a transition metal nucleating agent; (c) applying an electric current to the electrolysis cathode and the electrolysis anode in the cell to electrolyze the newly molten carbonate and generate carbon nano-onions on the electrolysis cathode, The activation of the transition metal nucleating agent is inhibited by: (i) using an electrolyte containing one or both of sodium carbonate and potassium carbonate and lithium carbonate to reduce the solubility of one or more transition metal nucleating agents during electrolysis, (ii) reducing the electrolysis temperature, (iii) reducing the concentration of lithium in the electrolyte, (iv) increasing the electrolysis current density, or (v) any combination of any of the foregoing.

35. The method of claim 34, wherein the oxide additive comprises lithium oxide.

36. A method for producing graphene carbon nanoscaffolds, include: (a) heating carbonate to obtain a molten carbonate electrolyte rich in non-lithium carbonate; (b) disposing the molten carbonate electrolyte between an electrolysis anode and an electrolysis cathode in a cell, wherein the electrolysis anode and / or the molten carbonate electrolyte further comprises a transition metal nucleating agent; and (c) applying an electric current to the electrolysis cathode and the electrolysis anode in the cell to electrolyze the carbonate and generate carbon nanoscaffolds, wherein if a transition metal nucleating agent is present, activation of the transition metal nucleating agent is inhibited during step (c) by: (i) using an electrolyte comprising one or both of sodium carbonate and potassium carbonate and lithium carbonate to reduce the solubility of one or more transition metal nucleating agents during electrolysis, (ii) reducing the electrolysis temperature, (iii) reducing the concentration of lithium in the electrolyte, (iv) increasing the electrolysis current density, or (v) any combination of any of the foregoing, and The non-lithium carbonate enrichment reduces the weight percentage of electrolyzed lithium carbonate to 70 weight percent or less based on 100% total weight of carbonates in the electrolyte.

37. A method according to claim 36, wherein the formation of transition metal nucleation sites is suppressed by carrying out step (c) at an electrolysis temperature below 700°C.

38. The method of claim 36, wherein the anode does not release a transition metal nucleating agent during the process.

39. The method of claim 36, wherein step (c) is performed at a temperature of at least 0.4 A cm -2 carried out at a current density of .

40. The method of claim 36, wherein the transition metal nucleating agent having reduced solubility is selected from the group consisting of nickel, chromium, iron, and any combination of any of the foregoing.

Citation Information

Patent Citations

  • Process for isolating rubbers

    EP0002015A1

  • Automatic identification of storage requirements, such as for use in selling data storage management solutions

    US20150199265A1

  • Apparatus for molten salt electrolysis with solar photovoltaic electricity supply and solar thermal heating of molten salt electrolyte

    US9683297B2

  • Process for electrosynthesis of energetic molecules

    US9758881B2

  • Methods and systems for carbon nanofiber production

    WO2016138469A1