AgNWs / rGO / TPU flexible strain sensor and preparation method thereof
Through the preparation method of AgNWs/rGO/TPU flexible strain sensor, using silver nanowires and reduced graphene oxide composite materials, the problem of small strain range and low sensitivity of the flexible strain sensor is solved, achieving high sensitivity and wide application effect.
Patent Information
- Application Number
- CN202111309416.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-06
- Publication Date
- 2024-10-08
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing flexible strain sensors have problems such as small strain range and low sensitivity, which limits their use in practical applications.
Using the preparation method of AgNWs/rGO/TPU flexible strain sensor, silver nanowires are combined with reduced graphene oxide to form a conductive material, which is coated on a polyurethane electrospun film and encapsulated into a sandwich structure using insulating flexible packaging materials. flexible strain sensor.
The sensitivity and strain range of the flexible strain sensor are improved, and a high-sensitivity detection effect is achieved. It is suitable for applications such as motion monitoring, gesture recognition, and expression recognition, and has good stability and environmental applicability.
Smart Images

Figure CN114034239B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of flexible strain sensor preparation, and specifically relates to a highly sensitive AgNWs / rGO / TPU flexible strain sensor and a preparation method thereof. Background Art
[0002] With the development of economy and the improvement of people's living standards, sensors are widely used in industrial production, medical equipment and communication connection, playing an important role in modern life and scientific research. However, traditional sensors generally use rigid materials such as silicon, which have defects such as brittleness, poor flexibility and poor ductility. They can only be used under specific conditions, which seriously restricts their application in actual production and life. Therefore, it is imperative to develop flexible sensors that are flexible, ductile and wearable.
[0003] Flexible sensors have the characteristics of flexibility, low modulus, and easy deformation, which make them very flexible and ductile. They can be used in a variety of occasions and can be easily applied to the human body to achieve wearability, and have broad application prospects. Silver nanowires have the advantages of high conductivity and flexibility, and are good active materials for preparing high-performance flexible sensors. Applying them to the preparation of flexible sensors is of great significance for the preparation of high-performance flexible sensors. However, it was found in the research process that if silver nanowires are used as active materials alone, there are still problems such as excessive contact resistance, which leads to a large amount of silver nanowires added, affecting the mechanical properties of the flexible sensor sensing material, and making the sensitivity and strain range of the flexible sensor unsatisfactory. Graphene has good flexibility and conductivity. The hydroxyl and carboxyl groups on the surface of graphene can combine with the -C=O contained in the PVP on the surface of silver nanowires through hydrogen bonds, thereby promoting the dispersion of silver nanowires and reducing the contact resistance of silver nanowires. At the same time, after the silver nanowires and graphene are composited, graphene has a certain wrapping effect on the silver nanowires, which can effectively reduce the direct exposure of the silver nanowires and reduce the resistance. However, the conductivity of graphene is relatively poor without the reduction process.
[0004] CN108562219 A provides a AgNWs / RGO composite material using vacuum filtration as a strain sensing material, which is encapsulated into a flexible strain sensor through PDMS, but the stretchability of the microporous filtration membrane is limited; the strain range is small, and the strain range and sensitivity are not discussed. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide an AgNWs / rGO / TPU flexible strain sensor and a preparation method thereof.
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a AgNWs / rGO / TPU flexible strain sensor, comprising the following steps:
[0007] 1) dissolving polyurethane in solvent I to obtain a polyurethane solution; and then electrospinning the polyurethane solution to obtain a TPU electrospun film;
[0008] 2) Set the mass ratio of AgNWs:GO=1:0.125-4 (preferably 1:1), and set the mass ratio of hydrazine hydrate:GO=7:10; then proceed as follows:
[0009] 2.1) Add the AgNWs dispersion into the GO dispersion and stir evenly to obtain an AgNWs / GO mixed dispersion;
[0010] The GO dispersion is obtained by dispersing graphene oxide in solvent II;
[0011] The AgNWs dispersion is obtained by dispersing silver nanowires in solvent III;
[0012] Note: In the GO dispersion, the concentration of GO is about 9 to 288 mg / 100 mL;
[0013] 2.2) Mix solvent II, ammonia water and hydrazine hydrate, stir evenly, and obtain a solvent II / NH3·H2O / N2H4·H2O mixed solution;
[0014] Ammonia: (step 2.1) GO dispersion solvent II + step 2.2) solvent II) = (6 ± 0.5)% by volume;
[0015] illustrate:
[0016] When solvent II is N,N-dimethylformamide (DMF), the resulting solution is named DMF / NH3·H2O / N2H4·H2O mixed solution;
[0017] The volume ratio of solvent III used for AgNWs dispersion: solvent II used for GO dispersion (step 2.1) + solvent II used in step 2.2) = (12 ± 2): 50;
[0018] 2.3) Add the AgNWs / GO mixed dispersion to a mixed solution of solvent II / NH3·H2O / N2H4·H2O, and perform a reduction reaction at a temperature of 90-100°C to reduce GO. The reduction reaction time is 10-30 min (preferably 95°C for 20 min);
[0019] The mixture was allowed to stand and cool to room temperature (~60 min), and then centrifuged to separate the solid and liquid phases. The solid phase was AgNWs / rGO, which was dispersed in solvent III (e.g., ethanol) to obtain an AgNWs / rGO / solvent dispersion.
[0020] The mass fraction of AgNWs / rGO in the AgNWs / rGO / solvent dispersion is 0.1wt%-0.5wt% (preferably 0.5wt%).
[0021] Note: rGO stands for reduced graphene oxide, which means that graphene has been reduced. Without reduction, the conductivity is poor. When solvent III is ethanol, the result is named AgNWs / rGO / ethanol dispersion.
[0022] 3) Apply (drip coating or spray coating) the AgNWs / rGO / solvent dispersion onto the surface of the TPU electrospun film, and form a coating layer after the wet film is dried; the obtained material is named AgNWs / rGO / TPU strain sensing material;
[0023] 4) Prepare the AgNWs / rGO / TPU strain sensing material into AgNWs / rGO / TPU flexible strain sensor.
[0024] The above steps 1) and 4) can be carried out using conventional steps.
[0025] As an improvement of the preparation method of the AgNWs / rGO / TPU flexible strain sensor of the present invention, solvent I, solvent II, and solvent III are any of the following: ethanol, N,N-dimethylformamide, acetone, and tetrahydrofuran.
[0026] As a further improvement of the preparation method of the AgNWs / rGO / TPU flexible strain sensor of the present invention, preferably:
[0027] Solvent I is N,N-dimethylformamide (DMF);
[0028] Solvent II is N,N-dimethylformamide (DMF);
[0029] Solvent III is ethanol.
[0030] As a further improvement of the preparation method of the AgNWs / rGO / TPU flexible strain sensor of the present invention, in step 3): the wet film thickness is (0.25±0.05) mm.
[0031] As a further improvement of the preparation method of the AgNWs / rGO / TPU flexible strain sensor of the present invention, in step 1):
[0032] The mass fraction of the polyurethane solution is 10wt% to 20wt% (preferably 15wt%); during the electrospinning process, the electrospinning temperature is 30°C, the humidity is 80 to 85%, the voltage is 20kV, the rotation speed is 1000r / min, the injection speed is 1.5mL / h, and the electrospinning time is 6-8h (preferably 8h).
[0033] As a further improvement of the preparation method of the AgNWs / rGO / TPU flexible strain sensor of the present invention, step 4) is:
[0034] A copper foil metal electrode is set on the coating layer of the AgNWs / rGO / TPU strain sensing material, and a wire is led out. Then, an insulating flexible packaging material is used to package it into a sandwich structure to obtain an AgNWs / rGO / TPU flexible strain sensor.
[0035] The present invention also provides a highly sensitive AgNWs / rGO / TPU flexible strain sensor prepared by any of the above methods.
[0036] The high-sensitivity AgNWs / rGO / TPU flexible strain sensor has a sandwich structure, which is encapsulated by an insulating flexible packaging material and prepared by arranging an AgNWs / rGO / TPU strain sensing material in the middle.
[0037] The present invention is used to solve the problems of small strain range and low sensitivity of the existing flexible strain sensors. The preparation method of the present invention is simple and efficient. The flexible strain sensor has light weight, large strain range and relatively high sensitivity.
[0038] The AgNWs / rGO / TPU flexible strain sensor and preparation method thereof of the present invention comprises the following steps: drop coating or spray coating of an AgNWs / rGO / ethanol dispersion on the surface of a TPU electrospun film to form a strain sensing material having an AgNWs / rGO microstructure on the surface, and encapsulating the material into a sandwich-structured flexible strain sensor using an insulating flexible packaging material. The AgNWs / rGO / TPU is a strain sensing material of the flexible strain sensor.
[0039] In the present invention:
[0040] Step 1): dissolving the polyurethane masterbatch in a solvent, stirring (mechanical stirring or magnetic stirring) until it is completely dissolved to obtain a polyurethane solution;
[0041] Step 2): according to different mass ratios of AgNWs / GO, GO is dispersed in a solvent, ultrasonicated, and stirred to obtain a GO dispersion; AgNWs are dispersed in a solvent, ultrasonicated, and stirred to obtain an AgNWs dispersion;
[0042] The high-sensitivity AgNWs / rGO / TPU flexible strain sensor prepared by the present invention has a strain range of up to 180% and a sensitivity coefficient of up to 2500 under the preferred embodiment, and also provides applications in motion monitoring, gesture recognition, expression recognition and stability detection.
[0043] The AgNWs / rGO / TPU flexible strain sensor and the preparation method thereof of the present invention have the following beneficial effects:
[0044] 1. In the AgNWs / rGO / TPU flexible strain sensor of the present invention, since the highly sensitive AgNWs / rGO / TPU flexible strain sensor uses polyurethane electrospun film as the base material, it has good flexibility and stretchability (experimental results Figure 4 ), can be flexibly and conveniently attached to the surface of objects of various shapes, is light in weight and has strong environmental applicability.
[0045] 2. The AgNWs / rGO / TPU flexible strain sensor of the present invention uses a drip coating or spray coating method to process the conductive material onto the surface of the flexible substrate to form a surface microstructure, so that it has a sensitivity coefficient of up to 2500 and a strain range of up to 180%.
[0046] 3. The AgNWs / rGO / TPU flexible strain sensor of the present invention is a flexible sensor, so it is suitable for wearable detection equipment. It can be used for motion monitoring, gesture recognition, expression recognition, etc., and has good stability. It has broad application prospects in wearable devices and medical detection.
[0047] In summary, the present invention prepares a silver nanowire / graphene oxide conductive material by compounding silver nanowires with graphene having good flexibility and conductivity, and reduces graphene oxide to prepare a silver nanowire / reduced graphene oxide composite material, and uses the composite material as a conductive material to prepare a flexible sensor, so as to achieve the purpose of improving the application performance of the flexible sensor. The flexible strain sensor prepared by the present invention has high durability, a wide strain range, and high sensitivity. It can be flexibly and conveniently attached to the surface of objects of various shapes, is light in weight, and has strong environmental applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings.
[0049] Figure 1 Schematic diagram of the structure of the invented AgNWs / rGO / TPU flexible strain sensor;
[0050] Figure 2 SEM morphology of the prepared AgNWs / rGO composite material;
[0051] The left picture is the SEM morphology of the AgNWs / rGO composite material, and the right picture is the SEM morphology of the AgNWs / rGO composite material enlarged in the selected area;
[0052] Figure 3 The SEM morphology of the prepared AgNWs / rGO / TPU strain sensing material;
[0053] The left picture is the SEM morphology of the TPU electrospun film, the middle picture is the SEM morphology of the AgNWs / rGO / TPU strain sensing material, and the right picture is the SEM morphology of the AgNWs / rGO / TPU strain sensing material enlarged in the selected area;
[0054] Figure 4 The stress-strain curves of the prepared TPU electrospun film and AgNWs / rGO / TPU strain sensing material;
[0055] Figure 5 The strain range test results of AgNWs / rGO / TPU strain sensing materials prepared with different drop coating amounts of AgNWs / rGO;
[0056] Figure 5 “1-5” in the table represent the dosage of AgNWs / rGO / ethanol dispersion as 1 ml, 2 ml, 3 ml, 4 ml, and 5 ml, respectively;
[0057] Figure 6 The sensitivity coefficient test results of the prepared AgNWs / rGO / TPU flexible strain sensor;
[0058] Figure 7 The stability test results of the prepared AgNWs / rGO / TPU flexible strain sensor;
[0059] The left picture shows the relative resistance change of the AgNWs / rGO / TPU flexible strain sensor after 3000 cycles of stretching, and the right picture shows the enlarged picture of the selected area after cyclic stretching;
[0060] Figure 8 Finger bending vibration signal measured by the prepared AgNWs / rGO / TPU flexible strain sensor.
[0061] Fig. 9 The vibration signals of walking and jogging measured by the prepared AgNWs / rGO / TPU flexible strain sensor.
[0062] Fig.10 The vibration signal of expression change measured by the prepared AgNWs / rGO / TPU flexible strain sensor.
[0063] Figure 2 to Figure 10 , all of which are for Example 4.
[0064] Fig.11 This is the principle diagram of the four-probe measurement method (conventional technology). DETAILED DESCRIPTION
[0065] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto:
[0066] In the following cases:
[0067] GO, graphene oxide, rGO, reduced graphene oxide;
[0068] DMF, N,N-dimethylformamide,
[0069] AgNWs, silver nanowires, average diameter ~77.6 nm; average length ~158.3 μm;
[0070] Polyurethane masterbatch, shuttle-shaped polyurethane particles with a particle size of 2.5 to 5 mm;
[0071] Ammonia water, an aqueous solution containing 25% to 28% (mass fraction) of ammonia.
[0072] During the electrospinning process, the electrospinning temperature was 30°C, the humidity was 80-85%, the voltage was 20 kV, the rotation speed was 1000 r / min, the injection speed was 1.5 mL / h, and the electrospinning time was 8 h.
[0073] Embodiment 1,
[0074] The invention relates to an AgNWs / rGO / TPU flexible strain sensor and a preparation method thereof, wherein the AgNWs / rGO / ethanol dispersion is drop-coated or sprayed on the surface of a TPU electrospun film and then encapsulated into a sandwich-structured flexible strain sensor by an insulating flexible packaging material.
[0075] The specific steps are as follows:
[0076] 1) Dissolve the polyurethane masterbatch in DMF, stir magnetically until completely dissolved, obtain a 15 wt% polyurethane solution, and electrospin for 8 h to obtain an electrospun TPU film (thickness is about 0.18 ± 0.05 mm);
[0077] 2) Set the mass ratio of AgNWs:GO = 1:0.125, and the mass ratio of hydrazine hydrate:GO = 7:10; then proceed as follows:
[0078] 2.1) Add the AgNWs dispersion into the GO dispersion and stir evenly to obtain an AgNWs / GO mixed dispersion;
[0079] The GO dispersion is prepared by dispersing 1.8 mg of graphene oxide in 20 ml of DMF under ultrasonic stirring conditions;
[0080] The AgNWs dispersion is obtained by dispersing 14.4 mg of silver nanowires in 12 ml of ethanol under ultrasonic stirring conditions;
[0081] 2.2) Mix 30 ml of DMF, 3 ml of ammonia water and 1.26 mg of hydrazine hydrate, stir evenly to obtain a DMF / NH3·H2O / N2H4·H2O mixed solution.
[0082] Therefore, the volume ratio of ammonia: (DMF used in step 2.1) GO dispersion + DMF used in step 2.2) = 6%;
[0083] 2.3) Add the AgNWs / GO mixed dispersion to a mixed solution of DMF / NH3·H2O / N2H4·H2O, and perform reduction reaction at 95°C for 20 min to reduce GO and obtain an AgNWs / rGO dispersion;
[0084] The mixture was allowed to stand and cool to room temperature (~60 min), and then centrifuged to separate the solid and liquid. The solid phase was AgNWs / rGO, and the solid phase was dispersed in ethanol to obtain an AgNWs / rGO / ethanol dispersion with a mass fraction of 0.5 wt% of AgNWs / rGO.
[0085] 3) Drop or spray 5 mL of AgNWs / rGO / ethanol dispersion onto the surface of TPU electrospun film (about 3×3 cm in size), with a wet film thickness of 0.25 mm, and dry (dry to constant weight at room temperature) to obtain AgNWs / rGO / TPU strain sensing material;
[0086] 4) Cut the above-mentioned AgNWs / rGO / TPU strain sensing material into 1×3cm, set a copper foil metal electrode on the coating layer of the AgNWs / rGO / TPU strain sensing material, lead out the wire, and then use the upper and lower layers of insulating flexible packaging material 3MVHB glue to package it into a sandwich structure to obtain an AgNWs / rGO / TPU flexible strain sensor.
[0087] The thickness of the single-sided VHB adhesive layer is about 1.0 mm.
[0088] Embodiment 2,
[0089] Step 2) of Example 1 is changed as follows:
[0090] The mass ratio of AgNWs:GO was set to 1:0.25, so in step 2), the silver nanowires were 14.4 mg, the graphene oxide was 3.6 mg, and the hydrazine hydrate was 2.52 mg;
[0091] The rest is the same as Example 1.
[0092] Embodiment 3,
[0093] Step 2) of Example 1 is changed as follows:
[0094] The mass ratio of AgNWs:GO was set to 1:0.5, so in step 2), the silver nanowires were 14.4 mg, the graphene oxide was 7.2 mg, and the hydrazine hydrate was 5.04 mg;
[0095] The rest is the same as Example 1.
[0096] Embodiment 4,
[0097] Step 2) of Example 1 is changed as follows:
[0098] The mass ratio of AgNWs:GO was set to 1:1, so in step 2), the silver nanowires were 14.4 mg, the graphene oxide was 14.4 mg, and the hydrazine hydrate was 10.08 mg;
[0099] That is, the entire step 2) is as follows:
[0100] 2) Set the mass ratio of AgNWs:GO = 1:1, and the mass ratio of hydrazine hydrate:GO = 7:10; then proceed as follows:
[0101] 2.1) Add the AgNWs dispersion into the GO dispersion and stir evenly to obtain an AgNWs / GO mixed dispersion;
[0102] The GO dispersion is prepared by dispersing 14.4 mg of graphene oxide in 20 ml of DMF under ultrasonic stirring, with a concentration of 72 mg / 100 mL;
[0103] The AgNWs dispersion is prepared by dispersing 14.4 mg of silver nanowires in 12 ml of ethanol under ultrasonic stirring, with a concentration of 0.12 g / 100 mL;
[0104] 2.2) Mix 30 ml of DMF, 3 ml of aqueous ammonia and 10.08 mg of hydrazine hydrate, stir evenly to obtain a DMF / NH3·H2O / N2H4·H2O mixed solution.
[0105] 2.3) Add the AgNWs / GO mixed dispersion to a mixed solution of DMF / NH3·H2O / N2H4·H2O, and perform reduction reaction at 95°C for 20 min to reduce GO and obtain an AgNWs / rGO dispersion;
[0106] The mixture was allowed to stand and cool to room temperature (~60 min), and then centrifuged to separate the solid and liquid. The solid phase was AgNWs / rGO, and the solid phase was dispersed in ethanol to obtain an AgNWs / rGO / ethanol dispersion with a mass fraction of 0.5 wt% of AgNWs / rGO.
[0107] The rest is the same as Example 1.
[0108] The SEM morphologies of the AgNWs / rGO composite material and the AgNWs / rGO / TPU strain sensing material prepared in Example 4 are shown in FIG. Figure 2 and Figure 3 shown.
[0109] Embodiment 5,
[0110] Step 2) of Example 1 is changed as follows:
[0111] The mass ratio of AgNWs:GO was set to 1:2, so in step 2), the silver nanowires were 14.4 mg, the graphene oxide was 28.8 mg, and the hydrazine hydrate was 20.16 mg;
[0112] The rest is the same as Example 1.
[0113] Embodiment 6,
[0114] Step 2) of Example 1 is changed as follows:
[0115] The mass ratio of AgNWs:GO was set to 1:4, so in step 2), the silver nanowires were 14.4 mg, the graphene oxide was 57.6 mg, and the hydrazine hydrate was 40.32 mg;
[0116] The rest is the same as Example 1.
[0117] Experiment 1
[0118] like Fig.11 , a dual-electric four-probe device is used to test the surface resistivity of conductive materials. The principle of the device is: four probes are made of tungsten wires and are arranged in a straight line with equal spacing. The spacing between every two tungsten wires is s (about 1mm). During measurement, the four needle tips are pressed on the surface of the sample to be tested, and a current I (0.5~2mA) is passed through the two outermost probes (i.e., probes 1 and 4). The voltage V is measured by the two inner probes. When the length and width of the sample to be tested are much larger than the needle tip spacing s, that is, when the closest distance between the edge and the probe is at least 4 times the needle tip spacing s, c=4.53 is set, and the square resistance of the sample to be tested is expressed as: R s =cV / I, the sheet resistance of the sample being tested is related to the measured voltage and the magnitude of the current passing through.
[0119] The results obtained in Examples 1 to 6 are shown in Table 1 below.
[0120] Table 1. Surface resistivity (Ω·cm) of AgNWs / rGO composite conductive materials prepared with different mass ratios of AgNWs to GO
[0121] Example 1 Example 2 Example 3 Example 4 Example 5 Example 6 67.08 43.18 25.98 10.43 59.87 91.47
[0122] Experiment 2
[0123] For Example 4, the structure of the AgNWs / rGO composite material was characterized by scanning electron microscopy. Figure 2 , the silver nanowires are inserted into the surface and interior of the reduced graphene oxide, forming a conductive network structure in which the graphene wraps the silver nanowires. The results of the remaining embodiments are not significantly different from those of embodiment 4.
[0124] Experiment 3
[0125] For Example 4, the AgNWs / rGO / TPU strain sensing material was characterized by scanning electron microscopy. Figure 3 , the pure TPU electrospun membrane presents a network structure with a diameter of about 0.5-1μm. After the AgNWs / rGO composite conductive material is drop-coated, the network structure of the TPU electrospun membrane disappears, and the composite conductive material forms a dense covering layer on its surface. Further magnifying the covering layer, it can be seen that the AgNWs are uniformly dispersed in the rGO, and the silver nanowires are inserted into the reduced graphene oxide to form a conductive path, which is conducive to improving the conductivity of the AgNWs / rGO / TPU electrospun membrane. The results of the remaining embodiments are not significantly different from those of Example 4.
[0126] Experiment 4
[0127] For Example 4, the stretchability of the TPU electrospun film and the AgNWs / rGO / TPU strain sensing material was tested using a universal experimental material machine. Figure 4 The TPU electrospun film and the AgNWs / rGO / TPU strain sensing material have good flexibility and stretchability, and can be stretched to more than 350%. The results of the remaining embodiments are not significantly different from those of embodiment 4.
[0128] Experiment 5: In order to demonstrate the importance of the amount of AgNWs / rGO, the amount of "AgNWs / rGO / ethanol dispersion" in step 3) of Example 4 was changed from 5 mL to 1 ml, 2 ml, 3 ml, and 4 ml respectively, and the rest was the same as Example 4. The obtained products were subjected to the following experiments:
[0129] The resistance change rate of the flexible strain sensor during the stretching process is tested by combining a universal experimental material machine with a digital multimeter to determine its strain range.
[0130] The resistance change rate can be calculated using the formula △R = (R-R0) / R0×100%, where △R is the resistance change rate, R is the real-time resistance during the stretching process, and R0 is the original resistance before stretching. Figure 5At different drop coating amounts of AgNWs / rGO, the AgNWs / rGO / TPU flexible strain sensor shows different strain ranges. When the drop coating amount of AgNWs / rGO is 5mL, the strain range of the AgNWs / rGO / TPU flexible strain sensor can reach 186.88%.
[0131] The details are shown in Table 2.
[0132] Table 2
[0133]
[0134] Experiment 6
[0135] For Example 4, the resistance change rate of the flexible strain sensor during the stretching process is tested by combining a universal experimental material machine with a digital multimeter, thereby obtaining the sensitivity coefficient of the flexible strain sensor. The sensitivity coefficient is calculated according to the formula GF = △R / (R0*ε), where △R is the resistance change rate, R is the real-time resistance during the stretching process, R0 is the original resistance before stretching, and ε is the strain change of the AgNWs / rGO / TPU strain sensitive material. Figure 6 When the drop coating amount of AgNWs / rGO is 5mL, the sensitivity coefficient of the AgNWs / rGO / TPU flexible strain sensor can reach more than 2500.
[0136] Experiment 7
[0137] For Example 4, a universal experimental material machine was combined with a digital multimeter to stretch the AgNWs / rGO / TPU flexible strain sensor by 25% of its original length, and the stretch-release cycle was repeated 3000 times to test the relative resistance change of the AgNWs / rGO / TPU flexible strain sensor during this process. Figure 7 It shows that the maximum value of the relative resistance of the AgNWs / rGO / TPU flexible strain sensor does not change much, and each stretching-release cycle has good reproducibility, showing good stability.
[0138] Experiment 8
[0139] For Example 4, the AgNWs / rGO / TPU flexible strain sensor was attached to different parts of the human body (fingers, knees, eyebrows), connected to a digital multimeter, and the relative resistance change of the AgNWs / rGO / TPU flexible strain sensor was tested when different parts of the human body moved, which was used for real-time detection of human physiological indicators. Figure 8 to Figure 10 The display can detect real-time movements such as bending fingers, walking, running and frowning.
[0140] Comparative Example 1-1: The amount of ammonia water in Example 4 was changed from "3 mL" to "6 mL". Therefore, the volume ratio of ammonia water: (DMF used in step 2.1) GO dispersion + DMF used in step 2.2)) = 12%; the rest is the same as Example 4.
[0141] Comparative Example 1-2: The amount of ammonia water in Example 4 was changed from "3 mL" to "1.5 mL". Therefore, the volume ratio of ammonia water: (DMF used in step 2.1) GO dispersion + DMF used in step 2.2)) = 3%; the rest is the same as Example 4.
[0142] Comparative Example 2-1: The mass ratio of hydrazine hydrate to graphene oxide in Example 4 was changed from "7:10" to "1:1";
[0143] That is, relative to Example 4, step 2) is changed as follows: the amount of hydrazine hydrate used is changed from "10.08 mg" to "14.4 mg". The rest is the same as Example 4.
[0144] Comparative Example 2-2: The mass ratio of hydrazine hydrate to graphene oxide in Example 4 was changed from "7:10" to "10:7";
[0145] That is, relative to Example 4, step 2) is changed as follows: the amount of hydrazine hydrate used is changed from "10.08 mg" to "20.57 mg". The rest is the same as Example 4.
[0146] The above Comparative Examples 1-1 to Comparative Example 2-2 were tested according to the above Experiment 1, and the obtained results were compared with those of Example 4, as shown in the following Table 3:
[0147] Table 3
[0148]
[0149] In the four comparative examples, the surface resistivity of AgNWs / rGO / TPU strain sensing materials all showed an increase to varying degrees.
[0150] Finally, it should be noted that the above examples are only some specific embodiments of the present invention. Obviously, the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by a person skilled in the art should be considered as the protection scope of the present invention.
Claims
1. Preparation method of AgNWs / rGO / TPU flexible strain sensor, characterized in that The steps include: 1) dissolving polyurethane in solvent I to obtain a polyurethane solution; and then electrospinning the polyurethane solution to obtain a TPU electrospun film; solvent I is N,N-dimethylformamide; 2) Set the mass ratio of AgNWs:GO = 1:1, and the mass ratio of hydrazine hydrate:GO = 7:10; then proceed as follows: 2.1) Add the AgNWs dispersion into the GO dispersion and stir evenly to obtain an AgNWs / GO mixed dispersion; The GO dispersion is obtained by dispersing graphene oxide in solvent II; The AgNWs dispersion is obtained by dispersing silver nanowires in solvent III; 2.2) Mix solvent II, aqueous ammonia and hydrazine hydrate, stir evenly, and obtain a solvent II / NH3·H2O / N2H4·H2O mixed solution; Ammonia: (step 2.1) GO dispersion solvent II + step 2.2) solvent II) = (6 ± 0.5)% by volume; 2.3) Add the AgNWs / GO mixed dispersion to a mixed solution of solvent II / NH3·H2O / N2H4·H2O, and perform a reduction reaction at a temperature of 90-100°C to reduce GO. The reduction reaction time is 10-30 min. The mixture was allowed to stand and cool to room temperature, and then centrifuged to separate the solid and liquid. The solid phase was AgNWs / rGO, which was dispersed in solvent III to obtain AgNWs / rGO / solvent dispersion. The mass fraction of AgNWs / rGO in the AgNWs / rGO / solvent dispersion is 0.5wt%; Solvent II is N,N-dimethylformamide; Solvent III is ethanol; 3) Applying the AgNWs / rGO / solvent dispersion to the surface of the TPU electrospun film, and drying the wet film to form a coating layer; the resulting material is named AgNWs / rGO / TPU strain sensing material; Wet film thickness is (0.25±0.05) mm; 4) Prepare the AgNWs / rGO / TPU strain sensing material into an AgNWs / rGO / TPU flexible strain sensor; In the step 1): The mass fraction of the polyurethane solution is 10wt% to 20wt%; during the electrospinning process, the electrospinning temperature is 30°C, the humidity is 80 to 85%, the voltage is 20kV, the rotation speed is 1000r / min, the injection speed is 1.5mL / h, and the electrospinning time is 6-8h; The step 4) is: A copper foil metal electrode is set on the coating layer of the AgNWs / rGO / TPU strain sensing material, and a wire is led out. Then, an insulating flexible packaging material is used to package it into a sandwich structure to obtain an AgNWs / rGO / TPU flexible strain sensor.
2. The AgNWs / rGO / TPU flexible strain sensor with high sensitivity prepared by the method as described in claim 1.