Solder paste for solar cell module manufacturing
By using solder alloy particle solder paste with a liquidus temperature of less than 225°C to connect photovoltaic cells, the tolerance and cost problems of conductive adhesives at extreme temperatures are solved, and high-reliability and low-cost solar module manufacturing is achieved.
Patent Information
- Application Number
- CN202080046825.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-22
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-05-22
AI Technical Summary
In the existing technology, the conductive adhesive used to connect photovoltaic cells has insufficient tolerance under extreme temperatures, resulting in weak connections, high power loss, and high cost, making it difficult to meet the reliability and economic requirements of solar modules.
Solder paste containing solder alloy particles is used as a conductive adhesive to interconnect photovoltaic cells. The solder alloy includes Sn-containing alloys with a liquidus temperature less than 225°C to reduce reflow temperature and improve the stability and reliability of the joint. .
A low-void, high-reliability joint is achieved, which avoids the effects of corrosion and moisture, provides better conductivity and adhesion, reduces module manufacturing costs, and improves reliability in harsh environments.
Smart Images

Figure CN114026701B_ABST
Abstract
Description
[0001] The present description relates to solar modules and methods of making solar modules, the solar modules comprising photovoltaic (PV) cells interconnected using a conductive adhesive comprising or consisting of a solder paste. Background Art
[0002] Conventional methods for assembling solar modules from photovoltaic (PV) cells include the so-called "string and interconnect" method, in which the PV cells are connected to each other by flat wire (bus) ribbons. The wire ribbons are typically coupled to busbar locations on the surface of the PV cells. Thicker wires have been found to be too stiff, and thin and wide wires can lead to shading effects and failures.
[0003] Therefore, other methods of interconnecting PV cells have been developed, including shingled construction, back contact and gluing. In these methods, conductive adhesive (ECA) is used to connect PV cells. For example, US9356184B2 describes a shingled construction method in which the bottom conductive surface of one PV cell contacts the upper surface of an adjacent PV cell. The interconnection of two PV cells is achieved via a conductive adhesive (ECA).
[0004] ECA generally includes conductive particles dispersed in an organic medium.ECA may not show enough tolerance to environmental effects (e.g., extreme temperatures). Conventional conductive adhesives may include epoxy resins. In such adhesives, the hardener is flaky and hard, resulting in reduced flexibility of the connection.ECA (especially those based on epoxy resins) is also easy to form gel after keeping storage for a long time. Some ECAs reportedly do not meet thermal cycle requirements and power loss can be as high as 7% (I.Ullmann, D.Rudolph, J.Rabanal-Arabach, A.Schneider, A.Halm, Research on the quality of adhesive joints of shingled solar cells by accelerated life test, 35th European Photovoltaic Solar Energy Conference and Exhibition, 2018, Brussels, Belgium, September 24-28, 2018, pp. 1210-1213). In addition, ECA (e.g., those containing silver particles) are generally not fully cured at low temperatures. Therefore, when circuits or conductive layers or interconnects are formed on a substrate using such ECAs, damage to the substrate or device reliability failures may occur. Another major limitation of ECAs is cost. Typically, the cost of silver-based ECAs is very high, which can result in a significant increase in module manufacturing costs.
[0005] The present disclosure seeks to address at least some of the problems associated with the prior art. Summary of the invention
[0006] In a first aspect, the present disclosure provides a method of manufacturing a solar module by interconnecting a plurality of photovoltaic (PV) cells, wherein at least a first PV cell is interconnected to a second PV cell using a conductive adhesive comprising or consisting of a solder paste;
[0007] The solder paste includes particles of a solder alloy dispersed in a flux;
[0008] The solder alloy includes a Sn-containing solder alloy, and the liquidus temperature of the Sn-containing solder alloy is less than 225°C.
[0009] The solder alloy used in conventional processes is usually used for strips or wires, wherein the copper strips or wires are coated with the solder alloy. In such conventional wires and strips, copper provides the required yield strength and electrical conductivity. Since copper is not solderable, the wire or strip is coated with the solder alloy. The present invention uses the solder alloy in the form of solder paste. For example, using advanced interconnect technology (such as "shingled construction"), it is easier to print / dispense solder paste on the silver pads than to place the strips.
[0010] The role of flux is to provide printing performance and stability of the paste and agglomeration of solder particles under given reflow conditions. One of the obstacles to successful solder joints is impurities at the joint site, such as dust, oil or oxidation. Impurities can be removed by mechanical cleaning or by chemical means, but the high temperatures required to melt the filler metal (solder) promote reoxidation of the workpiece (and solder). This effect is accelerated as the soldering temperature increases and can completely prevent the solder from joining to the workpiece. Flux can help prevent oxidation during the soldering process.
[0011] As used herein, the term "solder alloy" encompasses fusible metal alloys. The term "liquidus temperature" as used herein may encompass the temperature above which a material is completely liquid, as well as the maximum temperature at which a crystal can coexist with a melt in thermodynamic equilibrium. The liquidus temperature of Sn-based solder alloys is less than 225°C, preferably less than 220°C, more preferably less than 190°C, even more preferably 100°C to 180°C, further even more preferably 120°C to 160°C. Such liquidus temperatures may enable the use of low reflow temperatures (typically about 20°C to 60°C higher than the liquidus temperature), thereby reducing the occurrence of damage to photovoltaic (PV) cells. For example, when the PV cell comprises silicon, the solder alloy may be reflowed at a sufficiently low temperature to avoid warping relative to the PV cell.
[0012] In one embodiment, the alloy is lead-free and / or antimony-free, which means that lead and / or antimony are not intentionally added. Therefore, the content of lead and antimony is zero, or does not exceed the level of unexpected impurities. The presence of lead and antimony may be harmful to health. In an alternative embodiment, the alloy may contain lead. The presence of lead can result in favorable mechanical properties of the final weld joint.
[0013] Advantageously, the use of solder paste enables the creation of interconnections with low voiding (<10%), thereby producing reliable joints.
[0014] Furthermore, interconnects formed using solder paste can be fully cured, making them less susceptible to corrosion-induced failures. In addition, solder paste interconnects provide excellent stability to moisture, with better conductivity and adhesion. For example, solder paste can be applied to form excellent adhesion, for example, on metallized pads of PV cells, such as screen printed silver, copper, or copper plated or silver coated copper pads.
[0015] It should be understood that a solar module may include more than two interconnected PV cells. For example, greater than 10, optionally greater than 20, optionally greater than 30 PV cells may be interconnected in a single solar module. In one example, 60 PV standard size cells may be interconnected to form a solar module. (In a shingled configuration, this number is >300 cells, as each shingle cell is made by cutting a standard cell into 5-6 strips.)
[0016] In some embodiments, the interconnection of PV cells using solder paste may include interconnecting an interconnect of a first PV cell with an interconnect of a second PV cell. The interconnect may be, for example, a metallized area, a pad, a finger, a busbar, etc. The metallization may include, for example, copper or silver or copper or silver plating. The interconnect may be disposed on the front or rear of the PV cell. Each PV cell may include one or more interconnects on its front and / or its rear. The interconnect may be between an interconnect on the front or rear of the first PV cell and an interconnect on the front or rear of the second PV cell. The interconnect may be a direct soldered interconnect between the two interconnects. Alternatively, the interconnect may be an indirect interconnect, including, for example, a ribbon extending between the two interconnects that is soldered to the two interconnects.
[0017] In some embodiments, the method further comprises laminating a plurality of PV cells.
[0018] Advantageously, the solder paste may have the ability to flow at a first temperature during curing / reflow while keeping the joints more robust during the lamination process. Lamination ensures complete sealing of the interconnected PV cells. Thus, in the present disclosure, the use of solder paste as an interconnect material in combination with lamination results in the formation of solder joints that exhibit enhanced reliability in severe harsh environments. In addition, the solder paste of the present disclosure may form a compatible bond with lamination materials such as ethyl vinyl acetate (EVA) of polyolefins (POE).
[0019] In some embodiments, the interconnection between the first PV cell and the second PV cell is established, and then the plurality of PV cells are subsequently laminated. Lamination may optionally be performed at a lamination temperature below the liquidus temperature of the solder alloy. In this way, further reflow of the solder may be avoided. Lamination may alternatively be performed at a lamination temperature above the liquidus temperature of the solder alloy. In this way, some additional reflow of the solder may occur. However, it has been found that the solder joint remains strong even in the presence of such secondary reflow.
[0020] In some embodiments, the solder paste may include a non-eutectic solder alloy, and the lamination may be performed at a lamination temperature within the plastic range of the non-eutectic solder alloy.
[0021] In some other embodiments, the interconnection between the first PV cell and the second PV cell is established in situ during lamination of the plurality of PV cells;
[0022] Wherein lamination is performed at a lamination temperature equal to or higher than the liquidus temperature of the solder alloy. In these embodiments, low melting temperature bismuth-based solder paste is preferred.
[0023] In some embodiments, the solar module includes a shingled construction assembly wherein the first PV cell and the second PV cell at least partially overlap to form an overlap region;
[0024] And the rear face of the first PV cell and the front face of the second PV cell are interconnected in the overlapping area using the conductive adhesive comprising or consisting of the solder paste.
[0025] In some other embodiments, the solar module includes a back contact assembly, wherein the rear face of the first PV cell is interconnected to the rear face of the second PV cell by one or more ribbons, wherein the one or more ribbons are connected to the rear face of the first PV cell and the rear face of the second PV cell using the conductive adhesive comprising or consisting of the solder paste.
[0026] In some embodiments, the back contact assembly is an interdigitated back contact (IBC) assembly.
[0027] In some other embodiments, the solar module comprises a glued assembly, wherein the first PV cell and the second PV cell are non-overlapping, and the front face of the first PV cell is interconnected to the rear face of the second PV cell using one or more ribbons, preferably one or more light capturing ribbons;
[0028] Wherein the one or more ribbons are connected to the front face of the first PV cell and the rear face of the second PV cell using the conductive adhesive comprising or consisting of the solder paste.
[0029] The methods of the present disclosure are applicable to a wide range of PV cell technologies, including, for example, crystalline silicon (c-Si) architectures, such as bifacial, p-type and n-type, standard screen-printed silicon solar cells, passivated emitter rear cells (PERC) and heterojunction technology cells (HJT). The methods may additionally be applied to the manufacture of thin-film or flexible PV module manufacturing.
[0030] The disclosed method enables the fabrication of components with large surface areas, high mechanical flexibility and even stretchability. Thus, the method enables the fabrication of structures with electrically active surfaces of arbitrary shapes, such as those wrapped around car panels, aircraft wings, buildings and three-dimensional (3D) displays.
[0031] In some embodiments, the solder paste is stencil printed, jet printed or dispensed. For example, the solder paste may be printable and / or dispenseable and / or jettable and / or needle transferable onto a substrate, such as a PV cell, ribbon, etc. The solder paste may have a viscosity and flow properties that are particularly conducive to dispensing, which means that the solder paste can be used as a one-to-one replacement for conventional ribbon or wire solder.
[0032] Advantageously, the solder paste exhibits a stable viscosity, making it particularly suitable for application by stencil printing and achieving a longer stencil life of greater than 12 hours.
[0033] Advantageously, stencil printing or dispensing of solder paste enables better processability and throughput as well as more cost-effective manufacturing compared to conventional ECAs.
[0034] In some embodiments, the solder paste is reflowed by heating after printing, jet printing or dispensing. An infrared, convection oven or a zoned reflow oven may be used to reflow the solder paste for a period of less than 1.5 minutes, optionally less than 10 seconds.
[0035] Advantageously, the solder paste can be reflowed at low temperatures and has excellent wetting on the silver or copper pads of the PV cells.
[0036] The solder alloy preferably comprises:
[0037] 45 to 59 wt% Bi;
[0038] 0.1 wt % to 1.2 wt % Cu;
[0039] 0.01 wt% to 0.1 wt% Co; and
[0040] Optionally up to 1.1 wt.% Ag,
[0041] The remainder of tin, and any unavoidable impurities.
[0042] Such solder alloys are particularly suitable for providing the above advantages. The combination of elements in the amounts described (particularly the combination of Cu and Co) can provide the solder alloy with advantageous mechanical properties, such as high tensile strength, high elastic modulus, high toughness, high creep elongation and / or long creep rupture time. The combination of elements in the amounts described (particularly the combination of Cu and Co) can also provide high thermal fatigue resistance and / or high resistance to drop impact. The combination of elements in the amounts described (particularly the combination of Cu and Co) can also provide high thermal conductivity and electrical conductivity. Therefore, these alloys are particularly suitable for PV cell and photovoltaic ribbon applications. The alloy can be eutectic (having a melting point that is the same as the liquidus temperature) or non-eutectic (having a melting temperature range). The liquidus temperature can be less than 160°C, for example less than 155°C. Therefore, damage to the PV cell due to warping relative to the silicon substrate can be reduced.
[0043] It should be understood that the alloys described herein may contain unavoidable impurities, but generally these impurities are unlikely to exceed 1% by weight of the composition. Preferably, the alloy contains unavoidable impurities in an amount not exceeding 0.5% by weight of the composition, more preferably not exceeding 0.3% by weight of the composition, and even more preferably not exceeding 0.1% by weight of the composition.
[0044] The alloys described herein may consist essentially of the elements recited. Thus, it should be understood that, in addition to the mandatory elements (i.e., Sn, Bi, Cu, and Co), other unspecified elements may be present in the composition, provided that the basic characteristics of the composition are not substantially affected by their presence. Alternatively, the alloys described herein may consist essentially of the elements recited.
[0045] In the above solder alloy, the solder alloy contains 0.1 wt % to 1.2 wt % Cu. The solder alloy preferably contains 0.2 wt % to 1 wt % Cu. In a preferred embodiment, the solder alloy contains 0.7 wt % to 1.1 wt % Cu, preferably 0.8 wt % to 1 wt % Cu. In another preferred embodiment, the solder alloy contains 0.1 wt % to 0.3 wt % Cu, preferably 0.15 wt % to 0.25 wt % Cu, even more preferably about 0.2 wt % Cu. The presence of Cu in said amount can increase ductility, reduce the occurrence of copper leaching and increase thermal fatigue resistance. In addition, the presence of Cu can contribute to the favorable mechanical properties of the final welded joint, in particular high resistance to falling impact and high creep rupture.
[0046] In the above solder alloy, the solder alloy comprises 0.01 wt % to 0.1 wt % Co. In a preferred embodiment, the solder alloy comprises 0.02 wt % to 0.09 wt % Co. In another preferred embodiment, the solder alloy comprises 0.03 wt % to 0.08 wt % Co. In another preferred embodiment, the solder alloy comprises 0.02 wt % to 0.04 wt % Co, preferably about 0.03 wt % Co.
[0047] The presence of Co in the amount described may result in higher toughness, lower Cu dissolution, higher tensile strength and finer microstructure. In addition, the presence of Co in the amount described may result in a shiny joint.
[0048] The above solder alloy optionally contains up to 1.1 wt % Ag (e.g., 0.01 wt % to 1.1 wt % Ag). Preferably, the solder alloy contains up to 1.1 wt % Ag (e.g., 0.01 wt % to 1.1 wt % Ag), more preferably 0.5 wt % to 1.1 wt % Ag, even more preferably 0.8 wt % to 1 wt % Ag, and even more preferably 0.9 wt % to 1 wt % Ag. The presence of Ag can increase the ductility of the alloy and can also reduce surface oxidation.
[0049] In some embodiments, the solder alloy comprises 48 wt % to 51 wt % Bi, preferably 59 wt % to 50 wt % Bi. Advantageously, such Bi content results in the alloy exhibiting increased ductility compared to alloys having higher levels of Bi.
[0050] Preferably, the above solder alloy consists of:
[0051] 48 to 51 wt% of Bi,
[0052] 0.7 wt% to 1.1 wt% Cu,
[0053] 0.02 wt% to 0.09 wt% Co,
[0054] 0.8 wt% to 1.1 wt% Ag,
[0055] The remainder of tin, and any unavoidable impurities.
[0056] Such alloys may have a liquidus temperature of less than 155°C. Such alloys may be non-eutectic, having a melting temperature range of 138°C to 152°C. Such alloys may be particularly suitable for providing the above advantages. In this particularly preferred embodiment, the alloy consists of 49 wt% to 50 wt% Bi, 0.8 wt% to 1 wt% Cu, 0.03 wt% to 0.08 wt% Co, 0.9 wt% to 1 wt% Ag, the balance of tin, and any unavoidable impurities.
[0057] In some other embodiments, the solder alloy comprises 56 wt % to 59 wt % Bi, preferably 57 wt % to 58 wt % Bi. Advantageously, such Bi content reduces the melting point of the alloy compared to alloys comprising lower levels of Bi.
[0058] Preferably, the above solder alloy consists of:
[0059] 56 to 59 wt% Bi,
[0060] 0.1 wt% to 0.3 wt% Cu,
[0061] 0.02 wt% to 0.04 wt% Co,
[0062] The remainder of tin, and any unavoidable impurities.
[0063] Such alloys may exhibit a liquidus temperature of less than 140° C., such as about 138° C. Such alloys may be particularly suitable for providing the above advantages. In this particularly preferred embodiment, the alloy consists of 57 to 58 wt % Bi, 0.15 to 0.25 wt % Cu, 0.025 to 0.035 wt % Co, the balance of tin, and any unavoidable impurities.
[0064] In some embodiments, the solder alloy includes a SnPb solder alloy.SnPb solder alloys can exhibit particularly advantageous mechanical properties.
[0065] In these embodiments, the solder alloy preferably comprises 5 wt % to 70 wt % Sn and the balance Pb and any unavoidable impurities, more preferably 50 wt % to 70 wt % Sn and the balance Pb and any unavoidable impurities. The SnPb solder alloy is preferably a binary solder alloy. In a preferred embodiment, the SnPb alloy is Sn40Pb (liquidus temperature is about 183°C). In another preferred embodiment, the SnPb alloy is Sn37Pb (liquidus temperature is about 183°C).
[0066] In some embodiments, the solder alloy comprises:
[0067] 35 to 60 wt% Bi;
[0068] 0 wt% to 2 wt% Ag,
[0069] The balance of Sn, and any unavoidable impurities.
[0070] Such alloys may be particularly suitable for back contact components.
[0071] In these embodiments, the solder alloy preferably comprises 40 wt % to 60 wt % Bi, more preferably 41 wt % to 45 wt % Bi or 56 wt % to 60 wt % Bi. For example, the solder alloy may comprise a Sn57Bi43 alloy or a Bi58Sn42 alloy.
[0072] In these embodiments, the solder alloy preferably comprises 0.5 wt % to 1.5 wt % Ag, more preferably 0.7 wt % to 1.3 wt % Ag, even more preferably about 1 wt % Ag. For example, the solder alloy may comprise 57Bi-42Sn-1Ag.
[0073] In some embodiments, the solder alloy comprises:
[0074] 0.01 wt % to 5 wt % Ag;
[0075] 0.02 wt % to 1.5 wt % Cu;
[0076] Optionally:
[0077] 0.08 wt % to 20 wt % Bi;
[0078] 0 wt% to 0.1 wt% P;
[0079] 0 wt% to 0.02 wt% of a rare earth mixture consisting of a mixture of 53 wt% Ce, 24 wt% La, 16 wt% Nd and 5 wt% Pr;
[0080] as well as
[0081] 0 wt% to 0.01 wt% Sb
[0082] The balance of Sn, and any unavoidable impurities.
[0083] Such alloys may be particularly suitable for back contact components.
[0084] In these embodiments, the solder alloy preferably comprises 1.5 wt % to 4.5 wt % Cu, preferably 2 wt % to 4 wt % Cu, more preferably 2.5 wt % to 3.5 wt % Ag, even more preferably about 3 wt % Ag. In these embodiments, the solder alloy preferably comprises 0.1 wt % to 1 wt % Cu, more preferably 0.2 wt % to 0.8 wt % Cu, even more preferably 0.4 wt % to 0.6 wt % Cu, even more preferably about 0.5 wt % Cu. In these embodiments, the solder alloy preferably comprises SAC305.
[0085] In these embodiments, when the solder alloy comprises Bi, the solder alloy preferably comprises:
[0086] 0.08 to 8 wt% Bi, more preferably 3 to 6 wt% Bi;
[0087] 0.1 wt % to 0.7 wt % Cu;
[0088] 0.05 to 0.5 wt% Ag, more preferably 0.1 to 0.4 wt% Ag.
[0089] In other embodiments, solder paste may be used in combination with ECA. For example, alternating PV cells may be interconnected using solder paste and ECA. For example, a first PV cell may be interconnected to a second PV cell using a conductive adhesive comprising or consisting of solder paste as discussed above. A third PV cell may be interconnected to a second PV cell using an ECA. A fourth PV cell may be interconnected to a third PV cell using a conductive adhesive comprising or consisting of solder paste as discussed above, and so on. In another example of the use of a combined solder paste and ECA, the PV cells may be printed and interconnected with an ECA to provide a mechanical interconnection, and a conductive adhesive comprising or consisting of solder paste as discussed above may be used for bus connections.
[0090] The flux preferably comprises:
[0091] Rosin and / or resin, and / or
[0092] Activator, and / or
[0093] Surfactants, and / or
[0094] Solvent, and
[0095] Optional rheology modifiers and / or corrosion inhibitors.
[0096] The components of the flux are typically selected so that they can be removed from the paste (e.g., by evaporation and / or burnout) at a temperature below the target reflow temperature of the solder alloy. This can help promote nearly complete sintering of the metal particles. Inadequate sintering of the metal particles can occur when organic materials remain in the joint during reflow. This can produce a weak solder joint.
[0097] Rosin and / or resin may be particularly suitable for providing a paste with rheological properties that are beneficial for stencil printing pastes. Non-limiting examples of rosin / resin are gum rosin, hydrogenated rosin, esterified rosin, modified rosin resin or dimerized rosin with varying degrees of softening point and acid value. Rosin and / or resin is preferably rosin. The use of rosin is superior to epoxy or acrylic adhesives in terms of better reliability, diffusion, deoxidation and formation of non-interfering residues.
[0098] Activators can be used to remove any metal oxides that may be present from the surface to be printed (e.g., PV cell, strip light) and / or to remove any oxides that may be present in the solder alloy. Aryl or alkyl carboxylic acids can be used as activators, such as one or more of adipic acid, succinic acid, and glutaric acid.
[0099] Surfactants can control the rheology or other functional properties of the solder paste. Surfactants can be anionic, cationic or nonionic. Non-limiting examples include surfactants available under the trade names SPAN-80, SPAN-20, Tween-80, Triton-X-100, Sorbitan, IGEPAL-CA-630, Nonidet P-40, Cetyl alcohol, FS-3100, FS-2800, FS-2900, FS-230, FS-30.
[0100] The solvent (typically a combination of solvents) is typically selected to facilitate evaporation of the solvent prior to solidification of the solder. Typical solvent compositions include, for example, monoterpene alcohols, glycols, glycol esters, glycol ethers, and combinations thereof. Non-limiting examples include hexyl carbitol, diethylene glycol dibutyl ether, tripropylene glycol monobutyl ether terpineol, and diethylene glycol monobutyl ether.
[0101] The flux may also contain a rheology modifier to control the viscosity of the paste. Examples of suitable rheology modifiers include, but are not limited to, Thixcin R, Crayvallac Super, and combinations thereof.
[0102] The flux may also include a corrosion inhibitor, which preferably includes a triazole derivative, more preferably one or more of benzotriazole, tolyltriazole, and carboxybenzotriazole. The presence of such a corrosion inhibitor may help protect the resulting solder joint during ambient storage or during electrical reliability or thermal reliability testing conditions.
[0103] The solder paste preferably contains 75 to 95 wt% solder alloy particles, more preferably 80 to 92 wt% solder alloy particles.The solder paste preferably contains 5 to 25 wt% flux, more preferably 8 to 20 wt% flux.
[0104] The flux preferably comprises:
[0105] 25 to 40% by weight of rosin and / or resin, and / or
[0106] 12 to 20 wt. % of an activator, and / or
[0107] 10 to 20 wt% of a surfactant, and / or
[0108] 20 to 40 wt. % of a solvent, and / or
[0109] 1 to 10 wt. % of a rheology modifier, and / or
[0110] 0.5 wt % to 3 wt % of a corrosion inhibitor.
[0111] In a second aspect, the present disclosure provides a solar module comprising a plurality of interconnected photovoltaic (PV) cells;
[0112] wherein at least a first PV cell is interconnected to a second PV cell using a conductive adhesive comprising or consisting of a solder paste;
[0113] The solder paste includes particles of a solder alloy dispersed in a flux, and the solder alloy includes a Sn-containing solder alloy having a liquidus temperature of less than 225°C.
[0114] In some embodiments, a solar module may include:
[0115] A shingled construction assembly wherein the first PV cell and the second PV cell at least partially overlap to form an overlap region, and a rear face of the first PV cell and a front face of the second PV cell are interconnected in the overlap region; or
[0116] a back contact assembly in which the rear face of the first PV cell is interconnected to the rear face of the second PV cell by one or more ribbons; or
[0117] A glued assembly wherein the first PV cell and the second PV cell are non-overlapping and the front face of the first PV cell is interconnected to the rear face of the second PV cell using one or more ribbons, preferably one or more light capturing ribbons.
[0118] Preferably, the solar module is manufactured according to the method described in the first aspect above.
[0119] In a third aspect, the present disclosure provides a method of manufacturing a solar module by interconnecting a plurality of photovoltaic (PV) cells, wherein at least a first PV cell is interconnected to a second PV cell using a flux comprising a binder system but without a solder alloy.
[0120] Preferably, the binder system is an organic binder system.The binder system may correspond to the flux described herein.
[0121] Preferably, the interconnection comprises one or more ribbons connected to the front face of the first PV cell and the rear face of the second PV cell using solder. BRIEF DESCRIPTION OF THE DRAWINGS
[0122] One or more embodiments of the present disclosure will now be described, by way of example only, with reference to the accompanying drawings, in which:
[0123] Figure 1 and Figure 2 is a schematic diagram of a shingled construction assembly including a plurality of individual PV cells;
[0124] Figure 3 is a schematic diagram of a back contact assembly including a plurality of individual PV cells;
[0125] Figure 4 Plan and cross-sectional photographs of the light-trapping ribbon are shown;
[0126] Figure 5 is a schematic diagram of a glued assembly including a plurality of individual PV cells;
[0127] Figure 6 is a photograph of a solder paste stencil printed onto a 1mm wide busbar prior to reflow; and
[0128] Figure 7 After the reflow Figure 6 A photo of the solder pads. DETAILED DESCRIPTION
[0129] Unless otherwise defined, all technical and scientific terms used in this specification have the same meaning as commonly understood by readers in the field to which the claimed subject matter belongs. It should be understood that the above invention content and the following examples of the present disclosure are exemplary and illustrative only and do not limit any subject matter claimed.
[0130] The following description relates to embodiments of the present disclosure. The description of the embodiments is not intended to include all possible embodiments of the present disclosure claimed in the appended claims. Many modifications, improvements and equivalents not explicitly described in the following embodiments may fall within the scope of the appended claims. Unless the context clearly requires otherwise, the features described as part of one embodiment may be combined with the features of one or more other embodiments.
[0131] According to the present disclosure, a method of manufacturing a solar module by interconnecting a plurality of photovoltaic (PV) cells is provided, wherein at least a first PV cell is interconnected to a second PV cell using a conductive adhesive comprising or consisting of a solder paste.
[0132] At a general level, solder paste is used to create a solder joint using the following steps:
[0133] providing a flux having particles of a solder alloy dispersed in the flux to form a solder paste;
[0134] providing two or more workpieces to be joined, for example, two PV cells or a PV cell and an interconnect;
[0135] depositing solder paste on at least one of the two or more workpieces; and
[0136] The solder paste is heated adjacent to two or more workpieces to form a solder joint between the two or more workpieces.
[0137] In the following method of manufacturing a solar module, a description will be made for example only for a better understanding of the present disclosure.
[0138] In a shingled assembly, the solar cells can be cut into 3 to 6 strips (shingles), which are then assembled by connecting the front of each shingle to the back of the next shingle. A shingled strip is made of several PV cells and can be up to 2 meters long. The shingled strips can be connected in series or parallel arrangements by connecting straps.
[0139] Figure 1 and Figure 2 An example of a shingled construction assembly 1 comprising a plurality of individual PV cells 2 is schematically shown. Figure 2As best shown in the enlarged view of FIG. 1 , the shingled construction assembly 1 includes at least a first PV cell 4 and a second PV cell 5 that at least partially overlap to form an overlap region. The rear face of the first PV cell 4 and the front face of the second PV cell 5 are interconnected in the overlap region using a conductive adhesive containing or consisting of a solder paste to form a solder joint 8. The first PV cell 4 may include an interconnect 6 on its rear face, and the second PV cell 5 may include an interconnect 7 on its front face. In the example shown, the interconnects 6, 7 each include a metallized pad, such as a busbar that may extend across the width of the PV cells 4, 5. The solder joint 8 may be formed directly between the interconnects 6, 7.
[0140] The shingled construction can be applied to any PV cell architecture as long as the interconnects (e.g., contact pads) are on opposite sides of the PV cell. For example, it can be applied to BSF, PERC, bifare-PERC, n-PERT / PERL, HJ, and other architectures.
[0141] In a back contact assembly, all or part of the interconnect may be located on the rear face of the PV cell.
[0142] Figure 3 Schematically shown is an example of a back contact assembly 10 comprising a plurality of individual PV cells 11, 12. The rear face of a first PV cell 11 is interconnected to the rear face of a second PV cell 12 by one or more ribbons 13. The one or more ribbons 13 are connected to the rear face of the first PV cell 11 and the rear face of the second PV cell 12 using a conductive adhesive containing or consisting of a solder paste.
[0143] The one or more strips 13 may be copper foil strips.
[0144] In the glued assembly, the first PV cell and the second PV cell are non-overlapping, and the front face of the first PV cell is interconnected to the rear face of the second PV cell using one or more ribbons, preferably one or more light capturing ribbons. The light capturing ribbons are typically grooved, such as Figure 4 As shown, to enhance its light trapping capabilities. This can make it difficult to form a bond with the PV cell interconnect pad using conventional procedures.
[0145] Figure 5 Schematically shown is an example of a glued assembly 20 comprising a plurality of individual PV cells 21, 22 interconnected using light capturing tapes 23. The one or more light capturing tapes 23 are connected to the front face of a first PV cell 21 and the rear face of a second PV cell 22 using a conductive adhesive containing or consisting of solder paste to form a solder joint 28.
[0146] The solder paste may, for example, be stencil printed, jet printed or otherwise dispensed onto the front and / or back sides of the PV cells or light capturing tapes.
[0147] It has been found that the solder paste of the present disclosure exhibits excellent stability, with its metal content remaining almost unchanged even after 12 hours of continuous printing. Specifically, it has been found that viscosity build-up is limited, and therefore the solder paste can be template printed for hours without cleaning the template. In addition, the use of the solder paste enables high print clarity and high speed. For example, even at high printing speeds, the observed transfer efficiency of the solder paste can also exceed 90%. In contrast, ECAs generally do not have a template / screen life of more than 4 hours. Afterwards, the viscosity of the ECA increases rapidly and insufficient transfer and screen hole clogging are generally observed.
[0148] After being stencil printed, jet printed or dispensed, the solder paste can be reflowed by heating. For example, infrared, convection oven or zoned reflow oven can be used to reflow the solder paste for a period of less than 1 minute, optionally less than 10 seconds.
[0149] In other embodiments of the present invention, a method of manufacturing a solar module by interconnecting a plurality of photovoltaic (PV) cells is provided, wherein at least a first PV cell is interconnected to a second PV cell using a flux comprising a binder system but without a solder alloy.
[0150] Preferably, the binder system is an organic binder system.
[0151] Preferably, the interconnection comprises one or more ribbons connected to the front face of the first PV cell and the rear face of the second PV cell using solder.
[0152] The disclosed method can beneficially result in improved peel strength of interconnections between PV cells. For example, in a first test of the peel strength of a bus ribbon connection, it was found that the ECA produced a peel strength of about 0.5N compared to a peel strength of about 2.5N for a solder paste containing a Sn40Pb solder alloy.
[0153] The methods of the present disclosure may beneficially result in improved shear strength of interconnections between PV cells.
[0154] For example, in a second test of the shear strength of the interconnects, the PV cells were interconnected using:
[0155] 1)ECA,
[0156] 2) Solder paste containing Sn40Pb solder alloy, and
[0157] 3) A solder paste comprising a solder alloy consisting of:
[0158] 48 to 51 wt% of Bi,
[0159] 0.7 wt% to 1.1 wt% Cu,
[0160] 0.02 wt% to 0.09 wt% Co,
[0161] 0.8 wt% to 1.1 wt% Ag,
[0162] The remainder of tin, and any unavoidable impurities.
[0163] For 1), a shear strength of only 6.3 N was obtained and a broken interconnection along the ECA joint was observed. For 2), a shear strength of 9.8 N was obtained. For 3), a shear strength of 10.5 N was obtained. In 2) and 3), it was observed that no failure occurred at the weld joint, but shear failure occurred due to failure of the PV cell material.
[0164] The methods of the present disclosure may beneficially result in improved thermal aging of interconnections between PV cells. For example, in a third test, PV cells were interconnected using:
[0165] 1)ECA,
[0166] 2) Solder paste containing Sn40Pb solder alloy,
[0167] 3) A solder paste comprising a solder alloy consisting of:
[0168] 48 to 51 wt% of Bi,
[0169] 0.7 wt% to 1.1 wt% Cu,
[0170] 0.02 wt% to 0.09 wt% Co,
[0171] 0.8 wt% to 1.1 wt% Ag,
[0172] The balance of tin, and any unavoidable impurities, and
[0173] 4) A solder paste comprising a solder alloy consisting of:
[0174] 56 to 59 wt% Bi,
[0175] 0.1 wt% to 0.3 wt% Cu,
[0176] 0.02 wt% to 0.04 wt% Co,
[0177] The remainder of tin, and any unavoidable impurities.
[0178] The samples were then heat aged according to IEC Standard 61215. After 600 and 800 test cycles, the following % power changes were observed:
[0179] Power change % at T600 cycle Power change % at T800 cycles 1) -9% -9.5% 2) -0.5% -1.25% 3) -0.5% -1.25% 4) -1.0% -2.25%
[0180] The methods of the present disclosure may beneficially result in lower contact resistances for interconnections between PV cells. For example, in a fourth test, the same adhesive / solder alloy as used in the third test was used to interconnect PV cells. The following contact resistances were observed:
[0181] Contact resistance (mΩ.cm2) 1) 3.1 2) 2.3 3) 0.55 4) 1.5
[0182] The following examples are provided for a better understanding of the present disclosure and do not limit the scope of the appended claims.
[0183] Example 1
[0184] The front face of the shingled construction cell busbars is printed by a solder paste comprising a flux having dispersed therein particles of a solder alloy of the following composition:
[0185] 48 to 51 wt% of Bi,
[0186] 0.7 wt% to 1.1 wt% Cu,
[0187] 0.02 wt% to 0.09 wt% Co,
[0188] 0.8 wt% to 1.1 wt% Ag,
[0189] The balance of tin, and any unavoidable impurities
[0190] The shingled configuration cells were prepared by laser cutting a polycrystalline 6" Al-BSF (Aluminum Back Surface Field) solar cell into five individual shingle cell strips.
[0191] Use a 3mil stencil on a DEK03Xi printer to print solder paste onto a 1mm wide busbar, as shown in Figure 6 As shown. Before reflow, the width of the printed solder paste pad is 300 to 900 microns. Before reflow, the height of the printed solder paste pad is 65 microns. After fast reflow, the solder paste is completely spread to fill the width of the busbar, as shown Figure 7 As shown in Figure 1, the solder paste pad height is reduced to 55 microns.
[0192] The strips were then shingled with a fixed overlap of 1.0 mm. The assembly was rapidly reflowed in a reflow oven at a peak temperature of 175°C. The total reflow time was less than 1 minute in a standard reflow oven. Finally, bus soldering was performed using tape attach.
[0193] The quality and strength of the joints were evaluated by determining the strength of the adhesion of the interconnect material, the die (solder paste / ECA) to the silver pads, subjecting the die (solder paste / shingled cell) to stress parallel to the plane of the die attachment substrate, resulting in shear stress between the die-die attachment material interface and the die attachment material-substrate interface. In this technique, a die shear method was used to shear the reflowed solder paste and two cell shingled construction assemblies. The solder paste assembly produced a shear strength of more than 8N for use as a reflow test as well as 2 cell shingled construction assemblies. On the other hand, ECA produced a shear strength of only about 3.4N on the shingled construction assembly. Microscopic examination of the joints revealed that the solder paste formed a thin and continuous IMC (intermetallic compound) layer with silver pads, while no IMC was formed in the case of ECA, and silver particles were found to be suspended in an organic binder matrix.
[0194] The assemblies were then analyzed for voids and cracks and then laminated using a standard vinyl acetate (EVA) laminating material at 138°C for 20 minutes.
[0195] EL (electroluminescence) imaging, IV curve values, and mechanical and environmental tests are performed on the components. The test results indicate the maximum power (P max ) value changes less than ±5%, and thus the assembly passes the reliability requirements according to IEC 61215. The thermal cycle and damp heat tests were extended to 600 cycles and 2000 hours, respectively.
[0196] Example 2 .
[0197] Example 1 was repeated except that instead of a reflow oven, IR (infrared) curing was used to fabricate the assembly. IR reflow was performed at 50% IR power for 4-5 seconds.
[0198] Example 3 .
[0199] Example 1 was repeated except that ECA was used for the shingled construction and bussing to the tin-lead ribbon was accomplished by dispensing solder paste on silver pads.
[0200] Example 4 .
[0201] IBC cells were used to make back contact assemblies. The back side of the IBC cells consisted of thin silver wires (200 microns wide). The solder paste of Example 1 was printed on those tracks and a standard copper interconnect ribbon was placed on top. Another cell could be connected via these ribbons. Complete wetting of the solder paste on the silver pads was observed. No solder ball formation or silver leaching was noted. Peel strength > 1N. Similar assemblies with ECA did not produce acceptable joint strengths.
[0202] The entire assembly was then reflowed in a reflow oven with a peak temperature of 175° C. Lamination was then performed as described in Example 1.
[0203] IV curve values as well as mechanical and environmental tests are performed on the components. The test results indicate the maximum power (P max ) value varies less than ±5%, and therefore the component passes the reliability requirements according to IEC61215.
[0204] Example 5 .
[0205] Example 4 was repeated, except that welding and lamination were achieved in a single operation. Polyolefin elastomer (POE) laminates were used for this purpose, and the lamination temperature was 168°C for 20 minutes.
[0206] Example 6 .
[0207] Example 4 was repeated except that a conductive copper foil (conductive backplane) was used instead of tape for interconnection.
[0208] Example 7 .
[0209] The glued assembly of PV cells connected in series was manufactured by an automatic interconnection machine (Sunnyworld H1300 interconnection and stringing machine). The solder paste of Example 1 was dispensed or printed onto the PV cell busbars. A stretch tape was then placed on the solder paste. The assembly passed through the preheating zone of the automatic interconnection machine. After the specified preheating time, IR (infrared) soldering was performed at 50% power for 1-2 seconds. Multiple cells were interconnected and stringed in this process. The panels were laminated and analyzed for their IV curve values as well as mechanical and environmental tests. The test results indicated that the maximum power (P max ) value varies less than ±5%, and therefore the component passes the reliability requirements according to IEC61215.
[0210] Example 8 .
[0211] Example 7 is repeated, except that a flux is used instead of solder paste. The flux comprises a binder system, preferably an organic binder system, but does not comprise a solder alloy.
[0212] Example 9 .
[0213] Example 7 was repeated except that a light-capturing tape was used. The solder paste was printed on the tape and soldered at the back side of the cell. The solder paste was soldered by the usual fluxing method or using a ready-to-use tape. TM The panels were laminated and analyzed for IV curve values as well as mechanical and environmental tests. The test results indicated the maximum power (P max) value varies less than ±5%, and therefore the component passes the reliability requirements according to IEC61215.
[0214] It should be understood that at least some of the drawings and descriptions of the present disclosure have been simplified to focus on elements relevant to a clear understanding of the present disclosure, while other elements that would be known to readers in the art may also need to be eliminated for clarity. Because such elements are well known to readers in the art and because they are not necessarily conducive to a better understanding of the present disclosure, descriptions of such elements are not provided herein.
Claims
1. A method of manufacturing a solar module by interconnecting a plurality of photovoltaic (PV) cells, wherein at least a first PV cell is interconnected to a second PV cell using a conductive adhesive comprising or consisting of a solder paste; The solder paste includes particles of a solder alloy dispersed in a flux; Wherein the solder alloy comprises a Sn-containing solder alloy, the liquidus temperature of the Sn-containing solder alloy is less than 225 ℃; wherein the solar module comprises a back contact assembly, wherein the rear face of the first PV cell is interconnected to the rear face of the second PV cell by one or more ribbons, wherein the one or more ribbons are connected to the rear face of the first PV cell and the rear face of the second PV cell using the conductive adhesive comprising or consisting of the solder paste; or wherein the solar module comprises a glued assembly, wherein the first PV cell and the second PV cell are non-overlapping, and the front face of the first PV cell is interconnected to the rear face of the second PV cell using one or more ribbons; wherein the one or more ribbons are connected to the front face of the first PV cell and the rear face of the second PV cell using the conductive adhesive comprising or consisting of the solder paste. 2 . The method of claim 1 , further comprising laminating the first PV cell and the second PV cell. 3 . The method of claim 2 , wherein the interconnection between the first PV cell and the second PV cell is established and then the first PV cell and the second PV cell are subsequently laminated. 4 . The method according to claim 3 , wherein lamination is performed at a lamination temperature lower than the liquidus temperature of the solder alloy; or wherein lamination is performed at a lamination temperature higher than the liquidus temperature of the solder alloy.
5. The method of claim 2, wherein the interconnection between the first PV cell and the second PV cell is established in situ during lamination of the first PV cell and the second PV cell; wherein lamination is performed at a lamination temperature equal to or higher than the liquidus temperature of the solder alloy. The method of claim 1 , wherein the one or more strips are one or more light-trapping strips. The method of claim 1 , wherein the solder paste is stencil printed, jet printed, or dispensed.
8. The method of claim 7, wherein the solder paste is reflowed by heating after printing, jet printing, or dispensing.
9. The method of claim 8, wherein the solder paste is reflowed using an infrared, convection oven, or a zoned reflow oven for a period of less than 1 minute.
10. The method of any preceding claim, wherein the solder alloy comprises: 45 to 59 wt% Bi; 0.1 to 1.2 wt% Cu; 0.01 wt% to 0.1 wt% Co; and Up to 1.1 wt% Ag, The balance is Sn and any unavoidable impurities. The method of claim 10 , wherein the solder alloy comprises 0.2 wt % to 1 wt % Cu. 12 . The method of claim 10 , wherein the solder alloy comprises 0.02 wt % to 0.09 wt % Co.
13. The method of claim 10, wherein the solder alloy comprises 0.8 wt% to 1.1 wt% Ag. The method of claim 10 , wherein the solder alloy comprises 48 wt % to 51 wt % Bi.
15. The method of claim 13, wherein the solder alloy consists of: 48 to 51 wt% of Bi, 0.7 wt% to 1.1 wt% Cu, 0.02 to 0.09 wt% Co, 0.8 wt% to 1.1 wt% of Ag, The balance is tin and any unavoidable impurities. The method of claim 10 , wherein the solder alloy comprises 56 to 59 wt % Bi.
17. The method of claim 16, wherein the solder alloy consists of: 56 to 59 wt% of Bi, 0.1 wt% to 0.3 wt% Cu, 0.02 to 0.04 wt% Co, The balance is Sn and any unavoidable impurities.
18. The method of any one of claims 1 to 9, wherein the solder alloy comprises a SnPb solder alloy. The method of claim 18 , wherein the solder alloy comprises 5 wt % to 70 wt % Sn and the balance Pb.
20. The method of any one of claims 1 to 9, wherein the solder alloy comprises: 35 to 60 wt% Bi; 0 wt% to 2 wt% of Ag, The balance is Sn and any unavoidable impurities.
21. The method of any one of claims 1 to 9, wherein the solder alloy comprises: 0.01 wt% to 5 wt% Ag; 0.02 wt% to 1.5 wt% Cu; The balance is Sn and any unavoidable impurities.
22. The method of any one of claims 1 to 9, wherein the solder alloy comprises: 0.01 wt% to 5 wt% Ag; 0.02 wt% to 1.5 wt% Cu; 0.08 to 20 wt% of Bi; 0 wt% to 0.1 wt% P; 0% to 0.02% by weight of a rare earth mixture consisting of a mixture of 53% by weight Ce, 24% by weight La, 16% by weight Nd, and 5% by weight Pr; and 0 wt% to 0.01 wt% Sb The balance is Sn and any unavoidable impurities.
23. The method of claim 1 or claim 10, wherein the flux comprises: Rosin and / or resin, activator, surfactants, and solvent.
24. A solar module comprising a plurality of interconnected photovoltaic (PV) cells; wherein at least a first PV cell is interconnected to a second PV cell using a conductive adhesive comprising or consisting of a solder paste; Wherein the solder paste comprises particles of a solder alloy dispersed in a flux, and the solder alloy comprises a Sn-based solder alloy having a liquidus temperature of less than 225 ℃; wherein the solar module includes a back contact assembly, wherein the rear face of the first PV cell is interconnected to the rear face of the second PV cell by one or more ribbons; or Wherein the solar module comprises a glued assembly, wherein the first PV cell and the second PV cell are non-overlapping, and the front face of the first PV cell is interconnected to the rear face of the second PV cell using one or more ribbons.
25. The solar module of claim 24, wherein the one or more strips are one or more light capturing strips.
26. The solar module of claim 24, wherein the solar module Produced according to the method of claim 1 or claim 10.
Citation Information
Patent Citations
Shingled solar cell module
US9356184B2
Method of monolithic photo-voltaic module assembly
CN102217095A
Methods of soldering to high efficiency thin film solar panels
CN102441717A
Co-included Sn-Bi-based high-strength lead-free low-temperature welding flux
CN103406686A
High impact toughness solder alloy
CN103906598A