Reflective diffraction grating capable of resisting high peak energy ultrashort pulse light flux and manufacturing method thereof

By adopting a reflective diffraction grating with a multimetal layer structure, combining a metal layer with high reflection coefficient and a high electron-phonon coupling coefficient, the problem of high efficiency diffraction efficiency and high peak energy flux resistance over wide spectral bandwidth in the prior art is solved. , effectively resisting ultra-short pulse laser.

CN114041072BActive Publication Date: 2024-11-08HORIBA FRANCE SAS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080044906.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-04-19
Filing Date
2020-04-17
Publication Date
2024-11-08
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high-efficiency diffraction efficiency and high peak energy ultra-short pulse laser flux resistance at the wide spectral bandwidth. Especially in the femtosecond range, the damage threshold of traditional metal diffraction gratings is difficult to meet high-energy and ultra-short. Pulse laser demand.

Method used

The reflective diffraction grating adopts a multi-metal layer structure, including an outer reflective layer and an intermediate metal layer. The outer reflective layer is composed of a first metal with a high reflection coefficient, and the intermediate metal layer is composed of another metal with a high electron-phonon coupling coefficient, and Increase luminous flux resistance by optimizing thickness and material selection.

Benefits of technology

Maintaining high diffraction efficiency over a wide spectrum bandwidth, suitable for pulse compression, expands the working domain, can resist fluxes of more than 100mJ/cm² at 25fs pulses, and improves the durability of the diffraction grating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114041072B_ABST
    Figure CN114041072B_ABST
Patent Text Reader

Abstract

The invention relates to a reflective diffraction grating, comprising at least one intermediate metal layer (14), which is arranged between an outer reflective layer (13) and a surface (10) of a substrate comprising grating lines (11), the outer reflective layer (13) being formed of a first metal and a metal alloy, and the intermediate metal layer (14) being formed of another metal, the other metal having an electron-phonon coupling coefficient greater than that of the first metal or the metal alloy, the outer reflective layer (13) having a thickness within a range having a lower limit determined by the reflection coefficient of the first metal and an upper limit determined by the thermal diffusion length of the first metal, and the intermediate metal layer (14) having another thickness greater than a minimum value, so as to increase the resistance of the reflective diffraction grating to ultrashort pulse light flux having high peak energy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates generally to the field of diffraction gratings for use with high energy lasers, for example for laser pulse compression.

[0002] More specifically, the invention relates to a high peak energy ultrashort pulse laser flux-resistant reflection diffraction grating and a method for manufacturing the grating. Background Art

[0003] Especially in the research fields of nuclear fusion, plasma physics and fundamental physics, the energy of ultrashort pulse lasers (with pulse duration less than ~500fs) currently used is getting higher and higher, reaching peak energies approaching or exceeding petawatts (PW).

[0004] Currently, the maximum energy of the laser chain optics is limited by the flux resistance of the laser chain optics. The laser flux resistance of the optics depends inter alia on the pulse energy density per surface unit and duration.

[0005] The CPA (Chirped Pulse Amplification) technology partially solves the problem of damage threshold of optical components in high-energy pulsed lasers. The principle of CPA is to time-stretch the light pulse, thereby reducing its peak energy, amplify the time-stretched pulse, and then time-recompress the amplified pulse at the end of the laser chain to obtain high-energy short pulses. Therefore, the light energy during amplification can be reduced by several orders of magnitude. However, the risk of damaging optical components in the stage of performing pulse compression still exists, especially based on the use of diffraction gratings. Some of these components are indeed exposed to energy-amplified and time-compressed pulses, which have the highest peak energy. Therefore, the diffraction grating of the compressor is the limiting component in terms of flux resistance.

[0006] Diffraction gratings used for pulse compression are typically conventional metal gratings. For pulse compression in the infrared region (800nm, 1053nm or 1550nm), aluminum gratings are not used because their diffraction efficiency is usually below 90% and is insufficient. On the other hand, silver diffraction gratings are oxidizable and are therefore rarely used. Instead, gratings covered with a layer of gold are used. Gold-based gratings provide excellent diffraction efficiency over a wide spectral bandwidth, and since gold is a stainless material, no protective layer is required. However, the difficulty with gold-based gratings is the limited laser flux resistance in the femtosecond regime. In addition, the damage threshold of gold-based diffraction gratings depends on many parameters, such as laser fluence, pulse duration and repetition rate.

[0007] Another way to increase diffraction efficiency and flux resistance is to make diffraction gratings on dielectric mirrors (MLD: multi-layer dielectric). MLD gratings usually consist of an alternating stack of two large layers of completely transparent dielectric material with different optical indices and alternating in the thickness direction, and a grating formed in the last thin layer at the surface of the multilayer stack. These MLD gratings are described in detail in many articles, for example: Shore et al., "Design of high-efficiency dielectric reflection grating", JOSA A, Vol. 14, No. 5, pp. 1124-1136, Hehl et al., "High-Efficiency Dielectric Reflection Gratings: Design, Fabrication, and Analysis", Applied Optics, Vol. 38, No. 30, pp. 6257-6271, Bonod et al., "Design of diffraction gratings for multipetawatt laser compressors", Proc. SPIE, Vol. 5962, 59622M (2005). These publications suggest the fabrication of diffraction gratings based on completely dielectric, transparent and non-absorbing materials, including a large number of double layers, to allow obtaining MLD gratings with a flux resistance 2 to 3 times higher than that of gratings including a single layer of gold. In theory, MLD gratings also have a higher diffraction efficiency than gold-based gratings. Depending on the application, there is currently a competition between gold-based diffraction gratings and MLD gratings.

[0008] However, MLD gratings are more complex than metal gratings and therefore more expensive to manufacture. In addition, the spectral bandwidth of MLD gratings (tens of nm) is too limited to be used in ultrashort pulse (<50fs) laser chains. In fact, the duration of a laser pulse is linked to the spectral bandwidth of the laser through the Fourier transform, which means that the product of the pulse duration and the spectral bandwidth of the light is a constant. By way of information, at the central wavelength of 800nm ​​commonly used today, this product is approximately equal to 1000fs.nm, which means that to obtain pulses with a temporal width of less than 10fs, a bandwidth of more than 100nm is required. This article discusses very high efficiency bandwidths (>90%) over the wavelength domain around the central wavelength of interest. MLD diffraction gratings cannot have this type of bandwidth performance. The bandwidth of MLD gratings at the central wavelength of 1053nm is typically less than 50nm.

[0009] Flux resistance of optical components (materials, mirrors, diffraction gratings) exposed to laser pulses is still a vast field of research and all phenomena have yet to be explained. The damage induced in materials by laser flux in the nanosecond to picosecond pulse range is now well known. In the femtosecond regime, new phenomena emerge and the damage modes are different.

[0010] In the picosecond and nanosecond range, the main phenomena are thermal in nature and are related to absorption, especially for metallic gratings. Whatever the material, the damage threshold follows the square root law of the pulse duration. The following articles describe laser damage measurements and models for a certain number of mirrors and diffraction gratings: Stuart et al., "Optical ablation by high-power short-pulse lasers", JOSA B, Volume 13, Issue 2, Pages 459-468, Tien et al., "Short-pulse laser damage in transparent materials as a function of pulse duration", Physical Review Letters, Volume 82, Issue 19, May 10, 1999, Pages 3883-3886.

[0011] For femtosecond pulse durations, this law is deviated from and the physics at the local scale of the grating lines seems to be related to the square of the electric field of the electromagnetic light wave in the material. Thus, the following articles show that: Britten et al. "Multilayer dielectric gratings for petawatt-class laser systems", SPIE Proceedings, Vol. 5273, pp. 1-7 (2004), Neauport et al. "Effect of electric field on laser induced damage threshold of multilayer dielectric gratings", Optics Express, Vol. 15, No. 19, pp. 12508-12522, that in the femtosecond regime (pulse duration less than 500 fs) the damage of diffraction gratings is closely related to the square of the electric field in the material constituting the diffraction grating line profile.

[0012] In fact, for very efficient diffraction gratings, i.e., whose diffracted energy is almost entirely concentrated in the useful diffraction order (the -1 order for this type of grating), a standing wave is formed due to the interference of the incident field with the diffracted field, and the amplitude of the electric field near or inside the material can be twice that of the incident field. Electric field enhancement is then discussed.

[0013] There are conventional metallic diffraction gratings that operate in TE or TM polarization and are metallized, typically gold. The electric field at metal and metal-vacuum interfaces exhibits regions of significant electromagnetic field enhancement at certain points of the line profile that constitute flux-resistant weak regions.

[0014] Of course, the laser flux resistance also depends on the manufacturing quality of the grating, especially the purity, density, presence of impurities or defects (cracks, inclusions, bubbles, roughness) of the material used.

[0015] Patent document WO2010 / 125308_A1 describes a reflective diffraction grating, comprising a metal surface forming grating lines covered by a thin dielectric layer. This diffraction grating structure is intended to push the interference area of ​​the electric field out of the diffraction grating. This metal-dielectric grating has very high diffraction efficiency and better light flux resistance in the femtosecond regime.

[0016] However, in general, it is still desirable to push back the damage threshold of diffraction gratings that are intended to be exposed to very high energy, ultrashort pulsed optical fluxes.

[0017] Furthermore, it is desirable to increase the spectral response of a diffraction grating with improved flux resistance, ie to increase the diffraction efficiency and / or the spectral bandwidth.

[0018] However, modeling physical phenomena in the range of ultrashort optical pulses is very difficult, and in the current state of knowledge, it is not possible to predict the response of any diffraction grating to an intense laser flux, let alone to propose a diffraction grating structure that simultaneously exhibits improved flux resistance and high diffraction efficiency over a wide spectral bandwidth. Summary of the invention

[0019] In order to make up for the above-mentioned shortcomings of the prior art, the present invention proposes a high peak energy ultrashort pulse light flux resistant reflection diffraction grating, which includes grating lines formed on the surface of a substrate and an outer reflection layer.

[0020] More specifically, according to the present invention, a diffraction grating is proposed, comprising at least one intermediate metal layer, which is arranged between an outer reflection layer and a substrate surface including grating lines, the outer reflection layer having an interface with the intermediate metal layer, the outer reflection layer being composed of a first metal, and the intermediate metal layer being composed of another metal, the other metal having an electron-phonon coupling coefficient higher than that of the first metal, the outer reflection layer having a thickness within a range having a lower limit determined by the reflection coefficient of the first metal and an upper limit determined by the thermal diffusion length of the first metal, and the intermediate metal layer having another thickness greater than a minimum value, so as to increase the high peak energy ultrashort pulse light flux resistance of the reflection diffraction grating.

[0021] In this document, "first metal" refers to a material composed of a pure metal or a metal alloy.

[0022] Similarly, "another metal" refers to a material composed of another pure metal or another metal alloy.

[0023] Compared to conventional diffraction gratings with gold wires, the diffraction grating obtained in this way operates over a wide spectral bandwidth, is suitable for pulse compression, and maintains diffraction efficiency. For ultrashort pulses with duration less than 20 fs, the working domain of the diffraction grating obtained in this way is extended in both duration and fluence, allowing it to withstand more than 100 mJ.cm for a pulse of 25 fs, for example. -2 The injection amount.

[0024] Further non-limiting and advantageous features of the diffraction grating according to the invention, alone or in all technically possible combinations, are as follows:

[0025] - the first metal is selected from gold and silver, or alloys of gold and / or silver and / or other materials, such as gold-nickel, gold-copper, gold-silver, gold-silver-iridium or gold-copper-silver-iridium alloy;

[0026] - preferably, the first metal is gold or a gold alloy;

[0027] - the thickness of the outer reflective layer is between 100 nm and 500 nm, and preferably between 100 nm and 150 nm;

[0028] - the other metal is selected from nickel, copper, molybdenum, chromium, silver or a silver-iridium alloy;

[0029] The thickness of the intermediate metal layer is between 20 nm and 250 nm, for example between 50 nm and 150 nm.

[0030] In a specific and advantageous embodiment, the diffraction grating further comprises an adhesive layer arranged on the substrate surface comprising the grating lines, the adhesive layer being arranged between the substrate surface and the intermediate metal layer, the thickness of the adhesive layer being less than 25 nm, preferably less than 10 nm.

[0031] Advantageously, the bonding layer is made of chromium or titanium.

[0032] Advantageously, the substrate is made of silicon dioxide, silicon, glass-ceramic, pyrex or borosilicate (BK7).

[0033] Preferably, the grating lines are formed in the substrate. Alternatively, the grating lines are formed by a photosensitive resin deposited on the substrate.

[0034] Advantageously, the diffraction grating further includes a dielectric thin film coating formed at a surface of the outer reflective layer.

[0035] In a particular and advantageous embodiment, the diffraction grating further comprises at least one further intermediate metal layer arranged between the substrate and the intermediate metal layer, the intermediate metal layer and the further intermediate metal layer forming a stack of several intermediate metal layers.

[0036] The present invention also proposes a method for manufacturing a reflective diffraction grating, comprising the following steps: forming diffraction grating lines on the surface of a substrate; depositing an intermediate metal layer, and depositing an outer reflective layer, the outer reflective layer having an interface with the intermediate metal layer, the outer reflective layer being composed of a first metal, and the intermediate metal layer being composed of another metal, the other metal having an electron-phonon coupling coefficient higher than that of the first metal, the outer reflective layer having a thickness within a range having a lower limit determined by the reflection coefficient of the first metal and an upper limit determined by the thermal diffusion length of the first metal, and the intermediate metal layer having another thickness greater than a minimum value to increase the high peak energy ultrashort pulse light flux resistance of the reflective diffraction grating.

[0037] According to a particular and advantageous embodiment, the method further comprises an additional step of depositing an adhesion layer on the grating lines before the step of depositing the intermediate metal layer.

[0038] Of course, the different features, alternatives and embodiments of the invention can be associated with each other according to various combinations, as long as they are not mutually incompatible or mutually exclusive. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Furthermore, various other features of the present invention will become apparent from the additional description made with reference to the accompanying drawings showing non-limiting embodiments of the present invention, in which:

[0040] [ Figure 1 ] schematically shows a cross-sectional view of several lines of a metal diffraction grating according to the prior art in a plane transverse to the direction of the grating lines;

[0041] [ Figure 2 ] schematically shows a cross-sectional view of several lines of a multi-metal diffraction grating according to an embodiment of the present invention;

[0042] [ Figure 3 ] schematically shows a cross-sectional view of several lines of a multi-metal diffraction grating according to another embodiment of the present invention.

[0043] It should be noted that in these figures, structural and / or functional elements common to different alternative embodiments may be denoted by the same reference numerals. DETAILED DESCRIPTION

[0044] The present disclosure relates specifically to a method for increasing the laser flux resistance of a metal reflective diffraction grating subjected to ultraintense and ultrashort laser pulses (pulse duration <500 fs).

[0045] The current working spectral domain of ultrashort lasers is in the near infrared (700nm-1100nm). Ultrashort pulses are mainly generated at a central wavelength of 800nm, which is in the middle of the gain range of the most commonly used titanium:sapphire crystal in ultrashort pulse laser chains.

[0046] The fabrication of the diffraction grating will now be considered.

[0047] The substrate 1 is usually made of silicon dioxide, silicon or is formed of an optical ceramic matrix (for example, microcrystalline glass, heat-resistant glass or BK7 type). The surface 10 of the substrate 1 is polished in advance in such a way that the residual surface roughness is less than a part of the wavelength used. The surface 10 can be flat, concave or convex. Diffraction grating lines 11 are formed on the surface 10 of the substrate 1 by methods known to those skilled in the art. A known method is based on direct etching of the surface of the substrate to form grating lines. Another known method is based on holographic technology from a main grating and photolithography technology applied to a photosensitive resin layer deposited on the substrate. These lines extend in a direction roughly parallel to the surface of the substrate. The profile of the grating lines in a plane transverse to the direction of the lines can be square, rectangular, trapezoidal or pseudo-trapezoidal, symmetrical or asymmetrical triangle, or can also be a sine or pseudo-sine shape relative to a plane of the surface 10 of the substrate transverse to the direction including the grating lines. The pitch P of the diffraction grating is usually between about 800 and 2400 lines / mm.

[0048] Advantageously, it is also known to deposit a thin bonding layer 2, for example by evaporation, on the surface of the lines 11 comprising the diffraction grating. The thin bonding layer 2 is typically a thin layer of chromium or titanium with a thickness of a few nanometers (less than about 25 nm, preferably less than 10 nm). A reflective metal layer 3 is formed on the thin bonding layer 2, for example by evaporation. Alternatively, the reflective metal layer 3 can be formed directly on the surface of the diffraction grating lines 11 without a bonding layer. The reflective metal layer 3 is typically made of gold or aluminum, sometimes of silver. The thickness of the reflective layer 3 is typically between 100 nm and 500 nm. This thickness makes it possible to obtain a high reflection coefficient and therefore a high diffraction efficiency while limiting the surface roughness of the grating lines.

[0049] Figure 1 An example of a metal diffraction grating of the prior art is shown, comprising a substrate 1, diffraction grating lines 11 formed on a surface 10 of the substrate in a photosensitive resin layer, for example by photolithography, a thin adhesive layer 2 deposited on the grating lines 11, and a reflective metal layer 3 deposited on the thin adhesive layer 2.

[0050] A discovery within the scope of the present disclosure is that after exposure to very high energy, ultrashort pulsed optical flux, the damage of conventional metal diffraction gratings with a gold layer results in the formation of pits caused by a melting phenomenon of the gold layer. At the gold layer and the gold-vacuum interface, the optical flux corresponds to an electric field that shows significant areas of field enhancement at certain points of the grating profile, which constitute weak areas of resistance to very high energy, ultrashort pulsed laser flux.

[0051] In contrast to metal-dielectric gratings that are intended to push the electric field maximum out of the diffraction grating, the present disclosure proposes replacing the reflective metal layer 3 of the conventional grating with a stack of at least two metal layers, including an outer reflective layer 13 intended to be exposed to the incident light flux and at least another underlying intermediate metal layer 14. The outer reflective layer 13 and the intermediate metal layer 14 are composed of different metals and each has a thickness suitable for reducing the temperature in the outer reflective layer 13.

[0052] However, there is no simulation model that considers the distribution of the electromagnetic field of an ultrashort pulse coupled to a diffraction grating comprising a stack of multiple metal thin layers. In fact, the diffraction grating has a two-dimensional structure that changes the spatial distribution of the electromagnetic field. Therefore, the modeling of a reflective diffraction grating is much more complicated than the modeling of a flat mirror.

[0053] On the one hand, a first metal with high reflectivity in the spectral range of interest and relatively small thickness is selected for the outer reflective layer. On the other hand, another metal with high electron-phonon coupling coefficient, high heat resistance and sufficient thickness is selected for the intermediate metal layer.

[0054] When choosing the material for the intermediate metal layer, the electron-phonon coupling constant is essential. The electron-phonon coupling coefficient of most metal materials is known. The values ​​of the electron-phonon coupling coefficient of different metals at ambient temperature can be found in the scientific literature.

[0055] [Table 1] Table 1 shows the electron-phonon coupling coefficients of different metals.

[0056]

[0057] Without being bound by the explanation of the physical phenomena involved, the purpose of adding a metallic intermediate layer with high electron-phonon coupling in contact with the outer reflective layer is to increase the heat exchange kinetics between the heating-induced electrons in the outer reflective layer and the phonons of the intermediate metal layer. Therefore, the combination of the outer reflective layer 13 and the intermediate metal layer 14 and their respective thicknesses are therefore selected to allow a local reduction in the temperature in the outer reflective layer 13. The combination of different metal thin layers makes it possible to shift the thermal equilibrium point generated by the interaction of the laser with the material and to concentrate the thermal energy, preferably at the intermediate metal layer. The latter is selected because it has a higher resistance to thermal energy relative to the outer reflective layer.

[0058] Preferably, an intermediate metal layer 14 made of nickel, molybdenum, copper, chromium, silver or a silver-iridium alloy is selected. The intermediate metal layer 14 has a thickness (denoted by d) greater than a minimum value to allow absorption and diffusion of heat from the outer metal layer. However, in practice, the thickness d of the intermediate metal layer 14 is less than the maximum value, on the one hand to avoid increasing the surface roughness, and on the other hand to maintain the shape of the grating line profile. For example, the thickness d of the intermediate metal layer 14 is between 20nm and 250nm, for example, between 50nm and 150nm.

[0059] Here, the thickness d of the intermediate metal layer 14 is measured in a direction transverse to the surface 10 supporting the grating lines. However, in view of the grating line profile, the intermediate metal layer 14 does not necessarily have a uniform thickness over the entire surface.

[0060] The intermediate metal layer 14 is a continuous two-dimensional layer covering the surface of the grating lines. Similarly, the outer reflective layer 13 is a continuous two-dimensional layer covering the intermediate metal layer 14 below.

[0061] Figure 3 An example of a multi-metal diffraction grating with a pseudo-sinusoidal line profile according to an embodiment of the present invention is shown in a cross-sectional view. Grating lines 11 are formed directly in a substrate 1. An intermediate metal layer 14 with a thickness d is deposited on these lines, and an outer reflective layer 13 is deposited on the intermediate metal layer 14. The thickness e of the outer reflective layer 13 and the thickness d of the intermediate metal layer 14 are small enough to maintain the depth h of the grating lines.

[0062] In an alternative embodiment, a stack of several intermediate metal layers arranged between the substrate and the outer reflective layer is used. For example, a periodic stack consisting of a layer of chromium and a layer of gold is used, and this two-layer pattern is repeated twice to form a total stack consisting of four intermediate metal layers. Such a stack allows better mechanical damping and metal reinforcement.

[0063] The outer reflective layer 13 has a thickness e higher than the lower limit determined by the reflection coefficient, in this way, the diffraction grating has a high reflectivity in a spectral range extending over 100 nm around the central wavelength. On the other hand, the thickness e of the outer reflective layer 13 is less than another upper limit determined by the thermal diffusion length of the first metal. In addition, considering the cost of the first metal, especially when the first metal is gold, the thickness e of the outer metal layer 13 can be limited for economic reasons.

[0064] The thermal diffusion length is L th It is defined by the following equation, where D represents the diffusivity of the material: And it is particularly applicable to Gaussian beams, where t represents the full width at half maximum of the laser pulse.

[0065] [Table 2] Table 2 shows the thermal diffusion lengths of different metals.

[0066] Metal <![CDATA[Thermal diffusion length (×10 -6 .m -2 .s -1 )]]> Gold (Au) 127.2 Molybdenum (Mo) 53.9 Nickel (Ni) 23 Iridium (Ir) 50.2 Silver (Ag) 173 Copper (Cu) 117 Chromium (Cr) 29.9

[0067] Here, the thickness of the outer reflective layer 13 is measured in a direction transverse to the surface 10 supporting the grating lines. However, the outer reflective layer 13 does not necessarily have a uniform thickness over its entire surface in consideration of the grating line profile.

[0068] The thickness e of the outer reflective layer 13 is generally between about 100 nm and 500 nm, and preferably between 100 nm and 150 nm.

[0069] The thickness of the intermediate metal layer 14 and the outer reflective layer 13 is optimized using a test method. In addition, the ratio between the thickness (i) of the intermediate metal layer 14 and the thickness (r) of the outer reflective layer 13 is also optimized. Preferably, the ratio i / r is between 0 and 1.

[0070] Generally, the increase in the total thickness of the stack of multiple metal layers 13, 14 makes it possible to increase the volumetric heat dissipation capability of the stack compared to a single gold metal layer.

[0071] The minimum thickness e of the outer reflective layer 13 is determined to obtain a compromise between a high reflectivity and a maximum thickness e to ensure good flux resistance.

[0072] For example, an outer reflective layer 13 made of gold and an intermediate metal layer 14 made of nickel are selected. In order to obtain a high reflectivity in the spectral band greater than 100 nm at a wavelength of about 800 nm, a minimum thickness e of 100 nm is selected for the outer gold layer. In an exemplary embodiment, in order to increase the resistance of the diffraction grating, it seems interesting to use a 100 nm thick gold layer and a 50 nm thick nickel layer.

[0073] The intermediate metal layer 14 and the outer reflective layer 13 are deposited by any deposition technique known to a person skilled in the art. As a non-limiting example, evaporation techniques are used, possibly assisted by electron beam, ion beam sputtering, cathode sputtering and / or magnetron or atomic layer deposition.

[0074] This multi-metal diffraction grating structure allows the intermediate metal layer 14, for example made of nickel, to pump a part of the thermal energy of the gold layer and diffuse this thermal energy into the volume of the intermediate metal layer 14. This energy transfer can be explained by the mechanism of electronic thermalization of the metal of the outer reflection layer and the diffusion of a part of the thermal energy to the intermediate metal layer below. This multi-metal structure makes it possible to push back the melting threshold of the outer metal layer (for example made of gold) and distribute part of this thermal energy into the intermediate metal layer 14, for example made of nickel. Now, the melting point of nickel is higher than that of gold. Therefore, the diffraction grating based on a multi-metal stack has a higher resistance than the diffraction grating based on a single metal layer and has a higher resistance than the metal-dielectric diffraction grating consisting of a single metal layer covered with a dielectric layer stack.

[0075] The multi-metal reflective diffraction grating thus obtained operates with TM or TE polarization, similar to a reflective diffraction grating comprising a single reflective metal layer.

[0076] In an alternative, the diffraction grating comprises a stack of an outer reflective layer 14 and at least two intermediate metal layers.

[0077] exist Figure 2 In another alternative shown, the multi-metal diffraction grating further comprises an adhesive layer 2 arranged on the surface of the substrate 10 comprising the grating lines 11, the adhesive layer 2 being arranged between the substrate surface and the intermediate metal layer, the thickness of the adhesive layer being less than 25 nm, preferably less than 10 nm. The adhesive layer 2 is preferably made of chromium or titanium.

[0078] In another alternative, possibly in combination with one and / or another of the aforementioned alternatives, the polymetallic diffraction grating further comprises a thin dielectric layer deposited on the outer reflective layer 13. For example, the thin dielectric layer is made of silicon dioxide (SiO2). Preferably, the thickness of the thin dielectric layer is less than 50 nm. Such a thin dielectric layer has an effect on the spatial distribution of the electromagnetic field. The combination of the polymetallic grating and the thin dielectric layer provides a greater suppression of the high energy, ultrashort pulse light flux resistance of the reflective diffraction grating.

[0079] Advantageously, the multi-metal diffraction grating operates with TM or TE polarization.

[0080] Of course, various other modifications can be made to the invention within the framework of the attached claims.

Claims

1. A high peak energy ultrashort pulse flux-resistant reflection diffraction grating, the diffraction grating comprising grating lines (11) formed on a surface (10) of a substrate (1) and an outer reflection layer (13), characterized in that: The diffraction grating comprises at least one intermediate metal layer (14), the intermediate metal layer (14) being arranged between the outer reflection layer (13) and the substrate surface (10) comprising the grating lines (11), and the diffraction grating comprises an adhesive layer (2), the adhesive layer (2) being arranged on the surface of the substrate comprising the grating lines (11), the adhesive layer (2) being arranged between the substrate surface and the intermediate metal layer (14), the adhesive layer (2) having a thickness of less than 25 nanometers, the outer reflection layer (13) having an interface with the intermediate metal layer (14), the intermediate metal layer (14) being a continuous two-dimensional layer covering the surface of the grating lines (11), the outer reflection layer (13) being a continuous two-dimensional layer covering the intermediate metal layer (14), the outer reflection layer (13) being composed of a first metal, and the intermediate metal layer (14) being composed of another The invention relates to a reflective diffraction grating comprising a first metal, the second metal having an electron-phonon coupling coefficient higher than that of the first metal, the thickness of the outer reflective layer (13) being between 100 nm and 500 nm, the thickness of the outer reflective layer (13) being within a range having a lower limit determined by the reflection coefficient of the first metal and an upper limit determined by the thermal diffusion length of the first metal, and the thickness of the intermediate metal layer (14) being between 20 nm and 250 nm, the ratio between the thickness i of the intermediate metal layer (14) and the thickness r of the outer reflective layer (13) being between 0 and 1, and wherein the ratio i / r and the thickness of the intermediate metal layer (14) and the outer reflective layer (13) are optimized to increase the high peak energy ultrashort pulse light flux resistance of the reflective diffraction grating, wherein the second metal is selected from nickel, copper, molybdenum, chromium, silver or a silver-iridium alloy.

2. The diffraction grating according to claim 1, wherein: The first metal is selected from gold and silver, or an alloy of gold and / or silver, or gold-nickel, gold-copper, gold-silver, gold-silver-iridium or gold-copper-silver-iridium alloy.

3. The diffraction grating according to claim 2, wherein: The bonding layer (2) is made of chromium or titanium.

4. The diffraction grating according to claim 1 or 2, wherein: The substrate is made of silicon dioxide, silicon, microcrystalline glass, heat-resistant glass or borosilicate.

5. The diffraction grating according to claim 1 or 2, wherein: The grating lines (11) are formed in the substrate, or the grating lines (11) are formed by a photosensitive resin deposited on the substrate.

6. The diffraction grating according to claim 1 or 2, further comprising a dielectric thin film coating formed at a surface of the outer reflection layer (13).

7. The diffraction grating according to claim 1 or 2, further comprising at least one further intermediate metal layer arranged between the substrate and the intermediate metal layer (14), the intermediate metal layer (14) and the further intermediate metal layer forming a stack of several intermediate metal layers.

8. A method for manufacturing a reflective diffraction grating, comprising the steps of: Diffraction grating lines (11) are formed on a surface (10) of a substrate (1); an intermediate metal layer (14) is deposited, the intermediate metal layer (14) is a continuous two-dimensional layer covering the surface of the grating lines (11); and an outer reflection layer (13) is deposited, the outer reflection layer (13) is a continuous two-dimensional layer covering the intermediate metal layer (14), the outer reflection layer (13) has an interface with the intermediate metal layer (14), the outer reflection layer is composed of a first metal, and the intermediate metal layer (14) is composed of another metal, the another metal is selected from nickel, copper, molybdenum, chromium, silver or silver-iridium alloy, the another metal has an electron-phonon coupling coefficient higher than the electron-phonon coupling coefficient of the first metal, and the thickness of the outer reflection layer is 100 nm. m to 500 nm, the thickness of the outer reflection layer (13) is within a range having a lower limit determined by the reflection coefficient of the first metal and an upper limit determined by the thermal diffusion length of the first metal, the thickness of the intermediate metal layer (14) is between 20 nm and 250 nm, the ratio between the thickness i of the intermediate metal layer (14) and the thickness r of the outer reflection layer (13) is between 0 and 1, and wherein the ratio i / r and the thickness of the intermediate metal layer (14) and the outer reflection layer (13) are optimized to increase the high peak energy ultrashort pulse light flux resistance of the reflective diffraction grating, and the method further comprises an additional step of depositing an adhesion layer (2) on the grating lines before the step of depositing the intermediate metal layer (14).